Coating and bearing

A Cr-based base layer and DLC surface layer coating for bearings addresses the issues of brittleness and adhesion in existing coatings, effectively preventing electrolytic corrosion and ensuring robust protection against high motor voltages.

JP2024164642AActive Publication Date: 2024-11-27KOBE STEEL LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023080269
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-15
Publication Date
2024-11-27
Estimated Expiration
2043-05-15

AI Technical Summary

Technical Problem

Existing coatings for bearings, such as those described in Patent Documents 1, 2, and 3, are either brittle and difficult to handle or lack clear specifications for preventing electrolytic corrosion, particularly under varying motor voltages and environmental conditions, and suffer from insufficient adhesion to steel materials.

Method used

A coating comprising a Cr base layer with a thickness of 100 nm or more and a diamond-like carbon (DLC) surface layer with a plastic deformation hardness of 12 to 20 GPa, applied using unbalanced magnetron sputtering and plasma CVD methods, to enhance adhesion and prevent electrolytic corrosion.

Benefits of technology

The coating effectively suppresses electrolytic corrosion in steel materials by ensuring practical adhesion and maintaining a sufficient dielectric breakdown voltage, even under high motor voltages, thereby protecting bearings from damage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024164642000001_ABST
    Figure 2024164642000001_ABST
Patent Text Reader

Abstract

To provide a coating that can suppress generation of electric corrosion in a steel stock and has practically sufficient adhesion with respect to a steel stock.SOLUTION: A coating for a steel stock includes: a ground layer; and a surface layer formed on an upper side of the ground layer. The ground layer comprises Cr and has a thickness of 100 nm or more. The surface layer comprises diamond-like carbon and has plastic deformation hardness of 12-20 GPa.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating for steel and to a bearing having said coating. [Background technology]

[0002] Currently, in the field of automobiles and the like, drive devices are being shifted from internal combustion engines to electric motors such as motors worldwide in order to reduce the generation of greenhouse gases. At the same time, efforts are being made to shorten the charging time of rechargeable batteries for electric motors and to increase the drive voltage of electric motors in order to increase the output of electric motors. As motor drive voltages continue to increase in the future, it is predicted that the frequency of so-called electrolytic corrosion will increase in bearings such as ball bearings that support the rotating shaft of the motor.

[0003] Electrical corrosion is a phenomenon in which, when an electric current passes through the inside of a rotating bearing, sparks are generated at the point where the bearing race and rolling elements come into contact, causing the surfaces of the race and rolling elements at the contact point to melt and become damaged.

[0004] There are two ways to prevent the occurrence of electrolytic corrosion: to prevent current from flowing through the bearing, and to prevent the bearing itself from passing current. One way to prevent current from flowing through the bearing is to bypass it using an earth ring or the like. Another way to prevent current from flowing through the bearing itself is to use an insulating material such as ceramic for the rolling elements, or to coat the outer ring, which together with the inner ring constitutes the raceway, with an insulating film. Another method is to inject highly conductive lubricating oil between the raceway and the rolling elements to prevent sparks from occurring inside the bearing.

[0005] As a method for preventing current from flowing through a bearing, for example, Patent Document 1 discloses a coating method for a bearing in which at least one of an outer ring and an inner ring of a bearing that are arranged concentrically with each other are made of metal and are coated with an insulating film, characterized in that a mixed spray material is carried out in which aluminum oxide powder having an average particle size of 1 μm or more and less than 30 μm is added to silicon carbide powder having an average particle size of 2 μm or more and less than 10 μm and / or aluminum nitride powder having an average particle size of 2 μm or more and less than 10 μm in an amount of 2 to 40 mass % in total to form the insulating film on the outer ring and / or the inner ring.

[0006] Patent Document 2 discloses a method for manufacturing an insulated rolling bearing for preventing electrolytic corrosion, which comprises a metal outer ring with an outer ring raceway formed on its inner peripheral surface, a metal inner ring arranged inside the outer ring and with an inner ring raceway formed on its outer peripheral surface, and a plurality of rolling elements, each made of metal, arranged so as to be able to roll between the outer ring raceway and the inner ring raceway, and which is formed with an insulating coating, the method comprising: spraying an electrofusible material granulated to a particle size distribution of 10 to 70 μm and containing zirconia in a ratio of 5% by mass to 40% by mass of alumina onto at least the outer peripheral surface of the surface of the outer ring excluding the outer ring raceway to form a sprayed coating, and then filling pores in the sprayed coating with a sealing agent to perform a sealing treatment.

