Method for producing silicon clathrate electrode active material, and method for manufacturing lithium ion battery

By selectively removing type I silicon clathrate using a hydrogen fluoride solution, the method addresses the expansion and contraction issues in silicon clathrate electrode materials, enhancing the stability and performance of lithium ion batteries.

JP2024165107APending Publication Date: 2024-11-28TOYOTA JIDOSHA KK +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023080981
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Existing silicon clathrate electrode materials contain both type I and type II silicon clathrates, with type I exhibiting significant expansion and contraction during battery charging and discharging, which is undesirable.

Method used

A method involving the use of a hydrogen fluoride solution to selectively remove type I silicon clathrate from a mixture of type I and type II silicon clathrates, utilizing a specific ratio of hydrogen fluoride to silicon clathrate particles and a mixed solvent of water and an organic solvent to enhance the removal process.

Benefits of technology

The method effectively reduces the proportion of type I silicon clathrate, leading to suppressed expansion and contraction, thereby improving the stability and performance of silicon clathrate electrode materials in lithium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165107000001
    Figure 2024165107000001
  • Figure 2024165107000002
    Figure 2024165107000002
  • Figure 2024165107000003
    Figure 2024165107000003
Patent Text Reader

Abstract

To provide: a method for producing a silicon clathrate electrode active material, capable of removing at least part of a type-I silicon clathrate; and a method for manufacturing a lithium ion battery, including the production of such a silicon clathrate electrode active material.SOLUTION: A method of the present disclosure for producing a silicon clathrate electrode active material includes the steps of: (a) providing silicon clathrate particles containing a type-I silicon clathrate and a type-II silicon clathrate; and (b) bringing the silicon clathrate particles into contact with a hydrogen fluoride solution and removing at least part of the type-I silicon clathrate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a silicon clathrate electrode active material and a method for producing a lithium ion battery. [Background technology]

[0002] In recent years, the development of batteries has been actively carried out. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles is underway. Silicon is also known as an electrode active material for batteries, particularly lithium ion batteries.

[0003] Silicon electrode active materials have a large theoretical capacity and are effective in increasing the energy density of batteries. On the other hand, silicon electrode active materials have a problem of large expansion during charging. It is known that the expansion during charging can be suppressed by using a silicon clathrate electrode active material as the silicon electrode active material.

[0004] For example, Patent Document 1 discloses a silicon clathrate electrode active material having a silicon clathrate type II crystal phase, having voids inside the primary particles, and having a void volume of pores having a pore diameter of 100 nm or less of 0.05 cc / g or more and 0.15 cc / g or less. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2021-158004 Summary of the Invention [Problem to be solved by the invention]

[0006] There are two types of silicon clathrate crystals: type I silicon clathrate and type II silicon clathrate. In particular, type II silicon clathrate efficiently occludes lithium in the cage structure of the crystal, and therefore expands and contracts little during charging and discharging of the battery.

[0007] Under these circumstances, there is a need for the development of a method for removing type I silicon clathrate from a silicon clathrate that contains both type I silicon clathrate and type II silicon clathrate.

[0008] The present disclosure aims to provide a method for producing a silicon clathrate electrode active material capable of removing at least a portion of type I silicon clathrate, and a method for producing a lithium ion battery including producing such a silicon clathrate electrode active material. [Means for solving the problem]

