Stretchable gauze towel and manufacturing method thereof
The stretch gauze towel achieves enhanced comfort through stretchability by modifying cotton yarn twist and using liquid ammonia treatment, maintaining the texture and comfort of conventional gauze towels.
Patent Information
- Application Number
- JP2023072302
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-04-26
AI Technical Summary
Gauze towels lack stretchability, which is necessary for comfortable wear in garments like pajamas, while incorporating synthetic fibers for stretchability degrades their characteristic texture and comfort.
A manufacturing method for a stretch gauze towel using cotton yarns with a modified twist coefficient, combined with liquid ammonia treatment to shrink the fabric in the width direction, creating a loop pile structure with a length of 3 mm or less and an apparent twist coefficient of 2 or less, without using elastic fibers.
The method achieves a stretchability of 10% or more elongation rate and 60% or more elongation recovery rate, maintaining the texture and comfort of conventional gauze towels, suitable for practical clothing.
Smart Images

Figure 2024157757000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a stretch gauze towel and a manufacturing method thereof. In particular, the present invention relates to a stretch gauze towel with excellent stretchability, the front and back cotton of which are made of loop pile fabric and gauze fabric, respectively, and a manufacturing method thereof. [Background technology]
[0002] In recent years, multi-layer gauze fabrics, which are made by layering coarse plain weave gauze fabrics, have become popular. Multi-layer gauze fabrics are made by layering gauze fabrics, which are highly absorbent and flexible, and therefore have good moisture absorption, breathability, lightness, feel, and texture, giving the user a comfortable feeling. For these reasons, they are used in sweat towels, handkerchiefs, baby products, and more, as well as in practical clothing such as pajamas.
[0003] Furthermore, in the case of multi-layered gauze fabrics, gauze towels in which one side of the front or back has a loop pile structure in order to further improve the texture and comfort when worn are also being used in pajamas and other bedding.
[0004] Practical clothing such as pajamas are sewn with a loose fit that emphasizes comfort. If gauze towels are used for pajamas and the like with the pile side facing the skin, the texture and comfort are surely improved. Meanwhile, in recent years, practical clothing has often required moderate stretchability, known as comfort stretch. In particular, pajamas and the like are worn in a relaxed state and are worn while sleeping, so in addition to loose stitching, moderate stretchability is required. However, gauze towels have the problem of being poor in elasticity and lacking in stretchability because they are pile woven from cotton yarn.
[0005] For example, the following Patent Document 1 proposes a stretchable towel, although it is not a gauze towel. This stretchable towel uses urethane elastic yarn for the ground weft or the ground weft and ground warp among the pile warp, ground warp and ground weft that make up the towel fabric, and cotton yarn for the pile warp. This gives the towel fabric stretchability in both the warp and weft directions. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Utility Model Application Publication No. 53-154270 Summary of the Invention [Problem to be solved by the invention]
[0007] As in Patent Document 1, stretchability can be imparted to gauze towels by using urethane elastic yarn in the weave. However, even if cotton yarn is used in the loop pile structure, using synthetic fibers other than cotton yarn in the gauze structure will reduce the texture and comfort that are characteristic of gauze towels.
[0008] Therefore, the present invention aims to address the above issues by providing a stretch gauze towel that has evolved into practical clothing by achieving even greater comfort through stretchability without compromising the texture and comfort of conventional gauze towels, and a manufacturing method thereof. [Means for solving the problem]
[0009] In order to solve the above problems, the inventors conducted extensive research and focused on the flexibility and dimensional settability (shape stability effect) achieved by liquid ammonia treatment, a processing method for cotton fabrics, and discovered that the above object could be achieved by devising the twist coefficient of the cotton yarn used in the loop pile weave of the gauze towel, which led to the completion of the present invention.
[0010] That is, the stretch gauze towel according to the present invention is as described in claim 1. A cotton fabric made of gauze toweling, the front and back surfaces of which are made of gauze and loop pile structures, It is characterized by having stretchability in the width direction of the fabric without containing elastic fibers, an elongation rate of 10% or more when subjected to a load of [(7.35 N / 50 mm width) x 60 minutes], and an elongation recovery rate of 60% or more 24 hours after the load is released.
