Photosensitive resin composition, transfer film, pattern forming method, and cured product
The photosensitive resin composition with specific components achieves high-resolution transfer patterns and excellent physical properties, addressing the limitations of existing compositions in forming small-diameter vias with improved mechanical strength and dielectric properties.
Patent Information
- Application Number
- JP2023078493
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
AI Technical Summary
Existing photosensitive resin compositions used in build-up layers of printed wiring boards lack sufficient physical properties and resolution, particularly in forming small-diameter vias, with issues in mechanical strength, linear expansion, and dielectric properties.
A photosensitive resin composition comprising specific components such as an alkali-soluble resin, a compound with a phenylene ether structure, and ethylenically unsaturated bonds, balanced with a mass ratio and proportions to achieve high resolution and excellent physical properties, including a transfer film for forming vias with diameters less than 20 μm.
The composition enables high-resolution transfer patterns with improved mechanical strength, low linear expansion, and low dielectric loss tangent, suitable for insulating layers in printed wiring boards and semiconductor devices.
Smart Images

Figure 2024162690000001 
Figure 2024162690000002 
Figure 2024162690000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a photosensitive resin composition, a transfer film, a pattern forming method, and a cured product. [Background technology]
[0002] In recent years, electronic devices have become smaller and more powerful. For example, in printed wiring boards, the wiring density has increased due to finer wiring and more multi-layered build-up layers. Also, there is a demand for smaller diameter via holes (hereinafter sometimes simply referred to as "vias") provided for electrical continuity in the build-up layers.
[0003] A thermosetting resin composition is generally used as a material for the build-up layer, and the processing for forming vias is mainly performed by the laser via method. In order to meet the demand for smaller diameters, via processing (i.e., processing for forming vias) by the photolithography method using a photosensitive resin composition is expected. Photosensitive resin compositions have the advantages of being relatively inexpensive and the process for producing a cured product thereof is relatively simple.
[0004] For example, Patent Document 1 discloses an invention aimed at providing a photosensitive resin composition that can suppress the occurrence of undercuts at the bottom of a via, thereby allowing the formation of a small-diameter via. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2019-105857 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the photosensitive resin compositions described in the above patent documents sometimes had insufficient physical properties for their cured products to be applied to build-up layers, and the photosensitive resin compositions described in the patent documents also had room for improvement in the resolution of the transfer pattern obtained by using the compositions.
[0007] Therefore, an object of the present invention is to provide a photosensitive resin composition that can realize a high-resolution transfer pattern and, in addition, can realize a cured product having excellent physical properties (particularly, high mechanical strength, low linear expansion coefficient, and low dielectric tangent). Another object of the present invention is to provide a transfer film, a method for forming a pattern, and a cured product using the photosensitive resin composition. [Means for solving the problem]
[0008] [1] (A) component: an alkali-soluble resin; (D) component; a compound having a number average molecular weight (Mn) of 10,000 g / mol or less and having a phenylene ether structure; A photosensitive resin composition, in which the mass ratio of the component (D) to the component (A) {component (D) / component (A)} is 0.05 to 1.30. [2] 2. The photosensitive resin composition according to item 1, further comprising: (B) a component having an ethylenically unsaturated bond. [3] 3. The photosensitive resin composition according to item 1 or 2, wherein the number average molecular weight of the component (D) is 300 to 5,000 g / mol. [4] 4. The photosensitive resin composition according to any one of items 1 to 3, wherein the mass ratio of the component (D) to the component (A) {component (D) / component (A)} is 0.10 to 0.50. [5] 5. The photosensitive resin composition according to any one of items 1 to 4, wherein the component (D) has a polymerizable functional group. [6] 6. The photosensitive resin composition according to any one of items 1 to 5, wherein the proportion of the component (D) in the photosensitive resin composition is 2.0 to 24 mass %. [7] Component (E): The photosensitive resin composition according to any one of items 1 to 6, further comprising a phenolic resin. [8] 8. The photosensitive resin composition according to any one of items 1 to 7, wherein the component (A) contains a carboxyl group-containing epoxy (meth)acrylate resin. [9] A transfer film which is a laminate having a support and a photosensitive resin layer containing the photosensitive resin composition according to any one of items 1 to 8.
[10] 10. The transfer film according to item 9, which is for forming a via having a diameter of less than 20 (μm).
[11] 9. A method for forming a pattern, comprising the steps of exposing the photosensitive resin composition according to any one of items 1 to 8 to light and developing it.
[12] Item 12. The method for forming a pattern according to item 11, wherein the pattern includes vias having a via diameter of less than 20 (μm).
[13] 9. A cured product obtained by heat curing the photosensitive resin composition according to any one of items 1 to 8.
[14] Item 14. The cured product according to item 13, which is used as a protective film for wiring in a printed wiring board.
[15] Item 15. A semiconductor device comprising the cured product according to item 13 or 14. Effect of the Invention
[0009] According to the present invention, it is possible to provide a photosensitive resin composition that can realize a high-resolution transfer pattern and, in addition, can realize a cured product that has excellent physical properties (particularly, can achieve high mechanical strength, a low linear expansion coefficient, and a low dielectric tangent). Another object of the present invention is to provide a transfer film, a pattern forming method, and a cured product using the photosensitive resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment for carrying out the present invention (hereinafter, referred to as "the present embodiment") will be described. The present invention is not limited to the present embodiment, and can be carried out by appropriately modifying it within the scope of the gist of the present invention.
[0011] In this specification, the upper or lower limit of a numerical range described stepwise may be replaced by the upper or lower limit of another numerical range described stepwise, or may be replaced by a value shown in the Examples. When a plurality of structures represented by the same symbol are present in the same formula, the structures may be independently selected unless otherwise specified. Various measurements are carried out based on the methods described in the Examples unless otherwise specified. The term "step" includes an independent step, as well as a step that cannot be clearly distinguished from other steps, as long as the function of the step is achieved.
[0012] In this specification, "(meth)acrylate" means "acrylate" and / or "methacrylate". "Solid content" means non-volatile content excluding volatile content (water and solvent) that may be contained in the photosensitive resin composition, and means, for example, components that remain without volatilization when the composition is dried. The form of the photosensitive resin composition is not particularly limited, and may be, for example, any of liquid, starch syrup, and wax at around room temperature (e.g., 25°C).
[0013] [Photosensitive resin composition] The photosensitive resin composition of the present embodiment comprises (A) component: an alkali-soluble resin; (D) component; a compound having a number average molecular weight (Mn) of 10,000 g / mol or less and having a phenylene ether structure; The mass ratio of the component (D) to the component (A) {component (D) / component (A)} is 0.05 to 1.30. This provides a photosensitive resin composition capable of realizing a high-resolution transfer pattern, and also provides a photosensitive resin composition capable of realizing a cured product having excellent physical properties (particularly, high mechanical strength, low linear expansion coefficient, and low dielectric loss tangent) by heat curing the composition.
[0014] In addition to the above components, the photosensitive resin composition may further contain: a component (B) which is a compound having an ethylenically unsaturated bond; a component (C) which is a photopolymerization initiator; a component (E) which is a phenolic resin; a component (F) which is an epoxy resin; a component (G) which is a silane coupling agent; and a component (H) which is an optional component (other component) other than the above components (A) to (G). For example, the photosensitive resin composition may further contain the components (B) to (C) and may further contain at least one component selected from the group consisting of the components (D) to (H). Each of the components (A) to (H) may be used alone or in combination of two or more. Each of the raw material components for obtaining the components (A) to (H) may be used alone or in combination of two or more.
[0015] In one embodiment, the photosensitive resin composition is capable of easily forming small-diameter vias in a printed wiring board or the like by a photolithography method, and is also capable of easily forming a large number of vias at once. In another embodiment, the photosensitive resin composition is capable of achieving both high resolution and excellent physical properties in a well-balanced manner.
[0016] <Component (A): Alkali-soluble resin> <Outline configuration> The component (A) is an alkali-soluble resin, i.e., a resin that is soluble in an aqueous alkaline solution. "Soluble in an aqueous alkaline solution" means, for example, that it is soluble in a developer, particularly in the developer used in the examples. The component (A) may have a functional group for exerting alkali solubility, and such a functional group may be, for example, a carboxyl group.
