Matting agent based on precipitated silica

A precipitated silica with tailored properties addresses the challenges of maintaining gloss and clarity in matte coatings by reducing the amount used and enhancing dispersibility, resulting in efficient and cost-effective matte finishes.

JP2024160954APending Publication Date: 2024-11-15EVONIK OPERATIONS GMBH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024068903
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-05
Filing Date
2024-04-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing matting agents based on precipitated silica face challenges in maintaining gloss levels, clarity, and dispersibility without causing a grainy feel, particularly due to the tendency of fine particles to reagglomerate, which affects their efficiency and economic viability.

Method used

A precipitated silica with specific physicochemical parameters, including BET surface area, DOA, particle size distribution, and pore volume, is developed to reduce the amount used while maintaining gloss levels and improving dispersibility and transparency, characterized by a narrow particle size distribution and unique morphology.

Benefits of technology

The new silica reduces the amount needed for achieving desired gloss levels, enhances transparency, and improves dispersibility, leading to more efficient and cost-effective matte coatings with reduced reagglomeration tendencies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160954000001_ABST
    Figure 2024160954000001_ABST
Patent Text Reader

Abstract

To provide a matting agent capable of reducing the amount thereof to be used while keeping the level of glossiness without adversely affecting transparency, dispersibility, and / or the haptic characteristic.SOLUTION: A matting agent is to be based on precipitated silica specifically formed using the following physicochemical parameters. BET measured in accordance with ISO 9277 is 150 m2 / g to 400 m2 / g, preferably 200 m2 / g to 300 m2 / g, DOA measured in accordance with ISO 19246 is 220 mL / 100 g to 400 mL / 100 g, preferably 250 mL / 100 g to 350 mL / 100 g, d50 measured in accordance with ISO 13320 of Laser diffraction methods using CoulterLS is 3.0 μm to 5.0 μm, the ratio of particle sizes of d5:d50:d95 is >0.3:1:<2, and a particle size distribution is 1.3 to 1.7.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a matting agent based on precipitated silica, to a process for its preparation and to its use in paints and coatings. [Background technology]

[0002] Coatings are applied to surfaces or substrates for decorative, functional or protective purposes. They decorate, protect and preserve materials such as wood, metal or plastic. Coatings can be very glossy or matte.

[0003] It was once true that coatings such as paints and printing inks were then made matte by controllably roughening the surface in the microscale range. As a result, light incident on a rough surface is diffusely scattered rather than being reflected in one direction. The more diffusely the light is scattered, the more matte the surface appears to the human eye.

[0004] Nowadays, matting agents are used and incorporated into paint systems. They usually consist of precipitated or fumed silica, silica gel, polymethylurea, or waxes. There are many demands on matting agents. Thus, they must have a good matting effect, but must not adversely affect the tactile properties and / or transparency of the paint film surface. In addition, they must have good dispersibility in the paint production.

[0005] It should be possible to impart various levels of matt finish to the paint film surface, ranging from a silky matt to a dull matt appearance, without the surface appearing rough. Thus, the roughness of the matt surface is also determined by the particle size and shape of the matting agent. With a coarse matting agent, the paint film surface will appear matte but rough.

[0006] Matting agents are based on the effect of silica particles protruding from the surface, which form a microstructure when dry. Light rays are scattered in all directions at the resulting peaks and valleys. An established method to quantify the degree of matte / gloss is to measure the reflected light component at an angle of 60°.

[0007] Coarse particles are generally easier to disperse than finely divided particles because a much larger surface area must be wetted for fine particles, and fine particles have a much higher tendency to re-agglomerate due to their high surface energy. Summary of the Invention [Problem to be solved by the invention]

[0008] Avoiding or reducing this tendency is particularly important in paint manufacturing, so it would be desirable to provide a matting agent whose amount can be reduced while maintaining a constant gloss level, without adversely affecting transparency, dispersibility, and / or tactile properties. [Means for solving the problem]

[0009] The present invention therefore provides a precipitated silica characterized by the following physicochemical parameters: - BET measured according to ISO 9277 is 150m 2 / g~400m 2 / g, preferably 200m 2 / g~300m 2 / g. - DOA measured according to ISO 19246 is between 220 mL / 100 g and 400 mL / 100 g, preferably between 250 mL / 100 g and 350 mL / 100 g. - d measured according to ISO 13320 by laser diffraction method using Coulter LS 50 is 3.0μm~5.0μm. - Particle size ratio d5:d 50 :d 95 is >0.3:1:<2. -Particle size distribution:

[0010]

number

[0011] is 1.3 to 1.7.

