Kraft paper and packaging bag
By optimizing the freeness, fiber length, and polyacrylamide content in kraft paper, both tensile and tear strengths, as well as sizing properties, are significantly improved, addressing the shortcomings of existing heavy-duty packaging papers.
Patent Information
- Application Number
- JP2023072066
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-26
AI Technical Summary
Existing kraft paper for heavy-duty packaging lacks sufficient consideration for both specific tensile strength and tear strength, and the Steckigt sizing degree as an index of sizing has not been adequately addressed.
The kraft paper is formulated with wood pulp having a Canadian standard freeness of 500 mL or more, a polyacrylamide dry paper strength agent content between 0.05% to 0.75% by mass, and a weight average fiber length of 2.2 to 3.7 mm, with a high content of softwood kraft pulp, particularly from Douglas fir, to achieve enhanced tensile and tear strengths and sizing properties.
The kraft paper exhibits both specific tensile strength of 40.0 N m/g or more and specific tear strength of 10.0 mN m^2/g or more, along with a Steckigt sizing degree of 12 seconds or more, ensuring durability and printability.
Smart Images

Figure 2024157622000001 
Figure 2024157622000002
Abstract
Description
[Technical field]
[0001] The present invention relates to kraft paper and a packaging bag using the same. [Background technology]
[0002] Kraft paper is primarily used for large bags for carrying heavy industrial loads such as cement, fertilizer, and pesticides, as well as for packaging bags for salt, rice, wheat, and agricultural products. When manufacturing large bags for putting heavy objects in, the paper must be strong enough to withstand the impacts that may be applied during transportation, and must also be resistant to tearing when wet during use.
[0003] For example, Patent Document 1 discloses a heavy-duty packaging kraft paper characterized in that a paper support having a disintegration freeness of 600 to 680 mL is formed using kraft pulp with a weight-average fiber length of 2.3 to 4.0 mm, with the aim of reducing production costs and achieving high breathability without reducing the strength of the kraft paper. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2006-89889 A Summary of the Invention [Problem to be solved by the invention]
[0005] The heavy-duty packaging kraft paper described in Reference 1 has not been sufficiently examined to achieve both specific tensile strength and specific tear strength. Furthermore, the Stockigt sizing degree as an index of sizing property has not been sufficiently examined.
[0006] An object of the present invention is to provide a kraft paper that satisfies both specific tensile strength and specific tear strength and also has excellent sizing properties, and a packaging bag using the same. [Means for solving the problem]
[0007] The present inventors have found that the above-mentioned problems can be solved by setting the Canadian standard freeness of disintegrated pulp obtained by redisintegrating kraft paper and the content of polyacrylamide-based dry strength agent in the kraft paper to specific ranges. That is, the present invention provides the following: <1> ~ <12> Regarding. <1> A kraft paper whose main component is wood pulp, wherein the Canadian standard freeness of the disintegrated pulp obtained by redisintegrating the kraft paper is 500 mL or more, and the content of a polyacrylamide-based dry strength agent in the kraft paper is 0.05% by mass or more and 0.75% by mass or less. <2> The weight average fiber length of the pulp constituting the kraft paper is 2.2 mm or more and 3.7 mm or less. <1> 2. Kraft paper according to claim 1. <3> The wood pulp comprises softwood kraft pulp; <1> or <2> 2. Kraft paper according to claim 1. <4> The content of softwood kraft pulp in the wood pulp is 90% by mass or more. <3> 2. Kraft paper according to claim 1. <5> The raw materials for softwood kraft pulp include Douglas fir, <3> or <4> 2. Kraft paper according to claim 1. <6> The specific tensile strength is 40.0 N·m / g or more. <1> ~ <5> 2. The kraft paper according to claim 1 . <7> Specific tear strength is 10.0mN·m 2 / g or more, <1> ~ <6> 2. The kraft paper according to claim 1 . <8> Basis weight 30g / m 2 More than 200g / m 2 Below is the <1> ~ <7> 2. The kraft paper according to claim 1 . <9> The Stöckigt size is 12 seconds or more. <1> ~ <8> 2. The kraft paper according to claim 1 . <10> The elongation at break is 3.1% or more. <1> ~ <9> 2. The kraft paper according to claim 1 . <11> Kraft paper for heavy-duty bags. <1> ~ <10> 2. The kraft paper according to claim 1 . <12> <1> ~ <11> A packaging bag made using the kraft paper described in any one of the above. Effect of the Invention
[0008] According to the present invention, it is possible to provide kraft paper having both specific tensile strength and specific tear strength, and a packaging bag using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Kraft paper] The kraft paper of this embodiment is a kraft paper whose main component is wood pulp, and the Canadian standard freeness of the disintegrated pulp obtained by redisintegrating the kraft paper is 500 mL or more, and the content of a polyacrylamide-based dry strength agent in the kraft paper is 0.05 mass% or more and 0.75 mass% or less. The kraft paper of this embodiment can achieve both specific tensile strength and specific tear strength. Furthermore, the kraft paper of this embodiment can achieve both specific tensile strength and specific tear strength, and is also excellent in sizing. The mechanism by which this effect is achieved is unknown, but is presumed to be as follows. The kraft paper of this embodiment is mainly composed of wood pulp, and therefore can be formed from pulp with relatively long fiber length, making it possible to provide excellent specific tear strength. On the other hand, the more the pulp is beaten (i.e. the lower the Canadian Standard Freeness of the pulp that makes up the kraft paper), the lower the tear strength index. This is thought to be because when beating is accelerated, the fibers are fibrillated, and the tensile strength index improves due to the increased interfiber bond area, which increases the elastic modulus and makes the sheet harder, making the tear strength index more likely to decrease. It is also presumed that one of the reasons why the tear strength index is likely to decrease is that the fibers become shorter as a result of accelerated beating. The kraft paper of this embodiment uses moderately beaten pulp, and the Canadian standard freeness of the disintegrated pulp obtained by re-disintegration is 500 mL or more, which suppresses the decrease in specific tear strength due to the above phenomenon and makes it possible to achieve excellent specific tear strength. Furthermore, by having the content of the polyacrylamide-based dry strength agent in the kraft paper of this embodiment be 0.05% by mass or more, the strength of the bond points between the fibers is improved, thereby improving the tensile strength ratio and further improving the Stockigt sizing degree. On the other hand, by having the content of the polyacrylamide-based dry strength agent be 0.75% by mass or less, excessive aggregation of the pulp fibers can be prevented, and a significant decrease in tear strength can be suppressed. As described above, it is believed that the kraft paper of the present embodiment can achieve both specific tensile strength and specific tear strength, and further has excellent sizing properties. However, the scope of the present invention is not limited by the above mechanism.