[0009] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> A method for producing a silicon clathrate electrode active material, comprising the steps of: (a) providing silicon clathrate particles containing a silicon clathrate type I and a silicon clathrate type II; and (b) contacting the silicon clathrate particles with a hydrogen fluoride solution to remove at least a portion of the type I silicon clathrate. <Aspect 2> 2. The method of claim 1, wherein in step (b), the ratio of the amount of hydrogen fluoride to the mass of the silicon clathrate particles is greater than 0.0060 mol / g and less than 0.2500 mol / g. <Aspect 3> The method according to any one of the preceding claims, wherein the hydrogen fluoride solution is a mixed solvent of water and an organic solvent. <Aspect 4> The method according to any one of aspects 1 to 3, wherein in the mixed solvent, the ratio of the mass of the water to the total mass of the water and the organic solvent is 30 mass % or more and 90 mass % or less. <Aspect 5> The method according to any one of aspects 1 to 4, wherein the silicon clathrate electrode active material is for use as a negative electrode active material in a lithium ion battery. Aspect 6 Producing a silicon clathrate electrode active material by the method according to any one of aspects 1 to 5; and forming an electrode active material layer containing the silicon clathrate electrode active material; A method for producing a lithium ion battery, comprising: Effect of the Invention

[0010] According to the method of the present disclosure for producing a silicon clathrate electrode active material, at least a part of the I-type silicon clathrate can be removed. Also, according to the present disclosure, it is possible to provide a method for producing a lithium ion battery including producing such a silicon clathrate electrode active material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0012] <<Method for producing silicon clathrate electrode active material>> The disclosed method of producing a silicon clathrate electrode active material includes (a) providing silicon clathrate particles containing a silicon clathrate type I and a silicon clathrate type II, and (b) contacting the silicon clathrate particles with a hydrogen fluoride solution to remove at least a portion of the silicon clathrate type I.

[0013] The present inventors have found that there is a difference in solubility between I-type silicon clathrate and II-type silicon clathrate in hydrogen fluoride solution. That is, since I-type silicon clathrate has higher solubility in hydrogen fluoride solution, it is considered that I-type silicon clathrate can be removed from silicon clathrate particles by contacting silicon clathrate particles containing I-type silicon clathrate and II-type silicon clathrate with hydrogen fluoride solution.

[0014] By removing type I silicon clathrate, which expands and contracts more than type II silicon clathrate during charging and discharging of the battery, the ratio of type II silicon clathrate becomes relatively larger, thereby suppressing the increase in confining pressure during charging and discharging.

[0015] In the present disclosure, the "electrode active material" can be used as either a "positive electrode active material" or a "negative electrode active material", and is particularly used as a "negative electrode active material".

[0016] <Provision of silicon clathrate particles> The method of the present disclosure includes providing silicon clathrate particles that contain a silicon clathrate type I and a silicon clathrate type II.

[0017] Such silicon clathrate particles can be prepared by preparing a sodium silicon (NaSi) alloy and removing the sodium from the NaSi alloy.

[0018] Specifically, a silicon source is reacted with a sodium source such as sodium hydride to prepare a NaSi alloy. The NaSi alloy thus prepared is then heated to remove sodium from the NaSi alloy and form a clathrate, thereby preparing silicon clathrate particles. Alternatively, the NaSi alloy thus prepared is reacted with aluminum fluoride as a sodium trapping agent to remove sodium from the NaSi alloy and form a clathrate, thereby preparing silicon clathrate particles.

[0019] <Removal of type I silicon clathrate> The method of the present disclosure includes contacting silicon clathrate particles with a hydrogen fluoride solution to remove at least a portion of the type I silicon clathrate.

[0020] In the method of the present disclosure, the ratio of the amount of hydrogen fluoride (mol) in the hydrogen fluoride solution to the mass (g) of the silicon clathrate particles (HF [mol] / Si [g]) is preferably 0.006 mol / g or more and 0.25 mol / g or less. This ratio may be 0.01 mol / g or more, 0.02 mol / g or more, 0.03 mol / g or more, 0.04 mol / g or more, or 0.05 mol / g or more, and may be 0.20 mol / g or less, or 0.15 mol / g or less, 0.13 mol / g or less, or 0.11 mol / g or less. When this ratio is within the above range, the I-type silicon clathrate can be highly selectively removed from the silicon clathrate particles.

