CNTs @ MICROBEADS CORE-SHELL FILLER, CEMENT-BASED COMPOSITE MATERIAL AND PREPARATION METHOD AND APPLICATION
In-situ synthesis of CNTs@microbead core-shell materials addresses CNT agglomeration issues, achieving uniform dispersion and improved functional performance in cement-based composites for structural monitoring and electromagnetic wave absorption.
Patent Information
- Application Number
- JP2024075139
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-09
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-21
- Estimated Expiration
- 2044-05-07
AI Technical Summary
CNTs agglomeration and difficulty in achieving effective dispersibility and functionality in cement-based materials, hindering magnetic conduction and heat conduction performance.
In-situ synthesis of CNTs@microbead core-shell materials by dispersing GO in an organic solvent, adding pyrrole monomer, sonication, and microwave radiation with ferrocene solution to create uniformly distributed CNTs on glass microbeads, which are then incorporated into cement-based systems.
Ensures uniform dispersion of CNTs, enhancing electrical conductivity, electromagnetic wave absorption, and heat conduction, resulting in high-performance intrinsic sensors and electromagnetic wave absorption layers for infrastructure monitoring and military facilities.
Smart Images

Figure 2024163057000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a cement-based composite material, in particular to a CNTs@microbeads core-shell filler, a cement-based composite material and a method for producing and application. [Background technology]
[0002] This discussion is merely intended to provide background information related to the present invention and does not necessarily constitute prior art.
[0003] Cement-based composite materials have the advantages of being highly compatible with concrete substrates, and having excellent intrinsic mechanical strength and functional performance. Here, cement-based conductive composite materials mixed with conductive fillers can be developed into intrinsic electrical sensors, and have great potential applications in infrastructure health monitoring and deterioration warning through pasting or embedding. Cement-based electromagnetic wave absorbing composite materials mixed with electromagnetic wave absorbing fillers can be developed into intrinsic wall electromagnetic wave absorbing members for high-end buildings and military facilities.
[0004] In recent years, carbon nanotubes (CNTs) have been widely studied due to their excellent mechanical, electrical / magnetic, thermal and other physical properties. However, when the direct addition method is adopted, nano-scale CNTs are prone to winding and aggregation phenomena, and accordingly, it is difficult for the conductive / magnetic properties of CNTs to be effectively exerted in cement-based materials.
[0005] Some people have attempted to use other constituent materials of the cement base material - cement clinker, sand and gravel, mineral blends, and polymer emulsions - as dispersion media to attach CNTs to the surfaces of cement clinker, sand and gravel, mineral blends, and polymers, respectively, in order to achieve the final dispersion and functionality of CNTs in the cement base material. However, with this method, it is difficult to directly attach conductive / magnetically conductive CNTs to the surfaces of cement clinker, sand and gravel, and polymer emulsions are insulating materials, making it difficult to ensure the realization of macroscopic functions such as electrical conductivity, magnetic conductivity, and heat conduction in CNTs-based composite materials. Summary of the Invention
[0006] In view of the deficiencies existing in the prior art, the objective of the present invention is to provide a CNTs@microbeads core-shell filler, cement-based composite material and its manufacturing method and application.
[0007] In order to achieve the above objectives, the present invention is realized by the following technical solutions.
[0008] In a first aspect, the present invention provides a method for producing a composition comprising the steps of: uniformly dispersing GO in an organic solvent, and then adding pyrrole monomer therein to obtain a mixed solution; glass microbeads are washed and then added to the mixed solution, and ultrasonicated for a set time; then the glass microbeads are transferred to an FeCl3 aqueous solution and immersed for a set time to obtain PPy+GO@microbeads; mixing the PPy+GO@microbeads with ferrocene solution, then adding hexane, and then conducting microwave radiation, the power is 800-900 W, and the time is 20-30 s, to in-situ synthesize CNTs on the glass microbeads, to prepare CNTs@microbeads core-shell material; The mass ratio of GO, pyrrole monomer, ferrocene, hexane and glass microbeads is 0.01-0.1:1-10:10-25:0.1-0.7:30-50. A method for producing CNTs@microbeads core-shell filler is provided.