[0011] According to claim 2, the present invention provides a stretch gauze towel according to claim 1, The loop pile structure has a loop pile length of 3 mm or less from the woven fabric structure, The apparent twist coefficient of the cotton yarn constituting the loop pile is 2 or less.
[0012] The method for producing a stretch gauze towel according to the present invention is as described in claim 3. A cotton gauze towel fabric having a gauze structure and a loop pile structure on the front and back sides is woven using warp yarns, weft yarns, and pile yarns mainly made of cotton yarns; The cotton fabric after weaving is treated with liquid ammonia to shrink the cotton fabric mainly in the width direction of the fabric, The cotton fabric after the liquid ammonia treatment is characterized in that it does not contain elastic fibers, has stretchability in the width direction of the fabric, has an elongation rate of 10% or more when a load of [(7.35 N / 50 mm width) x 60 minutes] is applied, and has an elongation recovery rate of 60% or more 24 hours after the load is removed.
[0013] According to claim 4, the present invention provides a method for producing the stretch gauze towel according to claim 3, The liquid ammonia treatment is characterized in that the width of the cotton fabric is shrunk by 13% or more.
[0014] According to claim 5, the present invention provides a method for producing the stretch gauze towel according to claim 3 or 4, The loop pile structure after the liquid ammonia treatment has a loop pile length of 3 mm or less from the surface of the gauze structure, The apparent twist coefficient of the cotton yarn constituting the loop pile is 2 or less. Effect of the Invention
[0015] According to the above configuration, the stretch gauze towel of the present invention is a cotton woven gauze towel fabric with a gauze structure and a loop pile structure on the front and back sides, respectively. The towel does not contain elastic fibers and has stretchability in the width direction of the fabric, and has an elongation rate of 10% or more when a load of [(7.35N / 50mm width) x 60 minutes] is applied. The elongation recovery rate 24 hours after the load is removed is 60% or more.
[0016] This makes it possible to provide a stretch gauze towel that has evolved into practical clothing by achieving even greater comfort through stretchability without compromising the texture and comfort of conventional gauze towels.
[0017] Furthermore, according to the above configuration, the loop pile structure has a loop length of 3 mm or less from the surface of the gauze structure, and the apparent twist coefficient of the cotton yarn constituting the loop pile is 2 or less. This makes it possible to more specifically and effectively exert the above-mentioned effects.
[0018] According to the above configuration, the manufacturing method of the stretch gauze towel of the present invention uses warp yarns, weft yarns, and pile yarns mainly made of cotton yarns to weave a cotton fabric of gauze towel cloth, the front and back of which are made of a gauze structure and a loop pile structure, respectively. Next, the woven cotton fabric is treated with liquid ammonia to shrink the cotton fabric mainly in the width direction. As a result, the cotton fabric after the liquid ammonia treatment has stretchability in the width direction of the fabric without containing elastic fibers, and has an elongation rate of 10% or more when a load of [(7.35N / 50mm width) x 60 minutes] is applied. Also, the elongation recovery rate 24 hours after the load is removed is 60% or more.
[0019] This makes it possible to provide a manufacturing method for stretch gauze towels that have evolved into practical clothing by achieving even greater comfort through stretchability without compromising the texture and comfort of conventional gauze towels.