[0017] Component (A) exerts a predetermined function with respect to the resolution of the resulting transfer pattern and the physical properties of the resulting cured product. Component (A) imparts to the transfer pattern of the photosensitive resin composition the properties (e.g., high resolution) suitable for an insulating layer of a printed wiring board, and further imparts to the cured product of the photosensitive resin composition the properties (e.g., low linear thermal expansion coefficient) suitable for an insulating layer of a printed wiring board.
[0018] The (A) component preferably contains a carboxyl group-containing epoxy (meth)acrylate resin. This makes it easy to achieve a good balance between high resolution and excellent physical properties. From the same viewpoint, the proportion of the carboxyl group-containing epoxy (meth)acrylate resin is preferably 85% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more, when the solid content of the (A) component is 100% by mass. Such a proportion may be 100% by mass.
[0019] In the carboxyl group-containing epoxy (meth)acrylate resin, a part of the epoxy groups in the epoxy resin is modified to a (meth)acrylate group. From the viewpoint of increasing the crosslinking density and thus lowering the linear thermal expansion coefficient, the epoxy (meth)acrylate resin is preferably obtained from at least one selected from the group consisting of bisphenol A type epoxy (meth)acrylate, bisphenol F type epoxy (meth)acrylate, and biphenyl type epoxy (meth)acrylate, and more preferably obtained from a biphenyl type epoxy (meth)acrylate having two or more (meth)acrylate groups ((meth)acryloyl groups) in one molecule.
[0020] From the viewpoint of developability, the weight average molecular weight (Mw) of the component (A) is preferably 20,000 or less, more preferably 15,000 or less, and even more preferably 8,000 or less. On the other hand, from the viewpoint of resolution, the weight average molecular weight (Mw) is preferably 1,000 or more, more preferably 2,000 or more, and even more preferably 3,000 or more.
[0021] From the viewpoints of developability and resolution, the acid value of the component (A) is preferably from 50 to 500 mgKOH / g, and more preferably from 60 to 400 mgKOH / g or 60 to 200 mgKOH / g.
[0022] The proportion of the (A) component is preferably 10 to 70% by mass, more preferably 20 to 60% by mass, and even more preferably 30 to 50% by mass, relative to 100% by mass of the solid content of the photosensitive resin composition, which makes it easier to maintain a balance between developability and resolution, and also makes it easier to reduce the linear thermal expansion coefficient.
[0023] The weight average molecular weight is measured by gel permeation chromatography (GPC) and calculated using a calibration curve of polystyrene (Shodex STANDARD SM-105 manufactured by Shoko Science Co., Ltd.) The weight average molecular weight (Mw) can be measured, for example, using a GPC manufactured by JASCO Corporation under the following conditions. (conditions) Differential Refractometer: RI-1530 Pump: PU-1580 Degasser: DG-980-50 Column oven: CO-1560 Columns: KF-8025, KF-806M x 2, KF-807 Eluent: tetrahydrofuran (THF) Measurement temperature: 40℃ Flow rate: 1.0mL / min When the component (A) contains two or more alkali-soluble resins, the weighted average value taking into account the mass ratio of each alkali-soluble resin is treated as the weight average molecular weight (Mw) of the component (A).
[0024] <Carboxy group-containing epoxy (meth)acrylate resin> The component (A), particularly the carboxyl group-containing epoxy (meth)acrylate resin, can be, for example, a step of introducing an ethylenically unsaturated group into the epoxy resin by ring-opening addition of a carboxyl group of the unsaturated carboxylic acid to an epoxy group of the epoxy resin; a step of introducing a carboxyl group into the epoxy resin by adding an acid anhydride to at least a part of the hydroxyl groups generated by ring-opening of the epoxy groups of the epoxy resin; It can be synthesized through
[0025] In synthesizing an epoxy (meth)acrylate resin, examples of the epoxy resin that serves as the base raw material include bisphenol A type epoxy resin, hydrogenated bisphenol A type epoxy resin, bisphenol F type epoxy resin, hydrogenated bisphenol F type epoxy resin, and biphenyl type epoxy resin.
[0026] Examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, cinnamic acid, and crotonic acid.
[0027] Examples of acid anhydrides include maleic anhydride, succinic anhydride, itaconic anhydride, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenonetetracarboxylic dianhydride.
[0028] As the carboxy group-containing epoxy (meth)acrylate resin, a commercially available product may be used. Examples of the commercially available product include CCR-1291H, CCR-1235H, ZCR-1569H, ZCR-1601H, ZCR-1761H, ZCR-1797H, ZCR-1798H, ZCR-1809H, ZCR-1835H, ZCR-1834H, ZFR-1401H, ZFR-1491H, and ZAR-1035, ZAR-2000, UXE-3000, UXE-3024 (all manufactured by Nippon Kayaku Co., Ltd.), KRM8762 (manufactured by Daicel Allnex Co., Ltd.), etc. Further, examples of the carboxyl group-containing epoxy (meth)acrylate resin include those commercially available from Wako Pure Chemical Industries, Ltd., Tokyo Chemical Industry Co., Ltd., and the like.
[0029] <Other resins> The component (A) may contain other resins (other resins) in addition to the carboxy group-containing epoxy (meth)acrylate resin, or in addition to the carboxy group-containing epoxy (meth)acrylate resin. The other resin may be, for example, a resin obtained by using a first monomer described later, or may be a resin obtained by using both the first monomer and a second monomer described later.
[0030] The first monomer may have a carboxyl group in its molecule. Examples of the first monomer include (meth)acrylic acid, fumaric acid, cinnamic acid, crotonic acid, itaconic acid, 4-vinylbenzoic acid, maleic anhydride, and maleic acid half ester.
[0031] The second monomer has at least one polymerizable unsaturated group in its molecule. The second monomer may be, for example, Methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, benzyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, isobornyl (meth)acrylate, nonylphenoxypolyethylene glycol (meth)acrylate, pentamethy (Meth)acrylates such as rupiperidyl (meth)acrylate, tetramethylpiperidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, phenoxyethyl (meth)acrylate, ethyl carbitol (meth)acrylate, methoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, (2-methyl-2-ethyl-1,3-dioxolan-4-yl)methyl (meth)acrylate, cyclic trimethylolpropane formal (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, etc.; Styrene derivatives such as styrene, methylstyrene, vinyltoluene, tert-butoxystyrene, acetoxystyrene, styrene dimer, and styrene trimer; Esters of vinyl alcohol, such as vinyl acetate; and (Meth)acrylonitrile; Examples include: The second monomer may include a compound having an aromatic ring, such as benzyl (meth)acrylate or styrene derivatives, particularly benzyl (meth)acrylate or styrene.
[0032] The first monomer and the second monomer may each be used alone or in combination of two or more.
[0033] The other resins can be synthesized, for example, using the above-mentioned monomers by the following method. That is, the other resins can be synthesized by adding an appropriate amount of a radical polymerization initiator such as benzoyl peroxide or azoisobutyronitrile to a solution obtained by diluting one or more monomers with a solvent such as acetone, methyl ethyl ketone, isopropanol, etc., and then heating and stirring the solution. In some cases, synthesis is performed while dropping a part of the mixture into the reaction solution, and in other cases, after the reaction is completed, further solvent is added to adjust the concentration to the desired level.
[0034] <Component (B): Compound having an ethylenically unsaturated bond> The component (B) is a compound having one or more ethylenically unsaturated bonds, and among these, it preferably contains a compound having two ethylenically unsaturated bonds. However, the component (B) is different from the component (A) and does not have a phenylene ether structure as the component (D).
[0035] From the viewpoints of resolution and linear expansion coefficient, the component (B) preferably has a bisphenol A skeleton or a bisphenol F skeleton, and further preferably has an alkyleneoxy group.
