Reflective mask blank, method for producing reflective mask blank, and method for producing reflective mask

By using a hard mask film composed of Y, Al, or Pd, the etching selectivity is enhanced, addressing the inaccuracies in conventional reflective mask manufacturing by maintaining vertical sides and reducing processing time.

JP2024156304APending Publication Date: 2024-11-06AGC INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023070660
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-24
Publication Date
2024-11-06

AI Technical Summary

Technical Problem

Conventional reflective mask manufacturing processes face issues with insufficient selectivity between the hard mask film and the absorbing film during etching, leading to increased processing time and inaccurate line widths due to the inclination of opening sides in the resist and absorbing films.

Method used

Incorporating a hard mask film made of elements such as Y, Al, or Pd improves the selectivity of etching processes, allowing for thinner films and maintaining vertical side surfaces, thereby enhancing processing accuracy.

Benefits of technology

This approach ensures precise transfer of patterns by reducing the inclination of opening sides in the absorbing film, thus improving the overall processing accuracy and efficiency in reflective mask manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024156304000001_ABST
    Figure 2024156304000001_ABST
Patent Text Reader

Abstract

To provide a technique for improving the processing accuracy of an opening pattern in an absorption film.SOLUTION: A reflective mask blank includes a substrate, a multilayer reflective film, a protective film, an absorption film, and a hard mask film, in the stated order. The hard mask film contains at least one element X1 selected from Y, Al, Hf and Pd.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a reflective mask blank, a method for manufacturing a reflective mask blank, and a method for manufacturing a reflective mask. [Background technology]

[0002] In recent years, with the miniaturization of semiconductor devices, EUV lithography (EUVL), an exposure technology using extreme ultraviolet (EUV) light, has been developed. EUV includes soft X-rays and vacuum ultraviolet light, and specifically refers to light with a wavelength of about 0.2 nm to 100 nm. At present, EUV with a wavelength of about 13.5 nm is mainly being considered.

[0003] In EUVL, a reflective mask is used. The reflective mask has, in this order, a substrate such as a glass substrate, a multilayer reflective film that reflects EUV light, a protective film that protects the multilayer reflective film, and an absorbing film that absorbs EUV light. The absorbing film may not only absorb EUV light, but also shift the phase of the EUV light. In other words, the absorbing film may be a phase shift film. An opening pattern is formed in the absorbing film. In EUVL, the opening pattern of the absorbing film is transferred to a target substrate such as a semiconductor substrate. Transferring includes reducing and transferring.

[0004] The reflective mask blank described in Patent Document 1 comprises a substrate, a multilayer reflective film, a protective film, an absorbing film, an etching mask film corresponding to a hard mask film, and a resist film, in this order. The absorbing film contains iridium (Ir) and an additive element. The etching mask film contains chromium (Cr) and an additive element. The additive element for Cr is at least one selected from O, N, C, B, and H. Examples of materials for the etching mask film include CrN, CrO, CrC, CrON, CrOC, CrCN, and CrOCN. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2022 / 138360 Summary of the Invention [Problem to be solved by the invention]

[0006] The method for manufacturing a reflective mask includes transferring an opening pattern of a resist film to a hard mask film, and transferring the opening pattern of the hard mask film to an absorbing film. A first etching gas is used for processing the hard mask film, and a second etching gas is used for processing the absorbing film.

[0007] Conventionally, the selectivity of the hard mask film and the absorbing film to the second etching gas was insufficient depending on the combination of materials. Therefore, it is considered to make the hard mask film thicker in order to secure the processing time when processing the absorbing film.

[0008] When the hard mask film is thickened, the processing time for the hard mask film is extended. Conventionally, the line width of the resist film may become narrower over time. This is because oxygen radicals etch the side of the opening in the resist film during processing of the hard mask film.

[0009] When the line width of the resist film becomes narrower over time during processing of the hard mask film, the side of the opening in the hard mask film becomes inclined. If the absorbing film is processed using a hard mask film having such an opening, the side of the opening in the absorbing film also becomes inclined.

[0010] One aspect of the present disclosure provides a technique for improving the processing accuracy of an opening pattern in an absorbing film. [Means for solving the problem]

[0011] A reflective mask blank according to one embodiment of the present disclosure includes a substrate, a multilayer reflective film, a protective film, an absorbing film, and a hard mask film, in this order. The hard mask film contains at least one element X1 selected from Y, Al, Hf, and Pd. Effect of the Invention

[0012] According to one embodiment of the present disclosure, the hard mask film contains at least one element X1 selected from Y, Al, Hf, and Pd, which can improve the processing accuracy of the opening pattern of the hard mask film, and therefore the processing accuracy of the opening pattern of the absorbing film. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a cross-sectional view showing a reflective mask blank according to one embodiment. [Diagram 2] FIG. 2 is a flowchart showing a method for manufacturing a reflective mask blank according to one embodiment. [Diagram 3] FIG. 3 is a cross-sectional view showing a reflective mask according to an embodiment. [Figure 4] FIG. 4 is a flowchart showing a method for manufacturing a reflective mask according to an embodiment. [Diagram 5] FIG. 5(A) is a cross-sectional view showing an embodiment of a substrate preparation, FIG. 5(B) is a cross-sectional view showing an embodiment of a substrate at the end of processing a hard mask film, and FIG. 5(C) is a cross-sectional view showing an embodiment of a substrate at the end of processing an absorbing film. [Figure 6] FIG. 6(A) is a cross-sectional view showing a conventional example of substrate preparation, FIG. 6(B) is a cross-sectional view showing a conventional example during processing of a hard mask film, FIG. 6(C) is a cross-sectional view showing a conventional example at the completion of processing of the hard mask film, FIG. 6(D) is a cross-sectional view showing a conventional example during processing of an absorbing film, and FIG. 6(E) is a cross-sectional view showing a conventional example at the completion of processing of the absorbing film. [Figure 7] FIG. 7 is a cross-sectional view showing an example of EUV light reflected by the reflective mask of FIG. [Figure 8] FIG. 8 is an exaggerated cross-sectional view showing an example of the shape of the absorbing film at the end of processing. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In each drawing, the same or corresponding components are denoted by the same reference numerals, and the description may be omitted. In the specification, the symbol "~" indicating a range of values ​​means that the values ​​before and after the symbol are included as the lower and upper limits.

