Ink jet ink composition, ink jet recording method, and ink jet recording apparatus
The inkjet ink composition with specific additives and a controlled heating process addresses the issues of smoke and backside transfer in sublimation inks, ensuring effective drying and high-quality image production.
Patent Information
- Application Number
- JP2023078477
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
AI Technical Summary
Sublimation transfer inks containing glycerin evaporate during heating, leading to smoke generation and insufficient drying on the transfer medium, while inks with sugar alcohol have high boiling points, causing image transfer to the backside when wound up.
An inkjet ink composition comprising a sublimable dye, sugar alcohols with 4 or more OH groups, diols with 2 or 3 carbon atoms, glycol monoethers, amides, and (poly)glyceryl ethers, with limited glycerin content (1% or less), along with a specific inkjet recording method and device for heating and peeling processes.
The composition suppresses smoke generation and ensures effective drying on the transfer medium, preventing image transfer to the backside, while maintaining high-quality image production.
Smart Images

Figure 2024162680000001 
Figure 2024162680000002 
Figure 2024162680000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an ink-jet ink composition, an ink-jet recording method, and an ink-jet recording apparatus. [Background technology]
[0002] Inkjet recording is a method of recording by ejecting small droplets of ink from fine nozzles and depositing them on a recording medium. This method has the advantage that it can record high-resolution, high-quality images at high speed using relatively inexpensive equipment. Inkjet recording is also used to dye (print) fabrics.
[0003] As a recording method, there is a transfer type recording method using a sublimation dye, in which the inkjet ink composition is not directly applied to a recording medium to be transferred, but is applied to a transfer medium (paper or the like) that is the transfer source, and then the dye is transferred from the transfer medium to the transfer destination medium to dye it.
[0004] In the transfer recording method, a sublimation dye is blended in an inkjet ink composition, the composition is once attached to a medium from which the ink is to be transferred, and then the sublimation dye is sublimated, for example, by steam or heat, to dye the recording medium to be recorded. For example, Patent Documents 1 to 3 disclose compositions containing sublimation dyes containing glycerin or sugar alcohol as compositions used in such sublimation transfer. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2005 / 121263 [Patent Document 2] JP 2004-107647 A [Patent Document 3] JP 2004-107648 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, sublimation inks containing glycerin can cause smoke from minute droplets when the glycerin evaporates due to heating during sublimation transfer, and when cooled in the air and reaches a condensation point, sublimation inks containing sugar alcohols instead of glycerin can cause insufficient drying on the transfer medium surface due to the high boiling point of the sugar alcohol, resulting in the image being transferred to the back side of the medium when it is rolled up. [Means for solving the problem]
[0007] One embodiment of the ink-jet ink composition according to the present invention comprises: A sublimable dye; Sugar alcohols having four or more OH groups; a diol having 2 or 3 carbon atoms; one or more penetrating moisturizers selected from glycol monoethers, diols having 4 or more carbon atoms, amides, and (poly)glyceryl ethers; 1% by weight or less of glycerin based on the total weight of the composition; Includes.
[0008] One aspect of the inkjet recording method according to the present invention comprises: a recording step of depositing the ink-jet ink composition onto a sheet-like recording medium; a transfer step of superposing the recording surface of the recording medium on an object to be dyed and heating the object at a temperature of 150° C. or higher and 220° C. or lower to sublimate and transfer the sublimable dye onto the object to be dyed; A peeling step of peeling the recording medium from the object to be dyed after the image transfer; Includes.
[0009] One aspect of the inkjet recording method according to the present invention comprises: a recording step of depositing any one of the ink-jet ink compositions described above onto a sheet-like recording medium; a drying step of heating the recording medium to which the ink-jet ink composition has been applied to a temperature of 50° C. or higher; a recovery step of winding up the recording medium after drying into a roll; Includes.
[0010] One aspect of the inkjet recording apparatus according to the present invention is to an inkjet head for depositing the inkjet ink composition onto a sheet-like recording medium; A heater for heating the sheet-shaped recording medium to a temperature of 50° C. or higher; A roller for winding the recording medium into a roll; Includes. [Brief description of the drawings]
[0011] [Figure 1] Table illustrating penetrating moisturizers (Table 1). [Diagram 2] FIG. 1 is a schematic diagram of an example of an inkjet recording apparatus. [Diagram 3] Table 2 shows the compositions of the inkjet ink compositions of the examples. [Figure 4] Table 3 lists the compositions of the example inkjet ink compositions. [Diagram 5] Table 4 lists the compositions of the example inkjet ink compositions. [Figure 6] Table 5 lists the compositions of comparative inkjet ink compositions. [Figure 7] Table 6 shows the evaluation results of the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following describes an embodiment of the present invention. The embodiment described below is an example of the present invention. The present invention is not limited to the following embodiment, and includes various modified forms that are implemented within the scope of the present invention. Note that not all of the configurations described below are necessarily essential configurations of the present invention.
[0013] 1. Inkjet ink composition The inkjet ink composition according to this embodiment contains a sublimable dye, a sugar alcohol having four or more OH groups, a diol having two or three carbon atoms, one or more penetrating moisturizers selected from glycol monoethers, diols having four or more carbon atoms, amides, and (poly)glyceryl ethers, and 1% by mass or less of glycerin relative to the total mass of the composition.
[0014] 1.1.Sublimable dye The inkjet ink composition of the present embodiment contains a sublimation dye (hereinafter also referred to as a "sublimation dye" or "sublimation type dye"). A sublimation dye is a dye that is suitably used for dyeing hydrophobic synthetic fibers such as polyester, nylon, acetate, etc., and is a compound that is insoluble or poorly soluble in water. A sublimation dye is a dye that has the property of sublimating when heated. The sublimation dye used in the inkjet ink composition of the present embodiment is not particularly limited, but specific examples include the following.
[0015] As the sublimation dye, disperse dyes, solvent dyes, etc. having the above-mentioned properties can be used. Specific examples of such dyes include CI Disperse Yellow 3, 7, 8, 23, 39, 51, 54, 60, 71, 86; CI Disperse Orange 1, 1:1, 5, 20, 25, 25:1, 33, 56, 76; CI Disperse Brown 2; CI Disperse Red 11, 50, 53, 55, 55:1, 59, 60, 65, 70, 75, 93, 146, 158, 190, 190:1, 2 07, 239, 240; CI Bat Red 41; CI Disperse Violet 8, 17, 23, 27, 28, 29, 36, 57; CI Disperse Blue 19, 26, 26:1, 35, 55, 56, 58, 64, 64:1, 72, 72:1, 81, 81:1, 91, 95, 108, 131, 141, 145, 359; CI Solvent Blue 36, 63, 105, 111, etc. These may be used alone or in combination of two or more kinds.
[0016] Among the dyes exemplified above, in terms of storage stability of the inkjet ink composition, the inkjet ink composition of this embodiment preferably contains CI Disperse Yellow 3, 7, 8, 23, 51, 54, 60, 71, 86; CI Disperse Orange 20, 25, 25:1, 56, 76; CI Disperse Brown 2; and CI Disperse Red 11, 53, 55, 55:1, 59, 60, 65, 70, 75, 146. , 190, 190:1, 207, 239, 240; CI Bat Red 41; CI Disperse Violet 8, 17, 23, 27, 28, 29, 36, 57; CI Disperse Blue 26, 26:1, 55, 56, 58, 64, 64:1, 72, 72:1, 81, 81:1, 91, 95, 108, 131, 141, 145, 359; CI Solvent Blue 36, 63, 105, 111, etc. are more preferred.
