Method for producing magnesium oxide
A novel method for producing magnesium oxide with needle-like or plate-like crystals addresses the handling challenges of bulky particles by optimizing crystallization conditions, resulting in easier-to-handle magnesium oxide with enhanced tabletability and productivity.
Patent Information
- Application Number
- JP2023078593
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2043-05-11
AI Technical Summary
Existing methods for producing magnesium oxide often result in bulky particles that are difficult to handle, posing challenges in forming tablets, particularly in pharmaceutical and food applications.
A method involving a carbonation step, separation step, crystallization step, and firing step, with specific temperature and time conditions for crystallization to produce needle-like or plate-like magnesium carbonate crystals, which are then fired to obtain easier-to-handle magnesium oxide.
The method produces magnesium oxide with improved handling properties due to its reduced bulk, enhancing tabletability and productivity, aligning with Sustainable Development Goals.
Smart Images

Figure 2024162738000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel method for producing magnesium oxide. [Background technology]
[0002] Magnesium oxide is used in various industrial fields as an industrial and pharmaceutical raw material. For example, magnesium oxide is known to exhibit excellent properties in various applications such as medicines, foods, vulcanization accelerators, pigments, chemical heat storage materials, battery materials, ceramic materials, adsorbents, abrasives, and catalysts.
[0003] Magnesium oxide is industrially produced by various methods using seawater, irrigation, bittern, etc. as magnesium raw materials. Among these methods, a method is known in which magnesium oxide is produced by using a magnesium compound such as magnesium oxide, magnesium hydroxide, magnesium carbonate, etc. as a magnesium oxide precursor and calcining the magnesium oxide precursor, as disclosed in Patent Document 1, for example.
[0004] As a method for producing magnesium carbonate, for example, Patent Document 2 proposes a method for producing high-purity magnesium carbonate, particularly magnesium carbonate with a low iron content, from low-grade magnesium hydroxide produced as an ore. Specifically, the method proposes blowing an oxygen-containing gas together with carbon dioxide into a suspension of low-grade magnesium hydroxide to form a solution containing magnesium bicarbonate, and heating the liquid after solid-liquid separation to generate and precipitate magnesium carbonate. According to the production method of Patent Document 2, it is said that high-purity magnesium carbonate can be easily produced.
[0005] Patent Document 3 also proposes a method for removing impurities in a method for producing magnesium carbonate by reacting magnesium hydroxide slurry with carbon dioxide gas. Specifically, the proposed method for removing impurities involves maintaining the pH, which decreases during the carbonation process, at a pH value of 7.6 to 8.0 at which magnesium carbonate does not dissolve 100%, and filtering the reaction liquid after carbonation using undissolved magnesium produced at the end of carbonation as a precoat agent.
[0006] It is expected that high-purity magnesium oxide can be obtained by adopting the methods described in these patent documents as part of a method for producing magnesium oxide. Such high-purity magnesium oxide is used, for example, in tablets for pharmaceuticals or foods. As an example of such tablets, Patent Document 4 discloses a tablet containing magnesium oxide particles as a main component. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] International Publication No. 2017 / 195686 [Patent Document 2] JP 2010-132504 A [Patent Document 3] Japanese Patent Application Publication No. 63-40722 [Patent Document 4] International Publication No. 2011 / 030659 Summary of the Invention [Problem to be solved by the invention]
[0008] Such tablets are produced by molding a composition containing magnesium oxide as a main component into a predetermined shape by compression molding called tableting. However, when the methods described in Patent Documents 1 to 3 are used, bulky magnesium oxide may be obtained, which may make it difficult to handle the tablets.
[0009] In cases where magnesium oxide that is easier to handle is required, the magnesium oxide formed by the methods of Patent Documents 1 to 3 mentioned above is not sufficient, and further improvements are required.
[0010] Therefore, an object of the present invention is to provide a novel method for producing magnesium oxide which is easier to handle. [Means for solving the problem]
[0011] The present disclosure includes the following aspects.