[0015] In each drawing, the X-axis direction, the Y-axis direction, and the Z-axis direction are perpendicular to each other. The Z-axis direction is perpendicular to the first main surface 10a of the substrate 10. The X-axis direction is perpendicular to the incidence plane of the EUV light (plane including the incident light beam and the reflected light beam). As shown in FIG. 7, the incident light beam is inclined toward the positive Y-axis direction as it moves toward the negative Z-axis direction, and the reflected light beam is inclined toward the positive Y-axis direction as it moves toward the positive Z-axis direction.

[0016] A reflective mask blank 1 according to one embodiment will be described with reference to FIG. 1. The reflective mask blank 1 includes, for example, a substrate 10, a multilayer reflective film 11, a protective film 12, an absorbing film 13, and a hard mask film 14, in this order. The multilayer reflective film 11, the protective film 12, the absorbing film 13, and the hard mask film 14 are formed on a first main surface 10a of the substrate 10, in this order. The multilayer reflective film 11 reflects EUV light. The protective film 12 protects the multilayer reflective film 11 from a second etching gas when the absorbing film 13 is processed. The absorbing film 13 absorbs EUV light. The hard mask film 14 protects a part of the absorbing film 13 from a second etching gas when the absorbing film 13 is processed.

[0017] The reflective mask blank 1 may further have a functional film not shown in FIG. 1. For example, the reflective mask blank 1 may have a conductive film on the opposite side of the multilayer reflective film 11 with respect to the substrate 10. The conductive film is formed on the second main surface 10b of the substrate 10. The second main surface 10b is the surface facing opposite to the first main surface 10a. The conductive film is used, for example, to attach the reflective mask 2 to an electrostatic chuck of an exposure tool. The reflective mask blank 1 may have a diffusion barrier film (not shown) between the multilayer reflective film 11 and the protective film 12. The diffusion barrier film suppresses diffusion of metal elements contained in the protective film 12 into the multilayer reflective film 11.

[0018] Although not shown, the reflective mask blank 1 may have a buffer film between the protective film 12 and the absorbing film 13. The buffer film protects the protective film 12 from a second etching gas that forms an opening pattern 13a in the absorbing film 13. The buffer film is etched more slowly than the absorbing film 13. Unlike the protective film 12, the buffer film will ultimately have the same opening pattern as the opening pattern 13a of the absorbing film 13.

[0019] Next, a method for manufacturing a reflective mask blank 1 according to one embodiment will be described with reference to FIG. 2. The method for manufacturing the reflective mask blank 1 includes, for example, steps S101 to S105 shown in FIG. 2. In step S101, a substrate 10 is prepared. In step S102, a multilayer reflective film 11 is formed on a first main surface 10a of the substrate 10. In step S103, a protective film 12 is formed on the multilayer reflective film 11. In step S104, an absorbing film 13 is formed on the protective film 12. In step S105, a hard mask film 14 is formed on the absorbing film 13. The method for manufacturing the reflective mask blank 1 may further include a step of forming a functional film not shown in FIG. 2.

[0020] Next, a reflective mask 2 according to an embodiment will be described with reference to Fig. 3. The reflective mask 2 is produced, for example, by using the reflective mask blank 1 shown in Fig. 1, and includes an opening pattern 13a in an absorbing film 13. In EUVL, the opening pattern 13a in the absorbing film 13 is transferred to a target substrate such as a semiconductor substrate. Transferring includes reducing and transferring. Note that the hard mask film 14 shown in Fig. 1 is not included in the reflective mask 2.

[0021] Next, a method for manufacturing a reflective mask 2 according to one embodiment will be described with reference to Fig. 4 and Fig. 5. The method for manufacturing a reflective mask 2 has steps S201 to S204 shown in Fig. 4. In step S201, a reflective mask blank 1 is prepared as shown in Fig. 5(A). The reflective mask blank 1 includes a resist film 16 as shown in Fig. 5(A). The resist film 16 is formed on a hard mask film 14. An opening pattern to be transferred to the absorbing film 13 is formed in the resist film 16.

[0022] In step S202, as shown in FIG. 5B, the hard mask film 14 is processed using the resist film 16 having an opening pattern. In the openings of the resist film 16, the hard mask film 14 is exposed to a first etching gas, and the first etching gas etches the hard mask film 14. At the end of step S202, the resist film 16 remains. As a result, the opening pattern of the resist film 16 is transferred to the hard mask film 14.

