Thermosetting resin composition, winding magnetic field type rotor and power generator
A thermosetting resin composition with controlled viscosity improves adhesion between field windings and iron cores in wound field type rotors, enhancing rotor stability and reliability by reducing misalignment and facilitating efficient heat conduction.
Patent Information
- Application Number
- JP2023078486
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing thermosetting resin compositions used in wound field type rotors exhibit poor adhesion with field windings and/or iron cores, leading to potential misalignment and reduced reliability of generators.
A thermosetting resin composition with a minimum melt viscosity of 40 Pa·s or less, containing epoxy resin, a hardening agent, and inorganic filler, is used to create a fixing member that improves adhesion between field windings and/or iron cores, enhancing the rotor's stability and reliability.
The improved adhesion and filling properties of the resin composition enhance the rotor's reliability by reducing misalignment and enabling efficient heat conduction, while maintaining mechanical strength and insulation.
Smart Images

Figure 2024162685000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a thermosetting resin composition, a wound magnetic field type rotor, and a generator. [Background technology]
[0002] Various studies have been conducted on wound-field rotors. As this type of technology, the techniques described in Patent Documents 1 to 4 are known. Patent Document 1 describes a rotor in which components including a rotor core, a field winding, a permanent magnet, and a rotating shaft are integrally molded with a molding resin (Claim 1 of Patent Document 1, etc.). Patent Document 2 describes a rotor equipped with a winding unit having a field winding wound around an iron core and an insulating seal that seals the iron core and the field winding (claim 1 of Patent Document 2, etc.). It also describes that the iron core and the field winding are sealed in the case by the sealing resin when the sealing resin is poured and hardened (paragraph 0027 of Patent Document 2, etc.).
[0003] Patent Document 3 describes a rotor structure including a field winding wound around the outer periphery of a magnetic pole core, and multiple insulating plates interposed between the outer periphery of the magnetic pole core and the inner periphery of the field winding (Claim 1 of Patent Document 3, etc.). Materials such as aluminum nitride, aluminum oxide, silicon nitride, and boron nitride are given as insulating plates (Claim 3 of Patent Document 3, Claim 1 of Patent Document 4, etc.). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2009-232505 A [Patent Document 2] JP 2022-051589 A [Patent Document 3] JP 2017-108479 A [Patent Document 4] JP 2017-143644 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, as a result of investigations by the present inventors, it was found that in the molding resins described in Patent Documents 1 and 2, and in the insulating plates described in Patent Documents 3 and 4, there is room for improvement in terms of adhesion with the field winding and / or the iron core. [Means for solving the problem]
[0006] The present inventors have investigated the characteristics of the fixing member that fixes the field winding in a wound magnetic field type rotor and have found that by appropriately controlling the minimum melt viscosity of the thermosetting resin composition, it is possible to improve the adhesion between the fixing member made of a cured product of the thermosetting resin composition and the field winding and / or the iron core, thereby completing the present invention.
[0007] According to one aspect of the present invention, there are provided the following thermosetting resin composition, wound magnetic field type rotor, and generator. 1. A thermosetting resin composition used to form a fixing member for fixing a field winding in a wound magnetic field type rotor having a rotor core rotatable in an axial direction and a plurality of field windings held by the rotor core, the thermosetting resin composition comprising: The thermosetting resin composition comprises: Epoxy resin, A hardener; and an inorganic filler, A thermosetting resin composition having a minimum melt viscosity of 40 Pa·s or less as measured using a high-temperature flow tester. 2. The thermosetting resin composition according to 1., the fixing member fixes the field winding and an iron core around which the field winding is wound. 3. The thermosetting resin composition according to 1. or 2., the fixing member being interposed between the field winding and an iron core around which the field winding is wound. 4. The thermosetting resin composition according to any one of 1. to 3., A thermosetting resin composition, in which, when the torque value is measured over time using a Labo Plastomill at a rotation speed of 30 rpm and a measurement temperature of 175°C, the time T1 at which the torque value is equal to or less than twice the minimum torque value is 40 seconds or more and 90 seconds or less, and the minimum torque value is 0.8 N m or less. 5. The thermosetting resin composition according to any one of 1. to 4., The thermosetting resin composition has a flexural modulus at 25°C of 10 GPa or more and 30 GPa or less when cured. 6. The thermosetting resin composition according to any one of 1. to 5., A thermosetting resin composition having a gel time of 40 seconds or more and 100 seconds or less. 7. The thermosetting resin composition according to any one of 1. to 6., A thermosetting resin composition, wherein the thermal conductivity of a cured product of the thermosetting resin composition is 0.7 W / m·K or more. 8. The thermosetting resin composition according to any one of 1. to 7., A thermosetting resin composition, wherein the content of the inorganic filler is 50% by mass or more and 95% by mass or less based on the entire thermosetting resin composition. 9. The thermosetting resin composition according to any one of 1. to 8., The thermosetting resin composition, wherein the inorganic filler comprises crushed silica. 10. The thermosetting resin composition according to any one of 1. to 9., The epoxy resin comprises at least one selected from the group consisting of biphenyl-type epoxy resins, bisphenol-type epoxy resins, stilbene-type epoxy resins, novolac-type epoxy resins, multifunctional epoxy resins, phenol aralkyl-type epoxy resins, and naphthol-type epoxy resins. 11. The thermosetting resin composition according to any one of 1. to 10., A thermosetting resin composition in the form of a powder, granule, tablet or sheet. 12. A rotor core that is rotatable in an axial direction; A wound magnetic field type rotor comprising: a fixing member for fixing the field winding, the fixing member is made of a cured product of a thermosetting resin composition, The thermosetting resin composition comprises: Epoxy resin, A hardener; an inorganic filler; A wound magnetic field type rotor with a minimum melt viscosity of 40 Pa·s or less, measured using a high-speed flow tester. 13. A wound magnetic field type rotor according to 12., a fixed member for fixing the field winding and an iron core around which the field winding is wound; 14. The thermosetting resin composition according to 13., a fixed member disposed between adjacent field windings of the plurality of field windings arranged in a circumferential direction relative to an axial direction of the rotor; 15. A wound magnetic field type rotor according to 12., a wound magnetic field type rotor, wherein the fixed member is interposed between the field winding and an iron core around which the field winding is wound. 16. A wound magnetic field type rotor according to 15., A wound magnetic field type rotor, in which the iron core has a plurality of cores that protrude circumferentially outward relative to the axial direction and are arranged at equal intervals in the circumferential direction. 17. A wound magnetic field type rotor according to any one of 12. to 16., and a stator disposed inside or outside the wound magnetic field type rotor. Effect of the Invention
[0008] According to the present invention, there are provided a thermosetting resin composition having excellent adhesion to a field winding and / or an iron core, and a wound magnetic field type rotor and a generator using the same. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic cross-sectional view of an example of a wound magnetic field type rotor according to an embodiment of the present invention, taken in a direction perpendicular to the rotation axis direction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, similar components are given similar reference numerals and their explanations will be omitted as appropriate. Also, the drawings are schematic diagrams and do not correspond to the actual dimensional ratios.