[0020] According to the above configuration, it is preferable that the width of the cotton fabric is shrunk by 13% or more in the liquid ammonia treatment. It is also preferable that the loop pile length of the loop pile fabric after the liquid ammonia treatment is 3 mm or less from the surface of the gauze fabric, and the apparent twist coefficient of the cotton yarn constituting the loop pile fabric is 2 or less. This makes it possible to more specifically and effectively exert the above-mentioned effects. [Brief description of the drawings]
[0021] [Figure 1] 1 is a graph showing the elongation rate (%) of the stretch gauze towel of the embodiment from the first day to the fifth day. [Diagram 2] 1 is a graph showing the elongation recovery rate (%) of the stretch gauze towel of the embodiment from the first day to the fifth day. [Diagram 3] 1 is a graph showing monitor test results (overall evaluation of comfort) of the stretch gauze towel of the embodiment and the comparative example. [Figure 4]1 shows a graph illustrating monitor test results (comfort when legs are raised) for a stretch gauze towel according to an embodiment and a comparative example, and photographs illustrating test conditions. [Diagram 5] 1 is a graph showing monitor test results (comfort when squatting) of a stretch gauze towel according to an embodiment and a comparative example, and photographs showing test conditions. [Figure 6] 1 shows a graph illustrating monitor test results (comfort when curled up) of a stretch gauze towel according to an embodiment and a comparative example, and photographs illustrating test conditions. [Figure 7] 1 is a graph showing monitor test results (comfort when arms are raised) of a stretch gauze towel according to an embodiment and a comparative example, and photographs showing test conditions. [Figure 8] 1 is a graph showing the results of a questionnaire survey on the feel of the stretch gauze towel of the embodiment, the gauze towel of the comparative example, and a regular hand towel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] First, the terms used in the present invention will be explained. In the present invention, a gauze towel means a woven fabric that combines a gauze weave and a towel weave (loop pile weave), with one side of the front and back being a gauze weave and the other being a towel weave. In other words, the weave of a gauze towel is a gauze weave, and one side of this weave is a towel weave with loop pile. In general, a gauze weave is defined as a soft, thin cotton weave with a coarse plain weave made of loosely twisted yarn, and a towel weave is defined as one of the warp pile and double warp pile weaves of cotton with large pile on the surface of the cloth (New Textile Encyclopedia; Senken Shimbunsha). However, in the present invention, these definitions are not used and a weave that combines a gauze weave and a towel weave (loop pile weave) is broadly interpreted as a gauze towel.
[0023] In the present invention, a cotton gauze towel fabric (warp pile fabric) is woven using warp yarns, weft yarns, and pile yarns mainly made of cotton yarn, with the front and back sides each having a gauze structure and a loop pile structure. The warp yarns, weft yarns, and pile yarns are not limited to 100% cotton as in general gauze fabrics, and any yarn mainly made of cotton can be used. However, since the liquid ammonia treatment described below is carried out, it is required that the treatment be easily effective. Therefore, in the present invention, it is particularly preferable to use 100% cotton yarns for the warp yarns, weft yarns, and pile yarns.
[0024] Furthermore, the loop pile length of conventional gauze towels is 4 mm or more from the surface of the gauze fabric. In contrast, in the present invention, the loop pile length is preferably 3 mm or less, more preferably 2.5 mm or less, and even more preferably 2 mm or less. By shortening the loop pile, a towel fabric with a good texture is produced. Furthermore, the pile yarn that constitutes the loop pile is preferably 100% cotton yarn, and is non-twisted yarn or very loosely twisted yarn.
[0025] The twist of a thread is expressed by the twist factor. The twist factor is a coefficient that indicates the effect of twist (how tight the thread is), regardless of the thickness of the thread. In the case of cotton thread, the twist factor α is expressed as "α = number of twists / √N". Here, the number of twists is "turns / inch", and N is the "constant weight count". Regardless of the thickness (count) of the thread, generally, an α of 3.3 or less is called a loose twist, an α of 3.5 to 4.5 is called a normal twist, and any twist factor greater than this is called a hard twist (Why Cotton, "Product Knowledge for Cotton Products"; Japan Cotton Industry Promotion Association).
[0026] In the present invention, in order to impart stretchability, the gauze towel after weaving is treated with liquid ammonia to shrink it in the width direction of the fabric. Therefore, the weft yarn and pile yarn of the gauze towel shrink due to the liquid ammonia treatment, and the yarn thickness (count N) and twist factor (α) change from the yarn stage after weaving. Therefore, in the present invention, the yarn thickness that has shrunk after the liquid ammonia treatment is referred to as the "apparent count" and the twist factor is referred to as the "apparent twist factor." The twist factor and apparent twist factor of each woven fabric in the present invention will be described later.
[0027] In the present invention, the length and twist coefficient of the loop pile (apparent twist coefficient after shrinkage), which particularly affect the texture and comfort of the gauze towel, are important. As described above, the length of the loop pile is preferably 3 mm or less, and more preferably 2.5 mm or less. On the other hand, as described above, it is preferable to use 100% cotton yarn that is a non-twist yarn or a very loosely twisted yarn for the pile yarn. Therefore, the apparent twist coefficient of the pile yarn that has shrunk after the liquid ammonia treatment is preferably 2 or less, and more preferably 1.5 or less. For this reason, the twist coefficient of the pile yarn before shrinkage in the weaving stage is preferably 1.5 or less, and more preferably 1 or less.