[0007] In addition, in Patent Document 3, a rolling bearing that can prevent electrolytic corrosion even when used in a motor that generates shaft voltage, and that does not cause a decrease in rotational accuracy, is provided with a surface resistance of 10 6 A rolling bearing is disclosed which is characterized in that a diamond-like carbon (DLC) layer of Ω or more is formed. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2017-53481 A [Patent Document 2] JP 2015-212576 A [Patent Document 3] JP 2006-226500 A Summary of the Invention [Problem to be solved by the invention]

[0009] The insulating film disclosed in Patent Document 1 and the insulating coating disclosed in Patent Document 2 are formed by thermal spraying of raw materials. Coatings formed by thermal spraying have the problem of being brittle and difficult to handle. On the other hand, the DLC layer disclosed in Patent Document 3 is formed mainly by sputtering and is easier to handle than coatings formed by thermal spraying.

[0010] Patent Document 3 discloses, as an example, the relationship between the plastic deformation hardness and the volume resistivity of the DLC layer. However, Patent Document 3 does not disclose any specific thickness, sheet resistivity, volume resistivity, or voltage at which the DLC layer is broken down by a spark (hereinafter also referred to as "breakdown voltage"), etc., for any of the DLC layers in the examples and comparative examples used to examine the occurrence of electrolytic corrosion, and the specific conditions for preventing the occurrence of electrolytic corrosion were not clear. Patent Document 3 also discloses the provision of a chromium underlayer and a chromium carbide intermediate layer between the film-forming object and the DLC layer, but does not disclose the role of these layers, their effect on electrolytic corrosion, or their specific thickness.

[0011] Furthermore, the inventors' investigations revealed that the conditions under which electrolytic corrosion occurs vary depending on the voltage applied to the motor, the environment in which the motor and bearing are placed, the capacity of the battery connected to the motor, etc., and that it is difficult to specifically determine the thickness of the DLC layer and the dielectric breakdown voltage that can prevent electrolytic corrosion. Also, it was found that not only when the DLC layer is provided directly on the surface of the bearing, but also when a coating having some kind of underlayer is provided between the DLC layer and the surface of the bearing, the adhesion of the coating including the DLC layer and the underlayer to the bearing is practically insufficient depending on the type and thickness of the underlayer.

[0012] The present invention has been made in view of these problems, and has an object to provide a coating that can suppress the occurrence of electrolytic corrosion in steel material and has sufficient adhesion to the steel material for practical use, and also to provide a bearing having such a coating. [Means for solving the problem]

[0013] As a result of extensive investigations, the present inventors have found that the above object can be achieved by the following invention.

[0014] A coating according to one aspect of the present invention is a coating for a steel material, A substrate having a base layer and a surface layer formed on an upper side of the base layer, The underlayer is made of Cr and has a thickness of 100 nm or more. The surface layer is made of diamond-like carbon and has a plastic deformation hardness of 12 to 20 GPa.

[0015] In a bearing according to another aspect of the present invention, the coating is formed on at least a portion of the surface. Effect of the Invention

[0016] According to the present invention, it is possible to provide a coating that can suppress the occurrence of electrolytic corrosion in steel material and has sufficient adhesion to the steel material for practical use, and also to provide a bearing having such a coating. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic diagram of a coating according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of a bearing according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a schematic diagram of an apparatus for forming an underlayer. [Figure 4] FIG. 4 is a schematic diagram of an apparatus for forming a surface layer. [Diagram 5]FIG. 5 is a schematic diagram of a breakdown voltage measuring device used for measuring the breakdown voltage. [Figure 6] FIG. 6 is a graph showing the relationship between the plastic deformation hardness of the surface layer and the dielectric breakdown voltage per 1 μm of thickness. [Figure 7] FIG. 7 is a graph showing the relationship between the thickness of the surface layer and the dielectric breakdown voltage. [Figure 8] FIG. 8 is a graph showing the relationship between the thickness of the underlayer and the dielectric breakdown voltage. [Figure 9] 9(a) to (d) are photographs showing the state of the underlayer after the scratch test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS A coating and a bearing according to an embodiment of the present invention will be described below with reference to the drawings.

