Sewing yarn
A sewing thread made of alkali-soluble resin, particularly copolymerized polyester, addresses the durability issue in industrial washing by maintaining strength and enabling easy separation of clothing components through alkaline dissolution.
Patent Information
- Application Number
- JP2024039715
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-14
- Publication Date
- 2024-11-08
AI Technical Summary
Existing sewing threads used for recycling clothing are not durable enough to withstand industrial washing, leading to a decrease in strength and making it difficult to separate clothing components effectively.
A sewing thread made of alkali-soluble resin, specifically copolymerized polyester resin, with a high tenacity retention rate after 50 industrial washes and a weight loss rate of 50% or more when treated with an alkaline solution, ensuring durability and easy separation.
The sewing thread maintains strength during repeated industrial washing and can be easily dissolved in alkaline solutions, facilitating efficient recycling of clothing components without damage.
Smart Images

Figure 2024159515000001 
Figure 2024159515000002 
Figure 2024159515000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a sewing thread made of fibers formed from an alkali-soluble resin. [Background technology]
[0002] In recent years, from the perspective of environmental protection, there have been attempts to collect and recycle used clothing. Because clothing is made up of many parts, in order to recycle clothing, it is first necessary to separate the recyclable parts from the clothing. For this reason, clothing recycling begins with separating the constituent parts of the garment, such as the body, sleeves, collar, cuffs, hem, buttons, and zippers, and separating the recyclable parts from the non-recyclable parts. The parts can be easily separated by cutting the sewn parts or removing the sewing threads. However, both of these processes are usually done by hand, and there has been a demand for labor-saving and simplification of the work.
[0003] Therefore, when separating a garment into its constituent parts, it is conceivable to make the sewing thread that sews the constituent parts together dissolvable, thereby saving labor and simplifying the work. For example, Patent Document 1 discloses a technique for dissolving a sewing thread made of water-soluble polyvinyl alcohol fiber with warm water, and Patent Document 2 discloses a technique for dissolving a sewing thread made of alkali-soluble polyester fiber with a strong alkaline aqueous solution. If these sewing threads are used, the garment can be separated into its constituent parts simply by immersing the collected garment in warm water or a strong alkaline aqueous solution, without the trouble of cutting the sewn parts or removing the sewing thread.
[0004] However, clothes must be washed after wearing. In terms of removing dirt, for example, uniforms such as nursing clothes, medical clothes, work clothes, and sports clothes tend to have a wider range of dirt and adhere more firmly to the clothes than general clothes, so that regular home washing may not be able to remove the dirt sufficiently. For this reason, industrial washing in warm water using commercial detergent containing alkaline agents is common, and washing is generally done every time the clothes are worn.
[0005] In the case of clothing that requires repeated industrial washing, if sewing thread that cannot withstand industrial washing is used, the strength of the sewing thread will decrease during washing, causing significant inconvenience when wearing the garment. The sewing threads described in Patent Documents 1 and 2 are advantageous in terms of recycling clothes because they can be easily dissolved by simply immersing collected clothes in warm water or a strong alkaline aqueous solution. However, these sewing threads do not have durability against industrial washing. Therefore, there is a problem that sewing threads that do not have industrial washing resistance cannot be used for clothes that are subjected to industrial washing. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 8-81811 [Patent Document 2] Japanese Patent Application Publication No. 7-216615 Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention is intended to solve the above problems, and has as its technical object the provision of a novel sewing thread which is easily soluble in alkali and at the same time has excellent durability against industrial washing. [Means for solving the problem]
[0008] The gist of the present invention is a sewing thread comprising at least one of long fibers or short fibers formed of an alkali-soluble resin, characterized in that the thread has a strength retention rate of 70% or more after 50 industrial washes, and a weight loss rate of 50% or more when subjected to an alkali weight loss treatment at 100°C for 30 minutes using an alkaline aqueous solution with a concentration of 20 g / L. Effect of the Invention
[0009] The sewing thread of the present invention can be easily dissolved in a strong alkaline aqueous solution and has sufficient durability even after repeated industrial washing. Therefore, when used in uniform clothing that requires industrial washing every time it is worn, the strength of the sewing thread is unlikely to decrease during washing, making it possible to use it for a long period of time. Furthermore, when it is time to recycle the used garment, the garment can be easily separated into its component parts simply by immersing it in a strong alkaline aqueous solution, which is advantageous in terms of recycling the garment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below. The present invention relates to a sewing thread containing at least one of long fibers or short fibers formed from an alkali-soluble resin, and polyester resin is particularly suitable as the alkali-soluble resin. In general, sewing threads made of polyester fibers formed from polyester resin (polyester sewing threads) are considered to have a superior glossiness and a better appearance of the seams than sewing threads made from other fibers. The sewing thread of the present invention can achieve the effects of the present invention described above, as well as the characteristics of conventional sewing threads made from alkali-soluble resins, particularly polyester sewing threads.
