Inkjet ink

The inkjet ink with crosslinked resin-coated pigment particles addresses the challenge of achieving desired image density and preventing nozzle clogging by stabilizing pigment dispersion, ensuring effective ink flow and image quality.

JP2024162743APending Publication Date: 2024-11-21KYOCERA DOCUMENT SOLUTIONS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023078601
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing inkjet inks struggle to form images with desired image density while effectively suppressing nozzle clogging in inkjet recording apparatuses.

Method used

An inkjet ink containing pigment particles dispersed in an aqueous medium, where the pigment particles are coated with a crosslinked resin made from a specific copolymer and crosslinking agent, optimizing the composition and properties of the resin to enhance dispersion stability and hydrophilicity, thereby preventing nozzle clogging while maintaining image density.

Benefits of technology

The ink achieves desired image density while significantly reducing nozzle clogging, thanks to the optimized crosslinked resin structure that stabilizes pigment particles and maintains ink flow efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide an inkjet ink capable of forming an image having a desired image density while suppressing the occurrence of nozzle clogging.SOLUTION: There is provided an inkjet ink containing an aqueous medium and pigment particles dispersed in the aqueous medium. The pigment particles contain a pigment and a cross-linked resin. The cross-linked resin is a cross-linked product of a specific resin and a specific crosslinking agent. The specific resin is a neutralized product of a specific copolymer having a first repeating unit derived from α-methylstyrene, a second repeating unit derived from styrene, a third repeating unit derived from (meth)acrylic acid and a fourth repeating unit derived from alkylene glycol (meth)acrylate or dialkylene glycol(meth)acrylate. The specific crosslinking agent contains a multifunctional epoxy compound having two or more epoxy groups and one or more hydroxy groups in the molecule.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to ink-jet inks. [Background technology]

[0002] Inkjet recording devices may use aqueous inkjet inks containing a pigment and an aqueous medium. Inkjet inks are required to be able to suppress nozzle clogging in the recording head of the inkjet recording device and to impart a desired image density to the formed image. In response to such requirements, for example, inkjet inks have been proposed that include an aqueous pigment dispersion that contains an azomethine metal complex pigment and a polymer dispersant (Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-116600 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, even with the inkjet ink described in Patent Document 1, it is not possible to reliably form an image having a desired image density while sufficiently suppressing the occurrence of nozzle clogging.

[0005] The present invention has been made in view of the above problems, and an object of the present invention is to provide an inkjet ink that can form an image having a desired image density while suppressing the occurrence of nozzle clogging. [Means for solving the problem]

[0006] The inkjet ink according to the present invention contains an aqueous medium and pigment particles dispersed in the aqueous medium. The pigment particles contain a pigment and a crosslinked resin. The crosslinked resin is a crosslinked product of a specific resin and a specific crosslinking agent. The specific resin is a neutralized product of a specific copolymer having a first repeating unit derived from α-methylstyrene, a second repeating unit derived from styrene, a third repeating unit derived from (meth)acrylic acid, and a fourth repeating unit derived from an alkylene glycol (meth)acrylate or a dialkylene glycol (meth)acrylate. With respect to 100% by mass of all repeating units contained in the specific copolymer, the content ratio of the first repeating unit is 1% by mass or more and 65% by mass or less, the content ratio of the second repeating unit is 1% by mass or more and 60% by mass or less, the content ratio of the third repeating unit is 10% by mass or more and 40% by mass or less, and the content ratio of the fourth repeating unit is 1% by mass or more and 12% by mass or less. The acid value of the specific copolymer is 50 mgKOH / g or more and 300 mgKOH / g or less. The number average molecular weight of the specific copolymer is 3000 or more and 18000 or less. The neutralization rate of the specific resin is 20% or more and 100% or less. The specific crosslinking agent includes a polyfunctional epoxy compound having two or more epoxy groups and one or more hydroxyl groups in the molecule. The water solubility rate of the specific crosslinking agent is 80% or more. The crosslinking rate of the crosslinked resin is 25% or more and 90% or less. Effect of the Invention

[0007] The inkjet ink according to the present invention can form an image having a desired image density while suppressing the occurrence of nozzle clogging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, an embodiment of the present invention will be described. In the following, the volume median diameter (D 50 ) is a value measured using a dynamic light scattering particle size distribution analyzer ("Zetasizer Nano ZS" manufactured by Malvern Instruments, unless otherwise specified.

[0009] In this specification, the acid value can be determined according to the method described in JIS (Japanese Industrial Standards) K0070:1992.

[0010] The number average molecular weight (Mn) measurements, unless otherwise specified, are those determined using gel permeation chromatography.

[0011] In this specification, acrylic and methacrylic may be collectively referred to as "(meth)acrylic". In this specification, acrylate and methacrylate may be collectively referred to as "(meth)acrylate". Each component described in this specification may be used alone or in combination of two or more.

[0012] <Inkjet ink> Hereinafter, an inkjet ink (hereinafter, sometimes simply referred to as ink) according to an embodiment of the present invention will be described. The ink of this embodiment contains an aqueous medium and pigment particles dispersed in the aqueous medium. The pigment particles include a pigment and a crosslinked resin. The crosslinked resin is a crosslinked product of a specific resin and a specific crosslinking agent. The specific resin is a neutralized product of a specific copolymer having a first repeating unit derived from α-methylstyrene, a second repeating unit derived from styrene, a third repeating unit derived from (meth)acrylic acid, and a fourth repeating unit derived from an alkylene glycol (meth)acrylate or a dialkylene glycol (meth)acrylate. With respect to 100% by mass of all repeating units contained in the specific copolymer, the content ratio of the first repeating unit is 1% by mass or more and 65% by mass or less, the content ratio of the second repeating unit is 1% by mass or more and 60% by mass or less, the content ratio of the third repeating unit is 10% by mass or more and 40% by mass or less, and the content ratio of the fourth repeating unit is 1% by mass or more and 12% by mass or less. The acid value of the specific copolymer is 50 mgKOH / g or more and 300 mgKOH / g or less. The number average molecular weight of the specific copolymer is 3000 or more and 18000 or less. The neutralization rate of the specific resin is 20% or more and 100% or less. The specific crosslinking agent includes a multifunctional epoxy compound having two or more epoxy groups and one or more hydroxyl groups in the molecule. The water solubility rate of the specific crosslinking agent is 80% or more. The crosslinking rate of the crosslinked resin is 25% or more and 90% or less.