[0023] In this embodiment, the first etching gas contains Ar gas. It is preferable that the first etching gas does not substantially contain an oxygen-based gas in order to suppress the line width W of the resist film 16 from becoming narrow. The oxygen-based gas is O2 gas, O3 gas, or a mixed gas thereof. The content of the oxygen-based gas in the first etching gas is preferably 0.1 volume % or less. It is preferable that the first etching gas is composed of only Ar gas. It is preferable that the first etching gas is a plasma.

[0024] An example of processing conditions for the hard mask film 14 is shown below. <Hard mask film processing conditions> Etching gas: Ar gas plasma, Source power: 150W~1000W, Bias: 50W~150W, Pressure: 0.2Pa~1.0Pa.

[0025] In step S203, as shown in FIG. 5(C), the absorbing film 13 is processed using the hard mask film 14 having an opening pattern. In the openings of the hard mask film 14, the absorbing film 13 is exposed to a second etching gas, and the second etching gas etches the absorbing film 13. The hard mask film 14 has higher resistance to the second etching gas than the absorbing film 13. At the end of step S203, the hard mask film 14 remains. As a result, the opening pattern of the hard mask film 14 is transferred to the absorbing film 13.

[0026] The second etching gas includes a fluorine-based gas. The fluorine-based gas includes at least one selected from, for example, CF4 gas, CHF3 gas, C2F6 gas, C3F6 gas, C4F6 gas, C4F8 gas, CH2F2 gas, CH3F gas, C3F8 gas, F2 gas, SF6 gas, and NF3 gas. The second etching gas may include an active gas or an inert gas in addition to the fluorine-based gas. The active gas includes, for example, O2 gas. The inert gas includes, for example, at least one selected from N2 gas, He gas, and Ar gas. The second etching gas is preferably a plasma gas.

[0027] An example of processing conditions for the absorbing film 13 is shown below. <Absorbent film processing conditions> Etching gas: Plasma-mixed gas containing CF4 gas and O2 gas, Source power: 150W~2000W, Bias: 20W~150W, Pressure: 0.2Pa~1.0Pa.

[0028] In step S204, although not shown, the hard mask film 14 is removed. For example, a third etching gas is used to remove the hard mask film 14. The third etching gas contains Ar gas, similar to the first etching gas. The third etching gas is preferably a plasma gas. A chemical solution may be used to remove the hard mask film 14.

[0029] Next, a processing procedure of a conventional reflective mask blank 1 will be described with reference to Fig. 6. As shown in Fig. 6(A), the conventional reflective mask blank 1 has a substrate 10, a multilayer reflective film 11, a protective film 12, an absorbing film 13, a hard mask film 14A, and a resist film 16, in this order. The conventional hard mask film 14A contains Cr or Ru as a main component. A fourth etching gas is used to process the conventional hard mask film 14A.

[0030] The fourth etching gas includes a chlorine-based gas and an oxygen-based gas. The chlorine-based gas includes at least one selected from, for example, Cl2 gas, SiCl4 gas, CHCl3 gas, CCl4 gas, and BCl3 gas. The oxygen-based gas includes at least one selected from, for example, O2 gas and O3 gas. The fourth etching gas may include an inert gas in addition to the chlorine-based gas and the oxygen-based gas. The inert gas includes at least one selected from, for example, N2 gas, He gas, and Ar gas. The fourth etching gas is preferably a plasma gas.

[0031] The absorbing film 13 preferably contains a noble metal element. The noble metal element is, for example, Ir, Pt, Pd, Os, or Ru. These noble metal elements have a relatively small refractive index, so that the thickness of the absorbing film 13 can be reduced while ensuring the phase difference. However, these noble metal elements have a slow etching rate. Therefore, in order to ensure the processing time when processing the absorbing film 13, it is considered to thicken the hard mask film 14A.

[0032] When the hard mask film 14A is thickened, the processing time of the hard mask film 14A is extended. Conventionally, as shown in FIG. 6B, the line width W of the resist film 16 may become narrower over time. This is because oxygen radicals etch the side surfaces of the openings in the resist film 16 when the hard mask film 14A is processed.

[0033] As shown in Figures 6(B) and 6(C), the line width W of the resist film 16 narrows over time during processing of the hard mask film 14A, causing the side surfaces of the openings in the hard mask film 14A to become inclined. If the absorbing film 13 is processed using the hard mask film 14A having such openings, the side surfaces of the openings in the absorbing film 13 also become inclined, as shown in Figures 6(D) and 6(E).

[0034] This is because the hard mask film 14A has a trapezoidal cross-sectional shape as shown in Fig. 6(C). As shown in Fig. 6(D), in the positions where the hard mask film 14A is thin, the hard mask film 14A disappears earlier and etching of the absorption film 13 starts earlier than in the positions where the hard mask film 14A is thick. As a result, the side surface of the opening in the absorption film 13 also becomes inclined.

[0035] Next, the processing procedure of the reflective mask blank 1 of the embodiment will be described with reference to Fig. 5 again. The hard mask film 14 of the embodiment differs from the conventional hard mask film 14A in that it contains at least one element X1 selected from Y, Al, Hf, and Pd. The total content of the element X1 is preferably 30 at% to 100 at%, and more preferably 40 at% to 100 at%.

[0036] Table 1 shows the boiling points of fluorides under atmospheric pressure. When there are multiple valences of fluoride, it is considered that the fluoride with the lowest boiling point is generated. It is considered that the selectivity (ER1 / ER2) for the second etching gas containing a fluorine-based gas increases as the difference in the boiling points of the fluoride between the hard mask film 14 and the absorbing film 13 increases. ER1 is the etching rate of the absorbing film 13, and ER2 is the etching rate of the hard mask film 14.