[0011] The thermosetting resin composition of this embodiment will be outlined below. The thermosetting resin composition of the present embodiment is a fixing resin material for a wound magnetic field type rotor, which is used to form a fixing member that fixes a field winding in a wound magnetic field type rotor that includes a rotor core that can rotate in an axial direction and a plurality of field windings held by the rotor core.
[0012] Such a thermosetting resin composition contains an epoxy resin, a curing agent, and an inorganic filler, and is configured so as to have a minimum melt viscosity of 40 Pa·s or less as measured using a high-temperature flow tester.
[0013] According to the findings of the present inventors, it has been found that by appropriately controlling the minimum melt viscosity of the thermosetting resin composition, it is possible to improve the adhesion between the fixing member made of the cured product of the thermosetting resin composition and the field winding and / or the iron core. Although the detailed mechanism is unclear, it is presumed that by having an appropriate minimum melt viscosity during the molding process of the thermosetting resin composition, the filling property onto the surface of the field winding and / or the iron core becomes appropriate, thereby improving the adhesion thereto.
[0014] Furthermore, in the method for producing a wound magnetic field type rotor using the thermosetting resin composition of this embodiment, the filling property on the surface of the field winding and / or the iron core can be improved, and the workability in the fixing step can be improved.
[0015] [Wound magnetic field type rotor] The wound magnetic field type rotor of this embodiment can be combined with a stator to form a generator (motor). One example of this generator includes a wound magnetic field rotor and a stator disposed inside or outside the wound magnetic field rotor.
[0016] Here, a configuration example of the above-mentioned wound magnetic field type rotor 10 will be described with reference to FIG. 1 includes a rotor core 1 that is rotatable in the axial direction, a plurality of field windings 2 held by the rotor core 1, and a fixing member that fixes the field windings 2. This fixing member is made of a cured product of the thermosetting resin composition of this embodiment.
[0017] In the wound magnetic field type rotor 10 of the first embodiment, the fixing member may be a sealing member that fixes the field winding 2 and the iron core 3 around which the field winding 2 is wound. This suppresses misalignment of the field winding 2 and the iron core 3 due to rotational vibrations or the like in different components, thereby improving the reliability of the generator.
[0018] Furthermore, in the first embodiment, the fixing member may be filled between the most adjacent field windings 2 among the multiple field windings 2 arranged in the circumferential direction relative to the axial core direction. In this case, the fixing member filling at least a part or the entire space between the most adjacent windings can fix the adjacent field windings 2 and the iron core 3. This can further suppress misalignment of components due to the direction of rotation, thereby improving the reliability of the generator.
[0019] In the wound magnetic field type rotor 10 of the second embodiment, the fixed member may be an insulating member interposed between the field winding 2 and the iron core 3 around which the field winding 2 is wound. In this case, the fixed member may be a reel having a structure for winding the field winding 2. The reel structure of the fixed member can be formed by die molding or the like. This makes it possible to improve the insulation between the field winding 2 and the iron core 3 while stably fixing the field winding 2. In the second embodiment, the iron core 3 may include a plurality of iron cores 3 that protrude circumferentially outward relative to the axial direction and are arranged at equal intervals in the circumferential direction.
[0020] In the first embodiment, by increasing the filling ability of the thermosetting resin composition used to mold the fixing member, it is possible to suppress insufficient filling of the space between the nearest neighbors. In the second embodiment, the moldability of the fixing member having a thin layer structure is also increased in order to place the fixing member in the gap between the field winding 2 and the iron core 3.
[0021] By increasing the thermal conductivity of the fixing member, it becomes possible to efficiently transfer heat from the field winding 2 during rotation of the rotor core 1. This allows the wound magnetic field type rotor 10 to be made more compact. Typically, the thermal conductivity of the air that the outer surface of the field winding comes into contact with is approximately 0.02 W / m K at room temperature, and the thermal conductivity of the insulating paper used to insulate the field winding from the iron core is approximately 0.06 W / m K at room temperature.