[0017] The above-mentioned sublimation dyes are all compounds that are insoluble or poorly soluble in water, but can be well dispersed in water within a specific concentration range, for example, by using a dispersant described later. Also, the above-mentioned sublimation dyes are slightly different in dispersibility and solubility. That is, depending on the type of sublimation dye, the suitable concentration range of the dispersant differs, and the solubility of the dispersant also differs.
[0018] The sublimation dyes exemplified above may be used alone or in combination of two or more to form a mixed color.
[0019] The total content of the sublimation dyes is 10% by mass or less, preferably 0.1% by mass or more and 10% by mass or less, more preferably 0.2% by mass or more and 9.0% by mass or less, and even more preferably 0.3% by mass or more and 8.0% by mass or less, based on 100% by mass of the inkjet ink composition.
[0020] By making the content of the sublimation dye 0.1% by mass or more, the color development (OD value) of the obtained dyed product (transfer destination) tends to be more excellent. Also, by making the content of the sublimation dye 10% by mass or less, the ejection stability tends to be good.
[0021] The sublimation dye may be dispersed by a dispersant. The dispersant has a function of dispersing the above-mentioned sublimation dye in the inkjet ink composition. The dispersant is not particularly limited, but may be an anionic dispersant, a nonionic dispersant, or a polymer dispersant (resin dispersant).
[0022] As an anionic dispersant, a formalin condensation product of an aromatic sulfonic acid is preferably used. Examples of the "aromatic sulfonic acid" in the formalin condensation product of an aromatic sulfonic acid include creosote oil sulfonic acid, cresol sulfonic acid, phenol sulfonic acid, β-naphthalene sulfonic acid, and the like. Examples of the sulfonic acid include alkylnaphthalenesulfonic acids such as phthalocyanine sulfonic acid, methylnaphthalenesulfonic acid, and butylnaphthalenesulfonic acid, a mixture of β-naphthalenesulfonic acid and β-naphtholsulfonic acid, a mixture of cresolsulfonic acid and 2-naphthol-6-sulfonic acid, and ligninsulfonic acid and salts thereof.
[0023] As the anionic dispersant, a formalin condensate of β-naphthalenesulfonic acid, a formalin condensate of alkylnaphthalenesulfonic acid, and a formalin condensate of creosote oil sulfonic acid and their salts are preferred, with sodium salts being more preferred.
[0024] Examples of nonionic dispersants include ethylene oxide adducts of phytosterol and ethylene oxide adducts of cholestanol.
[0025] Among these, commercially available naphthalenesulfonic acid-based dispersants include Demol NL: naphthalenesulfonic acid, manufactured by Kao Corporation, Demol MS, Demol N, Demol RN, Demol RN-L, Demol SC-30, Demol SN-B, Demol SS-L, Demol T, and Demol T-45.
[0026] Examples of polymer dispersants (also referred to as "resin dispersants") include acrylic resins and salts thereof such as polyacrylic acid, acrylic acid-acrylonitrile copolymer, acrylic acid-acrylic acid ester copolymer, vinyl acetate-acrylic acid ester copolymer, vinyl acetate-acrylic acid copolymer, styrene-acrylic acid copolymer, styrene-methacrylic acid copolymer, styrene-methacrylic acid-acrylic acid ester copolymer, styrene-α-methylstyrene-acrylic acid copolymer, styrene-α-methylstyrene-acrylic acid-acrylic acid ester copolymer, and vinylnaphthalene-acrylic acid copolymer; styrene-acrylic acid copolymer, styrene-methacrylic acid copolymer, and styrene-methacrylic acid-acrylic acid ester copolymer. styrene-based resins and salts thereof, such as styrene-α-methylstyrene-acrylic acid copolymer, styrene-α-methylstyrene-acrylic acid-acrylic acid ester copolymer, styrene-maleic acid copolymer, and styrene-maleic anhydride copolymer; urethane-based resins and salts thereof, which are polymer compounds (resins) containing urethane bonds formed by a reaction between an isocyanate group and a hydroxyl group and may be linear and / or branched, and may have or may not have a crosslinked structure; polyvinyl alcohols and salts thereof; polyvinylpyrrolidones and salts thereof; vinylnaphthalene-maleic acid copolymers and salts thereof; vinyl acetate-maleic acid ester copolymers and salts thereof; and vinyl acetate-crotonic acid copolymers and salts thereof.
[0027] Examples of commercially available styrene-based resin dispersants include X-200, X-1, X-205, and X-220 (manufactured by Seiko PMC Co., Ltd.). Examples of commercially available acrylic resin dispersants include BYK-190, BYK-187, BYK-191, BYK-194N, and BYK-199 (manufactured by BYK-Chemie Co., Ltd.). Examples of commercially available urethane-based resin dispersants include BYK-184, BYK-182, BYK-183, and BYK-185 (manufactured by BYK-Chemie Co., Ltd.).
[0028] The dispersant may be used alone or in combination of two or more. The total content of the dispersant is 0.1% by mass or more and 30% by mass or less, preferably 0.5% by mass or more and 25% by mass or less, more preferably 1% by mass or more and 20% by mass or less, and even more preferably 1.5% by mass or more and 15% by mass or less, based on 100% by mass of the inkjet ink composition. By making the content of the dispersant 0.1% by mass or more, the dispersion stability of the sublimation dye can be obtained. In addition, if the content of the dispersant is 30% by mass or less, the sublimation dye is not dissolved too much and the viscosity can be suppressed to be small.
[0029] Among the above-listed dispersants, resin dispersants, particularly acrylic resins and styrene resins, are preferred. and urethane-based resins. In this case, the weight-average molecular weight of the dispersant is more preferably 500 or more. By using such a resin dispersant as the dispersant, the dispersion stability of the sublimation dye can be further improved.
[0030] 1.2. Sugar alcohols The inkjet ink composition of this embodiment contains sugar alcohols having four or more OH groups (hereinafter also referred to as "hydroxy groups" or "hydroxyl groups"). Examples of such sugar alcohols include sugars produced by reducing the carbonyl groups of aldoses and ketoses. Examples of such sugar alcohols include maltitol, lactitol, tetritol, pentitol, hexitol, erythritol, sorbitol, xylitol, mannitol, and inositol. Among these, one or more selected from D-sorbitol, erythritol, and D-mannitol are more preferable.
[0031] The molecular weights of some of the sugar alcohols exemplified above are shown below. Erythritol 122 Xylitol 152 D-Sorbitol 182 Lactitol 344
[0032] The viscosity (unit: mPa·s) of 60% by weight aqueous solutions of some of the sugar alcohols listed above is shown below. Xylitol 24.3 D-Sorbitol 32.8 The "60% by weight aqueous solution viscosity" refers to the viscosity at a shear rate of 200 s -1 The viscosity at 20°C is shown. Erythritol had a high viscosity and did not form an aqueous solution, so it was impossible to measure.
[0033] The surface tensions (unit: mN / m) of 10% by mass aqueous solutions of some of the sugar alcohols exemplified above are shown below. Xylitol 74.1 D-Sorbitol 73.5 The "surface tension of a 10% by mass aqueous solution" refers to the surface tension value at 20° C. measured by preparing a 10% by mass aqueous solution of each sugar alcohol and measuring it with a surface tensiometer DY-300 (manufactured by Kyowa Interface Science Co., Ltd.).
[0034] The above-listed sugar alcohols may be used alone or in combination of two or more. By including a sugar alcohol in the ink-jet ink composition, the ink-jet ink composition can reduce smoke generation and improve clogging recovery and color development of the image.
[0035] Furthermore, it is more preferable to use sugar alcohols having a viscosity of 35 mPa s or less in a 60% by mass aqueous solution, more preferably 33 mPa s or less, and even more preferably 30 mPa s or less. By using sugar alcohols having a viscosity of 35 mPa s or less in a 60% by mass aqueous solution, the effect of evaporation thickening caused by the sugar alcohol can be further reduced, and the intermittent ejection stability can be further improved.