[0037] [Table 1] As shown in Table 1, Y, Al, Hf, and Pd constituting the hard mask film 14 of the embodiment have higher boiling points of fluorides than Cr and Ru constituting the hard mask film 14A of the conventional example. Therefore, according to the embodiment, the difference in boiling points of fluorides between the hard mask film 14 and the absorbing film 13 is larger than that of the conventional example, and the selectivity (ER1 / ER2) to the second etching gas containing a fluorine-based gas is larger than that of the conventional example. Note that Ir shown in Table 1 is an example of an element constituting the absorbing film 13.

[0038] As described above, according to the embodiment, the selectivity (ER1 / ER2) for the second etching gas is larger than that of the conventional example. Therefore, according to the embodiment, the thickness of the hard mask film 14 can be reduced compared to the conventional example. As a result, the processing time when processing the hard mask film 14 can be shortened, and the side of the opening of the hard mask film 14 can be prevented from being inclined. Therefore, as shown in FIG. 5(C), the absorbing film 13 can be processed using the hard mask film 14 having an opening with a vertical side, and the side of the opening of the absorbing film 13 can be prevented from being inclined.

[0039] As described above, the boiling points of the fluorides of Y, Al, Hf, and Pd constituting the hard mask film 14 of the embodiment are high, and it is difficult to process them under the same conditions as in the conventional example. Therefore, the first etching gas is used instead of the fourth etching gas to process the hard mask film 14 of the embodiment.

[0040] The first etching gas contains Ar gas. As shown in Fig. 5(B), in the opening of the resist film 16, the hard mask film 14 is exposed to the first etching gas, and the first etching gas etches the hard mask film 14. Since the first etching gas does not substantially contain an oxygen-based gas, oxygen radicals do not etch the side surface of the opening of the resist film 16.

[0041] This makes it possible to prevent the line width W of the resist film 16 from becoming narrower over time, and to prevent the side surfaces of the openings in the hard mask film 14 from being inclined. Therefore, as shown in Fig. 5(C), the absorbing film 13 can be processed using the hard mask film 14 having an opening with vertical side surfaces, and it is possible to prevent the side surfaces of the openings in the absorbing film 13 from being inclined.

[0042] An example of the shape of the absorbing film 13 at the end of processing of the absorbing film 13 is shown in an exaggerated manner in Fig. 8. The shape of the absorbing film 13 can be evaluated based on the taper angle α and the side etching amount E shown in Fig. 8. The side etching amount is also called the undercut amount.

[0043] The taper angle α is the angle between the boundary line between the absorbing film 13 and the protective film 12 and the side surface of the opening in the absorbing film 13. The taper angle α is preferably 70° to 90°, and more preferably 80° to 90°. The larger the taper angle α, the more preferable it is, and it may be 90°.

[0044] The side etching amount E is a shift amount of the side surface of the opening of the hard mask film 14 with respect to the side surface of the opening of the hard mask film 14 at the boundary between the hard mask film 14 and the absorption film 13. The side etching amount E is preferably 0 nm to 10 nm, and more preferably 0 nm to 5 nm. The smaller the side etching amount E, the more preferable, and it may be 0 nm.

[0045] The hard mask film 14 may contain a compound of element X1. The compound of element X1 contains, for example, at least one element selected from O, N, B, H, and C. By adding at least one element selected from O, N, B, H, and C, crystallization of the hard mask film 14 can be suppressed, and roughness of the side surface of the opening in the hard mask film 14 can be reduced.

[0046] The compound of element X1 may contain at least one element selected from Ru and Cr. By adding at least one element selected from Ru and Cr, the amount of side etching E can be reduced.

[0047] In step S201, the thickness t of the hard mask film 14 is preferably 0.1 nm to 10 nm. If the thickness t of the hard mask film 14 is 0.1 nm or more, a sufficient amount of the hard mask film 14 remains when processing of the absorbing film 13 is completed. If the thickness t of the hard mask film 14 is 10 nm or less, the processing time during processing of the hard mask film 14 can be shortened, and the side surface of the opening of the hard mask film 14 can be prevented from being inclined. The thickness t of the hard mask film 14 is more preferably 0.1 nm to 6 nm.

[0048] When the material of the hard mask film 14 is Y2O3, the thickness t of the hard mask film 14 is preferably 0.1 nm to 5 nm. When the material of the hard mask film 14 is a Y alloy, the thickness t of the hard mask film 14 is preferably 0.1 nm to 10 nm. When the material of the hard mask film 14 is simple Al, the thickness t of the hard mask film 14 is preferably 2.0 nm to 10 nm.

[0049] 1 again, the substrate 10, the multilayer reflective film 11, the protective film 12, and the absorbing film 13 will be described in this order. The hard mask film 14 is as described above.

[0050] The substrate 10 is, for example, a glass substrate. The material of the substrate 10 is preferably quartz glass containing TiO2. Quartz glass has a smaller linear expansion coefficient and a smaller dimensional change due to temperature change than general soda-lime glass. Quartz glass may contain 80% to 95% by mass of SiO2 and 4% to 17% by mass of TiO2. When the TiO2 content is 4% to 17% by mass, the linear expansion coefficient is approximately zero near room temperature, and there is almost no dimensional change near room temperature. Quartz glass may contain a third component or impurity other than SiO2 and TiO2. The material of the substrate 10 may be crystallized glass in which a β-quartz solid solution is precipitated, silicon, metal, or the like.