[0022] Increasing the mechanical strength of the fixing member makes it possible to suppress deformation of the fixing member during rotation of the rotor core 1. This improves the reliability of the generator.
[0023] The rotor core 1 may have a cylindrical shape. A shaft hole is provided at the center of the rotor core 1. The rotor core 1 may be formed into a cylindrical shape by laminating a plurality of metal plates in the axial direction. The individual metal plates may be fixed to each other in an insulated state with an insulating adhesive interposed between them. In addition, the rotor core 1 may be provided with multiple permanent magnet units along the circumferential direction centered on the axial direction, each having a permanent magnet and a hole for accommodating the permanent magnet, but it is not necessary for the rotor core 1 to have such a permanent magnet unit.
[0024] A plurality of the field windings 2 may be held by the rotor core 1 so as to be arranged at equal intervals in the circumferential direction centered on the axial direction. The iron core 3 around which the field winding 2 is wound may be configured with a laminated structure of electromagnetic steel sheets. The iron core 3 may be configured with the same material as the rotor core 1, or may be configured with a different material. In the generator described above, the magnetic flux can be controlled to a desired amount by passing current through the field winding 2 from outside the rotor core 1 (rotor).
[0025] <Method of Manufacturing Wound Magnetic Field Type Rotor 10> An example of a manufacturing method for the wound magnetic field type rotor 10 of the first embodiment includes a step of filling a thermosetting resin composition into a rotor core 1 having a field winding 2 and an iron core 3, for example, by insert molding, to form a fixing member that fixes at least a portion of the field winding 2 and the iron core, and / or fills the space between the nearest adjacent parts. Furthermore, an example of a manufacturing method for the wound magnetic field type rotor 10 of the second embodiment may include a step of filling a thermosetting resin composition into a rotor core 1 having an iron core 3, for example, by insert molding or the like, forming a fixed member that serves as a reel around which the field winding 2 is wound, and winding the field winding 2 around the reel (fixed member).
[0026] [Thermosetting resin composition] Hereinafter, the components used in the thermosetting resin composition of the present embodiment (sometimes referred to simply as "resin composition" in this specification) will be described.
[0027] (Epoxy resin) Examples of the epoxy resin used in the thermosetting resin composition of the present embodiment include bifunctional or crystalline epoxy resins such as biphenyl type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, stilbene type epoxy resins, and hydroquinone type epoxy resins; novolac type epoxy resins such as cresol novolac type epoxy resins, phenol novolac type epoxy resins, and naphthol novolac type epoxy resins; phenol aralkyl type epoxy resins such as phenylene skeleton-containing phenol aralkyl type epoxy resins, biphenylene skeleton-containing phenol aralkyl type epoxy resins, and phenylene skeleton-containing naphthol aralkyl type epoxy resins; trifunctional type epoxy resins such as triphenol methane type epoxy resins and alkyl-modified triphenol methane type epoxy resins; modified phenol type epoxy resins such as dicyclopentadiene-modified phenol type epoxy resins and terpene-modified phenol type epoxy resins; heterocyclic type epoxy resins such as triazine nucleus-containing epoxy resins, etc. These may be used alone or in combination of two or more. From the viewpoints of ensuring the fluidity of the resulting resin composition and the strength of a cured product of the resin composition, the epoxy resin preferably contains one or more epoxy resins selected from the group consisting of phenol novolac type epoxy resins and phenol aralkyl type epoxy resins, and more preferably contains a cresol novolac type epoxy resin.
[0028] The content of the epoxy resin in the resin composition may be, for example, 3 mass% or more, preferably 8 mass% or more, more preferably 10 mass% or more, and even more preferably 12 mass% or more, based on the total solid content of the resin composition, from the viewpoint of improving the fluidity of the obtained resin composition and improving the workability and moldability. In addition, from the viewpoint of improving the strength and heat resistance of a cured product formed using the resin composition, the content of the epoxy resin is preferably 30 mass % or less, and more preferably 20 mass % or less, based on the total solid content of the resin composition.
[0029] In this embodiment, the total solid content of the resin composition refers to the non-volatile content in the resin composition, and refers to the remainder excluding volatile components such as water, solvent, etc. In addition, in this embodiment, the content relative to the total amount of the resin composition refers to the content relative to the total solid content of the resin composition excluding the solvent, when a solvent is included.
[0030] In one embodiment, the resin composition may further contain a thermosetting resin other than the epoxy resin. Examples of the thermosetting resin that can be used include bismaleimide resin, benzoxazine resin, phenol resin, urea resin, melamine resin, unsaturated polyester resin, polyurethane resin, diallyl phthalate resin, silicone resin, cyanate resin, polyimide resin, polyamideimide resin, and benzocyclobutene resin. These thermosetting resins may be used alone or in combination of two or more.
[0031] (hardening agent) The curing agent used in the thermosetting resin composition of the present embodiment is not limited as long as it is generally used in resin compositions containing epoxy resins, and examples thereof include phenolic resin-based curing agents, amine-based curing agents, acid anhydride-based curing agents, mercaptan-based curing agents, and other curing agents. Among these, phenolic resin-based curing agents are preferred in terms of the balance of flame resistance, moisture resistance, electrical properties, curability, storage stability, and the like.