[0010] <Pulp that makes up kraft paper> (Wood pulp) In this embodiment, the kraft paper is mainly composed of wood pulp. "The kraft paper is mainly composed of wood pulp" means that the content of wood pulp in the kraft paper is more than 50% by mass, and the content of wood pulp is preferably 80% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more. In this embodiment, the kraft paper may contain non-wood pulp as the pulp, but from the viewpoint of improving the specific tensile strength and specific tear strength, the content of wood pulp in the total pulp constituting the kraft paper is preferably more than 50 mass%, more preferably 80 mass% or more, even more preferably 90 mass% or more, and even more preferably 95 mass% or more, with the upper limit being 100 mass%. The wood pulp is not particularly limited, and known wood pulp can be used.Specific examples include chemical pulps such as hardwood kraft pulp (LKP) and softwood kraft pulp (NKP); mechanical pulps such as groundwood pulp (GP), pressurized groundwood pulp (PGW), refiner mechanical pulp (RMP), thermomechanical pulp (TMP), chemi-thermomechanical pulp (CTMP), chemi-mechanical pulp (CMP), and chemi-ground pulp (CGP).Hardwood kraft pulp (LKP) includes hardwood unbleached kraft pulp (LUKP) and hardwood bleached kraft pulp (LBKP).Softwood kraft pulp (NKP) includes softwood unbleached kraft pulp (NUKP) and softwood bleached kraft pulp (NBKP). Examples of non-wood pulp include waste paper pulp, non-wood fiber pulp such as kenaf, bagasse, bamboo, cotton, etc., synthetic pulp, etc. These pulps may be used alone or in combination of two or more. Among these, from the viewpoint of improving the specific tensile strength and specific tear strength of the resulting kraft paper, softwood kraft pulp (NKP) is preferred, at least one selected from the group consisting of softwood unbleached kraft pulp (NUKP) and softwood bleached kraft pulp (NBKP) is more preferred, and softwood unbleached kraft pulp (NUKP) is even more preferred.
[0011] When the wood pulp contains softwood kraft pulp (NKP) (preferably softwood unbleached kraft pulp (NUKP)), the content of softwood kraft pulp (NKP) (preferably softwood unbleached kraft pulp (NUKP)) in the wood pulp is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 100% by mass or more. Softwood kraft pulp (NKP) has a long average fiber length, so that a content of softwood kraft pulp (NKP) of 90% by mass or more in the wood pulp, which is the main component of the pulp constituting the kraft paper, is preferable because it allows the kraft paper to have a desired specific tensile strength and specific tear strength. Furthermore, when softwood kraft pulp (NKP) is used as the pulp constituting the kraft paper, the strength of the pulp fiber itself is higher than that of hardwood kraft pulp (LKP), so that the specific tensile strength and specific tear strength of the obtained kraft paper can be more easily improved.
[0012] From the viewpoint of improving the specific tensile strength and / or specific tear strength of the resulting kraft paper, the raw material for softwood kraft pulp (NKP) preferably contains one or more species selected from the group consisting of Caribbean pine, radiata pine, cedar, and larch, and more preferably contains Douglas fir.
[0013] (Freeness) The freeness (Canadian standard freeness) of the pulp constituting the kraft paper may be adjusted so that the freeness of the kraft paper after redisintegration, which will be described later, is 500 mL or more. The freeness of the pulp constituting the kraft paper is preferably 500 mL or more, more preferably 520 mL or more, from the viewpoint of the specific tear strength of the resulting kraft paper, and is preferably 760 mL or less, more preferably 700 mL or less, even more preferably 650 mL or less, and even more preferably 630 mL or less, from the viewpoint of the specific tensile strength and / or breaking elongation. The freeness of the pulp constituting the kraft paper is determined by a method conforming to JIS P 8121:1995. The freeness of the pulp constituting the kraft paper can be adjusted to fall within the above range by appropriately adjusting the beating treatment conditions.
[0014] (Average fiber length) The average fiber length of the pulp constituting the kraft paper is preferably 1.0 mm or more, more preferably 1.3 mm or more, and even more preferably 1.5 mm or more, from the viewpoint of achieving both the specific tensile strength and specific tear strength of the resulting kraft paper. The upper limit is not particularly limited, but from the viewpoint of the texture of the kraft paper, it is preferably 3.0 mm or less, more preferably 2.8 mm or less, and even more preferably 2.5 mm or less. The average fiber length of the pulp that makes up the kraft paper is measured in accordance with ISO 16065-2 (2007).