[0051] The substrate 10 has a first main surface 10a and a second main surface 10b facing opposite to the first main surface 10a. A multilayer reflective film 11 and the like are formed on the first main surface 10a. The size of the substrate 10 in plan view (viewed in the Z-axis direction) is, for example, 152 mm long and 152 mm wide. The vertical and horizontal dimensions may be 152 mm or more. The first main surface 10a and the second main surface 10b each have, for example, a square quality assurance area in the center. The size of the quality assurance area is, for example, 142 mm long and 142 mm wide. The quality assurance area of ​​the first main surface 10a preferably has a root-mean-square roughness (Rq) of 0.15 nm or less and a flatness of 100 nm or less. In addition, it is preferable that the quality assurance area of ​​the first main surface 10a does not have a defect that causes a phase defect.

[0052] The multilayer reflective film 11 reflects EUV light. The multilayer reflective film 11 is, for example, a laminate of high refractive index layers and low refractive index layers alternately. The high refractive index layers are made of, for example, silicon (Si), and the low refractive index layers are made of, for example, molybdenum (Mo), and a Mo / Si multilayer reflective film is used. Note that Ru / Si multilayer reflective film, Mo / Be multilayer reflective film, Mo compound / Si compound multilayer reflective film, Si / Mo / Ru multilayer reflective film, Si / Mo / Ru / Mo multilayer reflective film, Si / Ru / Mo / Ru multilayer reflective film, Si / Ru / Mo multilayer reflective film, and the like can also be used as the multilayer reflective film 11.

[0053] The thickness of each layer constituting the multilayer reflective film 11 and the number of repeating units of the layers can be appropriately selected depending on the material of each layer and the reflectance to EUV light. When the multilayer reflective film 11 is a Mo / Si multilayer reflective film, in order to achieve a reflectance of 60% or more to EUV light with an incident angle θ (see FIG. 7) of 6°, Mo layers with a thickness of 2.3±0.1 nm and Si layers with a thickness of 4.5±0.1 nm may be laminated so that the number of repeating units is 30 or more and 60 or less. The multilayer reflective film 11 preferably has a reflectance of 60% or more to EUV light with an incident angle θ of 6°. The reflectance is more preferably 65% ​​or more.

[0054] The film formation method for each layer constituting the multilayer reflective film 11 is, for example, a DC sputtering method, a magnetron sputtering method, an ion beam sputtering method, or the like. When forming a Mo / Si multilayer reflective film using the ion beam sputtering method, an example of the film formation conditions for each of the Mo layer and the Si layer is as follows. <Film formation conditions for Si layer> Target: Si target, Sputtering gas: Ar gas, Gas pressure: 1.3×10 -2 Pa~2.7×10 -2 Pa, Ion acceleration voltage: 300V~1500V, Film formation rate: 0.030nm / sec~0.300nm / sec, Film thickness of Si layer: 4.5±0.1nm. <Film formation conditions for Mo layer> Target: Mo target, Sputtering gas: Ar gas, Gas pressure: 1.3×10 -2 Pa~2.7×10 -2 Pa, Ion acceleration voltage: 300V~1500V, Film formation rate: 0.030nm / sec~0.300nm / sec, Film thickness of Mo layer: 2.3±0.1nm. <Repeating unit of Si layer and Mo layer> Number of repeating units: 30~60 (preferably 40~50).

[0055] The protective film 12 is formed between the multilayer reflective film 11 and the absorption film 13 to protect the multilayer reflective film 11. The protective film 12 protects the multilayer reflective film 11 from the second etching gas during the processing of the absorption film 13, that is, in step S203. The protective film 12 remains on the multilayer reflective film 11 without being removed even when exposed to the second etching gas.

[0056] The protective film 12 contains at least one element selected from, for example, Ru, Rh, and Si. When the protective film 12 contains Rh, the protective film 12 may contain only Rh, or may contain an Rh compound. The Rh compound may contain, in addition to Rh, at least one element Z1 selected from the group consisting of Ru, Nb, Mo, Ta, Ir, Pd, Zr, Y, and Ti.

[0057] By adding Ru, Nb, Mo, Zr, Y, or Ti to Rh, the extinction coefficient can be reduced while suppressing an increase in the refractive index, and the reflectance to EUV light can be improved. Also, by adding Ta, Ir, Pd, or Y to Rh, the resistance to the second etching gas can be improved.

[0058] The Rh compound may contain, in addition to Rh, at least one element Z2 selected from the group consisting of N, O, C, and B. The element Z2 reduces the resistance of the protective film 12 to the second etching gas, but improves the smoothness of the protective film 12 by reducing the crystallinity of the protective film 12. The Rh compound containing the element Z2 has an amorphous structure or a microcrystalline structure. When the Rh compound has an amorphous structure or a microcrystalline structure, the X-ray diffraction profile of the Rh compound does not have a clear peak.

[0059] The protective film 12 may be a film consisting of a single layer, or may be a multi-layer film having a lower layer and an upper layer. The lower layer of the protective film 12 is a layer formed in contact with the uppermost surface of the multilayer reflective film 11. The upper layer of the protective film 12 is in contact with the lowermost surface of the absorbing film 13. By forming the protective film 12 in this manner with a multi-layer structure, materials having excellent predetermined functions can be used for each layer, and therefore the protective film 12 as a whole can be made multifunctional.