[0032] The phenolic resin-based curing agent may be, for example, any one generally used in epoxy resin compositions. More specifically, the phenolic resin-based curing agent may be a novolac resin obtained by condensing or co-condensing phenols such as phenol novolac resin, cresol novolac resin, cresol, resorcin, catechol, bisphenol A, bisphenol F, phenylphenol, aminophenol, α-naphthol, β-naphthol, dihydroxynaphthalene, and the like with formaldehyde or ketones under an acid catalyst; a phenol aralkyl resin having a phenylene skeleton synthesized from the above-mentioned phenols and dimethoxyparaxylene or bis(methoxymethyl)biphenyl; a phenol aralkyl resin such as a phenol aralkyl resin having a biphenylene skeleton; and a phenolic resin having a trisphenylmethane skeleton. These may be used alone or in combination of two or more. The phenolic resin-based curing agent preferably includes a phenol novolac resin.
[0033] When the curing agent is a phenolic resin-based curing agent, the equivalent ratio between the epoxy resin and the curing agent, i.e., the ratio of (the number of moles of epoxy groups in the epoxy resin / the number of moles of phenolic hydroxyl groups in the phenolic resin-based curing agent) is preferably 0.5 or more, more preferably 0.6 or more, and even more preferably 0.8 or more, from the viewpoint of improving the moldability and reliability of the resin composition. Also, from the same viewpoint, the above ratio is preferably 2 or less, more preferably 1.8 or less, and even more preferably 1.5 or less.
[0034] Examples of amine-based curing agents include aliphatic polyamines such as diethylenetriamine (DETA), triethylenetetramine (TETA), and metaxylylenediamine (MXDA); aromatic polyamines such as diaminodiphenylmethane (DDM), m-phenylenediamine (MPDA), and diaminodiphenylsulfone (DDS); and polyamine compounds such as dicyandiamide (DICY) and organic acid dihydralazide. These may be used alone or in combination of two or more.
[0035] Examples of the acid anhydride curing agent include alicyclic acid anhydrides such as hexahydrophthalic anhydride (HHPA), methyltetrahydrophthalic anhydride (MTHPA), and maleic anhydride; and aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), benzophenonetetracarboxylic acid (BTDA), and phthalic anhydride. These may be used alone or in combination of two or more.
[0036] Examples of mercaptan-based curing agents include trimethylolpropane tris(3-mercaptobutyrate) and trimethylolethane tris(3-mercaptobutyrate). These may be used alone or in combination of two or more.
[0037] Examples of other curing agents include isocyanate compounds such as isocyanate prepolymers and blocked isocyanates; and organic acids such as carboxylic acid-containing polyester resins. The curing agent may be a combination of two or more different types of curing agents from the above.
[0038] From the viewpoint of realizing excellent fluidity and improving filling properties and moldability, the content of the curing agent in the resin composition is preferably 0.5 mass % or more, more preferably 1 mass % or more, and even more preferably 3 mass % or more, based on the total amount of the resin composition. On the other hand, from the viewpoint of improving the moisture resistance reliability and heat resistance of the cured resin product, the content of the curing agent is preferably 20 mass % or less, more preferably 15 mass % or less, even more preferably 10 mass % or less, and even more preferably 5 mass % or less, based on the total amount of the resin composition.
[0039] (Inorganic filler) Examples of inorganic fillers include fused silica such as fused crushed silica and fused spherical silica, silica such as crystalline silica, alumina, aluminum hydroxide, silicon nitride, and aluminum nitride. These may be used alone or in combination of two or more. From the viewpoint of making the mechanical properties or thermal properties of the cured product of the resin composition favorable, the inorganic filler preferably contains silica, and more preferably contains one or more selected from the group consisting of crushed silica and fused spherical silica.
[0040] The average particle size d50 of the inorganic filler is preferably 0.01 μm or more, more preferably 1 μm or more, and even more preferably 5 μm or more, from the viewpoint of improving the fluidity of the resin composition and improving moldability. Also, the average particle size d50 of the inorganic filler is preferably 50 μm or less, more preferably 40 μm or less, from the viewpoint of improving the filling property and suppressing the occurrence of unfilled portions.
[0041] In addition, two or more fillers having different average particle diameters d50 may be used in combination as the inorganic filler. This makes it possible to more effectively increase the filling ability of the inorganic filler relative to the total solid content of the resin composition. For example, from the viewpoint of improving the filling ability of the resin composition, the inorganic filler preferably includes a first filler having an average particle diameter of 1 μm or more and 12 μm or less, and a second filler having an average particle diameter of more than 12 μm and 30 μm or less. From the same viewpoint, the inorganic filler may include, for example, a first filler having an average particle diameter of 0.01 μm or more and 1 μm or less, and a second filler having an average particle diameter of more than 1 μm and 50 μm or less.
[0042] In addition, the value of (d50 / d90) calculated from the particle diameter d90 of the inorganic filler with a cumulative frequency of 90% measured using a laser diffraction particle size distribution analyzer and the average particle diameter d50 of the inorganic filler is preferably 0.2 or more, more preferably 0.25 or more, and even more preferably 0.3 or more, from the viewpoint of improving the fluidity of the resin composition. In addition, in order to improve the narrow-part filling property, the above ratio (d50 / d90) is preferably 1.0 or less, more preferably 0.9 or less, and even more preferably 0.8 or less.
[0043] Here, the particle size of the inorganic filler, specifically d50 and d90, can be obtained by measuring the particle size distribution of the particles on a volume basis using a commercially available laser diffraction particle size distribution measuring device (e.g., SALD-7000, manufactured by Shimadzu Corporation).