[0015] (weight average fiber length) The weight average fiber length of the pulp constituting the kraft paper is preferably 2.2 mm or more, more preferably 2.4 mm or more, even more preferably 2.5 mm or more, still more preferably 2.8 mm or more, and even more preferably 2.9 mm or more, from the viewpoint of achieving both the specific tensile strength and specific tear strength of the resulting kraft paper and also the Stockigt sizing degree. The upper limit is not particularly limited, but from the viewpoint of the texture of the kraft paper, it is preferably 3.7 mm or less, more preferably 3.5 mm or less, even more preferably 3.3 mm or less, and even more preferably 3.1 mm or less. The weight average fiber length of wood pulp is specifically measured in accordance with ISO 16065-2 (2007).
[0016] (average fiber width) From the viewpoint of improving the specific tensile strength and / or specific tear strength of the resulting kraft paper, the average fiber width of the pulp constituting the kraft paper is preferably 20 μm or more, more preferably 25 μm or more, even more preferably 30 μm or more, and is preferably 45 μm or less, more preferably 40 μm or less, even more preferably 35 μm or less. The average fiber width of wood pulp is specifically measured according to ISO 16065-2 (2007).
[0017] (Fine fiber content) The fine fiber content in the pulp constituting the kraft paper is preferably 18% or less, more preferably 15% or less, and even more preferably 12% or less, from the viewpoint of improving the specific tensile strength, specific tear strength and / or sizing property of the resulting kraft paper. The lower limit is not particularly limited, but is preferably 1% or more, more preferably 3% or more, and even more preferably 5% or more, from the viewpoint of productivity. In this embodiment, the fine fibers refer to fine fibers with a fiber length of 0.1 mm or less among the pulp constituting the kraft paper. The fine fiber content in the pulp constituting the kraft paper refers to the ratio (%) of the number of fine fibers to the total number of pulps constituting the kraft paper. The fines content in wood pulp is specifically measured in accordance with ISO 16065-2 (2007).
[0018] <Polyacrylamide-based dry strength agent> The craft paper of this embodiment contains 0.05% by mass or more and 0.75% by mass or less of a polyacrylamide-based dry strength agent. By making the content of the polyacrylamide-based dry strength agent in the kraft paper 0.05% by mass or more, the tensile strength index can be improved and the Stockigt sizing degree can be improved. On the other hand, by making the content of the polyacrylamide-based dry strength agent 0.75% by mass or less, the aggregation of pulp fibers can be prevented and the decrease in the tear strength index can be suppressed. The content of the polyacrylamide-based dry strength agent in the kraft paper is, from the viewpoint of improving the specific tensile strength, specific tear strength and / or sizing property of the resulting kraft paper, preferably 0.03% by mass or more, more preferably 0.10% by mass or more, even more preferably 0.20% by mass or more, and still more preferably 0.30% by mass or more, and from the viewpoint of improving the breaking elongation, is preferably 0.70% by mass or less, more preferably 0.60% by mass or less, even more preferably 0.50% by mass or less, still more preferably 0.40% by mass or less, and still more preferably 0.30% by mass or less. In this embodiment, in order to make the polyacrylamide-based dry strength agent in the kraft paper fall within the above range, the polyacrylamide-based dry strength agent may be added to the stock for producing the kraft paper when producing the kraft paper. In general, the content of the polyacrylamide-based dry strength agent in the kraft paper tends to be lower than the amount of the polyacrylamide-based dry strength agent added to the stock. Therefore, the amount of the polyacrylamide-based dry strength agent added to the stock may be appropriately adjusted taking this into consideration. The amount of the polyacrylamide-based dry strength agent added to the stock is 0.10 parts by mass or more and 0.78 parts by mass or less per 100 parts by mass of raw pulp in the stock.
[0019] The polyacrylamide-based dry strength agent is preferably one or more selected from the group consisting of anionic polyacrylamide, cationic polyacrylamide, and amphoteric polyacrylamide. These polyacrylamide-based dry strength agents can be used alone or in combination of two or more.
[0020] (anionic polyacrylamide) Examples of anionic polyacrylamides include water-soluble copolymers containing (meth)acrylamide and anionic monomers as constituent components, hydrolyzed polyacrylamides, etc. These anionic polyacrylamides can be used alone or in combination of two or more. In this specification, (meth)acrylamide refers to acrylamide and / or methacrylamide.
[0021] Examples of anionic monomers that can be used as components of the water-soluble copolymer include anionic vinyl monomers such as unsaturated monocarboxylic acids, unsaturated dicarboxylic acids, unsaturated tricarboxylic acids, unsaturated tetracarboxylic acids, unsaturated sulfonic acids, unsaturated phosphonic acids, and salts thereof. These anionic monomers can be used alone or in combination of two or more. In particular, monomers of acrylic acid and its salts are preferably used. In the polymerization of anionic water-soluble copolymers, auxiliary agents such as chain transfer agents generally used in polymerization may be added.
[0022] Hydrolyzed polyacrylamide is a decomposition product obtained by decomposing polyacrylamide by a conventionally known hydrolysis reaction. Hydrolyzed polyacrylamide can be obtained, for example, by causing an alkaline substance such as sodium hydroxide to act on a (meth)acrylamide copolymer and / or homopolymer to cause partial hydrolysis and convert the amide group into a carboxy group.