[0012] (First Disclosure) The first disclosure relates to a method for producing magnesium oxide. The method for producing magnesium oxide of the first disclosure includes the following carbonation step, separation step, crystallization step, and calcination step. The carbonation step is a step in which carbon dioxide gas is blown into a suspension of a magnesium compound to obtain an aqueous solution of magnesium hydrogen carbonate. The separation step is a step of subjecting the aqueous magnesium hydrogen carbonate solution to solid-liquid separation. The crystallization step is a step of crystallizing magnesium carbonate from the aqueous solution obtained in the separation step. The calcination step is a step of calcining the magnesium carbonate to obtain magnesium oxide. In the first disclosure, the crystallization step is carried out under crystallization conditions in which the crystallization temperature is equal to or higher than 50° C. and lower than 80° C. Furthermore, the crystallization step is carried out under crystallization conditions in which the product of the crystallization temperature and the crystallization time is equal to or higher than 60° C.·h and lower than 210° C.·h.
[0013] (Second Disclosure) A second disclosure is the production method according to the first disclosure, characterized in that the crystallization temperature is 60°C or higher and 70°C or lower.
[0014] (Third Disclosure) A third disclosure is the production method according to the first or second disclosure, characterized in that the product of the crystallization temperature and the crystallization time is 120°C·h or more and 140°C·h or less.
[0015] (Fourth Disclosure) A fourth disclosure is the manufacturing method according to any one of the first to third disclosures, characterized in that the crystallization step further includes a heating step of heating the crystallized magnesium carbonate.
[0016] (Fifth Disclosure) A fifth disclosure is the manufacturing method according to the fourth disclosure, characterized in that the heating step heats the magnesium carbonate at a temperature of 50°C or higher and 250°C or lower.
[0017] (Sixth Disclosure) A sixth disclosure is the manufacturing method according to the fourth or fifth disclosure, characterized in that the heating step heats the magnesium carbonate for a heating time of 1 hour or more and 72 hours or less.
[0018] (Seventh Disclosure) A seventh disclosure is the manufacturing method according to any one of the fourth to sixth disclosures, characterized in that the calcination step calcines the magnesium carbonate heated in the heating step at a temperature of 600°C or higher and 1500°C or lower. Effect of the Invention
[0019] According to the production method of the present invention, magnesium oxide which is easier to handle can be obtained. [Brief description of the drawings]
[0020] [Figure 1] 1 shows scanning electron micrographs of magnesium carbonate (a), which is an intermediate product, and magnesium oxide (b), which is a final product after firing, in Example 1, and magnesium carbonate (c), which is an intermediate product, and magnesium oxide (d), which is a final product after firing, in Comparative Example 5. The white lines in the figures indicate a length of 1 μm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] Hereinafter, preferred embodiments of the method for producing magnesium oxide of the present invention will be described in detail. In this specification, various numerical ranges include the upper and lower limit values unless otherwise specified.
[0022] [Magnesium oxide manufacturing method] One embodiment of the present invention is a method for producing magnesium oxide, which includes the following carbonation step, separation step, crystallization step, and calcination step. In the carbonation step, carbon dioxide gas is blown into a suspension of a magnesium compound to obtain an aqueous magnesium hydrogen carbonate solution. In the separation step, the aqueous magnesium hydrogen carbonate solution is subjected to solid-liquid separation. In the crystallization step, magnesium carbonate is crystallized from the aqueous solution obtained in the separation step. In the calcination step, magnesium oxide is obtained by calcining the magnesium carbonate.
[0023] In this embodiment, the crystallization step is performed under crystallization conditions in which the crystallization temperature is 50° C. or more and less than 80° C. Furthermore, the crystallization step is performed under crystallization conditions in which the product of the crystallization temperature and the crystallization time is 60° C. h or more and less than 210° C. h.
[0024] By carrying out the crystallization step under such specific crystallization conditions, the crystal form of the crystallized magnesium carbonate tends to be needle-like crystals or plate-like crystals. This reduces the bulk of the magnesium carbonate, and allows for improved handling of the magnesium carbonate. Furthermore, since the crystal form of the magnesium carbonate is inherited by the crystal form of the magnesium oxide obtained after firing, the crystal form of the magnesium oxide after firing also tends to be needle-like crystals or plate-like crystals. This reduces the bulk of the magnesium oxide after firing, and allows for improved handling during molding of the magnesium oxide. Therefore, according to the manufacturing method of this embodiment, magnesium oxide that is easier to handle can be obtained.