[0012] The average particle size of the precipitated silica according to the invention can be measured by laser diffraction particle size analysis in accordance with ISO 13320:2009. The measured particle size distribution is determined by dividing the average particle size by the median d 50 Used to define

[0013] The specific surface area (also simply called the BET surface area) is determined by nitrogen adsorption according to the Brunauer-Emmett-Teller method in accordance with DIN 9277:2014.

[0014] The DOA absorption value is measured by an absorptometer equipped with a torque measurement and processing system. It can be used to evaluate the liquid absorption capacity of silicon dioxide, calcium silicate, and sodium aluminosilicate. The daily absorption value is an indication of the carrier capacity of the filler.

[0015] Experience has shown that to achieve the same gloss level, larger amounts of smaller particle size precipitated silica are required than larger particle size precipitated silica.

[0016] Unexpectedly, it has been found that the amount of precipitated silica according to the invention can be reduced in comparison with commercially available fine matting agents, for example in various coating systems over a wide range of gloss levels, measured at an angle of 60°, see the examples.

[0017] The reduced use of precipitated silica according to the invention also constitutes an important product attribute with regard to efficiency (economic viability): the more efficient the silica, the less it needs to be used in the corresponding coating system to achieve a given gloss level.

[0018] Furthermore, it was found that the transparency of the clear coat could be increased. The density Dy (transparency) of the matte clear coat was measured with an X-Rite eXact densitometer according to DIN 55988. The matte clear coats of different paint systems were applied to a black PMMA sheet and adjusted to the same gloss level considered in the particular case, measured at 60°, to compare the different matting agents. The transparency was then ascertained by diffuse reflection at an angle of 45° by numerical calculation. The measurement parameters were set as follows:

[0019] [Table 1]

[0020] It should be noted that the transparency of matte clearcoat systems can only be compared to each other if the gloss levels are the same. Comparisons at equal silica dosages are not permitted. The measured transparency value Dy is a logarithmic value. Thus, the higher the Dy value, the more transparent the matte clearcoat.

[0021] The average pore size of the precipitated silica according to the invention is preferably less than 7.0 μm, preferably less than 5.0 μm, more preferably less than 3.0 μm, measured on an Autopore IV 9520 according to ISO 15901-1 using instrument settings of a contact angle of 140° and a pressure range of 0.003-420 MPa, in the pore size range of 3.5 nm to 500 μm after grinding of the silica.

[0022] The silica according to the invention preferably has a unique morphology, in particular its porosity, as measured by mercury porosimetry.

[0023] The precipitated silica according to the present invention preferably has a pore volume measured by Hg porosimetry of 2.40 mL / g Hg (d=0.1 μm to d=3.0 μm) to 2.90 mL / g Hg (d=0.1 μm to d=3.0 μm).

[0024] The precipitated silica according to the present invention preferably has a pore volume measured by Hg porosimetry of 2.40 mL / g Hg (d=0.1 μm to d=4.0 μm) to 3.10 mL / g Hg (d=0.1 μm to d=4.0 μm).

[0025] The precipitated silica according to the present invention preferably has a pore volume measured by Hg porosimetry of 2.50 mL / g Hg (d=0.1 μm to d=5.0 μm) to 3.30 mL / g Hg (d=0.1 μm to d=5.0 μm).

[0026] The measurement of the Hg pore size (d<4 μm or d<5 μm) is based on mercury intrusion according to DIN 66133, using an AutoPore V 9600 instrument from Micromeritics. The method principle is based on measuring the volume of mercury injected into the porous solid as a function of the applied pressure.