[0036] The content of sugar alcohols is preferably 3% by mass or more and 15% by mass or less, more preferably 3% by mass or more and 13% by mass or less, based on the total mass of the ink-jet ink composition. The sugar alcohol content is preferably from 4 to 7% by mass, more preferably from 4 to 7% by mass. When the sugar alcohol content is in this range, clogging recovery, color development, and intermittent ejection stability can be more satisfactorily achieved.
[0037] 1.3. Diols with 2 or 3 carbon atoms The inkjet ink composition according to this embodiment contains a diol having 2 or 3 carbon atoms. Examples of diols having 2 or 3 carbon atoms include ethylene glycol, 1,2-propanediol (propylene glycol), and 1,3-propanediol. Among these, it is more preferable to use propylene glycol. The inkjet ink composition may contain a plurality of these diols.
[0038] By including a diol having 2 or 3 carbon atoms in the ink-jet ink composition, the drying properties on paper are improved, while the effect of evaporation thickening can be further reduced, and the intermittent ejection stability can be further improved.
[0039] In the inkjet ink composition, the content of the diols having 2 or 3 carbon atoms is preferably from 5% to 15% by mass, more preferably from 6% to 14% by mass, and even more preferably from 7% to 13% by mass, relative to the total mass of the inkjet ink composition. When the content of the diols having 2 or 3 carbon atoms in the inkjet ink composition is within such a range, smoke generation can be further suppressed, and the paper surface drying property and intermittent ejection are further improved.
[0040] 1.4. Penetrating moisturizers The inkjet ink composition according to this embodiment contains one or more penetrating moisturizers selected from glycol monoethers, diols having 4 or more carbon atoms, amides, and (poly)glyceryl ethers.
[0041] By containing a penetrating moisturizer in the ink-jet ink composition, the drying property of the image formed by the ink-jet ink composition can be improved, and the intermittent ejection stability can be improved. In this specification, the penetrating moisturizer is treated as being different from the moisturizer, but the penetrating moisturizer does not necessarily have a characteristic of having penetrating property, and the penetrating moisturizer includes those with little penetrating property or those without penetrating property.
[0042] Table 1 shows examples of penetrating moisturizers.
[0043] In Table 1, the surface tension of a 10% by mass aqueous solution is shown as the result of preparing a 10% by mass aqueous solution of each penetrating moisturizer and measuring it with a surface tensiometer DY-300 (manufactured by Kyowa Interface Science Co., Ltd.).
[0044] The inkjet ink composition may contain a penetrating moisturizer other than those exemplified in Table 1. In addition, a plurality of penetrating moisturizers may be used. The tension is preferably 45 mN / m or more and 67 mN / m or less, more preferably 46 mN / m or more and 65 mN / m or less, and even more preferably 50 mN / m or more and 64 mN / m or less.
[0045] When the surface tension of the 10% by mass aqueous solution is within this range, the inkjet ink composition has better color development, intermittent ejection stability, paper surface drying property, and clogging recovery. In addition, when the surface tension is within this range, the inkjet ink composition has better permeability and better color development of the resulting image. Furthermore, the viscosity and / or evaporation thickening property are also better, so the inkjet ink composition has better clogging recovery and / or intermittent ejection stability.
[0046] The content of the penetrating moisturizer is preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less, based on the total mass of the inkjet ink composition. The lower limit of the content of the penetrating moisturizer is preferably 0.3% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. By including the penetrating moisturizer to this extent, the clogging recovery property of the inkjet ink composition and the color development of the image can be improved. In addition, the storage stability of the inkjet ink composition can be improved.
[0047] The penetrating moisturizer more preferably contains (poly)glyceryl ethers. Examples of (poly)glyceryl ethers include alkylene oxide adducts of glycerin or polyglycerin. (Poly)glyceryl ethers, i.e., polyglyceryl ethers and glyceryl ethers, are less likely to emit smoke and are more likely to suppress smoke generation during transfer. For example, the following results are obtained with Uniox G-450, Uniox G-750, SC-E750, SC-E350, and SC-P750, which are exemplified in Table 1.
[0048] The smoke generation of a 30% by weight aqueous solution was evaluated as follows. A 30% by weight aqueous solution of each (poly)glyceryl ether was prepared, and 10 drops were dropped onto a 100% polyester fabric, Karl Dry (manufactured by Toray Industries, Inc.), using a plastic dropper. The solution was then heated at 200°C for 40 seconds at 465 g / cm2 in a tabletop automatic sublimation transfer press, AF-54TEN (manufactured by Itsumi Corporation). 2 The results showed that Uniox G-450, Uniox G-750, SC-E750, SC-E350, and SC-P750 did not emit smoke.
[0049] Such an effect is considered to be due in part to the molecular weight of the (poly)glyceryl ethers. From this viewpoint, when the (poly)glyceryl ethers are used, the weight-average molecular weight is preferably 280 to 900, more preferably 300 to 800, and even more preferably 350 to 750. The upper limit of the weight-average molecular weight is preferably within the above range from the viewpoints of the viscosity of the solution and the rate of increase in viscosity when the solution dries.
[0050] Glycerin The inkjet ink composition of this embodiment contains glycerin in an amount of 1% by mass or less relative to the total mass of the composition. The inkjet ink composition does not contain glycerin in an amount of more than 1% by mass relative to the total mass of the composition.
[0051] In the ink-jet ink composition, the glycerin content is preferably not more than 0.5% by mass, more preferably not more than 0.1% by mass. Furthermore, the ink-jet ink composition may or may not contain glycerin, and even if it does contain glycerin, the content is not more than the above-mentioned amount.
[0052] When the glycerin content is within the above range, the ink-jet ink composition is less likely to emit smoke and exhibits excellent drying properties on paper.
[0053] 1.6.Other Ingredients In addition to the above components, the ink-jet ink composition may also contain the following components.
[0054] Surfactants The inkjet ink composition may contain a surfactant. The surfactant is not particularly limited, but examples thereof include acetylene glycol-based surfactants, fluorine-based surfactants, and silicone-based surfactants.
[0055] The acetylene glycol surfactant is not particularly limited, but examples thereof include Surfynol 104, 104E, 104H, 104A, 104BC, 104DPM, 104PA, 104PG-50, 104S, 420, 440, 465, 485, SE, SE-F, 504, 61, DF37, CT111, CT121, CT131, CT136, TG, GA, and DF110D (all trade names, manufactured by Air Products Japan Co., Ltd.), O Examples of such surfactants include Rufin B, Y, P, A, STG, SPC, E1004, E1010, PD-001, PD-002W, PD-003, PD-004, EXP.4001, EXP.4036, EXP.4051, AF-103, AF-104, AK-02, SK-14, and AE-3 (all trade names, manufactured by Nissin Chemical Industry Co., Ltd.), and Acetylenol E00, E00P, E40, and E100 (all trade names, manufactured by Kawaken Fine Chemical Co., Ltd.).
[0056] As the fluorosurfactant, it is preferable to use a fluorine-modified polymer, and a specific example thereof is BYK-340 (product name, manufactured by BYK Japan KK).