[0028] However, if the twist coefficient of the pile yarn is reduced, it is not possible to weave a gauze towel. This is because the tension applied to the pile yarn from the loom is large, and the pile yarn breaks during the weaving stage, making it impossible to weave. Therefore, measures are taken to increase the tensile strength of the yarn during the weaving stage. In the present invention, a single cotton yarn (twisted) is combined with a filament of water-soluble PVA (polyvinyl alcohol), and twisted in the opposite direction to the twist of the single yarn to form a two-ply yarn. If the single yarn is untwisted by the number of twists, the twist of the single yarn becomes zero. If a gauze towel is woven using this two-ply yarn of cotton and water-soluble PVA, and then the water-soluble PVA is dissolved, a loop pile of cotton non-twisted yarn or very loosely twisted yarn can be produced. Note that in the present invention, the manufacturing method of non-twisted yarn or very loosely twisted yarn is not limited to the above method, and non-twisted yarn or very loosely twisted yarn may be manufactured using a special spinning machine.
[0029] In the present invention, the liquid ammonia treatment is generally performed as a processing method for cotton fabrics, and is a treatment in which the cotton fabric is immersed in liquid ammonia (boiling point: -33.4°C) for a short time, and then brought into contact with a cylinder heated to about 130°C to remove the ammonia. In general, the wrinkle resistance, shrink resistance, strength, and flexibility of the cotton fabric are improved. In the present invention, it is preferable to shrink the gauze towel by 13% or more in the width direction of the fabric. It is more preferable to shrink the gauze towel by 15% or more, and even more preferable to shrink the gauze towel by 18% or more (details will be described later). By shrinking the gauze towel by 13% or more in the width direction of the fabric, it is possible to achieve practical and comfortable stretchability.
[0030] The stretch gauze towel of the present invention will be described below with reference to examples. In addition, a gauze towel (without stretchability) woven in the same manner as in the present embodiment and not treated with liquid ammonia was used as a comparative example for comparison with the stretch gauze towel of the present embodiment. Note that the present invention is not limited to the following examples. EXAMPLES
[0031] <Weaving of gauze towels> To manufacture the stretch gauze towel of this embodiment, first, the gauze towel is woven in a normal manner. For weaving the gauze towel, various looms such as a jacquard loom with a warp shedding device, a dobby loom, or a tappet loom can be used. In this embodiment, the towel was woven using a dobby loom.
[0032] In this embodiment, 100% cotton yarns are used for the warp, weft, and pile yarns, but the yarns are not limited to yarns that are pre-dyed, and they may be dyed after weaving. The yarn count of the warp and weft is not particularly limited, but it is preferable to use single or two-ply yarns of 30 to 60. In this embodiment, 80-count twin yarns (80 / 2) equivalent to 40-count yarns were used for the warp, and 40-count single yarns (40 / 1) were used for the weft. The twist coefficient is not particularly limited, and normal twist yarns were used for the warp and weft. The pile yarns are single yarns of 30 to 60 count yarns, and the twist coefficient at the weaving stage is preferably 1.5 or less, and more preferably 1.0 or less. In this embodiment, a two-ply yarn of cotton yarn with a twist coefficient of 0.948 (twist count: 6 times / inch) and water-soluble PVA was used. On the other hand, the gauze towel of the comparative example used the same warp and weft yarns as those of the present example, but the pile yarn was a plain twist yarn of 40-count cotton single yarn (40 / 1).
[0033] The warp and weft yarn density of the gauze towel at the weaving stage is not particularly limited, but may be adjusted in terms of breathability, lightness, touch, texture, etc. For example, the warp yarn density is preferably 40 to 60 yarns / inch. On the other hand, the weft yarn density is preferably 70 to 90 yarns / inch. The reason why the weft yarn density is larger than the warp yarn density is due to the pile structure. In the weaving stage of this embodiment, the warp yarn density was 50 yarns / inch, the weft yarn density was 79 yarns / inch, and the pile yarn density was 25 yarns / inch. In this embodiment, the loop pile length was 2 mm from the surface of the gauze structure. On the other hand, the warp yarn density, weft yarn density, pile yarn density, and loop pile length of the gauze towel of the comparative example were the same as those of this embodiment.