[0027] Figure 4 shows a graph of the measurement of pore volume by Hg porosimetry. It shows, for example, the unique morphology of the silica K2 of the present invention. The vertical lines at d=0.1 μm and d=4.0 μm represent the region designated for the present invention. The difference in cumulative pore volume (mL / g) represents the pore volume of this region (see Table C). For calculation, the intersection of each vertical line with the graph is read and calculated.

[0028] Furthermore, from the graph, it can be deduced that in the region of pore diameter d<1 μm, the cumulative pore volume is 4.9 mL / g. For this purpose, a vertical dotted line is set at d=1 μm. The value of the intersection with the graph can be read off. For pore volumes below 4.9 mL / g, the graph shows a flatter progression, resulting in a smaller pore volume for the silica particles.

[0029] The silicas according to the invention have a much smaller average pore size than comparable commercial silicas used as matting agents. They have been found to be able to absorb more mercury despite the much smaller pore size. The larger number of smaller pores on average has an important advantage in terms of transparency, which is particularly important in the case of water-based paint systems.

[0030] Figure 1 shows an SEM image of a cross section of a clearcoat coating loaded with silica particles. The morphology or porosity of the silica allows it to act like a sponge, filled throughout with a transparent binder. The refractive index of the binder and silica are similar, so the matte clearcoat remains nearly transparent after drying.

[0031] Aqueous binders are dispersions of polymer particles in an aqueous phase. The diameter of the spherical polymer particles ranges from tens of nanometers to several micrometers. As the paint film dries, the water and all co-solvents evaporate, reducing the volume and the dispersion begins to solidify. The dispersion particles move closer and closer to each other and eventually begin to fuse together. This is called coalescence. At the end of coalescence, a homogeneous binder film is formed in which the binder particle boundaries disappear. The binder particles can efficiently penetrate the numerous pores and form a film within the pores. The greater the number of pores, the more the refractive index difference between the silica and the binder is blurred, improving the transparency. This has been confirmed in the case of the silica according to the invention in the corresponding binder system.

[0032] The dispersion of the precipitated silica according to the invention in various paint systems is also surprisingly improved. Dispersibility can be measured indirectly using a grindometer. The measurement with the grindometer is carried out according to DIN EN ISO 1524. This correlates with the formation of spots in the dry paint film, so that the grindometer can be used to recognize undesirable spots or spots that are too large. Furthermore, this method also makes it possible to recognize the tendency of precipitated silica to re-agglomerate, which often increases as the particle size distribution decreases. See figures 2 and 3.

[0033] In the case of many precipitated silicas with d50 values ​​below 5 μm, the silica particles tend to re-agglomerate during storage, which can be recognized by an increase in the number of spots on the grindmeter image over time. Usually, the tendency of untreated silica to re-agglomerate is higher than when the surface is covered with organic matter. In the case of silicas with a high tendency to re-agglomerate, this may occur already after a few days, whereas in the case of silicas with high stability, this may not occur until after several weeks or months. In contrast, this is not observed in the case of silicas according to the invention, thus confirming a very low tendency to form spots. Without being bound by any theory, it is assumed that the particular morphology and pore distribution of the silicas according to the invention not only have a favorable effect on dispersibility, but also on their high stability against re-agglomeration.

[0034] The tapped density of various powdery or coarse granular materials can be measured according to DIN ISO 787-11:1995 "General test methods for pigments and extenders - Part 11: Determination of tapped volume and apparent density after tamping", which involves measuring the bulk density of the bulk material after stirring and tamping.

[0035] For a uniform matt effect, the goal is a very narrow particle size distribution. The particle size distribution can be measured in a simple manner, for example by measuring the d5, d50 and d95 values. Thus, the untreated or wax-coated precipitated silicas according to the invention have a particle size distribution (span) defined by the quotient (d95-d5):d50 of 1.3 to 1.7.

[0036] Further properties include the particle size ratio d5:d 50 :d 95 It is.

[0037] The precipitated silica according to the invention has 50 It is preferable that the thickness is 3.5 to 4.5 μm.

[0038] It is also known to use wax-coated silicas as matting agents, as well as untreated hydrophilic silicas, such wax treatment apparently improving the settling properties of the precipitated silica.