[0057] The silicone surfactant is not particularly limited, but a polysiloxane compound is preferred. The polysiloxane compound is not particularly limited, but for example, a polyether-modified organosiloxane is exemplified. Examples of commercially available polyether-modified organosiloxanes include BYK-306, BYK-307, BYK-333, BYK-341, BYK-345, BYK-346, BYK-348 (all trade names, manufactured by BYK Japan Co., Ltd.), KF-351A, KF-352A, KF-353, KF-354L, KF-355A, KF-615A, KF-945, KF-640, KF-642, KF-643, KF-6020, X-22-4515, KF-6011, KF-6012, KF-6015, KF-6017 (all trade names, manufactured by Shin-Etsu Chemical Co., Ltd.), Silface SAG503A, Silface SAG014 (all trade names, manufactured by Nissin Chemical Industry Co., Ltd.), and the like.
[0058] The above surfactants may be used alone or in combination of two or more kinds.
[0059] When a surfactant is contained, its content is preferably 0.1% by mass or more and 1.5% by mass or less relative to the total mass of the ink-jet ink composition.
[0060] 1.6.2. Polyglycerols and betaines The inkjet ink composition may further contain at least one selected from polyglycerols and betaines. Although polyglycerols and betaines have properties as moisturizing agents, in this specification, polyglycerols and betaines are treated as different from the above-mentioned penetrating moisturizing agents.
[0061] Polyglycerols include Diglycerol S (manufactured by Sakamoto Pharmaceutical Co., Ltd.) (weight average molecular weight: 166, 60% aqueous solution viscosity: 20.8, 10% aqueous solution surface tension: 72.5), R-PG (manufactured by Sakamoto Pharmaceutical Co., Ltd.) (weight average molecular weight: 240, 60% aqueous solution viscosity: 29), and Polyglycerol #310 (manufactured by Sakamoto Pharmaceutical Co., Ltd.) (weight average molecular weight: 310, 60% Viscosity of aqueous solution: 22.8).
[0062] Betaines refer to compounds that have a positive charge and a negative charge at non-adjacent positions in the same molecule, that have no dissociable hydrogen bonded to the positively charged atom, that can form an intramolecular salt, and that have no charge as a whole molecule. In this embodiment, the betaines are preferably those in which the positively charged site is a quaternary ammonium cation.
[0063] The betaines are not particularly limited, and examples thereof include trialkylglycines such as trimethylglycine and triethylglycine, γ-butyrobetaine, homarine, trigonelline, carnitine, homoserine betaine, valine betaine, lysine betaine, ornithine betaine, alanine betaine, stachydrine, and glutamic acid betaine. Among them, the glycines contained in the inkjet ink composition are preferably selected from trialkylglycines, and more preferably contain trimethylglycine. Trialkylglycines are compounds in which three alkyl groups are substituted on the nitrogen atom of glycine. This tends to improve clogging recovery. The betaines may be used alone or in combination of two or more.
[0064] When polyglycerins and betaines are used, the total content thereof relative to the total mass of the inkjet ink composition is preferably 2.5% by mass or more and 9.5% by mass or less, more preferably 3% by mass or more and 8% by mass or less, and even more preferably 4% by mass or more and 8% by mass or less.
[0065] In addition, polyglycerols may contain glycerol as an impurity, and adding a large amount may cause smoking. In addition, when betaines are solid, adding a large amount may cause poor clogging recovery. From these viewpoints, it is preferable to set the content within the above range.
[0066] Polyglycerols and betaines have low evaporation thickening properties, and by including at least one of polyglycerols and betaines in the inkjet ink composition, the intermittent ejection stability can be improved by adding a small amount. In addition, the inkjet ink composition can be prevented from flying in a curved direction or from failing to eject due to drying of the inkjet ink composition in the nozzles of the inkjet head, and clogging recovery can be improved.
[0067] 1.6.3.Water The inkjet ink composition of the present embodiment may be an aqueous composition containing water. An "aqueous" composition refers to a composition in which water is one of the main solvents. Examples of water include pure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, and distilled water, as well as ultrapure water with reduced ionic impurities. In addition, if water sterilized by ultraviolet irradiation or the addition of hydrogen peroxide is used, the growth of bacteria and fungi can be suppressed when the inkjet ink composition is stored for a long period of time.
[0068] The water content is 30% by mass or more, preferably 40% by mass or more, more preferably 45% by mass or more, and even more preferably 50% by mass or more, based on the total amount (100% by mass) of the ink-jet ink composition. The upper limit of the water content is preferably 97% by mass or less, even more preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less, based on the total amount (100% by mass) of the ink composition.
[0069] Other Ingredients The inkjet ink composition of the present embodiment may contain various additives, such as organic solvents, chelating agents, rust inhibitors, fungicides, antioxidants, reduction inhibitors, and evaporation promoters, as necessary. good.
[0070] 1.7. Manufacturing and Properties From the viewpoint of further improving the quality of an inkjet image, the inkjet ink composition of this embodiment preferably has a surface tension (static surface tension) of 18 mN / m to 40 mN / m, more preferably 20 mN / m to 35 mN / m, and even more preferably 22 mN / m to 33 mN / m at 20° C. The surface tension can be measured, for example, by using an automatic surface tensiometer CBVP-Z (product name, manufactured by Kyowa Interface Science Co., Ltd.) to confirm the surface tension when a platinum plate is wetted with the inkjet ink composition in an environment of 20° C.
[0071] From the same viewpoint, the viscosity of the inkjet ink composition at 20° C. is preferably from 3 mPa·s to 10 mPa·s, and more preferably from 3 mPa·s to 8 mPa·s. The viscosity can be measured, for example, using a viscoelasticity tester MCR-300 (product name, manufactured by Pysica) in an environment of 20° C.
[0072] The inkjet ink composition can be obtained by mixing the above-mentioned components in any order and removing impurities by filtration, etc., as necessary. As a method for mixing each component, a method in which materials are added sequentially to a container equipped with a stirring device such as a mechanical stirrer or a magnetic stirrer and stirred and mixed is preferably used. As a filtration method, centrifugal filtration, filter filtration, etc. can be performed as necessary.
[0073] 1.8.Effects According to the inkjet ink composition of this embodiment, sugar alcohols containing 4 or more OH groups are unlikely to volatilize at temperatures up to 220° C., and are unlikely to emit smoke when heated. Furthermore, according to this inkjet ink composition, by using diols having 2 or 3 carbon atoms, which have high drying properties and low viscosity, in combination with a penetrating moisturizer, it is possible to achieve both low smoke generation and good drying properties on the paper surface. Furthermore, according to this inkjet ink composition, the content of glycerin is 1% by mass or less, so smoke generation is suppressed.
[0074] 2. Inkjet recording method 2.1. First embodiment The inkjet recording method according to this embodiment includes a recording step of adhering the above-mentioned inkjet ink composition to a sheet-like recording medium (intermediate transfer medium), a transfer step of superimposing the recording surface of the recording medium (intermediate transfer medium) on an object to be dyed (recording medium) and heating at a temperature of 150°C or higher and 220°C or lower to sublimate and transfer the sublimable dye to the object to be dyed (recording medium), and a peeling step of peeling the recording medium (intermediate transfer medium) from the object to be dyed (recording medium) after image transfer.
[0075] The inkjet ink composition described above can be suitably applied to a dyeing method for fabrics and the like that utilizes sublimation transfer (sublimation transfer inkjet recording method). The inkjet recording method of the present embodiment can also be said to be a method for producing dyed products.
[0076] The inkjet recording method (dyed product manufacturing method) of this embodiment includes a step of attaching an inkjet ink composition to the recording surface of a recording medium, a step of placing a recording medium on the recording surface of the recording medium, a step of heating the recording medium and the recording medium, and a step of peeling off the recording medium (intermediate transfer medium) from the object to be dyed (recording medium). In other words, the inkjet recording method (dyed product manufacturing method) of this embodiment includes a recording step of applying the above-mentioned inkjet ink composition to an intermediate transfer medium using an inkjet method, and a step of placing the intermediate transfer medium to which the ink composition has been applied so that the surface to which the ink composition has been applied faces the dyed surface of the object to be dyed. The method includes a transfer step in which the intermediate transfer medium is heated in a cooled state to transfer the sublimation dye to the object to be dyed, and a peeling step in which the recording medium (intermediate transfer medium) is peeled off from the object to be dyed (recording medium) after the image transfer. Each step will be described below.
