EPDM composition
The EPDM composition addresses roll processability and biomass maintenance by blending liquid polybutadiene and terpene resin with plant-derived components, enhancing compatibility and preventing bagging, thus maintaining environmental sustainability.
Patent Information
- Application Number
- JP2023078600
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-21
AI Technical Summary
Existing EPDM compositions using plant-derived components face issues with poor roll processability due to bagging and reduced biomass content, necessitating the use of mineral oil plasticizers that compromise the environmental impact.
A composition incorporating 1.0 to 12.0 parts by weight of liquid polybutadiene and 1.0 to 12.0 parts by weight of terpene resin, both containing plant-derived components, is blended with an ethylene-propylene-diene ternary copolymer to enhance compatibility and maintain biomass while suppressing bagging.
The composition achieves improved roll processability by reducing dough viscosity and maintaining biomass content, with a minimal change in biomass degree of less than -1.5%, while preventing bagging during kneading.
Abstract
Description
[Technical field]
[0001] The present invention relates to an EPDM composition, and more particularly to an EPDM composition which is effectively used as a rubber vulcanization molding material for sealing and vibration isolation. [Background technology]
[0002] Ethylene-propylene-diene terpolymer rubber (EPDM) has good heat resistance due to its polymer structure and is widely used as a molding material for industrial parts.
[0003] Among these various parts, peroxide crosslinking is used for gaskets, valves, etc., which require good compression set resistance. Here, since the peroxide crosslinking system has a short crosslinking induction time and a fast rise in crosslinking, it is necessary to add a plasticizer to improve molding defects in items that require fluidity, such as complex or thin shapes, because the peroxide crosslinking system has a short crosslinking induction time and a fast rise in crosslinking.
[0004] The applicant has previously proposed a sealing rubber composition that satisfies moldability and provides a crosslinked product with good compression set resistance, comprising 100 parts by weight of ethylene-propylene-diene copolymer rubber, (A) 32 to 60 parts by weight of carbon black A having an average particle size of 60 to 100 nm, an iodine adsorption of 14 to 23 g / kg, and a DBP oil absorption of 100 ml / 100 g or more, (B) 10 to 30 parts by weight of carbon black B having an average particle size of 40 to 50 nm, an iodine adsorption of 35 to 49 g / kg, and a DBP oil absorption of 100 to 160 ml / 100 g, (C) 2 to 10 parts by weight of an ethylene-α-olefin copolymer, and (D) 0 to 16 parts by weight of silica (Patent Document 1).
[0005] On the other hand, in recent years, with a view to realizing a sustainable society, it has become increasingly important to actively utilize plant-derived raw materials, which absorb and fix carbon dioxide during their production process, because they are superior to petroleum-based raw materials in that they can be recycled without changing the total amount of carbon dioxide in the atmosphere and because they are a non-depletable raw material.
[0006] From this viewpoint, there is a strong demand for the use of plant-derived raw materials in rubber compositions, particularly in EPDM compositions which are widely used for sealing materials, anti-vibration rubbers and the like.