[0013] In this specification, the crosslinking rate refers to the ratio of the number of functional groups forming a crosslinked structure in the crosslinked resin when the total number of functional groups (groups capable of reacting with the specific crosslinking agent) contained in the raw material of the crosslinked resin (specific resin) is taken as 100%. The specific crosslinking agent used in the ink of this embodiment mainly reacts with acid groups (particularly -COOH). Therefore, the "total number of functional groups contained in the raw material of the crosslinked resin" corresponds to the total number of acid groups contained in the specific resin. The crosslinking rate can be calculated, for example, by applying the number of moles X of the crosslinked functional groups (epoxy groups) contained in the specific crosslinking agent and the number of moles Y of the carboxyl groups contained in the specific resin to the following formula. Crosslinking rate [%] = 100 × number of moles of crosslinking functional groups X / number of moles of carboxyl groups Y

[0014] The number of moles X of the crosslinking functional group of the specific crosslinking agent is calculated, for example, by dividing the amount [g] of the specific crosslinking agent used by the epoxy equivalent [g / eq.] of the crosslinking agent. The number of moles Y of the carboxyl group contained in the specific resin is calculated by multiplying the amount of the specific resin used by the number of moles of the carboxyl group per gram of the specific resin. The number of moles of the carboxyl group per gram of the specific resin is calculated by dividing the acid value of the specific copolymer that is the raw material of the specific resin by the molecular weight of KOH (56.1).

[0015] The application of the ink of the present embodiment is not particularly limited, and can be used, for example, for forming an image on a permeable recording medium or a non-permeable recording medium. The ink of the present embodiment is suitable for forming an image on a permeable recording medium. Permeable recording media have excellent ink permeability. Examples of permeable recording media include printing paper and media made of fibers (e.g., fabric). Examples of printing paper include plain paper, copy paper, recycled paper, thin paper, thick paper, and glossy paper.

[0016] The ink of the present embodiment, having the above-mentioned configuration, can form an image having a desired image density while suppressing the occurrence of nozzle clogging. The reason for this is presumed to be as follows. In known inks, imparting high dispersion stability to the pigment particles is effective in suppressing the occurrence of nozzle clogging. However, known inks having pigment particles with high dispersion stability tend to form images with low image density. This is because, when known inks containing pigment particles with high dispersion stability are dropped onto a recording medium, the pigment particles penetrate deep into the recording medium together with the aqueous medium. Thus, in known inks, it is difficult to achieve both the suppression of nozzle clogging and the image density of the formed image.

[0017] In contrast, the pigment particles contained in the ink of this embodiment include a pigment and a crosslinked resin. The crosslinked resin is a crosslinked product of a specific resin and a specific crosslinking agent. The specific resin is a neutralized product of a specific copolymer. Here, the crosslinked resin has a relatively large number of acid groups because the acid value of the specific copolymer, which is the raw material, is relatively high. In addition, the acid groups of the crosslinked resin are moderately neutralized. The acid groups (especially neutralized acid groups) are highly hydrophilic. Therefore, the crosslinked resin has a moderately high hydrophilicity. In addition, the specific crosslinking agent has a hydroxy group and a high water solubility, so that it has a relatively high hydrophilicity. Furthermore, the specific crosslinking agent has an epoxy group, which is a crosslinkable group with excellent reactivity, so that it can efficiently form a crosslinked structure with the specific resin. The crosslinked resin is a crosslinked product of a specific resin with a moderately high hydrophilicity and a specific crosslinking agent, so that it has a moderately high hydrophilicity. Furthermore, the crosslinked resin can efficiently cover the pigment particles because the molecular size of the specific copolymer, which is the raw material, is appropriate. Furthermore, the crosslinked resin has a crosslinked structure, so that it is difficult to detach from the pigment particles. By including such a crosslinked resin, the pigment particles can be stably dispersed in an aqueous medium, and as a result, the pigment particles have suitably excellent dispersion stability.

[0018] The specific copolymer, which is the raw material of the crosslinked resin, has the first repeating unit to the fourth repeating unit in a predetermined content ratio. The first repeating unit derived from α-methylstyrene moderately increases the affinity between the crosslinked resin and the pigment particles. The second repeating unit derived from styrene imparts moderate hydrophobicity to the crosslinked resin and adjusts the dispersion stability of the pigment particles. The third repeating unit derived from (meth)acrylic acid and the fourth repeating unit derived from alkylene glycol (meth)acrylate or dialkylene glycol (meth)acrylate impart moderate hydrophilicity to the crosslinked resin and impart dispersion stability to the pigment particles. As a result, the dispersion stability of the pigment particles is optimized. Therefore, the ink of this embodiment can form an image having a desired image density while suppressing the occurrence of nozzle clogging.

[0019] The ink of this embodiment will be described in more detail below. Each of the components described below may be used alone or in combination of two or more.

[0020] [Solid content in the supernatant] Among the crosslinked resins contained in the ink of this embodiment, some of the crosslinked resins may be detached from the pigment particles during the production or storage of the ink of this embodiment and may be free in the aqueous medium. Such crosslinked resins free in the aqueous medium are referred to as free resins. The solid content contained in the supernatant obtained by centrifuging the ink of this embodiment at 1,050,000 G for 3 hours can be regarded as free resin. The free resin has a function of improving the abrasion resistance of the image formed by the ink of this embodiment, but if the amount is large, it may cause nozzle clogging. Therefore, in the ink of this embodiment, it is preferable that the content ratio of free resin is low. However, in the ink of this embodiment, free resin is inevitably generated and it is difficult to completely remove it.

[0021] From the above, in the ink of this embodiment, the solid content in the supernatant obtained by centrifuging at 1,050,000G for 3 hours is preferably 2.0% by mass or less, more preferably 0.1% by mass to 1.5% by mass or less, and even more preferably 0.5% by mass to 1.0% by mass or less. By making the solid content in the above-mentioned supernatant 2.0% by mass or less, the ink of this embodiment can more effectively suppress the occurrence of nozzle clogging. The above-mentioned solid content can be measured by the method described in the examples or a method based thereon.

[0022] [Pigment particles] The pigment particles contain a pigment and a crosslinked resin. The pigment particles are composed of, for example, a core containing a pigment and a crosslinked resin that coats the core. The total content of the pigment and the crosslinked resin in the pigment particles is preferably 90% by mass or more, and more preferably 100% by mass.

[0023] From the viewpoint of optimizing the color density, hue, or stability of the ink of this embodiment, the volume median diameter of the pigment particles is preferably 30 nm or more and 200 nm or less, and more preferably 80 nm or more and 130 nm or less.

[0024] In the ink of this embodiment, the content of pigment particles is preferably 6.0% by mass or more and 20.0% by mass or less, and more preferably 10.0% by mass or more and 15.0% by mass or less. By making the content of pigment particles 5.0% by mass or more, the ink of this embodiment can more easily form an image having a desired image density. In addition, by making the content of pigment particles 20.0% by mass or less, the fluidity of the ink of this embodiment can be optimized.