[0039] Thus, the present invention further comprises: BET measured according to ISO 9277 is 150m 2 / g~400m 2 / g, preferably 200m 2 / g~300m 2 / g, DOA measured according to ISO 19246 is 220mL / 100g to 400mL / 100g, preferably 250mL / 100g to 350mL / 100g; d measured according to ISO 13320 by laser diffraction (Coulter LS) 50 is 3.0 μm to 5.0 μm, Particle size ratio d5:d 50 :d 95 is >0.3:1:<2, Particle size distribution:

[0040]

number

[0041] is 1.3 to 1.7, The carbon content, measured according to ISO 3262-19 at LECO, is 1.0 to 6.0% by weight, preferably 2.4 to 3.8% by weight. A wax-coated precipitated silica is provided.

[0042] The procedure for producing the precipitated silica according to the invention is, for example, as follows.

[0043] First, 13.5 m of water was poured into the settling tank at 50°C. 3 of water was added while stirring continuously, and 14.85 ml of commercially available water glass was added. 3 / hour, and the addition is terminated after 10-15 minutes. The mixture is then heated to a temperature of 70°C. Next, 0.27 ml of 96% sulfuric acid is added. 3 / hr within 25-35 minutes and continuously shear and stir while maintaining the temperature at 85°C by closed loop control. After 1.5-3.5 hours, the suspension is acidified with sulfuric acid within 50-80 minutes until the pH is in the range of 3.5-3.9.

[0044] The solids can be separated from the suspension by known filtration operations, for example by filter presses (membrane filter presses). The filter cake, washed with demineralized water, is then dried. For this purpose, many types of drying methods are known to the skilled person (Ullman's Encyclopedia of Industrial Chemistry, 5th Edition, Vol. B1, pp. 7-25, 1992). Advantageous drying operations have been found to be flow dryers, spray dryers, staged dryers, belt dryers, rotary tube dryers, spin flash dryers or drying operations by nozzle towers. More preferably, drying is carried out by means of spray dryers or staged dryers.

[0045] In the spray drying, the filter cake is liquefied with water under the action of shear forces to adjust the solids content to less than 15%, preferably 7.0-14.0%, more preferably 9-12%.

[0046] The precipitated silica obtained after drying can be directly subjected to classification and grinding or, during classification and grinding, it is also possible to coat the silica of the invention with wax at the same time, in which case a coating of 2 to 15% by weight, preferably 5 to 10% by weight, more preferably 3 to 6% by weight, has proven useful.

[0047] In addition to the aforementioned wax impregnation of the silica, other methods for this purpose are also known and can be found, for example, in DE 1006100, DE 1592865 or EP 0922691. The wax suspension is reacted with the silica suspension, optionally via a disperser.

[0048] The desired narrow particle distribution of precipitated silica and the desired d of 3.0-5.0 μm 50 A classifying and grinding operation was carried out using a conventional air jet mill, e.g., Netzsch CGS 50, to obtain

[0049] The untreated or wax-coated precipitated silicas according to the invention can be used as matting agents in paints or coatings, in particular in the manufacture of dispersions, millbases, paints, coatings or printing inks, inkjet inks, grind resins, pigment concentrates, colorants, pigment preparations, filler preparations or coating compositions.

[0050] The following examples are intended to further clarify the invention and are not intended to limit the scope of protection claimed.

[0051] method The tapped density [g / L] was determined according to DIN ISO 787-11:1995. BET specific surface area [m 2 / g] was determined by nitrogen adsorption according to the Brunauer-Emmett-Teller method according to DIN 9277:2014. The DOA absorption value was measured according to ISO 19246 using a Brabender absorptometer equipped with torque measurement and processing system. It can be used to evaluate the liquid absorption capacity of silicon dioxide, calcium silicate, and sodium aluminosilicate. The daily absorption value is an indication of the carrier capacity of the filler. The density Dy (transparency) of the matte clear coats was measured with an X-Rite eXact densitometer according to DIN 55988. The matte clear coats of the various paint systems were applied to black PMMA sheets and the various matting agents were compared, always adjusted to the same gloss level considered in the particular case, measured at 60°. The transparency was then ascertained by diffuse reflection at an angle of 45° by logarithmic calculation. The measurement parameters were set as follows:

[0052] [Table 2]

[0053] Grindometer measurements are in accordance with DIN EN ISO 1524.

