Method for producing silicon clathrate electrode active material, and method for manufacturing lithium ion battery
By employing aluminum fluoride particles with controlled sizes to manage the reaction with sodium silicon alloys, the method reduces the formation of undesirable by-products, improving the stability and performance of silicon clathrate as an electrode active material in lithium ion batteries.
Patent Information
- Application Number
- JP2023080817
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2043-05-16
AI Technical Summary
The production of by-products such as I-type silicon clathrate and diamond-type silicon during the removal of sodium from sodium-silicon alloys limits the effectiveness of silicon clathrate as an electrode active material in lithium ion batteries due to uncontrolled reactions and thermal runaway.
A method involving the use of aluminum fluoride particles with specific particle size ranges to control the reaction with sodium silicon alloys, minimizing the formation of undesirable by-products by suppressing rapid and excessive reactions.
The method effectively suppresses the formation of I-type silicon clathrate and diamond-type silicon, enhancing the stability and performance of silicon clathrate as an electrode active material in lithium ion batteries.
Smart Images

Figure 2024165014000001_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for manufacturing a silicon-class rate electrode active material and a method for manufacturing a lithium-ion battery.
Background Art
[0002] In recent years, battery development has been actively carried out. For example, in the automotive industry, the development of batteries used in electric vehicles or hybrid vehicles has been promoted. Also, silicon is known as an electrode active material used in batteries, particularly lithium-ion batteries.
[0003] The silicon electrode active material has a large theoretical capacity and is effective for increasing the energy density of the battery. On the other hand, the silicon electrode active material has a problem of large expansion during charging. In contrast, it is known that by using a silicon-class rate electrode active material as the silicon electrode active material, expansion during charging can be suppressed.
[0004] For example, Patent Document 1 discloses a silicon-class rate electrode active material having a silicon-class rate type II crystal phase and having a composition of Na x Si 136 (1.98 < x < 2.54).
Prior Art Documents
Patent Documents
[0005]
Patent Document 1
Summary of the Invention
Problems to be Solved by the Invention
[0006] The silicon-class rate can be manufactured by removing sodium from a sodium-silicon alloy.
[0007] The types of silicon clathrate crystals obtained include type I silicon clathrate and type II silicon clathrate. In particular, type II silicon clathrate efficiently occludes lithium in the cage structure of the crystals, and therefore expands and contracts little during charging and discharging of the battery.
[0008] In addition, in the sodium removal process, in addition to silicon clathrate, by-products such as diamond-type silicon (d-Si) may be generated. Since such by-products do not function as electrode active materials, the effect of reducing expansion and contraction during charging and discharging when using II-type silicon clathrate as an electrode active material may be limited.
[0009] Under these circumstances, it is desirable to develop a method capable of suppressing the generation of by-products such as I-type silicon clathrate and diamond-type silicon when removing sodium from a sodium-silicon alloy.
[0010] The present disclosure aims to provide a method for producing a silicon clathrate electrode active material capable of suppressing the production of by-products such as I-type silicon clathrate and diamond-type silicon, and a method for producing a lithium-ion battery including producing such a silicon clathrate electrode active material. [Means for solving the problem]
[0011] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> A method for producing a silicon clathrate electrode active material, comprising the steps of: Providing a sodium silicon alloy; and contacting the sodium silicon alloy with aluminum fluoride particles having a D10 particle size of 15.0 μm or greater to remove at least a portion of the sodium from the sodium silicon alloy. <Aspect 2> 2. The method of claim 1, wherein the aluminum fluoride particles have a (D90 particle size-D10 particle size) / D50 particle size value of 1.10 or less. <Aspect 3> 3. The method of any one of the preceding claims, wherein the silicon clathrate electrode active material is for use as an anode active material in a lithium ion battery. <Aspect 4> Producing a silicon clathrate electrode active material by the method according to any one of aspects 1 to 3; and forming an electrode active material layer containing the silicon clathrate electrode active material; A method for producing a lithium ion battery, comprising: Effect of the Invention
[0012] According to the present disclosure, it is possible to provide a method for producing a silicon clathrate electrode active material capable of suppressing the production of by-products such as I-type silicon clathrate and diamond-type silicon, and a method for producing a lithium-ion battery including producing such a silicon clathrate electrode active material. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a graph showing the measurement results of particle size distribution of aluminum fluoride particles ((a): Comparative Example, (b): Example 1, (c): Example 2). [Diagram 2] FIG. 2 is a graph showing XRD patterns of reaction products containing silicon clathrates of Examples 1 and 2 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.