[0025] (Pigments) Examples of pigments include yellow pigments, orange pigments, red pigments, blue pigments, purple pigments, and black pigments. Examples of yellow pigments include CI Pigment Yellow (74, 93, 95, 109, 110, 120, 128, 138, 139, 151, 154, 155, 173, 180, 185, and 193). Examples of orange pigments include CI Pigment Orange (34, 36, 43, 61, 63, and 71). Examples of red pigments include CI Pigment Red (122 and 202). Examples of blue pigments include CI Pigment Blue (15, more specifically 15:3). Examples of purple pigments include CI Pigment Violet (19, 23, and 33). Examples of black pigments include CI Pigment Black (7).

[0026] In the ink of this embodiment, the pigment content is preferably 3.0 parts by mass to 15.0 parts by mass, and more preferably 7.0 parts by mass to 12.0 parts by mass. The pigment content in the pigment particles is preferably 45% by mass to 80% by mass, and more preferably 55% by mass to 70% by mass.

[0027] (Crosslinked resin) The crosslinked resin, for example, coats the pigment in the pigment particles. The crosslinked resin is a crosslinked product of a specific resin and a specific crosslinking agent. The crosslinking rate of the crosslinked resin is 25% or more and 90% or less, preferably 35% or more and 65% or less, and more preferably 35% or more and 45% or less. By setting the crosslinking rate of the crosslinked resin to 25% or more, it is possible to suppress the crosslinked resin from being detached from the pigment particles. By setting the crosslinking rate of the crosslinked resin to 90% or less, it is possible to optimize the dispersion stability of the pigment particles. The crosslinking rate of the crosslinked resin can be calculated by the method described in the Examples or a method based thereon.

[0028] In the ink of this embodiment, the content of the crosslinked resin is preferably 0.5% by mass or more and 10.0% by mass or less, and more preferably 2.0% by mass or more and 4.5% by mass or less. By making the content of the crosslinked resin 0.5% by mass or more, the dispersion stability of the pigment particles can be further optimized. By making the content of the crosslinked resin 10.0% by mass or more, the generation of free resin can be suppressed.

[0029] In the pigment particles, the content of the crosslinked resin relative to 100 parts by mass of the pigment is preferably from 25 to 60 parts by mass, and more preferably from 30 to 45 parts by mass. By setting the content of the crosslinked resin relative to 100 parts by mass of the pigment to be from 25 to 60 parts by mass, the dispersion stability of the pigment particles can be further optimized.

[0030] (Specific resin) The specific resin is a neutralized product of a specific copolymer. The neutralization rate of the specific resin is 20% or more and 100% or less, preferably 40% or more and 95% or less, and more preferably 50% or more and 70% or less. By setting the neutralization rate of the specific resin to 20% or more and 100% or less, it is possible to impart an appropriately high hydrophilicity to the crosslinked resin and optimize the dispersion stability of the pigment particles.

[0031] The specific resin preferably contains an alkali metal atom. That is, the specific resin is preferably a neutralized product obtained by neutralizing a specific copolymer with a neutralizing agent containing an alkali metal atom. The alkali metal atom does not volatilize from the ink of the present embodiment even when the ink of the present embodiment is exposed to a dry state. Therefore, by neutralizing the specific copolymer with a neutralizing agent containing an alkali metal atom, the neutralized state (hydrophilicity) of the crosslinked resin is maintained even when the ink of the present embodiment is exposed to a dry state. The alkali metal atom is preferably a potassium atom or a sodium atom. The neutralizing agent is preferably a hydroxide containing an alkali metal atom, and more preferably NaOH or KOH.

[0032] (Specific copolymer) The number average molecular weight of the specific copolymer is preferably from 3000 to 18000, more preferably from 5000 to 12000, and even more preferably from 8000 to 10000. By setting the number average molecular weight of the specific resin to be from 3000 to 18000, the crosslinked resin can efficiently cover the pigment particles. This makes it possible to suppress the crosslinked resin from being detached from the pigment particles.

[0033] The acid value of the specific copolymer is 50 mgKOH / g or more and 300 mgKOH / g or less, preferably 100 mgKOH / g or more and 200 mgKOH / g or less, and more preferably 150 mgKOH / g or more and 200 mgKOH / g or less. By setting the acid value of the specific copolymer to 50 mgKOH / g or more and 300 mgKOH / g or less, it becomes easy to sufficiently introduce a crosslinked structure into the crosslinked resin, and the dispersion stability of the pigment particles can be optimized. By setting the acid value of the specific copolymer to 300 mgKOH / g or less, it is possible to prevent the dispersion stability of the pigment particles from becoming excessively high. As a result, the desired image density can be imparted to the image formed by the ink of this embodiment.

[0034] The specific copolymer has a first repeating unit derived from α-methylstyrene, a second repeating unit derived from styrene, a third repeating unit derived from (meth)acrylic acid, and a fourth repeating unit derived from an alkylene glycol (meth)acrylate or a dialkylene glycol (meth)acrylate.

[0035] Examples of the alkylene glycol (meth)acrylate include ethylene glycol (meth)acrylate, propylene glycol (meth)acrylate, and butylene glycol (meth)acrylate, with ethylene glycol (meth)acrylate being preferred.

[0036] Examples of dialkylene glycol (meth)acrylates include diethylene glycol (meth)acrylate, dipropylene glycol (meth)acrylate, and dibutylene glycol (meth)acrylate, with dipropylene glycol (meth)acrylate being preferred.

[0037] The content of the first repeating unit derived from α-methylstyrene is from 1 to 65% by mass, preferably from 15 to 55% by mass, more preferably from 25 to 50% by mass, and even more preferably from 40 to 48% by mass, relative to 100% by mass of all repeating units in the specific copolymer. By setting the content of the first repeating unit to be from 1 to 65% by mass, the dispersion stability of the pigment particles can be further optimized.

[0038] The content of the second repeating unit derived from styrene is from 1 to 60% by mass, preferably from 10 to 40% by mass, and more preferably from 15 to 27% by mass, relative to 100% by mass of all repeating units in the specific copolymer. By setting the content of the second repeating unit to be from 1 to 60% by mass, the dispersion stability of the pigment particles can be further optimized.

[0039] The content of the third repeating unit derived from (meth)acrylic acid is from 10 to 40% by mass, preferably from 20 to 35% by mass, and more preferably from 25 to 32% by mass, based on 100% by mass of all repeating units in the specific copolymer. By setting the content of the third repeating unit to be from 10 to 40% by mass, the dispersion stability of the pigment particles can be further optimized.

[0040] The content of the fourth repeating unit derived from an alkylene glycol (meth)acrylate or a dialkylene glycol (meth)acrylate is from 1 to 12% by mass, preferably from 4 to 11% by mass, and more preferably from 4 to 8% by mass, based on 100% by mass of all repeating units in the specific copolymer. By setting the content of the fourth repeating unit to be from 1 to 12% by mass, the dispersion stability of the pigment particles can be further optimized.

[0041] It is preferable that, relative to 100% by mass of all repeating units in the specific copolymer, the content of the first repeating unit is from 15% by mass to 55% by mass, the content of the second repeating unit is from 10% by mass to 40% by mass, the content of the third repeating unit is from 20% by mass to 35% by mass, and the content of the fourth repeating unit is from 4% by mass to 11% by mass.

