Quantum dot electroluminescence element and method for manufacturing the same
The quantum dot electroluminescent device with a fluorine-treated metal oxide electron transport layer and organic intermediate layer addresses structural defects, achieving high efficiency and purity while enabling low-voltage light emission.
Patent Information
- Application Number
- JP2024027766
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-02-27
- Publication Date
- 2024-11-27
AI Technical Summary
Existing quantum dot electroluminescent devices face challenges in suppressing structural defects, leading to decreased luminous efficiency and color purity, and require high driving voltages for light emission.
A quantum dot electroluminescent device structure comprising a cathode, a fluorine-treated metal oxide electron transport layer, an organic intermediate layer, and a light-emitting layer with quantum dots, which facilitates efficient carrier recombination and low-voltage light emission through Auger recombination and upconversion processes.
The device achieves high luminous efficiency, high color purity, and low-voltage light emission by effectively reducing structural defects and utilizing organic materials to enhance carrier recombination and energy transfer.
Smart Images

Figure 2024164800000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a quantum dot electroluminescent device and a method for manufacturing the same. [Background technology]
[0002] In order to improve the color reproducibility of displays, quantum dot electroluminescent devices that emit light with high color purity have been attracting attention in recent years. Quantum dots are particles with a particle size of about several nm, and emit light (band edge emission) associated with electronic transition from the conduction band to the valence band. The color of the light emitted by quantum dots changes significantly depending on the particle size, and the smaller the particle size, the shorter the wavelength of light emitted. In general, organic materials have a large difference in structure between the ground state and the excited state, so the line width of the emission spectrum is large, whereas quantum dots have a small difference in structure between the ground state and the excited state, so they emit light with a narrow half-width. Therefore, in principle, quantum dot electroluminescent devices emit light with higher color purity than organic electroluminescent devices. However, if defects exist within or on the surface of quantum dot particles, in addition to band edge emission, emission originating from the defects is emitted at a different wavelength, resulting in a decrease in color purity. Thermal deactivation also occurs on the defects, resulting in a significant decrease in luminous efficiency. Furthermore, if there are structural defects in the carrier transport layer adjacent to the luminescent layer containing quantum dots, secondary emission and thermal deactivation occur at the interface between the luminescent layer containing quantum dots and the carrier transport layer, resulting in the same problem. Therefore, in order to obtain highly efficient and high color purity emission in quantum dot electroluminescent devices, it is necessary to sufficiently reduce the structural defect density of the quantum dots and the carrier transport material.
[0003] In response to this, core-shell quantum dots, in which the surface of the quantum dot is covered with a shell, are widely used to suppress light emission and thermal deactivation due to structural defects in the quantum dots (Non-Patent Document 1). In the core-shell quantum dots, the core of the light-emitting quantum dot is covered with a shell with a larger energy gap, so that the excitons generated within the quantum dot can be confined within the core, thereby suppressing deactivation due to defects on the quantum dot surface, and thus it is possible to obtain highly efficient light emission with high color purity. However, it is difficult to completely eliminate defects on the quantum dot surface, and with current technology, it is unavoidable to some extent to generate secondary emission components and thermal deactivation of excitons. In addition, perovskite quantum dot electroluminescent devices, which have attracted attention in recent years, require alternative means because perovskite quantum dots do not have a shell structure (Non-Patent Document 2).
[0004] On the other hand, zinc oxide (ZnO) is widely used in the electron transport layer of quantum dot electroluminescent devices with an inverted structure, but it has a problem that structural defects are easily generated. Therefore, magnesium-doped zinc oxide (ZnMgO) has recently been widely used (Non-Patent Document 3). When ZnMgO is used in the electron transport layer, the band gap is wider than when ZnO is used, so it is less susceptible to the influence of structural defects and the luminous efficiency is improved. However, even if ZnMgO is used in the electron transport layer, it is still difficult to completely eliminate the influence of defects.
[0005] In addition, in recent years, in order to realize a society with a low environmental load, it is also desirable to reduce the power consumption of displays. In the electroluminescent element described above, in order to reduce the power consumption, it is effective to reduce the driving voltage, and various researches are being conducted to reduce the driving voltage of the element. Among such researches, electroluminescent elements that emit light at a voltage lower than the conventional theoretical limit have recently attracted attention. For example, in the following Non-Patent Documents 4 and 5, an ultra-low driving voltage is realized in an organic electroluminescent element by utilizing upconversion using triplet-triplet annihilation at an interface. In addition, in the following Non-Patent Document 6, an organic electroluminescent element, a quantum dot electroluminescent element, and an LED element that are driven at an ultra-low voltage are realized by transferring the energy obtained by recombination in the light-emitting layer to a charge carrier. In addition, in the following Non-Patent Document 7, a green-emitting perovskite quantum dot electroluminescent element that emits light at an ultra-low voltage is realized by upconversion using the energy of Auger recombination at an interface, and light emission is observed at 1.7V, which is lower than the band gap of the quantum dot, which is 2.3 eV. [Prior art documents] [Non-patent literature]
[0006] [Non-Patent Document 1] BO Dabbousi et al., “(CdSe)ZnS Core-Shell Quantum Dots: Synthesis and Characterization of a Size Series of Highly Luminescent Nanocrystallites”, Journal of Physical Chemistry B, 1997, 101, 9463-9475 [Non-Patent Document 2] Cunlong Li et al., “Highly pure green light emission of perovskite CsPbBr3 quantum dots and their application for green light-emitting diodes”, Optics Express, 2016, 24, 15071-15078 [Non-Patent Document 3] Di Zhang et al., “3-4: Highly Efficient Green Top-Emission Light-Emitting Diodes Based on Indium-Phosphide Quantum Dots”, SID 2022 DIGEST, 2022, 53, 9-11 [Non-Patent Document 4] “Efficient Interfacial Upconversion Enabling Bright Emission at an Extremely Low Driving Voltage in Organic Light-Emitting Diodes”,Advanced Optical Materials, vol. 10, 2101710 (2022) [Non-Patent Document 5] “Blue organic light-emitting diode with a turn-on voltage of 1.47 V”,Nature Communications, vol. 14, 5494 (2023) [Non-Patent Document 6] “Ultralow-voltage operation of light-emitting diodes”,Nature Communications, vol. 13, 3845 (2022) [Non-Patent Document 7] “Pure Formamidinium-Based Perovskite Light-Emitting Diodes with High Efficiency and Low Driving Voltage”,Advanced Materials, vol. 23, 1603826 (2017) Summary of the Invention [Problem to be solved by the invention]
[0007] As described above, existing methods are unable to sufficiently suppress the generation of secondary emission components and the decrease in luminous efficiency caused by structural defects in the quantum dots and the carrier transport layer. As described above, in electroluminescent elements, the use of upconversion makes it possible to emit light below the band gap. However, among electroluminescent elements, the light emission onset voltage that has been achieved in quantum dot electroluminescent elements is still high, and there is a demand for the realization of light emission at even lower voltages.
[0008] In view of these problems, the present invention aims to provide a quantum dot electroluminescent device that can suppress the effects of structural defects in the quantum dots and carrier transport layer and emit light with high luminous efficiency and high color purity. Another object of the present invention is to provide a quantum dot electroluminescence device capable of emitting light at a low voltage. A further object of the present invention is to provide a method for producing such a quantum dot electroluminescence device. [Means for solving the problem]
[0009] The quantum dot electroluminescence device and the method for producing the same according to the present invention that solve the above problems are outlined below.
[0010] [1] A cathode, an electron transport layer made of a metal oxide, an intermediate layer made of an organic material, a light emitting layer including quantum dots, and an anode, in this order; 3. A quantum dot electroluminescent device, wherein the electron transport layer is fluorine-treated. The quantum dot electroluminescence device of the present invention described in [1] above has high luminous efficiency and can emit light with high color purity. In addition, the quantum dot electroluminescence device described in [1] above can also emit light at a low voltage.
[0011] [2] The quantum dot electroluminescent device according to [1], wherein the organic material constituting the intermediate layer contains a pyridine ring. The quantum dot electroluminescent device described in [2] above has higher luminous efficiency and can emit light with higher color purity. In addition, the quantum dot electroluminescent device described in [2] above can emit light at a lower voltage.