[0023] (cationic polyacrylamide) Examples of cationic polyacrylamides include water-soluble copolymers composed of (meth)acrylamide and cationic monomers, Mannich-modified polyacrylamides, and Hoffman-decomposed polyacrylamides. These cationic polyacrylamides can be used alone or in combination of two or more.
[0024] Examples of cationic monomers that can be used as components of the water-soluble copolymer include cationic vinyl monomers such as vinyl monomers having a tertiary amino group or quaternary ammonium salts. These cationic monomers can be used alone or in combination of two or more. In the polymerization of the cationic water-soluble copolymer, an auxiliary agent such as a chain transfer agent that is generally used in polymerization may be added.
[0025] Mannich-modified polyacrylamide is a reaction product obtained by modifying polyacrylamide by the conventionally known Mannich reaction. Mannich-modified polyacrylamide can be obtained, for example, by reacting a (meth)acrylamide copolymer and / or homopolymer with formaldehyde and a secondary amine to cationize some of the amide groups. Either an aqueous solution (formalin) or paraformaldehyde may be used as formaldehyde. Examples of secondary amines include dimethylamine, diethylamine, dipropylamine, dibutylamine, diethanolamine, and dipropanolamine. These secondary amines may be used alone or in combination of two or more.
[0026] Hoffman decomposition polyacrylamide is a decomposition product obtained by decomposing polyacrylamide by the conventionally known Hoffman reaction. Hoffman decomposition polyacrylamide can be obtained, for example, by reacting a hypohalite such as hypochlorite (NaOCl) with a (meth)acrylamide copolymer and / or homopolymer in the presence of an alkaline substance such as sodium hydroxide (NaOH) to convert amide groups (-C=ONH-) to amino groups (-NH2).
[0027] (Amphoteric polyacrylamide) Examples of amphoteric polyacrylamides include water-soluble copolymers composed of (meth)acrylamide, anionic monomers, and cationic monomers. These amphoteric polyacrylamides can be used alone or in combination of two or more.
[0028] Examples of the anionic monomer and cationic monomer used as the constituents of the amphoteric water-soluble copolymer include those exemplified as the constituents of the anionic polyacrylamide and cationic polyacrylamide described above. In polymerizing the amphoteric water-soluble copolymer, an auxiliary agent such as a chain transfer agent generally used in polymerization may be added.
[0029] In this embodiment, from the viewpoint of improving the specific tensile strength and sizing property of the resulting kraft paper, the polyacrylamide-based dry strength agent is preferably an amphoteric polyacrylamide, and more preferably a water-soluble copolymer having as its constituent components (meth)acrylamide, an anionic monomer, and a cationic monomer.
[0030] <Optional ingredients> The kraft paper may contain optional components as necessary, such as anionic, cationic or amphoteric retention agents, drainage improvers, wet strength agents, sizing agents, fixing agents, internal additives such as fillers, water-resistant agents, dyes, and fluorescent whitening agents.
[0031] Examples of the wet strength agent include polyamide polyamine epichlorohydrin, urea formaldehyde resin, melamine formaldehyde resin, etc. The content of the wet strength agent in the kraft paper is not particularly limited, but is preferably 3.0% by mass or less.
[0032] Examples of the sizing agent include internal sizing agents such as rosin sizing agents, synthetic sizing agents, and petroleum resin-based sizing agents, and surface sizing agents such as styrene / acrylic acid copolymers and styrene / methacrylic acid copolymers. The content of the sizing agent in the kraft paper is not particularly limited, but is preferably 3.0% by mass or less.
[0033] Examples of the fixing agent include aluminum sulfate, polyethyleneimine, etc. The content of the fixing agent in the kraft paper is not particularly limited, but is preferably 3.0% by mass or less.
[0034] Examples of the filler include inorganic fillers such as talc, kaolin, calcined kaolin, calcium carbonate, calcium sulfate, barium sulfate, titanium dioxide, zinc oxide, alumina, magnesium carbonate, magnesium oxide, silica, white carbon, bentonite, zeolite, sericite, and smectite, and organic fillers such as acrylic resins and vinylidene chloride resins.
[0035] <Physical properties of kraft paper> (Basic weight) The basis weight of the kraft paper is not particularly limited, but in the case of packaging bags, it is preferably 30 g / m 2 More preferably, 40 g / m 2 More preferably, 50 g / m 2 and preferably 200 g / m 2 Less than 150 g / m 2 More preferably, 100 g / m 2 More preferably, 80 g / m or less 2 The basis weight of kraft paper is measured in accordance with JIS P 8124:2011.
[0036] (Thickness) The thickness of the kraft paper is not particularly limited, but in the case of packaging bag applications, it is preferably 60 μm or more, more preferably 80 μm or more, even more preferably 100 μm or more, and preferably 200 μm or less, more preferably 180 μm or less, even more preferably 160 μm or less. The thickness of the kraft paper is measured in accordance with JIS P 8118:2014.
[0037] (density) The density of the kraft paper is not particularly limited, but in the case of packaging bags, it is preferably 0.3 g / cm 3 More preferably, 0.4 g / cm 3 and preferably 1.0 g / cm 3 Less than or equal to 0.8 g / cm 3 Less than 0.7 g / cm, more preferably 0.7 g / cm 3 More preferably, 0.6 g / cm 3 The density of the kraft paper is calculated from the basis weight and thickness of the kraft paper obtained by the above-mentioned measurement method.