[0042] The specific copolymer may be a random polymer or a block polymer, and is preferably a random polymer.

[0043] The composition of the monomers that are the raw materials for the specific copolymer is preferably any one of compositions 1 to 3 shown in Table 1 below. In Table 1 below, the numerical values ​​indicate the numerical range of the preferable content ratio [mass %]. For example, "18-22" for styrene in composition 1 indicates that styrene is contained in an amount of 18 mass % or more and 22 mass % or less.

[0044] [Table 1]

[0045] (Specific cross-linking agent) The specific crosslinking agent includes a polyfunctional epoxy compound having two or more epoxy groups and one or more hydroxyl groups in the molecule (hereinafter, may be referred to as a polyfunctional epoxy compound (X)). The water solubility of the specific crosslinking agent is 80% or more, preferably 90% or more, and more preferably 98% or more. By making the water solubility of the specific crosslinking agent 80% or more, the dispersion stability of the pigment particles can be optimized. The water solubility of the specific crosslinking agent is the ratio (100×A / 10g) of the mass A of the specific crosslinking agent dissolved in water to the total amount (10g) of the specific crosslinking agent when 10g of the specific crosslinking agent and 90g of water are mixed at 25°C. For example, when 10g of the specific crosslinking agent and 90g of water are mixed at 25°C, if 9g of the specific crosslinking agent is dissolved in water and 1g of the specific crosslinking agent is precipitated without dissolving in water (mass A: 9g), the water solubility is 90%.

[0046] In the polyfunctional epoxy compound (X), the number of epoxy groups in the molecule is preferably from 2 to 8, and more preferably from 2 to 5. In the polyfunctional epoxy compound (X), the number of hydroxyl groups in the molecule is preferably from 1 to 5, and more preferably from 1 to 3.

[0047] The polyfunctional epoxy compound (X) is preferably glycerol polyglycidyl ether, polyglycerol polyglycidyl ether (particularly, diglycerol polyglycidyl ether or triglycerol polyglycidyl ether) or sorbitol polyglycidyl ether, and more preferably glycerol polyglycidyl ether, diglycerol polyglycidyl ether or triglycerol polyglycidyl ether.

[0048] The specific crosslinking agent may further contain other polyfunctional epoxy compounds in addition to the polyfunctional epoxy compound (X). As the other polyfunctional epoxy compound, a compound represented by the following chemical formula (2) (glycerol triglycidyl ether) is preferable. In the specific crosslinking agent, the total content of the polyfunctional epoxy compound (X) and glycerol triglycidyl ether is preferably 80 mass% or more, more preferably 95 mass% or more, and even more preferably 100 mass%.

[0049] Examples of the polyfunctional epoxy compound (X) include compounds represented by the following chemical formulas (1), (3), (4) and (5). The specific crosslinking agent is preferably a mixture of a compound represented by the following chemical formula (1) and a compound represented by the following chemical formula (2), a compound represented by the following chemical formula (3), a compound represented by the following chemical formula (4) or a compound represented by the following chemical formula (5).

[0050] [ka]

[0051] The epoxy equivalent of the specific crosslinking agent is preferably 100 g / eq. or more and 250 g / eq. or less, more preferably 130 g / eq. or more and 200 g / eq. or less, and even more preferably 130 g / eq. or more and 170 g / eq. or less. The epoxy equivalent can be determined, for example, according to the method described in JIS (Japanese Industrial Standards) K7236:2009.

[0052] [Aqueous medium] The aqueous medium contained in the ink of this embodiment is a medium containing water. The aqueous medium may function as a solvent or as a dispersion medium. Specific examples of the aqueous medium include aqueous media containing water and a water-soluble organic solvent.

[0053] (water) In the ink of this embodiment, the water content is preferably from 25.0% to 80.0% by mass, and more preferably from 35.0% to 60.0% by mass.

[0054] (Water-soluble organic solvent) Examples of the water-soluble organic solvent include glycol compounds, triol compounds, glycol ether compounds, lactam compounds, nitrogen-containing compounds, acetate compounds, thiodiglycol, and dimethylsulfoxide.

[0055] Examples of the glycol compound include ethylene glycol, 1,3-propanediol, propylene glycol, 1,2-pentanediol, 1,5-pentanediol, 1,2-octanediol, 1,8-octanediol, 3-methyl-1,3-butanediol, 3-methyl-1,5-pentanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, and 2-ethyl-1,2-hexanediol. Examples of the glycol compound include ethylene glycol, diethylene glycol, 2-ethyl-1,2-hexanediol, 3-methyl-1,5-pentanediol, 1,3-propanediol, 1,5-pentanediol, and propylene glycol.

[0056] Triol compounds include, for example, glycerin and 1,2,3-butanetriol.

[0057] Examples of glycol ether compounds include diethyl diglycol, diethylene glycol monobutyl ether, ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether (diethyl diglycol), triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monobutyl ether and propylene glycol monomethyl ether. As the glycol ether compound, triethylene glycol monobutyl ether is preferred.

[0058] Examples of lactam compounds include 2-pyrrolidone and N-methyl-2-pyrrolidone. Of the lactam compounds, 2-pyrrolidone is preferred.

[0059] Examples of nitrogen-containing compounds include 1,3-dimethylimidazolidinone, formamide, and dimethylformamide.

[0060] An example of the acetate compound is diethylene glycol monoethyl ether acetate.

[0061] The water-soluble organic solvent is preferably a glycol compound or a glycol ether compound, and more preferably ethylene glycol or diethyl diglycol.

[0062] The content of the water-soluble organic solvent in the ink of this embodiment is preferably from 10.0% to 50.0% by mass, and more preferably from 30.0% to 40.0% by mass.

[0063] The content of the glycol compound in the ink of this embodiment is preferably from 5.0% by mass to 45.0% by mass, and more preferably from 15.0% by mass to 25.0% by mass.

[0064] The content of the glycol ether compound in the ink of this embodiment is preferably from 5.0% by mass to 30.0% by mass, and more preferably from 10.0% by mass to 20.0% by mass.

[0065] [Surfactants] The ink of the present embodiment preferably further contains a surfactant. The surfactant can optimize the permeability (wettability) of the ink of the present embodiment to the recording medium. Examples of the surfactant include anionic surfactants, cationic surfactants, and nonionic surfactants. The surfactant is preferably a nonionic surfactant.

[0066] Examples of the nonionic surfactant include polyoxyethylene dodecyl ether, polyoxyethylene hexadecyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene sorbitan monooleate ether, monodecanoyl sucrose, and ethylene oxide adducts of acetylene glycol. As the nonionic surfactant, ethylene oxide adducts of acetylene glycol are preferred.

[0067] The content of the surfactant in the ink of this embodiment is preferably from 0.05% by mass to 3.0% by mass, and more preferably from 0.1% by mass to 0.5% by mass.