[0009] The ultrasonic treatment is to better disperse the GO and pyrrole monomers and make them uniformly adsorbed on the surface of the glass microbeads for easy subsequent polymerization. The FeCl3 aqueous solution acts as an oxidizing agent to oxidize the pyrrole monomers to polypyrrole. The iron atoms generated by the decomposition of ferrocene at high temperature act as a catalyst to promote the reaction, and hexane is a supplementary carbon source. The power and time of microwave radiation are important; if the power is too small or the time is too short, the reaction temperature will be insufficient, and if the power is too high or the time is too long, the structure of CNTs will be destroyed by ablation.
[0010] Taking advantage of the high surface area of GO to provide a large amount of polymerization sites for pyrrole monomer, the electrostatic interactions between the negative charges of GO and the positive charges of pyrrole, as well as the π-π interactions between the conjugated bonds of GO and pyrrole rings, promoted the polymerization of pyrrole on the surface of GO sheets, and a stable and uniform GO@PPy layer was deposited on the surface of the spherical glass microbeads.
[0011] Microwave irradiation was applied to the microbeads coated with a GO@PPy layer in a ferrocene solution (hexane) to grow CNTs in situ with uniform diameter and favorable size distribution, ultimately resulting in the CNTs@microbeads core-shell material.
[0012] When CNTs@microbeads core-shell materials are doped into cement-based systems, the problem of CNTs being difficult to disperse and prone to aggregation in cement-based materials in the direct addition method is effectively solved, and the functions of self-sensing, electromagnetic shielding, electromagnetic wave absorption, thermal conduction and other properties of the corresponding cement-based composite materials are greatly improved, leading to the development of applications in high-performance intrinsic sensors for structural monitoring or intrinsic wall electromagnetic wave absorbing layers for high-end buildings and military facilities.
[0013] In some embodiments, the glass microbeads are micron glass microbeads.
[0014] Preferably, the glass microbeads have an average particle size of 2 to 10 μm.
[0015] More preferably, the glass microbeads have an average particle size of 2.3 μm.
[0016] In some embodiments, the concentration of the FeCl3 aqueous solution is 0.1-0.15 g / ml.
[0017] Preferably, the immersion time of the glass microbeads in the FeCl3 aqueous solution is 10 to 30 minutes.
[0018] In some embodiments, the number of layers of the GO is 1-5 layers, and the oxygen content is more than 40%, where % is mass percent. The number of layers of GO and the oxygen content are related to the dispersibility of GO in aqueous solution, with a higher oxygen content promoting the dispersion of GO and a lower number of layers allowing GO to better function as a nanomaterial and avoid agglomeration.
[0019] In some embodiments, the organic solvent is N-methylpyrrolidone (NMP).
[0020] Preferably, the mass ratio of N-methylpyrrolidone to the pyrrole monomer is 80-150:1-10.
[0021] In some embodiments, the glass microbeads are washed with acetone.
[0022] In some embodiments, the ultrasonic treatment time is 0.5 to 1.5 hours, and the ultrasonic treatment temperature is 20 to 30°C.
[0023] In a second aspect, the present invention provides a CNTs@microbeads core-shell filler produced by the above-mentioned production method.
[0024] In a third aspect, the present invention provides a cement-based composite material comprising the following components in parts by weight: 100 parts cement, 5-15 parts fly ash, 4-9 parts silica fume, 25-35 parts water, 0.5-1.5 parts water reducer, and 0.4-5 parts CNTs@microbeads core shell filler.
[0025] In some embodiments, the cement-based composite further comprises an antifoaming agent, the antifoaming agent being organosilicone-based or tributyl phosphate.
[0026] In some embodiments, the cement is Portland cement of type PI 52.5, P.II 52.5, PI 62.5 or P.II 62.5.
[0027] In some embodiments, the fly ash is a primary fly ash; Or, the silica fume is S96 grade or higher silica fume, Alternatively, the water reducing agent is a polycarboxylic acid high-efficiency water reducing agent having a water reduction rate of more than 30%.