[0012] [3] The quantum dot electroluminescent device according to [1] or [2], wherein the organic material constituting the intermediate layer has a triazine skeleton. The quantum dot electroluminescent device described in [3] above has higher luminous efficiency and can emit light with higher color purity. In addition, the quantum dot electroluminescent device described in [3] above can emit light at a lower voltage.
[0013] [4] The quantum dot electroluminescent device according to any one of [1] to [3], wherein the light-emitting layer further contains an organic material. The quantum dot electroluminescent device described in [4] above is capable of emitting light at a lower voltage.
[0014] [5] The quantum dot electroluminescent device according to [4], wherein the organic material contained in the light-emitting layer has a highest occupied molecular orbital (HOMO) level of 5.5 eV or less. The quantum dot electroluminescent device described in [5] above is capable of emitting light at even lower voltages.
[0015] [6] The quantum dot electroluminescent device according to [4] or [5], wherein the organic material contained in the light-emitting layer has a lowest unoccupied molecular orbital (LUMO) level of 3.1 eV or less. The quantum dot electroluminescent device described in [6] above is also capable of emitting light at an even lower voltage.
[0016] [7] The organic material contained in the light-emitting layer has the following structural formula: [ka] The quantum dot electroluminescent device according to any one of [4] to [6], wherein the quantum dot electroluminescent device is DIC-TRZ represented by the formula: The quantum dot electroluminescent device described in [7] above is capable of emitting light at an even lower voltage.
[0017] [8] forming a cathode; forming an electron transport layer made of a metal oxide; fluorinating the electron transport layer; forming an intermediate layer made of an organic material; forming a light-emitting layer including quantum dots; and forming an anode, in this order. According to the method for producing a quantum dot electroluminescence device of the present invention described in [8] above, a quantum dot electroluminescence device capable of emitting light with high luminous efficiency and high color purity can be obtained.
[0018] [9] The method for producing a quantum dot electroluminescence device according to [8], wherein in the step of fluorine-treating the electron transport layer, the electron transport layer is subjected to oxygen plasma treatment in an atmosphere of a fluorine source. According to the method for producing a quantum dot electroluminescence device described in [9] above, a quantum dot electroluminescence device capable of emitting light with higher luminous efficiency and higher color purity can be obtained. Effect of the Invention
[0019] According to the present invention, it is possible to provide a quantum dot electroluminescence device that has high luminous efficiency and is capable of emitting light with high color purity. Moreover, according to the present invention, it is possible to provide a quantum dot electroluminescence device capable of emitting light at a low voltage. Moreover, according to the present invention, a method for producing such a quantum dot electroluminescence device can be provided. [Brief description of the drawings]
[0020] [Figure 1] 1 is a schematic diagram showing an example of the structure of a quantum dot electroluminescence device according to the present invention. [Diagram 2] 1 is an example of a light-emitting scheme of a conventional quantum dot electroluminescent device. [Diagram 3] 1 shows an EL spectrum of an example of a conventional quantum dot electroluminescent device. [Figure 4] 1 is an example of a light emission scheme of a quantum dot electroluminescent device of the present invention. [Diagram 5] 1 shows an EL spectrum of an example of a quantum dot electroluminescent device of the present invention. [Figure 6] 1 is an example emission scheme of a quantum dot electroluminescent device, comprising an emission layer including quantum dots and an organic material. [Figure 7] 1 shows the EL spectrum of an example quantum dot electroluminescent device comprising an emissive layer including quantum dots and an organic material. [Figure 8] The F1s spectra obtained by XPS analysis for samples (1), (2), and (3) are shown. [Figure 9] The O1s spectrum obtained by XPS analysis of sample (1) and the fitting results when decomposed into O1, O2, and O3 components are shown. [Figure 10]The O1s spectrum obtained by XPS analysis of sample (2) and the fitting results when decomposed into O1, O2, and O3 components are shown. [Figure 11] The O1s spectrum obtained by XPS analysis of sample (3) and the fitting results when decomposed into O1, O2, and O3 components are shown. [Figure 12] 1 shows EL spectra of the quantum dot electroluminescent devices of Comparative Examples 1 to 5. [Figure 13] 1 shows EL spectra of the quantum dot electroluminescent devices of Examples 1 to 3. [Figure 14] 1 shows the current density-voltage characteristics of the quantum dot electroluminescent devices of Examples 4 to 6. [Figure 15] 1 shows the luminance-voltage characteristics of the quantum dot electroluminescent devices of Examples 4 to 6. [Figure 16] 1 shows the external quantum efficiency-current density characteristics of the quantum dot electroluminescent devices of Examples 4 to 6. [Figure 17] 1 shows EL spectra of the quantum dot electroluminescent devices of Examples 4 to 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the quantum dot electroluminescence device and the manufacturing method thereof of the present invention will be illustrated and described in detail based on the embodiments.
[0022] <Quantum dot electroluminescent device> The quantum dot electroluminescence device of the present embodiment includes a cathode, an electron transport layer made of a metal oxide, an intermediate layer made of an organic material, a light emitting layer containing quantum dots, and an anode, in this order. The quantum dot electroluminescence device of the present embodiment is characterized in that the electron transport layer is fluorine-treated.
[0023] The quantum dot electroluminescence device of this embodiment has an electron transport layer made of a metal oxide between the cathode and the light emitting layer. In general, the electron transport layer made of a metal oxide is bound to water in the atmosphere, and a certain proportion of metal hydroxide (e.g., ZnOH when the metal oxide is ZnO) is present on the surface. Carriers are trapped in the metal hydroxide, which inhibits recombination of carriers in the light emitting layer and causes secondary emission components due to recombination outside the light emitting layer. In contrast, in the quantum dot electroluminescent device of the present embodiment, the electron transport layer made of a metal oxide is fluorinated (for example, when the metal oxide is ZnO, it is made into ZnOF), thereby suppressing the generation of metal hydroxide. Since the fluorinated metal oxide (for example, ZnOF, etc.) does not trap carriers, carrier recombination is sufficiently performed in the light-emitting layer, enabling highly efficient light emission and suppression of secondary emission components. Furthermore, in the quantum dot electroluminescent device of this embodiment, an intermediate layer made of an organic material is provided between the electron transport layer made of a metal oxide and the light-emitting layer, and a gap is provided between the electron transport layer and the light-emitting layer, thereby making it possible to reduce the effect of slight defects remaining in the electron transport layer made of a metal oxide. Therefore, the quantum dot electroluminescent device of this embodiment can emit light with high luminous efficiency and high color purity.
[0024] Next, one embodiment of the quantum dot electroluminescence device of the present invention will be described in detail with reference to the drawings.
[0025] Fig. 1 is a schematic diagram showing an example of the structure of the quantum dot electroluminescence device of the present invention. The quantum dot electroluminescence device 100 shown in Fig. 1 has a structure in which a cathode 120, an electron transport layer 130 made of a metal oxide, an intermediate layer 140 made of an organic material, a light-emitting layer 150 containing quantum dots, a hole transport layer 160, a hole injection layer 170, and an anode 180 are laminated in this order on a substrate 110. In addition, the cathode 120, the electron transport layer 130, the intermediate layer 140, the light-emitting layer 150, the hole transport layer 160, the hole injection layer 170, and the anode 180 provided on the substrate 110 are sealed by a sealing structure 190.
[0026] The quantum dot electroluminescent device 100 shown in FIG. 1 is configured so that electrons are injected from the cathode 120 located at the bottom and holes are injected from the anode 180 located at the top, but the quantum dot electroluminescent device of the present invention is not limited to this configuration and may have an inverted structure.
[0027] The hole transport layer 160 and the hole injection layer 170 may each be a single layer, or each layer may have a structure in which it plays multiple roles. For example, one layer may function as both a hole injection layer and a hole transport layer. In addition, the structure may have other layers between the cathode 120, the electron transport layer 130, the intermediate layer 140, the light-emitting layer 150, the hole transport layer 160, the hole injection layer 170, and the anode 180.