[0068] [Other ingredients] The ink of this embodiment may further contain known additives (for example, a dissolution stabilizer, a drying inhibitor, an antioxidant, a viscosity adjuster, a pH adjuster, and an anti-mold agent) as necessary.

[0069] [Ink manufacturing method] Next, an example of a method for producing the ink of this embodiment will be described. The ink production method includes, for example, a neutralization process for preparing a specific resin by neutralizing a specific copolymer, a dispersion process for preparing a pigment particle dispersion by dispersing a pigment and a specific resin in water, a crosslinking process for adding a specific crosslinking agent to the pigment particle dispersion, and an addition process for preparing an ink by adding an aqueous medium to the pigment particle dispersion after the crosslinking process. The ink production method of this embodiment preferably further includes a centrifugation process for centrifuging the pigment particle dispersion after the crosslinking process and then replacing the supernatant with an aqueous medium.

[0070] (Neutralization process) In this step, the specific resin is prepared by neutralizing the specific copolymer. For example, the specific copolymer may be mixed with a neutralizing agent (e.g., an aqueous alkali solution).

[0071] (Pigment processing process) In this step, the pigment and the specific resin are dispersed in water to prepare a pigment particle dispersion. Examples of the dispersion device used for the dispersion treatment include a wet dispersion device such as a media type disperser.

[0072] In this process, the content of the specific resin in the solution to be subjected to the dispersion treatment is, for example, 5.0% by mass or more and 25.0% by mass or less. The content of the pigment in the solution to be subjected to the dispersion treatment is, for example, 1.0% by mass or more and 10.0% by mass or less. In this process, it is preferable that the solution to be subjected to the dispersion treatment further contains an antifoaming agent. The content of the antifoaming agent in the solution to be subjected to the dispersion treatment is, for example, 0.01% by mass or more and 0.1% by mass or less.

[0073] In this step, it is preferable to remove coarse particles from the obtained pigment particle dispersion by filtering using a filter (for example, with a pore size of 5 μm).

[0074] (Crosslinking process) In this process, a specific crosslinking agent is added to the pigment particle dispersion. This causes a reaction between the specific resin contained in the pigment particle dispersion and the specific crosslinking agent, and the specific resin is crosslinked. As a result, a crosslinked resin is generated as a reaction product of the specific crosslinking agent and the specific resin. In this process, after the addition of the specific crosslinking agent, it is preferable to heat the pigment particle dispersion while stirring. The heating temperature can be, for example, 70°C or higher and 95°C or lower. The heating time can be, for example, 2 minutes or higher and 6 hours or lower.

[0075] (Centrifugation process) In this step, the pigment particle dispersion liquid after the crosslinking step is centrifuged, and the supernatant liquid is replaced with an aqueous medium. This makes it possible to remove free components contained in the aqueous medium of the pigment particle dispersion liquid. The centrifugation conditions can be, for example, a rotation speed of 10,000 rpm or more and 100,000 rpm or less, and a centrifugation time of 12 hours or more and 48 hours or less.

[0076] (addition process) In this step, an aqueous medium is added to the pigment particle dispersion after the crosslinking step (if a centrifugation step is performed, the pigment particle dispersion after the centrifugation step). This allows the ink to be obtained. In this step, other components (more specifically, at least one of a surfactant, a dissolution stabilizer, a moisturizer, a penetrating agent, and a viscosity modifier) ​​may be further added as necessary. In this step, after the addition of the aqueous medium, it is preferable to stir the resulting mixture with a stirrer. The resulting ink may be filtered (e.g., a filter with a pore size of 5 μm or less) to remove foreign matter and coarse particles. EXAMPLES

[0077] Examples of the present invention will be described below, but the present invention is not limited to the following examples.

[0078] In the examples, the crosslinking rate of the crosslinking resin was calculated by the following method. First, the number of moles X of the crosslinking functional group (epoxy group) contained in the crosslinking agent was calculated. The number of moles X of the crosslinking functional group of the crosslinking agent was calculated by dividing the amount [g] of the crosslinking agent used by the epoxy equivalent [g / eq.] of the crosslinking agent. Next, the number of moles Y of the carboxy group contained in the specific resin was calculated. The number of moles Y of the carboxy group contained in the specific resin was calculated by integrating the amount of the specific resin used and the number of moles of the carboxy group per 1 g of the specific resin. The number of moles of the carboxy group per 1 g of the specific resin was calculated by dividing the acid value of the specific resin by the molecular weight (56.1) of KOH. Next, the crosslinking rate of the crosslinking resin was calculated by applying the value obtained above to the following formula. Crosslinking rate [%] = 100 × number of moles of crosslinking functional groups X / number of moles of carboxyl groups Y

[0079] [Preparation of Resin (R-1)] In a four-neck flask equipped with a stirrer, a nitrogen inlet tube, a condenser, and a dropping funnel, 100.0 parts by mass of isopropyl alcohol and 250.0 parts by mass of methyl ethyl ketone were added. Separately, 20.0 parts by mass of styrene, 40.0 parts by mass of α-methylstyrene, 5.0 parts by mass of ethylene glycol acrylate, 25.0 parts by mass of methacrylic acid, and 0.3 parts by mass of azobisisobutyronitrile (AIBN, polymerization initiator) were mixed to prepare a monomer solution. In addition, 150.0 parts by mass of methyl ethyl ketone and 0.1 parts by mass of AIBN were mixed to prepare a methyl ethyl ketone solution.

[0080] Next, nitrogen gas was introduced into the four-neck flask to create a nitrogen atmosphere. Next, while the contents of the four-neck flask were heated to reflux at 70°C, the entire amount of the monomer solution was supplied to the four-neck flask over 2 hours using a dropping funnel. After the monomer solution was supplied, the contents of the four-neck flask were heated to reflux at 70°C for another 6 hours. Next, while the contents of the four-neck flask were heated to reflux at 70°C, the entire amount of the methyl ethyl ketone solution was supplied to the four-neck flask over 15 minutes using a dropping funnel. After the methyl ethyl ketone solution was supplied, the contents of the four-neck flask were heated to reflux at 70°C for another 5 hours. This resulted in a resin aqueous solution containing the specific copolymer resin (R-1). Resin (R-1) was isolated by distilling off methyl ethyl ketone and isopropyl alcohol from the resin aqueous solution.

[0081] (Acid value measurement) The acid value of the resin (R-1) was measured according to the method described in JIS (Japanese Industrial Standards) K0070:1992 (Testing methods for acid value, saponification value, ester value, iodine value, hydroxyl value and unsaponifiable matter of chemical products). The measurement results are shown in Tables 3 and 4 below.

[0082] (Measurement of number average molecular weight) The number average molecular weight of the resin (R-1) was measured by gel permeation chromatography (GPC) under the following conditions. The measurement results are shown in Tables 3 and 4 below.