[0015] <<Method for producing silicon clathrate electrode active material>> The method for producing a silicon clathrate electrode active material of the present disclosure includes providing a sodium silicon alloy, and contacting the sodium silicon alloy with aluminum fluoride (AlF3) particles having a D10 particle size of 15.0 μm or more to remove at least a portion of the sodium from the sodium silicon alloy.
[0016] One possible method for producing a silicon clathrate electrode active material is, for example, reacting a sodium silicon (NaSi) alloy with aluminum fluoride as a sodium trapping agent to partially remove sodium from the NaSi alloy to form a clathrate.
[0017] However, this reaction may produce not only type II silicon clathrate, which has a large expansion-inhibiting effect, but also type I silicon clathrate, which has a small expansion-inhibiting effect, and diamond-type silicon, which has no expansion-inhibiting effect.
[0018] The present inventors have found that in the above reaction, fine AlF3 particles react with the NaSi alloy excessively quickly, generating strong heat, thereby promoting the production of type I silicon clathrate and diamond-type silicon.
[0019] Therefore, the present inventors have investigated the particle size of AlF3 particles and found that the generation of I-type silicon clathrate and diamond-type silicon can be suppressed by using AlF3 particles with few fine particles. Without intending to be bound by theory, it is believed that the use of such AlF3 can suppress excessively rapid reaction and the accompanying thermal runaway, thereby suppressing the generation of I-type silicon clathrate and diamond-type silicon.
[0020] In the present disclosure, the "electrode active material" can be used as either a "positive electrode active material" or a "negative electrode active material", and is particularly used as a "negative electrode active material".
[0021] <Provision of sodium silicon alloy> The method of the present disclosure includes providing a NaSi alloy.
[0022] The NaSi alloy can be prepared by reacting a silicon (Si) source with a sodium (Na) source.
[0023] As the Si source, commercially available Si powder or Si powder prepared by a conventional method can be used.
[0024] The Na source includes, but is not limited to, sodium hydride (NaH).
[0025] The molar ratio of the Si source to the Na source may be 1:0.5-1.5, 1:0.7-1.3, or 1:0.9-1.1.
[0026] An example of a method for reacting the Si source and the Na source is to dry mix these reaction raw materials and then heat them. A cutter mill can be used for the dry mixing. The heating temperature may be 300°C to 700°C, and the heating time may be 20 hours to 60 hours. The heating may be performed under an inert gas atmosphere such as argon.
[0027] <Sodium Removal> The method of the present disclosure includes contacting the NaSi alloy with AlF3 particles to remove at least a portion of the Na from the NaSi alloy.
[0028] The D10 particle size of AlF3 particles is 15 μm or more. The D10 particle size of AlF3 particles may be 20 μm or more, 25 μm or more, 30 μm or more, 33 μm or more, or 35 μm or more, and may be 100 μm or less, 90 μm or less, 80 μm or less, 75 μm or less, or 70 μm or less. When the D10 particle size of AlF3 particles is within the above range, that is, when there are few fine AlF3 particles, the generation of I-type silicon clathrate and diamond-type silicon can be suppressed.
[0029] The D50 particle size of the AlF3 particles may be 30 μm or more, 35 μm or more, 40 μm or more, 45 μm or more, or 50 μm or more, and may be 120 μm or less, 110 μm or less, or 100 μm or less.
[0030] The D90 particle size of the AlF3 particles may be 50 μm or more, 60 μm or more, 65 μm or more, 70 μm or more, or 75 μm or more, and may be 160 μm or less, 150 μm or less, or 140 μm or less.
[0031] The value of (D90 particle size-D10 particle size) / D50 particle size of the AlF3 particles may be 1.10 or less. This value may be 0.40 or more, 0.50 or more, 0.60 or more, 0.65 or more, or 0.70 or more, and may be 1.00 or less, 0.90 or less, 0.95 or less, or 0.80 or less.
[0032] The particle size and particle size distribution of the AlF3 particles can be measured using a particle size distribution measuring device (Shimadzu SALD-7500, Shimadzu Corporation) under the conditions of a refractive index (2.25-0.00i) and built-in ultrasonic irradiation time (10 seconds).
[0033] The AlF3 particles used in the present disclosure may be commercially available or may be AlF3 particles prepared by a conventional method.
[0034] The above AlF3 particles may be subjected to a particle size adjustment means so that the D10 particle size falls within the range of the present disclosure. Examples of particle size adjustment means include, but are not limited to, sieving.
[0035] The molar ratio of the NaSi alloy to the AlF3 particles may be 1:0.10-0.60, 1:0.20-0.50, or 1:0.30-0.40.