[0060] The upper layer of the protective film 12 preferably contains Rh, and more preferably contains an Rh compound. The lower layer of the protective film 12 preferably contains at least one element selected from the group consisting of Ru, Nb, Mo, Zr, Y, C, and B, and more preferably contains Ru. In addition, when the protective film 12 is a multilayer film, the thickness of the protective film 12 described below means the total thickness of the multilayer film.

[0061] The thickness of the protective film 12 is preferably 1.0 nm to 4.0 nm, more preferably 2.0 nm to 3.5 nm, and even more preferably 2.5 nm to 3.0 nm. If the thickness of the protective film 12 is 1.0 nm or more, the etching resistance is good. Also, if the thickness of the protective film 12 is 4.0 nm or less, the reflectivity with respect to EUV light is good.

[0062] The density of the protective film 12 is preferably 10.0 g / cm 3 ~14.0 g / cm 3 . If the density of the protective film 12 is 10.0 g / cm 3 or more, the etching resistance is good. Also, if the density of the protective film 12 is 14.0 g / cm 3 or less, a decrease in the reflectivity with respect to EUV light can be suppressed.

[0063] The upper surface of the protective film 12, that is, the surface on which the absorption film 13 of the protective film 12 is formed, preferably has a root mean square roughness Rq of 0.20 nm or less, more preferably 0.17 nm or less. If the root mean square roughness Rq is 0.20 nm or less, an absorption film 13 or the like can be smoothly formed on the protective film 12. Also, scattering of EUV light can be suppressed, and the reflectivity with respect to EUV light can be improved. The root mean square roughness Rq is preferably 0.05 nm or more.

[0064] The method for forming the protective film 12 is, for example, a DC sputtering method, a magnetron sputtering method, an ion beam sputtering method, or the like. When forming a Rh film using the DC sputtering method, an example of the film formation conditions is as follows. <Film formation conditions of Rh film> Target: Rh target, Sputtering gas: Ar gas, Gas pressure: 1.0×10 -2 Pa to 1.0×10 0 Pa, Output density of target: 1.0 W / cm 2 ~8.5 W / cm 2 、 Film formation rate: 0.020nm / sec~1.000nm / sec, Film thickness: 1nm~10nm.

[0065] The absorbing film 13 absorbs EUV light. The absorbing film 13 is a film in which an opening pattern 13a is to be formed. The opening pattern 13a is not formed in the manufacturing process of the reflective mask blank 1, but is formed in the manufacturing process of the reflective mask 2. The absorbing film 13 may not only absorb EUV light, but also shift the phase of the EUV light. In other words, the absorbing film 13 may be a phase shift film. The phase shift film shifts the phase of the second EUV light L2 relative to the first EUV light L1 shown in FIG. 7.

[0066] The first EUV light L1 is light that passes through the opening pattern 13a without passing through the absorbing film 13, is reflected by the multilayer reflective film 11, and passes through the opening pattern 13a without passing through the absorbing film 13 again. The second EUV light L2 is light that passes through the absorbing film 13 while being absorbed by the absorbing film 13, is reflected by the multilayer reflective film 11, and passes through the absorbing film 13 while being absorbed by the absorbing film 13 again.

[0067] The phase difference (≧0) between the first EUV light L1 and the second EUV light L2 is, for example, 170° to 250°. The phase of the first EUV light L1 may be ahead of or behind the phase of the second EUV light L2. The absorbing film 13 improves the contrast of the transferred image by utilizing the interference between the first EUV light L1 and the second EUV light L2. The transferred image is an image obtained by transferring the opening pattern 13a of the absorbing film 13 onto the target substrate.

[0068] In EUVL, a so-called projection effect (shadowing effect) occurs. The shadowing effect refers to a region in which the sidewall of the opening pattern 13a blocks the EUV light due to the incident angle θ of the EUV light being not 0° (for example, 6°), resulting in a positional or dimensional shift of the transferred image. In order to reduce the shadowing effect, it is effective to reduce the height of the sidewall of the opening pattern 13a, and it is also effective to thin the absorbing film 13.

[0069] The thickness of the absorbing film 13 is, for example, 60 nm or less, and preferably 50 nm or less, in order to reduce the shadowing effect. The thickness of the absorbing film 13 is preferably 20 nm or more, and more preferably 30 nm or more, in order to ensure a phase difference between the first EUV light L1 and the second EUV light L2.

[0070] In order to reduce the thickness of the absorbing film 13 so as to reduce the shadowing effect while ensuring the phase difference between the first EUV light L1 and the second EUV light L2, it is effective to reduce the refractive index n of the absorbing film 13. Also, in order to reduce the reflectance for EUV light, it is effective to increase the extinction coefficient k of the absorbing film 13. Thus, the absorbing film 13 is required to have excellent optical properties.

[0071] The refractive index n of the absorbing film 13 is preferably 0.940 or less, more preferably 0.930 or less, even more preferably 0.929 or less, particularly preferably 0.925 or less, even more particularly preferably 0.920 or less, even more particularly preferably 0.918 or less, even more preferably 0.910 or less, and most preferably 0.900 or less. The smaller the refractive index n of the absorbing film 13, the thinner the absorbing film 13 can be. The refractive index n of the absorbing film 13 is preferably 0.885 or more. In this specification, the refractive index is the refractive index for EUV light (for example, light with a wavelength of 13.5 nm).

