Method for manufacturing silicon clathrate electrode active material, and method for manufacturing lithium-ion battery

By employing a hydrogen fluoride solution to remove sodium from silicon clathrate electrode active materials, the method addresses inefficient sodium removal, enhancing processing efficiency and reducing residual sodium content, thereby improving lithium ion battery performance.

JP2024165116AActive Publication Date: 2024-11-28TOYOTA JIDOSHA KK

Patent Information

Application Number
JP2023080996
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-28
Estimated Expiration
2043-05-16

AI Technical Summary

Technical Problem

The production of silicon clathrate electrode active materials is hindered by inefficient sodium removal processes, leading to high residual sodium content, which affects the processing efficiency and performance of lithium ion batteries.

Method used

A method involving the use of a hydrogen fluoride solution, preferably a mixed solvent of water and an organic solvent, to remove sodium from sodium-containing silicon clathrate, optimizing the sodium removal process and reducing residual sodium content in the silicon clathrate electrode active material.

Benefits of technology

The method enhances the processing efficiency of sodium removal and significantly reduces the residual sodium content in the silicon clathrate electrode active material, improving its suitability for lithium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024165116000001
    Figure 2024165116000001
Patent Text Reader

Abstract

To provide a method for manufacturing a silicon clathrate electrode active material capable of increasing the throughput of a sodium-containing silicon clathrate in a sodium removal step and capable of reducing the amount of sodium remaining in the obtained silicon clathrate electrode active material, and a method for manufacturing a lithium-ion battery comprising manufacturing such a silicon clathrate electrode active material.SOLUTION: The method of the present disclosure for manufacturing a silicon clathrate electrode active material comprises (a) providing a sodium-containing silicon clathrate; and (b) contacting the sodium-containing silicon clathrate with a hydrogen fluoride solution to remove at least a portion of sodium from the sodium-containing silicon clathrate.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for producing a silicon clathrate electrode active material and a method for producing a lithium ion battery. [Background technology]

[0002] In recent years, the development of batteries has been actively carried out. For example, in the automobile industry, development of batteries for use in electric vehicles or hybrid vehicles is underway. Silicon is also known as an electrode active material for batteries, particularly lithium ion batteries.

[0003] Silicon electrode active materials have a large theoretical capacity and are effective in increasing the energy density of batteries. On the other hand, silicon electrode active materials have a problem of large expansion during charging. It is known that the expansion during charging can be suppressed by using a silicon clathrate electrode active material as the silicon electrode active material.

[0004] For example, Patent Document 1 discloses a silicon clathrate electrode active material having a silicon clathrate type II crystal phase, having voids inside the primary particles, and having a void volume of pores having a pore diameter of 100 nm or less of 0.05 cc / g or more and 0.15 cc / g or less. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2021-158004 Summary of the Invention [Problem to be solved by the invention]

[0006] Silicon clathrate electrode active materials can be produced by removing sodium from sodium-containing silicon clathrates, but there is a need to improve the efficiency of treating the sodium-containing silicon clathrate in this process and to reduce the amount of sodium remaining in the resulting silicon clathrate electrode active material.

[0007] An object of the present disclosure is to provide a method for producing a silicon clathrate electrode active material, which can improve the treatment efficiency of sodium-containing silicon clathrate in a sodium removal step and reduce the amount of sodium remaining in the obtained silicon clathrate electrode active material, and a method for producing a lithium ion battery, which includes producing such a silicon clathrate electrode active material. [Means for solving the problem]

[0008] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> A method for producing a silicon clathrate electrode active material, comprising the steps of: (a) providing a sodium-containing silicon clathrate; and (b) contacting the sodium-containing silicon clathrate with a hydrogen fluoride solution to remove at least a portion of the sodium from the sodium-containing silicon clathrate. <Aspect 2> The method according to aspect 1, wherein the solvent for the hydrogen fluoride solution is a mixed solvent of water and an organic solvent. <Aspect 3> 3. The method of any one of the preceding claims, wherein the sodium-containing silicon clathrate has a porous structure. <Aspect 4> The method according to any one of aspects 1 to 3, wherein the silicon clathrate electrode active material is for use as a negative electrode active material in a lithium ion battery. <Aspect 5> Producing a silicon clathrate electrode active material by the method according to any one of aspects 1 to 4; and forming an electrode active material layer containing the silicon clathrate electrode active material; A method for producing a lithium ion battery, comprising: Effect of the Invention