[0077] <Recording process> In this step, the inkjet ink composition is applied to the recording surface of the intermediate transfer medium (first recording medium) by the inkjet method. The inkjet ink composition can be ejected by the inkjet method using a droplet ejection device (for example, an inkjet recording device described later).
[0078] As the droplet ejection method (method of inkjet method), a piezoelectric method or a method of ejecting ink by bubbles generated by heating the ink can be used. From the viewpoint of the ink composition being less likely to deteriorate, the piezoelectric method is preferred. Also, according to the inventor's investigation, in a recording head of the thin film piezoelectric method, the shear rate applied to the inkjet ink composition is 100 s -1 This is a more preferable shear rate in the ink-jet ink composition of this embodiment.
[0079] Examples of intermediate transfer media include sheet-shaped recording media, such as plain paper and recording media with an ink-receiving layer (called inkjet paper, coated paper, etc.), but paper with an ink-receiving layer made of inorganic fine particles such as silica is more preferable. This makes it possible to obtain an intermediate recording material in which bleeding or the like is suppressed on the recording surface during the process in which the inkjet ink composition applied to the intermediate transfer medium dries. In addition, such a medium makes it easier to retain the sublimation dye on the surface of the recording surface, and in the subsequent transfer process, the sublimation of the sublimation dye can be more efficiently performed.
[0080] In this step, a plurality of ink-jet ink compositions may be used, which may, for example, make it possible to produce a wider color gamut.
[0081] <Transfer process> Thereafter, the recording surface of the intermediate transfer medium to which the ink composition has been applied is heated in a state in which it faces the object to be dyed (a state in which a second recording medium is placed on the recording surface of the first recording medium), and the sublimable dye constituting the inkjet ink composition is transferred to the object to be dyed. This results in a dyed object on the object to be dyed, such as a fabric.
[0082] The heating temperature in this step is from 150° C. to 220° C., and preferably from 160° C. to 210° C. This makes it possible to impart sufficient energy to transfer the sublimable dye to the object to be dyed, thereby improving the productivity of the dyed object.
[0083] The heating time in this step is 30 to 90 seconds, preferably 45 to 60 seconds, depending on the heating temperature, which provides sufficient energy for transferring the sublimable dye to the dyed article, and thus the productivity of the dyed article can be improved.
[0084] This step may be carried out by heating the intermediate transfer medium to which the ink composition has been applied in a state in which it faces the object to be dyed, but it is more preferable to carry out the step by heating the intermediate transfer medium in a state in which it is in close contact with the object to be dyed. This makes it possible, for example, to record (dye) a clearer image on the second recording medium.
[0085] As the substrate to be dyed, for example, sheet-like objects such as fabrics (hydrophobic fiber fabrics, etc.) and resin (plastic) films are suitably used, but objects having three-dimensional shapes such as spheres and rectangular parallelepipeds other than sheets may also be used.
[0086] The substrate may be made of resin or plastic, glass, metal, or ceramic. The fibers constituting the fabric as the substrate may be polyester fiber, nylon fiber, triacetate fiber, diacetate fiber, polyamide fiber, or a blend of two or more of these fibers. Blends of these fibers with regenerated fibers such as rayon or natural fibers such as cotton, silk, or wool may also be used.
[0087] Examples of resin (plastic) films as substrates include polyester films, polyurethane films, polycarbonate films, polyphenylene sulfide films, polyimide films, polyamideimide films, etc. The resin (plastic) film may be a laminate in which a plurality of layers are laminated, or may be made of a gradient material in which the composition of the material changes in a gradient manner.
[0088] <Peeling process> In this step, after the image is transferred in the transfer step, the recording medium (intermediate transfer medium) is peeled off from the object to be dyed (recording medium). There is no particular limitation on the method of peeling off, and it can be performed using an appropriate device.
[0089] According to the inkjet recording method of this embodiment, the sublimation transfer temperature is 150° C. or more and 220° C. or less, so that volatilization of the sugar alcohol is suppressed and generation of smoke is suppressed.
[0090] 2.2. Second embodiment The inkjet recording method according to this embodiment includes a recording step of applying the above-mentioned inkjet ink composition to a sheet-like recording medium, a drying step of heating the recording medium to which the inkjet ink composition has been applied to a temperature of 50° C. or higher, and a recovery step of winding up the dried recording medium into a roll.
[0091] The recording process in the inkjet recording method of this embodiment is similar to the recording process in the first embodiment, and therefore a description thereof will be omitted.
[0092] <Drying process> In the drying step, the recording medium (intermediate transfer medium) to which the inkjet ink composition has been applied in the recording step is heated to a temperature of 50° C. or higher. The heating method is not particularly limited, and can be performed, for example, by using an after-heater of an inkjet recording device described later.
[0093] <Recovery process> In the recovery step, the recording medium (intermediate transfer medium) after the drying step is wound up in a roll shape. The recovery step can be performed using an appropriate winding device.
[0094] <Other processes> The inkjet recording method of this embodiment may further include a transfer step, a peeling step, and the like. The transfer step and the peeling step are the same as those in the first embodiment described above, and therefore will not be described. In this embodiment, the intermediate transfer medium is wound into a roll and then used in the transfer step. This increases the degree of freedom in the process for obtaining a printed item.
[0095] According to the inkjet recording method of this embodiment, the diol evaporates in the drying step of heating to a temperature of 50° C. or higher, so that the paper surface drying property is good and smoke generation during transfer can be suppressed. In addition, since the inkjet ink composition described above is used, the paper surface drying property in the drying step of heating to a temperature of 50° C. or higher is also good, and offset is unlikely to occur even when the recording medium is wound into a roll.
[0096] 3. Inkjet recording device The inkjet ink composition can be suitably used in an inkjet recording device. The inkjet recording device is not particularly limited as long as it has at least an ink storage container (cartridge, tank, etc.) that stores the inkjet ink composition and a recording head connected thereto, and can eject the inkjet ink composition from the recording head to form an image on an intermediate transfer medium (transfer paper, etc.).
[0097] The inkjet recording apparatus of the present embodiment can be either a serial type or a line type. These types of inkjet recording apparatuses are equipped with a recording head, and while changing the relative positional relationship between a recording medium (intermediate transfer medium) and the recording head, droplets of the inkjet ink composition are discharged from the nozzle holes of the recording head at a predetermined timing (intermittently) and in a predetermined volume (mass), so that the inkjet ink composition is deposited on the recording medium (intermediate transfer medium) to form a predetermined image.
[0098] Generally, in a serial type inkjet recording device, the transport direction of the recording medium and the direction of the reciprocating motion of the recording head intersect, and the relative positional relationship between the recording medium and the recording head is changed by a combination of the reciprocating motion of the recording head and the transport motion of the recording medium (including the reciprocating motion). In this case, generally, a plurality of nozzle holes (holes for ejecting the ink composition) are arranged in the recording head, and a row of nozzle holes (nozzle row) is formed along the transport direction of the recording medium. In addition, the recording head may be formed with a plurality of nozzle rows depending on the type and number of ink compositions.
[0099] Generally, in a line-type inkjet recording device, the recording head does not perform a reciprocating motion, but changes the relative positional relationship between the recording medium and the recording head by conveying the recording medium. Even in this case, generally, the recording head has a plurality of nozzle holes arranged therein, and a row of the nozzle holes (nozzle row) is formed along a direction intersecting the conveying direction of the recording medium.