[0044] The content of the inorganic filler in the resin composition is preferably 50% by mass or more, more preferably 65% by mass or more, and even more preferably 80% by mass or more, based on the total amount of the resin composition, from the viewpoint of suppressing the moisture absorption and thermal expansion of the resin composition and more effectively improving the temperature cycle resistance and moisture resistance of the cured product of the resin composition. In addition, from the viewpoint of more effectively improving the flowability and filling property during molding of the resin composition, the content of the inorganic filler is preferably 95% by mass or less, more preferably 93% by mass or less, based on the total amount of the resin composition.
[0045] In addition, when the inorganic filler contains silica, the content of silica in the resin composition is preferably 50 mass % or more, more preferably 65 mass % or more, and even more preferably 80 mass % or more, based on the total amount of the resin composition, from the viewpoint of suppressing the moisture absorption and thermal expansion of the resin composition and more effectively improving the temperature cycle resistance and moisture resistance of the cured product of the resin composition. From the viewpoint of more effectively improving the fluidity and filling property of the resin composition during molding, the content of silica in the resin composition is preferably 95% by mass or less, and more preferably 93% by mass or less.
[0046] (Other Ingredients) In this embodiment, the resin composition may further contain other components in addition to the above-mentioned components. Examples of other components include a curing accelerator, a coupling agent, a release agent, a low stress component, a flame retardant, an ion trapping agent, a colorant, and an antioxidant. These may be used alone or in combination of two or more.
[0047] The curing accelerator may be any accelerator that accelerates the crosslinking reaction between the epoxy resin and the curing agent, and any accelerator that is generally used in epoxy resin compositions may be used. Specific examples of the curing accelerator include diazabicycloalkenes and derivatives thereof such as 1,8-diazabicyclo(5,4,0)undecene-7; organic phosphines such as triphenylphosphine and methyldiphenylphosphine; imidazole compounds (imidazole-based curing accelerators described below); and tetra-substituted phosphoniums such as tetraphenylphosphonium tetraphenylborate and tetraphenylphosphonium 2,3-dihydroxynaphthalate.
[0048] Examples of the imidazole-based curing accelerator include imidazole, 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, and 1-cyanoethyl-2-phenylimidazolium trimellitate. imidazole, 2,4-diamino-6-[2-methylimidazolyl(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4-methylimidazolyl(1')]-ethyl-s-triazine, an isocyanuric acid adduct of 2,4-diamino-6-[2'-methylimidazolyl(1')]-ethyl-s-triazine, an isocyanuric acid adduct of 2-phenylimidazole, an isocyanuric acid adduct of 2-methylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4,5-dihydroxydimethylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole.
[0049] As the coupling agent, for example, various silane-based compounds such as epoxysilane, mercaptosilane, aminosilane, alkylsilane, ureidosilane, vinylsilane, methacrylsilane, titanium-based compounds, aluminum chelates, aluminum / zirconium-based compounds, and other known coupling agents can be used. Examples of these include vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-methacryloxypropyltriethoxysilane, vinyltriacetoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-anilinopropyltrimethoxysilane, γ-anilinopropylmethyldimethoxysilane, γ-[bis(β-hydroxyethyl)]aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyl N-(vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, N-(vinylbenzylaminoethyl)-γ-aminopropyltriethoxysilane, N-(vinylbenzylaminoethyl)-γ-aminopropylmethyldimethoxysilane, phenylaminopropyltrimethoxysilane, γ-(β-aminoethyl)aminopropyldimethoxymethylsilane, N-(trimethoxysilylpropyl)ethylenediamine, N-(dimethoxymethylsilylisopropyl)ethylenediamine, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, N-(vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, hexamethyldisilane, vinyltrimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-triethoxysilyl-N-(1,Silane coupling agents such as hydrolyzate of 3-dimethyl-butylidene)propylamine, isopropyl triisostearoyl titanate, isopropyl tris(dioctyl pyrophosphate) titanate, isopropyl tri(N-aminoethyl-aminoethyl) titanate, tetraoctyl bis(ditridecyl phosphite) titanate, tetra(2,2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphate)oxyacetate titanate Examples of titanate-based coupling agents include ethylene titanate, bis(dioctyl pyrophosphate) titanate, isopropyl trioctanoyl titanate, isopropyl dimethacryl isostearoyl titanate, isopropyl tridodecylbenzenesulfonyl titanate, isopropyl isostearoyl diacryl titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumyl phenyl titanate, and tetraisopropyl bis(dioctyl phosphite) titanate. These may be used alone or in combination of two or more. Among these, silane-based compounds such as epoxy silane, mercapto silane, amino silane, alkyl silane, ureido silane, or vinyl silane are more preferred. In addition, from the viewpoint of more effectively improving filling properties and moldability, it is even more preferred to use secondary amino silanes such as phenyl aminopropyl trimethoxy silane.
[0050] When a coupling agent is used, the content is preferably 0.05% by mass or more, more preferably 0.10% by mass or more, based on the total solid content of the resin composition, from the viewpoint of making the flowability of the resin composition favorable. Also, from the viewpoint of improving the mechanical strength of the cured product of the resin composition, the content of the coupling agent is preferably 1.5% by mass or less, more preferably 1.0% by mass or less, and even more preferably 0.5% by mass or less, based on the total solid content of the resin composition.