[0007] In rubber compositions using EPDM, when the processability during kneading with an open roll (hereinafter referred to as roll processability) is poor, the rubber wound around the roll peels off from the surface, a phenomenon known as bagging. In order to suppress this bagging, a mineral oil-based plasticizer that is compatible with EPDM is generally added. However, when EPDM containing at least a portion of plant-derived components is used, the biomass degree of the rubber composition is reduced by the mineral oil-based plasticizer. Therefore, it is required to maintain the biomass degree while suppressing the occurrence of bagging. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2023-30734 A Summary of the Invention [Problem to be solved by the invention]
[0009] An object of the present invention is to provide an EPDM composition using at least a portion of a plant-derived component, which can maintain the biomass degree of the resulting EPDM while suppressing the occurrence of bagging. [Means for solving the problem]
[0010] The object of the present invention is achieved by an EPDM composition comprising 100 parts by weight of plant-derived component-containing ethylene-propylene-diene terpolymer, 1.0 to 12.0 parts by weight of liquid polybutadiene, and 1.0 to 12.0 parts by weight of plant-derived component-containing terpene resin. Effect of the Invention
[0011] The EPDM composition of the present invention is prepared by adding liquid polybutadiene, which has good compatibility with EPDM containing at least a plant-derived component that has a small environmental impact and which enables improved roll processability by reducing the base viscosity, to EPDM, and further using a specific amount of a terpene resin containing a plant-derived component to reduce the biomass degree, which is inevitably reduced by the addition of this liquid polybutadiene, thereby suppressing the occurrence of bagging during roll mixing while maintaining the biomass degree of the obtained EPDM; specifically, this produces the excellent effect of maintaining the rate of change in biomass degree by less than -1.5% compared to a composition to which the liquid polybutadiene and the terpene resin containing a plant-derived component are not added. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] As the EPDM, ethylene and propylene containing at least a part of plant-derived components, specifically 40 to 80% by weight, copolymerized with a small amount of various non-conjugated diene components are used. Here, the plant-derived components include ethylene purified from sugar cane, and as such EPDM, for example, commercially available products such as ARLANXEO's Keltan ECO 6950 (percentage of ethylene purified from sugar cane: 48% by weight), 5470 (percentage of ethylene purified from sugar cane: 70% by weight), and 8550 (percentage of ethylene purified from sugar cane: 55% by weight) can be used as they are.
[0013] The liquid polybutadiene to be blended is one having a 1,2-vinyl content of 25% by weight or more, preferably 28 to 99% by weight. If any other type of plasticizer or one having a lower 1,2-vinyl content is used, the desired molding processability cannot be satisfied. In practice, commercially available products such as the NISSO-PB series manufactured by Nippon Soda and the RICON series manufactured by CRAYVALLEY can be used as is.
[0014] Liquid polybutadiene is used in an amount of 1 to 12 parts by weight, preferably 2 to 10 parts by weight, per 100 parts by weight of EPDM. If the amount of liquid polybutadiene used is greater than this amount, the dough will stick during kneading, causing deterioration in roll processability. On the other hand, if the amount of liquid polybutadiene used is less than this amount, the Mooney viscosity ML 1+4 (125℃) becomes greater than 65, causing bagging to occur.
[0015] From the viewpoint of satisfying a good balance between the tensile strength and the elongation at break in addition to the molding processability judged from the flow volume, it is preferable to use a combination of 10 to 30 parts by weight of liquid polybutadiene having a 1,2-vinyl content of 25 to 35% by weight and 5 to 15 parts by weight of liquid polybutadiene having a 1,2-vinyl content of 90 to 99% by weight.
[0016] Terpene resins containing plant-derived components include terpene resins at least partially containing plant-derived components, such as terpene resins obtained by further refining turpentine oil or orange oil refined from pine or orange peel. Such plant-derived terpene resins include, for example, the commercially available YS Resin series, such as YS Resin 105 (plant-derived components: 70% by weight) manufactured by Yasuhara Chemical, which is blended in a ratio of 1 to 12 parts by weight, preferably 2 to 10 parts by weight, per 100 parts by weight of EPDM. If the plant-derived terpene resin is used in a ratio greater than this, the dough will stick during kneading, causing deterioration in roll processability, while if it is used in a ratio less than this, the Mooney viscosity ML 1+4If the temperature (125°C) exceeds 65, bagging will occur, making it difficult to suppress the decrease in biomass content.
[0017] By using a terpene resin containing plant-derived components, it is possible to compensate for the inevitable decrease in biomass content caused by the addition of liquid polybutadiene, and it is possible to maintain the biomass content of the resulting EPDM while also suppressing the occurrence of bagging during roll mixing.
[0018] The EPDM composition consisting of the above essential components contains an organic peroxide as a crosslinking agent. Examples of organic peroxides that can be used include tertiary butyl peroxide, dicumyl peroxide, tertiary butyl cumyl peroxide, 1,1-di(tertiary butyl peroxy)-3,3,5-trimethylcyclohexane, 2,5-dimethyl-2,5-di(tertiary butyl peroxy)hexane, 2,5-dimethyl-2,5-di(tertiary butyl peroxy)hexyne-3, 1,3-di(tertiary butyl peroxy isopropyl)benzene, 2,5-dimethyl-2,5-di(benzoyl peroxy)hexane, tertiary butyl peroxy benzoate, tertiary butyl peroxy isopropyl carbonate, and n-butyl-4,4-di(tertiary butyl peroxy)valerate.
