Method for making polyurea resin fireproof
A flame-retardant adhesive composition with a synthetic resin binder and inorganic porous powder addresses the nonflammability of polyurea resins, enhancing adhesion and providing effective flame resistance.
Patent Information
- Application Number
- JP2023089198
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polyurea resins lack effective methods to render them nonflammable, with existing flame retardants posing challenges in workability and adhesion issues, particularly with water-based non-combustible paints and coatings.
A flame-retardant adhesive composition comprising a synthetic resin binder, inorganic porous powder, and auxiliary substances is applied to polyurea resin surfaces, forming a nonflammable coating through a mixture that enhances flame resistance.
The method results in a polyurea resin that meets nonflammable criteria, offering improved adhesion and workability, with potential additional benefits like design properties, antibacterial effects, and enhanced insulation.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for rendering a polyurea resin and a polyurea foam flame retardant, and an adhesive composition for use therein. [Background technology]
[0002] In recent years, objects of any shape or size can be coated with polyurea resin to The object Polyurea resins have become widely known as lining materials that improve the waterproofing, chemical resistance, abrasion resistance, heat resistance, and corrosion resistance of structures. Polyurea resin is a resin compound based on urea bonds generated by the chemical reaction of isocyanate and polyamine. Its quick-drying property, which takes just a few seconds to a few minutes to harden, enables it to be used in a wide range of situations, which is said to be one of the reasons why it is so popular in the market. It is also generally known that some grades have an elongation rate of over 900%, and it has been reported that the strength that comes from this flexibility is such that it is also used as an explosion-proofing measure for military facilities.
[0003] As mentioned above, the only weakness of polyurea resin as an excellent lining material is that it is said to have some heat resistance but not fire resistance. For this reason, developers in related industries have been discussing the fire resistance, fire prevention, and flame retardancy of polyurea resin. and flame retardant Developments have been made to improve this. For example, a "polyurea foam" is known that contains at least one flame retardant selected from a phosphate-containing flame retardant, a bromine-containing flame retardant, a boron-containing flame retardant, an antimony-containing flame retardant, and a metal hydroxide. For details, see Patent Document 1.
[0004] For example, a strong cabin is installed on a barge with a double-bottom structure, made of laminated boards made of laminated timber, insulating material, and metal plates joined together with adhesive and metal connectors, and coated with multi-layer polyurethane resin and insulating non-combustible paint to enhance impact resistance, environmental performance, and fire resistance, and used as a disaster prevention shelter that can withstand earthquakes and fires, and floats on the water surface in the event of a flood disaster, with the aim of protecting the lives and property of the people. For details, see Patent Document 2.
[0005] Also, for example, a development project for "Thermal insulation and fireproofing of aquaculture facilities using recycled porous lightweight foamed materials" is known, which is characterized in that the exterior wall and roof materials of the non-combustible and heat-insulating structure for container aquaculture facilities are formed by bonding plate-shaped recycled porous lightweight foamed material plates and foamed resin insulation materials with an adhesive, spray-coating the surface with polyurea resin, forming glass fiber net bands at the joints of the composite polyurea resin materials for the walls and roof, and applying glass paint to the entire surface, which is a non-combustible and heat-insulating enclosure wall structure for container aquaculture facilities. For details, see Patent Document 3.
[0006] Also, for example, a development project for a "fish farming and breeding system in which recycled porous lightweight foamed material is molded into a plate shape so that it does not become a fuel replenishment role in the event of a fire, and aquariums and facilities are manufactured using the recycled porous lightweight foamed material so that it does not become a fuel replenishment role in the event of a fire, and the recycled porous lightweight foamed material plate is formed into a plate shape and laminated with an adhesive to form a composite plate material, which is cut to a specified size and laminated with an adhesive in multiple pieces, in which the recycled porous lightweight foamed material plate is placed on the outside and the foamed resin insulation plate is placed on the inside, and a polyurea resin is sprayed and coated on part or all of the surface of the composite plate material, and a fireproof glass paint is applied to the surface for surface fire prevention, is known. For details, see Patent Document 4.
[0008] [Patent Document 1] Patent Registration No. 6925554 [Patent Document 2] Registered Utility Model No. 3216207 [Patent Document 3] Patent registration number 6629953 [Patent Document 4] Patent registration number 6564969 DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0009] However, the development project of the "polyurea foam" in Patent Document 1 is characterized in that at least one flame retardant for the polyurea foam selected from a phosphate-containing flame retardant, a bromine-containing flame retardant, a boron-containing flame retardant, an antimony-containing flame retardant, and a metal hydroxide is mixed into the raw material when the polyurea foam is sprayed on-site, but problems have been pointed out regarding workability on-site and variation during mixing. For example, when spraying polyurea foam on-site, a dedicated spray applicator is required, and it is extremely important to check things like "adequate power supply," "applicator pressure management," "applicator temperature management," "type of gun to be used," and "selection of mix chamber to be used." It has been pointed out that using the equipment with an incorrect understanding can lead to poor mixing of the paint film and poor application, and is extremely dangerous.