[0011] The alkali-soluble resin in the present invention can be any resin that can be easily dissolved in a strong alkaline aqueous solution when used as a sewing thread and that is expected to have sufficient durability when repeatedly washed industrially.Specific examples include polyvinyl alcohol resin, polyethylene oxide resin, alginic acid resin, polyacrylamide resin, carboxymethyl cellulose resin, and polyester resins composed of specific components.Of these, polyester resins composed of specific components are preferred, and examples of such polyester resins include polycaprolactone resin, polylactic acid resin, polyhydroxybutyrate resin, polyglycolic acid resin, polyethylene adipate resin, and copolymer polyester resins using specific copolymer components.In the present invention, copolymer polyester resins and polylactic acid resins are particularly preferred from the viewpoint of achieving both alkali solubility and industrial washability.
[0012] The copolymer polyester resin preferably contains 80 mol % or more of terephthalic acid when the total amount of all acid components constituting the polyester is 100 mol %. If the content of terephthalic acid is less than 80 mol %, the crystallinity of the resin decreases, resulting in a decrease in the strength of the fiber, making it impossible to obtain a sewing thread with sufficient strength to withstand use. On the other hand, the upper limit of the content of terephthalic acid is not particularly limited, but it is preferable to set the upper limit at 97.5 mol %. If it exceeds 97.5 mol %, the content of aromatic dicarboxylic acid having a metal sulfonate group and aliphatic dicarboxylic acid having 5 to 10 carbon atoms, which will be described later, decreases, making it difficult to impart alkali solubility, and therefore it is not preferable that the sewing thread is difficult to dissolve even if the garment is immersed in a strong alkaline aqueous solution.
[0013] In addition, the acid component constituting the copolymerized polyester resin preferably contains an aromatic dicarboxylic acid having a metal sulfonate group as a copolymerization component in an amount of 0.5 to 5 mol %, and more preferably 0.8 to 3 mol %. If the content (copolymerization amount) is less than 0.5 mol %, the resin becomes highly crystalline, making it difficult to impart alkali solubility to the fiber. On the other hand, if it exceeds 5 mol %, the resistance to an alkaline aqueous solution decreases, making it difficult to obtain a sewing thread that can withstand industrial washing. Furthermore, the heat resistance of the fiber decreases, and when the sewing thread is used as a sewing thread, the frictional heat during sewing makes it easy for the sewing thread to break or skip stitches.
[0014] Examples of aromatic dicarboxylic acids having a metal sulfonate group include 5-sodium sulfoisophthalic acid, 5-potassium sulfoisophthalic acid, 5-lithium sulfoisophthalic acid, sodium sulfonaphthalenedicarboxylic acid, sodium sulfophenyldicarboxylic acid, 5-sodium sulfoterephthalic acid, etc., and two or more of them may be used in combination or their derivatives may be used. In the present invention, 5-sodium sulfoisophthalic acid is preferred from the viewpoints of operability and cost during melt spinning.
[0015] Furthermore, the copolymer polyester resin may contain an acid component other than terephthalic acid and aromatic dicarboxylic acid having a metal sulfonate group, as long as the effect of the present invention is not impaired. Specific examples include isophthalic acid, phthalic acid, phthalic anhydride, naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, dodecanedioic acid, trimellitic anhydride, trimellitic acid, pyromellitic acid, adipic acid, sebacic acid, 1,4-cyclohexanedicarboxylic acid, and dimer acid. In the present invention, two or more of these may be used in combination, and derivatives of these may also be used.
[0016] The glycol component, which is the other component constituting the polyester, preferably contains 80 mol % or more of ethylene glycol and 0.1 to 1.0 mol % of a polyether compound, when the total amount of all glycol components constituting the polyester is taken as 100 mol %. If the ethylene glycol content is less than 80 mol%, the heat resistance of the fiber tends to decrease, and as a result, when used as sewing thread, thread breakage and skipped stitches are likely to occur due to frictional heat during sewing, which is not preferable. On the other hand, the upper limit of the ethylene glycol content is not particularly limited, but it is preferable to set the upper limit at 99 mol%. If it exceeds 99 mol%, the content of the polyether compound decreases, making it difficult to impart alkali solubility, and as a result, even if the garment is immersed in a strong alkaline aqueous solution, the sewing thread is difficult to dissolve, which is not preferable.