[0036] The component (B) is The following general formula (I): [ka] (wherein R1 and R2 are each independently a hydrogen atom or a methyl group, A and B are an alkylene group having 2 to 6 carbon atoms, and when A and B are different from each other, the structure consisting of the repeating units of -(A-O)- and -(B-O)- may be formed randomly or in blocks, m1, m2, m3, and m4 are integers of 0 or more, m1+m2 and m3+m4 are integers of 0 to 8, and m1+m2+m3+m4 is an integer of 2 to 8), The following general formula (II): [ka] (wherein R3 and R4 are each independently a hydrogen atom or a methyl group; C and D are an alkylene group having 2 to 6 carbon atoms; and when C and D are different from each other, the structure consisting of repeating units of -(CO)- and -(DO)- may be formed randomly or in blocks; m5, m6, m7, and m8 are integers of 0 or more; m5+m6 and m7+m8 are integers of 0 to 28; and m5+m6+m7+m8 is an integer of 10 to 28), and The following general formula (III): [ka] (wherein R5 and R6 are each independently a hydrogen atom or a methyl group, E and F are an alkylene group having 2 to 6 carbon atoms, and when E and F are different from each other, the structure consisting of repeating units of -(EO)- and -(FO)- may be constituted randomly or in blocks, m9, m10, m11, and m12 are integers of 0 or more, m9+m10 and m11+m12 are integers of 0 to 50, and m9+m10+m11+m12 is an integer of 30 to 50), It is preferable that the composition contains at least one selected from the group consisting of:
[0037] Examples of the compound represented by the above formula (I) include 2,2-bis{(4-acryloxypolyethyleneoxy)phenyl}propane and 2,2-bis{(4-methacryloxypolyethyleneoxy)phenyl}propane. The polyethyleneoxy group contained in the compound is preferably at least one group selected from the group consisting of monoethyleneoxy, diethyleneoxy, triethyleneoxy, tetraethyleneoxy, pentaethyleneoxy, hexaethyleneoxy, heptaethyleneoxy, and octaethyleneoxy.
[0038] In addition, the compound represented by the above formula (I) may also include 2,2-bis{(4-acryloxypolyalkyleneoxy)phenyl}propane or 2,2-bis{(4-methacryloxypolyalkyleneoxy)phenyl}propane. The polyalkyleneoxy group contained in the compound may include a propyleneoxy group or an ethyleneoxy group, and a propyleneoxy group. Among the compounds, 2,2-bis{(4-methacryloxydiethyleneoxy)phenyl}propane is preferred.
[0039] Examples of the compound represented by the above formula (I) include Dimethacrylate of polyethylene glycol with an average of 2 moles of ethylene oxide attached to each end of bisphenol A; Dimethacrylate of polyalkylene glycol in which an average of 1 mole of ethylene oxide is added to each end of bisphenol A; Other examples include:
[0040] Examples of the compound represented by the above formula (II) include Dimethacrylate of polyethylene glycol in which an average of 5 moles of ethylene oxide are added to each end of bisphenol A (NK Ester BPE-500, manufactured by Shin-Nakamura Chemical Co., Ltd.); Dimethacrylate of polyalkylene glycol in which an average of 6 mol of ethylene oxide and an average of 2 mol of propylene oxide are added to both ends of bisphenol A; Examples include:
[0041] Examples of the compound represented by the above formula (III) include Dimethacrylate of polyethylene glycol with an average of 15 moles of ethylene oxide attached to each end of bisphenol A; Dimethacrylate of polyalkylene glycol in which an average of 15 mol of ethylene oxide and an average of 2 mol of propylene oxide are added to both ends of bisphenol A; Examples include:
[0042] The ratio of the compound represented by the formula (I), the compound represented by the formula (II), and the compound represented by the formula (III) is preferably 5 to 60% by mass, and more preferably 20 to 50% by mass, when the solid content of the photosensitive resin composition is 100% by mass. This amount is preferably the lower limit value or more from the viewpoints of resolution and linear expansion coefficient, and is preferably the upper limit value or less from the viewpoints of mechanical strength and electrical properties.
[0043] The proportion of the compound represented by the above formula (I), the compound represented by the above formula (II), and the compound represented by the above formula (III) is preferably 50 to 100 mass %, more preferably 70 mass % or more, and even more preferably 80 mass % or more, based on the total mass of the (B) component.
[0044] The proportion of the compound represented by the formula (I) is preferably 0.5 to 50% by mass, more preferably 1.0 to 45% by mass, and even more preferably 2.0 to 40% by mass, when the solid content of the photosensitive resin composition is taken as 100% by mass. This amount is preferably equal to or more than the lower limit from the viewpoint of resolution, and is preferably equal to or less than the upper limit from the viewpoints of mechanical strength and electrical properties.
[0045] The proportion of the compound represented by the general formula (II) is preferably 0.5 to 50% by mass, more preferably 1 to 45% by mass, and even more preferably 2 to 40% by mass. From the viewpoints of resolution and linear expansion coefficient, this amount is preferably the lower limit or more, and from the viewpoints of mechanical strength and electrical properties, it is preferably the upper limit or less.
[0046] The proportion of the compound represented by the general formula (III) is preferably 1 to 50% by mass, more preferably 5 to 45% by mass, and even more preferably 10 to 40% by mass. From the viewpoints of resolution and linear expansion coefficient, this amount is preferably the lower limit or more, and from the viewpoints of mechanical strength and electrical properties, it is preferably the upper limit or less.
[0047] The component (B) may contain other compounds in addition to the compounds represented by the above formulas (I) to (III) or in addition to the compounds represented by the above formulas (I) to (III). Other usable compounds having an ethylenically unsaturated bond include, for example, 1,6-hexanediol di(meth)acrylate, 1,4-cyclohexanediol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, 2-di(p-hydroxyphenyl)propane di(meth)acrylate, glycerol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, polyoxypropyl trimethylolpropane tri(meth)acrylate, polyoxyethyl trimethylolpropane triacrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and trimethylolpropane triglycidyl ether tri(meth)acrylate. acrylate, bisphenol A diglycidyl ether di(meth)acrylate, β-hydroxypropyl-β'-(acryloyloxy)propyl phthalate, phenoxy polyethylene glycol (meth)acrylate, nonylphenoxy polyethylene glycol (meth)acrylate, nonylphenoxy polyalkylene glycol (meth)acrylate, polypropylene glycol mono(meth)acrylate, triethylene glycol dodecapropylene glycol, dimethacrylates of polyalkylene glycols in which ethylene oxide has been further added to both ends of a polypropylene glycol to which propylene oxide has been added (polypropylene glycol to which an average of 12 mol of propylene oxide has been added to both ends, and to which an average of 3 mol of ethylene oxide has been further added to each end).
[0048] Other usable compounds having an ethylenically unsaturated bond include urethane compounds. Examples of the urethane compounds include Examples of the urethane compound include hexamethylene diisocyanate, tolylene diisocyanate, or a diisocyanate compound (e.g., 2,2,4-trimethylhexamethylene diisocyanate) and a compound having a hydroxyl group and a (meth)acrylic group in one molecule (e.g., 2-hydroxypropyl acrylate, oligopropylene glycol monomethacrylate).Specific examples include a reaction product of hexamethylene diisocyanate and oligopropylene glycol monomethacrylate (manufactured by NOF Corporation, Blenmer PP1000).
[0049] The proportion of the (B) component may be 5 to 70% by mass, and preferably 10 to 60% by mass, based on 100% by mass of the solid content of the photosensitive resin composition. From the viewpoints of sensitivity and resolution, it is preferably equal to or more than the lower limit, and from the viewpoints of mechanical strength and suppression of peeling during curing, it is preferably equal to or less than the upper limit.
[0050] <Component (C): Photopolymerization initiator> The component (C) is a photopolymerization initiator. Any known photopolymerization initiator may be used. The proportion of the component (C) may be 0.01 to 30% by mass, preferably 0.05 to 10% by mass, when the solid content of the photosensitive resin composition is 100% by mass. From the viewpoint of sensitivity, the proportion of the component (C) is preferably equal to or more than the lower limit, and from the viewpoint of allowing sufficient light transmission to the bottom surface of the film coated on the substrate and thus obtaining high resolution, the proportion of the component (C) is preferably equal to or less than the upper limit.