[0010] Furthermore, the development project for the "health-prolonging life-floating box" in Patent Document 2, for example, is described in paragraph (0015) of the specification as "...protecting the coating of multi-layered polyurethane resin or urethane urea resin, which has hardened together with the first layer of polyurethane resin or urethane urea resin, by painting a heat insulating non-flammable paint on the coating." However, there is no detailed description of the heat insulating non-flammable paint, and generally known "non-flammable paints" are often water-based. It has been pointed out that water-based heat insulating non-flammable paints have problems with their adhesion, cohesion and bonding to the coating of multi-layered polyurethane resin or urethane urea resin.
[0011] Furthermore, in the development project of “Thermal insulation and fireproofing of aquaculture facilities using recycled porous lightweight foam materials” in Patent Document 3, for example, paragraph (0045) of the specification states that “Furthermore, by applying a fireproof glass paint to the surface, fire is prevented on the surface and does not progress to deeper areas,” but there is no detailed description of the fireproof glass paint. Generally known “fireproof glass paints” are often water-based, and it has been pointed out that water-based fireproof glass paints have problems with their adhesion, cohesion and retention on polyurethane resin composite materials.
[0012] In addition, in the development project of Patent Document 4, "An aquaculture and breeding system in which recycled porous lightweight foamed materials are molded into plates so as not to be used for fuel replenishment in the event of a fire, and aquariums and facilities are constructed and provided using these materials," for example, paragraph (0024) of the specification states, "Furthermore, a secondary cement mortar finish coat is applied over the glass fiber net and net band, and the final finish is applied with non-combustible glass paint," but there is no detailed description of the non-combustible glass paint, and generally known "non-combustible glass paints" are often water-based, and it has been pointed out that water-based non-combustible glass paints have problems with their adhesion, adhesion, and sticking ability to polyurethane resin.
[0013] The present invention has been made to solve the above-mentioned problems, and has an object to provide a method for making a polyurea resin flame retardant or non-combustible by applying or spraying a flame retardant or non-combustible adhesive composition to the surface of the polyurea resin, polyurea foam, multilayer polyurea resin, polyurea resin composite material, etc. described in this specification. [Means for solving the problem]
[0014] The first means for solving the problem (claim 1) is to provide a method for making a polyurea resin flame retardant, which is characterized by the fact that the inventors of the present application discovered the phenomenon that the inside of the flame retardant adhesive composition-coated body and the surface part of the flame retardant adhesive composition-coated body are made flame retardant by applying a polyurethane resin to an object of any shape or any dimension, curing the applied polyurethane resin, applying a predetermined amount of a flame retardant adhesive composition that makes the polyurethane resin-coated surface flame retardant and thoroughly drying it, and then applying a predetermined amount of a flame retardant adhesive composition that makes the inside or surface of the flame retardant adhesive composition-coated body flame retardant, thereby making the inside of the flame retardant adhesive composition-coated body and the surface part of the flame retardant adhesive composition-coated body flame retardant, and arrived at the present invention.
[0015] Moreover, since the polyurea resin is a generally well-known material, any type available on the market may be used. Further, in this specification, references to polyurea resins are intended to include polyurea foams, multi-layer polyurea resins, polyurea resin composites, and the like. As for the adhesive composition constituting the flame retardant adhesive composition, any adhesive material that is considered to adhere to the surface coated with the polyurethane resin may be used. For example, phenol resin, melamine resin, urea resin, polyester resin, epoxy resin, vinyl chloride resin, silicone resin, modified silicone resin, polyvinyl chloride, silicone rubber, etc. are generally known, and at least one of these may be selected and used. The adhesive composition constituting the fireproof adhesive composition may generally be considered to include commercially available water-based fireproof adhesives and water-based fireproof paints as a part of the fireproof adhesive composition. In this case, one of the main components of the water-based fireproof adhesive may be selected from a water-glass adhesive composition, a silanol adhesive composition, a colloidal silica adhesive composition, etc. One of the main components of the water-based fireproof paint may be selected from a water-glass adhesive composition, a silanol adhesive composition, a colloidal silica adhesive composition, etc.
[0016] The second means for solving the problem (Claim 2) is to provide a method for making a polyurea resin flame retardant as described in the first means for solving the problem (Claim 1), characterized in that the flame retardant adhesive composition is composed of a synthetic resin binder, an inorganic porous powder, and an auxiliary substance.