[0100] The inkjet recording method uses a serial or line type inkjet recording device, and the method is not particularly limited as long as the ink composition can be discharged as droplets from a fine nozzle hole and the droplets can be attached to a recording medium. For example, as a droplet discharge method (method of inkjet method), a piezo method or a method of discharging ink by bubbles generated by heating the ink can be used, and the piezo method is preferred from the viewpoint of the ink composition being less likely to deteriorate.
[0101] For the inkjet recording apparatus used in this embodiment, known configurations such as a heating unit, a drying unit, a roll unit, and a winding unit can be used without any restrictions.
[0102] An example of a recording apparatus suitable for the inkjet recording method of this embodiment will be described below. A schematic cross-sectional view of an inkjet recording apparatus according to one embodiment is shown in Fig. 2. As shown in Fig. 2, the recording apparatus 1 includes a supply roll 9, a recording head 2, an IR heater 3, a platen heater 4, an after-heater 5, a cooling fan 6, a pre-heater 7, a ventilation fan 8, and a take-up roll 10.
[0103] The recording head 2 ejects the inkjet ink composition onto a recording medium M (intermediate transfer medium) fed from a supply roll 9. The recording head 2 may be of a conventionally known type. One example of such a known type is a head that ejects droplets by utilizing the vibration of a piezoelectric element, that is, a head that forms ink droplets by the mechanical deformation of an electrostrictive element. The recording head 2 may be, for example, a head that ejects dots of the inkjet ink composition from one nozzle. It can be dispensed in multiple sizes.
[0104] In the drying step, the recording medium (intermediate transfer medium) is heated after the recording step, and this step can be performed by the after-heater 5 in the recording apparatus 1. Although not shown, a hot air mechanism (not shown) and a thermostatic bath (not shown) may be used. The after-heater 5 heats and dries the recording medium (intermediate transfer medium) to which the ink-jet ink composition is attached. The after-heater 5 heats the recording medium (intermediate transfer medium) to which an image is recorded, thereby evaporating and scattering moisture contained in the ink-jet ink composition more quickly, thereby suppressing bleeding and the like. The after-heater 5 heats the recording medium (intermediate transfer medium) to preferably 50° C. or higher, and more preferably 60° C. or higher and 110° C. or lower.
[0105] The recording apparatus 1 also includes an IR heater 3 that directly heats the recording head 2, and a platen heater 4 that heats the recording head 2 via a recording medium (intermediate transfer medium).
[0106] By using the IR heater 3, it is also possible to heat the recording medium (intermediate transfer medium) from the recording head 2 side. As a result, the recording head 2 is also likely to be heated at the same time, but compared to heating the recording medium (intermediate transfer medium) from its rear side using the platen heater 4 or the like, the temperature can be increased without being affected by the thickness of the recording medium (intermediate transfer medium). In addition, by using the platen heater 4, it is possible to heat the recording medium (intermediate transfer medium) from the side opposite the recording head 2 side. As a result, the recording head 2 is relatively less likely to be heated.
[0107] Incidentally, the above-mentioned "heating the recording medium (intermediate transfer medium)" refers to raising the temperature of the recording medium (intermediate transfer medium) to a desired temperature, and is not limited to directly heating the recording medium (intermediate transfer medium). The recording device 1 may have a cooling fan 6. After drying, the ink composition on the recording medium (intermediate transfer medium) is cooled by the cooling fan 6, which tends to form a coating with good adhesion on the recording medium (intermediate transfer medium).
[0108] The recording apparatus 1 may also include a preheater 7 that preheats the recording medium (intermediate transfer medium) before the ink composition is ejected onto the recording medium (intermediate transfer medium). Furthermore, the recording apparatus 1 may also include a ventilation fan 8 so that the ink composition attached to the recording medium (intermediate transfer medium) can be dried more efficiently.
[0109] The recording medium M (intermediate transfer medium) on which the recording is performed and which has been subjected to a drying process is taken up by a take-up roll 10. Note that the recording device 1 does not necessarily have to have the take-up roll 10, and for example, the recording medium M (intermediate transfer medium) on which the drying process has been performed may be transported to a transfer device (not shown) and proceed to a transfer process and a peeling process.
[0110] 4. Examples and Comparative Examples The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following, "parts" and "%" are based on mass unless otherwise specified. The evaluation was performed under an environment of a temperature of 25.0°C and a relative humidity of 40.0%, unless otherwise specified.
[0111] 4.1. Preparation of Inkjet Ink Composition The components were placed in a container so as to obtain the compositions shown in Tables 2 to 5, and mixed and stirred for 2 hours using a magnetic stirrer, and then filtered through a membrane filter having a pore size of 5 μm to obtain the inkjet ink compositions of Examples 1 to 24 and Comparative Examples 1 to 5. The values in the tables represent mass %.
[0112] Details of the components listed in Tables 2 to 5 by product name, abbreviation, etc. are as follows. Uniox G-450: Glyceryl ethers: NOF Corporation Sannix GP-250: Glyceryl ethers: Sanyo Chemical Industries, Ltd. SC-E350: Polyglyceryl ethers: manufactured by Sakamoto Pharmaceutical Co., Ltd. SC-P750: Polyglyceryl ethers: manufactured by Sakamoto Pharmaceutical Co., Ltd. Wilbride S-753: Glyceryl ethers: NOF Corporation Polyglycerin #310: Polyglycerin: Manufactured by Sakamoto Pharmaceutical Co., Ltd. BYK-348: Silicone surfactant: BYK Japan Co., Ltd.
[0113] Dye dispersion 1 shown in the table was prepared as follows. <Dye dispersion 1 (surfactant dispersion)> A mixture of Kayaset Red B (CI Disperse Red 60, manufactured by Nippon Kayaku Co., Ltd.) (30 parts) as a sublimation dye, Labellin RTMW-40 (40% aqueous solution of formalin condensate of creosote oil sulfonate, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) (45 parts) as an anionic dispersant, NIKKOLRTMBPS-30 (30 moles of phytosterol EO (ethylene oxide) adduct, manufactured by Nikko Chemicals Co., Ltd.) (2 parts) as a nonionic dispersant, and ion-exchanged water (23 parts) was dispersed in a sand mill using 0.2 mm diameter glass beads for about 15 hours under cooling. After the dispersion treatment, ion-exchanged water (100 parts) was added to the liquid after the dispersion treatment to adjust the dye content to 15%, and then the dye dispersion liquid 1 was obtained by filtering with glass fiber filter paper GC-50 (manufactured by Toyo Roshi Co., Ltd., filter pore size: 0.5 μm).
[0114] Dye dispersion 2 listed in the table was prepared as follows. <Dye dispersion 2 (resin dispersion)> 20 parts of Joncryl RTM 678 (manufactured by BASF) was added to a mixture of 48% lithium hydroxide (3.2 parts), ion-exchanged water (56.8 parts), and propylene glycol (20 parts), and the mixture was heated to 90 to 120 ° C. and stirred for 5 hours to obtain an emulsion of Joncryl RTM 678. A mixture of Kayaset Red B (manufactured by Nippon Kayaku Co., Ltd., CI Disperse Red 60) (30 parts) as a sublimable dye, the emulsion of Joncryl RTM 678 (60 parts), Proxel RTMGXL (0.2 parts), Surfynol 104PG50 (0.4 parts), and ion-exchanged water (24 parts) was dispersed in a sand mill using 0.2 mm diameter glass beads for about 15 hours under cooling. To the liquid after the dispersion treatment, ion-exchanged water (60 parts) and the above-mentioned Joncryl RTM678 emulsion liquid (30 parts) were added to adjust the dye content to 15%, and then the liquid was filtered through glass fiber filter paper GC-50 (manufactured by Toyo Roshi Kaisha, Ltd., filter pore size: 0.5 μm) to obtain dye dispersion liquid 2.