[0051] The release agent can include, for example, one or more selected from the group consisting of natural waxes such as carnauba wax; synthetic waxes such as Montan acid ester wax and oxidized polyethylene wax; higher fatty acids such as zinc stearate and metal salts thereof; paraffin; and carboxylic acid amides such as erucic acid amide. An example of the ion scavenger is hydrotalcite. Examples of low stress components include silicones such as silicone oil, silicone rubber, silicone elastomer, and silicone resin; and acrylonitrile butadiene rubber. Examples of the flame retardant include aluminum hydroxide, magnesium hydroxide, zinc borate, zinc molybdate, and phosphazene. Examples of the antioxidant include hindered phenol compounds, hindered amine compounds, and thioether compounds.
[0052] Examples of the colorant include carbon black, red iron oxide, titanium oxide, etc. Among them, carbon black is preferably used as the colorant. The content of the colorant is preferably 0.05% by mass or more, more preferably 0.10% by mass or more, based on the total amount of the resin composition, from the viewpoint of obtaining a preferable appearance of the cured product of the resin composition. Also, from the viewpoint of obtaining a preferable resin viscosity, the content of the colorant is preferably 1.5% by mass or less, more preferably 1.0% by mass or less, and even more preferably 0.5% by mass or less, based on the total amount of the resin composition.
[0053] (Characteristics of the thermosetting resin composition or its cured product) Next, the properties of the thermosetting resin composition of this embodiment or the cured product thereof will be described. The thermosetting resin composition of the present embodiment containing the above components has a minimum melt viscosity of 40 Pa·s or less, and preferably 35 Pa·s or less, which can improve the filling property of the thermosetting resin composition. The lower limit of the minimum melt viscosity of the resin composition is, for example, 5 Pa·s or more, which can improve the insulating properties of the fixing member. Furthermore, the resin composition of the present embodiment has a minimum melt viscosity within the above range, and as a result, has good filling properties and good workability.
[0054] When the torque value of the resin composition of this embodiment is measured over time using a Labo Plastomill at a rotation speed of 30 rpm and a measurement temperature of 175°C, the time T1 at which the torque value is equal to or less than twice the minimum torque value is 40 seconds or more and 90 seconds or less, and the minimum torque value is 0.8 N m or less.
[0055] The flexural modulus of the cured product of the resin composition measured at 25° C. is 10 GPa or more, more preferably 12 GPa or more, from the viewpoint of increasing the strength of the cured product. Also, from the viewpoint of making the stress relaxation property of the cured product preferable, the flexural modulus of the cured product measured at 25° C. is 30 GPa or less, more preferably 25 GPa or less. The flexural modulus of the cured resin composition is measured in accordance with JIS K 7171, for example.
[0056] The gel time of the resin composition of the present embodiment is preferably 40 seconds or more, more preferably 50 seconds or more, from the viewpoint of improving the moldability of the resin composition and accelerating the molding cycle, and is preferably 100 seconds or less, more preferably 90 seconds or less, from the viewpoint of realizing a cured product with excellent curability.
[0057] The gel time can be measured by melting the resin composition on a hot plate heated to 175° C., and then kneading the composition with a spatula while measuring the time it takes for the composition to become tack-free (gel time).
[0058] The resin composition of this embodiment has a thermal conductivity of, for example, 0.7 W / m·K or more, preferably 2 W / m·K or more, and more preferably 3 W / m·K or more, after curing.
[0059] [Method for producing thermosetting resin composition] The resin composition of the present embodiment can be produced by uniformly mixing the above components and other additives used as necessary in a mixer or blender such as a tumbler mixer or Henschel mixer to a predetermined content, and then kneading while heating with a kneader, roll, disperser, azihomobister, planetary mixer, etc. The temperature during kneading must be in a temperature range in which a curing reaction does not occur, and although it depends on the composition of the epoxy resin and curing agent, it is preferable to melt-knead at about 70 to 150 ° C. After kneading, it may be cooled and solidified, and the kneaded product may be processed into a powder, granule, tablet, or sheet.
[0060] A method for obtaining a powdered resin composition includes, for example, a method of crushing the kneaded material with a crushing device. The kneaded material may be formed into a sheet and crushed. Examples of the crushing device that can be used include a hammer mill, a stone mill, and a roll crusher.
[0061] As a method for obtaining a granular or powdery resin composition, for example, a granulation method represented by a hot-cut method can be used in which a die having a small diameter is provided at the outlet of a kneading device, and the molten kneaded material discharged from the die is cut to a predetermined length with a cutter, etc. In this case, after obtaining a granular or powdery resin composition by a granulation method such as the hot-cut method, it is preferable to perform degassing before the temperature of the resin composition drops too much.
[0062] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. EXAMPLES
[0063] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.
[0064] The raw material components used in each of the Examples and Comparative Examples are shown below. (Epoxy resin) Epoxy resin 1: Orthocresol novolac type epoxy resin (DIC, EPICRON N-670) Epoxy resin 2: Orthocresol novolac type epoxy resin (DIC, EPICRON N-660) Epoxy resin 3: Biphenyl type epoxy resin (Mitsubishi Chemical Corporation, YX-4000K)
[0065] (hardening agent) Hardener 1: Novolac-type phenol compound (Sumitomo Bakelite Co., Ltd., PR-51470) Hardener 2: Novolac-type phenol compound (Sumitomo Bakelite Co., Ltd., PR-51714) Hardener 3: Triphenolmethane type phenolic resin (Meiwa Kasei Co., Ltd., MEH-7500)
[0066] (Inorganic filler) Inorganic filler 1: Fused spherical silica (Denka, FB-950) Inorganic filler 2: Fused spherical silica (Denka, FB-105) Inorganic filler 3: Fused crushed silica (Fumitec, FMT-15C) Inorganic filler 4: Glass fiber (manufactured by Nitto Boseki, CS3E479) Inorganic filler 5: Crystal crushed silica (Tatsumori Co., Ltd., HFC-7) Inorganic filler 6: Fused spherical alumina (Denka, DAB-45SI)
[0067] (Cure accelerator) Curing accelerator 1: Tetraphenylphosphonium 2,3-dihydroxynaphthalate Curing accelerator 2: 2-phenyl-4,5-dihydroxymethylimidazole (Shikoku Chemical Industry Co., Ltd., 2PHZ-PW)
[0068] (Release agent) Wax 1: Carnauba wax (TOWAX-132, manufactured by Toa Kasei Co., Ltd.)