[0028] In a fourth aspect, the present invention provides a method for producing a composition comprising the steps of: Dry mixing cement, fly ash, silica fume and CNTs@microbeads core-shell filler in a proportion to obtain a dry mixed material; and mixing the dry mix with water having a water-reducing agent dissolved therein, stirring slowly for 30 to 60 s, and then stirring rapidly for 2 to 5 min to obtain the cement-based composite material.
[0029] In a fifth aspect, the present invention provides an application of said cement-based composite material in the fields of traffic & structural intelligence monitoring, electromagnetic wave absorbing coating & electromagnetic shielding, and outdoor snow melting and ice melting projects.
[0030] Beneficial effects obtained by one or more of the embodiments of the present invention described above include the following:
[0031] 1. Taking advantage of the feature that microbeads can be sufficiently stirred and uniformly dispersed in cement-based materials, CNTs are synthesized in situ on microbeads by the method of microwave radiation to form CNTs@microbeads core-shell material, and the CNTs@microbeads core-shell material is then added into the cement-based material as a functional filler, so that the CNTs can be uniformly dispersed in the cement base material, and the electrical conductivity and electromagnetic wave absorption properties of CNTs can be greatly exerted, and the force-electrical sensing and electromagnetic wave absorption performance of the cement-based material can be greatly improved.
[0032] 2. Other dispersion methods will more or less damage the structure of CNTs, but this in situ synthesis method can ensure that the CNTs structure is intact and achieve good dispersion effect by relying on the CNTs@microbeads core-shell medium, thereby maximizing the functional effects of CNTs.
[0033] 3. As an intermediate material, GO can be ablated by microwave radiation to remove oxygen-containing groups, which can then be converted into CNTs, making the final CNTs more consistent in diameter and more uniform in size distribution.
[0034] 4. The CNTs@microbeads core-shell material reinforced cement-based composite material of the present invention not only has the characteristics of excellent mechanical properties, high durability, and high compatibility with concrete materials, but also has good intelligent electrical sensing, electromagnetic shielding performance and thermal conductivity performance, and can be widely used in the fields of traffic & structural intelligent monitoring, wall material electromagnetic shielding & electromagnetic wave absorption, and outdoor snow and ice melting projects.
[0035] The drawings in the specification which form a part of the present invention are intended to provide a further understanding of the present invention, and the illustrative embodiments of the present invention and the description thereof are intended to interpret the present invention and are not intended to unduly limit the present invention. [Brief description of the drawings]
[0036] [Figure 1]1 is a fabrication flow chart of CNTs@microbeads core-shell material reinforced cement-based composites. [Diagram 2] The electrical conductivity test results of CNTs@microbeads core-shell material reinforced cement-based composites. [Diagram 3] The reflectance test results of CNTs@microbeads core-shell material reinforced cement-based composites. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0037] It should be noted that the following detailed description is all illustrative and is intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meaning as commonly understood by those skilled in the art.
[0038] In the following the invention will be further described with reference to examples.
[0039] Example 1 The CNTs@microbeads core-shell material consisted of the following parts by weight of raw materials: 0.01 parts GO, 1 part pyrrole, 5 parts FeCl3 solution, 10 parts ferrocene, 0.1 parts hexane, 30 parts microbeads, 80 parts NMP, and some acetone.
[0040] The preparation method of the CNTs@microbeads core-shell material specifically includes the following steps: 1-1) GO and PPy were deposited on the surface of microbeads: GO was first dispersed in NMP and sonicated for 1 h, then purified pyrrole monomer was added to the dispersed GO solution, followed by the addition of acetone-washed microbeads and sonication for 1 h in a water bath at 25°C, after which the microbeads were taken out and placed in an FeCl3 aqueous solution for 15 min, and finally the coated PPy+GO@microbeads were taken out, washed and dried in an oven for 48 h. 1-2) Microwave irradiation was performed on the PPy+GO@microbeads after the deposition was completed. That is, the PPy+GO@microbeads after the deposition was completed in step 1-1) were mixed with a ferrocene solution, hexane was added, and the sample was subjected to microwave irradiation at a power of 850 W in a microwave oven for 30 s, thereby synthesizing CNTs in situ on the microbeads and producing CNTs@microbeads core-shell material.