[0115] The properties of the materials used in the examples and comparative examples are given below. Xylitol: 60% aqueous solution viscosity = 24.3 mPa s D-Sorbitol: 60% aqueous solution viscosity = 32.8 mPa s Erythritol: 60% aqueous solution viscosity = insoluble Propylene glycol: 60% aqueous solution Viscosity = 9.8 mPa s: 10% aqueous solution Surface tension = 62.7 mN / m 1,3-Propanediol: 60% aqueous solution viscosity = 8.7 mPa s: 10% aqueous solution surface tension = 67.8 mN / m Uniox G-450: Weight average molecular weight = 450: 10% aqueous solution surface tension = 63.7 mN / m Sannix GP-250: Weight average molecular weight = 250: 10% aqueous solution surface tension = 49.6 mN / m ·SC-E350: Weight average molecular weight = 350: 10% aqueous solution surface tension = 58.6mN / m · SC-P750: Weight average molecular weight = 750: 10% aqueous solution surface tension = 46.1 mN / m · Wilbride S-753: Weight average molecular weight = 950: 10% aqueous solution surface tension = 43.3 mN / m Triethylene glycol monomethyl ether: 10% aqueous solution Surface tension = 60.6 mN / m Diethylene glycol monobutyl ether: Surface tension of 10% aqueous solution = 35.0 mN / m Triethylene glycol: Surface tension of 10% aqueous solution = 66.0 mN / m 1,2-butanediol: 10% aqueous solution Surface tension = 53.7mN / m ε-caprolactam: 10% aqueous solution surface tension = 54.1mN / m Glycerin: 60% aqueous solution viscosity = 11.4 mPa s Polyglycerin #310: 60% aqueous solution viscosity = 22.8 mPa s Trimethylglycine: 60% aqueous solution viscosity = 15.1 mPa s
[0116] Evaluation method 4.2.1.Paper surface drying properties Using the inkjet ink compositions of the Examples and Comparative Examples, the ink was applied to sublimation transfer paper EPSON DS Transfer Multi-Purpose (manufactured by Seiko Epson Corporation) using a PX-G930 (manufactured by Seiko Epson Corporation) at an ink deposition rate of 8±0.5 mg / inch. 2 A solid pattern was printed so that the pattern was as follows. After a predetermined time had passed, the printed surface was lightly wiped with Bemcot and the presence or absence of transfer was visually evaluated. Evaluation was based on the following criteria, and the results are shown in Table 6. A: No transfer occurs within 120 seconds after printing B: Transfer occurs 120 seconds after printing, but does not occur 150 seconds after printing. C: Transfer occurs even 150 seconds after printing
[0117] 4.2.2. Smoke generation Using the inkjet ink compositions of the Examples and Comparative Examples, the ink was applied to sublimation transfer paper EPSON DS Transfer Multi-Purpose (manufactured by Seiko Epson Corporation) using a PX-G930 (manufactured by Seiko Epson Corporation) at an ink deposition rate of 8±0.5 mg / inch. 2 A solid pattern was printed so that the pattern was printed as follows. Then, the pattern was printed at 200°C for 40 seconds at 465 g / cm using a tabletop automatic sublimation transfer press AF-54TEN (manufactured by Itsumi Co., Ltd.). 2 The ink was transferred to a 100% polyester fabric, Karl Dry (Toray Industries, Inc.), and the amount of smoke generated after transfer was visually evaluated. The evaluation was based on the following criteria, and the results are shown in Table 6. A: No smoke occurs after transfer B: Smoke occurs after transfer, but disappears within 5 seconds C: Smoke occurs after transfer and continues for more than 5 seconds
[0118] 4.2.3. Intermittent Discharge Stability Using the inkjet ink compositions of the examples and comparative examples, the head voltage was adjusted to a dot weight of 6±0.5 ng using a PX-G930 (manufactured by Seiko Epson Corporation), and 700 passes of idle operation were performed with the preliminary ejection turned off. After that, a nozzle check pattern was printed, and the presence or absence of landing deviation of the ink droplets was evaluated. The evaluation was based on the following criteria, and the results are shown in Table 6. AA: No missing pixels or distortion A: Less than 80% of nozzles have twisting. B: More than 80% of nozzles have twisted. C: More than 50% of the nozzles do not eject
[0119] 4.2.4.Clogging recovery After filling the PX-G930 (manufactured by Seiko Epson Corporation) with each ink, The printer was left with the cap open for five days in a temperature-controlled room at a temperature of 40°C and humidity of 20%. After that, the printer was cleaned three times at room temperature (with 4g of ink suction, 2g, and 2g of ink suction in that order) and the number of unrecovered nozzles was counted. The printer was evaluated according to the following criteria, and the results are shown in Table 6. A: No unrecovered nozzles B: 1 to 10 unrecovered nozzles C: 11 or more unrecovered nozzles
[0120] 4.2.5.Color development Using the inkjet ink compositions of the Examples and Comparative Examples, the ink was applied to sublimation transfer paper EPSON DS Transfer Multi-Purpose (manufactured by Seiko Epson Corporation) using a PX-G930 (manufactured by Seiko Epson Corporation) at an ink deposition rate of 8±0.5 mg / inch. 2 A solid pattern was printed so that the pattern was printed as follows. Then, the pattern was printed at 200°C for 40 seconds at 465 g / cm using a tabletop automatic sublimation transfer press AF-54TEN (manufactured by Itsumi Co., Ltd.). 2 The ink was transferred to a 100% polyester fabric, Karl Dry (Toray Industries, Inc.), with a pressure of 1000 psi. The OD value on the fabric was then measured using a colorimeter, ilPR03 (X-Rite Corporation). The measurement conditions were light source D65 and density status T. The results were evaluated according to the following criteria, and are shown in Table 6. AA:OD value 1.55 or more A:OD value 1.50 or more, less than 1.55 B:OD value 1.45 or more, less than 1.50 C:OD value less than 1.45
[0121] 4.3.Evaluation Results Looking at Tables 2 to 6, it was found that the inkjet ink compositions of each Example, which contain a sublimable dye, a sugar alcohol having four or more OH groups, a diol having two or three carbon atoms, one or more penetrating humectants selected from glycol monoethers, diols having four or more carbon atoms, amides, and (poly)glyceryl ethers, and 1% by mass or less of glycerin relative to the total mass of the composition, have good drying properties on paper and are less likely to smoke.
[0122] The present invention includes configurations that are substantially the same as the configurations described in the embodiments, for example, configurations with the same functions, methods, and results, or configurations with the same purpose and effects. The present invention also includes configurations in which non-essential parts of the configurations described in the embodiments are replaced. The present invention also includes configurations that achieve the same effects as the configurations described in the embodiments, or configurations that can achieve the same purpose. The present invention also includes configurations in which publicly known technology is added to the configurations described in the embodiments.
[0123] The following can be derived from the above-described embodiment and modified examples.
[0124] The inkjet ink composition comprises A sublimable dye, Sugar alcohols having four or more OH groups; a diol having 2 or 3 carbon atoms; one or more penetrating moisturizers selected from glycol monoethers, diols having 4 or more carbon atoms, amides, and (poly)glyceryl ethers; glycerin in an amount of 1% by mass or less based on the total mass of the inkjet ink composition; Includes.