[0017] The content of the polyether compound is preferably 0.1 to 1.0 mol%, and more preferably 0.15 to 0.5 mol% as a copolymerization component. If the content (copolymerization amount) is less than 0.1 mol%, it becomes difficult to impart alkali solubility to the fiber. On the other hand, if it exceeds 1.0 mol%, the resistance to an alkaline aqueous solution decreases, making it difficult to obtain a sewing thread that can withstand industrial washing.
[0018] Examples of the polyether compound in the present invention include polyethylene glycol, polypropylene glycol, polytetramethylene glycol, and copolymers of ethylene oxide and propylene oxide, with polyethylene glycol and polytetramethylene glycol being preferred.
[0019] The number average molecular weight of the polyether compound is preferably 1000 to 15000. If the number average molecular weight of the polyether compound is less than 1000, the alkali solubility of the resulting fiber is likely to decrease. On the other hand, if the number average molecular weight of the polyether compound exceeds 15000, the thermal stability of the polyester resin is impaired, and yarn breakage is likely to occur frequently during spinning.
[0020] Furthermore, the copolymerized polyester resin may contain glycol components other than ethylene glycol and polyether compounds, as long as the effects of the present invention are not impaired. Specifically, diethylene glycol, neopentyl glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexamethylenediol, 1,4-cyclohexanedimethanol, dimer diol, ethylene oxide adducts of bisphenol A or bisphenol S, and the like can be used. In the present invention, two or more of these may be used in combination, and derivatives of these may also be used. In addition, the glycol components other than ethylene glycol and polyether compounds may be included as by-products that may be generated during the production of the copolymerized polyester resin.
[0021] The above-mentioned copolymer polyester resin may be obtained by material recycling in which a polyester resin that has been used once is reused, or may be obtained by chemical recycling.
[0022] The polylactic acid resin may be any of poly-L-lactic acid, poly-D-lactic acid, poly-D,L-lactic acid which is a copolymer of L-lactic acid and D-lactic acid, and a mixture (stereocomplex) of poly-L-lactic acid and poly-D-lactic acid which has a high melting point.
[0023] In the polylactic acid resin used in the present invention, when poly-D,L-lactic acid, which is a copolymer of L-lactic acid and D-lactic acid, is used, the copolymerization ratio of D-lactic acid to L-lactic acid (D-lactic acid / L-lactic acid) is preferably 100 / 0 to 95 / 5, or 5 / 95 to 0 / 100.
[0024] Furthermore, the polylactic acid resin may contain cyclic lactones such as ε-caprolactone, α-hydroxyacids such as α-hydroxybutyric acid, α-hydroxyisobutyric acid, α-hydroxyvaleric acid, and the like, glycols such as ethylene glycol, 1,4-butanediol, and dicarboxylic acids such as succinic acid, sebacic acid, and the like, as long as the object of the present invention is not impaired.
[0025] The sewing thread of the present invention contains at least one of long fibers and short fibers formed from the above-mentioned alkali-soluble resin. The sewing thread of the present invention may be one consisting of only long fibers, one consisting of only short fibers, or one containing both fibers.
[0026] In particular, the long fibers or short fibers formed from the above-mentioned alkali-soluble resin preferably contain 90% by mass or more of the above-mentioned alkali-soluble resin, and more preferably are made only of the above-mentioned alkali-soluble resin. In other words, the long fibers or short fibers formed from the alkali-soluble resin preferably are made only of the alkali-soluble resin, but may be composite fibers containing other resins as long as the effects of the present invention are not impaired. Examples of the form of the composite fiber include a side-by-side type, a core-sheath type, and an island-in-the-sea type.
[0027] The sewing thread of the present invention preferably contains 50% by mass or more of long or short fibers formed from the above-mentioned copolymer polyester resin or polylactic acid resin, more preferably 70% by mass or more, even more preferably 90% by mass or more, and most preferably 100% by mass.
[0028] The content of the above-mentioned copolymer polyester resin or polylactic acid resin in the sewing thread is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and most preferably 100% by mass.