[0069] (Silane coupling agent) Silane coupling agent 1: N-phenyl-3-aminopropyltrimethoxysilane (Toray Dow Corning, CF-4083) (Coloring agent) Colorant 1: Carbon black (Mitsubishi Chemical, Carbon #5)
[0070] (Preparation of Thermosetting Resin Composition) The raw materials formulated according to Table 1 were mixed at room temperature using a mixer, and then roll-kneaded at 70° C. to 110° C. The resulting kneaded product was then cooled and pulverized to obtain a thermosetting resin composition.
[0071] [Table 1]
[0072] The thermosetting resin composition obtained in each example was subjected to the following measurements. The measurement results are shown in Table 1.
[0073] (Minimum melt viscosity) The obtained thermosetting resin composition was subjected to a test at a temperature of 175°C, a test pressure P (load 40 kgf, piston area 1 cm) using a high-temperature flow tester (Shimadzu Corporation, CFT-500C). 2 , 3.9×10 6 The flow rate Q (cm Pa) of the thermosetting resin composition dissolved in a constant temperature test under the conditions of a die hole diameter D of 0.50 mm and a die length L of 1.00 mm. 3 The apparent viscosity η (Pa·sec) was calculated based on the following formula. The minimum viscosity during flow among the apparent viscosities η was defined as the "minimum melt viscosity." Formula: Apparent viscosity η = (π D 4 P×10 3 / 128×L Q) η: Apparent viscosity D: Die hole diameter (mm) P: Test pressure (Pa) L: Die length (mm) Q: Flow rate (cm 3 / sec) In the formula, Q is the flow rate of the thermosetting resin composition flowing per unit time.
[0074] (Spiral Flow) Spiral flow measurements were performed using a low-pressure transfer molding machine ("KTS-15" manufactured by Kotaki Seiki Co., Ltd.) by injecting the thermosetting resin composition into a mold for spiral flow measurement conforming to EMMI-1-66 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 120 seconds, and measuring the flow length (cm).
[0075] (Gel Time) The gel time was measured by melting the thermosetting resin composition on a hot plate heated to 175° C., and then kneading the composition with a spatula while measuring the time it took for the composition to harden (gel time: seconds).
[0076] (glass transition temperature, linear expansion coefficient (α1)) Using a transfer molding machine, the thermosetting resin composition was injected and molded at a mold temperature of 175°C, injection pressure of 9.8MPa, and curing time of 3 minutes to obtain a test piece of 15mm x 4mm x 4mm. The obtained test piece was then post-cured at 175°C for 4 hours, and then measured using a thermomechanical analyzer (Seiko Denshi Kogyo Co., Ltd., TMA100) under the conditions of a measurement temperature range of 40°C to 300°C and a heating rate of 5°C / min. From the measurement results, the glass transition temperature and the linear expansion coefficient (α1) in the measurement temperature range of 40°C to 80°C were calculated.
[0077] (Flexural modulus) The thermosetting resin composition was transfer molded at 175° C. for 3 minutes, and then cured at 175° C. for 4 hours. The flexural modulus at 25° C. was measured in accordance with JIS K 7171.
[0078] (Bending strength) A cured product was prepared in the same manner as in the measurement of the flexural modulus above, and the flexural strength at 25° C. was measured in accordance with JIS K 7171.
[0079] (Thermal Conductivity) Using a transfer molding machine, the thermosetting resin composition was injected and molded at a mold temperature of 175° C., an injection pressure of 9.8 MPa, and a curing time of 3 minutes to obtain a cured body measuring 10 mm×10 mm×1 mm. The thermal conductivity of the obtained cured material was calculated using the following formula from the thermal diffusion coefficient (α) measured by the laser flash method (half-time method), the specific heat (Cp) measured by the DSC method, and the density (ρ) measured in accordance with JIS K 6911. The unit of thermal conductivity is W / m K. Thermal conductivity [W / m K]=α[mm 2 / s]×Cp[J / kg K]×ρ[g / cm 3 ]
[0080] (Dielectric breakdown strength) Using a transfer molding machine, the thermosetting resin composition was injected and molded at a mold temperature of 175° C., an injection pressure of 9.8 MPa, and a curing time of 3 minutes to obtain a cured body of 100 mmφ×2 mm. The dielectric breakdown voltage of the cured product obtained above was measured in accordance with JIS K 6911 as follows. First, the cured product obtained was sandwiched between circular electrodes and placed in insulating oil. Next, an AC voltage was applied to both electrodes using a Kikusui Electronics TOS9201 so that the voltage increased at a rate of 2.5 kV / sec. The voltage at which the test piece broke down was taken as the dielectric breakdown voltage.