[0028] (substrate) The substrate 110 is preferably made of a transparent material in the case of a bottom emission type element in which light is extracted from the side of the substrate 110. Examples of such transparent materials include glass, quartz, and plastic films. Examples of materials for the plastic films include polyimide, polyethylene terephthalate, polyethylene naphthalate, polypropylene, cycloolefin polymer, polyamide, polyethersulfone, polymethyl methacrylate, polycarbonate, and polyarylate. On the other hand, in the case of a top emission type element in which light is extracted from the upper electrode side, the material of the substrate 110 does not necessarily have to be a transparent material. When an opaque substrate is used as the substrate 110, examples of the opaque substrate include a colored plastic film substrate, a substrate made of a ceramic material such as alumina, and a substrate in which an oxide film (insulating film) is formed on the surface of a metal plate such as stainless steel. Furthermore, when a flexible substrate such as a plastic film is used as the substrate 110 and a quantum dot electroluminescent element is formed thereon, a flexible quantum dot electroluminescent element can be obtained in which the image display portion can be easily deformed.
[0029] The average thickness of the substrate 110 is not particularly limited, but is preferably 0.001 to 30 mm, and more preferably 0.01 to 1 mm.
[0030] (cathode) The cathode 120 is preferably made of a transparent and highly conductive material in the case of a bottom emission type element in which light is extracted from the substrate 110 side. In this case, the cathode 120 may be made of a conductive transparent oxide such as indium tin oxide (ITO) or indium zinc oxide (IZO). On the other hand, in the case of a top emission type element in which light is extracted from the upper electrode side, the material of the cathode 120 does not necessarily need to be a transparent material, so a metal electrode may be used as the cathode 120. Here, as the material of the cathode 120, a metal with a relatively small work function is preferable. By using a metal with a small work function, it is possible to lower the electron injection barrier from the cathode 120 to the organic layer, and it is possible to easily inject electrons. Examples of metals used for the cathode 120 include, but are not limited to, Al, Mg, Ca, Ba, Li, and Na.
[0031] The average thickness of the cathode 120 is not particularly limited, but is preferably 10 to 500 nm, and more preferably 50 to 200 nm.
[0032] (electron transport layer) The electron transport layer 130 is used for the purpose of facilitating the injection and transport of electrons from the cathode 120. The electron transport layer 130 is made of a metal oxide, and more specifically, the material of the electron transport layer 130 is zinc oxide (ZnO), titanium oxide (TiO 2 ), silicon oxide (SiO 2 ), tin oxide (SnO 2 ), tungsten oxide (WO 3 ), tantalum oxide (Ta 2 O 3 ), zirconium oxide (ZrO 2 ), hafnium oxide (HfO 2 ), aluminum oxide (Al 2 O3 ), gallium oxide (Ga 2 O 3 ), magnesium oxide (MgO), lithium oxide (Li 2 O), yttrium oxide (Y 2 O 3 ), zinc oxide doped with magnesium (ZnMgO), zinc oxide doped with aluminum (ZnAlO), zinc oxide doped with lithium (ZnLiO), zinc oxide doped with yttrium (ZnYO), zinc oxide doped with gallium (ZnGaO), and the like are preferred, and among these, from the viewpoints of electron injection property and electron transport property, zinc oxide, titanium oxide, zinc oxide doped with magnesium, zinc oxide doped with aluminum, zinc oxide doped with lithium, zinc oxide doped with yttrium, and zinc oxide doped with gallium are more preferred, and zinc oxide and zinc oxide doped with magnesium are particularly preferred.
[0033] Nanoparticles are preferably used to form the electron transport layer 130. The particle size of the nanoparticles is preferably 1 nm to 100 nm, more preferably 1 nm to 10 nm, and even more preferably 1 nm to 5 nm. Preferably, a thin film formed by spin-coating nanoparticles of a metal oxide, such as zinc oxide nanoparticles, can be used as the electron transport layer 130.
[0034] The electron transport layer 130 is characterized by being fluorine-treated. The fluorine source used in the fluorine treatment is not particularly limited, and may be, for example, fluorocarbon. The method of fluorine treatment is not particularly limited, but oxygen plasma treatment is preferred. The oxygen plasma treatment will be described in detail in the manufacturing method section below. By fluorine-treating the electron transport layer 130, it is possible to prevent the metal oxide constituting the electron transport layer 130 from combining with water in the atmosphere to become a metal hydroxide, and carrier recombination in the light-emitting layer 150 is sufficiently performed, enabling highly efficient light emission and suppression of secondary light emission components. The amount of fluorine introduced (fluorine content) in the electron transport layer 130 measured by XPS (X-ray photoelectron spectroscopy) analysis is preferably 5 atomic % or more, and preferably 20 atomic % or less.
[0035] The average thickness of the electron transport layer 130 is not particularly limited, but is preferably 5 to 200 nm, and more preferably 10 to 100 nm.
[0036] (Middle class) The intermediate layer 140 is made of an organic material. By providing the intermediate layer 140 made of an organic material between the electron transport layer 130 and the light emitting layer 150 and providing a gap between the electron transport layer 130 and the light emitting layer 150, the influence of slight defects remaining in the electron transport layer 130 can be reduced. In addition, when an organic material having an appropriate lowest unoccupied molecular orbital (LUMO) level is used as the intermediate layer 140, the electron injection barrier from the electron transport layer 130 to the intermediate layer 140 is relaxed, and the electron injection barrier from the intermediate layer 140 to the light emitting layer 150 is relaxed. In addition, when the organic material used for the intermediate layer 140 has an appropriate highest occupied molecular orbital (HOMO) level, holes that do not recombine in the light emitting layer 150 and flow out to the counter electrode are prevented. As a result, holes are trapped in the light emitting layer 150, and the recombination efficiency in the light emitting layer 150 is increased.
[0037] Furthermore, light emission at a low voltage is possible by providing an intermediate layer 140 made of an organic material between the electron transport layer 130 and the light emitting layer 150. This is because charge accumulation at the interface where Auger recombination occurs and suppression of quenching allow efficient upconversion using Auger recombination. Hereinafter, the mechanism by which low-voltage light emission is made possible by providing an intermediate layer made of an organic material between the electron transport layer and the light emitting layer will be described in detail with reference to the drawings.
[0038] First, for comparison, FIG. 2 shows an example of a light emission scheme of a conventional quantum dot electroluminescent device not according to the present invention (i.e., when upconversion using Auger recombination does not occur efficiently). The configuration of the conventional quantum dot electroluminescent device shown in FIG. 2 is ITO (cathode) / zinc oxide (electron transport layer) / perovskite quantum dot (light emitting layer) / hole transport layer / molybdenum oxide (hole injection layer) / aluminum (anode). Electrons are injected into the device from the cathode, and holes are injected from the anode, and the electrons and holes recombine at the interface between the electron transport layer and the light emitting layer. The energy obtained by recombination is emitted in the form of infrared light.
[0039] Figures 3(a) and (b) show electroluminescence (EL) spectra obtained from a conventional quantum dot electroluminescence device. Figure 3(a) shows the EL spectrum of a conventional quantum dot electroluminescence device in the wavelength range of 380 nm to 775 nm, and Figure 3(b) shows the EL spectrum of a conventional quantum dot electroluminescence device in the wavelength range of 600 nm to 1030 nm. In addition to the emission from the perovskite quantum dots at a wavelength of 531 nm, infrared radiation due to interface recombination is observed at wavelengths longer than 650 nm.
[0040] Next, FIG. 4 shows an example of a light emission scheme of a quantum dot electroluminescence device according to the present invention (i.e., when upconversion using Auger recombination occurs efficiently). The configuration of the quantum dot electroluminescence device according to the present invention shown in FIG. 4 is ITO (cathode) / fluorine-treated (more specifically, plasma-treated under a fluorine atmosphere) zinc oxide (electron transport layer) / TmPPPyTz (an intermediate layer made of an organic material, the structural formula of which is shown below) / perovskite quantum dots (light-emitting layer) / hole transport layer / molybdenum oxide (hole injection layer) / aluminum (anode). Electrons are injected into the device from the cathode, and holes are injected from the anode, and electrons and holes accumulate at the interface of the fluorine-treated electron transport layer / intermediate layer made of an organic material / light-emitting layer containing quantum dots, and Auger recombination occurs. Here, since the intermediate layer made of an organic material is sufficiently thin, Auger recombination of electrons and holes occurs. The energy obtained by the Auger recombination of the electrons and holes is absorbed by the electrons accumulated at the interface, generating electrons in a high energy state. The generated electrons in a high energy state overcome the electron injection barrier between the fluorine-treated electron transport layer and the quantum dot-containing light-emitting layer, and are injected into the quantum dot-containing light-emitting layer. The electrons injected into the light-emitting layer after overcoming the electron injection barrier and the holes injected into the quantum dot-containing light-emitting layer recombine to emit light. Normally, a voltage needs to be applied to overcome the electron injection barrier, but the light-emitting mechanism of the quantum dot electroluminescent device according to the present invention can utilize the energy obtained by Auger recombination, making it possible to emit light at a low voltage.