[0029] The sewing thread of the present invention may contain other fibers other than the long fibers or short fibers formed of the alkali-soluble resin. Any other fibers may be used as the other fibers as long as they do not impair the effects of the present invention, and specific examples include polyethylene terephthalate fibers, nylon fibers, acrylic fibers, and cellulose fibers. The other fibers may be in the form of either long fibers or short fibers.
[0030] The sewing thread of the present invention may be in the form of a filament yarn, a spun yarn, or a long-short composite yarn containing at least one of the long fibers or short fibers formed from the alkali-soluble resin, but it is practically preferable to use a filament yarn or a spun yarn. In that case, it may be a decorative yarn depending on the purpose, or may be a yarn of one color or a composite of multiple yarns of dyed yarns to give a mottled look.
[0031] The thickness of the sewing thread of the present invention may be set arbitrarily depending on the purpose, and is preferably 20 to 1500 dtex for filament yarn, and 4 to 200 (British cotton count) for spun yarn or long and short composite yarn.
[0032] Furthermore, the sewing thread of the present invention may be either a non-twisted thread or a twisted thread. Since the strength of a thread generally increases when the thread is twisted, a twisted thread is preferred from the viewpoint of strength. On the other hand, in order to efficiently separate a garment into its constituent parts, a faster alkali reduction rate is preferred, and the less twist there is, the faster the alkali reduction rate becomes. Therefore, a non-twisted thread is preferred from the viewpoint of alkali solubility. The choice of non-twisted thread or twisted thread can be made depending on the purpose of the sewing thread.
[0033] The sewing thread may be made of only one thread, but from the viewpoint of increasing the strength of the sewing thread, it is preferable to combine multiple threads. Specifically, various types can be selected depending on the purpose, such as preparing multiple threads and simply drawing them together, or drawing them together and twisting them. The thread prepared in this case may be a non-twisted thread, but from the viewpoint of increasing the strength, it is preferable to use a twisted thread. In addition, multiple threads that have been twisted while being drawn together may be prepared, and these may be further twisted.
[0034] When the sewing thread of the present invention is a filament yarn, the filament yarn may be in the form of raw silk, false twisted yarn, mixed yarn, etc. In the case of a mixed yarn, an interlaced mixed yarn, a taslan textured yarn, etc. may be used. Also, a false twisted mixed yarn which is false twisted and mixed may be used.
[0035] In the case where the sewing thread is in the form of a non-twisted yarn, when the sewing thread is made of only one filament yarn, the spun filament yarn may be used as the sewing thread as is, or the false twisted or mixed filament yarn may be used as the sewing thread as is. In either form, the thickness of the filament yarn is preferably 20 to 1500 dtex as described above. In addition, when the filament yarn is combined to make the sewing thread, in either form, a plurality of filament yarns, preferably about 2 to 5 filament yarns, each having a thickness of about 20 to 200 dtex, are prepared, and these are pulled together using a winder or the like.
[0036] On the other hand, when the sewing thread is in the form of a twisted thread, it may be composed of only one filament thread. In this case, the twist direction is preferably the Z direction in either form, and the twist number is preferably about 100 to 1800 T / m. In the case of doubling, when only the first twist is applied, each filament yarn is first twisted in either form, and then these are drawn together using a winder, etc. In this case, the thickness of each filament yarn is preferably 20 to 200 dtex, and the twist direction is preferably the Z direction.
[0037] When only the upper twist is applied, in either case, a plurality of untwisted filament yarns, preferably about 2 to 5, are simultaneously fed to a ring twister and twisted while being aligned, or a plurality of untwisted filament yarns are combined in a winder and then fed to a double twister for twisting. In this case, the thickness of each filament yarn is preferably 20 to 200 dtex, the twist direction is preferably Z-direction, and the twist number is preferably about 100 to 1800 T / m.
[0038] Furthermore, when applying the final twist and the first twist, a plurality of untwisted filament yarns, preferably with a thickness of about 20 to 200 dtex, are prepared, each of which is first twisted in the S direction at about 100 to 1500 T / m, and then a final twist of about 0.5 to 0.9 times the first twist in the Z direction is applied to each of the first twist. The final twist is preferably performed using a ring twisting machine or the like. When applying the final twist, the first twist, and the intermediate twist, for example, a plurality of filament yarns, preferably 2 to 5 filament yarns, each of which is first twisted in the Z direction and intermediate twisted in the S direction, are prepared, and these are aligned and final twisted in the Z direction at about 100 to 1000 T / m. This provides a sewing thread with excellent sewability.