[0017] As for the synthetic resin binder, it is preferable to select and use at least one of the thermosetting resins and flame-retardant resins that are generally available on the market. For example, as the thermosetting resin, phenol resin, melamine resin, urea resin, polyester resin, epoxy resin, etc. are generally known as materials that are easily available, and at least one of these may be selected and used. Also, as the flame-retardant resin, for example, phenol resin, melamine resin, vinyl chloride resin, silicone resin, modified silicone resin, polyvinyl chloride, silicone rubber, etc. are generally known, and at least one of these may be selected and used. Regarding the inorganic porous powder, one of the uses in the present invention is to utilize the substance adsorption effect of the inorganic porous powder. The inventors of the present application discovered a phenomenon that, after a predetermined amount of the synthetic resin binder is adsorbed into the inorganic porous powder and thoroughly dried, a mixture of the inorganic porous powder and the synthetic resin is formed, thereby making it possible to make the synthetic resin binder flame retardant, and thus arrived at the present invention. Therefore, any inorganic porous material that can exert the effect of the flame retardant phenomenon can be used. Regarding the auxiliary substance, any material may be used as long as it is determined that the effect of the inorganic porous powder described in this specification can be improved.
[0018] The third means for solving the problem (Claim 3) is to provide a method for making a polyurea resin fireproof as described in the method for making a polyurea resin fireproof as described in the first means for solving the problem (Claim 1), characterized in that the fireproof adhesive composition is composed of an aqueous inorganic binder, an inorganic porous powder, an organic powder, and an auxiliary substance.
[0019] The aqueous inorganic binder may generally be considered to include commercially available aqueous non-flammable adhesives and aqueous non-flammable paints. In this case, one of the main components of the aqueous non-flammable adhesive may be selected from a water glass-based adhesive composition, a silanol-based adhesive composition, a colloidal silica-based adhesive composition, etc. Also, one of the main components of the aqueous non-flammable paint may be selected from a water glass-based adhesive composition, a silanol-based adhesive composition, a colloidal silica-based adhesive composition, etc. Regarding the inorganic porous powder, one of the uses in the present invention is to utilize the substance adsorption effect of the inorganic porous powder, and any inorganic porous material may be used as long as it is possible to obtain an aqueous fireproofing mixture that makes a non-flammable substance or a non-flammable substance fireproof by causing the inorganic porous powder to adsorb a predetermined amount of the aqueous inorganic binder and thoroughly drying the powder, and then producing a mixture of the inorganic porous powder with the aqueous fireproofing adhesive or the aqueous fireproofing paint. Regarding the auxiliary substance, any material may be used as long as it is determined that the effect of the flame retardant adhesive composition described in this specification can be improved, for example, a material that can improve viscosity, improves flame retardancy or flame resistance, improves adhesion, or improves fire resistance or heat insulation.
[0020] The water glass in the water glass adhesive composition generally refers to a concentrated aqueous solution of potassium silicate, sodium silicate, etc., and generally, commercially available water glass contains 100 parts by weight of water, and the potassium silicate or sodium silicate is 10 to 30 parts by weight, and in the present invention, it is preferable to use an aqueous solution of sodium silicate. Sodium silicate is one of the silicates represented by the chemical formula: Na2SiO3·nH2O, and although it is a powdery solid itself, it is often commercially available as an aqueous solution, making it one of the materials that is easily available. Furthermore, the silanol in the silanol-based adhesive composition may be of any type so long as it has a structure having a siloxane skeleton obtained by the hydration reaction of metallic silicon. Furthermore, the colloidal silica in the colloidal silica-based adhesive composition may be of a type (particle diameter 5 to 300 μm) that is widely used in water-based paints and is easily available, but preferably, the particle size must be adjusted. The preferred particle size range is generally 10 to 20 μm. If the particle size is less than 10 μm, colloidal silica is prone to gelation and it is difficult to obtain a high concentration, so that when used as an adhesive, cracks are likely to occur in the adhesive. Since colloidal silica has a smaller bond strength than other water glass-based adhesive compositions and silanol-based adhesive compositions, a liquid with as high a concentration as possible under normal conditions, preferably 35 to 40% by weight, is used. On the other hand, if the particle size exceeds 20 μm, the adhesive strength becomes small, which is not preferred. A particularly preferred particle size range is 15 to 20 μm. Colloidal silica is a colloidal solution in which negatively charged amorphous silica particles are dispersed in water; when heated, most of the water of crystallization is lost at 200°C, and the silanol groups on the surface undergo dehydration and condensation to form siloxane bonds between the particles, resulting in a water-resistant structure, making it suitable for use in areas where water resistance is required.
[0021] A fourth means for solving the problem (Claim 4) can provide a method for making a polyurea resin fireproof as described in the second means for solving the problem (Claim 2) and the third means for solving the problem (Claim 3), characterized in that the powder is at least one type selected from the group consisting of diatomaceous earth, montmorillonite, zeolite, volcanic ash, perlite, foamed glass, cement, coal ash, vermiculite, baked shells, and the like.