[0072] The extinction coefficient k of the absorbing film 13 is preferably 0.030 or more, more preferably 0.034 or more, even more preferably 0.036 or more, and particularly preferably 0.038 or more. The larger the extinction coefficient k of the absorbing film 13, the easier it is to obtain a desired reflectance with a thin film thickness. The extinction coefficient k of the absorbing film 13 is preferably 0.065 or less. In this specification, the extinction coefficient is the extinction coefficient for EUV light (for example, light with a wavelength of 13.5 nm).

[0073] The optical properties (refractive index n and extinction coefficient k) of the absorbing film 13 are taken from the database of the Center for X-Ray Optics, Lawrence Berkeley National Laboratory, or values ​​calculated from the "incident angle dependence" of reflectance described below.

[0074] The incident angle θ of the EUV light, the reflectance R for the EUV light, the refractive index n of the absorbing film 13, and the extinction coefficient k of the absorbing film 13 satisfy the following formula (1). R = |(sinθ-((n+ik) 2 -cos 2 θ) 1 / 2 ) / (sinθ+((n+ik) 2 -cos 2 θ) 1 / 2 )|···(1) A number of combinations of the incident angle θ and the reflectance R are measured, and the refractive index n and the extinction coefficient k are calculated by the least squares method so that the error between the multiple measurement data and equation (1) is minimized.

[0075] The absorbing film 13 preferably contains a noble metal element. The noble metal element is, for example, Ir, Pt, Pd, Os, or Ru. These noble metal elements have a relatively small refractive index, so that the thickness of the absorbing film 13 can be reduced while ensuring the phase difference. However, these noble metal elements have a slow etching rate. Therefore, in this embodiment, a hard mask film 14 is used.

[0076] The absorbing film 13 may contain at least one element selected from Ir, Pt, Pd, Co, Ni, Os, and Ru. These elements have a relatively small refractive index, so that the thickness of the absorbing film 13 can be reduced while ensuring the phase difference. However, these elements have a slow etching rate. Therefore, in this embodiment, a hard mask film 14 is used.

[0077] The absorbing film 13 preferably has a layer made of an Ir-based material. In this embodiment, the absorbing film 13 is a single layer, but may be a multi-layer. In any case, it is preferable that at least one layer constituting the absorbing film 13 is made of an Ir-based material. The Ir-based material is a material containing Ir as a main component. The Ir-based material preferably contains 25 at% to 100 at% of Ir, more preferably contains 30 at% to 100 at% of Ir, further preferably contains 40 at% to 100 at% of Ir, and particularly preferably contains 50 at% to 100 at% of Ir. The Ir-based material may be simple Ir, but is preferably an Ir compound.

[0078] The Ir compound preferably contains at least one element selected from O, B, C, and N. By adding at least one element selected from O, B, C, and N, it is possible to suppress crystallization while suppressing deterioration of optical properties, and to reduce roughness of the side surface of the opening pattern 13a. The Ir compound preferably contains O, and more preferably contains O and N.

[0079] Incidentally, inside the EUV exposure tool, the reflective mask 2 may be exposed to hydrogen gas. Hydrogen gas is used for the purpose of reducing carbon contamination, for example. Therefore, the absorbing film 13 may be exposed to hydrogen gas.

[0080] O, B, C, or N contained in the Ir compound may react with hydrogen gas to generate a hydride (e.g., HO). When a hydride is generated, the hydride is highly volatile, and O, B, C, or N is desorbed from the Ir compound, resulting in a decrease in the thickness of the absorbing film 13. The change in the film thickness leads to a change in the phase difference.

[0081] Therefore, it is preferable that the Ir compound contains at least one element selected from Ta, Cr, Mo, W, Re, and Si. By adding these elements, hydrogen resistance can be improved. Among these elements, Ta, Cr, W, and Re can improve hydrogen resistance while suppressing deterioration of optical properties. Moreover, Mo and Si can further improve hydrogen resistance.

[0082] The method for forming the absorption film 13 is, for example, a DC sputtering method, a magnetron sputtering method, an ion beam sputtering method, or the like. The oxygen content of the absorption film 13 can be controlled by the content of O2 gas in the sputtering gas. Also, the nitrogen content of the absorption film 13 can be controlled by the content of N2 gas in the sputtering gas.

[0083] When forming an IrTaON film using a reactive sputtering method, an example of the film formation conditions is as follows. <Film Formation Conditions of IrTaON Film> Target: Ir target and Ta target (or IrTa target), Output density of Ir target: 1.0 W / cm 2 ~8.5 W / cm 2 , Output density of Ta target: 1.0 W / cm 2 ~8.5 W / cm 2 , Sputtering gas: Mixed gas of Ar gas, O2 gas, and N2 gas, Volume ratio of O2 gas in the sputtering gas (O2 / (Ar + O2 + N2)): 0.01~0.25, Volume ratio of N2 gas in the sputtering gas (N2 / (Ar + O2 + N2)): 0.01~0.25, Film formation rate: 0.020 nm / sec~0.060 nm / sec, Film thickness: 20 nm~60 nm.