[0036] An example of a method for contacting the NaSi alloy with AlF3 particles is to dry mix these reaction raw materials and then heat them. A cutter mill can be used for the dry mixing. The heating temperature may be 200°C to 500°C, and the heating time may be 40 hours to 80 hours. The heating may be performed under an inert gas atmosphere such as argon.
[0037] <Application> The silicon clathrate electrode active material obtained by the method of the present disclosure can be used as a negative electrode active material for lithium ion batteries.
[0038] <Method of manufacturing lithium-ion batteries> The disclosed method of making a lithium ion battery includes making a silicon clathrate electrode active material and forming an electrode active material layer containing the silicon clathrate electrode active material.
[0039] For the method for producing the silicon clathrate electrode active material, reference can be made to the above description regarding the method for producing the silicon clathrate electrode active material of the present disclosure.
[0040] The method for forming the electrode active material layer is not particularly limited, and a known method can be adopted. For example, when the electrode active material layer is used as a negative electrode active material layer, a slurry containing a silicon clathrate electrode active material is applied to a negative electrode current collector and dried to obtain a negative electrode active material layer formed on the negative electrode current collector layer.
[0041] The method for forming the battery is not particularly limited, and any known method can be used. Hereinafter, a battery in which the electrode active material layer is used as the negative electrode active material layer will be described.
[0042] The method for manufacturing a battery according to the present disclosure may include, in addition to manufacturing a silicon clathrate electrode active material and forming a negative electrode active material layer containing the silicon clathrate electrode active material, arranging, in this order, a negative electrode current collector layer, a negative electrode active material layer, an electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer.
[0043] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, copper, a copper alloy, and copper plated or vapor-deposited with nickel, chromium, carbon, or the like may be used, but is not limited to these.
[0044] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.
[0045] <Negative electrode active material layer> The negative electrode active material layer of the present disclosure is a layer containing a negative electrode active material, and optionally an electrolyte, a conductive assistant, and a binder.
[0046] (Negative electrode active material) The negative electrode active material comprises a silicon clathrate electrode active material of the present disclosure.
[0047] (electrolyte) The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.
[0048] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li2S-P2S5-based (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2(Li 13 GeP3S 16 , Li 10 GeP2S 12 ), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x P.S. 6-x Cl xetc.; or combinations thereof, but are not limited to these.
[0049] The sulfide solid electrolyte may be a glass or a crystallized glass (glass ceramic).
[0050] When the negative electrode active material layer contains a solid electrolyte, the mass ratio of the silicon clathrate electrode active material to the solid electrolyte in the negative electrode active material layer (mass of silicon clathrate electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.
[0051] The electrolyte preferably contains a supporting salt and a solvent.
[0052] Examples of supporting salts (lithium salts) for electrolytes having lithium ion conductivity include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6, and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3.
[0053] Examples of the solvent used in the electrolytic solution include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolytic solution preferably contains two or more kinds of solvents.
[0054] (Conductive assistant) The conductive assistant is not particularly limited. For example, the conductive assistant may be VGCF (Vapor Grown Carbon Fiber), acetylene black (AB), Ketjen Black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.
[0055] (binder) The binder is not particularly limited. For example, the binder may be a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.
[0056] The negative electrode active material layer may have a thickness of, for example, 0.1 to 1000 μm.
[0057] <Electrolyte layer> The electrolyte layer includes at least an electrolyte. The electrolyte layer may include a binder, etc., if necessary, in addition to the electrolyte. For the electrolyte and the binder, the above description regarding the negative electrode active material layer of the present disclosure can be referred to.
[0058] The thickness of the electrolyte layer is, for example, 0.1 to 300 μm, and preferably 0.1 to 100 μm.
[0059] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally an electrolyte, a conductive assistant, a binder, and the like.
[0060] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material may be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li 1+x Mn 2-x-y Li-Mn spinel substituted with different elements, which has a composition represented by MyO4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), and lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO4, M is one or more metals selected from Fe, Mn, Co, and Ni), and the like, but are not limited thereto.
[0061] The positive electrode active material may have a coating layer. The coating layer is a layer containing a substance that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials constituting the coating layer include LiNbO3, Li4Ti5O 12 , Li3PO4, etc., but are not limited to these.
[0062] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).
[0063] For the electrolyte, the conductive assistant, and the binder, reference can be made to the above descriptions regarding the negative electrode active material layer of the present disclosure.
[0064] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.
[0065] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.
[0066] <Positive electrode current collector layer> The material used for the positive electrode current collector layer is not particularly limited, and any material that can be used as a positive electrode current collector for a battery can be appropriately adopted. For example, SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium, zinc, etc., and these metals plated or vapor-deposited with nickel, chromium, carbon, etc. may be used, but is not limited to these.
[0067] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.