[0019] <Coating composition> Fig. 1 is a schematic diagram of a coating according to this embodiment. The coating 1 according to this embodiment is a coating for a steel material, and has a base layer 2 and a surface layer 3 formed on the upper side of the base layer, the base layer 2 being made of Cr and having a thickness of 100 nm or more, and the surface layer 3 being made of diamond-like carbon and having a plastic deformation hardness of 12 to 20 GPa. By providing the coating 1 on the surface of the steel material, it is possible to suppress the occurrence of electrolytic corrosion in the steel material. Furthermore, the coating 1 has sufficient adhesion to the steel material for practical use.

[0020] The coating 1 is formed on the surface of a steel material 4. The application and chemical composition of the steel material are not particularly limited. When the coating 1 is used for a bearing such as a ball bearing, for example, the steel material may be SUJ2 to SUJ5 as specified in JIS G 4805:2019 (high carbon chromium bearing steel material).

[0021] The underlayer 2 is made of Cr (chromium) and has a thickness of 100 nm or more. The underlayer 2 is disposed between the steel material 4 and the surface layer 3. The underlayer 2 has high adhesion to both the steel material 4 and the surface layer 3. Therefore, the coating 1 according to this embodiment has high adhesion to the steel material 4 compared to a case in which the surface layer 3 is formed directly on the surface of the steel material 4.

[0022] The thickness of the underlayer 2 is 100 nm or more. If the thickness of the underlayer 2 is less than 100 nm, sufficient adhesion of the coating 1 cannot be obtained. From the viewpoint of increasing the dielectric breakdown voltage of the coating 1, the thickness of the underlayer 2 is preferably 200 nm or less, and more preferably close to 100 nm.

[0023] The surface layer 3 is made of diamond-like carbon (DLC) and has a plastic deformation hardness of 12 to 20 GPa. By setting the plastic deformation hardness of the surface layer 3 to 12 to 20 GPa, the dielectric breakdown voltage per 1 μm of thickness of the surface layer 3 can be set to 35 V / μm or more. As a result of studies by the present inventors, it has been found that the occurrence of electrolytic corrosion in the steel material 4 on which the coating 1 is formed can be suppressed by setting the dielectric breakdown voltage per 1 μm of thickness of the surface layer 3 to 35 V / μm or more.

[0024] The plastic deformation hardness of the surface layer 3 is preferably 13 GPa or more. This can further suppress the occurrence of electrolytic corrosion in the steel material 4 on which the coating 1 is formed. The plastic deformation hardness of the surface layer 3 is more preferably 14 GPa or more. This can further suppress the occurrence of electrolytic corrosion in the steel material 4. Furthermore, the plastic deformation hardness of the surface layer 3 is preferably 17 GPa or less. This can further suppress the occurrence of electrolytic corrosion in the steel material 4. The plastic deformation hardness of the surface layer 3 is more preferably 15 GPa or less. This can further suppress the occurrence of electrolytic corrosion in the steel material 4.

[0025] Furthermore, if the plastic deformation hardness of the surface layer 3 is insufficient, the surface layer 3 may be damaged, for example, when a bearing on which the coating 1 is formed is incorporated into a bearing support member installed inside an automobile or into a rotating shaft of a motor. However, the plastic deformation hardness of the surface layer 3 in this embodiment is 12 GPa or more, which is harder than the plastic deformation hardness of 8.5 GPa of the above-mentioned SUJ2, and therefore such damage can be suppressed.

[0026] In this embodiment, "plastic deformation hardness" refers to a numerical value calculated from the load applied to an indenter and the indentation depth of the indenter when an indenter of a predetermined shape is pressed against a measurement object with a specified load to plastically deform the measurement object, and can be measured by a nanoindentation test.

[0027] The thickness of the surface layer 3 may be determined according to the actual use environment of the product on which the coating 1 is formed. The thickness of the surface layer 3 is preferably 1 to 10 μm. If the thickness of the surface layer 3 is 1 μm or more, the surface layer 3 has a sufficient dielectric breakdown voltage of 60 V or more. The thicker the surface layer 3, the higher the dielectric breakdown voltage of the surface layer 3 and the coating 1, so a thicker surface layer 3 is preferable. If the surface layer 3 has a sufficient dielectric breakdown voltage, the insulating performance of the coating 1 is improved, and damage to the coating 1 can be suppressed even if electrolytic corrosion occurs in the steel material 4. However, the thicker the surface layer 3, the longer it takes to form the surface layer 3, so the thickness of the surface layer 3 is preferably 10 μm or less.