[0039] Next, when the sewing thread of the present invention is a spun yarn, any type of spun yarn may be used, such as ring spun yarn, open-end spun yarn, or bundled spun yarn, and it may have a core-sheath structure, such as a multi-layered yarn, or may be one that has been subjected to a fluff-suppressing process, such as a compact spun yarn.
[0040] In the case of spun yarn, the sewing thread may be made of only one spun yarn, and the thickness in this case is preferably 4 to 200 (British cotton count) as described above. The twist direction is preferably the Z direction, and the twist number is preferably about 100 to 2000 T / m.
[0041] When doubling spun yarns to make sewing threads, if only first twisting is required, it is sufficient to prepare multiple pieces of spun yarns, preferably about 2 to 5 pieces, each having a thickness of 10 to 60 (British cotton count) and a twist of about 100 to 2000 T / m in the Z direction, and then align them using a winder or the like.
[0042] When applying the final twist and the first twist, it is preferable to prepare multiple spun yarns with a count of 10 to 60 (British cotton count) and a first twist of about 100 to 2000 T / m in the S direction, and then give a final twist of about 0.5 to 0.9 times the first twist in the Z direction. The final twist is preferably performed using a ring twisting machine as described above.
[0043] Furthermore, when applying final twist, primary twist and medium twist, multiple pieces of spun yarn, preferably 2 to 5 pieces, each having a primary twist in the Z direction and a medium twist in the S direction are prepared, and these are aligned and final twisted in the Z direction to obtain the desired sewing thread.
[0044] When the sewing thread of the present invention is a long and short composite thread, for example, one obtained by simultaneously spinning a filament thread in the core and a staple roving in the sheath can be used. In the case of a long and short composite yarn, like the filament yarn and spun yarn, the sewing thread may be made of only one yarn, or multiple yarns may be combined to make the sewing thread. When a long and short composite yarn is used to make a sewing thread, the thickness, number of twists, etc. may basically be the same as those of the above-mentioned spun yarn.
[0045] The sewing thread of the present invention is both highly soluble in alkali and resistant to industrial washing. The term "alkali solubility" refers to the ability to be easily dissolved in a strong alkaline aqueous solution, and as an indicator of this, the sewing thread of the present invention must satisfy a specific weight loss rate when subjected to an alkaline weight loss treatment at 100°C for 30 minutes using an alkaline aqueous solution with a concentration of 20 g / L. Specifically, the weight loss rate must be 50% or more, preferably 60% or more, more preferably 70% or more, even more preferably 80% or more, and most preferably 90% or more.
[0046] When the weight loss rate reaches 50% or more, the sewing thread becomes easily broken with even a small amount of force. This makes it possible to greatly simplify the task of separating the garment into its constituent parts during recycling. In addition, when the strength retention rate is 25% or less after alkaline weight loss treatment at 100°C for 30 minutes using an alkaline aqueous solution with a concentration of 20g / L, the thread tends to break even more easily.
[0047] The conditions of the alkali weight reduction treatment adopted in the present invention (concentration 20g / L, 30 minutes at 100°C) are those that take into consideration the reduction of environmental load and subsequent recycling. In other words, it is not enough for the sewing thread to simply have alkali solubility, but the desired alkali solubility must be achieved while suppressing damage to the clothing components caused by the alkali aqueous solution while suppressing the environmental load. For example, if the concentration of the alkaline aqueous solution is increased, the alkali solubility is promoted accordingly, but this increases the amount of neutralizing agent required in wastewater treatment, which increases the environmental load. In addition, if the clothing components contain, for example, polyester fibers, the elution of the fibers will also progress, resulting in a reduction in the total amount of materials that can be recycled. Therefore, it is necessary to realize the desired alkali solubility under not too severe conditions of concentration 20g / L, 30 minutes at 100°C.
[0048] On the other hand, in terms of industrial washing resistance, the strength retention after 50 washes must be 70% or more, more preferably 75% or more, and even more preferably 80% or more. This makes it possible to apply the material to a wide range of textile products, not only for general clothing but also for uniform clothing that requires industrial washing every time it is worn, since the strength of the sewing thread is unlikely to decrease during washing. Industrial washing is applied to washing uniforms and the like, and is carried out under stricter conditions than household washing, such as using a high-temperature alkaline bath.
[0049] The conditions for the industrial washing in the present invention are as follows: the steps shown in Table 1 are performed according to the conditions for each step (temperature, amount of water, time, detergent, amount of detergent added). The detergent used is "Bioharvest (product name)" manufactured by Kao Professional Services.