[0041] The CNTs@microbeads core-shell material reinforced cement-based composite material is composed of the following parts by weight of raw materials: 100 parts of PI52.5 type Portland cement, 5 parts of fly ash, 4 parts of silica fume, 25 parts of water, 1.5 parts of water reducer, 1 part of CNTs@microbeads core-shell material, and 0.05 parts of antifoaming agent.
[0042] The method for preparing the CNTs@microbeads core-shell material reinforced cement-based composite material specifically includes the following steps: 2-1) The CNTs@microbeads core-shell material was mixed into the cement-based material as a functional filler. That is, the CNTs@microbeads core-shell material obtained in step 1-2) and mineral blend (fly ash, silica fume) were put into a planetary mixer together with cement and stirred rapidly for 5 min to form a CNTs@microbeads core-shell material reinforced cement-based dry mix material. 2-2) The CNTs@microbeads core-shell material reinforced cement-based dry mix material was added to water in which a water-reducing agent had been dissolved in advance, stirred slowly for 60 seconds, then stirred quickly for 3 minutes, and an appropriate amount of defoamer was added. After that, press molding or injection molding was carried out, and after processes such as vibration curing, the CNTs@microbeads core-shell material reinforced cement-based composite material was finally produced.
[0043] Example 2 The CNTs@microbeads core-shell material is composed of the following parts by weight of raw materials: 0.02 parts GO, 5 parts pyrrole, 10 parts FeCl3 solution, 20 parts ferrocene, 0.2 parts hexane, 40 parts microbeads, 120 parts NMP, and multiple acetones. The preparation method is the same as in Example 1.
[0044] The CNTs@microbeads core-shell material reinforced cement-based composite material is composed of the following parts by weight of raw materials: 100 parts of PI52.5 type Portland cement, 5 parts of fly ash, 4 parts of silica fume, 25 parts of water, 1.5 parts of water reducer, 2 parts of CNTs@microbeads core-shell material, and 0.06 parts of defoamer. The preparation method is the same as that of Example 1.
[0045] Example 3 The CNTs@microbeads core-shell material is composed of the following parts by weight of raw materials: 0.03 parts GO, 10 parts pyrrole, 15 parts FeCl3 solution, 25 parts ferrocene, 0.4 parts hexane, 50 parts microbeads, 150 parts NMP, and multiple acetones. The preparation method is the same as in Example 1.
[0046] The CNTs@microbeads core-shell material reinforced cement-based composite material is composed of the following parts by weight of raw materials: 100 parts of PI52.5 type Portland cement, 5 parts of fly ash, 4 parts of silica fume, 30 parts of water, 1 part of water reducer, 3 parts of CNTs@microbeads core-shell material, and 0.07 parts of defoamer. The preparation method is the same as that of Example 1.
[0047] Example 4 The CNTs@microbeads core-shell material is composed of the following parts by weight of raw materials: 0.04 parts GO, 5 parts pyrrole, 15 parts FeCl3 solution, 20 parts ferrocene, 0.7 parts hexane, 50 parts microbeads, 150 parts NMP, and multiple acetones. The preparation method is the same as in Example 1.
[0048] The CNTs@microbeads core-shell material reinforced cement-based composite material is composed of the following parts by weight of raw materials: 100 parts of P.II.52.5 type Portland cement, 5 parts of fly ash, 4 parts of silica fume, 35 parts of water, 0.5 parts of water reducer, 4 parts of CNTs@microbeads core-shell material, and 0.08 parts of defoamer. The preparation method is the same as that of Example 1.
[0049] Comparative Example There is no CNTs@microbeads core-shell material.