[0038] (Specific tensile strength) From the viewpoint of improving the strength when used as a packaging bag, the specific tensile strength of the kraft paper is preferably 40.0 N·m / g or more, more preferably 45.0 N·m / g or more, even more preferably 50.0 N·m / g or more, and even more preferably 52.0 N·m / g or more. There is no particular upper limit to the specific tensile strength, but it is preferably 100 N·m / g or less, and more preferably 90.0 N·m / g or less. Specific tensile strength (N·m / g) is the tensile strength (N / m) measured in accordance with JIS P 8113:2006, multiplied by the basis weight (g / m 2 ) is the value divided by In addition, if the kraft paper is oriented, the specific tensile strength (N m / g) is calculated by measuring the tensile strength in the machine direction and the tensile strength in the cross direction in accordance with JIS P 8113:2006, calculating the geometric mean of the tensile strength in the machine direction and the tensile strength in the cross direction, and then dividing this by the basis weight. In this specification, the term "machine direction" refers to a direction parallel to the papermaking direction, and the term "transverse direction" refers to a direction perpendicular to the papermaking direction. The specific tensile strength of kraft paper can be adjusted by the content of the polyacrylamide-based dry strength agent in the kraft paper (i.e., the amount of polyacrylamide-based dry strength agent added to the paper material), etc. When the content of the polyacrylamide-based dry strength agent in the kraft paper is increased, the specific tensile strength of the kraft paper tends to increase.
[0039] (Specific tear strength) The tear strength of the kraft paper is preferably 10.0 mN m from the viewpoint of improving the strength when used as a packaging bag. 2 / g or more, preferably 11.0 mN m 2 / g or more, and more preferably 12.0 mN m 2 The upper limit of the specific tear strength is not particularly limited, but is preferably 40.0 mN·m 2 / g or less, more preferably 30.0 mN m 2 / g or less. Specific tear strength (mN m 2 / g) is the tear strength (mN) measured in accordance with JIS P 8116:2000, multiplied by the basis weight (g / m 2 ) is the value divided by In addition, when the kraft paper is oriented, the specific tear strength (mN m 2 The tear strength in the machine direction and the tear strength in the cross direction are measured in accordance with JIS P 8116:2000, the geometric mean of the tear strength in the machine direction and the tear strength in the cross direction are calculated, and the geometric mean is divided by the basis weight. The tear strength index of kraft paper can be adjusted by the content of polyacrylamide-based dry strength agent in the kraft paper (i.e., the amount of polyacrylamide-based dry strength agent added to the paper stock), the post-redisintegration freeness of the kraft paper (i.e., the freeness of the pulp that constitutes the kraft paper), etc. If the content of polyacrylamide-based dry strength agent in the kraft paper is reduced, the tear strength index of the kraft paper tends to increase. If the post-redisintegration freeness of the kraft paper is increased, the tear strength index of the kraft paper tends to increase.
[0040] (Stockigt size) The Stockigt sizing degree of the kraft paper is preferably 12 seconds or more, more preferably 14 seconds or more, even more preferably 15 seconds or more, still more preferably 17 seconds or more, and even more preferably 18 seconds or more, from the viewpoints of improving sizing properties, suppressing ink bleeding during printing and improving printability, and improving strength when wetted with water. The upper limit of the Stockigt sizing degree is not particularly limited, but is preferably 40 seconds or less, more preferably 30 seconds or less. The Stockigt sizing degree is measured in accordance with JIS P 8122:2004. The Stoeckigt sizing degree of kraft paper can be adjusted by the content of the polyacrylamide-based dry strength agent in the kraft paper (i.e., the amount of the polyacrylamide-based dry strength agent added to the paper stock), the post-redisintegration freeness of the kraft paper (i.e., the freeness of the pulp that constitutes the kraft paper), etc. When the content of the polyacrylamide-based dry strength agent in the kraft paper is increased, the Stoeckigt sizing degree of the kraft paper tends to increase. When the post-redisintegration freeness of the kraft paper is decreased, the Stoeckigt sizing degree of the kraft paper tends to increase.
[0041] (Elongation at break) From the viewpoint of improving the strength when used as a packaging bag, the breaking elongation of the kraft paper is preferably 3.1% or more, more preferably 3.5% or more, even more preferably 3.8% or more, and even more preferably 4.0% or more. The upper limit of the breaking elongation is not particularly limited, but from the viewpoint of manufacturability, it is preferably 20% or less, more preferably 10% or less. The breaking elongation is measured in accordance with JIS P 8113:2006. In addition, when the kraft paper is oriented kraft paper, the breaking elongation is the geometric mean of the breaking elongation in the longitudinal direction and the breaking elongation in the transverse direction measured in accordance with JIS P 8113:2006. The breaking elongation of kraft paper can be adjusted by the content of polyacrylamide-based dry strength agent in the kraft paper (i.e., the amount of polyacrylamide-based dry strength agent added to the paper stock), the post-redisintegration freeness of the kraft paper (i.e., the freeness of the pulp that constitutes the kraft paper), etc. Increasing the content of polyacrylamide-based dry strength agent in the kraft paper tends to increase the breaking elongation of the kraft paper. Decreasing the post-redisintegration freeness of the kraft paper tends to increase the breaking elongation of the kraft paper.