[0083] (GPC conditions) Measuring device: Tosoh Corporation "HLC-8020GPC" Column: Ultra-high performance semi-micro SEC column ("TSKgel SuperMultipore HZ-H" manufactured by Tosoh Corporation, packing material: styrene-divinylbenzene resin, column size: inner diameter 4.6 mm x length 15 cm, packing material particle size: 6 μm) Number of columns: 3 Eluent: Tetrahydrofuran Eluent flow rate: 0.35mL / min Amount of sample solution: 10μL Column temperature: 40℃ Detector: RI (refractive index) detector Calibration curve: A calibration curve created using monodisperse polystyrene standard samples (F-40, F-20, F-4, F-1, A-5000, A-2500 and A-1000) manufactured by Tosoh Corporation and n-propylbenzene.

[0084] [Preparation of Resins (R-2) to (R-14)] Resins (R-2) to (R-14) were prepared in the same manner as in the preparation of resin (R-14), except that in the preparation of the monomer solutions, the types and amounts of monomers used were changed as shown in Table 3 below. In Table 3 below, "EG acrylate" refers to ethylene glycol acrylate. "DPGA" refers to dipropylene glycol acrylate.

[0085] (Preparation of resin aqueous solutions (r-1) to (r-14)) Resins (specifically, any of resins (R-1) to (R-14)) as shown in Table 3 below were mixed with potassium hydroxide and water to obtain aqueous resin solutions (r-1) to (r-14). The aqueous resin solutions (r-1) to (r-14) contained neutralized resins (corresponding to specific resins). The amount of potassium hydroxide added was such that the neutralization rate of the neutralized resin was as shown in Table 3 below. The amount of water added was such that the solids concentration (content of neutralized resin) of the aqueous resin solutions (r-1) to (r-14) was 30 mass%.

[0086] [Table 2]

[0087] For resins (R-1) to (R-14), the respective contents [mass %] of the first to fourth repeating units are shown in Table 4 below.

[0088] [Table 3]

[0089] <Ink Preparation> Inks of Examples 1 to 4 and Comparative Examples 1 to 16 were prepared by the following method. First, the manufacturers and product names of the crosslinking agents used in the examples are shown below. The chemical names, chemical formulas, epoxy equivalents, and water solubility rates of the crosslinking agents are shown in Table 5 below. In Table 5 below, the chemical formula "(1)+(2)" of the crosslinking agent (EX-313) indicates that it contains a compound represented by chemical formula (1) and a compound represented by chemical formula (2).

[0090] Crosslinking agent (EX-313): "Denacol (registered trademark) EX-313" manufactured by Nagase ChemteX Corporation Crosslinking agent (EX-512): "Denacol (registered trademark) EX-512" manufactured by Nagase ChemteX Corporation Crosslinking agent (EX-521): "Denacol (registered trademark) EX-521" manufactured by Nagase ChemteX Corporation Crosslinking agent (EX-614B): "Denacol (registered trademark) EX-614B" manufactured by Nagase ChemteX Corporation Crosslinking agent (EX-612): "Denacol (registered trademark) EX-612" manufactured by Nagase ChemteX Corporation Crosslinking agent (EX-810): "Denacol (registered trademark) EX-810" manufactured by Nagase ChemteX Corporation Crosslinking agent (EX-145): "Denacol (registered trademark) EX-145" manufactured by Nagase ChemteX Corporation

[0091] [Table 4]

[0092] [ka]

[0093] Among the crosslinking agents, the crosslinking agents (EX-313), (EX-512), (EX-521), and (EX-614B) were specific crosslinking agents.

[0094] [Preparation of Ink in Example 1] (Distributed Processing) A mixture was obtained by mixing 15.0 parts by mass of a pigment (Orion Engineered Carbons "Printex (registered trademark) 80", carbon black), 15.0 parts by mass of the above-mentioned resin aqueous solution (r-1) (containing 4.5 parts by mass of neutralized resin (R-1)), 0.1 parts by mass of a defoamer (San Nopco Ltd. "SN DEFORMER 1340", an amide wax surfactant), and ion-exchanged water. The amount of ion-exchanged water added was an amount that would make the mixture 100 parts by mass.

[0095] The mixture was subjected to a dispersion treatment for 4 hours using a media-type disperser (Dynomill, manufactured by Willy & Bachofen (WAB)). Zirconia beads with a diameter of 0.5 mm were used as media in the dispersion treatment. The media filling rate was 60 volume % relative to the capacity of the vessel. The treatment temperature (chiller temperature) in the dispersion treatment was set to 10°C. After the dispersion treatment, the media was removed from the contents of the media-type disperser to obtain a pigment particle dispersion. Next, the pigment particle dispersion was filtered through a filter with a pore size of 5 μm to remove foreign matter and coarse particles.

[0096] (Cross-linking treatment) A three-neck flask equipped with a thermometer and a stirring blade was used as a reaction vessel. 100.0 parts by mass of the pigment particle dispersion after filtration was put into the reaction vessel. The temperature of the contents of the reaction vessel was maintained at 30°C using a water bath. Next, 0.82 parts by mass of a crosslinking agent (EX-313) was put into the reaction vessel. Next, the contents of the reaction vessel were stirred at 250 rpm for 1 hour. Next, while stirring the contents of the reaction vessel at 250 rpm, the temperature of the contents of the reaction vessel was increased to 80°C at a heating rate of 0.5°C / min. Next, while maintaining the temperature of the contents of the reaction vessel at 80°C, the contents of the reaction vessel were stirred at 250 rpm for 4 hours. This allowed the contents of the reaction vessel to react. Through the reaction, the neutralized resin (R-1) was crosslinked with the crosslinking agent (EX-313) to form a crosslinked resin. Next, the temperature of the contents of the reaction vessel was allowed to cool to room temperature. This resulted in the pigment particle dispersion after crosslinking treatment.

[0097] In the pigment particle dispersion of Example 1, the crosslinking rate of the crosslinking resin was calculated by the following method. For the sake of convenience, the calculation was performed assuming that 1 part by mass = 1 g. The number of moles X of the crosslinking functional group of the crosslinking agent was calculated by dividing the amount of the crosslinking agent used (0.82 g) by the epoxy equivalent of the crosslinking agent (141 g / eq). In Example 1, the number of moles X of the crosslinking functional group of the crosslinking agent was 5.82 mmol.

[0098] Next, the number of moles Y of carboxy groups contained in the neutralized resin (R-1) was calculated. First, the acid value (181 mg KOH / g) of the resin (R-1) was divided by the molecular weight (56.1) of KOH to calculate the number of moles of carboxy groups per 1 g of the neutralized resin (R-1). The number of moles of carboxy groups per 1 g of the neutralized resin (R-1) was 3.23 mmol / g. Next, the number of moles Y of carboxy groups contained in the neutralized resin (R-1) was calculated by integrating the amount of the neutralized resin (R-1) used (4.5 g) and the number of moles of carboxy groups per 1 g of the neutralized resin (R-1). The number of moles Y of carboxy groups contained in the neutralized resin (R-1) was 14.54 mmol.