[0028] Bearing structure 2 is a cross-sectional view of the bearing according to this embodiment. The bearing 30 is a so-called rolling bearing, specifically a ball bearing. The bearing 30 has an inner ring 31 and an outer ring 33 constituting raceways, and a spherical rolling element 32 sandwiched between the raceways. The bearing 30 is used to support a rotating shaft of a motor inside an automobile or the like. An outer peripheral surface 33a of the outer ring 33 of the bearing 30 is supported by a support member (not shown) provided inside the automobile or the like. The inner ring 31 of the bearing 30 supports the rotating shaft of the motor (not shown) by means of the inner ring 31.

[0029] In the bearing 30 according to the present embodiment, the coating is formed on at least a part of the surface. In the bearing 30, the coating may be formed at any location, and is preferably formed on the surface of the outer ring 33. When formed on the surface of the outer ring 33, the coating may be formed on the entire surface of the outer ring 33. In addition, the coating may be formed on the outer peripheral surface 33a of the outer ring 33. By forming the coating at least on the outer peripheral surface 33a of the outer ring 33, it is possible to block leakage current flowing from the motor to a support member inside an automobile or the like, and it is possible to suppress the occurrence of electrolytic corrosion between the inner ring 31 and the outer ring 33 constituting the raceway and the spherical rolling element 32 sandwiched between the raceway.

[0030] <Method of producing the coating> A method for producing the coating according to the present embodiment will be described below. Note that the method for producing the coating is not limited to the following method.

[0031] FIG. 3 is a schematic diagram of an apparatus for forming an underlayer, and FIG. 4 is a schematic diagram of an apparatus for forming a surface layer. The underlayer of the coating according to this embodiment can be manufactured using an unbalanced magnetron sputtering (UBMS) apparatus 10 shown in FIG. 3. The UBMS apparatus 10 includes a chamber 11, a cathode 13 and a stage 16 disposed in the chamber 11, a sputtering power supply 12 connected to the cathode 13, and a bias power supply 15 connected to the stage 16. The chamber 11 has an inlet 11a through which a process gas 18 is introduced, and an exhaust outlet 11b through which an exhaust gas 19 is exhausted. The cathode 13 has a plurality of magnets 13a, 13b, and 13c disposed so as to be exposed in a line on the surface of the cathode 13, and a plate-shaped target 14 made of Cr is disposed on the surface of the cathode 13. A substrate 17 made of a steel material is disposed on the stage 16.

[0032] In the UBMS apparatus 10, when voltages are applied to the sputtering power supply 12 and the bias power supply 15 and Ar (argon) gas, which is the process gas 18, is introduced, Ar atoms 18a collide with the target 14, ejecting Cr ions 14a, which are then adsorbed onto the substrate 17, forming a base layer.

[0033] The conditions for forming the underlayer can be set, for example, as follows: the power of the sputtering power supply 12 can be 2 kW, the bias voltage applied to the bias power supply 15 can be 50 V, and the pressure of the process gas 18 (argon gas) in the chamber 11 can be 0.6 Pa. These values ​​are merely examples and can be changed depending on the thickness of the underlayer to be formed and the size and shape of the substrate.

[0034] The surface layer of the coating according to this embodiment can be formed using a plasma CVD (Chemical Vapor Deposition) apparatus 20 shown in Fig. 4. The plasma CVD apparatus 20 includes a chamber 21, a high-frequency application electrode 23 and a stage 26 disposed within the chamber 21, a high-frequency power supply 22 connected to the high-frequency application electrode 23, and a bias power supply 25 connected to the stage 26. The chamber 21 has an inlet 21a through which a source gas 28 is introduced, and an exhaust port 21b through which an exhaust gas 29 is exhausted. A substrate 27 on which a base layer 27a is formed is disposed on the stage 26. When forming a surface layer made of diamond-like carbon according to this embodiment, CH is used as the source gas 28. 4 (Methane), C 2 H 2 (Acetylene), C 7 H 8 A hydrocarbon gas such as (toluene) can be used.