[0042] (Canadian Standard Freeness of Disintegrated Pulp Obtained by Disintegrating Kraft Paper (Freeness after Disintegration)) In the kraft paper of this embodiment, the Canadian standard freeness of the disintegrated pulp obtained by redisintegrating the kraft paper (freeness of the kraft paper after redisintegration) is 500 mL or more. When the disintegrated pulp obtained by redisintegrating kraft paper has a Canadian standard freeness of 500 mL or more, the decrease in specific tear strength can be suppressed and the specific tear strength can be made excellent, as described above. The Canadian standard freeness of the disintegrated pulp obtained by redisintegrating the kraft paper is preferably 520 mL or more, more preferably 540 mL or more, from the viewpoint of the tear strength index of the resulting kraft paper, and is preferably 800 mL or less, more preferably 780 mL or less, even more preferably 760 mL or less, still more preferably 700 mL or less, and even more preferably 650 mL or less, from the viewpoint of the tensile strength index and / or breaking elongation. The Canadian standard freeness of disintegrated pulp obtained by redefibrating kraft paper is determined by disintegrating the kraft paper in a manner conforming to JIS P 8220-1:2012, and then using the resulting disintegrated pulp in a manner conforming to JIS P 8121:1995. The freeness of the kraft paper after redisintegration can be adjusted within the above range depending on the freeness of the pulp constituting the kraft paper.
[0043] [Kraft paper manufacturing method] In the present embodiment, the method for producing the kraft paper is not particularly limited. For example, the method may include a cooking process for cooking the pulp constituting the kraft paper (hereinafter also referred to as "raw material pulp"), a beating process for beating a dispersion containing the cooked raw material pulp, and a papermaking process for making the beaten raw material pulp. Each step of the method is described below.
[0044] (Cooking process) The cooking process is a process for cooking raw pulp. In this process, although not particularly limited, it is preferable to treat raw chips used as a material for the raw pulp with a chemical solution containing sodium hydroxide, and as a method for treating with a chemical solution containing sodium hydroxide, a known treatment method using a known chemical solution can be used.
[0045] The raw chips used as the material for the raw pulp are preferably mainly composed of softwood pulp. "Raw chips mainly composed of softwood pulp" refers to raw chips in which the softwood chip content is more than 50% by mass, and the softwood chip content is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and even more preferably 100% by mass.
[0046] The raw material pulp may be unbleached or may be bleached. The raw material pulp is preferably one or more selected from the group consisting of bleached kraft pulp and unbleached kraft pulp, and more preferably unbleached kraft pulp.
[0047] (beating process) The beating step is a step of beating a dispersion containing the digested raw pulp. In the beating step of this embodiment, the beating is performed so that the Canadian standard freeness of the disintegrated pulp obtained by re-disintegrating the obtained kraft paper is in the range of 500 mL or more. By performing the beating treatment so that the Canadian standard freeness of the disintegrated pulp obtained by re-disintegrating the kraft paper is in the above range, the decrease in the specific tear strength can be suppressed and the specific tear strength can be excellent as described above. In the beating step, the raw pulp concentration of the dispersion is not particularly limited, but is preferably 1 mass% or more, and preferably 35 mass% or less, more preferably 15 mass% or less. The method of the beating treatment is not particularly limited, but it is preferable to disperse the digested raw pulp in water to prepare a dispersion having the above raw pulp concentration, and beat it. The method of the beating treatment is not particularly limited, but can be performed using a beater such as a double disc refiner, a single disc refiner, a conical refiner, or a deluxe refiner.
[0048] By beating a dispersion containing the digested raw pulp, kraft paper having excellent specific tensile strength, specific tear strength and sizing properties can be obtained, and productivity is also excellent.
[0049] (Paper making process) The papermaking process is a process of making paper from beaten raw pulp. In the papermaking process of this embodiment, a polyacrylamide-based dry strength agent is added so that the content of the polyacrylamide-based dry strength agent in the obtained kraft paper is 0.05% by mass or more and 0.75% by mass or less. In order to make the content of the polyacrylamide-based dry strength agent in the obtained kraft paper within the above range, it is preferable that the amount of the polyacrylamide-based dry strength agent added in the papermaking process is 0.10 parts by mass or more and 0.78 parts by mass or less per 100 parts by mass of raw pulp. By making paper so that the content of the polyacrylamide-based dry strength agent in the kraft paper is within the above range, both the specific tensile strength and specific tear strength can be improved, and the Stockigt sizing degree can be improved, thereby improving sizing properties. The papermaking method is not particularly limited, and examples thereof include an acidic papermaking method in which papermaking is performed at a pH of about 4.5, and a neutral papermaking method in which papermaking is performed at a pH of about 6 to about 9. In the papermaking process, papermaking process chemicals such as pH adjusters, antifoamers, pitch control agents, slime control agents, etc. can be added as necessary. The papermaking machine is also not particularly limited, and examples thereof include continuous papermaking machines such as Fourdrinier, cylinder, and tilt types, or multi-layer papermaking machines that combine these.
[0050] <Application> As described above, the kraft paper of the present embodiment has excellent specific tensile strength, specific tear strength, and sizing properties, and therefore can be suitably used as kraft paper for packaging bags (particularly for heavy-duty packaging bags). In particular, it can be suitably used as kraft paper for heavy-duty packaging bags for industrial use, such as cement, fertilizer, and pesticides.
[0051] The packaging body of this embodiment is a packaging body made of the above-mentioned craft paper. Since the above-mentioned kraft paper has excellent specific tensile strength, specific tear strength and sizing properties, the packaging body of this embodiment can be particularly suitably used as a packaging bag for carrying heavy industrial goods such as cement, fertilizer, and pesticides. EXAMPLES
[0052] Examples are given below to specifically explain the present invention, but the present invention is not limited to these examples. Unless otherwise specified, the following operations were performed under conditions of 23°C and a relative humidity of 50%RH. Furthermore, in the examples and comparative examples, "parts" and "%" respectively refer to "parts by mass" and "% by mass" unless otherwise specified.