[0034] <Dissolving pile yarn in PVA> The loop pile of the gauze towel after weaving is still in a state of two-ply yarn of cotton and water-soluble PVA. Therefore, the gauze towel after weaving is washed with hot water to dissolve the water-soluble PVA and become a loop pile of 100% cotton. It is then dried and spun to the specified woven width, and the next process of liquid ammonia treatment is carried out. On the other hand, the gauze towel of the comparative example uses normal twist cotton yarn (not containing water-soluble PVA) for the pile yarn, so PVA was not dissolved, and after normal desizing and drying, fabric softener was added and spun to the specified woven width.
[0035] <Liquid ammonia treatment> In this embodiment, a general liquid ammonia treatment device can be used. Usually, the liquid ammonia treatment device is composed of an immersion device for immersing the fabric in liquid ammonia, a timing device for promoting the penetration and reaction of the liquid ammonia, a drying device for evaporating the liquid ammonia, and a steaming device for removing the residual ammonia, and the fabric is continuously treated by moving the fabric.
[0036] The gauze towel of this embodiment shrinks rapidly when it absorbs liquid ammonia. As the gauze towel runs continuously through the liquid ammonia treatment device, tension is applied to the length direction (warp direction) of the fabric, suppressing the shrinkage of the warp. On the other hand, no tension is applied to the width direction (weft direction) of the fabric, and the weft shrinks significantly. Furthermore, the loop pile also shrinks without tension. After the liquid ammonia is removed, the gauze towel retains its shape with the fabric width greatly shrunk. After the liquid ammonia treatment, the gauze towel is washed and dried, and then softener is added and the towel is stretched to a specified width to obtain a stretch gauze towel.
[0037] In this example, the stretch gauze towel after removing the liquid ammonia had a warp density of 64 threads / inch, a weft density of 81 threads / inch, and a pile density of 32 threads / inch. This means that the stretch gauze towel hardly shrunk (approximately 2% shrinkage) in the length direction of the fabric (warp direction) due to the liquid ammonia treatment, but shrunk by 21% in the width direction of the fabric (weft direction).
[0038] In this way, the warp yarns of the gauze towel hardly shrink, and only the weft yarns shrink significantly. As a result, the warp yarn count and twist factor of the stretch gauze towel after liquid ammonia treatment hardly change. In contrast, the weft yarn count becomes larger (thicker) and the twist factor also becomes larger (tighter yarn), resulting in the yarn exhibiting stretchability like a strong twist yarn. The pile yarn also shrinks like the weft yarn (especially the loop pile portion). For this reason, in the present invention, a non-twist yarn or a very loosely twisted yarn is used for the pile yarn. As a result, even if the twist factor of the pile yarn increases, it does not become a tight yarn, and the loop pile is configured to maintain its flexibility.
[0039] It is preferable to control the running conditions of the gauze towel introduced into the liquid ammonia treatment device to fix the fabric width to a predetermined value. In this embodiment, as described above, the fabric width was shrunk by 21%. As a result, as described later, the elongation rate was 10% or more and the elongation recovery rate was 60% or more, which was a good result.
[0040] In addition, in the present invention, liquid ammonia treatment is used to shrink the gauze towel in the width direction of the fabric. In addition to liquid ammonia, there are other methods for shrinking cotton fabric, such as mercerization using a highly concentrated aqueous solution of sodium hydroxide. However, liquid ammonia treatment has a greater effect on the flexibility of the fabric after treatment and shape stability of the shrunk state compared to mercerization, and can achieve the comfortable fit achieved by the flexibility and stretchability that is the objective of the present invention.
[0041] <Physical property evaluation> Next, the physical properties of the stretch gauze towel obtained in this example were evaluated. The pile yarn apparent count and apparent twist coefficient were calculated as evaluation items. Next, to evaluate the stretchability, the elongation modulus (elongation rate and elongation recovery rate) at a constant load was evaluated. In addition, the comfort of using it for pajamas (loop pile used on the skin side) was evaluated in a monitor test. The various physical properties for pajamas (water absorbency, heat retention, breathability) were also confirmed.