[0021] The solvent of the hydrogen fluoride solution may be water, an organic solvent, or a mixed solvent of water and an organic solvent. When the solvent contains water, that is, when the solvent is water or a mixed solvent of water and an organic solvent, particularly when the solvent is a mixed solvent of water and an organic solvent, sodium silicofluoride (Na 2 SiF 6 This is preferable in that the production of by-products such as

[0022] Furthermore, when the contact involves a mixing operation such as stirring, foaming occurs when the solvent is water alone, whereas foaming can be suppressed when a mixed solvent of water and an organic solvent is used.

[0023] In the mixed solvent, the ratio of the mass of water to the total mass of water and the organic solvent may be 30% by mass or more and 90% by mass or less, and this ratio may be 40% by mass or more, 50% by mass or more, 60% by mass or more, 70% by mass or more, 80% by mass or more, or 85% by mass or less, and may be 89% by mass or less, 88% by mass or less, or 87% by mass or less.

[0024] The organic solvent may be any organic solvent capable of dissolving hydrogen fluoride, and when the organic solvent is used in combination with water, any organic solvent capable of dissolving hydrogen fluoride and compatible with water may be used. The organic solvent is preferably an alcohol, more preferably a lower alcohol, and even more preferably ethanol.

[0025] The time for which the silicon clathrate particles are contacted with the hydrogen fluoride solution may be 0.1 hours or more, 0.3 hours or more, or 0.5 hours or more, and may be 6 hours or less, 5 hours or less, or 4 hours or less.

[0026] The content ratio of the I-type silicon clathrate and the II-type silicon clathrate in the silicon clathrate particles can be calculated, for example, from the peak intensity ratio in the measurement results of X-ray diffraction (XRD).

[0027] <Application> The silicon clathrate electrode active material in the method of the present disclosure can be used as the negative electrode active material in a lithium ion battery.

[0028] <<How lithium-ion batteries are manufactured>> The disclosed method of making a lithium ion battery includes making a silicon clathrate electrode active material and forming an electrode active material layer containing the silicon clathrate electrode active material.

[0029] For the method for producing the silicon clathrate electrode active material, reference can be made to the above description regarding the method for producing the silicon clathrate electrode active material of the present disclosure.

[0030] The method for forming the electrode active material layer is not particularly limited, and a known method can be adopted. For example, when the negative electrode active material layer contains the silicon clathrate electrode active material of the present disclosure, the electrode active material layer formed on the negative electrode current collector layer, i.e., the negative electrode active material layer, can be obtained by applying a slurry containing the silicon clathrate electrode active material to the negative electrode current collector and drying it.

[0031] The method for forming the battery is not particularly limited, and any known method can be used. Hereinafter, a method for producing a battery in which the negative electrode active material layer contains the silicon clathrate electrode active material of the present disclosure will be described.

[0032] The method for manufacturing a battery according to the present disclosure may include, in addition to manufacturing a silicon clathrate electrode active material and forming a negative electrode active material layer containing the silicon clathrate electrode active material, arranging, in this order, a negative electrode current collector layer, a negative electrode active material layer, an electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer.

[0033] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, copper, a copper alloy, and copper plated or vapor-deposited with nickel, chromium, carbon, or the like may be used, but is not limited to these.

[0034] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0035] <Negative electrode active material layer> The negative electrode active material layer of the present disclosure is a layer containing a negative electrode active material, and optionally an electrolyte, a conductive assistant, and a binder.

[0036] (Negative electrode active material) The negative electrode active material comprises a silicon clathrate electrode active material of the present disclosure.

[0037] (electrolyte) The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.

[0038] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li 2 SP 2 S 5 System (Li 7 P 3 S 11 , Li 3 P.S. 4 , Li 8 P 2 S 9 etc.), Li 2 S-SiS 2 , LiI-Li 2 S-SiS 2 , LiI-Li 2 SP 2 S 5 , LiI-LiBr-Li 2 SP 2 S 5 , Li 2 SP 2 S 5 -GeS 2 (Li 13 GeP 3 S 16 , Li 10 GeP 2 S 12 etc.), LiI-Li 2 SP 2 O 5 , LiI-Li 3 PO 4 -P 2 S 5 , Li 7-x P.S. 6-x Cl x etc.; or combinations thereof, but are not limited to these.