[0009] According to the method for producing a silicon clathrate electrode active material of the present disclosure, the efficiency of treating the sodium-containing silicon clathrate in the sodium removal step can be improved, and the amount of sodium remaining in the obtained silicon clathrate electrode active material can be reduced. In addition, the present disclosure can provide a method for producing a lithium-ion battery, which includes producing a silicon clathrate electrode active material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0011] <<Method for producing silicon clathrate electrode active material>> The disclosed method of making a silicon clathrate electrode active material includes (a) providing a sodium-containing silicon clathrate, and (b) contacting the sodium-containing silicon clathrate with a hydrogen fluoride solution to remove at least a portion of the sodium from the sodium-containing silicon clathrate.

[0012] As a method for producing a silicon clathrate electrode active material, for example, a sodium-containing silicon clathrate (e.g., Na 20 S 136 ) is mixed with zinc chloride and calcined to remove sodium (Na) from the sodium-containing silicon clathrate, resulting in a silicon clathrate with a reduced amount of sodium (e.g., Na2Si 136 ) is one method.

[0013] However, since the reaction in this method is a solid-phase reaction, it requires a relatively long reaction time. The present inventors have found that instead of or in addition to this reaction, Na can be efficiently removed from the sodium-containing silicon clathrate by contacting the sodium-containing silicon clathrate with a hydrogen fluoride (HF) solution.

[0014] In addition, with respect to the present disclosure, the "electrode active material" can be used as either a "positive electrode active material" or a "negative electrode active material", and is particularly used as a "negative electrode active material".

[0015] <Provision of sodium-containing silicon clathrate> The method of the present disclosure includes providing a sodium-containing silicon clathrate.

[0016] Sodium-containing silicon clathrates can be prepared by removing sodium from sodium silicon (NaSi) alloys.

[0017] Specifically, a silicon source is reacted with a sodium source such as sodium hydride to prepare a NaSi alloy. The NaSi alloy thus prepared is then heated to remove sodium from the NaSi alloy and form a clathrate, thereby preparing a silicon clathrate. Alternatively, the NaSi alloy thus prepared is reacted with aluminum fluoride as a sodium trapping agent to remove sodium from the NaSi alloy and form a clathrate, thereby preparing a silicon clathrate.

[0018] The sodium-containing silicon clathrate may have a porous structure, which is preferable in that the contact area between the sodium-containing silicon clathrate and the hydrogen fluoride (HF) solution is large, improving the efficiency of removing Na.

[0019] <Sodium Removal> The method of the present disclosure includes contacting a sodium-containing silicon clathrate with a hydrogen fluoride solution to remove at least a portion of the sodium from the sodium-containing silicon clathrate.

[0020] The solvent of the hydrogen fluoride solution may be water, an organic solvent, or a mixed solvent of water and an organic solvent. When the solvent contains water, that is, when the solvent is water or a mixed solvent of water and an organic solvent, particularly when the solvent is a mixed solvent of water and an organic solvent, it is preferable in that the generation of by-products such as sodium silicofluoride (Na2SiF6) can be suppressed.

[0021] It is preferable that the solvent contains an organic solvent in order to reduce the amount of water remaining in the silicon clathrate electrode active material. The proportion of the organic solvent in the solution may be 80% by mass or more, 90% by mass or more, or 95% by mass or more.

[0022] The organic solvent may be any organic solvent capable of dissolving hydrogen fluoride, and when the organic solvent is used in combination with water, any organic solvent capable of dissolving hydrogen fluoride and compatible with water may be used. The organic solvent is preferably an alcohol, more preferably a lower alcohol, and even more preferably ethanol.

[0023] In the method of the present disclosure, the ratio of the amount of hydrogen fluoride (mol) to the mass (g) of silicon clathrate (HF [mol] / Si [g]) may be 0.01 mol / g or more, 0.02 mol / g or more, 0.03 mol / g or more, or 0.04 mol / g or more, and may be 0.20 mol / g or less. When this ratio is within the above range, Na can be efficiently removed from the sodium-containing silicon clathrate to Na.

[0024] The method for contacting the sodium-containing silicon clathrate with the hydrogen fluoride solution includes, but is not limited to, a mixing operation such as stirring.

[0025] The sodium-containing silicon clathrate may be contacted with the hydrogen fluoride solution for a period of time that is 0.5 hours or more, 1 hour or more, or 2 hours or more, and 6 hours or less, 5 hours or less, or 4 hours or less.