[0022] Diatomaceous earth is known to be a material whose components, color, and specific gravity tend to vary depending on the place of origin, and may be avoided depending on the application, so celite made from diatomaceous earth is often used. Celite is a white powder with excellent heat insulation properties due to its lightness and porosity, with a specific gravity of 0.2 to 0.3 compared to diatomaceous earth, and is excellent in stability. Its main component is silicon dioxide, and its heat resistance temperature is about 1700°C, so the use of celite is preferable in the present invention. The present invention was developed by focusing on the heat insulation properties and adsorption properties of celite. The montmorillonite has the property of taking in water between the layers and swelling remarkably, and has high ion exchange properties. It develops adhesive strength at a water content of 150%, and is used as a binder for foundry sand molds and as soil dressing for absorbing fertilizer. The present invention was developed by focusing on the function of the montmorillonite as a binder and its adsorption action. The zeolite is also called zeolite and is a microporous crystalline aluminosilicate with a pore size of 0.3 to 1 nm. It is generally used as an ion exchange material, catalyst, and adsorption material, and is an industrially important substance. Currently, synthetic zeolites with various structures and physical properties are used industrially in addition to those mined from nature. The present invention was developed by focusing on the function of the zeolite as an adsorption material. The volcanic ash is generally called shirasu or shirasu balloons, and is used industrially as a fire-resistant, heat-resistant, and insulating material, and is also used as a soil conditioner in agriculture because it is a porous material with good drainage. The present invention was made by focusing on the fact that the volcanic ash is a porous material and has excellent fire resistance, heat resistance, and insulating properties. The perlite is made by heating glassy volcanic rock at high temperatures and rapidly evaporating the water, which makes the internal structure porous. This gives the perlite a low specific gravity and excellent drainage, water retention, and air permeability, as well as excellent heat insulation. The present invention was developed by focusing on the fact that the perlite is a porous material, has excellent air permeability, and also has excellent heat insulation. The foamed glass is a lightweight foamed material made from 100% waste glass, and is lightweight, porous, and has excellent water permeability and water retention properties, and therefore has a wide range of applications, including civil engineering, greening, architecture, agriculture, water purification, etc. The present invention was developed by focusing on the fact that the foamed glass is lightweight, porous, and has excellent water permeability. The cement has excellent reactivity with the water-based non-flammable adhesive and the water-based non-flammable paint, and generates a compound that is used as a hardener. However, since it has poor fire resistance, alumina cement is used when fire resistance or heat resistance is required. Therefore, the use of alumina cement is preferable in the present invention. The present invention was arrived at by focusing on the fact that the cement has excellent reactivity with the water-based non-flammable adhesive and the water-based non-flammable paint, generates a compound that functions as a hardener. The coal ash is also known as fly ash, and since its main components are silicon dioxide and aluminum oxide, it has a heat-resistant temperature of about 1700 to about 2000°C. It is relatively light with a specific gravity of 1.0, and is porous, so it has heat insulating properties. The present invention was developed by focusing on the fact that the coal ash is porous and has heat insulating properties. The vermiculite is composed mainly of silicon dioxide, magnesium oxide, and aluminum oxide, and therefore has a heat-resistant temperature of about 1700 to about 2000°C, making it an excellent fire-resistant material, and is a light porous material with a specific gravity of about 0.1, and has high heat insulation properties, making it an excellent heat-insulating material. The present invention has been developed by focusing on the heat resistance, fire resistance, heat resistance, and adsorption action of the vermiculite. Regarding the baked shells, baked scallop shells are generally known and are characterized by their antibacterial and antifungal effects. The present invention was developed by focusing on the antibacterial and antifungal effects of the baked shells.
[0023] A fifth means for solving the problem (Claim 5) can provide a method for making a polyurea resin fireproof as described in the third means for solving the problem (Claim 3), characterized in that the organic porous powder is at least one type selected from the group consisting of plant powder, plant sintered charcoal powder, pulp powder, dietary fiber powder, and foamed plastic powder.