[0068] The lithium ion battery produced by the method of the present disclosure may be a liquid battery containing an electrolytic solution as an electrolyte layer, or may be a solid battery having a solid electrolyte layer as an electrolyte layer. In the present disclosure, a "solid-state battery" means a battery using at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. The solid-state battery of the present disclosure may also be an all-solid-state battery, i.e., a battery using only a solid electrolyte as an electrolyte.
[0069] The lithium ion battery produced by the method of the present disclosure may be a primary battery or a secondary battery.
[0070] Examples of the shape of the lithium ion battery include a coin type, a laminate type, a cylindrical type, and a square type. EXAMPLES
[0071] 《Synthesis of silicon clathrate electrode active material》 <Alloying> As a silicon (Si) source, Si powder (Kojundo Kagaku, SIEPB32) was prepared. This Si powder and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0, and the weighed Si powder and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere and treated with hydrogen fluoride (HF) to obtain a Si powder having voids inside the primary particles, i.e., a Si powder having a porous structure.
[0072] A sodium silicon (NaSi) alloy was produced using Si powder having a porous structure and sodium hydride (NaH) as a sodium (Na) source. The NaH used was washed with hexane in advance. NaH and Si powder having a porous structure were weighed out so that the molar ratio was 1.05:1, and the weighed NaH and Si powder having a porous structure were mixed in a cutter mill. The resulting mixture was heated in a heating furnace under an argon atmosphere at 500°C for 40 hours to obtain a powdered NaSi alloy.
[0073] <Clathrate formation (sodium removal)> Example 1 The obtained NaSi alloy and aluminum fluoride (AlF3) particles as a Na trapping agent were weighed out to a molar ratio of 1:0.35, and the weighed NaSi alloy and AlF3 were mixed with a cutter mill to obtain a reaction raw material. The obtained powdered reaction raw material was placed in a stainless steel reaction vessel and heated in a heating furnace under an argon atmosphere at 310°C for 60 hours to obtain a reaction product containing a silicon clathrate electrode active material. In Example 1, AlF3 particles that did not pass through a sieve with a mesh size of 75 μm were used.
[0074] Example 2 A reaction product containing the silicon clathrate electrode active material of Example 2 was obtained in the same manner as in Example 1, except that in the clathration (sodium removal), AlF3 particles that passed through a sieve with a mesh size of 75 μm but did not pass through a sieve with a mesh size of 32 μm were used.
[0075] Comparative Example 1 A reaction product containing a silicon clathrate electrode active material of Comparative Example 1 was obtained in the same manner as in Example 1, except that AlF3 particles passed through a sieve with a mesh size of 32 μm were used in the clathration (sodium removal).
[0076] "evaluation" <Particle size and particle size distribution> The particle size and particle size distribution of the AlF3 particles were measured using a particle size distribution measuring device (Shimadzu SALD-7500, Shimadzu Corporation) under the conditions of refractive index (2.25-0.00i) and built-in ultrasonic irradiation time (10 seconds).
[0077] <XRD> As an index for evaluating the proportion of components contained in the reaction product in each example, measurement was carried out by XRD (X-ray diffraction method).
[0078] "result" The measurement results of the particle size distribution of AlF3 used in each example are shown in Table 1 and Figure 1, and the XRD pattern of the reaction product of each example is shown in Figure 2.
[0079] [Table 1]
[0080] As shown in Table 1 and Figures 1 and 2, the reaction products of the examples produced by the method of the present disclosure using AlF3 particles with a D10 particle size within the range of the present disclosure, i.e., with few fine particles, had small peaks in XRD indicating I-type silicon clathrate and diamond-type silicon (d-Si).
Claims
1. A method for producing a silicon clathrate electrode active material, comprising the steps of: Providing a sodium silicon alloy; and contacting the sodium silicon alloy with aluminum fluoride particles having a D10 particle size of 15.0 μm or more to remove at least a portion of the sodium from the sodium silicon alloy.
2. The method according to claim 1, wherein the aluminum fluoride particles have a (D90 particle size - D10 particle size) / D50 particle size value of 1.10 or less.
3. 10. The method of claim 1, wherein the silicon clathrate electrode active material is for use as an anode active material in a lithium ion battery.
4. Producing a silicon clathrate electrode active material by the method according to any one of claims 1 to 3; and forming an electrode active material layer containing the silicon clathrate electrode active material; A method for producing a lithium ion battery, comprising:
Citation Information
Patent Citations
Method for manufacturing negative electrode active material
JP2023043948A
Active material, negative electrode layer, battery, and manufacturing method thereof
JP2023044620A
Active material, negative electrode layer, battery and these manufacturing methods
JP2021158003A