[0035] In the plasma CVD apparatus 20, when a voltage is applied to the high-frequency power supply 22 and the bias power supply 25 and the raw material gas 28 is introduced, the raw material gas 28 is converted into plasma, and the plasma 28a is adsorbed onto the base layer 27a of the substrate 27, and a surface layer made of diamond-like carbon is formed on the base layer 27a.

[0036] The conditions for forming the surface layer can be set as follows, for example: the power frequency of the high frequency power source 22 is 300 kHz, the bias voltage applied to the bias power source 25 is 600 V, and the pressure of the source gas 28 in the chamber 21 is CH 4 or C 2H 2 In this case, the pressure can be 5 to 10 Pa. These values ​​and gas types are merely examples, and can be changed depending on the thickness of the surface layer to be formed, the size and shape of the substrate, etc.

[0037] Furthermore, the plastic deformation hardness of the surface layer, i.e., the diamond-like carbon, can be controlled by the pressure and gas species of the source gas 28 in the chamber 21. Specifically, the surface layer can be hardened by lowering the pressure of the source gas 28. Furthermore, a gas species having a larger number of carbon atoms constituting the gas molecules of the source gas 28 has a larger change in the plastic deformation hardness of the diamond-like carbon with a change in pressure than a gas species having a smaller number of carbon atoms.

[0038] Summary of the disclosed technology As described above, this specification discloses various aspects of the technology, the main technologies of which are summarized below.

[0039] As described above, a coating according to one aspect of the present invention is a coating for a steel material, and has a base layer and a surface layer formed on the upper side of the base layer, the base layer being made of Cr and having a thickness of 100 nm or more, and the surface layer being made of diamond-like carbon and having a plastic deformation hardness of 12 to 20 GPa.

[0040] According to this configuration, it is possible to suppress the occurrence of electrolytic corrosion in the steel material, and to obtain a coating having sufficient adhesion to the steel material for practical use.

[0041] In the coating having the above configuration, the surface layer preferably has a thickness of 1 to 10 μm.

[0042] According to this configuration, the coating can have a sufficient dielectric breakdown voltage, and even if electrolytic corrosion occurs, damage to the coating can be suppressed.

[0043] In the coating having the above configuration, the underlayer preferably has a thickness of 200 nm or less.

[0044] This configuration makes it possible to increase the dielectric breakdown voltage of the coating.

[0045] The coating of the above configuration may be formed on a steel bearing.

[0046] As described above, in a bearing according to another aspect of the present invention, the coating is formed on at least a portion of the surface. EXAMPLES

[0047] The thickness, plastic deformation hardness, dielectric breakdown voltage and adhesion of the undercoat layer and surface layer formed on the surface of the steel material were measured or evaluated.

[0048] Samples Used The following specimens were prepared: specimen A, in which only a surface layer made of diamond-like carbon was formed directly on the surface of the steel material; specimen B, in which a base layer made of Cr and a surface layer made of diamond-like carbon were formed on the surface of the steel material; and specimen C, in which only a base layer made of Cr was formed on the surface of the steel material.

[0049] Sample A was used for the evaluation of plastic deformation hardness. Samples A and B were used for the evaluation of dielectric breakdown voltage. Sample C was used for the evaluation of adhesion.

[0050] The steel material for each sample was a steel plate made of SUJ2 specified in JIS G 4805:2019, with a thickness of 5 mm and a diameter of 50 mm.

[0051] The underlayers of Samples B and C were formed using the UBMS apparatus shown in Fig. 3. The conditions for forming the underlayers were as follows.

[0052] Sputtering power: 2kW Bias voltage: 50V Process gas: Ar Process gas pressure: 0.6Pa The surface layers of Sample A and Sample B were formed using the plasma CVD apparatus shown in Figure 4. The conditions for forming the surface layers were as follows: The surface layer of Sample A was formed on a base layer.