[0024] The plant powder may be any part of a plant that has been dried and powdered. For example, the fruit, flower, leaf, branch, trunk, or root of a plant may be any part of a plant that has been dried and powdered. The plant powder may be produced using commercially available equipment such as a food dehydrator or grinder. There are various kinds of plant powders, for example, starch (a powder formed by plants to store glucose produced by photosynthesis) is contained in rice, wheat, corn, potato, etc., and these may be used alone or in any combination. Also, rice flour, wheat flour, corn powder, potato powder, etc. may be used alone or in any combination. Regarding the sintered plant charcoal powder, any part of a plant may be used as long as it is carbonized and powdered, for example, fruits, flowers, leaves, branches, trunks, roots, etc. of a plant may be used as long as it is carbonized and powdered. The pulp powder is made by mechanically and chemically treating wood and other plant matter to separate the cellulose fibers, which are then suspended in water or made into cardboard form, and is roughly divided into two types, chemical pulp and mechanical pulp, depending on the manufacturing method. Any pulp can be used as long as it is a raw material for paper, artificial fibers, etc. In addition, both virgin pulp and recycled paper pulp can be used. Regarding dietary fiber powder, first, there are known types of dietary fiber, such as (a) soluble dietary fiber, (b) soluble dietary fiber contained in seaweed, (c) insoluble dietary fiber, (d) fiber that has the properties of both insoluble dietary fiber and soluble dietary fiber, (e) viscous dietary fiber, and (f) non-viscous dietary fiber, and these may be used alone or in any combination. As for (a) water-soluble dietary fiber, known examples include pectin (an intercellular adhesive substance in the cell walls of plants, found in large amounts in fruits), enzymatic hydrolysis products of guar beans (used as a thickening stabilizer), glucomannan (a storage carbohydrate in konjac yam, the raw material for konjac), β-glucan (found in large amounts in mushrooms), polydextrose (a chemically synthesized artificial water-soluble dietary fiber), fructan (a polymer of fructose molecules found in shallots, Jerusalem artichokes, and the like. Inulin, levan, and graminan are also included in fructans), inulin (a storage carbohydrate found in the roots and underground stems of Asteraceae plants, such as burdock and Jerusalem artichoke), gum arabic (dried secretions from wounds in the bark of Acacia acacia trees or related plants of the same genus), maltitol, psyllium, indigestible oligosaccharides, indigestible dextrin, and the like, and these may be used alone or in any combination. Regarding (b) water-soluble dietary fiber contained in seaweed, known examples include agarose (a major component of the cell wall of red seaweed, and the main component of agar extracted from red seaweed), sodium alginate (a major component of the cell wall of brown seaweed, and contained in kelp, etc.), carrageenan (a polysaccharide contained in large amounts in red algae such as Acanthus rotundus and Acanthus ginseng), fucoidan, porphyran, laminaran, etc., and these may be used alone or in any combination. As for (c) insoluble dietary fiber, cellulose, hemicellulose, lignin, etc. are the main components of plant cell walls and are obtained in large quantities from vegetable foods such as vegetables. Chitin, chitosan, etc. are the main components of crustacean shells and fungal cell walls. The like are known, and these may be used alone or in any combination. In addition, (d) resistant starch is known to have the properties of both insoluble and soluble dietary fiber. As for (e) viscous dietary fiber (which becomes gel-like when dissolved and slows down the absorption of nutrients), pectin, β-glucan, guar gum, psyllium, etc. are known, and these may be used alone or in any combination. As for (f) non-viscous dietary fiber (which becomes gel-like when dissolved and slows down nutrient absorption), cellulose, lignin, etc. are known, and these may be used alone or in any combination. Regarding the foamed plastic powder, foamed plastic refers to a material formed into a foam or porous shape by finely dispersing gas in synthetic resin, and any material may be used as long as it can be defined as a heterogeneous dispersion system of solid synthetic resin and gas. Foamed plastic is known to have characteristics such as being lightweight and having excellent heat insulation and shock-absorbing properties. In addition, types of foamed plastic include polyurethane foam, polystyrene foam, polyethylene foam, polypropylene foam, etc., and these may be used alone or in any combination.
[0025] In addition, the particle size of the organic porous powder can be about 0.1 μm to 1 mm, and is preferably about 1 to 100 μm. If the particle size of the organic porous powder is 100 μm or more, the rheological properties will be too strong to be practical, and if the particle size of the organic porous powder is 1 μm or less, the cost will be too high to be practical, but this is not the case when it is applied to molded products with high added value. The amount of the organic porous powder added is preferably 0.1 to 50 parts by weight relative to 100 parts by weight of the aqueous noncombustible adhesive, and more preferably 1 to 20 parts by weight. For example, when the aqueous noncombustible adhesive is 100 parts by weight, if the pulp powder is 0.1 part by weight or less, the rheological properties are too weak to be practical, and if the organic porous powder powder is 20 parts by weight or more, the cost becomes too high to be practical, but this does not apply when applied to molded products with high added value.
[0026] A sixth means for solving the problem (Claim 6) can provide a fiber powder-containing inorganic adhesive composition according to the second means for solving the problem and the third means for solving the problem (Claim 3), characterized in that the auxiliary substance is at least one selected from the group consisting of a viscosity adjuster, a curing agent, and a colorant.