[0050] The control cement-based composite material is made of the following parts by weight of raw materials: 100 parts of P.II.52.5 type Portland cement, 5 parts of fly ash, 4 parts of silica fume, 35 parts of water, 0.5 parts of water-reducing agent and 0.08 parts of antifoaming agent. The manufacturing method is the same as that of Example 1.
[0051] The performance test experimental methods of the CNTs@microbeads core-shell materials prepared in Examples 1 to 4, the CNTs@microbeads core-shell materials reinforced cement-based composite materials, and the comparative examples are as follows:
[0052] The characteristics and purity of the CNTs in the CNTs@microbeads core-shell material were characterized by infrared and Raman spectroscopy, respectively. The results showed that the CNTs have a peak at 1750 cm -1 The characteristic peaks of the carboxyl functional group are at 1340 cm -1 , 1580 cm -1 It is shown that there are typical D and G peaks in the vicinity.
[0053] The material's pressure resistance and bending tests were conducted based on the provisions of the standard "Cement Mortar Strength Test Method (ISO Method)" (GB / T17671-1999), and tests were conducted on the bending and pressure resistance of mortar test blocks with different mix ratios and different ages (7d, 28d). The sample dimensions were 160mm x 40mm x 40mm, with three samples in one group, and the experimental results were the average of the three samples.
[0054] The mechanical properties of the comparative example and the samples of Examples 1 to 4 were tested, and the results are shown in Table 1. Compared with the comparative example in which the CNTs@microbeads core-shell material is not added, the mechanical properties of Examples 1 to 4 are obviously improved. The mixed CNTs@microbeads core-shell material ensures good dispersion of CNTs, maximizes the effect of nanomaterials, and CNTs with a high slenderness ratio are easier to bond and prevent the expansion of microcracks inside the cement-based material, thereby improving the macroscopic mechanical properties. The 7d compressive strength can reach 70 MPa or more, the bending strength is generally around 10 MPa, and the 28d compressive strength is 90 MPa or more, and the bending strength is around 13 MPa. Such an intrinsic sensing material has high compatibility with the concrete material itself of the construction structure, does not destroy the original structure, and can even reinforce the original concrete structure. Due to its excellent mechanical properties, it can meet more severe challenges during actual construction.
[0055] [Table 1]
[0056] For the electrical conductivity test of CNTs@microbeads core-shell material reinforced cement-based composite material, the four-electrode method is used to test the electrical conductivity of the CNTs@microbeads core-shell material reinforced cement-based composite material sample after drying. The sample size is 60mm×20mm×20mm. After the slurry is put into the die and vibrated, four copper meshes are manually inserted as electrodes, and the inner and outer two pairs of electrodes are 30mm and 50mm apart respectively. For the thermal conductivity test of CNTs@microbeads core-shell material reinforced cement-based composite material, the flat plate thermal conduction method is used to measure the thermal conductivity of the dried sample. The sample size is a rectangular columnar sample with a size of 300mm×300mm×30mm. Three samples are grouped into one group, and the experimental results are the average value of the three samples.
[0057] For intelligent electrical sensing testing, a combination of Wheatstone bridge technique and dynamic signal collection technique is used to test the changes in stress, strain and resistivity experienced by a sensor encapsulated in a CNTs@microbeads core-shell material reinforced cement-based composite when embedded in the midsection of a simply supported beam system and subjected to a three-point bending load.
[0058] The self-sensing performance of the comparative example and the samples of Examples 1-4 was tested. The Wheatstone bridge technique and dynamic signal collection technique were combined to study the change in resistivity of the sensor sealed with the CNTs@microbeads core-shell material reinforced cement-based composite when it was embedded in the middle part of a simply supported beam system and subjected to three-point bending load, and the results are shown in Table 2. Compared with the control group, the maximum resistivity change rate, stress sensitivity, strain sensitivity, linearity, and sharp sensing range of the sample added with CNTs@microbeads core-shell material are all significantly improved, and the maximum resistivity change rate of Example 1 can reach about 23.46%, the stress sensitivity is 0.45% / MPa, the strain sensitivity is 23, the linearity is 0.69%, the sharp sensing range is 0-60% peak stress, and the zero point drift after 10,000 cycles of loading is 3.54%. This is because the mixed CNTs@microbeads core-shell material ensures good dispersion of CNTs, so that when the specimen is subjected to pressure, the CNTs are more likely to bond with each other, which is conducive to the generation of CNT tunneling effect and contact conduction.