[0053] Power frequency: 300kHz Bias voltage: 600V Feed gas: CH 4 , C 2 H 2 Raw gas pressure: 5~10Pa Measurement and evaluation methods for each characteristic (Thickness measurement method) The thickness of the surface layer of Sample A and the thickness of the underlayer of Sample C were measured by the following method. A surface layer or underlayer was formed on a steel plate partially masked, and the masking was then removed. The height of the step formed between the part where the masking was removed and the part where the surface layer or underlayer was formed was measured with a stylus-type step gauge, and this height was regarded as the thickness of the surface layer or underlayer.

[0054] The thickness of the undercoat layer and the surface layer of the above sample B was measured by the following method. First, a undercoat layer was formed on a steel plate with two maskings, and then one of the maskings was removed and a surface layer was formed on the steel plate and on the undercoat layer. The height of the step formed between the remaining part where the masking was removed and the part where only the undercoat layer was formed or the part where only the surface layer was formed was measured, and this height was regarded as the thickness of the undercoat layer or the surface layer.

[0055] (Method of measuring plastic deformation hardness) The plastic deformation hardness was measured by a nanoindentation test using the above-mentioned sample A. The nanoindentation tester used was a product of Elionix Co., Ltd. The indenter used was a triangular pyramid Berkovich indenter, and the load was 10 mN.

[0056] (Method of measuring dielectric breakdown voltage) The dielectric breakdown voltage was measured using the above-mentioned Sample A and Sample B in accordance with JIS C 2110-1:2016 (Solid electrical insulating materials - Test methods for dielectric breakdown strength - Part 1: Tests using applied power frequency AC voltage).

[0057] FIG. 5 is a schematic diagram of a breakdown voltage measuring device used to measure the breakdown voltage. The breakdown voltage measuring device 40 has a stage 41 made of a metal plate, a metal ball 45, a weight 42 provided on the upper part of the metal ball 45 via a metal rod 46, an electrode 43 connected to the stage 41, and an electrode 44 connected to the metal rod 46. The sample S in the figure is the above-mentioned sample A or sample B, and is sandwiched between the stage 41 and the metal ball 45 so that the surface layer faces the metal ball 45. The voltage applied to the sample S sandwiched between the stage 41 and the metal ball 45 was increased at a voltage increase rate of 10 V / s, and the voltage at which the current value reached 1 mA was defined as the breakdown voltage.

[0058] (Method of evaluating adhesion) The adhesion was evaluated by a scratch test using the above-mentioned sample C. Specifically, the scratch test was performed by placing sample C on a stage with the base layer facing up and placing a needle on the base layer. The needle was moved over the base layer at 10 mm / min, and the load on the needle was increased from 0 N to 100 N over 1 minute. The load at which the base layer started to peel (hereinafter referred to as the "peeling start load") and the observed peeling state of the base layer were used to evaluate the adhesion. The peeling start load was calculated from the length of the scratch mark made by the needle.

[0059] <Measurement and evaluation results of each characteristic> (Surface thickness, plastic deformation hardness and dielectric breakdown voltage of sample A) For sample A, several types of samples (samples No. A1 to A11) were prepared with a surface layer made of diamond-like carbon formed on the surface of the steel sheet by changing the gas type and pressure of the raw material gas. The gas type and pressure used in the preparation of each sample and the measurement results of each characteristic are shown in Table 1. A surface layer was deemed to have passed if it had a dielectric breakdown voltage of 35 V / μm or more per 1 μm of thickness, which is capable of suppressing the occurrence of electrolytic corrosion in the coating.

[0060] [Table 1]

[0061] Figure 6 is a graph showing the relationship between the plastic deformation hardness of the surface layer and the dielectric breakdown voltage per 1 μm of thickness obtained from the results shown in Table 1. It was found from Table 1 and Figure 6 that if the plastic deformation hardness of the surface layer is 12 to 20 GPa, the dielectric breakdown voltage per 1 μm of thickness of the surface layer can be passed with a value of 35 V / μm or more.

[0062] It was also found that by setting the plastic deformation hardness of the surface layer to 13 GPa or more or 17 GPa or less, the dielectric breakdown voltage per 1 μm of thickness can be made 60 V / μm or more. Furthermore, it was found that by setting the plastic deformation hardness of the surface layer to 14 GPa or more or 15 GPa or less, the dielectric breakdown voltage per 1 μm of thickness can be made 80 V / μm or more.