[0054] The dispersion characteristics of various matting agents were evaluated using a black melamine stoving lacquer and a Labman TIDAS instrument for automated grindmeter drawdown to measure the fineness of dispersion.

[0055] To produce the grindometer images shown in Figures 2 and 3, a black medium solid stoving lacquer (DUPLEX D 1326, formulation number: B11830875) from AXALTA Coating Systems Austria GmbH was used together with the appropriate V0003 thinner (from Axalta). The appropriate amount of precipitated silica required to adjust the gloss level of the dried paint layer to 20 GU, measured at an angle of 60°, was stirred into 100 g of paint using a paddle stirrer at 2000 rpm for 10 minutes. The paint was then applied in liquid form to a grindometer block with a maximum groove depth of 70 μm, automatically applied by knife coating and evaluated with a TIDAS instrument.

[0056] The carbon content [wt.%] was determined according to EN ISO3262-20:2000 (chapter 8) by elemental analysis with a C632 carbon measurement system (manufacturer: LECO). The analyzed samples were weighed into ceramic crucibles, mixed with combustion additives and heated in an induction furnace under oxygen flow. The carbon present was oxidized to CO2. The amount of CO2 gas was quantified by an infrared detector (IR). If SiC is present, it does not burn and therefore does not affect the value of the carbon content.

[0057] The measurements of Hg pore volume (d<4 μm, d<5 μm) were carried out based on mercury intrusion according to DIN 15901-1 using a Micromeritics AutoPore V 9520 instrument. The instrument settings were a contact angle of 140°, a pressure range of 0.003-420 MPa, and after crushing of the silica, pore sizes in the range 3.5 nm-500 μm were measured. [Brief description of the drawings]

[0058] [Figure 1] FIG. 1 shows an SEM image of a cross section of a clearcoat coating loaded with silica particles. [Diagram 2] Figure 2 shows the grindometer images of K1 and K2. [Diagram 3] FIG. 3 shows grindometer images of VG1 and VG2. [Figure 4] 1 shows a graph of pore volume measurement by Hg porosimeter. EXAMPLES

[0059] 1. Preparation of the Precipitated Silicas K1 and K2 of the Invention 20m 3 First, 13.5 m of sewage was poured into the settling tank at a temperature of 50°C. 3 of water was added while stirring continuously, and 14.85 ml of commercially available water glass (SiO2: 27.1%, Na2O: 8.07%, concentration: 1.335) was added. 3 / hr, and the addition was terminated after 13 minutes. The mixture was then heated to a temperature of 70°C. Next, 0.27 ml of 96% sulfuric acid was added. 3 / h was added within 30 min and constantly sheared and stirred while the temperature was maintained at 85 °C by closed loop control. After 120 min, the suspension was acidified again with sulfuric acid within 60 min until the pH reached a value in the range of 3.5-3.9. The solids were separated from the suspension using a membrane filter press and the filter cake was washed with demineralized water and then dried in a spray dryer. For spray drying, the filter cake was liquefied with water under the action of shear forces and the solids content was adjusted to 10%.

[0060] The dried precipitated silica according to the invention was milled and classified according to the desired particle size distribution using a Netzsch CGS 50 air jet mill.

[0061] K1 is an untreated silica according to the invention having the physicochemical properties of Tables AC.

[0062] K2 was produced in the same manner, and during classification and grinding in a mill, the surface of K2 was covered with a commercially available PE wax, and the amount of wax was adjusted so that the carbon content measured by a LECO elemental analyzer was 3.4%. The physicochemical indices of K2 are also clear from Tables A to C.

[0063] The comparative example cited is a commercially available precipitated silica from Tosho.

[0064] [Table A]

[0065] [Table B]

[0066] [Table C]

[0067] Tables A to C show the physicochemical parameters of the precipitated silica according to the invention and the comparative silicas VG1 and VG2. K1 is an untreated precipitated silica according to the invention. K2 is a wax-treated precipitated silica according to the invention. The comparative examples VG1 and VG2 are precipitated silicas manufactured by Tosoh under the trade names Nipsil E-1011 (organically post-treated according to the data sheet) (VG2) and Nipsil E-220A (VG1). The average particle size of these commercially available precipitated silicas is d = 0.01, similar to K1 and K2. 50 VG1 and VG2 are known to be used as matting additives.