[0025] The manufacturing method of this embodiment has the advantage that if magnesium oxide that is easy to handle can be obtained, the productivity of products containing the magnesium oxide can be improved, and it can contribute to the achievement of the SDGs (Sustainable Development Goals) adopted at the United Nations Summit.
[0026] The magnesium compound suspension that can be used in the production method of this embodiment is not particularly limited, and examples thereof include suspensions containing magnesium hydroxide, magnesium silicate, magnesium oxide, magnesium carbonate, or a mixture of two or more of these.
[0027] For example, when a magnesium hydroxide suspension is used as the suspension of the magnesium compound, the magnesium hydroxide suspension can be obtained by a magnesium hydroxide suspension production step using seawater or an aqueous magnesium chloride solution as a raw material. That is, the production method of the present embodiment may include such a magnesium hydroxide suspension production step prior to the carbonation step.
[0028] The magnesium hydroxide suspension production process may be a process in which a magnesium source and an alkali source are mixed and reacted. Alternatively, the magnesium hydroxide suspension production process may be a process in which magnesium hydroxide produced as a mineral is suspended in water. When the former process is adopted as the magnesium hydroxide suspension production process, the magnesium source may be, for example, seawater or an aqueous magnesium chloride solution. It is preferable to use seawater as the magnesium source.
[0029] On the other hand, the alkali source to be reacted with the magnesium source is not particularly limited, and for example, calcium hydroxide can be used. An example of calcium hydroxide is slaked lime. Slaked lime can be obtained by slaked lime, which is calcium oxide. Slaked lime may be in the form of milk of lime, for example.
[0030] The above-mentioned production process is an example of a production process for a magnesium hydroxide suspension, but when a suspension of a magnesium compound other than magnesium hydroxide is used, a production process according to the type of magnesium compound may be adopted. Note that, when a suspension of a magnesium compound can be obtained without a production process, such a production process may not be included.
[0031] The suspension of the magnesium compound obtained by the above-mentioned production process is then subjected to the subsequent carbonation process.
[0032] Various steps that may be included in the method for producing magnesium oxide of this embodiment will be described in detail below.
[0033] <Carbonation process> The carbonation step is a step of blowing carbon dioxide gas into a suspension of a magnesium compound to obtain an aqueous magnesium hydrogen carbonate solution. The carbon dioxide gas that can be used in the carbonation step may contain other gases within a range that does not inhibit the carbonation of the magnesium compound. In addition, when blowing carbon dioxide gas into a suspension of a magnesium compound, it is preferable to blow the carbon dioxide gas while stirring the suspension.
[0034] Furthermore, in the carbonation step, it is preferable to adjust the pH of the suspension of the magnesium compound. At this time, the pH of the suspension of the magnesium compound may be adjusted according to the type of impurities contained in the suspension or the type of impurities to be preferentially removed so that impurity components with relatively low ionization tendency are precipitated as solids. Examples of impurities include Fe, Al, Si, As, and Pb.
[0035] For example, the pH of the magnesium compound suspension is preferably adjusted to less than 7.5 or less than 7.4. Alternatively, the pH of the magnesium compound suspension is preferably adjusted to 7.0 or more or 7.1 or more. In the carbonation step, by adjusting the pH of the magnesium compound suspension within such a range, impurities contained in the suspension can be sufficiently precipitated as solids while the magnesium bicarbonate, which is the magnesium component, is left dissolved. Furthermore, as a result, magnesium oxide of higher purity can be obtained. Note that, when the pH of the magnesium compound suspension is 7.5 or more, the amount of dissolved magnesium component is reduced, and there is a risk that a good yield cannot be obtained.