Example

[0084] Hereinafter, the experimental data will be described. In Examples 1 to 6, a reflective mask blank 1 shown in FIG. 5(A) or FIG. 6(A) was prepared. The prepared reflective mask blank 1 had the same configuration except for the film type and film thickness of the hard mask film 14. In Examples 1 to 6, the processing of the hard mask film 14 (step S202) and the processing of the absorption film 13 (step S203) were performed in this order. Then, the cross-section was observed with an SEM (Scanning Electron Microscope), and the taper angle α was measured. Examples 1 to 3 are examples, and Examples 4 to 6 are comparative examples.

[0085] A SiO2-TiO2-based glass substrate (6-inch (152 mm) square outer dimensions, 6.3 mm thick) was prepared as the substrate 10. This glass substrate has a thermal expansion coefficient of 0.02×10 -7 / °C, Young's modulus is 67 GPa, Poisson's ratio is 0.17, and specific stiffness is 3.07 × 10 7 m 2 / s 2 The quality assurance area of ​​the first main surface 10a of the substrate 10 was polished to have a root-mean-square roughness (Rq) of 0.15 nm or less and a flatness of 100 nm or less. A Cr film having a thickness of 100 nm was formed on the second main surface 10b of the substrate 10 by magnetron sputtering. The sheet resistance of the Cr film was 100 Ω / □.

[0086] A Mo / Si multilayer reflective film was formed as the multilayer reflective film 11. The Mo / Si multilayer reflective film was formed by repeating the deposition of a Si layer (thickness 4.5 nm) and a Mo layer (thickness 2.3 nm) 40 times using an ion beam sputtering method. The total thickness of the Mo / Si multilayer reflective film was 272 nm ((4.5 nm + 2.3 nm) × 40).

[0087] A Rh film (thickness: 5 nm) was formed as the protective film 12. The Rh film was formed by using an ion beam sputtering method.

[0088] An Ir film (thickness: 35 nm) was formed as the absorbing film 13. The Ir film was formed by using a DC sputtering method.

[0089] The film type and film thickness of the hard mask film 14 were as shown in Table 2. In processing the hard mask film 14 (step S202), plasmatized Ar was used in Examples 1 to 3, and plasmatized mixed gas containing Cl2 gas and O2 gas (Cl2:O2=50:50 (volume ratio)) was used in Examples 4 to 6.

[0090] In Examples 1 to 6, a plasma-converted mixed gas containing CF4 gas and O2 gas was used in processing (step S203) of the absorbing film 13. The detailed processing conditions for the absorbing film 13 were as follows. <Absorbent film processing conditions> Etching gas: Plasma-mixed gas containing CF4 gas and O2 gas, CF4 gas flow rate: 48sccm, O2 gas flow rate: 12sccm, Source power: 720W, Bias: 80W, Pressure: 0.4Pa.

[0091] The experimental conditions and results of Examples 1 to 6 are shown in Table 2.

[0092] [Table 2] As shown in Table 2, in Examples 1 to 3, the hard mask film 14 contains at least one element X1 selected from Y, Al, Hf, and Pd, so the etching rate ER2 of the hard mask film 14 was slower and the selectivity (ER1 / ER2) with the absorbing film 13 was sufficiently large compared to Examples 4 to 6. As a result, the taper angle α could be increased.

[0093] The reflective mask blank, the manufacturing method of the reflective mask blank, and the manufacturing method of the reflective mask according to the present disclosure have been described above, but the present disclosure is not limited to the above-mentioned embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. These naturally fall within the technical scope of the present disclosure. [Explanation of symbols]

[0094] 1 Reflective mask blank 2 Reflective mask 10 Substrate 11 Multilayer reflective film 12 Protective film 13 Absorbing membrane 14 Hard mask film

Claims

1. A reflective mask blank having a substrate, a multilayer reflective film, a protective film, an absorbing film, and a hard mask film in this order, The hard mask film comprises at least one element X1 selected from Y, Al, Hf, and Pd.

2. The reflective mask blank according to claim 1 , wherein the hard mask film has a thickness of 10 nm or less.

3. The reflective mask blank according to claim 1 or 2, wherein the hard mask film contains a compound of the element X1, and the compound of the element X1 contains at least one element selected from the group consisting of O, N, B, H and C.

4. The reflective mask blank according to claim 1 , wherein the hard mask film contains a compound of the element X1, and the compound of the element X1 contains at least one element selected from the group consisting of Ru and Cr.

5. 3. The reflective mask blank according to claim 1, wherein the absorbing film contains at least one element selected from Ir, Pt, Pd, Co, Ni, Os, and Ru.

6. The reflective mask blank according to claim 1 , wherein the protective film contains at least one element selected from the group consisting of Ru, Rh and Si.

7. The reflective mask blank according to claim 1 , wherein the protective film contains Rh.

8. 3. The reflective mask blank according to claim 1, wherein the protective film is a multilayer film having a lower layer and an upper layer, and the upper layer contains Rh.

9. depositing a multilayer reflective film, a protective film, an absorbing film, and a hard mask film in this order on a substrate; The hard mask film contains at least one element X1 selected from Y, Al, Hf, and Pd.

10. Preparing a reflective mask blank according to claim 1 or 2; forming an opening pattern in the hard mask film; forming an opening pattern in the absorbing film; A method for manufacturing a reflective mask comprising the steps of:

11. The method for manufacturing a reflective mask according to claim 10, wherein forming an opening pattern in the hard mask film includes etching the hard mask film with Ar gas plasma.

Citation Information

Patent Citations

  • Reflective mask blank, reflective mask, and method for manufacturing semiconductor device

    WO2022138360A1