[0053] [Kraft paper manufacturing] <Example 1> Kraft cooking was carried out using softwood chips including Douglas fir. After kraft cooking, the black liquor was separated, and the resulting chips were disintegrated using a disintegrator. The chips were then centrifuged and washed three times using a filter cloth, and the undigested material was removed using a screen. The chips were then centrifuged to obtain unbleached softwood kraft pulp (NUKP). The resulting NUKP was beaten using a refiner. The properties of the pulp obtained after beating are shown in Tables 1 and 2. To the NUKP slurry obtained after beating, 0.04 parts of rosin as a sizing agent, 1.2 parts of aluminum sulfate as a fixing agent, and 0.75 parts of amphoteric polyacrylamide (OKS-20 manufactured by Arakawa Chemical Industries Co., Ltd.) as a paper strength agent were added with stirring per 100 parts of NUKP content (dry mass) to prepare paper stock. Using the above paper material, a hand-made sheet was produced according to a method conforming to JIS P 8222:2015, with a basis weight of 62.2 g / m 2 Kraft paper was obtained.
[0054] <Example 2> A hand-made sheet was prepared in the same manner as in Example 1, except that the amount of amphoteric polyacrylamide added in the paper stock was changed to 0.60 parts, and the basis weight was 60.5 g / m. 2 Kraft paper was obtained.
[0055] <Example 3> A hand-made sheet was prepared in the same manner as in Example 1, except that the degree of beating of the pulp was increased and the amount of amphoteric polyacrylamide added to the paper stock was changed to 0.60 parts. The basis weight was 65.6 g / m. 2 Kraft paper was obtained.
[0056] <Example 4> A hand-made sheet was prepared in the same manner as in Example 1, except that the degree of beating of the pulp was increased and the amount of amphoteric polyacrylamide added to the paper stock was changed to 0.30 parts. The basis weight was 62.5 g / m. 2 Kraft paper was obtained.
[0057] <Example 5> A hand-made sheet was prepared in the same manner as in Example 4, except that the amount of amphoteric polyacrylamide added in the paper stock was changed to 0.10 parts, and the basis weight was 63.5 g / m. 2 Kraft paper was obtained.
[0058] <Comparative Example 1> A hand-made sheet was prepared in the same manner as in Example 1, except that no amphoteric polyacrylamide was added to the paper stock, and the basis weight was 62.5 g / m. 2 Kraft paper was obtained.
[0059] <Comparative Example 2> A hand-made sheet was prepared in the same manner as in Example 4, except that the amount of amphoteric polyacrylamide added in the paper stock was changed to 1.00 part, and the basis weight was 63.6 g / m. 2 Kraft paper was obtained.
[0060] <Comparative Example 3> A hand-made sheet was prepared in the same manner as in Example 1, except that the degree of beating of the pulp was increased and the amount of amphoteric polyacrylamide added to the paper stock was changed to 0.30 parts. The basis weight was 64.5 g / m. 2 Kraft paper was obtained.
[0061] <Comparative Example 4> A hand-made sheet was prepared in the same manner as in Comparative Example 3, except that no amphoteric polyacrylamide was added to the paper stock, and the basis weight was 64.4 g / m. 2 Kraft paper was obtained.
[0062] <Example 6> Using the paper stock prepared in the same manner as in Example 1, kraft paper was produced on a Fourdrinier papermaking machine at a papermaking speed of 700 m / min.
[0063] [Measurement method] <Measurement of pulp properties> (Freeness) The Canadian standard freeness of the pulp in the pulp slurry obtained after beating was measured by a method in accordance with JIS P 8121:1995.
[0064] (length average fiber length, weight average fiber length, average fiber width and fines content) The average fiber length, weight average fiber length, average fiber width, and fine fiber content of the pulp in the pulp slurry obtained after beating were measured using a fiber length measuring instrument (model name: FS-5 (with UHD base unit), manufactured by Valmet) in accordance with ISO 16065-2 (2007).
[0065] <Measurement of Kraft Paper Properties> (Specific tensile strength) For the kraft papers obtained in the examples and comparative examples, the tensile strength was measured by a method in accordance with JIS P 8113:2006, and the specific tensile strength was calculated by dividing the obtained tensile strength (for Example 6, the geometric average of the tensile strength in the longitudinal direction and the tensile strength in the transverse direction) by the basis weight.
[0066] (Specific tear strength) For the kraft papers obtained in the examples and comparative examples, the tear strength was measured according to a method in accordance with JIS P 8116:2000, and the specific tear strength was calculated by dividing the obtained tear strength (for Example 6, the geometric mean of the tear strength in the longitudinal direction and the tear strength in the transverse direction) by the basis weight.
[0067] (Stockigt size) The Stockigt sizing degree of the kraft papers obtained in the examples and comparative examples was measured by a method in accordance with JIS P 8122:2004.
[0068] (Elongation at break) In accordance with JIS P 8113:2006, the kraft paper obtained in the Examples and Comparative Examples was left to stand for one day or more in an environment of 23±5°C and 50±10% humidity to adjust the temperature and humidity, and then cut into samples with a width of 15 mm and a length of 150 mm. The sample was attached to a tensile testing machine (model RTC-1210A, manufactured by A&D Co., Ltd.) with a chuck distance of 100 mm, and a tensile test was performed at a speed of 10 mm / min to measure the breaking elongation.
[0069] (Re-disintegrated freeness (Canadian standard freeness of disintegrated pulp obtained by re-disintegrating kraft paper)) The kraft papers of the Examples and Comparative Examples were disintegrated by a method in accordance with JIS P 8220-1:2012, and the Canadian standard freeness of the resulting disintegrated pulp was measured by a method in accordance with JIS P 8121:1995.