[0039] The sulfide solid electrolyte may be a glass or a crystallized glass (glass ceramic).

[0040] When the negative electrode active material layer contains a solid electrolyte, the mass ratio of the silicon clathrate electrode active material to the solid electrolyte in the negative electrode active material layer (mass of silicon clathrate electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0041] The electrolyte preferably contains a supporting salt and a solvent.

[0042] As a supporting salt (lithium salt) of the electrolyte having lithium ion conductivity, for example, LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 Inorganic lithium salts such as LiCF 3 SO 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , LiN(FSO 2 ) 2 , LiC(CF 3 SO 2 ) 3 Examples of organic lithium salts include those mentioned above.

[0043] Examples of the solvent used in the electrolytic solution include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolytic solution preferably contains two or more kinds of solvents.

[0044] (Conductive assistant) The conductive assistant is not particularly limited. For example, the conductive assistant may be VGCF (Vapor Grown Carbon Fiber), acetylene black (AB), Ketjen Black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.

[0045] (binder) The binder is not particularly limited. For example, the binder may be a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.

[0046] The thickness of the negative electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0047] <Electrolyte layer> The electrolyte layer includes at least an electrolyte. The electrolyte layer may include a binder, etc., if necessary, in addition to the electrolyte. For the electrolyte and the binder, the above description regarding the negative electrode active material layer of the present disclosure can be referred to.

[0048] The thickness of the electrolyte layer is, for example, 0.1 to 300 μm, and preferably 0.1 to 100 μm.

[0049] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally an electrolyte, a conductive assistant, a binder, and the like.

[0050] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material is lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), lithium manganate (LiMn 2 O 4 ), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2 , Li 1+x Mn 2-x-y MyO 4 Li-Mn spinel substituted with different elements having a composition represented by the formula (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO 4 , M may be one or more metals selected from Fe, Mn, Co, and Ni), but is not limited thereto.

[0051] The positive electrode active material may have a coating layer. The coating layer is a layer containing a material that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials that constitute the coating layer include LiNbO 3 In addition, Li 4 Ti 5 O 12 , Li 3 PO 4 These include, but are not limited to, the following.

[0052] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0053] For the electrolyte, the conductive assistant, and the binder, reference can be made to the above descriptions regarding the negative electrode active material layer of the present disclosure.

[0054] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.

[0055] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0056] <Positive electrode current collector layer> The material used for the positive electrode current collector layer is not particularly limited, and any material that can be used as a positive electrode current collector for a battery can be appropriately adopted. For example, SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium, zinc, etc., and these metals plated or vapor-deposited with nickel, chromium, carbon, etc. may be used, but is not limited to these.

[0057] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0058] The lithium ion battery produced by the method of the present disclosure may be a liquid battery containing an electrolytic solution as an electrolyte layer, or may be a solid battery having a solid electrolyte layer as an electrolyte layer. In the present disclosure, a "solid-state battery" means a battery using at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. The solid-state battery of the present disclosure may also be an all-solid-state battery, i.e., a battery using only a solid electrolyte as an electrolyte.

[0059] The lithium ion battery produced by the method of the present disclosure may be a primary battery or a secondary battery.