[0050] First, the clothes are washed at room temperature in pre-wash 1, and then the water temperature is raised without draining, and pre-wash 2 is washed with warm water at a temperature of 35 degrees. The washing liquid can be prepared as an alkaline bath with a pH of about 10.0±1.0 by adding water and detergent as shown in Table 1. Next, the water is replaced and the clothes are washed. The bath ratio (detergent:water) is 1:30 for both pre-wash and main wash. Next, water is poured while maintaining the water level until the water temperature reaches 40°C, and from that point on the clothes are cooled down for 5 minutes. The water is then replaced and soak rinse 1 is performed, and then soak rinse is performed with the water replaced each time in rinses 2 to 5. The clothes are then dehydrated and dried.
[0051] [Table 1]
[0052] In the present invention, the strength retention rate after 50 industrial washes is evaluated based on the strength retention rate after 50 repeated washes as shown in Table 1, but repeating the washes 50 times is quite a cumbersome task. Therefore, in the present invention, the strength retention rate of the sewing thread after 50 industrial washes is measured by assuming that repeating the steps shown in Table 2 5 times has the same washing effect as repeating the washes shown in Table 1 50 times.
[0053] [Table 2]
[0054] As described above, according to the present invention, a sewing thread that can be easily dissolved in a strong alkaline aqueous solution while being sufficiently resistant to repeated industrial washing can be provided. This makes it possible to apply the sewing thread to not only general clothing but also uniform clothing that requires industrial washing every time it is worn. Any type of sewing thread can be used, such as sewing machine thread or hand sewing thread.
[0055] Furthermore, from the viewpoint of preventing puckering when subjected to heat from an iron after sewing, the sewing thread of the present invention preferably has a dry heat shrinkage of 5% or less when dry-heat treated for 10 minutes at 160° C. and a hot-water shrinkage of 3% or less when hot-water treated for 20 minutes at 100° C. The methods for measuring the dry heat shrinkage and hot-water shrinkage will be described in detail in the Examples.
[0056] The sewing thread of the present invention is preferably made of polyester resin, which gives it an excellent glossiness inherent to polyester resin, and allows stitches to be finished with a good appearance. In addition, the polyester sewing thread also exhibits heat resistance. As a result, the sewing thread can withstand not only the frictional heat caused by the rotation of a sewing machine when used as a sewing thread, but also the heat caused by autoclave treatment (high-pressure steam sterilization treatment) that is carried out at the same time as industrial washing of medical clothing, etc.
[0057] Next, a method for producing the sewing thread of the present invention will be described. The above-mentioned alkali-soluble resin is melt spun by a known means to form a multifilament or staple fiber yarn, and the yarn can be processed into the above-mentioned filament yarn, spun yarn, or long and short composite yarn to form the desired sewing thread.
[0058] Here, a method for producing a sewing thread in the case of obtaining a multifilament using a copolymerized polyester resin containing the above-mentioned specific component will be described. First, the copolymerized polyester resin is produced through a polymerization process, and the obtained copolymerized polyester resin is chipped, and the chips are dried and melt-spun to obtain a multifilament. The conditions for melt spinning include a spinning temperature of 270 to 300°C, a spinning speed of 1000 to 2000 m / min, a drawing temperature of 65 to 85°C, a heat setting temperature of 120 to 160°C, and a drawing speed of 300 to 1000 m / min, and the drawing ratio may be about 0.25 to 0.45 times the maximum drawing ratio of the undrawn yarn. The conditions for spinning and drawing are not limited to the above, and the POY method in which a semi-undrawn yarn is wound by high-speed spinning at 2000 m / min or more, or a spin-draw method in which a high-speed spinning at 2000 m / min or more is performed and drawn continuously without being wound once, can be appropriately used. Thereafter, the resulting multifilament is twisted in the Z direction at 300 to 800 T / M using a double twister, and the twist is set at 50 to 100° C. for about 30 minutes to obtain the sewing thread of the present invention. EXAMPLES