[0070] (Measurement of residual dry strength agent amount (method for measuring polyacrylamide compound content)) The content (solid content equivalent) of polyacrylamide-based compounds contained in the kraft paper of the Examples and Comparative Examples was measured under the following conditions using a pyrolysis GC / MS analyzer, and quantified using a calibration curve from the results of the detected ion m / z 125 (3-Ethylidene-2,5-pyrrolidinedione). [Measurement sample] About 100 to 150 μg of the craft paper of each of the examples and comparative examples was precisely weighed out and used as a measurement sample. [Measurement conditions] GC: Column HP-INNOWAX (length 30 m, inner diameter 0.25 μm, outer diameter 0.25 mm) Carrier gas: He MS: EI(+) Conditions: 50℃→(10℃ / min)→260℃held for 15 minutes Pyrolysis equipment: Frontier Lab PY-3030D, decomposition temperature 500℃ Analysis: Calculate the content of polyacrylamide compounds using the selected ion m / z 125
[0071] [Creating a calibration curve] (1) Measurement of the concentration of polyacrylamide compound stock solution 1 g of a stock solution of a polyacrylamide compound (OKS-20, manufactured by Arakawa Chemical Industries, Ltd.) was weighed out and placed in an aluminum cup with a known mass, and dried at 105°C for 2 hours or more until it was solidified. The total mass of the aluminum cup and the dried stock solution of a polyacrylamide compound was then measured, and the concentration of the stock solution of a polyacrylamide compound was calculated using the following formula. Concentration of the undiluted polyacrylamide compound (mass%) = {Total mass (g) of the dried aluminum cup and the dried undiluted polyacrylamide compound (mass) - mass (g) of the aluminum cup} ÷ mass (g) of the undiluted polyacrylamide compound (mass) × 100 (2) Preparation of standard solutions of polyacrylamide compounds A specified amount of the polyacrylamide compound stock solution was placed in a 50 mL cup, and the solution was diluted to 10 g with ion-exchanged water to prepare a standard solution of the polyacrylamide compound. At this time, the amount of the polyacrylamide compound stock solution was 1.0 g, 2.5 g, and 5.0 g, and three standard solutions with different concentrations were obtained. The concentrations of the obtained standard solutions were measured using the same method as in (1) above. (3) Preparation of standard filter paper samples After measuring the dry mass of the filter paper, the filter paper was soaked in the target amount of a standard solution of a polyacrylamide compound and dried in a dryer at 105°C for 1 hour to prepare a standard filter paper sample. The standard filter paper sample was pulverized in a grinder, precisely weighed out to about 100-150μg, and used to create a calibration curve. The target amount of the standard solution of polyacrylamide compound to be added to the filter paper to prepare the standard filter paper sample was calculated using the following formula. Target amount of standard solution added (g) = dry mass of filter paper (g) × target polyacrylamide compound content (mass%) ÷ standard solution concentration of polyacrylamide compound (mass%) (4) Preparation of calibration curve The obtained standard filter paper sample was measured using a pyrolysis GC / MS analyzer, and a calibration curve was created from the measurement results of the detected ion m / z 125 (3-Ethylidene-2,5-pyrrolidinedione).
[0072] [Table 1]
[0073] [Table 2]
[0074] The results in Tables 1 and 2 show that the kraft papers of Examples 1 to 6 are excellent in both specific tensile strength and specific tear strength, as well as in sizing ability.
Claims
1. Kraft paper made primarily of wood pulp, The Canadian standard freeness of the disintegrated pulp obtained by redisintegrating the kraft paper is 500 mL or more; The content of the polyacrylamide-based dry strength agent in the kraft paper is 0.05% by mass or more and 0.75% by mass or less. Kraft paper.
2. 2. The kraft paper according to claim 1, wherein the weight average fiber length of the pulp constituting the kraft paper is 2.2 mm or more and 3.7 mm or less.
3. 10. The kraft paper of claim 1, wherein the wood pulp comprises softwood kraft pulp.
4. 4. The kraft paper according to claim 3, wherein the content of softwood kraft pulp in the wood pulp is 90% by mass or more.
5. 4. The kraft paper of claim 3, wherein the softwood kraft pulp source comprises Douglas fir.
6. 2. The kraft paper according to claim 1, having a specific tensile strength of 40.0 N·m / g or more.
7. Specific tear strength is 10.0 mN・m 2 2. The kraft paper of claim 1, wherein the kraft paper has a viscosity of 1:1 or more.
8. Basis weight 30g / m 2 More than 200g / m 2 2. The kraft paper of claim 1, wherein:
9. 2. The kraft paper of claim 1, having a Stockigt sizing degree of 12 seconds or more.
10. 2. The kraft paper of claim 1, having an elongation at break of 3.1% or more.
11. 2. The kraft paper of claim 1, which is a kraft paper for heavy-duty bags.
12. A packaging bag made using the kraft paper according to any one of claims 1 to 11.
Citation Information
Patent Citations
Conditioning paper and method for producing the same
JP2002004193A
Heavy-duty packaging kraft paper and method for producing the same
JP2006089889A
Kraft paper usable as decorating paper or reinforcing paper of kraft paper bag
JP2007262603A
One-side glazed kraft paper and method for producing one-side glazed kraft paper
JP2009299208A
Kraft paper for bag making
JP2010202997A
Cited By
Optical waveguide member and method for manufacturing optical waveguide member
CN121657203A
Kraft paper and method for manufacturing kraft paper
WO2026167996A1