[0081] (Curing behavior measurement) Using a kneading extrudability tester (4C150, manufactured by Toyo Seiki Seisakusho Co., Ltd.), the melt torque of the thermosetting resin composition was measured over time under conditions of a rotation speed of 30 rpm and a measurement temperature of 175°C. Next, the time T1 at which the torque value was equal to or less than twice the minimum torque value was calculated based on the measurement results. The measurement start point was the point at which the torque started to decrease after the material was put into the kneading extrudability tester and the torque rose sharply. The minimum torque value was also calculated from the measurement results.
[0082] (Adhesion) The obtained thermosetting resin composition was used to mold ten adhesion strength test pieces, each having a size of 3.6 mmφ×3 mm, onto a 9×29 mm rectangular test copper lead frame or onto a laminated steel plate, using a low-pressure transfer molding machine (manufactured by Yamashiro Seiki Co., Ltd., "AV-600-50-TF") under conditions of a mold temperature of 175°C, an injection pressure of 10 MPa, and a curing time of 180 seconds. The samples were then cured at 175°C for 3 hours, and the die shear strength (MPa) was measured at room temperature of 25°C using an automatic die shear measuring device (Nordson Advanced Technology Corp., DAGE4000).
[0083] The thermosetting resin compositions of Examples 1 to 4 showed good adhesion to copper and to laminated steel sheets. In addition, it was found that the thermosetting resin compositions of Examples 1 to 4 exhibited good filling properties into narrow gaps due to their relatively large spiral flow values, and / or good insulating properties due to their relatively large dielectric breakdown strength values. The thermosetting resin composition of such an embodiment can be suitably used as a fixing member for fixing the field winding and / or the iron core in a wound magnetic field type rotor. [Explanation of symbols]
[0084] 1 Rotor core 2 Field Winding 3. Iron Core 10 Winding Magnetic Field Rotor
Claims
1. A thermosetting resin composition used to form a fixing member for fixing a field winding in a wound magnetic field type rotor including a rotor core rotatable in an axial direction and a plurality of field windings held by the rotor core, the thermosetting resin composition comprising: The thermosetting resin composition comprises: Epoxy resin, A hardener; and an inorganic filler, A thermosetting resin composition having a minimum melt viscosity of 40 Pa·s or less as measured using a high-temperature flow tester.
2. The thermosetting resin composition according to claim 1, the fixing member fixes the field winding and an iron core around which the field winding is wound.
3. The thermosetting resin composition according to claim 1, the fixing member being interposed between the field winding and an iron core around which the field winding is wound.
4. The thermosetting resin composition according to claim 2 or 3, When the torque value was measured over time using a Labo Plastomill at a rotation speed of 30 rpm and a measurement temperature of 175° C., the time T at which the torque value was equal to or less than twice the minimum torque value was determined. 1 The thermosetting resin composition has a hardness of 40 seconds or more and 90 seconds or less, and a minimum torque value of 0.8 N·m or less.
5. The thermosetting resin composition according to claim 2 or 3, The thermosetting resin composition has a flexural modulus at 25°C of 10 GPa or more and 30 GPa or less when cured.
6. The thermosetting resin composition according to claim 2 or 3, A thermosetting resin composition having a gel time of 40 seconds or more and 100 seconds or less.
7. The thermosetting resin composition according to claim 2 or 3, A thermosetting resin composition, wherein the thermal conductivity of a cured product of the thermosetting resin composition is 0.7 W / m·K or more.
8. The thermosetting resin composition according to claim 2 or 3, A thermosetting resin composition, wherein the content of the inorganic filler is 50% by mass or more and 95% by mass or less based on the entire thermosetting resin composition.
9. The thermosetting resin composition according to claim 2 or 3, The thermosetting resin composition, wherein the inorganic filler comprises crushed silica.
10. The thermosetting resin composition according to claim 2 or 3, The epoxy resin comprises at least one selected from the group consisting of a biphenyl-type epoxy resin, a bisphenol-type epoxy resin, a stilbene-type epoxy resin, a novolac-type epoxy resin, a multifunctional epoxy resin, a phenol aralkyl-type epoxy resin, and a naphthol-type epoxy resin.
11. The thermosetting resin composition according to claim 2 or 3, A thermosetting resin composition in the form of a powder, granule, tablet or sheet.
12. A rotor core that is rotatable in an axial direction; A wound magnetic field type rotor comprising: a fixing member for fixing the field winding, the fixing member is made of a cured product of a thermosetting resin composition, The thermosetting resin composition comprises: Epoxy resin, A hardener; and an inorganic filler, A wound magnetic field type rotor having a minimum melt viscosity of 40 Pa·s or less as measured using a high-temperature flow tester.
13. 13. The wound magnetic field type rotor according to claim 12, a fixed member for fixing the field winding and an iron core around which the field winding is wound;
14. The thermosetting resin composition according to claim 13, a fixed member disposed between adjacent field windings of the plurality of field windings arranged in a circumferential direction relative to an axial direction of the rotor;
15. 13. The wound magnetic field type rotor according to claim 12, a wound magnetic field type rotor, wherein the fixed member is interposed between the field winding and an iron core around which the field winding is wound.
16. 16. The wound magnetic field type rotor according to claim 15, A wound magnetic field type rotor, in which the iron core has a plurality of cores that protrude circumferentially outward relative to the axial direction and are arranged at equal intervals in the circumferential direction.
17. A wound magnetic field type rotor according to any one of claims 12 to 16, and a stator disposed inside or outside the wound magnetic field type rotor.
Citation Information
Patent Citations
Rotating field type synchronous machine
JP2009232505A
Rotor structure for rotary electric machine
JP2017108479A
Rotary electric machine
JP2017143644A
Rotor and rotary machine
JP2022051589A