[0059] The present invention will now be described in detail with reference to examples. The characteristics of the sewing thread were measured by the following methods. 1. Strength retention after 50 industrial washes First, the obtained sewing thread was tubularly knitted to prepare a 200 g washable sample. The washed sample and a guide fabric (knitted fabric made of polyester fibers, basis weight: 300 g / m 2 ) was placed in an industrial washing machine, and the process shown in Table 2 was repeated five times under the conditions shown in Table 2. Next, the sewing thread before cylindrical knitting and the sewing thread carefully removed from the washed sample after washing were prepared, and the tensile strength of the sewing thread was measured based on JIS L1013 8.5.1 when the sewing thread was in the form of filament yarn, and based on JIS L1095 9.5.1 when the sewing thread was in the form of spun yarn. Then, the strength retention was calculated using the following formula. Strength retention rate (%) = (tensile strength after washing (mN) / tensile strength before tubular knitting (mN)) x 100
[0060] 2. Weight loss rate and strength retention rate when treated with alkali First, the obtained sewing thread was woven into a cylindrical shape to prepare a weight loss sample, which was then weighed. Next, the weight loss sample was sealed in a cylindrical container together with a 20 g / L aqueous sodium hydroxide solution in a bath ratio of 1:50 (weight loss sample: aqueous sodium hydroxide solution). Next, the container was immersed in an oil bath heated to 100°C with the longitudinal direction of the container horizontal, so that about half of the container was submerged, and rotated 20 times in one circumferential direction at a speed of 1 rotation / second, and then reversed the same number of times at the same speed. After repeating this for 30 minutes, the cylindrical container was lifted from the oil bath, and the sample was removed from the container. The sample was then carefully washed with water, placed on a flat table, and dried at room temperature. The weight loss sample after drying was then weighed, and the weight loss rate was calculated using the following formula. Weight loss rate (%) = (mass before alkali reduction (g) - mass after alkali reduction (g)) / mass before alkali reduction (g) x 100 Furthermore, the sewing thread before tubular knitting and the sewing thread carefully removed from the weight-reduced sample after weight reduction were prepared, and the strength retention rate was calculated in the same manner as in "1. Strength retention rate after 50 industrial washes" above. Strength retention rate (%) = (tensile strength after weight reduction (mN) / tensile strength before tubular knitting (mN)) x 100
[0061] 3. Copolymer component content Measurements were performed using a nuclear magnetic resonance device "ECA500 (trade name)" (room temperature probe) manufactured by JEOL Ltd. 15 mg of suture and 0.7 mL of trifluoroacetic acid were placed in a test tube, and a measurement solution was prepared by ultrasonic treatment and stirring at room temperature for 30 minutes. 1 H, Measured at a measurement frequency of 500 MHZ.
[0062] Example 1 We prepared a copolymer polyester resin chip whose main repeating unit is ethylene terephthalate, containing 97.4 mol% terephthalic acid (TPA), 2.2 mol% 5-sodium sulfoisophthalic acid (SIPM), and 0.4 mol% isophthalic acid (IPA) relative to 100 mol% of the acid components of the entire polyester, and 93.6 mol% ethylene glycol (EG), 6.0 mol% diethylene glycol (DEG), and 0.4 mol% polyethylene glycol (PEG) with a number average molecular weight of 4000 relative to 100 mol% of the glycol components of the entire polyester.
[0063] The chips were then dried and fed into a spinning machine equipped with a spinneret, and melt spun from a 36-hole round cross-section spinneret at a spinning temperature of 290°C and a spinning speed of 1600 m / min to obtain an undrawn yarn, which was then drawn at a drawing speed of 600 m / min, a drawing temperature of 78°C, a heat treatment temperature of 150°C, and a maximum draw ratio of 0.720 to obtain a polyester fiber yarn of 56 dtex 36f. Thereafter, the polyester fiber yarn was twisted in the Z direction at 500 T / M using a double twister, and the twist was set at 70° C. for 30 minutes to obtain a sewing thread of the present invention.
[0064] Example 2 The polylactic acid chips were melt spun at a spinning temperature of 210°C and a spinning speed of 3000 m / min to obtain an undrawn yarn, which was then drawn at a drawing speed of 700 m / min, a drawing temperature of 70°C, a heat treatment temperature of 110°C, and a draw ratio of 1.26 to produce a polylactic acid fiber yarn of 56 dtex and 36 f. Thereafter, the same procedure as in Example 1 was carried out to obtain a suture of the present invention.
[0065] Example 3 We prepared a copolymer polyester resin chip whose main repeating unit is ethylene terephthalate, containing 98.0 mol % terephthalic acid (TPA) and 2.0 mol % 5-sodium sulfoisophthalic acid (SIPM) relative to 100 mol % of the acid components of the entire polyester, and containing 96.7 mol % ethylene glycol (EG), 3.1 mol % diethylene glycol (DEG), and 0.2 mol % polyethylene glycol (PEG) with a number average molecular weight of 6000 relative to 100 mol % of the glycol components of the entire polyester.