[0027] As for the colorant, any inorganic colorant based on metal oxide such as titanium oxide (white), iron oxide (red), or copper oxide (green) or a pigment-based colorant generally available on the market may be used. The amount of the inorganic colorant added may be 0 to 50 parts by weight relative to 100 parts by weight of the aqueous non-flammable adhesive, but it is preferable to use about 1 to about 20 parts by weight. If the aqueous non-flammable adhesive is 100 parts by weight, the coloring effect is too weak to be practical if the inorganic colorant is 1 part by weight or less, and the cost is too high to be practical if the inorganic colorant is 20 parts by weight or more. The inorganic colorant can be added to the aqueous non-flammable adhesive at any time before, during, or after the manufacturing process.
[0028] The hardener may be selected from diatomaceous earth, celite, kaolinite, illite, talc, montmorillonite, cordierite, mullite, sepiolite, sintered shell powder, and the like. The viscosity adjusting agent may be selected from wheat flour, rice flour, starch, gelatin, agar, carrageenan, collagen, sodium alginate, polyvinyl alcohol, and the like. The amount of the curing agent or viscosity modifier added can be 0 to 50 parts by weight relative to 100 parts by weight of the fiber powder-containing inorganic adhesive composition, but it is preferable to use about 1 to about 20 parts by weight. If the amount of the aqueous nonflammable adhesive is 100 parts by weight, if the amount of the curing agent or viscosity modifier is 1 part by weight or less, the curing property and thickening effect are too weak to be practical, and if the amount of the curing agent or viscosity modifier is 20 parts by weight or more, the cost becomes too high to be practical. In addition, the liquid component separation preventing substance can be added to the fiber powder-containing inorganic adhesive composition at any time before, during, or after the manufacturing process, but it is preferable to add it at the latter time, as this is particularly advantageous from a practical standpoint. Effect of the Invention
[0030] The method for making a polyurea resin flame retardant of the present invention having the above-mentioned configuration can provide the following excellent effects. (1) According to the invention of the first means (claim 1) for solving the problems described in this specification to the sixth means (claim 6) for solving the problems described in this specification, after applying a predetermined amount of a flame-retardant adhesive composition to the polyurea resin coating surface and drying it sufficiently, the organic solvent contained in the synthetic resin-inorganic mixture composition is removed from the inside and surface of the flame-retardant adhesive composition-coated body, and as a result, a mixture of a synthetic resin composition and an inorganic porous powder is formed inside the flame-retardant adhesive composition-coated body or on the surface of the flame-retardant adhesive composition-coated body, and the inorganic porous powder mixture is flame-retarded. As a result, it is possible to provide a flame-retardant polyurea resin.
[0031] (2) As an additional effect of the invention due to the effect (1) of the invention described above, when a practitioner of the invention determines that the polyurethane resin of the invention is sufficient in terms of flame retardancy even if it does not go so far as to render it flame-resistant, the flame-retardant adhesive composition can be used as a flame-retardant adhesive for a surface coated with the polyurethane resin. Furthermore, for example, the flame-retardant adhesive can adhere paper, cloth, and synthetic resin sheet materials by utilizing the synthetic resin binder described in this specification, and as such, it becomes possible to attach a sheet body to the polyurethane resin-coated surface, which can have functionality selected from design properties, antibacterial properties, light-blocking properties, heat insulation properties, sound insulation properties, sound absorption properties, deodorizing properties, insect repellency, etc., either alone or in combination.
[0032] (3) As a further effect of the invention due to the effect (1) of the invention described above, after a predetermined amount of a flame-retardant adhesive composition is applied to the polyurea resin-coated surface and sufficiently dried, the organic solvent contained in the synthetic resin-inorganic mixture composition is removed from the inside and surface of the flame-retardant adhesive composition-coated body, and as a result, a mixture of the synthetic resin composition and the inorganic porous powder is formed inside the flame-retardant adhesive composition-coated body or on the surface of the flame-retardant adhesive composition-coated body. After the synthetic resin-inorganic mixture is flame-retarded, the synthetic resin-inorganic mixture is contained in the inside and surface of the flame-retardant adhesive composition-coated body described in this specification. The surface is characterized in that by applying a predetermined amount of the flame retardant adhesive composition described in this specification to the inside of the flame retardant adhesive composition-coated body and to the surface portion of the flame retardant adhesive composition-coated body, a predetermined amount of the flame retardant adhesive composition penetrates into the inside of the flame retardant adhesive composition-coated body, a nonflammable mixture is formed inside the flame retardant adhesive composition-coated body, and the inside of the flame retardant adhesive composition-coated body is formed, and a predetermined amount of the flame retardant adhesive composition adheres to the surface portion of the flame retardant adhesive composition-coated body, and a nonflammable coating film is formed on the surface portion of the flame retardant adhesive composition-coated body, thereby forming a coating film portion of the flame retardant adhesive composition-coated body. As a result, it is possible to provide a flame-retardant polyurea resin. BEST MODE FOR CARRYING OUT THEINVENTION Example 1