[0068] The precipitated silicas K1 and K2 of the present invention showed much higher DOA values ​​compared to VG1 and VG2 from Tosoh having comparable particle size distributions (see Table A).

[0069] The specific porosity of the silicas K1 and K2 according to the invention could be demonstrated by mercury porosimetry. The corresponding values ​​are given in Table C.

[0070] The average pore size of the silicas K1 and K2 according to the invention was about 2.8 μm, much smaller than the 8.9 μm of precipitated Nipsil E 1011 (VG2) and 8.0 μm of Nipsil E-220A (VG1). Nevertheless, K1 and K2 were able to absorb more mercury within the pore ranges of 0.1-3.0 μm, 0.1-4.0 μm, and 0.1-5.0 μm. The higher number of smaller pores on average provides a decisive advantage in terms of transparency, especially in the case of water-based paint systems.

[0071] 2.Paint system manufacturing Various paint systems were prepared for paint testing.

[0072] 2.1 Paint system 1:2K PUR paint (DD paint) Solvent-based 2K PUR paints were prepared according to the details in Table 1. Table 1: Paint system 1

[0073] [Table 1]

[0074] The individual paint ingredients were weighed out stepwise in the order listed above and homogenized in a laboratory dissolver. Homogenization was required after each of items 4, 5, 6, and 7. A final homogenization of the paint was performed after item 8.

[0075] 2.2 Paint system 2:1K PU acrylate, wb (clear coat) A water-based 1K PU acrylate coating was prepared according to the details in Table 2. Table 2: Paint system 2

[0076] [Table 2]

[0077] Premix 1 was prepared from items 6 and 7 by adding AMP95 to adjust the pH to 8.5-9.0. Premix 2 was prepared similarly from items 6 and 7. Then, item 1 was charged first and premix 1 was added while stirring. Items 4 and 5 were added successively, followed by premix 2. Finally, the clear coat was homogenized at 1500 rpm for 10 minutes and placed in a closed container.

[0078] 2.3 Paint system 3:1K acrylate, wb (clear coat) A water-based 1K acrylate paint was prepared according to the details in Table 3. Table 3: Paint system 3

[0079] [Table 3]

[0080] The pH was adjusted to 8.5-9.0 by adding AMP95 and a premix was prepared from items 4 and 5. Item 1 was charged first and the premix was added while stirring. After sequential addition of items 2 and 3, the clearcoat was homogenized at 1500 rpm for 10 minutes and placed in a closed container.

[0081] 3 Application of coating system and evaluation of surface properties 3.1 Incorporation of silica into coating systems Paint system 1: Silica was introduced into paint system 1 (100 parts by weight) in a 350 mL PE cup according to the weights in Table 3.1. It was ensured that the silica was introduced properly and did not adhere to the rim of the cup. The matte paint system 1 was then dispersed using a 4.2 cm paddle stirrer at 2000 rpm for 10 minutes.

[0082] Paint system 2: 95 parts by weight of paint system 2 and 5 parts by weight of Dowanol DPM (dipropylene glycol methyl ether, manufactured by Dow Chemical Co.) were mixed with stirring and stirred at 1000 rpm for 5 minutes using a paddle stirrer. The appropriate weight of silica was introduced into the mixture according to Table 3.2, except that the mixture was continuously stirred with a paddle stirrer during the addition of the silica.

[0083] Paint system 3: Silica was introduced as in paint system 2 according to the weights in Table 3.3.

[0084] VG1 and VG2 were introduced as well as the respective paint systems and weights in Tables 3.1 to 3.3.

[0085] 3.2 Application of non-glossy paint systems and evaluation of surface properties After a degassing phase of 30 minutes, each matte paint system was applied onto a black PMMA sheet using a Coatmaster 509 MC film applicator. For this purpose, a box-type coating bar with a gap height of 200 μm was used. The application speed was set at 25 mm / s. The coated PMMA sheets were allowed to dry overnight under climatically controlled conditions of 21-25 °C and 40-60% relative humidity. One day after application, the gloss level at 60 ° and the transparency of the dry matte surface were measured.