[0026] In the silicon clathrate electrode active material produced by the method of the present disclosure, the amount of sodium in the silicon clathrate electrode active material may be 6.5% by mass or less, 6.0% by mass or less, 5.5% by mass or less, 5.2% by mass or less, 5.0% by mass or less, 4.8% by mass or less, or 4.6% by mass or less.

[0027] The amount of sodium in the silicon clathrate electrode active material can be measured, for example, by inductively coupled plasma (ICP) analysis.

[0028] <Application> The silicon clathrate electrode active material obtained by the method of the present disclosure can be used as a negative electrode active material for lithium ion batteries.

[0029] <<How lithium-ion batteries are manufactured>> The disclosed method of making a lithium ion battery includes making a silicon clathrate electrode active material by the disclosed method and forming an electrode active material layer containing the silicon clathrate electrode active material.

[0030] For the method for producing the silicon clathrate electrode active material, reference can be made to the above description regarding the method for producing the silicon clathrate electrode active material of the present disclosure.

[0031] The method for forming the electrode active material layer is not particularly limited, and a known method can be adopted. For example, when the negative electrode active material layer contains the silicon clathrate electrode active material of the present disclosure, the electrode active material layer formed on the negative electrode current collector layer, i.e., the negative electrode active material layer, can be obtained by applying a slurry containing the silicon clathrate electrode active material to the negative electrode current collector and drying it.

[0032] The method for forming the battery is not particularly limited, and any known method can be used. Hereinafter, a method for producing a battery in which the negative electrode active material layer contains the silicon clathrate electrode active material of the present disclosure will be described.

[0033] The method for manufacturing a battery according to the present disclosure may include, in addition to manufacturing a silicon clathrate electrode active material and forming a negative electrode active material layer containing the silicon clathrate electrode active material, arranging, in this order, a negative electrode current collector layer, a negative electrode active material layer, an electrolyte layer, a positive electrode active material layer, and a positive electrode current collector layer.

[0034] <Negative electrode current collector layer> The material used for the negative electrode current collector layer is not particularly limited, and any material that can be used as a negative electrode current collector for a battery can be appropriately adopted. For example, copper, a copper alloy, and copper plated or vapor-deposited with nickel, chromium, carbon, or the like may be used, but is not limited to these.

[0035] The shape of the negative electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0036] <Negative electrode active material layer> The negative electrode active material layer of the present disclosure is a layer containing a negative electrode active material, and optionally an electrolyte, a conductive assistant, and a binder.

[0037] (Negative electrode active material) The negative electrode active material comprises a silicon clathrate electrode active material of the present disclosure.

[0038] (electrolyte) The material of the solid electrolyte is not particularly limited, and any material that can be used as a solid electrolyte for use in lithium ion batteries can be used. For example, the solid electrolyte may be a sulfide solid electrolyte.

[0039] Examples of sulfide solid electrolytes include, but are not limited to, sulfide amorphous solid electrolytes, sulfide crystalline solid electrolytes, and argyrodite-type solid electrolytes. Specific examples of sulfide solid electrolytes include Li2S-P2S5-based (Li7P3S 11 , Li3PS4, Li8P2S9, etc.), Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-P2S5-GeS2(Li 13 GeP3S 16 , Li 10 GeP2S 12 etc.), LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, Li 7-x P.S. 6-x Cl x etc.; or combinations thereof, but are not limited to these.

[0040] The sulfide solid electrolyte may be a glass or a crystallized glass (glass ceramic).

[0041] When the negative electrode active material layer contains a solid electrolyte, the mass ratio of the silicon clathrate electrode active material to the solid electrolyte in the negative electrode active material layer (mass of silicon clathrate electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 40:60.

[0042] The electrolyte preferably contains a supporting salt and a solvent.

[0043] Examples of supporting salts (lithium salts) for electrolytes having lithium ion conductivity include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6, and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3.

[0044] Examples of the solvent used in the electrolytic solution include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolytic solution preferably contains two or more kinds of solvents.

[0045] (Conductive assistant) The conductive assistant is not particularly limited. For example, the conductive assistant may be VGCF (Vapor Grown Carbon Fiber), acetylene black (AB), Ketjen Black (KB), carbon nanotube (CNT), carbon nanofiber (CNF), etc., but is not limited thereto.