[0051] Examples of the component (C) include: quinones such as 2-ethylanthraquinone, octaethylanthraquinone, 1,2-benzanthraquinone, 2,3-benzanthraquinone, 2-phenylanthraquinone, 2,3-diphenylanthraquinone, 1-chloroanthraquinone, 2-chloroanthraquinone, 2-methylanthraquinone, 1,4-naphthoquinone, 9,10-phenanthraquinone, 2-methyl-1,4-naphthoquinone, 9,10-phenanthraquinone, 2-methyl-1,4-naphthoquinone, 2,3-dimethylanthraquinone, and 3-chloro-2-methylanthraquinone; Aromatic ketones such as benzophenone, Michler's ketone [4,4'-bis(dimethylamino)benzophenone], and 4,4'-bis(diethylamino)benzophenone; benzoins or benzoin ethers such as benzoin, benzoin ethyl ether, benzoin phenyl ether, methylbenzoin, and ethylbenzoin; Dialkyl ketals such as benzyl dimethyl ketal and benzyl diethyl ketal; Thioxanthones such as diethylthioxanthone and chlorothioxanthone; Dialkylaminobenzoic acid esters such as ethyl dimethylaminobenzoate; Oxime esters such as 1-phenyl-1,2-propanedione-2-O-benzoyloxime and 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)oxime; Lophine dimers such as 2-(o-chlorophenyl)-4,5-diphenylimidazolyl dimer, 2-(o-chlorophenyl)-4,5-bis-(m-methoxyphenyl)imidazolyl dimer, and 2-(p-methoxyphenyl)-4,5-diphenylimidazolyl dimer; Among these, 4,4'-bis(diethylamino)benzophenone or 2-(o-chlorophenyl)-4,5-diphenylimidazolyl dimer is preferred.
[0052] <Component (D): Compound having a phenylene ether structure> The component (D) is a compound having a number average molecular weight (Mn) of 10,000 g / mol or less and having a phenylene ether structure. The number average molecular weight (Mn) of the component (D) is 10,000 g / mol or less. If Mn exceeds the upper limit, the desired resolution and tensile strength cannot be obtained. The component (D) may be called an oligomer. The number average molecular weight (Mn) of the component (D) is preferably 300 to 10,000 g / mol, more preferably 300 to 5,000 g / mol, and even more preferably 500 to 3,000 g / mol. With such a component (D), it is easy to achieve excellent electrical properties and high tensile strength. The number average molecular weight (Mn) can be measured by the same method as the method for measuring the weight average molecular weight (Mw) described above.
[0053] From the viewpoint of a low linear expansion coefficient and excellent electrical properties (e.g., low dielectric tangent), it is preferable that the (D) component has a polymerizable functional group. The polymerizable functional group may be any functional group that is polymerized by light and / or heat, and examples thereof include ethylenically unsaturated bonds and epoxy groups, among which ethylenically unsaturated bonds are preferable. The polymerizable functional group is preferably present at the main chain terminal of the (D) component.
[0054] Examples of the component (D) include compounds represented by the following general formula (D1): [ka] [In the formula, R1 to R6 each independently represent a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, preferably a hydrogen atom; A represents a compound represented by the following general formula (D2) and the following general formula (D3): [ka] In the formula, B is represented by the following general formulae (B1), (B2), and (B3): [ka] (In the formula, R 15 ~R 34 are each independently a hydrogen atom, a phenyl group, or an alkyl group having 6 or less carbon atoms, preferably a hydrogen atom or a methyl group, and E is a linear, branched, or cyclic divalent hydrocarbon group having 20 or less carbon atoms. At least one selected from the group consisting of: [ka] In the formula, D represents the following general formula (D4): [ka] (In the formula, R7~R 14 are each independently hydrogen, a phenyl group, or an alkyl group having 6 or less carbon atoms, preferably hydrogen or a methyl group, and more preferably R, R, and R 13 , and / or R 14 is a methyl group, a and b are integers from 0 to 100, and at least one of them is not 0, B is the same as in the above formulae (B1), (B2), and / or (B3), and B in formula (D4) may be the same as or different from B in formula (D2). At least one selected from the group consisting of: Examples of the compound include compounds represented by the following formula:
[0055] From the viewpoints of heat resistance, dielectric properties, and processability, the component (D) is a compound represented by the following general formula (D5) and the following formula (D6): [ka] (In the formula, R1 to R6, B, a, and b are the same as above.) [ka] and more preferably the compound represented by the above formula (5).
[0056] Examples of the component (D) include OPE-2St1200 and OPE-2St2200 (both manufactured by Mitsubishi Gas Chemical Company, Inc.; corresponding to the above formula (D5)), and bixylenol diallyl ether resin ("YL7776" manufactured by Mitsubishi Chemical Corporation; corresponding to the above formula (6)).
[0057] The proportion of the (D) component is 2.0 to 24% by mass, relative to 100% by mass of the solid content of the photosensitive resin composition. When this proportion is 2.0% by mass or more, high sensitivity is easily obtained, and when it is 24% by mass or less, high resolution is easily obtained. The proportion of the (D) component having a phenylene ether structure in its main chain is preferably 2.0 to 20 mass%, more preferably 2.0 to 17 mass%, even more preferably 2.0 to 14 mass%, and particularly preferably 3.0 to 7.0 mass%, based on 100 mass% of the solid content of the photosensitive resin composition.
[0058] <Mass ratio {(D) component / (A) component}> In this embodiment, when the mass ratio {(D) component / (A) component} is 0.05 or more, a high-resolution transfer pattern can be realized, and when the mass ratio is 1.30 or less, a cured product with excellent physical properties (particularly, a cured product capable of achieving high mechanical strength, low linear expansion coefficient, and low dielectric tangent) can be realized. From the same viewpoint, the mass ratio {(D) component / (A) component} is preferably 0.05 or more and 1.00 or less, more preferably 0.1 or more and 0.9 or less, even more preferably 0.3 or more and 0.7 or less, and particularly preferably 0.3 or more and 0.5 or less.
[0059] When the photosensitive composition contains a plurality of (D) components, the total amount thereof is used in calculating the above mass ratio. Similarly, when the photosensitive composition contains a plurality of (A) components, the total amount thereof is used in calculating the above mass ratio.
[0060] <Component (E): Phenolic resin> The photosensitive resin composition may contain component (E) a phenolic resin. Component (E) functions as a curing agent for component (F) an epoxy resin, which will be described later. By containing component (E), the photosensitive resin composition can easily impart various properties (e.g., excellent mechanical strength, low linear thermal expansion coefficient, etc.) suitable for an insulating layer of a multilayer printed wiring board to the obtained cured product.
[0061] Examples of the component (E) include compounds having a phenolic hydroxyl group. From the viewpoint of increasing the crosslink density and thereby reducing the linear thermal expansion coefficient, phenol-biphenyldiyl resin, phenol novolac resin, and biphenyl novolac resin are preferred.
[0062] The proportion of the (E) component is preferably 2 to 30 mass%, more preferably 5 to 20 mass%, and even more preferably 8 to 12 mass%, relative to 100 mass% of the solid content of the photosensitive resin composition, which makes it easier to maintain a balance between developability and resolution, and also makes it easier to reduce the linear thermal expansion coefficient.
[0063] <Component (F): Epoxy resin> The photosensitive resin composition may contain an epoxy resin as component (F). By containing the component (F), the photosensitive resin composition can easily impart properties such as excellent mechanical strength and excellent thermal properties to the resulting cured product. In this specification, the "component (F)" does not include a carboxyl group-containing epoxy (meth)acrylate resin, which is one embodiment of the component (A).
[0064] The component (F) preferably has two or more epoxy groups in one molecule. From the viewpoint of suitably obtaining the effects of this embodiment, the ratio of the epoxy resin having two or more epoxy groups in one molecule is preferably 3% by mass or more, more preferably 5% by mass or more, and particularly preferably 8% by mass or more, when the solid content of the photosensitive resin composition is 100% by mass. The component (F) may contain up to two epoxy groups in one molecule. The above ratio may be 15% by mass or less, assuming that the solid content of the photosensitive resin composition is 100% by mass.
[0065] The component (F) is preferably a compound having an epoxy group, such as bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type epoxy resin, cresol novolac type epoxy resin, biphenyl type epoxy resin, linear aliphatic epoxy resin, epoxy resin having a butadiene structure, alicyclic epoxy resin, heterocyclic epoxy resin, spiro ring-containing epoxy resin, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, naphthylene ether type epoxy resin, trimethylol type epoxy resin, tetraphenylethane type epoxy resin, and the like.
[0066] Examples of the component (F) include: DIC "HP4032", "HP4032D", "HP4032SS" (naphthalene type epoxy resin); Mitsubishi Chemical Corporation's "828US", "jER828EL", "825", and "Epicoat 828EL" (bisphenol A type epoxy resin); Mitsubishi Chemical Corporation's "jER807" and "1750" (bisphenol F type epoxy resin); Mitsubishi Chemical Corporation's "jER152" (phenol novolac type epoxy resin); Mitsubishi Chemical's "630" and "630LSD" (glycidylamine type epoxy resins); Nippon Steel & Sumikin Chemical's "ZX1059" (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin); Nagase ChemteX Corporation's "EX-721" (glycidyl ester type epoxy resin); Daicel's "Celloxide 2021P" (alicyclic epoxy resin with an ester structure); Daicel's "PB-3600" (epoxy resin with butadiene structure); Nippon Steel & Sumikin Chemical's "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin); and Nippon Kayaku "NC-3000", "NC-3000-L", "NC-3000-H", "NC-3000-H", "NC-3100"; etc.