[0066] The chips were then dried and placed in a spinning device equipped with a spinneret. The chips were then melt spun from a 36-hole round cross-section spinneret at a spinning temperature of 280°C and a spinning speed of 1100 m / min to obtain an undrawn yarn, which was then drawn at a drawing speed of 361 m / min, a drawing temperature of 75°C, a heat treatment temperature of 140°C, and a maximum draw ratio of 0.333 to obtain a polyester fiber yarn of 56 dtex 36f. The subsequent steps were carried out in the same manner as in Example 1 to obtain a sewing thread of the present invention.
[0067] Comparative Example 1 A polyester resin chip was prepared containing 100 mol % terephthalic acid when the total amount of all acid components constituting the polyester is 100 mol %, and 100 mol % ethylene glycol when the total amount of all glycol components constituting the polyester is 100 mol %. A polyester fiber yarn was obtained in the same manner as in Example 1, except that the spinning speed was set to 1200 m / min using the above chip and the thickness of the polyester fiber yarn was set to 84 dtex 36f. Thereafter, the polyester fiber yarn was twisted in the Z direction at 400 T / M using a double twister, and the twist was set at 70° C. for 30 minutes to obtain a sewing thread of the present invention.
[0068] Example 4 The 56 dtex 36 f polyester fiber yarn obtained in Example 1 was cut to 3.8 mm to produce staple fibers (synthetic cotton), which were then spun in a conventional manner to produce a 40-count spun yarn having a first twist of 950 T / M in the S direction. Next, three of these spun yarns were twisted together to obtain a sewing yarn count of 40 having a top twist of 650 T / M in the Z direction.
[0069] Comparative Example 2 The 84 dtex 36 f polyester fiber yarn obtained in Comparative Example 1 was cut to 3.8 mm to produce short fibers (synthetic cotton), which were then spun in a conventional manner to produce a spun yarn of 50 count with a first twist of 1050 T / M in the S direction. Subsequently, three of these spun yarns were twisted together to obtain a sewing yarn count of 50 having a top twist of 700 T / M in the Z direction.
[0070] The property values of the sewing threads obtained in Examples 1 to 4 and Comparative Examples 1 and 2 are shown in Table 3.
[0071] [Table 3]
[0072] As is clear from Table 3, the sewing threads obtained in Examples 1 to 4 had high strength retention after 50 industrial washings, and when subjected to an alkali weight loss treatment, the weight loss rate was 50% or more. On the other hand, the sewing threads obtained in Comparative Examples 1 and 2 had a low weight loss rate due to the alkali weight loss treatment, and were not suitable for use in the recycling applications targeted by the present invention.
[0073] The sewability of the sewing threads was evaluated by sewing five layers of cotton plain weave fabric (warp and weft count 30, warp density 78 threads / 2.54 cm, weft density 72 threads / 2.54 cm) at a sewing speed of 4500 spm and stitch pitch of 2 mm using a lockstitch sewing machine (JUKI "DDL-5530N (product name)"). The sewing was performed in a straight line with a length of 1 m, and five tests were performed for each sewing thread. As a result, no thread breakage or skipped stitches were observed in any of the sewing threads obtained in Examples 1 to 4, and the sewing properties were good.
Claims
1. A sewing thread comprising at least one of long fibers or short fibers formed of an alkali-soluble resin, the thread having a strength retention rate of 70% or more after 50 industrial washes, and a weight loss rate of 50% or more when subjected to an alkali weight loss treatment at 100°C for 30 minutes using an alkaline aqueous solution having a concentration of 20 g / L.
2. 2. The sewing thread according to claim 1, wherein the alkali-soluble resin is a polylactic acid resin.
3. 2. The sewing thread according to claim 1, wherein the alkali-soluble resin is a copolymer polyester resin which, when the total amount of all acid components constituting the polyester is taken as 100 mol %, contains 80 mol % or more of terephthalic acid and 0.5 to 5 mol % of an aromatic dicarboxylic acid having a metal sulfonate group, and, when the total amount of all glycol components constituting the polyester is taken as 100 mol %, contains 80 mol % or more of ethylene glycol and 0.1 to 1.0 mol % of a polyether compound.
Citation Information
Patent Citations
Clothes
JP1995216615A
Clothing having structural part made of soluble fiber yarn in its part
JP1996081811A