[0046] (binder) The binder is not particularly limited. For example, the binder may be a material such as polyvinylidene fluoride (PVdF), butadiene rubber (BR), or styrene butadiene rubber (SBR), or a combination thereof, but is not limited thereto.

[0047] The negative electrode active material layer may have a thickness of, for example, 0.1 to 1000 μm.

[0048] <Electrolyte layer> The electrolyte layer includes at least an electrolyte. The electrolyte layer may include a binder, etc., if necessary, in addition to the electrolyte. For the electrolyte and the binder, the above description regarding the negative electrode active material layer of the present disclosure can be referred to.

[0049] The thickness of the electrolyte layer is, for example, 0.1 to 300 μm, and preferably 0.1 to 100 μm.

[0050] <Cathode active material layer> The positive electrode active material layer is a layer containing a positive electrode active material, and optionally an electrolyte, a conductive assistant, a binder, and the like.

[0051] The material of the positive electrode active material is not particularly limited. For example, the positive electrode active material may be lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), lithium manganese oxide (LiMn2O4), LiCo 1 / 3 Ni 1 / 3 Mn 1 / 3 O2, Li 1+x Mn 2-x-y Li-Mn spinel substituted with different elements, which has a composition represented by MyO4 (M is one or more metal elements selected from Al, Mg, Co, Fe, Ni, and Zn), and lithium titanate (Li x TiO y ), lithium metal phosphate (LiMPO4, M is one or more metals selected from Fe, Mn, Co, and Ni), and the like, but are not limited thereto.

[0052] The positive electrode active material may have a coating layer. The coating layer is a layer containing a substance that has lithium ion conductivity, is low in reactivity with the positive electrode active material and the solid electrolyte, and can maintain the shape of the coating layer without flowing even when it comes into contact with the active material and the solid electrolyte. Specific examples of materials constituting the coating layer include LiNbO3, Li4Ti5O 12 , Li3PO4, etc., but are not limited to these.

[0053] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0054] For the electrolyte, the conductive assistant, and the binder, reference can be made to the above descriptions regarding the negative electrode active material layer of the present disclosure.

[0055] When the positive electrode active material layer contains a solid electrolyte, the mass ratio of the positive electrode active material to the solid electrolyte in the positive electrode active material layer (mass of positive electrode active material: mass of solid electrolyte) is preferably 85:15 to 30:70, and more preferably 80:20 to 50:50.

[0056] The thickness of the positive electrode active material layer is, for example, 0.1 μm to 1000 μm, preferably 1 μm to 100 μm, and more preferably 30 μm to 100 μm.

[0057] <Positive electrode current collector layer> The material used for the positive electrode current collector layer is not particularly limited, and any material that can be used as a positive electrode current collector for a battery can be appropriately adopted. For example, SUS, nickel, chromium, gold, platinum, aluminum, iron, titanium, zinc, etc., and these metals plated or vapor-deposited with nickel, chromium, carbon, etc. may be used, but is not limited to these.

[0058] The shape of the positive electrode current collector layer is not particularly limited, and examples thereof include a foil shape, a plate shape, a mesh shape, etc. Among these, a foil shape is preferred.

[0059] The lithium ion battery produced by the method of the present disclosure may be a liquid battery containing an electrolytic solution as an electrolyte layer, or may be a solid battery having a solid electrolyte layer as an electrolyte layer. In the present disclosure, a "solid-state battery" means a battery using at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. The solid-state battery of the present disclosure may also be an all-solid-state battery, i.e., a battery using only a solid electrolyte as an electrolyte.

[0060] The lithium ion battery produced by the method of the present disclosure may be a primary battery or a secondary battery.

[0061] Examples of the shape of the lithium ion battery include a coin type, a laminate type, a cylindrical type, and a square type. EXAMPLES

[0062] 《Synthesis of silicon clathrate electrode active material》 <Alloying> A sodium silicon (NaSi) alloy was produced using Si powder and sodium hydride (NaH) as a sodium (Na) source. The NaH used was washed with hexane in advance. NaH and Si powder were weighed out so that the molar ratio was 1.05:1, and the weighed NaH and Si powder were mixed in a cutter mill. The resulting mixture was heated in a heating furnace under an argon atmosphere at 500°C for 40 hours to obtain a powdered NaSi alloy.