[0036] Incidentally, impurities precipitated as solids by adjusting the pH of the suspension can be removed by solid-liquid separation in the subsequent separation step. In this way, by sufficiently reducing impurities at the carbonation step or separation step, the magnesium oxide obtained through the subsequent crystallization step and firing step has an extremely low impurity content and is therefore a magnesium oxide with a higher purity.
[0037] In the carbonation step, the pH of the suspension of the magnesium compound may be adjusted by blowing in carbon dioxide gas. In this case, the carbonation step is preferably performed while continuously or intermittently measuring the pH of the suspension of the magnesium compound.
[0038] In the carbonation step, the supply amount of carbon dioxide gas when blowing the carbon dioxide gas into the suspension of the magnesium compound is not particularly limited. For example, the supply amount of carbon dioxide gas is 5.0 L / min or less. For example, the supply amount of carbon dioxide gas is 0.1 L / min or more. The preferred upper limit of the supply amount of carbon dioxide gas is 3.0 L / min or less. The preferred lower limit of the supply amount of carbon dioxide gas is 0.2 L / min or more.
[0039] In the carbonation step, the concentration of the magnesium compound suspension is not particularly limited. For example, the concentration of the magnesium compound suspension is 30 g / L or less. For example, the concentration of the magnesium compound suspension is 1 g / L or more. The concentration of the magnesium compound suspension is preferably 28 g / L or less. In addition, the concentration of the magnesium compound suspension is preferably 3 g / L or more. The concentration of the magnesium compound suspension can be calculated by the following formula. Concentration of suspension (g / L) = weight of magnesium compound (g) / volume of suspension (L)
[0040] In the carbonation step, the temperature of the suspension when blowing in carbon dioxide gas is not particularly limited, but it is preferable to blow in carbon dioxide gas after bringing the suspension of the magnesium compound to a temperature of 0°C or higher and 50°C or lower. When the temperature of the suspension is within this range, multiple types of impurities contained in the suspension can be more reliably precipitated. As a result, magnesium oxide with even higher purity can be obtained.
[0041] In the carbonation step, the more preferred upper limit temperature of the suspension of the magnesium compound is 40° C. In the carbonation step, the even more preferred upper limit temperature of the suspension of the magnesium compound is 30° C. In the carbonation step, the more preferred lower limit temperature of the suspension of the magnesium compound is 20° C.
[0042] In the carbonation step, it is preferable that the aqueous magnesium hydrogen carbonate solution after the carbon dioxide gas is blown in contains undissolved magnesium carbonate. If the aqueous magnesium hydrogen carbonate solution after the carbon dioxide gas is blown in contains such undissolved magnesium carbonate, solid-liquid separation after the carbonation step becomes easy. As a result, magnesium oxide of higher purity can be obtained.
[0043] In the carbonation step, carbon dioxide gas may be blown into the suspension of the magnesium compound, followed by blowing air. By first blowing carbon dioxide gas into the suspension of the magnesium compound, the magnesium component can be dissolved while Fe, which is an impurity, can be precipitated. Next, by blowing air into the suspension, the still dissolved Fe can be precipitated as FeO. This makes it possible to obtain magnesium oxide of even higher purity, with Fe as an impurity further reduced.
[0044] The impurities precipitated as solids in the carbonation step as described above can be removed by solid-liquid separation in the next separation step. That is, the aqueous magnesium hydrogen carbonate solution obtained in the carbonation step is subjected to the next separation step.
[0045] <Separation process> The separation step is a step of performing solid-liquid separation of the aqueous magnesium hydrogen carbonate solution after the carbonation step. More specifically, the separation step is a step of separating the aqueous magnesium hydrogen carbonate solution, which is a liquid component, from impurities, which are solid components. This step removes the impurities from the aqueous magnesium hydrogen carbonate solution, thereby obtaining an aqueous magnesium hydrogen carbonate solution with high purity.
[0046] In this specification, the term "separation" includes not only the case where the solid content and the liquid content are completely separated, but also the case where a small amount of water is unavoidably contained in the solid content.
[0047] The separation means that can be used in the separation step is not particularly limited, and examples thereof include filtration means, membrane separation means, centrifugation means, solid-liquid separation means, and natural settling means.