[0059] Therefore, the CNTs@microbeads core-shell material reinforced cement-based composite material of the present invention has good intelligent electrical sensing performance.
[0060] [Table 2]
[0061] According to the manufacturing method of Example 1, by ensuring that the compounding ratio of other raw materials other than GO is not changed (same as Example 1), CNTs@microbeads core-shell filler reinforced cement-based composites are respectively manufactured when GO occupies different proportions of pyrrole monomer (0%, 0.02%, 0.04%, 0.06%, 0.08%), and their electrical conductivity is tested, and Figure 2 is obtained. According to Figure 2, when GO is not added, the cyclopentadienyl group generated by ferrocene under high temperature can be used as a carbon source to generate CNTs, but because of the macroscopic mixture between ferrocene and microbeads, the diameter, length and uniformity of the obtained CNTs are not very good, and the improvement of the electrical conductivity of the sample is accordingly limited.
[0062] After GO is added, the high surface area of GO provides a large number of polymerization sites for pyrrole monomer, and the electrostatic interaction between the negative charges of GO and the positive charges of pyrrole, as well as the π-π interaction between the conjugated bonds of GO and pyrrole rings, promote the polymerization of pyrrole on the surface of the GO sheet, resulting in the deposition of a stable and uniform GO@PPy layer on the surface of the spherical glass microbeads. The inherent oxygen-containing groups of GO disappear at high temperature and are transformed into CNTs. The obtained CNTs have good dimensions and high uniformity, and the electrical conductivity of the sample is greatly improved.
[0063] For the reflectance test, according to the national military standard GJB2038A-2011, the radar absorbing material (RAM) reflectance test method includes the radar scattering cross section (RCS) test method and the arc test method, and the arc test method is used to test the reflectance of the sample. The sample size is 200mm×200mm×25mm, the test frequency is 2~18GHz, the sample is dried before testing, there are three samples in each group, and the experimental results are the average value of the three samples.
[0064] Using the manufacturing method of Example 1, ensuring that the mixing ratio of other raw materials other than GO is not changed (same as in Example 1), CNTs@microbeads core-shell filler reinforced cement-based composite materials with GO accounting for different proportions of pyrrole monomer (0%, 0.01%, 0.05%) were respectively manufactured, and the electromagnetic wave absorption performance test was performed. The results are shown in Figure 3. Within the range of 2 to 18 GHz, each sample curve also has multiple peaks below -10 dB. When the amount of GO mixed in is 0, the sample has a maximum absorption peak of -14.5 dB at 3 GHz, and the frequency bandwidth below -10 dB is 5.1 GHz. When the amount of GO mixed in is 0.01%, the sample has a maximum absorption peak of -32.7 dB at 10 GHz, and the frequency bandwidth below -10 dB reaches 6.5 GHz. When the amount of GO mixed in is 0.05%, the sample has a maximum absorption peak of -42 dB at 4.7 GHz, and the frequency bandwidth below -10 dB reaches 11.5 GHz. The polarization degree and electric dipole moment rearrangement of long-tube and large-diameter CNTs under the action of an electric field will cause more dielectric loss. As can be seen from the above, the diameter, length and uniformity of CNTs are all improved by the addition of GO, and the sample with GO added has excellent electromagnetic wave absorption performance.