[0042] 1. Apparent yarn count and apparent twist factor First, the apparent counts (after shrinkage) of the warp yarns, weft yarns, and pile yarns after the liquid ammonia treatment were calculated. The apparent twist coefficient (after shrinkage) of the pile yarns was also calculated. As described above, in this embodiment, the liquid ammonia treatment caused almost no shrinkage (approximately 2% shrinkage) in the length direction (warp direction) of the fabric, but 21% shrinkage in the width direction (weft direction) of the fabric. Therefore, the apparent count was calculated assuming that the weight (weight per unit length) of the weft yarn increased by 21%. In addition, the apparent twist coefficient was calculated from the twist coefficient formula "α = twist number / √N" assuming that the number of twists (number of times / inch) of the pile yarn increased by 21%. The counts and apparent counts of the warp yarns, weft yarns, and pile yarns before shrinkage, and the twist coefficients and apparent twist coefficients of the pile yarns before shrinkage are shown in Table 1. In addition, the pile yarn also shrunk by 21%, so the loop pile length after the liquid ammonia treatment was approximately 1.6 mm.
[0043] [Table 1]
[0044] In Table 1, the pile yarn shrinks by 21%, resulting in a slightly thicker apparent count. In addition, the apparent twist factor of the pile yarn, calculated using the 21% increased twist number (7.26 turns / inch) and apparent count (32), is less than 2, indicating that the flexibility of the loop pile is maintained.
[0045] 2. Elongation modulus (elongation rate and elongation recovery rate) Since this example concerns a stretch gauze towel for use as pajamas, an original test method (by the Boken Quality Evaluation Organization, a general incorporated foundation) was adopted to evaluate the appropriate stretchability of lightweight woven fabrics.
[0046] The test method for the elongation rate is based on JIS L 1096 (B-1 method), with the load and time changed. Specifically, a test piece with a width of 50 mm and a length of 300 mm is set in a tensile tester, and marks are made at intervals of 200 mm (L0). After holding the test piece for 60 minutes under a specified load (7.35 N / 50 mm width), the length between the marks (L1) is measured, and the elongation rate is calculated using the following formula (1). Elongation rate (%) = [(L1-L0) / L0] × 100 (1) The elongation rate (%) was calculated. The above test was conducted on the first day, and the elongation rate (%) was calculated on the second to fifth days using the same test piece. The obtained elongation rate (%) values on the first to fifth days for this example and comparative example are shown in Table 2. These values are also shown in a graph in Figure 1. Note that Figure 1 also shows predictions (hypothetical values) on the sixth to eighth days.
[0047] On the other hand, the test method for the elongation recovery rate is as follows: 24 hours after the load is released, an initial load is applied to the test piece with the above elongation rate, the length between the marks (L2) is measured, and the test result is calculated using the following formula (2). Elongation recovery rate (%)=[(L1-L2) / (L1-L0]×100...(2) The elongation recovery rate (%) was determined. The above test was conducted on the first day, and the elongation recovery rate (%) was determined on the second to fifth days for the same test piece. The obtained elongation recovery rate (%) values on the first to fifth days for this example and comparative example are shown in Table 2. These values are also shown in a graph in Figure 2. Note that Figure 2 also shows predictions (hypothetical values) on the sixth to eighth days.
[0048] [Table 2]
[0049] In Table 2 and FIG. 1, the examples had elongation rates (%) of 13% or more from the first day to the fifth day, and showed stable and good stretchability of 10% or more over five days. In contrast, the comparative examples had elongation rates (%) of about 4% from the first day to the fifth day, which is a value for a normal cotton fabric and does not have stretchability. In addition, in Table 2 and FIG. 2, the examples had elongation recovery rates (%) of 63% or more from the first day to the fifth day, and showed stable and good results of 60% or more over five days. In contrast, the comparative examples had elongation recovery rates (%) of 60% or more from the first day to the fifth day, which is a value for a normal cotton fabric because the elongation rate is about 4%. From these results, the stretch gauze towel according to this example had stable and good stretchability.
[0050] 3. Comfort (monitor test) Next, the stretch gauze towel according to this embodiment was actually sewn into pajamas, and a monitor test was conducted on comfort. Specifically, five monitors evaluated the comfort (overall evaluation) and each item (comfort when lifting legs, comfort when squatting, comfort when curling up, comfort when raising arms). The comparative example was also sewn into pajamas and evaluated in the same manner. The evaluation results of this embodiment and the comparative example are shown in Table 3. The evaluation results are also shown in graphs in Figures 3 to 7.