[0048] In the separation step, the magnesium hydrogen carbonate aqueous solution after the carbonation step may be used as it is, but is not limited to such a form. For example, in the separation step, water may be added to the magnesium hydrogen carbonate aqueous solution in advance to adjust the concentration. The water used in this case may be, for example, ion-exchanged water. In addition, the separation step may be performed only once, or may be performed in two or more separate steps.
[0049] In the separation step, the pH may be adjusted according to the type of impurities to be removed. Furthermore, the carbonation step and the separation step may be regarded as one set, and these steps may be repeated in multiple sets. In this case, the pH of the suspension may be adjusted to be different for each set. Alternatively, the pH of the suspension may be adjusted to be the same for each set.
[0050] The aqueous magnesium hydrogen carbonate solution from which impurities have been removed by the above separation steps is subjected to the next crystallization step.
[0051] <Crystallization process> The crystallization step is a step of crystallizing magnesium carbonate from the aqueous solution obtained in the separation step. In the crystallization step, the aqueous solution after the separation step is heated at a predetermined temperature for a predetermined time, thereby crystallizing magnesium carbonate. In this specification, the "heating temperature when crystallizing magnesium carbonate" is referred to as the "crystallization temperature" to distinguish it from the heating temperature in the heating step described below. Similarly, the "heating time when crystallizing magnesium carbonate" is referred to as the "crystallization time".
[0052] (crystallization temperature) In this embodiment, the crystallization temperature when crystallizing magnesium carbonate is 50° C. or more and less than 80° C. Furthermore, the crystallization temperature is preferably 60° C. or more and 70° C. or less. If the crystallization temperature is 80° C. or more, the crystal form of the obtained magnesium carbonate becomes petal-like crystals, and the bulk tends to be large.
[0053] Furthermore, in this embodiment, the crystallization step is performed under crystallization conditions in which the product of the crystallization temperature and the crystallization time is 60°C·h or more and less than 210°C·h. By performing the crystallization step under specific crystallization conditions in which the crystallization temperature is 50°C or more and less than 80°C, and the product of the crystallization temperature and the crystallization time is 60°C·h or more and less than 210°C·h, magnesium carbonate in the form of needle-like crystals or plate-like crystals can be crystallized. In this way, when the crystal form of the crystallized magnesium carbonate becomes needle-like crystals or plate-like crystals, the crystal form of the magnesium oxide after firing also tends to become needle-like crystals or plate-like crystals. As a result, the bulk of the magnesium oxide becomes low, and magnesium oxide that is easier to handle can be obtained. Note that, when the product of the crystallization temperature and the crystallization time is 210°C·h or more, the crystal form of the obtained magnesium carbonate becomes petal-like crystals, and the bulk tends to be high.
[0054] The crystallization conditions are preferably such that the crystallization temperature is 60° C. or higher and 70° C. or lower, and the product of the crystallization temperature and the crystallization time is 60° C. h or higher and less than 210° C. h. When the crystallization step is carried out under such crystallization conditions, magnesium carbonate can be more reliably crystallized into needle-like or plate-like crystals.
[0055] The crystallization conditions are preferably such that the crystallization temperature is 50° C. or higher and lower than 80° C., and the product of the crystallization temperature and the crystallization time is 120° C. h. or higher and 140° C. h. When the crystallization step is carried out under such crystallization conditions, magnesium carbonate can be more reliably crystallized into needle-like or plate-like crystals.
[0056] Furthermore, the crystallization conditions are particularly preferably such that the crystallization temperature is from 60° C. to 70° C., and the product of the crystallization temperature and the crystallization time is from 120° C. h to 140° C. h. When the crystallization step is carried out under such crystallization conditions, magnesium carbonate can be more reliably crystallized into needle-like or plate-like crystals.
[0057] (Crystallization time) In this embodiment, the crystallization time when crystallizing magnesium carbonate is not particularly limited as long as the product of the crystallization temperature and the crystallization time is 60°C·h or more and less than 210°C·h. That is, the crystallization time may be in the range of 0.75 hours or more and less than 4.2 hours. In this specification, the crystallization time means the time during which the temperature is maintained from the point at which the aqueous solution after the separation step is heated to the crystallization temperature.