[0067] From the viewpoints of tensile strength and thermal properties, the proportion of the (F) component is preferably 2% by mass or more, more preferably 5% by mass or more, and even more preferably 8% by mass or more, based on 100% by mass of the solid content of the photosensitive resin composition. From the viewpoint of suitably obtaining the effects of this embodiment, this proportion is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 12% by mass or less.
[0068] <Component (G): Silane coupling agent> The photosensitive resin composition may contain component (G) which is a silane coupling agent. Examples of component (G) include 3-mercaptopropyltrimethoxysilane (e.g., Shin-Etsu Chemical Co., Ltd.: trade name KBM803, Chisso Corporation: trade name Sila-Ace S810), 3-mercaptopropyltriethoxysilane (Azmax Corporation: trade name SIM6475.0), 3-mercaptopropylmethyldimethoxysilane (e.g., Shin-Etsu Chemical Co., Ltd.: trade name LS1375, AZmax Corporation: trade name SIM6474.0), mercaptomethyltrimethoxysilane (AZmax Corporation: trade name SIM6473.5C), mercaptomethyltrimethoxysilane (AZmax Corporation: trade name SIM6473.0), 3-mercaptopropyldiethoxymethoxysilane, 3-mercaptopropylethoxydimethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropyldiethoxypropoxysilane, 3-mercaptopropylethoxydipropoxysilane, 3-mercaptopropyldimethoxypropoxysilane, 3-mercaptopropylmethoxydipropoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyldiethoxymethoxysilane, 2-mercaptoethyl Mercaptoethylethoxydimethoxysilane, 2-mercaptoethyltripropoxysilane, 2-mercaptoethyltripropoxysilane, 2-mercaptoethylethoxydipropoxysilane, 2-mercaptoethyldimethoxypropoxysilane, 2-mercaptoethylmethoxydipropoxysilane, 4-mercaptobutyltrimethoxysilane, 4-mercaptobutyltriethoxysilane, 4-mercaptobutyltripropoxysilane, N-(3-triethoxysilylpropyl)urea (manufactured by Shin-Etsu Chemical Co., Ltd.: trade name LS3610, manufactured by Azmax Corporation: trade name SIU9055.0), N-(3-trimethoxysilylpropyl)urea (manufactured by Azmax Corporation: trade name SIU9058.0), N-(3-diethoxymethoxysilylpropyl)urea, N-(3-ethoxydimethoxysilylpropyl)urea, N-(3-tripropoxysilylpropyl)urea, N-(3-diethoxypropoxysilylpropyl)urea, N-(3-ethoxydipropoxysilylpropyl)urea, N-(3-dimethoxypropoxysilylpropyl)urea, N-(3-methoxydipropoxysilylpropyl)urea, N-(3-trimethoxysilylethyl)urea, N-(3-ethoxydimethoxysilylethyl)urea A, N-(3-tripropoxysilylethyl)urea, N-(3-tripropoxysilylethyl)urea, N-(3-ethoxydipropoxysilylethyl)urea, N-(3-dimethoxypropoxysilylethyl)urea, N-(3-methoxydipropoxysilylethyl)urea, N-(3-trimethoxysilylbutyl)urea, N-(3-triethoxysilylbutyl)urea, N-(3-tripropoxysilylbutyl)urea, 3-(m-aminophenoxy)propyltrimethoxysilane (manufactured by AZMAX Corporation: trade name), Examples of such silanes include SLA0598.0), m-aminophenyltrimethoxysilane (manufactured by AZMAX Corporation: trade name SLA0599.0), p-aminophenyltrimethoxysilane (manufactured by AZMAX Corporation: trade name SLA0599.1), aminophenyltrimethoxysilane (manufactured by AZMAX Corporation: trade name SLA0599.2), and 2-(trimethoxysilylethyl)pyridine (manufactured by AZMAX Corporation: trade name SIT8396.0).
[0069] Examples of the silane coupling agent include 2-(triethoxysilylethyl)pyridine, 2-(dimethoxysilylmethylethyl)pyridine, 2-(diethoxysilylmethylethyl)pyridine, (3-triethoxysilylpropyl)-t-butylcarbamate, (3-glycidoxypropyl)triethoxysilane, tetramethoxysilane, tetraethoxysilane, tetra-n-propoxysilane, tetra-i-propoxysilane, tetra-n-butoxysilane, tetra-i-butoxysilane, tetra-t-butoxysilane, tetrakis(methoxyethoxysilane), tetrakis(methoxy-n-propoxysilane), tetra Kis(ethoxyethoxysilane), tetrakis(methoxyethoxyethoxysilane), bis(trimethoxysilyl)ethane, bis(trimethoxysilyl)hexane, bis(triethoxysilyl)methane, bis(triethoxysilyl)ethane, bis(triethoxysilyl)ethylene, bis(triethoxysilyl)octane, bis(triethoxysilyl)octadiene, bis[3-(triethoxysilyl)propyl]disulfide, bis[3-(triethoxysilyl)propyl]tetrasulfide, di-t-butoxydiacetoxysilane, di-i-butoxyaluminoxytriethoxysilane, bis(pentadionate)titanium-O,O'-Bis(oxyethyl)-aminopropyltriethoxysilane, trimethoxyphenylsilane, trimethoxy(p-tolyl)silane, N-phenyl-3-aminopropyltrimethoxysilane, phenylsilanetriol, methylphenylsilanediol, ethylphenylsilanediol, n-propylphenylsilanediol, isopropylphenylsilanediol, n-butyldiphenylsilanediol, isobutylphenylsilanediol, tert-butylphenylsilanediol, diphenylsilanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolylsilane, ethylmethylphenylsilanol, n-propylmethylphenylsilanol, isopropylmethylphenylsilanol, n-butylmethylphenylsilanol, isobutylmethylphenylsilanol, tert-butylmethylphenylsilanol, ethyl n-propylphenylsilanol, ethylisopropylphenylsilanol, n-butylethylphenylsilanol, isobutylethylphenylsilanol, tert-butylethylphenylsilanol, methyldiphenylsilanol, ethyldiphenylsilanol, n-propyldiphenylsilanol, isopropyldiphenylsilanol, n-butyldiphenylsilanol, isobutyldiphenylsilanol, tert-butyldiphenylsilanol, triphenylsilanol, and tris(3-trimethoxysilylpropyl)isocyanurate.
[0070] Among the above, from the viewpoint of storage stability of the photosensitive resin composition, phenylsilanetriol, trimethoxyphenylsilane, trimethoxy(p-tolyl)silane, diphenylsilanediol, dimethoxydiphenylsilane, diethoxydiphenylsilane, dimethoxydi-p-tolylsilane, triphenylsilanol, N-phenyl-3-aminopropyltrimethoxysilane, and tris(3-trimethoxysilylpropyl)isocyanurate are preferred. As the (G) component, a phenylaminosilane coupling agent or a silane coupling agent having an isocyanurate group is also preferred.
[0071] The proportion of the component (G) is preferably 0.0120% by mass or more and preferably 20% by mass or less, based on 100% by mass of the photosensitive resin composition.
[0072] <Component H: Optional components other than (A) to (G) above (other components)> The photosensitive resin composition may contain component (H) and other components, such as various solvents, inorganic fillers, rust inhibitors, adhesion aids, polymerization inhibitors, antioxidants, defoamers, dyes, etc.
[0073] A preparation liquid of the photosensitive resin composition can be obtained by adding a solvent, which is the component (H), to the photosensitive resin composition. An example of the inorganic filler is silica. The filler, which is the component (H) in the photosensitive resin composition, may be less than 40% by mass, less than 35% by mass, or below the detection limit (e.g., 0% by mass) when the solid content of the photosensitive resin composition is 100% by mass.