[0035] The present invention is based on the above configuration, but in the first embodiment, 250 g of water glass No. 3 specified in Japanese Industrial Standard JIS K1408 is prepared in a beaker in advance. About 50 g of dried virgin pulp powdered to about 5 μm in a mortar is added to this water glass solution, and kneaded with a hand mixer (500 rpm / minute) at room temperature (about 20° C.) for about 3 minutes to obtain 300 g of non-flammable water-based adhesive. Next, 140 g of a commercially available PVC resin adhesive was prepared in a beaker. About 60 g of commercially available Shirasu balloons were added to the PVC resin adhesive solution and kneaded for about 3 minutes at room temperature (about 20° C.) using a hand mixer (500 rpm / 1 min), to obtain 200 g of a synthetic resin-inorganic mixture composition. Next, three polyurea test specimens were prepared by spraying polyurea onto one side of three 20 cm x 20 cm x 1 cm boards so that the thickness when dry was 2 mm; these were designated polyurea test specimen P1, polyurea test specimen P2, and polyurea test specimen P3. Example 2
[0036] Next, as a second embodiment, 20 g of the synthetic resin / inorganic mixed composition of Example 1 was applied with a brush to the surfaces of the polyurea test specimens P1, P2, and P3 of Example 1 and left at room temperature (about 20°C) for about 12 hours, and then 20 g of the synthetic resin / inorganic mixed composition of Example 1 was applied with a brush to the surface of the polyurea test specimen P1 and left at room temperature (about 20°C) for about 12 hours, and then a combustion experiment was performed in an in-house laboratory as described below. (A1) Product name: Polyurea test specimen P1 (A2) Test item: Flammability (A3) Test method: JIS L1091A-2 method (45° Meckel burner method) Evaluation criteria (if the following criteria are met, the product is considered non-flammable) ·Afterflame time: 10 seconds or less ⇒If a flame does occur, remove the burner and extinguish it within 10 seconds. Evaluation that there is no problem Afterglow time: 30 seconds or less ⇒Even if smoldering occurs, it is considered to be no problem as long as it lasts for less than 30 seconds. ·Carbonized area: 70cm2 or less No flames or smoldering should be observed 15 minutes after heating has ended. (A4) Test items (A5) Test results Flammability (2 minutes heating: afterflame time [seconds])────────────0 seconds There was no combustion. Flammability (2 minutes heating: afterflame time + afterglow time)────────0 seconds There was no combustion. Flammability (2 minutes heating: burning area [cm2])──────────101cm2 ⇒Although it did not meet the evaluation standard of 70cm2 or less, organic materials As a result, flame retardancy was recognized. Flammability (After 6 seconds of heating: Afterflame time [seconds])─────────0 seconds ⇒ Flame occurred but no combustion occurred. Flammability (heating for 6 seconds after ignition: afterflame time + afterglow time)──────0 seconds ⇒ Flame occurred but no combustion occurred. Flammability (heating for 6 seconds after ignition: burning area [cm2])───────23cm2 ⇒The standard of 70cm2 or less was achieved. Flammability (smoldering after heating (minutes))───────────60 minutes ⇒The standard of no flames or smoldering 15 minutes after heating ended was not met. ※comprehensive evaluation Since it was not possible to satisfy all of the above evaluation criteria, the polyurea test specimen P1 is not evaluated as a non-combustible material. However, since it was found to be non-combustible in the above four items, it is judged to be a flame-retardant material, taking into account that it is an organic material. Example 3
[0037] Next, as a third embodiment, 30 g of the non-flammable water-based adhesive of Example 1 was applied with a brush to the surfaces of polyurea test specimens P2 and P3 of Example 2, and then left at room temperature (approximately 20°C) for approximately 12 hours, after which a combustion experiment was conducted in an in-house laboratory as described below. (B1) Product name: Polyurea test specimen P2 (B2) Test item: Flammability (B3) Test method: JIS L1091A-2 method (45° Meckel burner method) Evaluation criteria (if the following criteria are met, the product is considered non-flammable) ·Afterflame time: 10 seconds or less ⇒If a flame does occur, there is no problem as long as you remove the burner and extinguish the flame within 10 seconds. The evaluation is Afterglow time: 30 seconds or less ⇒Even if smoldering occurs, it is considered to be no problem as long as it lasts for less than 30 seconds. ·Carbonized area: 70cm2 or less No flames or smoldering should be observed 15 minutes after heating has ended. (B4) Test items (B5) Test results