[0041] Figure 5 shows the electroluminescence (EL) spectrum obtained from the quantum dot electroluminescence device according to the present invention. Unlike Figure 3(a), only the emission from the perovskite quantum dots at a wavelength of 531 nm was observed, indicating that the energy due to Auger recombination at the interface is efficiently utilized for emission in the light-emitting layer containing the quantum dots.
[0042] The organic material constituting the intermediate layer 140 may be, for example, a material having the following structural formula: [ka] pyridine derivatives such as tris-1,3,5-(3'-(pyridin-3"-yl)phenyl)benzene (TmPyPB), quinoline derivatives such as (2-(3-(9-carbazolyl)phenyl)quinoline (mCQ)), pyrimidine derivatives such as 2-phenyl-4,6-bis(3,5-dipyridylphenyl)pyrimidine (BPyPPM), pyrazine derivatives, phenanthroline derivatives such as bathophenanthroline (BPhen), 2,4-bis(4-biphenyl)-6-(4'-(2-pyridinyl)-4-biphenyl)-[1,3,5]triazine (M triazine derivatives such as 3-phenyl-4-(1'-naphthyl)-5-phenyl-1,2,4-triazole (TAZ), triazole derivatives such as 2-(4-biphenylyl)-5-(4-tert-butylphenyl-1,3,4-oxadiazole) (PBD), imidazole derivatives such as 2,2',2"-(1,3,5-benzotriyl)-tris(1-phenyl-1-H-benzimidazole) (TPBi), aromatic ring tetracarboxylic anhydrides such as naphthalene and perylene, bis[2-(2'-hydroxyphenyl)pyridine]beryllium (Bepp 2 ), tris(8-hydroxyquinolinato)aluminum (Alq 3 ), organic silane derivatives such as silole derivatives such as 2,5-bis(6'-(2',2"-bipyridyl))-1,1-dimethyl-3,4-diphenylsilole (PyPySPyPy), and boron-containing compounds, and these may be used alone or in combination.
[0043] The organic material constituting the intermediate layer 140 preferably contains a pyridine ring. Examples of such organic materials containing a pyridine ring include pyridine derivatives such as the above-mentioned 3TPyMB, TmPPyTz, TmPPPyTz, and tris-1,3,5-(3'-(pyridin-3"-yl)phenyl)benzene (TmPyPB). Organic materials containing a pyridine ring have coordination ability, and for example, when the light-emitting layer 150 is provided on the intermediate layer 140, they play a role in filling structural defects on the quantum dot surface. Therefore, by using an organic material containing a pyridine ring for the intermediate layer 140, it is possible to reduce both the influence of slight defects remaining in the electron transport layer made of a metal oxide and the influence of structural defects on the quantum dot surface, thereby further increasing the luminous efficiency and further suppressing secondary emission components, making it possible to emit light with even higher color purity. In addition, by using an organic material containing a pyridine ring for the intermediate layer 140, Auger recombination of electrons and holes occurs more easily, and upconversion using Auger recombination occurs more efficiently, making it possible to emit light at a lower voltage.
[0044] The organic material constituting the intermediate layer 140 preferably has a triazine skeleton. Examples of such organic materials having a triazine skeleton include triazine derivatives such as the above-mentioned TmPPyTz, TmPPPyTz, and 2,4-bis(4-biphenyl)-6-(4'-(2-pyridinyl)-4-biphenyl)-[1,3,5]triazine (MPT). The organic material having a triazine skeleton also has coordination ability, and plays a role in filling structural defects on the quantum dot surface when, for example, the light-emitting layer 150 is provided on the intermediate layer 140. Therefore, by using an organic material having a triazine skeleton for the intermediate layer 140, it is possible to reduce both the influence of slight defects remaining in the electron transport layer made of metal oxide and the influence of structural defects on the quantum dot surface, thereby further increasing the luminous efficiency and further suppressing secondary emission components, making it possible to emit light with even higher color purity. Furthermore, by using an organic material having a triazine skeleton for the intermediate layer 140, Auger recombination of electrons and holes occurs more easily, and upconversion using Auger recombination occurs more efficiently, making it possible to emit light at a lower voltage.
[0045] It is more preferable that the organic material constituting the intermediate layer 140 contains a pyridine ring and has a triazine skeleton. Examples of such organic materials containing a pyridine ring and having a triazine skeleton include the above-mentioned TmPPyTz, TmPPPyTz, 2,4-bis(4-biphenyl)-6-(4'-(2-pyridinyl)-4-biphenyl)-[1,3,5]triazine (MPT), etc. Organic materials containing a pyridine ring and having a triazine skeleton have high coordination ability, and are highly effective in filling structural defects on the quantum dot surface when, for example, the light-emitting layer 150 is provided on the intermediate layer 140. Therefore, by using an organic material containing a pyridine ring and having a triazine skeleton for the intermediate layer 140, it is possible to further reduce both the influence of slight defects remaining in the electron transport layer made of metal oxide and the influence of structural defects on the quantum dot surface, thereby enabling more efficient light emission and further suppression of secondary light emission components. Furthermore, by using an organic material containing a pyridine ring and having a triazine skeleton for the intermediate layer 140, Auger recombination of electrons and holes occurs more easily, upconversion using Auger recombination occurs more efficiently, and light emission at an even lower voltage becomes possible.
[0046] The average thickness of the intermediate layer 140 is not particularly limited, but is preferably 5 to 200 nm, and more preferably 10 to 100 nm.
[0047] (Light Emitting Layer) The light-emitting layer 150 includes quantum dots. The light-emitting layer 150 may further include an organic material, if necessary, or may be formed only from quantum dots.
[0048] In the light-emitting layer 150, holes injected from the anode 180 and electrons injected from the cathode 120 recombine to emit light from the quantum dots. The color of light emitted from the light-emitting layer 150 can be changed by changing the crystal grain size and type (material) of the quantum dots contained in the light-emitting layer 150. The crystal grain size of the quantum dots can be selected according to the desired color of light emitted, and is preferably, for example, 1 to 10 nm.
[0049] The quantum dots are preferably perovskite quantum dots or core-shell quantum dots.
[0050] The perovskite quantum dots include CsPbBr 3 Perovskite quantum dots are preferred. Also, CsPbBr 3 FACsPbBr in which part of the Cs in the PbBr has been exchanged with formamidinium (FA) ions 3 Here, the exchange ratio of Cs and FA is not particularly limited.
[0051] The core-shell quantum dots preferably have a central portion called a core, which is made of a semiconductor particle, one or more semiconductor layers called shells surrounding the core, and an organic substance called a ligand that covers the surface of the shell.
[0052] Examples of the semiconductor constituting the core portion of the quantum dot include II-VI group compounds, II-V group compounds, III-VI group compounds, III-V group compounds, IV-VI group compounds, I-III-VI group compounds, II-IV-VI group compounds, and II-IV-V group compounds, such as ZnS, ZnSe, ZnTe, ZnSeTe, CdS, CdSe, CdTe, InN, InP, InAs, InSb, and CuInS. Among these, the core of the quantum dot is preferably CdSe, CdS, InP, ZnSe, ZnTe, or ZnSeTe from the viewpoints of ease of synthesis, ease of control of particle size and / or particle size distribution to obtain light emission of a desired wavelength, and quantum yield of light emission. In addition, in the semiconductor constituting the core portion, the ratio of each element may be stoichiometric or not stoichiometric.
[0053] The semiconductor constituting the shell part of the quantum dot can also be a semiconductor of the same composition as the semiconductor constituting the core part. The shell of the quantum dot is preferably selected according to the semiconductor used for the core to be coated, and it is preferable to use a semiconductor having a larger band gap than the core as the shell. In this case, the excitation energy of the core is efficiently confined within the core by the shell. Specifically, for example, when the core is made of CdSe, CdS, or InP, it is preferable to use ZnS or ZnSe, which has a larger band gap, for the shell. In addition, in the semiconductor constituting the shell part, the ratio of each element may be stoichiometric or not.