[0060] Examples of the shape of the lithium ion battery include a coin type, a laminate type, a cylindrical type, and a square type. EXAMPLES

[0061] 《Synthesis of silicon clathrate electrode active material》 <Alloying> (Synthesis Example 1) As a silicon (Si) source, Si powder (Kojundo Kagaku, SIEPB32) was prepared. This Si powder and metallic lithium (Li) were weighed out in a molar ratio of Li / Si=4.0, and the weighed Si powder and Li were mixed in a mortar in an argon atmosphere to obtain a lithium silicon (LiSi) alloy. The obtained LiSi alloy was reacted with ethanol in an argon atmosphere and treated with hydrogen fluoride (HF) to obtain a Si powder having voids inside the primary particles, i.e., a Si powder having a porous structure.

[0062] A sodium silicon (NaSi) alloy was produced using Si powder having a porous structure and sodium hydride (NaH) as a sodium (Na) source. The NaH used was washed with hexane in advance. NaH and Si powder having a porous structure were weighed out so that the molar ratio was 1.05:1, and the weighed NaH and Si powder having a porous structure were mixed in a cutter mill. The resulting mixture was heated in a heating furnace under an argon atmosphere at 500°C for 40 hours to obtain a powdered NaSi alloy.

[0063] <Clathrate formation> Aluminum Fluoride (AlF 3 The ratio of the amount of the NaSi alloy to the amount of the NaSi alloy was 0.34. 3 The powdered reaction raw material was mixed in a cutter mill to obtain a reaction raw material. The obtained powdered reaction raw material was placed in a stainless steel reaction vessel and heated in a heating furnace under an argon atmosphere at 340°C for 60 hours to obtain a reaction product containing silicon clathrate particles. The obtained reaction product was dissolved in HNO 3 and H 2 The reaction product was washed with an acid using a mixed solvent of 10:90 by volume of O, and the by-products in the reaction product were removed. After washing, the mixture was filtered, and the filtered solid was dried at 120°C for 3 hours or more to obtain a composition containing silicon clathrate particles containing silicon clathrate I and silicon clathrate II.

[0064] (Synthesis Examples 2 to 5) Compositions containing silicon clathrate particles of Synthesis Examples 2 to 5 were obtained in the same manner as in Synthesis Example 1, except that the production conditions for clathration were as shown in Table 1.

[0065] The content ratio of each component in the composition containing the silicon clathrate particles of each synthesis example, and the ratio of the mass of the II-type silicon clathrate to the total mass of the I-type silicon clathrate and the II-type silicon clathrate are shown in Table 1. The ratio of the contained components was calculated from the peak intensity ratio in the XRD measurement results. In addition, in Table 1 and Tables 2 and 3 described later, "II-type" indicates the II-type silicon clathrate, and "I-type" indicates the I-type silicon clathrate.

[0066] [Table 1]

[0067] <Removal of type I silicon clathrate> Example 1 To 2.2 g of the composition containing silicon clathrate particles of Synthesis Example 1, 75 ml of ion-exchanged water and 20 ml of ethanol were added and stirred so that the ratio of the mass of water to the total mass of water and ethanol was 86.7 mass%. A 46 wt% HF aqueous solution was added thereto so that HF ​​[mol] / Si [g] was 0.0055 mol / g. This solution was reacted by stirring for 0.5 hours to remove the I-type silicon clathrate. The resulting reaction solution was filtered, and the filtered solid was washed three times with 50 ml of ion-exchanged water and once with 20 ml of ethanol. After washing, the mixture was dried overnight at 120°C to obtain the silicon clathrate electrode active material of Example 1.

[0068] (Examples 2 to 8) Silicon clathrate electrode active materials of Examples 2 to 8 were obtained in the same manner as in Example 1, except that the conditions for removing the I-type silicon clathrate were as shown in Table 2.

[0069] The results of Examples 1 to 8 regarding the yield of the I-type silicon clathrate removal step, the content ratio of each component in the silicon clathrate electrode active material, and the ratio of the mass of the II-type silicon clathrate to the total mass of the I-type silicon clathrate and the II-type silicon clathrate are shown in Table 2. In Table 2 and Table 3 described later, "Si" indicates a composition containing silicon clathrate particles.