[0019] These organic peroxides are used in a ratio of about 1 to 8 parts by weight, preferably about 2 to 7 parts by weight, per 100 parts by weight of EPDM. If the blending ratio is less than this, sufficient crosslink density cannot be obtained, and the heat resistance and compression set resistance properties become poor, while if the blending ratio is more than this, foaming occurs and it becomes impossible to obtain a crosslinked molded product.
[0020] In addition to the above-mentioned components, the composition may contain compounding agents generally used in the rubber industry, such as stearic acid, palmitic acid, paraffins, esters, poly-α-olefins, process oils, waxes, and other processing aids, fillers or reinforcing agents such as carbon black and silica, oxides or hydroxides of divalent metals such as zinc oxide and magnesium oxide, acid acceptors such as hydrotalcite, plasticizers other than liquid polybutadiene, and antioxidants, which are added appropriately within the range that does not impair the physical properties.
[0021] The composition is prepared by kneading using an internal kneader or the like, and the crosslinking is carried out by press vulcanization at about 150 to 220°C for about 1 to 20 minutes, and oven vulcanization (secondary vulcanization) at about 120 to 200°C for about 0.1 to 20 hours, which is performed as necessary. EXAMPLES
[0022] The present invention will now be described with reference to examples.
[0023] Example 1 EPDM containing plant-derived ingredients (ARLANXEO product Keltan ECO 6950) 100 parts by weight Carbon black (Tokai Carbon Products Seast S) 55 〃 Liquid polybutadiene (Nippon Soda Product B-3000) 2 Same Terpene resin containing plant-derived ingredients (YS resin 105) 5 Same Zinc oxide (Sakai Chemical Industry Co., Ltd. Zinc oxide type 1) 4 Same Organic peroxide (Japan Oil Products Percumyl D) 3.5 Same The above components were kneaded using a kneader and an open roll, and the kneaded product was crosslinked at 180°C at a crosslinking rate of t90 x 1.5 seconds, and then post-cured at 150°C for 15 hours to obtain a test piece with a thickness of 2 mm.
[0024] Example 2 In Example 1, the amount of liquid polybutadiene was changed to 5 parts by weight, and the amount of terpene resin was changed to 2 parts by weight.
[0025] Example 3 In Example 1, the amount of liquid polybutadiene used was changed to 5 parts by weight.
[0026] Example 4 In Example 1, the amount of liquid polybutadiene was changed to 5 parts by weight, and the amount of terpene resin was changed to 10 parts by weight.
[0027] Example 5 In Example 1, the amount of liquid polybutadiene used was changed to 10 parts by weight.
[0028] Example 6 In Example 1, the amount of liquid polybutadiene was changed to 10 parts by weight, and the amount of terpene resin was changed to 10 parts by weight.
[0029] Comparative Example 1 In Example 1, no liquid polybutadiene and no terpene resin were used.
[0030] Comparative Example 2 In Comparative Example 1, the same amount (100 parts by weight) of EPDM not containing plant-derived components (Keltan 6950, product of ARLANXEO) was used as the EPDM.
[0031] Comparative Example 3 In Comparative Example 1, 10 parts by weight of a plasticizer (Idemitsu Kosan product PW-380) was further used.
[0032] Comparative Example 4 In Comparative Example 2, 10 parts by weight of a plasticizer (Idemitsu Kosan product PW-380) was further used.
[0033] Comparative Example 5 In Example 1, no terpene resin was used.
[0034] Comparative Example 6 In Example 5, no terpene resin was used.
[0035] Comparative Example 7 In Example 1, no liquid polybutadiene was used.
[0036] Comparative Example 8 In Example 4, no liquid polybutadiene was used.
[0037] Comparative Example 9 In Example 1, the amount of liquid polybutadiene was changed to 15 parts by weight.
[0038] Comparative Example 10 In Example 2, the amount of terpene resin was changed to 20 parts by weight.