[0065] The above is only a preferred embodiment of the present invention, and is not intended to limit the present invention. Those skilled in the art can make various modifications and changes to the present invention. All modifications, equivalent replacements, improvements, etc. made without departing from the spirit and principle of the present invention shall be included within the protection scope of the present invention. [Explanation of symbols]
[0066] 1. Microbeads 2. Pyrrole monomer 3 GO-NMP dispersion 4. FeCl3 Solution 5 PPy+GO@microbeads 6 CNTs@microbeads core-shell material 7. Gelling materials and sand dry mixing materials 8. Mixture of water and water-reducing agent 9. CNTs@Microbeads Core-Shell Material Reinforced Cement-Based Composites 10 Ultrasonic dispersion 11 Oxidative polymerization 12 Microwave irradiation 13 Mixing and stirring A Probe-type ultrasonic cell grinder B Constant temperature water bath pot C. Microwave
Claims
1. uniformly dispersing GO in an organic solvent, and then adding pyrrole monomer therein to obtain a mixed solution; The glass microbeads are washed and then added to the mixed solution, and ultrasonicated for a set time. Then, the glass microbeads are dissolved in FeCl 3 transferring to an aqueous solution and immersing for a set time to obtain PPy+GO@microbeads; mixing the PPy+GO@microbeads with ferrocene solution, then adding hexane, followed by microwave irradiation, power 800-900W, time 20-30s, to synthesize CNTs in situ on the glass microbeads, to prepare CNTs@microbeads core-shell material; The mass ratio of GO, pyrrole monomer, ferrocene, hexane and glass microbeads is 0.01-0.1:1-10:10-25:0.1-0.7:30-50; The method for producing CNTs@microbeads core-shell filler is characterized in that the glass microbeads are micron-class glass microbeads, and the average particle size of the glass microbeads is 2-10 μm.
2. The method for producing CNTs@microbeads core-shell filler according to claim 1, characterized in that the average particle size of the glass microbeads is 2.3 μm.
3. The FeCl 3 The method for preparing CNTs@microbeads core-shell filler according to claim 1, characterized in that the concentration of the aqueous solution is 0.1-0.15g / ml.
4. FeCl in glass microbeads 3 The method for producing CNTs@microbeads core-shell filler according to claim 3, characterized in that the immersion time in the aqueous solution is 10-30 min.
5. The method for producing CNTs@microbeads core-shell filler according to claim 1, characterized in that the number of layers of GO is 1-5 layers, the oxygen content is more than 40%, and % is mass percent.
6. The organic solvent is N-methylpyrrolidone, the ultrasonic treatment time is 0.5-1.5 h, and the ultrasonic treatment temperature is 20-30° C.; The method for preparing CNTs@microbeads core-shell filler according to claim 1, characterized in that the mass ratio of N-methylpyrrolidone to pyrrole monomer is (80-150):(1-10).
7. A CNTs@microbeads core-shell filler, characterized in that it is produced by the production method according to any one of claims 1 to 6.
8. A cement-based composite material, characterized in that it comprises the following components in parts by weight: 100 parts cement, 5-15 parts fly ash, 4-9 parts silica fume, 25-35 parts water, 0.5-1.5 parts water reducer and 0.4-5 parts CNTs@microbeads core shell filler according to claim 7.
9. 9. The cement-based composite material according to claim 8, further comprising an antifoaming agent, the antifoaming agent being organosilicon-based or tributyl phosphate.
10. The cement is Portland cement of type P.I. 52.5, P.II 52.5, P.I. 62.5 or P.II 62.5; The cement-based composite material according to claim 8, characterized in that the fly ash is a first-class fly ash.
11. 9. The cement-based composite material according to claim 8, characterized in that the silica fume is S96 grade or higher silica fume, and the water reducing agent is a polycarboxylic acid high-efficiency water reducing agent with a water reduction rate of more than 30%.
12. Dry mixing the cement, the fly ash, the silica fume and the CNTs@microbeads core-shell filler in a proportion to obtain a dry mixed material; and mixing the dry mix with water containing a water-reducing agent, slowly stirring for 30-60 s, and then rapidly stirring for 2-5 min to obtain a cement-based composite material.
Citation Information
Patent Citations
Nanocarbon and method for producing the nanocarbon
JP2006219358A
Method for converting cement source into fuel
JP2008050224A
Composite materials based on binders modified with rice husks and carbon nanostructures.
JP2014501862A
Preparation and use process of silica-carbon allotrope composites
JP2017518243A
Anode materials for lithium-ion batteries
JP2019536210A