[0074] [Photosensitive resin composition preparation] One aspect of this embodiment is a prepared liquid obtained by adding a solvent to a photosensitive resin composition. Examples of the solvent include Ketones such as methyl ethyl ketone (MEK) and propylene glycol monomethyl ether acetal (PGMEA); Alcohols such as methanol, ethanol, and isopropyl alcohol; From the viewpoint of coatability of the photosensitive resin composition, it is preferable to mix the solvent and the photosensitive resin composition so that the viscosity of the prepared solution is 500 to 4000 mPa·sec at 25°C.
[0075] [Transfer film] A further aspect of the present embodiment is a transfer film that is a laminate having a support and a photosensitive resin layer containing the above-mentioned photosensitive resin composition. The transfer film may be for forming a via having a via diameter of less than 20 (μm).
[0076] <Support (support film)> The support is preferably transparent and transmits the light emitted from the exposure light source. Examples of such supports include polyethylene terephthalate film, polyvinyl alcohol film, polyvinyl chloride film, vinyl chloride copolymer film, polyvinylidene chloride film, vinylidene chloride copolymer film, polymethyl methacrylate copolymer film, polystyrene film, polyacrylonitrile film, styrene copolymer film, polyamide film, and cellulose derivative film. As these films, those that are stretched as necessary can also be used.
[0077] The haze of the support is preferably 5 or less. The thickness of the support is preferably as thin as possible from the viewpoints of relief pattern formation and economic efficiency, but is preferably from 10 to 30 μm from the viewpoint of maintaining strength.
[0078] ≪Photosensitive resin layer≫ The photosensitive resin layer contains the above-mentioned photosensitive resin composition. The photosensitive resin layer can be formed by, for example, applying the photosensitive resin composition to the support and drying it.
[0079] The thickness of the photosensitive resin layer is preferably 1 to 100 μm, more preferably 7 to 60 μm, and further preferably 10 to 50 μm. If it is 100 μm or less, practically sufficient resolution is easily obtained, and if it is 1 μm or more, practically good strength is easily obtained. The thinner the photosensitive resin layer, the easier it is to improve the resolution, and the thicker the photosensitive resin layer, the easier it is to improve the film strength, so the thickness can be appropriately selected depending on the use of the transfer film and, by extension, the use of the final product obtained using the same.
[0080] <Protective layer (protective film)> The transfer film may have a photosensitive resin layer, a support supporting the photosensitive resin layer, and a protective film on the opposite side of the photosensitive resin layer to the support, if necessary. It is preferable that the protective film has a sufficiently smaller adhesive force to the photosensitive resin layer than the support, and in this case, the protective film can be easily peeled off from the transfer film.
[0081] Examples of protective films include polyethylene films and polypropylene films, and also include films with excellent peelability such as those disclosed in JP-A-59-202457.
[0082] From the viewpoint of peelability, the thickness of the protective film is preferably from 10 to 100 μm, more preferably from 10 to 80 μm, and even more preferably from 10 to 50 μm.
[0083] [Transfer film manufacturing method] A further aspect of this embodiment is a manufacturing method for manufacturing the transfer film. The transfer film can be obtained by laminating a support, a photosensitive resin layer, and, if necessary, a protective film.
[0084] The method for producing the transfer film is, for example, A step of applying the prepared liquid of the photosensitive resin composition onto a support using a bar coater or a roll coater and drying the applied liquid; Following this step, laminating a protective film on the photosensitive resin layer; may optionally include As various conditions in the method for producing the transfer film, known conditions in known production methods may be adopted.
[0085] [Method of forming transfer pattern (method of manufacturing transfer pattern)] A further aspect of the present embodiment is a method for forming a transfer pattern, comprising the steps of exposing the photosensitive resin composition to light and developing it. Here, the "transcription pattern" is a resin pattern obtained by exposure using a transfer film and subsequent development; After development, a cured product (cured product pattern) is obtained by heat curing the resin pattern; Includes.
[0086] [Pattern formation method] A further aspect of this embodiment is a method for forming a pattern. The pattern may include a via having a via diameter of less than 20 (μm). The resin pattern and the cured product pattern will be described below.
[0087] <Resin pattern and manufacturing method thereof> A further aspect of this embodiment is a resin pattern and a method for producing the same. In one embodiment, the method for producing a resin pattern comprises the steps of exposing the above-mentioned photosensitive resin composition to light and developing it.
[0088] In one embodiment, the method comprises the steps of: A step of laminating the photosensitive resin layer of the transfer film onto a predetermined substrate (lamination step); a step of exposing the laminated photosensitive resin layer to light (exposure step); and a step of removing the unexposed portion of the photosensitive resin layer after exposure with a developer (development step); has.
[0089] <Lamination process> In this step, for example, a photosensitive resin layer is provided on a substrate using a predetermined laminator. Specifically, when the transfer film has a protective film, the protective film is peeled off, and then the photosensitive resin layer is heated and pressed onto the substrate using a laminator.
[0090] Examples of the substrate include copper, SUS, glass, ITO, and silicon wafer. The photosensitive resin layer may be laminated on only one side of the substrate, or may be laminated on both sides as necessary. The heating temperature is generally 40 to 160°C. In addition, by performing the thermocompression bonding two or more times, the adhesion of the transfer pattern to the substrate is easily improved. In this case, a two-stage laminator equipped with two rolls can be used for the compression bonding, and the laminate of the substrate and the photosensitive resin layer may be passed through the rolls repeatedly multiple times.
[0091] <Exposure process> In this step, for example, the photosensitive resin layer is exposed using an exposure machine. The exposure may be performed without peeling the support from the transfer film, or may be performed after peeling the support from the transfer film as necessary. When the exposure is performed through a photomask, the exposure amount is determined by the light source illuminance and the exposure time. The exposure amount may be measured using an actinometer.
[0092] In the exposure step, maskless exposure may be performed. In maskless exposure, the substrate is directly exposed by a drawing device without using a photomask. In this case, a semiconductor laser or an ultra-high pressure mercury lamp having a wavelength of 350 to 410 nm is preferably used as the light source. The drawing pattern is preferably controlled by a computer, and the exposure amount in this case is determined by the illuminance of the exposure light source and the moving speed of the substrate.
[0093] <Developing process> In this step, for example, the unexposed portion of the photosensitive resin layer after exposure is removed with a developer. In addition, when a support is provided on the photosensitive resin layer after exposure, it is preferable to remove the support before carrying out the development step.
[0094] In the development step, the unexposed portion is removed using an alkaline aqueous developer, thereby obtaining a resist image (resin pattern). The developer is preferably an aqueous solution of Na2CO3, K2CO3, NaOH, or the like. The developer is selected according to the characteristics of the photosensitive resin layer, and examples of the developer include a 0.2-2 mass % Na2CO3 aqueous solution and a 1-5 mass % NaOH aqueous solution. The developer may be one used in the examples.
[0095] The developer may contain a surfactant, an antifoaming agent, a small amount of an organic solvent for promoting development, etc. The temperature of the developer in the development step is, for example, 20 to 60° C., and is preferably kept at a constant temperature.
[0096] <Cured product (cured product pattern)> A further aspect of this embodiment is a cured product (cured product pattern) and a method for producing the same. The cured product is obtained by heating and curing the above-mentioned photosensitive resin composition.
[0097] In one embodiment, a method for producing a cured product pattern includes the steps of: A step of heat-curing the resin pattern obtained by the above-mentioned step (curing step); has.
[0098] As a heating method, for example, a heating furnace using a method such as hot air, infrared, vacuum, or far infrared can be used. The heating temperature is preferably 100 to 300°C, more preferably 120 to 250°C, and even more preferably 120 to 230°C. If it is 100°C or higher, the film strength after heat curing is likely to be high, and if it is 300°C or lower, decomposition of the resin component contained in the photosensitive resin composition is likely to be suppressed. The heating time is preferably 10 to 120 minutes, more preferably 15 to 90 minutes. The atmosphere during heating can be an N2 atmosphere, or an N2 and O2 atmosphere.
[0099] In addition, the method for producing a transfer pattern includes the steps of: A step of further exposing the pattern (post-exposure step), and / or A process of further heating the pattern (heating process) may have By including such a post-exposure step and / or heating step, the insulating reliability and heat resistance of the obtained cured product (insulating film) are likely to be further improved.
[0100] The exposure dose in the post-exposure process is 200 mJ / cm 2 ~1000mJ / cm 2 In the heating step, the heating temperature is preferably 40 to 250°C, and from the viewpoint of the manufacturing process, the heating time is preferably 90 minutes or less. As a heating method, for example, a heating furnace using hot air, infrared rays, vacuum, or far infrared rays can be used. As an atmosphere during heating, an N2 atmosphere, or an N2 and O2 atmosphere can be used.