[0039] For the kneaded products or the obtained test pieces of each of the above Examples and Comparative Examples, the roll processability, Mooney viscosity, biomass ratio and normal physical properties were measured, evaluated and calculated. Roll processability: Using 10-inch open rolls, gap 4 mm, front roll 14 rpm The mixing was carried out under the following conditions: Rating by ○: Roll mixing can be performed without problems ×: Difficult to knead due to bagging *: The dough sticks to the rolls and is difficult to knead. Mooney Viscosity ML 1+4 : JIS K6300 compliant (125℃) Biomass ratio: The percentage of plant-derived components (wt%), calculated using the following formula: {Weight of plant-derived component in EPDM composition (g) / EPDM composition weight (g)}×100 Normal state physical properties: Compliant with JIS K6253 and 6251
[0040] The results obtained are shown in the following Tables 1-2. Table 1 Measurement and evaluation items Fruit 1 Fruit 2 Fruit 3 Real 4 Real 5 Fruit 6 Roll processability ○ ○ ○ ○ ○ ○ Mooney Viscosity ML 1+4 63 56 55 55 45 43 Biomass content (wt%) 30.4 29.1 29.8 31.0 29.2 30.1 Hardness (JIS A) 69 71 70 64 71 66 Tensile strength Ts (MPa) 17.0 16.7 16.5 15.7 15.4 17.0 Elongation at break Eb(%) 210 170 200 250 170 200 Table 2 Measurement and evaluation items ratio 1 ratio 2 ratio 3 ratio 4 ratio 5 ratio 6 ratio 7 ratio 8 ratio 9 ratio 10 Roll processability × × ○ ○ × ○ × × * * Mooney Viscosity ML 1+4 78 78 57 57 66 50 69 67 32 48 Biomass content (wt%) 29.5 0 27.8 0 29.2 27.8 30.7 31.9 28.2 33.1 Hardness (JIS A) 70 70 67 66 72 76 68 64 74 60 Tensile strength Ts (MPa) 12.8 11.5 16.9 17.0 12.8 14.5 15.9 15.2 15.7 17.3 Elongation at break Eb(%) 140 140 240 220 140 100 210 260 100 360
[0041] From the above, the following can be said: (1) The EPDM compositions obtained in the respective examples have good processability during kneading, and the biomass content of the resulting EPDM is maintained while suppressing the occurrence of bagging. (2) If liquid polybutadiene and / or terpene resins are not used, the Mooney viscosity ML 1+4 (125°C) becomes greater than 65, causing bagging (Comparative Examples 1 to 2, 5, and 7 to 8). (3) Even if liquid polybutadiene and terpene resins are not used, the Mooney viscosity ML can be increased by adding a plasticizer. 1+4 (125°C) can be set to 65 or less, the occurrence of bagging can be suppressed, and roll processability is also good, but a decrease in the biomass content cannot be avoided (Comparative Example 3). (4) If a terpene resin is not used, a decrease in the biomass ratio cannot be avoided (Comparative Example 6). (5) Even if terpene resin containing plant-derived components is used, the Mooney viscosity ML is low unless liquid polybutadiene is used. 1+4 (125°C) becomes greater than 65, causing bagging (Comparative Examples 1-2, 5, 7-8). (6) Even when liquid polybutadiene or terpene resin containing plant-derived components is used, if it is used in a ratio exceeding the specified amount, the dough sticks during kneading, causing deterioration in roll processability (Comparative Examples 9 to 10).
Claims
1. An EPDM composition comprising 100 parts by weight of ethylene-propylene-diene terpolymer containing plant-derived components, 1.0 to 12.0 parts by weight of liquid polybutadiene, and 1.0 to 12.0 parts by weight of terpene resin containing plant-derived components.
2. 2. The EPDM composition according to claim 1, which has a change in biomass ratio of less than -1.5% compared to a composition to which the liquid polybutadiene portion and the terpene resin containing a plant-derived component are not added.
3. Mooney Viscosity ML 1+4 The EPDM composition according to claim 1, wherein the (125°C) is 65 or less.
4. A vulcanized molded article made from the EPDM composition according to claim 1.
5. 5. The vulcanization molded article according to claim 4, which is a sealing material or a vibration-isolating rubber.