[0058] (Heating process) In this embodiment, the crystallization step may further include a heating step of heating the crystallized magnesium carbonate. By heating the crystallized magnesium carbonate, the crystal form of the magnesium carbonate is more likely to become needle-like crystals or plate-like crystals. As a result, the bulk of the magnesium carbonate is more likely to be reduced, and the handling of the magnesium carbonate can be more reliably improved.
[0059] (Heating temperature) In the heating step, the heating temperature of magnesium carbonate is not particularly limited, but may be, for example, a temperature of 50° C. or more and 250° C. or less. From the viewpoint of handling magnesium carbonate, the lower limit of the heating temperature is preferably 60° C. From the viewpoint of ease of handling magnesium carbonate or productivity, the upper limit of the heating temperature is preferably 150° C.
[0060] (Heating time) In the heating step, the heating time of magnesium carbonate is not particularly limited, but may be, for example, 1 hour or more and 72 hours or less. From the viewpoint of handling magnesium carbonate, the preferable lower limit of the heating time is 3 hours. From the viewpoint of ease of handling magnesium carbonate or productivity, the preferable upper limit of the heating time is 48 hours.
[0061] The magnesium carbonate crystallized by the above-described crystallization step is obtained as a solid content in an aqueous solution. Therefore, magnesium carbonate as a solid can be obtained by subjecting an aqueous solution containing the crystallized magnesium carbonate to solid-liquid separation. That is, the crystallization step may further include a step of subjecting an aqueous solution containing the crystallized magnesium carbonate to solid-liquid separation to obtain magnesium carbonate as a solid.
[0062] The means for performing solid-liquid separation of the aqueous solution containing the crystallized magnesium carbonate is not particularly limited, and for example, the same separation means as those in the above-mentioned separation step can be used.
[0063] In the crystallization step, a washing step of the crystallized magnesium carbonate may be carried out, if necessary.
[0064] The magnesium carbonate obtained by the above crystallization step is subjected to the next calcination step.
[0065] <Firing process> The calcination step is a step in which the magnesium carbonate obtained in the crystallization step is calcined to obtain magnesium oxide.
[0066] The calcination means for calcining magnesium carbonate is not particularly limited as long as it can produce magnesium oxide. Examples of such calcination means include a calcination furnace or a microwave calcination means.
[0067] The calcination temperature when calcining magnesium carbonate is not particularly limited as long as it is a temperature at which magnesium oxide can be produced. Examples of such a calcination temperature include a temperature of 600°C or higher. The upper limit of the calcination temperature is not particularly limited, but is, for example, 1500°C from the viewpoint of the quality or productivity of magnesium oxide. The calcination temperature is preferably 700°C or higher. Also, the calcination temperature is preferably 1200°C or lower.
[0068] The calcination time when calcining magnesium carbonate is not particularly limited as long as it is a time that can produce magnesium oxide. Such a calcination time can be 1 minute or more. The upper limit of the calcination time is not particularly limited, but is, for example, 24 hours from the viewpoint of productivity. The calcination time is preferably 30 minutes or more. Also, the calcination time is preferably 6 hours or less.
[0069] The magnesium oxide obtained by the above firing step may be subjected to an additional treatment step, if necessary, such as a surface treatment step in which the surface of magnesium oxide particles is treated with various surface treatment agents, a crushing step in which magnesium oxide is crushed into powder, a classification step in which magnesium oxide is classified according to particle size, or a molding step in which magnesium oxide is molded into a predetermined shape.
[0070] According to the manufacturing method of this embodiment as described above, magnesium oxide that is easier to handle can be obtained.
[0071] The manufacturing method of the present invention is not limited to the above-described embodiment or the examples described below, and appropriate combinations, substitutions, modifications, etc. are possible within the scope that does not deviate from the object and spirit of the present invention. EXAMPLES
[0072] The present invention will be described in more detail below by way of examples and comparative examples, but the present invention is not limited to these examples.