[0063] Also, CH 4 Compared to C 2 H 2 It was found that the change in the plastic deformation hardness of the surface layer due to the change in gas pressure was greater in the case of

[0064] Figure 7 is a graph showing the relationship between the thickness of the surface layer and the dielectric breakdown voltage obtained from the results shown in Table 1. From Figure 7, it was found that when the plastic deformation hardness of the surface layer is 13 GPa or more and 17 GPa or less, the dielectric breakdown voltage of the surface layer is proportional to the thickness of the surface layer. In addition, from the approximation line of the measurement results shown in Figure 7, it was found that when the thickness of the surface layer is 1 μm or more, the dielectric breakdown voltage is 60 V or more.

[0065] (Thickness of surface layer and underlayer and breakdown voltage of sample B) For sample B, several types of samples (samples B1 to B4) were prepared by changing the thickness of the underlayer made of Cr formed on the steel sheet surface. 2 H 2 The pressure of the raw material gas was set at 10 Pa. Table 2 shows the measurement results for each sample, including the thickness of the underlayer, the thickness of the surface layer, the total thickness of the underlayer and the surface layer, the combined dielectric breakdown voltage of the underlayer and the surface layer, the dielectric breakdown voltage per μm of surface layer thickness, and the dielectric breakdown voltage per μm of the combined thickness of the underlayer and the surface layer.

[0066] [Table 2]

[0067] FIG. 8 is a graph showing the relationship between the thickness of the underlayer and the dielectric breakdown voltage obtained from the results shown in Table 2. From FIG. 8, it was found that in the range of underlayer thickness of 200 nm or less, the thinner the underlayer, the higher the dielectric breakdown voltage. Also, from Table 2, it was found that in the range of underlayer thickness of 200 nm or less, it is possible to obtain a dielectric breakdown voltage per 1 μm of surface layer thickness that satisfies the pass value, and that the thinner the underlayer, the higher the dielectric breakdown voltage per 1 μm of surface layer thickness. The same is true for the dielectric breakdown voltage per 1 μm of the total thickness of the surface layer and underlayer.

[0068] (Adhesion of the undercoat layer of sample C) For sample C, several types of samples (samples No. C1 to C4) were prepared by varying the thickness of the underlayer made of Cr. Table 3 shows the measurement results of the underlayer thickness and peeling start load for each sample. Figure 9 is a photograph showing the state of the underlayer of each sample after the scratch test. Figure 9(a) is a photograph of sample No. C1, Figure 9(b) is a photograph of sample No. C2, Figure 9(c) is a photograph of sample No. C3, and Figure 9(d) is a photograph of sample No. C4.

[0069] [Table 3]

[0070] From Table 3, it was found that there was no significant difference in the peeling load depending on the thickness of the base layer. On the other hand, when the base layer was 100 nm or more as shown in Figures 9(b) to (d), no significant peeling was observed around the scratch mark, whereas when the base layer was less than 100 nm as shown in Figure 9(a), large, scaly peeling was clearly observed around the scratch mark as shown in the area surrounded by ellipse A. From these results, it was found that the thickness of the base layer must be 100 nm or more to obtain sufficient adhesion to steel.

[0071] The measurement results for samples B and C showed that although a thinner underlayer can increase the breakdown voltage per 1 μm of surface layer thickness, taking adhesion into consideration, the underlayer needs to be 100 nm or thicker. [Explanation of symbols]

[0072] 1 coating 2 Base layer 3 Surface layer 4 Steel material 30 Bearings

Claims

1. A coating for steel, comprising: A substrate having a base layer and a surface layer formed on an upper side of the base layer, The underlayer is made of Cr and has a thickness of 100 nm or more. The surface layer is made of diamond-like carbon and has a plastic deformation hardness of 12 to 20 GPa.

2. The coating according to claim 1, wherein the surface layer has a thickness of 1 to 10 μm.

3. The coating of claim 1 , wherein the underlayer has a thickness of 200 nm or less.

4. The coating of claim 1 formed on a steel bearing.

5. A bearing having the coating according to any one of claims 1 to 4 formed on at least a part of its surface.

Citation Information

Patent Citations

  • Rolling slide member

    JP2002349577A

  • Amorphous hard carbon film and sliding member using the same

    JP2003293136A

  • Rolling bearing

    JP2006226500A

  • Ball joint and method of manufacturing the same

    JP2014211190A

  • Piston ring

    JP2020200803A