[0054] In the quantum dots, in order to stabilize the semiconductor surface and suppress the aggregation of the semiconductor fine particles, it is preferable to cap the semiconductor fine particle surface with an organic ligand called a ligand. If the ligand portion for capping contains a lipophilic long-chain alkyl group or the like, the solubility in an organic solvent is improved, and a quantum dot solution can be prepared by dissolving the quantum dots in an organic solvent. Examples of the ligand (organic ligand) include amines bonded to a hydrocarbon group, carboxylic acids bonded to a hydrocarbon group, phosphines bonded to a hydrocarbon group, phosphine oxides bonded to a hydrocarbon group, and thiols bonded to a hydrocarbon group. The hydrocarbon group is preferably a lipophilic chain-like hydrocarbon group. Examples of amines bonded to a lipophilic chain-like hydrocarbon group include hexadecylamine and oleylamine. Examples of carboxylic acids bonded to a lipophilic chain-like hydrocarbon group include oleic acid. Examples of phosphines bonded to a lipophilic chain-like hydrocarbon group include trioctylphosphine. Examples of phosphine oxides bonded to a lipophilic chain-like hydrocarbon group include tri-n-octylphosphine oxide. Examples of thiols having a lipophilic chain hydrocarbon group bonded thereto include dodecanethiol.
[0055] The light-emitting layer 150 may further include an organic material in addition to the quantum dots. When the light-emitting layer 150 includes the quantum dots and an organic material, quenching due to the aggregation of the quantum dots can be suppressed. Here, the organic material is preferably an electron transport material (i.e., an organic material having electron transport properties). The electron transport material does not hinder the flow of electrons injected from the cathode 120 side to the light-emitting layer 150, and has the effect of not allowing holes injected from the anode 180 side to pass to the cathode 120 side to the light-emitting layer 150 (i.e., the effect of blocking the hole current flowing out from the light-emitting layer 150), so that leakage current can be suppressed, and the electrons injected from the cathode 120 and the holes injected from the anode 180 can be efficiently recombined in the light-emitting layer 150. When the light-emitting layer 150 includes an electron transport material, charges are injected into the quantum dots via the electron transport material, and the effect of crystal defects on light emission can be suppressed, and defective light emission seen in the EL spectrum can be suppressed. The electron transport material is preferably present, for example, in a form mixed with the quantum dots and filling the gaps between the quantum dots in the light-emitting layer 150. When the electron transport material is used in a form mixed with the quantum dots, it is preferably a material that dissolves in a dispersion liquid of the quantum dots.
[0056] In addition, it has been difficult to mix organic materials (especially organic aromatic compounds) into thin films of quantum dots (especially perovskite quantum dots). 3 Using the technology described in "Development of Nanocrystals and High-Performance LEDs," it is easy to mix organic materials into thin films of quantum dots.
[0057] Furthermore, the light-emitting layer 150 can emit light at a lower voltage by including quantum dots and an organic material. Hereinafter, the mechanism by which low-voltage light emission is possible by including quantum dots and an organic material in the light-emitting layer will be described in detail with reference to the drawings.
[0058] Figure 6 shows an example of a light-emitting scheme of a quantum dot electroluminescent device having an emission layer containing quantum dots and an organic material. The quantum dot electroluminescent device shown in Figure 6 is configured as follows: cathode / fluorine-treated (more specifically, plasma-treated under a fluorine atmosphere) zinc oxide (electron transport layer) / TmPPPyTz (intermediate layer made of organic material) / emission layer containing perovskite quantum dots and DIC-TRZ (organic material) / TCTA (hole transport layer, the structural formula of which is shown in the "hole transport layer" section below) / hole injection layer / anode. The energy levels of the materials used in each layer are shown in Table 1.
[0059] [Table 1]
[0060] The DIC-TRZ (organic material) used in the light-emitting layer has a lower ionization potential and electron affinity than the perovskite quantum dots. Therefore, holes can be injected from the hole transport layer (TCTA) more easily, and holes can be injected at a low voltage. The injected holes move to the interface of the fluorine-treated electron transport layer (zinc oxide), and the energy obtained by the interface recombination is absorbed by the electrons accumulated at the interface, resulting in a high-energy state. The high-energy electrons are injected into the DIC-TRZ (organic material), and recombine with the holes injected into the DIC-TRZ (organic material), resulting in an excited state. Energy is transferred from this excited state to the perovskite quantum dots, resulting in light emission. In this embodiment, the voltage required for hole injection is reduced, making it possible to emit light at a low voltage.
[0061] 7 shows an electroluminescence (EL) spectrum obtained from an example of a quantum dot electroluminescence device having a light-emitting layer containing quantum dots and an organic material. Only light emission from the perovskite quantum dots was observed, and in the quantum dot electroluminescence device of this embodiment, the carrier balance can be controlled by mixing an organic material (DIC-TRZ) into the light-emitting layer, so that the light-emitting efficiency can be improved.
[0062] The organic material contained in the light-emitting layer preferably has a small ionization potential, specifically, the highest occupied molecular orbital (HOMO) level is preferably 5.5 eV or less, more preferably 5.2 eV or less. When the light-emitting layer contains an organic material having a HOMO level of 5.5 eV or less together with the quantum dots, hole injection into the organic material of the light-emitting layer becomes easier, and the voltage required for hole injection is further reduced, making it possible to emit light at a lower voltage. In this specification, the HOMO level is synonymous with the ionization potential obtained by ultraviolet photoelectron spectroscopy.
[0063] The organic material contained in the light-emitting layer preferably has a small electron affinity, specifically, the lowest unoccupied molecular orbital (LUMO) level is preferably 3.1 eV or less, more preferably 2.3 eV or less. The organic material contained in the light-emitting layer more preferably has a HOMO level of 5.5 eV or less and a LUMO level of 3.1 eV or less. By containing an organic material with a LUMO level of 3.1 eV or less together with quantum dots in the light-emitting layer, electron injection into the organic material of the light-emitting layer becomes easier, and light emission at a lower voltage becomes possible. In this specification, the LUMO level is synonymous with the electron affinity obtained by adding the band gap obtained from the optical absorption spectrum to the HOMO level obtained by ultraviolet photoelectron spectroscopy.
[0064] Examples of organic materials optionally used in the light-emitting layer 150 include pyridine derivatives such as 3TPyMB, TmPPyTz, TmPPPyTz, tris-1,3,5-(3'-(pyridin-3"-yl)phenyl)benzene (TmPyPB), pyrimidine derivatives such as 2-phenyl-4,6-bis(3,5-dipyridylphenyl)pyrimidine (BPyPPM), pyrazine derivatives, pyridazine derivatives, triazine derivatives such as 2,4-diphenyl-6-bis(12-phenylindolo)[2,3-a]carbazol-11-yl)-1,3,5-triazine (DIC-TRZ), 2,4-bis(4-biphenyl)-6-(4'-(2-pyridinyl)-4-biphenyl)-[1,3,5]triazine (MPT), and the like. Examples of the organic material include triazole derivatives such as triazole (TAZ), imidazole derivatives such as 2,2',2"-(1,3,5-pentriyl)-tris(1-phenyl-1-H-benzimidazole) (TPBi), phenanthroline derivatives such as bathophenanthroline (BPhen), oxazole derivatives, oxadiazole derivatives such as 2-(4-biphenylyl)-5-(4-tert-butylphenyl-1,3,4-oxadiazole) (PBD), benzoxazole derivatives, benzothiazole derivatives such as 2,2'-(para-phenylenedivinylene)-bisbenzothiazole, benzothiadiazole derivatives, benzimidazole derivatives, quinoline derivatives such as (2-(3-(9-carbazolyl)phenyl)quinoline (mCQ), isoquinoline derivatives, and quinoxaline derivatives. Among these, DIC-TRZ is preferable as the organic material contained in the light-emitting layer 150. DIC-TRZ has a HOMO level of 5.1 eV and a LUMO level of 2.1 eV, which satisfies the above-mentioned criteria of a HOMO level of 5.5 eV or less and a LUMO level of 3.1 eV or less. Since the voltage required for hole injection and electron injection is further reduced, light emission at a lower voltage is possible. As the organic material contained in the light-emitting layer 150, an organic material containing a pyridine ring or an organic material having a triazine skeleton, as explained in the above section "Intermediate layer 140 made of organic material", is also preferable. The amount of the organic material added to the light-emitting layer 150 is preferably in the range of 0.05 to 10, and more preferably in the range of 0.5 to 3, in terms of mass ratio to the quantum dots. In addition, from the viewpoint of achieving both a reduction in driving voltage and an improvement in external quantum efficiency, the amount of organic material added to the light-emitting layer 150 is preferably in the range of 0.01 to 1 in terms of mass ratio to the quantum dots, more preferably in the range of 0.03 to 0.3, and even more preferably in the range of 0.05 to 0.1.