[0101] [Printed wiring board] A further aspect of this embodiment is The printed wiring board includes a circuit board and a cured film provided on the circuit board. The "cured film" referred to here is a transfer pattern produced by the above method. The cured film is preferably used as a protective film for a conductor portion in a printed wiring board. Various characteristics are required for a protective film for wiring in a printed wiring board, and the transfer pattern of the present embodiment can preferably meet such requirements.
[0102] Examples of the circuit board include a flexible printed wiring board and a rigid board. The printed wiring board can be obtained by using a circuit board as the substrate, and performing a lamination step, an exposure step, a development step, a curing step, and other steps as necessary. When this embodiment is applied to an embodiment related to a flexible printed wiring board, the Young's modulus of the cured film is preferably 3.5 Gpa or less from the viewpoint of the flexibility of the cured film. The Young's modulus may be measured by a known method.
[0103] [Semiconductor Devices] A further aspect of this embodiment is The semiconductor device includes the transfer pattern. Some semiconductor devices have insulating layers formed in multiple layers. The transfer pattern of the present embodiment is particularly useful for semiconductor devices having such insulating layers with a multi-layer structure. EXAMPLES
[0104] The present embodiment will be described in more detail below, but is not limited to the following examples.
[0105] The [measurement methods], [raw materials and samples, etc.], and [evaluation items] for the physical properties, etc., for the examples are as follows:
[0106] [Measurement method] Weight average molecular weight (Mw) and number average molecular weight (Mn) As stated above.
[0107] ≪Mass ratio {(D) component / (A) component}≫ The mass ratio may be determined by analyzing the photosensitive resin layer or the transferred pattern (e.g., an insulating layer in a semiconductor device) by nuclear magnetic resonance spectroscopy (NMR) or gas chromatography / mass spectrometry (GC / MS). Here, the ratio determined from the raw material ratio of the photosensitive resin composition is treated as the mass ratio {component (D) / component (A)}. The mass ratio {component (D) / component (A)} determined from the analysis value of the pattern and the mass ratio {component (D) / component (A)} determined from the raw material ratio of the photosensitive resin composition may be considered to be the same.
[0108] [Raw materials, samples, etc.] ≪(A)~(H) ingredients≫ <Component (A): Alkali-soluble resin> (A-1) ZCR-1797H Acid-modified biphenyl epoxy acrylate {solid content 62% by mass, weight average molecular weight (Mw) 6,500, acid value 98 mgKOH / g; manufactured by Nippon Kayaku Co., Ltd.} (A-2) ZFR-1401H Acid-modified bisphenol F epoxy acrylate {solid content 62% by mass, weight average molecular weight (Mw) 15,000, acid value 98 mgKOH / g; manufactured by Nippon Kayaku Co., Ltd.} (A-3) ZAR-1035 Acid-modified bisphenol A epoxy acrylate {solid content 62% by mass, weight average molecular weight (Mw) 13,000, acid value 98 mgKOH / g; manufactured by Nippon Kayaku Co., Ltd.}
[0109] <Component (B): Compound having an ethylenically unsaturated bond> (B-1) Dimethacrylate of polyethylene glycol with an average of 2 moles of ethylene oxide added to each end of bisphenol A. (B-2) Dimethacrylate of polyethylene glycol with an average of 1 mole of ethylene oxide added to each end of bisphenol A.
[0110] <Component (C): Photopolymerization initiator> (C-1) 4,4'-Bis(diethylamino)benzophenone (C-2) 2-(o-Chlorophenyl)-4,5-diphenylimidazolyl dimer
[0111] <Component (D): Compound having a phenylene ether structure> (D-1) OPE-2St1200 Phenylene ether with an ethylenically unsaturated bond at the end of the main chain, number average molecular weight (Mn) 1,200; manufactured by Mitsubishi Gas Chemical Company, Inc. (D-2) OPE-2St2200 Phenylene ether with an ethylenically unsaturated bond at the end of the main chain, number average molecular weight (Mn) 2,200; manufactured by Mitsubishi Gas Chemical Company, Inc. (D-3) YL7776 Phenylene ether with an ethylenically unsaturated bond at the end of the main chain, number average molecular weight (Mn) 331; manufactured by Mitsubishi Chemical Corporation (D'-1)S201A Polyphenylene ether, number average molecular weight (Mn) 18,000; Asahi Kasei Corporation
[0112] <Component (E): Phenolic resin> (E-1) MEH-7851-4H Phenol-biphenyldiyl resin, weight average molecular weight (Mw) 10,000; manufactured by Meiwa Kasei Co., Ltd.
[0113] <Component (F): Epoxy resin> (F-1)NC-3000H Biphenyl type epoxy resin; manufactured by Nippon Kayaku Co., Ltd.
[0114] <Component (G): Silane coupling agent> (G-1)KBM-573 Phenylaminosilane coupling agent; manufactured by Shin-Etsu Chemical Co., Ltd. (G-2)KBM-9659 Silane coupling agent with isocyanurate group; manufactured by Shin-Etsu Chemical Co., Ltd.
[0115] <Component (H); Solvent> (H-1) Propylene glycol monomethyl ether acetal (PGMEА); Wako Pure Chemical Industries, Ltd.
[0116] ≪Photosensitive resin composition≫ Each component was weighed into a 250 ml plastic bottle according to the composition shown in the table below (where the numbers for each component indicate the proportion (parts by mass) of solid content). Then, PGMEA was mixed so that the solid content concentration was 60 mass%, and the mixture was stirred for 12 hours using a stirrer. In this way, a preparation of a photosensitive resin composition (Examples and Comparative Examples) was obtained. Here, the total amount of components (A) to (G) excluding the solvent contained in component (H) corresponds to the solid content of the photosensitive resin composition.
[0117] <Evaluation film> The prepared solution of the photosensitive resin composition (Examples and Comparative Examples) was uniformly applied to the surface of a 16 μm thick polyethylene terephthalate film (R310-16B, manufactured by Mitsubishi Chemical Corporation) serving as a support film using a blade coater, and then dried for 5 minutes in a dryer at 95° C. Thus, a photosensitive resin layer was formed on the support. The thickness of the photosensitive resin layer after drying (thickness of the photosensitive resin layer before curing) was 15 μm. Thus, a photosensitive resin laminate, i.e., a transfer film, was obtained. Here, a 33 μm thick polyethylene film (GF-858, manufactured by Tamapoly Co., Ltd.) was further laminated as a protective film on the surface of the photosensitive resin layer, and the film was treated as a transfer film (Example and Comparative Example). This transfer film was used as an evaluation sample (evaluation sample), and the following items were evaluated for this. The evaluation results are shown in the table.
[0118] [Evaluation items] <Resolution> While peeling off the protective film from the evaluation sample prepared above, lamination was performed on a flexible copper-clad laminate (Nippon Steel Chemical & Material Co., Ltd., Espanex: MC12-25-00HRM) measuring 10 cm x 15 cm, using a hot roll laminator (Taisei Laminator Co., Ltd., VA-400III). This resulted in a laminate consisting of a three-layer structure of support film / photosensitive resin layer / flexible copper-clad laminate. Here, the lamination conditions were set to a roll temperature of 100°C, air pressure of 0.4 MPa, and speed of 1.0 m / min.
[0119] After leaving it for 15 minutes, a PET mask and a Stoufer 21-step step tablet (a step tablet with an optical density of 0.00 as the first step and an optical density of 0.15 increasing with each step) were placed on the support film, and exposed from the PET mask and step tablet side using a parallel light exposure machine (Oak Manufacturing Co., Ltd., HMW-801). The exposure amount was set to the optimum exposure amount. The PET mask used had a pattern with circular holes in the unexposed areas.
[0120] After the exposure, the substrate was left to stand for 20 minutes or more (here, 30 minutes). After that, the support film was peeled off, and then, using a Fuji Kiko Co., Ltd. developing device, the unexposed portion of the photosensitive resin layer was developed (dissolved and removed) by spraying a developer from a full cone type nozzle. Here, the development conditions were set as follows: spray pressure 0.14 MPa; developer: 3 mass % NaOH aqueous solution at 50°C; and development time (spray time) was twice the time (break point) until the photosensitive resin layer was completely dissolved.