[0051] [Table 3]
[0052] In Table 3 and Figures 3 to 7, all five monitors gave the pajamas sewn with the stretch gauze towel of this example a perfect score in all evaluation items. The comparative example is also highly regarded in the market as a conventional, comfortable pajamas. From these results, it can be seen that the comfort of the pajamas sewn with the stretch gauze towel of this example was rated even higher than that of the conventional product (comparative example) which is highly regarded in the market.
[0053] 4. Texture (survey) Next, a questionnaire survey was conducted to compare the feel of the stretch gauze towel of this embodiment with the feel of the gauze towel of the comparative example and a normal hand towel. Specifically, 20 randomly selected men and women were asked which of the above three items felt the best. The results of the survey are shown in Table 4 and Figure 8.
[0054] [Table 4]
[0055] As shown in Table 4 and Figure 8, a large number of people, both males and females, rated the feel of the stretch gauze towel of this example as the best. The comparative example is also a gauze towel that is highly rated in the market and was evaluated accordingly. This shows that the feel of the stretch gauze towel of this example is even better than the conventional product (comparative example) that is highly rated in the market, and was rated much higher than ordinary hand towels.
[0056] 5. Physical properties for pajamas The stretch gauze towel of this example was evaluated for water absorption, heat retention, and breathability, and compared with the gauze towel of the comparative example and normal woven fabrics (cotton twill and cotton broadcloth). The evaluation results are shown in Table 4.
[0057] [Table 5]
[0058] In Table 4, the physical properties of the stretch gauze towel of this example were good for use as pajamas. The comparative example was also evaluated in the market as a conventional pajama that was comfortable to wear, and was good for use as pajamas. In Table 4, it can be seen that both this example and the comparative example have better performance for use as pajamas than regular woven fabrics such as cotton twill and cotton broadcloth.
[0059] As explained above, according to the present invention, it is possible to provide a stretch gauze towel and a manufacturing method thereof that have evolved into practical clothing by achieving even greater comfort through stretchability without compromising the texture and comfort of conventional gauze towels.
Claims
1. A cotton fabric made of gauze toweling, the front and back surfaces of which are made of gauze and loop pile structures, This stretch gauze towel is characterized in that it does not contain elastic fibers, has stretchability in the width direction of the fabric, has an elongation rate of 10% or more when a load of [(7.35 N / 50 mm width) x 60 minutes] is applied, and has an elongation recovery rate of 60% or more 24 hours after the load is released.
2. The loop pile structure has a loop length of 3 mm or less from the surface of the gauze structure, 2. The stretch gauze towel according to claim 1, wherein the apparent twist factor of the cotton yarn constituting said loop pile is 2 or less.
3. A cotton gauze towel fabric having a gauze structure and a loop pile structure on the front and back sides is woven using warp yarns, weft yarns, and pile yarns mainly made of cotton yarns; The cotton fabric after weaving is treated with liquid ammonia to shrink the cotton fabric mainly in the width direction of the fabric, The cotton fabric after the liquid ammonia treatment is free of elastic fibers, has stretchability in the width direction of the fabric, has an elongation rate of 10% or more when a load of [(7.35 N / 50 mm width) x 60 minutes] is applied, and has an elongation recovery rate of 60% or more 24 hours after the load is released.
4. 4. The method for producing a stretch gauze towel according to claim 3, wherein the width of the cotton fabric is shrunk by 13% or more in the liquid ammonia treatment.
5. The loop pile structure after the liquid ammonia treatment has a loop pile length of 3 mm or less from the surface of the gauze structure, 5. The method for producing a stretch gauze towel according to claim 3, wherein the apparent twist factor of the cotton yarn constituting the loop pile is 2 or less.
Citation Information
Patent Citations
Wood fiber / tencel cashmere imitation double-layer fabric
CN109930278A
Production of stretchable woven / Knitted fabric consisting of cellulose-based fiber
JP2000248461A
Stretch multiple fabric and its manufacturing method
JP2022033469A
Stretch fabric
JP3172230U
JP1978154270U