[0063] <Clathrate formation> The obtained NaSi alloy and aluminum fluoride (AlF3) were weighed out to a molar ratio of 1:0.35, and the weighed NaSi alloy and AlF3 were mixed in a cutter mill to obtain a reaction raw material. The obtained powdered reaction raw material was placed in a stainless steel reaction vessel and heated in a heating furnace under an argon atmosphere at 310°C for 60 hours to obtain a sodium-containing silicon clathrate (Na 20 S 136 ) was obtained.

[0064] <Sodium removal> Example 1 The obtained Na 20 S 136 100 ml of ethanol and 3.71 ml of 46% by mass aqueous hydrogen fluoride (HF) solution were added to the mixture and stirred. The solution was filtered, and the solid matter separated by filtration was washed with 25 ml of ethanol eight times and dried overnight at 60° C. under reduced pressure. 20 S 136 Thus, the silicon clathrate electrode active material of Example 1 was obtained, from which at least a portion of the sodium had been removed.

[0065] Comparative Example 1 Na 20 S 136 and zinc chloride (ZnCl2) were weighed out to a molar ratio of 1:0.75, and the weighed Na20 S 136 and ZnCl2 were mixed to obtain a powdered reaction raw material. The powdered reaction raw material was placed in a stainless steel reaction vessel and fired in a heating furnace under an Ar atmosphere at 430°C to cause a reaction. The reaction product was washed with a mixed solvent of HNO3 and H2O in a volume ratio of 10:90. This removed by-products from the reaction product. After washing, the mixture was filtered, and the filtered solid content was dried at 120°C for 3 hours or more to obtain a silicon clathrate electrode active material of Comparative Example 1.

[0066] Comparative Example 2 A silicon clathrate electrode active material of Comparative Example 2 was obtained in the same manner as in Comparative Example 1, except that the firing temperature was 450°C.

[0067] "evaluation" <Na 20 S 136 Processing capacity of In the sodium removal process, Na 20 S 136 The daily processable amount was calculated and expressed as a relative value with the value of Comparative Example 1 being set as 1.

[0068] <Sodium content after sodium removal process> The amount of sodium remaining in the silicon clathrate electrode active material after the sodium removal step was measured by inductively coupled plasma (ICP) analysis.

[0069] "result" The evaluation results are shown in Table 1.

[0070] [Table 1]

[0071] As shown in Table 1, Na 20 S 136 In the method of Example 1, sodium removal from the 20 S 136The amount of sodium that could be treated was large, and the amount of sodium remaining in the silicon clathrate electrode active material was small.

Claims

1. A method for producing a silicon clathrate electrode active material, comprising the steps of: (a) providing a sodium-containing silicon clathrate; and (b) contacting the sodium-containing silicon clathrate with a hydrogen fluoride solution to remove at least a portion of the sodium from the sodium-containing silicon clathrate.

2. The method according to claim 1 , wherein the hydrogen fluoride solution is a mixed solvent of water and an organic solvent.

3. The method of claim 1 , wherein the sodium-containing silicon clathrate has a porous structure.

4. 10. The method of claim 1, wherein the silicon clathrate electrode active material is for use as an anode active material in a lithium ion battery.

5. Producing a silicon clathrate electrode active material by the method according to any one of claims 1 to 4; and forming an electrode active material layer containing the silicon clathrate electrode active material; A method for producing a lithium ion battery, comprising:

Citation Information

Patent Citations

  • Manufacturing method of active material, active material and battery

    JP2020064716A

  • Method for producing purified silicon fine particles

    JP2021042112A

  • Active material, negative electrode layer, battery, and manufacturing method thereof

    JP2023044620A

  • Silicon clathrate electrode active material, negative electrode mixture, negative electrode active material layer, solid-state lithium-ion battery, and method for manufacturing negative electrode active material layer

    JP2024160567A

  • Silicon clathrate electrode active material, negative electrode mixture, negative electrode active material layer, solid-state lithium-ion battery

    JP2024162152A

Cited By

  • Method for producing porous silicon electrode active material particles, porous silicon electrode active material particles, electrode composite material, and battery

    CN122748654A

  • Method for producing porous silicon electrode active material particles, porous silicon electrode active material particles, electrode mixture, and battery

    EP4806842A1

  • Method for manufacturing porous silicon electrode active material particles, porous silicon electrode active material particles, electrode composite material, and battery

    JP2026150843A

  • Method for producing porous silicon electrode active material particles, porous silicon electrode active material particles, electrode mixture, and battery

    KR1020260139020A