[0086] [Table 3.1]

[0087] [Table 3.2]

[0088] [Table 3.3]

[0089] The three paint systems shown are representative of many standard binder systems where a high quality matte surface is desired. Especially in matte coatings, aspects such as transparency and feel play an important role.

[0090] Compared to conventional precipitated silicas, the inventive silicas K1 and K2 showed higher efficiency (economic feasibility) in all three coating systems over the entire gloss range of 20 gloss points measured at 60° angle, down to the deep matt of two gloss values ​​at 60° angle. This means that less silica is needed to achieve the gloss levels shown in Tables 3.1 to 3.3 than with the conventional comparison silicas VG1 and VG2. Comparison of efficiency is only meaningful if the silicas being compared to each other have similar particle size distributions [see Table A (d5, d50, and d95)].

[0091] The inventive silicas K1 and K2 showed higher transparency Dy values ​​compared to conventional silicas in the solvent-based paint system 1 over the gloss range of 20 to 2 gloss points at an angle of 60° (Table 3.1). The two water-based paint systems 2 and 3 (Tables 3.2 and 3.3) also showed higher transparency values ​​overall over the gloss range of 20 to 5 gloss units (at an angle of 60°). It should be noted that the transparency of the matte clearcoat systems 1, 2 and 3 can only be compared if the gloss levels are the same. A comparison with equal loadings of matting agents is not acceptable. The measured transparency Dy values ​​are logarithmic. Thus, the higher the Dy value, the higher the transparency of the matte clearcoat.

[0092] For example, the untreated precipitated silica K1 in a 1K acrylate paint system (paint system 3) has a Dy value of 2.19 at 20 gloss units (angle 60°), whereas the competitive untreated precipitated silica Nipsil E-220A (VG1) has a transparency value of only 2.10. The transparency of K1 is therefore approximately 23% higher. The dark eye can visually discern even a difference of 0.03, as confirmed by measurements.

[0093] This particular porosity of the silicas K1 and K2 according to the invention therefore has a positive effect on the efficiency and transparency in various coating systems.

[0094] 4. Dispersion characteristics measured by a grindmeter Into a 350 mL polyethylene cup, 100 g of DUPLEX D 1326 paint was weighed out and 20 g of V0003 thinner was weighed out. The amount of silica specified in Table 4 was then weighed out and carefully mixed into the diluted test paint with a spatula. The mixture was then dispersed with an O43 mm paddle stirrer at 2000 rpm for 10 minutes while the PE cup was covered to avoid evaporation losses. After mixing in the silica, the matte paint was left to degas in a closed beaker for 30 minutes.

[0095] To ensure comparability of the various silicas, Duplex D 1326 black paints were each adjusted to a gloss level of 20 gloss units (±0.1) measured at an angle of 60° using the matting agents listed in Table 4. The gloss level adjustment was investigated as follows:

[0096] Once degassing was complete, the paints were applied to cleaned glass plates (130 x 90 x 3 mm) using a motorized applicator (Erichsen Coatmaster 509 MC) with a square coating bar with a gap height of 120 μm at a speed of 25 mm / s. The square coating bar was held down with a VA steel block (dimensions: 71 x 30 x 24 mm, weight: approximately 420 g) to increase the applied load. Two glass plates were coated with each dispersion sample. The applied paints were flashed off using fixed flash-off conditions: Temperature: 20℃~25℃ Relative humidity: 40%~60% Flash off time: 10-20 minutes

[0097] The paints were then baked for 20 minutes at 150°C in a circulating paint drying cabinet. The reflectometer values ​​were measured on a BYK Haze Gloss after the glass plates had cooled (after at least 30 minutes). The reflectometer values ​​were taken as the average of two measurements.