[0070] [Table 2]

[0071] As shown in Examples 1 to 3 in Table 2, the content ratio of I-type silicon clathrate decreased after the I-type silicon clathrate removal process. According to the methods of Examples 2 and 3 in which HF [mol] / Si [g] was 0.0545 mol / g and 0.1091 mol / g, respectively, the I-type silicon clathrate could be removed with high selectivity.

[0072] As shown in Examples 4 to 6 in Table 2, even if the stirring time in the I-type silicon clathrate removal step was different, the I-type silicon clathrate could be removed with high selectivity.

[0073] As shown in Examples 7 and 8 in Table 2, when removal of type I silicon clathrate was carried out using a composition containing silicon clathrate particles with a small proportion of type I silicon clathrate, the type I silicon clathrate could be completely removed.

[0074] Example 9 100 ml of ethanol was added to 2.2 g of a composition containing silicon clathrate particles and stirred. A 46 wt% HF aqueous solution was added thereto so that HF ​​[mol] / Si [g] was 0.0449 mol / g. The solution was reacted by stirring for 3 hours to remove the I-type silicon clathrate. The resulting reaction solution was filtered, and the filtered solid was washed 8 times with 25 ml of ethanol. After washing, the mixture was dried overnight at 60°C to obtain the silicon clathrate electrode active material of Example 9.

[0075] Example 10 A silicon clathrate electrode active material of Example 10 was obtained in the same manner as in Example 9, except that the conditions for removing the I-type silicon clathrate were changed as shown in Table 3.

[0076] [Table 3]

[0077] As shown in Table 3, the method of Example 9 was able to highly selectively remove the I-type silicon clathrate. However, since the solvent in the I-type silicon clathrate removal step was only ethanol, the by-product Na 2 SiF 6 was thought to have been a large proportion.

[0078] In the method of Example 10, the I-type silicon clathrate could be removed. However, because the HF [mol] / Si [g] was large and the stirring time in the I-type silicon clathrate removal step was too long, not only the I-type silicon clathrate but also the II-type silicon clathrate was dissolved, resulting in a low yield and a small proportion of the II-type silicon clathrate. In addition, because the solvent in this step was only ethanol, the by-product Na 2 SiF 6 was thought to have been a large proportion.

Claims

1. A method for producing a silicon clathrate electrode active material, comprising the steps of: (a) providing silicon clathrate particles containing a silicon clathrate type I and a silicon clathrate type II; and (b) contacting the silicon clathrate particles with a hydrogen fluoride solution to remove at least a portion of the I-type silicon clathrate.

2. The method according to claim 1, wherein in step (b), the ratio of the amount of hydrogen fluoride to the mass of the silicon clathrate particles is greater than 0.0060 mol / g and less than 0.2500 mol / g.

3. The method according to claim 1 , wherein the hydrogen fluoride solution is a mixed solvent of water and an organic solvent.

4. The method according to claim 1 , wherein in the mixed solvent, a ratio of the mass of the water to a total mass of the water and the organic solvent is 30 mass % or more and 90 mass % or less.

5. 10. The method of claim 1, wherein the silicon clathrate electrode active material is for use as an anode active material in a lithium ion battery.

6. Producing a silicon clathrate electrode active material by the method according to any one of claims 1 to 5; and forming an electrode active material layer containing the silicon clathrate electrode active material; A method for producing a lithium ion battery, comprising:

Citation Information

Patent Citations

  • Method for producing purified silicon fine particles

    JP2021042112A

  • Method for manufacturing negative electrode active material

    JP2023043948A

  • Active material, negative electrode layer, battery, and manufacturing method thereof

    JP2023044620A

  • Negative electrode active material, negative electrode comprising negative electrode active material, secondary battery comprising negative electrode, and method for preparing negative electrode active material

    WO2023033370A1

  • Active material, negative electrode layer, battery and these manufacturing methods

    JP2021158004A