[0073] Example 1 A 15 g / L magnesium hydroxide suspension was placed in a reaction vessel. Carbon dioxide gas was blown into the magnesium hydroxide suspension at a rate of 500 mL / min while stirring until the pH of the suspension reached a predetermined value, to obtain an aqueous magnesium hydrogen carbonate solution.
[0074] The obtained aqueous magnesium hydrogen carbonate solution was subjected to solid-liquid separation using a Nutsche separator to remove solid impurities. The solution was then heated to 70°C and held at that temperature for 1 hour to precipitate magnesium carbonate. The solution was then filtered to obtain a solid product of magnesium carbonate. The obtained solid product was then heated at 105°C for 24 hours to obtain a powder of basic magnesium carbonate.
[0075] A crucible for firing was prepared and basic magnesium carbonate was placed in it. This crucible was placed in a firing furnace that had been heated and maintained at 900°C in advance. After being placed in the crucible, firing was carried out at 900°C for 2 hours under atmospheric pressure to obtain a magnesium oxide fire product. The obtained fire product was sieved through a 150 micron filter to obtain the magnesium oxide powder of Example 1.
[0076] Example 2 Magnesium oxide powder of Example 2 was obtained in the same manner as in Example 1, except that the crystallization time was changed to 2 hours.
[0077] Example 3 Magnesium oxide powder of Example 3 was obtained in the same manner as in Example 1, except that the crystallization temperature was changed to 60°C.
[0078] Example 4 Magnesium oxide powder of Example 4 was obtained in the same manner as in Example 1, except that the crystallization temperature and crystallization time were changed to 60° C. and 2 hours, respectively.
[0079] Example 5 Magnesium oxide powder of Example 5 was obtained in the same manner as in Example 1, except that the crystallization temperature and crystallization time were changed to 60° C. and 3 hours, respectively.
[0080] Example 6 Magnesium oxide powder of Example 6 was obtained in the same manner as in Example 1, except that the firing temperature was changed to 800°C.
[0081] Comparative Example 1 Magnesium oxide powder of Comparative Example 1 was obtained in the same manner as in Example 1, except that the crystallization time was changed to 3 hours.
[0082] Comparative Example 2 Magnesium oxide powder of Comparative Example 2 was obtained in the same manner as in Example 1, except that the crystallization temperature was changed to 80°C.
[0083] Comparative Example 3 Magnesium oxide powder of Comparative Example 3 was obtained in the same manner as in Example 1, except that the crystallization temperature and crystallization time were changed to 90° C. and 0.5 hours, respectively.
[0084] Comparative Example 4 Magnesium oxide powder of Comparative Example 4 was obtained in the same manner as in Example 1, except that the crystallization temperature was changed to 90°C.
[0085] Comparative Example 5 Magnesium oxide powder of Comparative Example 5 was obtained in the same manner as in Example 1, except that the crystallization temperature and crystallization time were changed to 95° C. and 3 hours, respectively.
[0086] Comparative Example 6 Magnesium oxide powder of Comparative Example 6 was obtained in the same manner as in Example 1, except that the crystallization temperature and crystallization time were changed to 95° C. and 6 hours, respectively.
[0087] The bulk (mL / 10 g) of each of the magnesium carbonate intermediate products and magnesium oxide final products obtained in the above-described manner in Examples 1 to 6 and Comparative Examples 1 to 6 was measured according to the following measurement method. The measurement results are shown in Table 1 below.
[0088] (How to measure bulk) Weigh out 5 g of the magnesium carbonate or magnesium oxide sample to be measured, place it in a 100 mL measuring cylinder, and measure the volume (mL) of the sample. Convert the volume (mL) per 5 g of sample obtained to the volume (mL) per 10 g, and use this as the volume (mL / 10 g).
[0089] [Table 1]
[0090] Magnesium carbonate, which is the intermediate product of Example 1, and magnesium oxide, which is the final product after firing, were observed with a scanning electron microscope to confirm their respective crystal forms. Similarly, magnesium carbonate, which is the intermediate product of Comparative Example 5, and magnesium oxide, which is the final product after firing, were observed with a scanning electron microscope to confirm their respective crystal forms. These scanning electron microscope photographs are shown in FIG.