[0121] In the water washing step after development, water was sprayed from a flat type nozzle, where the water washing conditions were set to a spray pressure of 0.08 MPa and a water washing time equal to the development time.
[0122] After washing with water, the evaluation sample was dried by air blowing. The above-mentioned optimum exposure amount means an exposure amount at which the number of steps remaining in the film is 7 to 8 steps when exposed through a Stouffer 21-step tablet.
[0123] The circular hole portion removed by development in the thus obtained sample was observed under an optical microscope to determine the minimum circular hole size (μm; minimum via diameter) that could be developed without residue. The smaller the minimum via diameter, the better the resolution.
[0124] Electrical characteristics While peeling off the protective film from the evaluation sample prepared above, lamination was performed on an easily peelable PET (X-25, manufactured by Lintec Corporation) measuring 10 cm x 15 cm, using a hot roll laminator (VA-400III, manufactured by Taisei Laminator Co., Ltd.). This resulted in a laminate consisting of a three-layer structure of support film / photosensitive resin layer / easily peelable PET. The lamination conditions were set as follows: roll temperature 100°C; air pressure 0.4 MPa; and speed 1.0 m / min.
[0125] After leaving it for 15 minutes, it was exposed from the support film side using a parallel light exposure machine (Oak Manufacturing Co., Ltd., HMW-801). The exposure amount was set to the optimum exposure amount (the definition of which is the same as that in the item "Developability").
[0126] After the exposure, the film was left to stand for 20 minutes or more (30 minutes in this example). Then, the film was developed, washed, and dried in the same manner as in the item "Developability". Then, the film was exposed to 500 mJ / cm 2 from the photosensitive resin layer side using a scattered light exposure machine (Oak Manufacturing Co., Ltd., HMW-201KB). 2 Then, the film was heated in a hot air circulating oven at 220° C. for 60 minutes. The easily peelable PET was then peeled off to obtain a single film of a cured photosensitive resin layer.
[0127] The thus obtained sample was conditioned for 24 hours in an environment of 23° C. and 50% RH. After that, the dielectric loss tangent (Df) and the relative dielectric constant (Dk) at 10 GHz were measured for the sample after the conditioned humidity using the following measuring instruments.
[0128] (Measuring equipment) Network analyzer: PNA Network Analyzer E8362B (Keysight Technologies) Resonator: Split cylinder resonator 10GHz (EM Lab, CR-710)
[0129] <Thermal properties> The support film and the protective film were peeled off from the evaluation sample prepared above, thereby exposing both sides of the photosensitive resin layer. The exposed photosensitive resin layers were then repeatedly stacked together using a laminator to obtain a laminate with a thickness of about 400 μm. The obtained laminate was heated at 220° C. for 60 minutes to obtain a cured sample. The linear expansion coefficient (CTE) of the obtained cured sample was measured in the temperature range from 25° C. to 150° C. using a TMA device under the conditions of a heating rate of 10° C. / min and a force of 50 N. The TMA device used was a TMA7100 (manufactured by Hitachi High-Tech Science Corporation).
[0130] <Tensile strength> A 6-inch silicon wafer substrate with an aluminum vapor deposition layer on the outermost surface was prepared. While peeling off the protective film from the evaluation sample prepared above, lamination was performed on an easily peelable PET (X-25, manufactured by Lintec Corporation) measuring 10 cm x 15 cm, using a hot roll laminator (VA-400III, manufactured by Taisei Laminator Co., Ltd.). This resulted in a laminate consisting of a three-layer structure of a 6-inch silicon wafer substrate with an aluminum vapor deposition layer / a photosensitive resin layer / an easily peelable PET. Here, the lamination conditions were set to a roll temperature of 100°C; an air pressure of 0.4 MPa; and a speed of 1.0 m / min.
[0131] After leaving it for 15 minutes, the easy-peel PET side was exposed to light using a parallel light exposure machine (Oak Manufacturing Co., Ltd., HMW-801). The exposure amount was set to the optimum exposure amount (the definition of which is the same as that in the item "Developability").
[0132] After the exposure, the film was left to stand for 20 minutes or more (30 minutes in this example). Then, the film was developed, washed, and dried in the same manner as in the item "Developability". Then, the film was exposed to 500 mJ / cm 2 from the photosensitive resin layer side using a scattered light exposure machine (Oak Manufacturing Co., Ltd., HMW-201KB). 2 Then, the film was heated in a hot air circulating oven at 220° C. for 60 minutes. The easily peelable PET was then peeled off to obtain a single film of a cured photosensitive resin layer.
[0133] The sample thus obtained was cut into 3 mm widths with a dicing saw to produce 20 cut bodies. After that, the photosensitive resin layer of each cut body was peeled off from the wafer using a dilute hydrochloric acid aqueous solution, thereby obtaining 20 single-film samples. The 20 single-film samples obtained were left to stand for 24 hours or more in an atmosphere of 23°C and 50% relative humidity, and then the tensile strength (Mpa) was measured using a tensile tester (Tensilon). The single-film samples were cured at 220°C before measurement, and the "tensile strength" value in the table indicates the average value of 20 samples. The measurement conditions for the tensile tester were set as follows.
[0134] (Measurement conditions) Temperature: 23℃ Relative humidity: 50% Length of hardened sample: 50mm Thickness of cured sample: 12μm Test speed: 40mm / min Load cell rating: 2kgf
[0135] [Table 1]
[0136] As can be seen from the table, according to the examples, good results were obtained in all of "resolution", "tensile strength", "thermal properties", and "electrical properties". In contrast, the comparative examples were insufficient in at least one of the <<resolution>>, <<tensile strength>>, <<thermal properties>>, and <<electrical properties>>. Comparative Example 1, for example, was insufficient in <<resolution>>, Comparative Example 2, for example, was insufficient in <<tensile strength>> and <<electrical properties>>, and Comparative Example 3, for example, was insufficient in <<resolution>> and <<tensile strength>>.
[0137] According to the examples, it was possible to manufacture a printed wiring board and, in turn, a semiconductor device using this in a conventional manner. [Industrial Applicability]
[0138] According to the present invention, it is possible to provide a photosensitive resin composition capable of obtaining a transfer film that can be patterned by exposure and development, and a cured product pattern that is excellent in mechanical strength and electrical properties. For example, the composition has industrial applicability as an insulating layer for a multilayer printed wiring board, a solder resist, and a part of a semiconductor device. The present invention is also useful as a low dielectric resin composition for realizing a protective material for wiring in FPCs (flexible printed circuits) and an insulating layer for printed wiring boards.
Claims
1. Component (A): an alkali-soluble resin; (D) component: a compound having a number average molecular weight (Mn) of 10,000 g / mol or less and having a phenylene ether structure; a mass ratio of the component (D) to the component (A) {component (D) / component (A)} is 0.05 to 1.
30.
2. The photosensitive resin composition according to claim 1, further comprising: component (B): a compound having an ethylenically unsaturated bond.
3. 3. The photosensitive resin composition according to claim 1, wherein the number average molecular weight of the component (D) is 300 to 5,000 g / mol.
4. 3. The photosensitive resin composition according to claim 1, wherein a mass ratio of the component (D) to the component (A) {component (D) / component (A)} is 0.10 to 0.
50.
5. The photosensitive resin composition according to claim 1 or 2, wherein the component (D) has a polymerizable functional group.
6. 3. The photosensitive resin composition according to claim 1, wherein the proportion of the component (D) in the photosensitive resin composition is 2.0 to 24 mass%.
7. Component (E): The photosensitive resin composition according to claim 1 or 2, further comprising a phenolic resin.
8. The photosensitive resin composition according to claim 1 or 2, wherein the component (A) comprises a carboxyl group-containing epoxy (meth)acrylate resin.
9. A transfer film which is a laminate having a support and a photosensitive resin layer containing the photosensitive resin composition according to claim 1 or 2.
10. The transfer film according to claim 9, which is for forming a via having a diameter of less than 20 (μm).
11. A method for forming a pattern, comprising the steps of exposing the photosensitive resin composition according to claim 1 or 2 to light and developing it.
12. The method for forming a pattern according to claim 11 , wherein the pattern includes vias having a via diameter of less than 20 (μm).
13. A cured product obtained by heat curing the photosensitive resin composition according to claim 1 or 2.
14. The cured product according to claim 13, which is used as a protective film for wiring in a printed wiring board.
15. A semiconductor device comprising the cured product according to claim 13.
Citation Information