[0065] The method for forming the light-emitting layer 150 is not particularly limited, but a solution of quantum dots dissolved in an organic solvent or water can be prepared, and the layer can be formed by a spin coating method, an inkjet method, a printing method, etc. At this time, materials that emit red, green, and blue light can be finely coated separately to form pixels of a display device capable of color display.
[0066] The average thickness of the light-emitting layer 150 is not particularly limited, but is preferably 5 to 200 nm, and more preferably 10 to 50 nm.
[0067] (Hole transport layer) The hole transport layer 160 is used to transport holes injected from the anode 180 to the light emitting layer 150. As a material for the hole transport layer 160, an organic material or an inorganic material having a hole transporting property can be used. The material for the hole transport layer 160 is preferably an organic material having a hole transporting property, for example, a material represented by the following structural formula: [ka] In addition to triphenylamine compounds such as 4,4',4"-tris(carbazol-9-yl)triphenylamine (TCTA), 4,4',4"-trimethyltriphenylamine, and 4,4',4"-tris(N-3-methylphenyl-N-phenylamino)triphenylamine (m-MTDATA), 2,2'-bis(N-carbazolyl)-9,9'-spirobifluorene (CFL), 4,4'-bis(carbazol-9-yl)biphenyl (CBP), N,N,N',N'-tetraphenyl-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-1,1'-biphenyl-4,4' -diamine (TPD1), N,N'-diphenyl-N,N'-bis(4-methoxyphenyl)-1,1'-biphenyl-4,4'-diamine (TPD2), N,N,N',N'-tetrakis(4-methoxyphenyl)-1,1'-biphenyl-4,4'-diamine (TPD3), N,N'-di(1-naphthyl)-N,N'-diphenyl-1,1'-biphenyl-4,4'-diamine (α-NPD), and the like can be used alone or in combination. Among these, triphenylamine compounds are preferred from the viewpoint of hole transporting properties, and 4,4',4"-triphenylamine (TCTA) is particularly preferred.
[0068] The average thickness of the hole transport layer 160 is not particularly limited, but is preferably 10 to 500 nm, and more preferably 20 to 100 nm.
[0069] (Hole injection layer) The hole injection layer 170 is formed to facilitate the injection of holes from the anode 180. For the hole injection layer 170, it is preferable to use a material with high charge acceptance, and either an inorganic material or an organic material can be used. A typical inorganic material used for the hole injection layer 170 is molybdenum trioxide (MoO 3 ), vanadium oxide (V 2 O 5 ), ruthenium oxide (RuO 2Examples of the organic material used for the hole injection layer 170 include 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (HAT-CN), 2,3,5,6-tetrafluoro-7,7,8,8-tetracyano-quinodimethane (F4-TCNQ), and hexafluorotetracyanonaphthoquinodimethane (F6-TNAP). The hole injection layer 170 may contain one or more of these materials. Among these materials, molybdenum trioxide and HAT-CN are preferred as the material used for the hole injection layer 170 from the viewpoint of hole injection properties.
[0070] The average thickness of the hole injection layer 170 is not particularly limited, but is preferably 1 to 500 nm, and more preferably 3 to 50 nm.
[0071] (anode) The material of the anode 180 is preferably a metal having a relatively large work function. By using a metal having a large work function, the hole injection barrier from the anode to the organic layer can be lowered, and holes can be easily injected. In addition, the metal used for the anode 180 is preferably a metal having a high reflectance in the visible light region, and examples of the metal include, but are not limited to, Al, Au, Pt, Ni, W, Cr, Mo, Fe, Co, and Cu. In addition, if a transparent material is used for the anode 180, a top emission type element in which light is extracted from the upper electrode can be obtained.
[0072] The average thickness of the anode 180 is not particularly limited, but is preferably 10 to 500 nm, and more preferably 30 to 150 nm.
[0073] (Sealed structure) As the sealing structure 190, any form capable of sealing the above-mentioned cathode 120, electron transport layer 130, intermediate layer 140, light-emitting layer 150, hole transport layer 160, hole injection layer 170, and anode 180 can be used. For example, various forms can be adopted, such as hollow sealing such as can sealing, thin film sealing, solid sealing, etc.
[0074] (Method of forming each layer) The method of forming the cathode 120, the electron transport layer 130, the intermediate layer 140, the light-emitting layer 150, the hole transport layer 160, the hole injection layer 170, and the anode 180 is not particularly limited, and methods such as vacuum deposition, electron beam, sputtering, spin coating, inkjet, and printing can be used. Furthermore, using these methods, the thicknesses of the cathode 120, the electron transport layer 130, the intermediate layer 140, the light-emitting layer 150, the hole transport layer 160, the hole injection layer 170, and the anode 180 can be appropriately adjusted depending on the purpose. Furthermore, it is preferable to select these methods depending on the characteristics of the material of each layer, and the manufacturing method may be different for each layer. Through the above steps, the quantum dot electroluminescent device 100 shown in FIG. 1 is completed.
[0075] (Application) The quantum dot electroluminescence element of the present invention can be used in display devices, etc. A display device incorporating the quantum dot electroluminescence element of the present invention has excellent light emission characteristics because it includes a quantum dot electroluminescence element that has high light emission efficiency and is capable of emitting light with high color purity.
[0076] <Method of Manufacturing Quantum Dot Electroluminescence Device> The method for manufacturing a quantum dot electroluminescent device of this embodiment is characterized by including, in this order, a step of forming a cathode, a step of forming an electron transport layer made of a metal oxide, a step of fluorine-treating the electron transport layer, a step of forming an intermediate layer made of an organic material, a step of forming a light-emitting layer containing quantum dots, and a step of forming an anode.
[0077] In the method for producing the quantum dot electroluminescence device of this embodiment, the method for forming each layer, the cathode, the electron transport layer made of a metal oxide, the intermediate layer made of an organic material, the light-emitting layer, and the anode, is not particularly limited, and for example, the above-mentioned vacuum deposition method, electron beam method, sputtering method, spin coating method, inkjet method, printing method, etc. can be used. In addition, it is preferable to select these methods depending on the characteristics of the material of each layer, and the production method may be different for each layer.
[0078] In the method for producing the quantum dot electroluminescence device of the present embodiment, after forming an electron transport layer made of a metal oxide, the electron transport layer is fluorinated. The step of fluorinating the electron transport layer can be carried out by any method capable of fluorinating the metal oxide constituting the electron transport layer. Here, the fluorine source used for the fluorination is not particularly limited, and examples thereof include fluorocarbons.
[0079] In the step of fluorine-treating the electron transport layer, it is preferable to subject the electron transport layer to oxygen plasma treatment in an atmosphere of a fluorine source. By subjecting the electron transport layer to oxygen plasma treatment in an atmosphere of a fluorine source, a quantum dot electroluminescent device capable of emitting light with higher luminous efficiency and higher color purity can be obtained. The reason why the oxygen plasma treatment has a particularly excellent effect is not necessarily clear, but is considered to be as follows. Here, the case where the metal oxide is ZnO nanoparticles will be specifically described, but in the present invention, the metal oxide constituting the electron transport layer is not limited to ZnO nanoparticles, and any metal oxide can be used.