[0091] (Tableting test) Using a manual tabletop tablet molding machine HAND-TAB (Ichihashi Seiki Co., Ltd., HANDTAB-100R), magnesium oxides (250 mg, φ10 flat punch) of Examples 1 to 6 were compressed under a pressure of 10 kN to form tablets. The obtained tablets were measured for thickness (mm) and hardness (N) as tablet evaluation. Tablet hardness was measured using a load cell type tabletop hardness tester (Okada Seiko Co., Ltd., DC-50). The measured value of tablet hardness was the average value of three measurements. The results of tablet evaluation are shown in Table 2 below.
[0092] [Table 2]
[0093] As shown in Table 1, it was found that the magnesium oxides of Examples 1 to 6 produced by the production method of the present invention all had low bulk and could be easily handled during molding. In addition, it was found that the magnesium carbonates, which were the intermediate products of Examples 1 to 6, also had low bulk and were easy to handle. On the other hand, it was found that the magnesium oxides of Comparative Examples 1 to 6, which were produced by the production methods with different crystallization conditions, were all bulky and difficult to handle during molding. In addition, it was found that the magnesium carbonates, which were the intermediate products of Comparative Examples 1 to 6, were also bulky and difficult to handle.
[0094] Furthermore, as shown in Fig. 1, the magnesium carbonate intermediate product of Example 1 and the magnesium oxide final product after firing both had a crystal morphology of needle-like crystals. On the other hand, the magnesium carbonate intermediate product of Comparative Example 5 and the magnesium oxide final product after firing both had a crystal morphology of bulky petal-like crystals. It is presumed that the difference in bulk between the above-mentioned Examples and Comparative Examples is due to the difference in crystal morphology.
[0095] In addition, as shown in Table 2, the magnesium oxides of Examples 1 to 6 were found to have excellent tabletability. [Industrial Applicability]
[0096] The method for producing magnesium oxide of the present invention can be suitably utilized for producing magnesium oxide that can be used for various applications such as pharmaceuticals, foods, vulcanization accelerators, pigments, chemical heat storage materials, battery materials, ceramic materials, adsorbents, abrasives, and catalysts.
Claims
1. a carbonation step of blowing carbon dioxide gas into the suspension of the magnesium compound to obtain an aqueous magnesium hydrogen carbonate solution; A separation step of subjecting the aqueous magnesium hydrogen carbonate solution to solid-liquid separation; a crystallization step of crystallizing magnesium carbonate from the aqueous solution obtained in the separation step; A calcination step of calcining the magnesium carbonate to obtain magnesium oxide, The crystallization step is carried out under crystallization conditions in which the crystallization temperature is 50° C. or higher and lower than 80° C., and the product of the crystallization temperature and the crystallization time is 60° C. h or higher and lower than 210° C. h.
2. The method according to claim 1, wherein the crystallization temperature is 60° C. or higher and 70° C. or lower.
3. The method according to claim 1, wherein the product of the crystallization temperature and the crystallization time is 120° C.·h or more and 140° C.·h or less.
4. The method according to claim 1 , wherein the crystallization step further comprises a heating step of heating the crystallized magnesium carbonate.
5. The method according to claim 4, wherein the heating step heats the magnesium carbonate at a temperature of 50° C. or more and 250° C. or less.
6. The method according to claim 4, wherein the heating step heats the magnesium carbonate for a heating time of 1 hour or more and 72 hours or less.
7. The method according to claim 5 , wherein the calcination step calcines the magnesium carbonate heated in the heating step at a temperature of 600° C. or more and 1500° C. or less.
Citation Information
Patent Citations
Preparation method of nanometer magnesia
CN104445297A
Magnesia particle and its manufacturing method
JP2004175644A
Method for removing impurity in production of magnesium carbonate
JP1988040722A
Method for producing high purity magnesium carbonate
JP2010132504A
Antacid and laxative tablet
WO2011030659A1