[0098] Figure 2 shows the grindometer images of K1 and K2. FIG. 3 shows grindometer images of VG1 and VG2. Table 4: Evaluation of grindometer images

[0099] [Table 4]

[0100] The grindometer images of the inventive silicas K1 and K2 shown in Figures 2 and 3 show values ​​3 μm lower than those of the comparative silicas VG1 and VG2. This is also related to the lower d95% values ​​in Table A, since the grindometer values ​​are determined crucially by the coarse components of the particle aggregate. As in the case of clearcoat systems 1, 2 and 3 above, the inventive silicas also showed a high efficiency in the black pigmented Duplex D 1326 test paint, since less matting agent was added to obtain a gloss level of 20 measured at an angle of 60°. It is also noteworthy that K1 and K2 in Figure 2 have a much narrower transition range and are completely free of spots. In the case of many precipitated silicas with d50 values ​​below 5 μm, the silica particles tend to re-agglomerate during storage, which can be seen in the grindometer images by an increase in the number of spots over time. Untreated silicas usually have a higher tendency to agglomerate than silicas with organic surface coatings. This may be the case already after a few days for silicas with a high tendency to re-agglomeration, and only after weeks or months for those with a high stability.In contrast, this is not observed for the silicas K1 and K2 of the invention, thus confirming a very low tendency to speckle formation.It is assumed that the particular morphology and pore distribution of the silicas K1 and K2 not only has a beneficial effect on dispersibility, but also on their high stability against re-agglomeration.

Claims

1. BET measured according to ISO 9277 is 150m 2 / g to 400m 2 / g, preferably 200m 2 / g to 300m 2 / g, a DOA measured according to ISO 19246 of 220 mL / 100 g to 400 mL / 100 g, preferably 250 mL / 100 g to 350 mL / 100 g; d measured according to ISO 13320 by laser diffraction method using Coulter LS 50 is 3.0 μm to 5.0 μm, Particle size ratio d 5 :d 50 :d 95 is >0.3:1:<2, Particle size distribution: [0010] Precipitated silica, wherein the Mn is 1.3 to 1.

7.

2. 2. A precipitated silica according to claim 1, having an average pore size of less than 7.0 μm, preferably less than 5.0 μm, more preferably less than 3.0 μm, measured according to ISO 15901-1 with an Autopore IV 9520 at an instrument setting of a contact angle of 140° and a pressure range of 0.003-420 MPa, and calculated over the pore size range of 3.5 nm to 500 μm.

3. 3. The precipitated silica of claim 1, having a pore volume measured by Hg porosimetry of greater than 2.40 mL / g (d=0.1 μm to d=4.0 μm) to 3.10 mL / g (d=0.1 μm to d=4.0 μm).

4. 4. The precipitated silica according to claim 1, having a pore volume, measured by Hg porosimetry, of greater than 2.50 mL / g (d=0.1 μm to d=5.0 μm) to 3.30 mL / g (d=0.1 μm to d=5.0 μm).

5. d 50 5. Precipitated silica according to claim 1, wherein the average particle size is between 3.5 and 4.5 μm.

6. 6. Use of the precipitated silica according to any one of claims 1 to 5 as matting agent for the production of dispersions, millbases, paints, coatings or printing inks, inkjet inks, grind resins, pigment concentrates, colorants, pigment preparations, filler preparations or coating compositions.

7. BET measured according to ISO 9277 is 150m 2 / g to 400m 2 / g, preferably 200m 2 / g to 300m 2 / g, a DOA measured according to ISO 19246 of 220 mL / 100 g to 400 mL / 100 g, preferably 250 mL / 100 g to 350 mL / 100 g; d measured according to ISO 13320 by laser diffraction method (Coulter LS) 50 is 3.0 μm to 5.0 μm, Particle size ratio d 5 :d 50 :d 95 is >0.3:1:<2, Particle size distribution: [0025] is 1.3 to 1.7, A wax-coated precipitated silica having a carbon content of 1.0-6.0% by weight, preferably 2.4-3.8% by weight, measured according to ISO 3262-19 at LECO.

8. 8. Use of the precipitated silica according to claim 7 as a matting agent for producing a dispersion, a millbase, a paint, a coating or a printing ink, an inkjet ink, a grind resin, a pigment concentrate, a colorant, a pigment preparation, a filler preparation or a coating composition.