[0080] When the metal oxide is ZnO nanoparticles, it is believed that the reason for the inhibition of efficient light emission is ZnOH, which exists at a certain rate on the surface of the ZnO nanoparticles. Carriers are trapped by ZnOH, which prevents recombination in the light-emitting material (i.e., quantum dots) of the light-emitting layer. It also causes secondary emission components due to recombination outside the light-emitting layer. Therefore, it is important to reduce ZnOH. In contrast, by performing oxygen plasma treatment, the residual solvent incorporated in the ZnO film is removed. Since the residual solvent is incorporated in the form of being coordinated to the ZnO nanoparticles, the ZnO nanoparticles are exposed by oxygen plasma treatment. There are many dangling oxygen bonds on the surface of the exposed ZnO nanoparticles. Therefore, fluorine present in the plasma atmosphere bonds with the dangling oxygen bonds to form ZnOF. Here, in the examples described later, fluorine is introduced in the form of fluorocarbon, but the bonds of the fluorocarbon are cleaved in the plasma to generate fluorine. The formed ZnOF does not act as a carrier trap, leading to highly efficient emission and suppression of secondary emission components. Here, in the absence of fluorine, dangling oxygen bonds remain on the surface of ZnO, and water in the atmosphere bonds to form ZnOH, so surface treatment with fluorine is important. Although the effect of introducing fluorine into the ZnO terminals can be obtained by performing plasma treatment using only fluorocarbon, the ZnO film itself will be removed by dry etching. Therefore, it is preferable to perform oxygen plasma treatment in an atmosphere containing a fluorine source.
[0081] In the oxygen plasma treatment, the conditions such as the flow rate of oxygen, pressure, power of plasma treatment, and treatment time are not particularly limited, but generally, the higher the power of plasma treatment and the longer the treatment time, the more the ends of the metal oxide constituting the electron transport layer can be treated, but on the other hand, the electron transport ability of the metal oxide deteriorates. Therefore, it is preferable to perform the oxygen plasma treatment under optimal conditions for each quantum dot electroluminescence device to be fabricated.
[0082] According to the method for manufacturing a quantum dot electroluminescent device of the present embodiment described above, it is possible to obtain a quantum dot electroluminescent device capable of emitting light with high luminous efficiency and high color purity. EXAMPLES
[0083] Examples are given below to explain the present invention in more detail, but the present invention is not limited to the following examples. In the following examples, ZnO was mainly used as the metal oxide, but it has been confirmed that other metal oxides such as ZnMgO can also achieve the same effects.
[0084] <Details of UV ozone treatment> For the UV ozone treatment, a UV ozone cleaner manufactured by Filgen Co., Ltd. was used. The substrate on which the electron transport layer (metal oxide) 130 was formed was placed inside the UV ozone cleaner. The distance between the UV lamp and the substrate was set to 3 cm. After introducing oxygen for 2 minutes, UV light was irradiated for 20 minutes to generate ozone and oxidize the metal oxide. Thereafter, nitrogen gas was introduced by flow for 5 minutes to remove the remaining ozone, and then the substrate was taken out.
[0085] <Details of oxygen plasma treatment> For the oxygen plasma treatment, a PC-300 plasma cleaner manufactured by Samco was used. The substrate on which the carbon fluoride film was formed was placed inside the plasma cleaner, evacuated, and then oxygen gas was introduced by flow at 10 sccm. The back pressure was set to 15 Pa, and the treatment was performed with a traveling wave RF plasma of 100 W for 5 minutes. Thereafter, evacuation was performed while flowing nitrogen gas to remove the residual gas, and the pressure was returned to atmospheric pressure by introducing nitrogen gas, and the substrate was taken out. By this treatment, the inside of the plasma cleaner was coated with carbon fluoride. Next, the substrate on which the electron transport layer (metal oxide) 130 was formed was placed inside the plasma cleaner, evacuated, and then oxygen gas was introduced by flow at 10 sccm. The back pressure was set to 15 Pa, and the treatment was performed with a traveling wave RF plasma of 50 W for 1 minute. Thereafter, evacuation was performed while flowing nitrogen gas to remove the residual gas, and the pressure was returned to atmospheric pressure by introducing nitrogen gas, and the substrate was taken out.
[0086] <Evaluation of fluorine introduction amount by XPS (X-ray photoelectron spectroscopy) analysis> Samples (1), (2), and (3) for XPS evaluation were prepared as follows. A glass substrate with 100 nm ITO was cleaned, then UV ozone treated, and moved into a glove box filled with nitrogen. A ZnO solution (solvent: 1-butanol) adjusted to a predetermined concentration to obtain a film thickness of 20 nm was dropped onto the substrate fixed on the spin stage of a spin coater, and the substrate was spun at 2000 rpm for 40 seconds to coat and form an electron transport layer made of ZnO. Next, the substrate was subjected to a heat treatment in nitrogen at 180° C. for 20 minutes. The ZnO / ITO-attached substrate obtained by this heat treatment was designated as sample (1).
[0087] The heat-treated ZnO / ITO-attached substrate (i.e., the same as sample (1)) was taken out of the glove box and subjected to UV ozone treatment according to the above procedure. The ZnO / ITO-attached substrate obtained by this UV ozone treatment was designated as sample (2).
[0088] On the other hand, the ZnO / ITO-attached substrate (i.e., the same as sample (1)) that had been subjected to the heat treatment was taken out of the glove box and subjected to oxygen plasma treatment according to the above procedure. The ZnO / ITO-attached substrate obtained by this oxygen plasma treatment was designated as sample (3).
[0089] For each of the samples (1), (2), and (3), the XPS spectrum was measured (zinc, oxygen, fluorine, and carbon were measured) using a PHI Quantera II [X-ray source: monochromated Al (1486.6 eV)]. FIG. 8 shows the F1s spectra of samples (1), (2), and (3).
[0090] As can be seen from Figure 8, no fluorine was detected in sample (1) and sample (2), but fluorine was detected in sample (3). In addition, the percentage of F in the metal oxide film of sample (3) was calculated from the XPS spectra of zinc, oxygen, and fluorine, and was found to be 13.5 atomic %.
[0091] Next, Figures 9 to 11 show the measurement results of the O1s spectrum of oxygen for samples (1), (2), and (3), and the fitting results when decomposed into O1, O2, and O3 components. Here, O1 represents the Zn-O bond state, O2 represents the bond state of Zn-OH, Zn-OF, etc., and O3 represents the bond state of C=O and COC. Table 2 shows the ratio of oxygen bond states for samples (1), (2), and (3).
[0092] [Table 2]
[0093] As can be seen from Table 2, the area ratios of Sample (1) and Sample (2) were almost the same. This indicates that the UV ozone treatment hardly changes the oxygen bonding state. On the other hand, sample (3) showed a large decrease in O1 and a large increase in O2. Because sample (3) contains a large amount of fluorine, the large increase in O2 is thought to be due to the formation of ZnOF bonds.
[0094] <Device manufacturing process and evaluation of Comparative Examples 1 to 5 and Examples 1 to 3> A glass substrate with 100 nm ITO was cleaned, then UV ozone treated, and moved into a glove box filled with nitrogen. A ZnO solution (solvent: 1-butanol) adjusted to a predetermined concentration to obtain a film thickness of 20 nm was dropped onto the substrate fixed on the spin stage of a spin coater, and the substrate was spun at 2000 rpm for 40 seconds to coat and form an electron transport layer made of ZnO. Next, heat treatment was performed under nitrogen at 180° C. for 20 minutes.
[0095] Next, the substrates were taken out of the glove box, and the samples of Comparative Example 3 and Comparative Example 5 were subjected to a UV ozone treatment, while the samples of Comparative Example 4 and Examples 1 to 3 were subjected to an oxygen plasma treatment. It was then transferred back into the nitrogen filled glove box.
[0096] Next, for the samples of Comparative Example 2, Comparative Example 5, and Examples 1 to 3, a chloroform solution containing 1 mg / mL of 3TPyMB (Comparative Example 2, Comparative Example 5, Example 1), TmPPyTz (Example 2), or TmPPPyTz (Example 3) represented by the above structural formula was dropped onto a substrate fixed on the spin table of a spin coater and spun at 2000 rpm for 40 seconds to coat and form an intermediate layer made of an organic material. Next, heat treatment was performed under nitrogen at 100° C. for 20 minutes.
[0097] Next, CsPbBr 3 A solution of the perovskite quantum dot material dissolved in n-octane was dropped onto a substrate fixed on the spin stage of a spin coater, and the substrate was spun at 2000 rpm for 40 seconds to form a coating film, forming a light-emitting layer.
[0098] Next, the substrate was transferred into a vacuum chamber, and Al was evaporated at a deposition rate of 1 to 10 Å / sec to form a 100 nm anode film.
[0099] Next, the substrate was removed from the vacuum chamber into a glove box filled with nitrogen, and the element was covered with a UV-curable adhesive in a glass tube with a desiccant and irradiated with UV light to seal the hollow. 2 It is.