Flammability (2 minutes heating: afterflame time [seconds])────────────0 seconds There was no combustion. Flammability (2 minutes heating: afterflame time + afterglow time)─────────0 seconds There was no combustion. Flammability (2 minutes heating: burning area [cm2])──────────41cm2 ⇒The standard of a carbonized area of 70 cm2 or less is met. Flammability (heating for 6 seconds after ignition: afterflame time [seconds])─────────No ignition ⇒Evaluation: Almost non-flammable Flammability (heating for 6 seconds after ignition: afterflame time + afterglow time)──────No ignition ⇒Evaluation: Almost non-flammable Flammability (heating for 6 seconds after ignition: burning area [cm2]) ───────No ignition ⇒Evaluation: Almost non-flammable Flammability (smoldering after heating (minutes))───────────10 minutes ⇒The criterion of no flames or smoldering 15 minutes after heating ended was met. ※comprehensive evaluation Since all of the above evaluation criteria are satisfied, the polyurea test specimen P2 is judged to be a noncombustible material. Example 4
[0038] Next, as a fourth embodiment, 30 g of the non-flammable water-based adhesive of Example 1 was applied with a brush to the surface of the polyurea test specimen P3 of Example 3, and then the specimen was left at room temperature (approximately 20°C) for approximately 12 hours, after which a combustion experiment was conducted in the in-house laboratory as described below. (C1) Product name: Polyurea test piece P3 (C2) Test item: Flammability (C3) Test method: JIS L1091A-2 method (45° Meckel burner method) Evaluation criteria (if the following criteria are met, the product is considered non-flammable) ·Afterflame time: 10 seconds or less ⇒Even if a flame does occur, if it goes out within 10 seconds after removing the burner, there is no problem. Afterglow time: 30 seconds or less ⇒Even if smoldering occurs, it is considered to be no problem as long as it lasts for less than 30 seconds. ·Carbonized area: 70cm2 or less No flames or smoldering should be observed 15 minutes after heating has ended. (C4) Test items (C5) Test results Flammability (2 minutes heating: afterflame time [seconds])────────────0 seconds There was no combustion. Flammability (2 minutes heating: afterflame time + afterglow time)─────────0 seconds There was no combustion. Flammability (2 minutes heating: burning area [cm2])──────────41cm2 ⇒The standard of a carbonized area of 70 cm2 or less is met. Flammability (heating for 6 seconds after ignition: afterflame time [seconds])─────────No ignition ⇒Evaluation: Almost non-flammable Flammability (heating for 6 seconds after ignition: afterflame time + afterglow time)──────No ignition ⇒Evaluation: Almost non-flammable Flammability (heating for 6 seconds after ignition: burning area [cm2]) ───────No ignition ⇒Evaluation: Almost non-flammable Flammability (smoldering after heating (minutes))───────────5 minutes ⇒The criterion of no flames or smoldering 15 minutes after heating ended was met. ※comprehensive evaluation As it meets all the above evaluation criteria, the polyurea specimen P3 is judged to be a non-combustible material. It is the most non-combustible of the three specimens tested. [Industrial Applicability]
[0040] The materials used in the method for making polyurea resin flame retardant of the present invention can also be applied to other fields where materials are easily combustible, and therefore it can be determined that the materials have great industrial applicability.
Claims
1. A method for making a polyurea resin flame retardant, comprising: applying a polyurea resin to an object of any shape or any dimension, curing the applied polyurea resin, applying a predetermined amount of a flame retardant adhesive composition that makes the polyurea resin-coated surface flame retardant and thoroughly drying the applied surface, and then applying a predetermined amount of a flame retardant adhesive composition that makes the inside or surface of the flame retardant adhesive composition-coated body flame retardant, thereby making the inside of the flame retardant adhesive composition-coated body and the surface of the flame retardant adhesive composition-coated body flame retardant.
2. 2. The method for making a polyurea resin flame retardant according to claim 1, wherein the flame retardant adhesive composition comprises a synthetic resin binder, an inorganic porous powder, and an auxiliary substance.
3. 2. The method for making a polyurea resin flame retardant according to claim 1, wherein the flame retardant adhesive composition is composed of an aqueous inorganic binder, an inorganic porous powder or an organic powder, and an auxiliary substance.
4. The method for making a polyurea resin fireproof according to claim 2 or 3, characterized in that the inorganic porous powder is at least one type selected from the group consisting of powders of diatomaceous earth, montmorillonite, zeolite, volcanic ash, perlite, foamed glass, cement, coal ash, vermiculite, and fired shells.
5. The method for making a polyurea resin fireproof according to claim 3, characterized in that the organic powder is at least one type selected from the group consisting of powders of plants, sintered plant charcoal, pulp, dietary fiber, plastics, and the like.
6. 4. The method for making a polyurea resin flame retardant according to claim 2, wherein the auxiliary substance is at least one selected from the group consisting of a viscosity modifier, a hardener, and a colorant.