[0099] Next, the crosslinking rate of the crosslinked resin was calculated by applying the above-obtained value to the following formula: The crosslinking rate of the crosslinked resin was 40%. Crosslinking rate [%] = 100 × number of moles of crosslinking functional groups X / number of moles of carboxyl groups Y

[0100] (Centrifugation) The pigment particle dispersion after the crosslinking treatment was transferred to a container, and the container was placed in a centrifugal adhesion measuring device (NS-C100 manufactured by Nano Seeds Co., Ltd.). Using the centrifugal adhesion measuring device described above, the pigment particle dispersion after the crosslinking treatment described above was centrifuged at a rotation speed of 50,000 rpm for 24 hours. After the centrifugation, the supernatant was removed from the container, and then ion-exchanged water of the same volume as the removed supernatant was added to the container. In this way, free components were removed from the aqueous medium of the pigment particle dispersion after the crosslinking treatment.

[0101] (Additive treatment) Each component was added to a container so as to obtain composition 1 shown in Table 6 below. Specifically, in Example 1, 60.0 parts by mass of the pigment particle dispersion after centrifugation (about 9 parts by mass of pigment, about 3 parts by mass of resin), 20.0 parts by mass of ethylene glycol, 15.0 parts by mass of diethyl diglycol, 0.3 parts by mass of a nonionic surfactant ("Olfine (registered trademark) E1004" manufactured by Nissin Chemical Industry Co., Ltd.), and 4.7 parts by mass of ion-exchanged water were added. The contents of the above-mentioned container were stirred at a rotation speed of 400 rpm using a stirrer ("Three-one Motor BL-600" manufactured by Shinto Scientific Co., Ltd.) to obtain a mixture. The obtained mixture was filtered using a filter (pore size: 5 μm). In this way, the ink of Example 1 was obtained.

[0102] [Preparation of inks in Examples 2 to 4 and Comparative Examples 1 to 16] The inks of Examples 2 to 4 and Comparative Examples 1 to 16 were prepared in the same manner as in the preparation of the ink of Example 1, except that the type of resin dispersion, the type and amount of crosslinking agent used, and the composition in the addition process (any of Compositions 1 to 3 in Table 6 below) were changed as shown in Table 7 below.

[0103] [Table 5]

[0104] [Table 6]

[0105] [Measurement of supernatant solids] The inks of Examples 1 to 4 and Comparative Examples 1 to 16 were centrifuged by the following method. The solid content ratio in the resulting supernatant was then measured. Specifically, the measurement target (any of the inks of Examples 1 to 4 and Comparative Examples 1 to 16) was first centrifuged at a rotation speed of 140,000 rpm (1,050,000 G) for 3 hours using an ultracentrifuge ("himac (registered trademark) CS150FNX" manufactured by Eppendorf-Himac Technologies, Ltd., rotor: S140AT). This allowed the pigment particles contained in the measurement target to settle.

[0106] Next, 30 μL of the supernatant liquid contained in the measurement object after the centrifugation process was transferred to an aluminum container for thermogravimetric measurement. Next, the mass (A) of 30 μL of the supernatant liquid was measured. Next, using a thermogravimetric analyzer ("TG / DTA7200" manufactured by Hitachi High-Tech Science Corporation), thermogravimetric analysis was performed according to the scheme shown in Table 8 below. Then, the mass loss (B) of the measurement object between temperatures of 200°C and 500°C was measured. The mass loss (B) was considered to be the mass of solids (mainly free resin) in the supernatant liquid. The content ratio of solids in the supernatant liquid was calculated according to the following formula. The measurement results are shown in Table 9 below. Solid content in the supernatant [mass%] = 100 × B / A

[0107] [Table 7]

[0108] The solid content in the supernatant was rated as "A (preferable)" when it was 2.0% by mass or less, and "B (unfavorable)" when it exceeded 2.0% by mass.

[0109] <Evaluation> Using the following methods, the inks of Examples 1 to 4 and Comparative Examples 1 to 16 were evaluated for nozzle clogging and image density of formed images. The evaluation results are shown in Table 9 below.

[0110] [Evaluation machine] The evaluation machine used was a line head-equipped inkjet recording device (a test machine manufactured by Kyocera Document Solutions, Inc.) The inks to be evaluated of Examples 1 to 4 and Comparative Examples 1 to 16 were each filled into a black ink tank of the evaluation machine.

[0111] [Nozzle clogging] The evaluation of nozzle clogging was performed under an environment of 25°C temperature and 60% RH humidity. Inkjet matte paper (Seiko Epson Corporation's "Super Fine Paper") was used as the recording medium. Using the evaluation machine, solid images (150 mm x 200 mm) were continuously formed on 100 sheets of recording medium. Next, a purge process was performed to purge ink from the recording head of the evaluation machine. Next, a wipe process was performed to wipe the ink ejection surface of the recording head of the evaluation machine with a cleaning wiper. Next, a nozzle check pattern was formed on the above-mentioned matte paper using the evaluation machine. As a result, it was confirmed that ink was ejected from all nozzles (7968 nozzles) in all evaluation subjects. That is, the number of nozzles in which nozzle clogging occurred was 0. Next, a purge process and a wipe process were performed on the recording head of the evaluation machine. Next, the evaluation machine was left stationary for 7 days without a cap on the recording head of the evaluation machine. Next, the above-mentioned purge process and wipe process were performed on the recording head of the evaluation machine. Next, a nozzle check pattern was formed on the above-mentioned matte paper using the evaluation machine. The formed nozzle check pattern was then observed to confirm the number of nozzles where nozzle clogging had occurred. The ratio of the number of nozzles where nozzle clogging had occurred to the total number of nozzles in the recording head of the evaluation machine was taken as the evaluation value for nozzle clogging. Nozzle clogging was judged according to the following criteria.

[0112] (Nozzle clogging criteria) A (Good): Evaluation value is less than 10% B (bad): Evaluation value is 10% or more

[0113] [Image Density] The image density was evaluated under an environment of a temperature of 25° C. and a humidity of 50% RH. The recording medium was PPC paper ("C 2 ") was used. A 10 cm x 10 cm solid image was formed on the recording medium using the evaluation machine. In forming the solid image, the evaluation machine was set so that the volume of each drop of ink ejected from the recording head was 11 pL (11 pL of ink per pixel). The image density of the formed solid image was measured using a reflection densitometer (X-Rite Corp., "RD-19"). In measuring the image density, the image density was measured at each of 10 randomly selected points in the solid image, and the arithmetic mean value of the image densities at the 10 points was adopted as the evaluation value (ID) of the image density. The image density was judged according to the following criteria.

[0114] (Image density standard) A (Good): ID is 1.15 or higher. B (bad): ID is less than 1.15.