[0100] Table 3, FIG. 12 and FIG. 13 show the measurement results of the electro-optical characteristics and the EL spectra of the quantum dot electroluminescent devices of Comparative Examples 1 to 5 and Examples 1 to 3. The maximum external quantum efficiency and the driving voltage are relative values, with the value for the quantum dot electroluminescent device of Comparative Example 1 taken as 100.
[0101] The secondary emission intensities are shown in Table 3 as percentages of the intensity at a wavelength of 780 nm when the intensity of the main emission component is taken as 100.
[0102] [Table 3]
[0103] From the results of Figures 12 and 13, it can be seen that, compared to the quantum dot electroluminescent devices of Comparative Examples 1 to 5, the quantum dot electroluminescent devices of Examples 1 to 3 have a suppressed intensity of the secondary emission component on the longer wavelength side of the main emission component having a peak wavelength of 518 nm. Furthermore, it can be seen from Table 3 that the quantum dot electroluminescence devices of Examples 1 to 3 also have a significantly improved maximum external quantum efficiency compared to the quantum dot electroluminescence devices of Comparative Examples 1 to 5. This indicates that the ends of ZnO are fluorinated to fill defects, and that the intermediate layer made of an organic material functions to suppress deactivation due to defects in ZnO and the quantum dots.
[0104] From the above results, it is seen that the present invention can provide a quantum dot electroluminescent device that exhibits high efficiency and high color purity emission compared to quantum dot electroluminescent devices manufactured using conventional techniques.
[0105] <Device manufacturing process and evaluation of Examples 4 to 6> A glass substrate with 100 nm ITO was cleaned, then UV ozone treated, and moved into a glove box filled with nitrogen. A ZnO solution (solvent: 1-butanol) adjusted to a predetermined concentration to obtain a film thickness of 20 nm was dropped onto the substrate fixed on the spin stage of a spin coater, and the substrate was spun at 2000 rpm for 40 seconds to coat and form an electron transport layer made of ZnO. Next, heat treatment was performed under nitrogen at 180° C. for 20 minutes.
[0106] The substrates were then removed from the glove box, and the samples of Examples 4, 5, and 6 were subjected to oxygen plasma treatment in a fluorine atmosphere as described above. It was then transferred back into the nitrogen filled glove box.
[0107] Next, a chloroform solution containing 1 mg / mL of TmPPyTz was dropped onto the substrate fixed on the spin stage of a spin coater, and the substrate was spun at 2000 rpm for 40 seconds to coat an intermediate layer made of an organic material. Next, heat treatment was performed under nitrogen at 100° C. for 20 minutes.
[0108] Next, F.A. 0.9 Cs 0.1 PbBr 3 n-octane solution (10 mg / mL) in which perovskite quantum dot material was dissolved (Example 4); A solution in which 6 parts by mass of DIC-TRZ is mixed with 100 parts by mass of the perovskite quantum dot material in an n-octane solution of the perovskite quantum dot material (Example 5), or A solution (Example 6) obtained by mixing 60 parts by mass of DIC-TRZ with 100 parts by mass of the perovskite quantum dot material in an n-octane solution was dropped onto a substrate fixed on the spin table of a spin coater, and the substrate was spun at 2000 rpm for 40 seconds to form a coating film, thereby forming a light-emitting layer.
[0109] Next, the substrate was transferred into a vacuum chamber, and Al was evaporated at a deposition rate of 1 to 10 Å / sec to form a 100 nm anode film.
[0110] Next, the substrate was removed from the vacuum chamber into a glove box filled with nitrogen, and the element was covered with a UV-curable adhesive in a glass tube with a desiccant and irradiated with UV light to seal the hollow. 2 It is.
[0111] FIG. 14 shows the current density-voltage characteristics of the quantum dot electroluminescent devices of Examples 4 to 6, FIG. 15 shows the luminance-voltage characteristics of the quantum dot electroluminescent devices of Examples 4 to 6, FIG. 16 shows the external quantum efficiency-current density characteristics of the quantum dot electroluminescent devices of Examples 4 to 6, and FIG. 17 shows the electroluminescence (EL) spectra of the quantum dot electroluminescent devices of Examples 4 to 6. The electroluminescence (EL) spectrum was measured using a Konica Minolta CS-2000 spectroradiometer.
[0112] 16, the maximum external quantum efficiency (EQE) of the quantum dot electroluminescent device of Example 4 was 2.1%, whereas the quantum dot electroluminescent device of Example 5, in which DIC-TRZ was mixed in the emission layer, had an improved maximum EQE of 2.9%. On the other hand, the quantum dot electroluminescent device of Example 6 had a significantly lower maximum EQE than that of Example 5, which is believed to be due to a loss of carrier balance. As can be seen from FIG. 17, all EL spectra showed only light emission originating from the perovskite quantum dots.
[0113] Table 4 shows the relative values of the emission intensity at a wavelength of 531 nm in the EL spectrum near the emission threshold voltage. In Table 4, the emission intensity at a wavelength of 531 nm of the quantum dot electroluminescent device of Example 4 at 1.6 V is set to 100, and the emission intensity at a wavelength of 531 nm of each quantum dot electroluminescent device at each voltage is expressed as a relative value.
[0114] [Table 4]
[0115] The emission threshold voltages at which the EL spectrum of each quantum dot electroluminescent device could be observed were 1.55 V (Example 4), 1.40 V (Example 5), and 1.30 V (Example 6), respectively. The quantum dot electroluminescent devices of Examples 5 and 6, in which DIC-TRZ was mixed, exhibited a significantly lower voltage, which is believed to be due to the ease of hole injection from the hole transport layer to the emitting layer. In addition, as can be seen from FIG. 17, the EL spectra of Examples 5 and 6, in which DIC-TRZ was mixed, were not different from the EL spectrum of Example 4, in which DIC-TRZ was not mixed. These results show that by including DIC-TRZ (organic material) together with quantum dots in the emitting layer, the driving voltage can be significantly lowered without changing the shape of the EL spectrum.
[0116] These results show that when the light-emitting layer contains an organic material together with the quantum dots, light can be emitted at a voltage 1 V lower than the quantum dot band gap of 2.34 eV. This shows that when the light-emitting layer contains an organic material together with the quantum dots, light emission at an ultra-low voltage is possible. [Explanation of symbols]
[0117] 100: Quantum dot electroluminescent device 110: Substrate 120: Cathode 130: Electron transport layer 140: Middle class 150: Light-emitting layer 160: Hole transport layer 170: Hole injection layer 180:Anode 190: Sealing structure
Claims
1. The device comprises a cathode, an electron transport layer made of a metal oxide, an intermediate layer made of an organic material, a light emitting layer including quantum dots, and an anode, in this order; 3. A quantum dot electroluminescent device, wherein the electron transport layer is fluorine-treated.
2. The quantum dot electroluminescent device according to claim 1 , wherein the organic material constituting the intermediate layer contains a pyridine ring.
3. The quantum dot electroluminescent device according to claim 1 , wherein the organic material constituting the intermediate layer has a triazine skeleton.
4. The quantum dot electroluminescent device of claim 1 , wherein the light-emitting layer further comprises an organic material.
5. The quantum dot electroluminescent device according to claim 4 , wherein the organic material contained in the light-emitting layer has a highest occupied molecular orbital (HOMO) level of 5.5 eV or less.
6. The quantum dot electroluminescent device according to claim 5 , wherein the organic material contained in the light-emitting layer has a lowest unoccupied molecular orbital (LUMO) level of 3.1 eV or less.
7. The organic material contained in the light-emitting layer has the following structural formula: 【Chemistry 1】 The quantum dot electroluminescence device according to claim 6, which is DIC-TRZ represented by the formula:
8. forming a cathode; forming an electron transport layer made of a metal oxide; fluorinating the electron transport layer; forming an intermediate layer made of an organic material; forming a light-emitting layer including quantum dots; The method for manufacturing a quantum dot electroluminescence device according to any one of claims 1 to 7, further comprising the steps of: forming an anode; and forming a gate electrode on the gate electrode.
9. 9. The method for producing a quantum dot electroluminescence device according to claim 8, wherein in the step of fluorine-treating the electron transport layer, the electron transport layer is subjected to oxygen plasma treatment in an atmosphere of a fluorine source.