[0125] According to this inkjet ink composition, sugar alcohols containing 4 or more OH groups are unlikely to volatilize at temperatures up to 220° C., and are unlikely to emit smoke when heated. In addition, according to this inkjet ink composition, by using diols having 2 or 3 carbon atoms, which have high drying properties and low viscosity, in combination with a penetrating moisturizer, it is possible to achieve both low smoke generation and good drying properties on the paper surface. Furthermore, since the ink-jet ink composition contains glycerin at 1% by mass or less, smoke generation is suppressed.
[0126] In the inkjet ink composition, The surface tension of a 10% by mass aqueous solution of the penetrating moisturizer may be 45 mN / m or more and 67 mN / m or less.
[0127] This inkjet ink composition is excellent in color development, intermittent ejection stability, and clogging recovery. Since the surface tension is more appropriate, the permeability is more appropriate, and the color development of the obtained image is better. Furthermore, since the viscosity and / or evaporation thickening property are also better, the clogging recovery and / or intermittent ejection stability are also better.
[0128] In the inkjet ink composition, The penetrating humectant may be present in an amount of 5% by weight or less based on the total weight of the ink-jet ink composition.
[0129] The ink-jet ink composition has excellent clogging recovery properties and color development properties, and also has excellent ink storage stability.
[0130] In the inkjet ink composition, It may further contain at least one selected from polyglycerins and betaines.
[0131] This ink-jet ink composition has excellent intermittent ejection stability. Polyglycerins and betaines have low evaporation thickening properties, and the addition of a small amount of them improves the intermittent ejection stability.
[0132] In the inkjet ink composition, The content of the diol having 2 or 3 carbon atoms may be 5% by mass or more and 15% by mass or less with respect to the total mass of the inkjet ink composition.
[0133] This ink-jet ink composition can further suppress smoke generation, and is also excellent in paper surface drying properties and intermittent ejection.
[0134] In the inkjet ink composition, The sugar alcohol may have a viscosity of 35 mPa·s or less in a 60% by mass aqueous solution.
[0135] This ink-jet ink composition is less susceptible to the evaporation thickening effect of the sugar alcohol, and has even better intermittent ejection stability.
[0136] In the inkjet ink composition, The content of the sugar alcohol may be 3% by mass or more and 15% by mass or less with respect to the total mass of the inkjet ink composition.
[0137] In addition to the above-mentioned effects, this ink-jet ink composition can also provide better recovery from clogging, color development, and intermittent ejection stability.
[0138] In the inkjet ink composition, The penetrating moisturizer may include (poly)glyceryl ethers.
[0139] This ink-jet ink composition produces less smoke and the above-mentioned effects are more pronounced.
[0140] In the inkjet ink composition, The (poly)glyceryl ether may have an average weight molecular weight of 300 or more and 800 or less.
[0141] This ink-jet ink composition can further suppress smoke generation and further improve the color development of images.
[0142] The inkjet recording method includes a recording step of depositing any one of the ink-jet ink compositions described above onto a sheet-like recording medium; a transfer step of superposing the recording surface of the sheet-like recording medium on an object to be dyed and heating the recording surface at a temperature of 150° C. or higher and 220° C. or lower to sublimate and transfer the sublimable dye onto the object to be dyed; a peeling step of peeling the sheet-like recording medium from the object to be dyed after the image transfer; Includes.
[0143] According to this inkjet recording method, the sublimation transfer temperature is 150° C. or higher and 220° C. or lower, so that the volatilization of the sugar alcohol is suppressed and the generation of smoke is suppressed.
[0144] The inkjet recording method includes a recording step of depositing any one of the ink-jet ink compositions described above onto a sheet-like recording medium; a drying step of heating the sheet-like recording medium to which the ink-jet ink composition has been applied to a temperature of 50° C. or higher; a recovery step of winding up the sheet-like recording medium after drying into a roll; Includes.
[0145] According to this inkjet recording method, the diol is evaporated in a drying step of heating to a temperature of 50° C. or higher, so that the paper surface drying property is good and smoke generation during transfer can be suppressed. In addition, since the above-mentioned inkjet ink composition is used, the paper surface drying property is good and offset is unlikely to occur.
[0146] The inkjet recording device an inkjet head for depositing any one of the inkjet ink compositions described above onto a sheet-like recording medium; A heater for heating the sheet-shaped recording medium to a temperature of 50° C. or higher; A roller for winding the sheet-like recording medium into a roll; Includes.
[0147] According to this inkjet recording apparatus, since the above-mentioned inkjet ink composition is used, the paper surface on the recording medium dries well and offset is unlikely to occur even when the recording medium is wound around a roller. [Explanation of symbols]
[0148] 1... recording device, 2... recording head, 3... IR heater, 4... platen heater, 5... after-heater, 6... cooling fan, 7... pre-heater, 8... ventilation fan, 9... supply roll, 10... take-up roll, M... recording medium (intermediate transfer medium)
Claims
1. A sublimable dye, Sugar alcohols having four or more OH groups; a diol having 2 or 3 carbon atoms; one or more penetrating moisturizers selected from glycol monoethers, diols having 4 or more carbon atoms, amides, and (poly)glyceryl ethers; glycerin in an amount of 1% by weight or less based on the total weight of the inkjet ink composition; 1. An ink-jet ink composition comprising:
2. In claim 1, The ink-jet ink composition, wherein a surface tension of a 10% by mass aqueous solution of the penetrating moisturizer is 45 mN / m or more and 67 mN / m or less.
3. In claim 1, The ink-jet ink composition has a penetrating humectant content of 5% by weight or less, based on the total weight of the ink-jet ink composition.
4. In claim 1, The ink-jet ink composition further comprises at least one member selected from polyglycerins and betaines.
5. In claim 1, the content of the diol having 2 or 3 carbon atoms is 5% by mass or more and 15% by mass or less relative to the total mass of the inkjet ink composition.
6. In claim 1, The ink-jet ink composition, wherein the sugar alcohol has a viscosity of 35 mPa·s or less in a 60% by mass aqueous solution.
7. In claim 1, The ink-jet ink composition has a sugar alcohol content of 3% by mass or more and 15% by mass or less relative to the total mass of the ink-jet ink composition.
8. In claim 1, An ink-jet ink composition, wherein the penetrating humectant comprises a (poly)glyceryl ether.
9. In claim 8, The (poly)glyceryl ether has an average weight molecular weight of 300 or more and 800 or less.
10. A recording step of depositing the ink-jet ink composition according to claim 1 onto a sheet-shaped recording medium; a transfer step in which the recording surface of the sheet-like recording medium is superimposed on an object to be dyed, and the recording surface is heated at a temperature of 150° C. or higher and 220° C. or lower to sublimate and transfer the sublimable dye to the object to be dyed; a peeling step of peeling the sheet-like recording medium from the object to be dyed after the image transfer; An inkjet recording method comprising the steps of:
11. The ink-jet ink composition according to any one of claims 1 to 9 is a recording step of attaching the recording medium to a recording medium; a drying step of heating the sheet-shaped recording medium to which the ink-jet ink composition has been applied to a temperature of 50° C. or higher; a recovery step of winding up the sheet-like recording medium after drying into a roll; An inkjet recording method comprising the steps of:
12. An inkjet head that applies the inkjet ink composition according to any one of claims 1 to 9 to a sheet-like recording medium; a heater for heating the sheet-shaped recording medium to a temperature of 50° C. or higher; A roller for winding the sheet-like recording medium into a roll; An inkjet recording apparatus comprising:
Citation Information
Patent Citations
Inkjet recording ink for sublimation transcription and dyeing method
JP2004107647A
Inkjet recording ink for sublimation transfer printing and printing technique
JP2004107648A
Aqueous dispersion, ink composition and inkjet recording method using same