[0115] [Table 8]

[0116] As shown in Table 9, the inks of Examples 1 to 4 contained an aqueous medium and pigment particles dispersed in the aqueous medium. The pigment particles contained a pigment and a crosslinked resin. The crosslinked resin was a crosslinked product of a specific resin and a specific crosslinking agent. The specific resin was a neutralized product of a specific copolymer having a first repeating unit derived from α-methylstyrene, a second repeating unit derived from styrene, a third repeating unit derived from (meth)acrylic acid, and a fourth repeating unit derived from an alkylene glycol (meth)acrylate or a dialkylene glycol (meth)acrylate. With respect to 100% by mass of all repeating units contained in the specific copolymer, the content ratio of the first repeating unit was 1% by mass or more and 65% by mass or less, the content ratio of the second repeating unit was 1% by mass or more and 60% by mass or less, the content ratio of the third repeating unit was 10% by mass or more and 40% by mass or less, and the content ratio of the fourth repeating unit was 1% by mass or more and 12% by mass or less. The acid value of the specific copolymer was 50 mgKOH / g or more and 300 mgKOH / g or less. The number average molecular weight of the specific copolymer was 3000 or more and 18000 or less. The neutralization rate of the specific resin was 20% or more and 100% or less. The specific crosslinking agent contained a polyfunctional epoxy compound having two or more epoxy groups and one or more hydroxyl groups in the molecule. The water solubility rate of the specific crosslinking agent was 80% or more. The crosslinking rate of the crosslinked resin was 25% or more and 90% or less. The inks of Examples 1 to 4 were able to form images having desired image density while suppressing the occurrence of nozzle clogging.

[0117] On the other hand, the cross-linking rate of the cross-linked resin in the ink of Comparative Example 1 was less than 25%. If the cross-linking rate of the cross-linked resin is too low, it is judged that the specific resin is easily detached from the pigment particles. As a result, the ink of Comparative Example 1 could not suppress the occurrence of nozzle clogging.

[0118] The ink of Comparative Example 2 had a crosslinking rate of over 90%. If the crosslinking rate of the crosslinking resin is too high, it is determined that the hydrophilicity of the crosslinking resin decreases, and the dispersion stability of the pigment particles decreases. As a result, the ink of Comparative Example 2 could not suppress the occurrence of nozzle clogging. Furthermore, the ink of Comparative Example 2 also had poor image density of the images formed.

[0119] The ink of Comparative Example 3 had a water solubility of less than 80% of the crosslinking agent. It is determined that the ink of Comparative Example 3 has low dispersion stability of the pigment particles due to the low water solubility of the crosslinking agent. As a result, the ink of Comparative Example 3 could not suppress the occurrence of nozzle clogging.

[0120] The crosslinking agent in the inks of Comparative Examples 4 and 5 did not have a hydroxy group. It is considered that the dispersion stability of the pigment particles in the inks of Comparative Examples 4 and 5 is low because the crosslinking agent does not have a hydroxy group. As a result, the inks of Comparative Examples 4 and 5 could not suppress the occurrence of nozzle clogging.

[0121] The inks of Comparative Examples 6 to 13 had a different structure of the repeating unit contained in the specific resin from that described above. As a result, it is determined that the inks of Comparative Examples 6 to 13 have low dispersion stability of the pigment particles. As a result, the inks of Comparative Examples 6 to 13 could not suppress the occurrence of nozzle clogging. Furthermore, the inks of Comparative Examples 10 and 12 formed images with poor image density.

[0122] In the ink of Comparative Example 14, the neutralization rate of the specific resin was 20% or less. A specific resin with a neutralization rate of 20% or less is considered to have low hydrophilicity. As a result, the ink of Comparative Example 14 had low dispersion stability of the pigment particles, and was unable to suppress the occurrence of nozzle clogging.

[0123] In the inks of Comparative Examples 15 and 16, the number average molecular weight of the specific copolymer was less than 3000 or more than 18000. It is considered that in the inks of Comparative Examples 15 and 16, the molecular size of the specific resin was not appropriate, and therefore the pigment could not be efficiently coated with the specific resin. As a result, the inks of Comparative Examples 15 and 16 could not suppress the occurrence of nozzle clogging. Furthermore, the image density of the image formed by the ink of Comparative Example 15 was poor. [Industrial Applicability]

[0124] The ink of the present embodiment can be used to form an image.

Claims

1. The ink contains an aqueous medium and pigment particles dispersed in the aqueous medium, The pigment particles include a pigment and a crosslinked resin, The crosslinked resin is a crosslinked product of a specific resin and a specific crosslinking agent, the specific resin is a neutralized product of a specific copolymer having a first repeating unit derived from α-methylstyrene, a second repeating unit derived from styrene, a third repeating unit derived from (meth)acrylic acid, and a fourth repeating unit derived from an alkylene glycol (meth)acrylate or a dialkylene glycol (meth)acrylate; With respect to 100% by mass of all repeating units contained in the specific copolymer, The content of the first repeating unit is 1% by mass or more and 65% by mass or less, The content of the second repeating unit is 1% by mass or more and 60% by mass or less, The content of the third repeating unit is 10% by mass or more and 40% by mass or less, The content of the fourth repeating unit is 1% by mass or more and 12% by mass or less, The specific copolymer has an acid value of 50 mgKOH / g or more and 300 mgKOH / g or less, The number average molecular weight of the specific copolymer is 3,000 or more and 18,000 or less, The neutralization rate of the specific resin is 20% or more and 100% or less, The specific crosslinking agent includes a polyfunctional epoxy compound having two or more epoxy groups and one or more hydroxyl groups in the molecule, The water solubility of the specific crosslinking agent is 80% or more, The crosslinking rate of the crosslinked resin is 25% or more and 90% or less.

2. 2. The ink-jet ink according to claim 1, wherein the solid content in a supernatant obtained by centrifuging at 1,050,000 G for 3 hours is 2.0% by mass or less.

3. The ink-jet ink according to claim 1 or 2, wherein the specific crosslinking agent comprises at least one of glycerol polyglycidyl ether, polyglycerol polyglycidyl ether, and sorbitol polyglycidyl ether.

4. With respect to 100% by mass of all repeating units contained in the specific copolymer, The content of the first repeating unit is 15% by mass or more and 55% by mass or less, The content of the second repeating unit is 10% by mass or more and 40% by mass or less, The content of the third repeating unit is 20% by mass or more and 35% by mass or less, The ink-jet ink according to claim 1 or 2, wherein a content ratio of the fourth repeating unit is 4% by mass or more and 11% by mass or less.

5. 3. The ink-jet ink according to claim 1, wherein the specific crosslinking agent has an epoxy equivalent of 100 g / eq. or more and 250 g / eq.

Citation Information

Patent Citations

  • Manufacturing method of pigment aqueous dispersion

    JP2019116600A