Sanitary ware

The sanitary ware design with a specific glaze layer and perfluoropolyether chains addresses the challenge of dirt adhesion and durability by enabling easy stain removal and maintaining appearance under high-load conditions.

JP2024167402AInactive Publication Date: 2024-12-03TOTO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024153474
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-08-08
Filing Date
2024-09-05
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Sanitary ware surfaces in high-load environments lose functionality due to adhesion of dirt and stains, requiring excessive cleaning effort and compromising durability.

Method used

A sanitary ware design incorporating a glaze layer with specific surface roughness and perfluoropolyether chains, characterized by a ratio of oxygen atoms and carbon-fluorine bonds, enhances sliding resistance and durability while maintaining antifouling properties.

Benefits of technology

The design allows for easy removal of dirt and stains with minimal cleaning effort, even under heavy use, while maintaining a durable and aesthetically pleasing appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167402000001_ABST
    Figure 2024167402000001_ABST
Patent Text Reader

Abstract

To provide a sanitary ware having both good antifouling property and high durability.SOLUTION: A sanitary ware includes a base material 1 for a sanitary ware, and a glazed layer 2 provided on a surface of the base material, wherein the glazed layer has arithmetic average line roughness Ra of the surface of 0.03 μm or more and 2.5 μm or less, the surface of the sanitary ware contains a perfluoropolyether chain 3, a ratio of the number of oxygen atoms in the perfluoropolyether chain to the number of all the carbon atoms having a C-F bond of the perfluoropolyether chain, which is obtained by peak separation of spectra of the surface of the sanitary ware by X-ray photoelectron spectroscopy (XPS), is 0.1 or more and 1.0 or less, and a ratio of the number of carbon atoms having a CF3 bond in the perfluoropolyether chain to the number of all the carbon atoms having a C-F bond of the perfluoropolyether chain is 20 at% or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sanitary ware that is used in an environment where it may be splashed with water and that has both good stain resistance and high durability. [Background technology]

[0002] Components used in wet areas (so-called wet area components) are used in environments where water is present. Therefore, water easily adheres to the surfaces of wet area components. When the water that adheres to the surface dries, limescale containing silica and calcium, which are components contained in tap water, is formed on the surface of the wet area component. In addition, dirt such as proteins, sebum, microorganisms such as mold, and metal soaps also easily adhere to the surface of the wet area component. In order to prevent the adhesion of dirt such as limescale to the surface of the wet area component and to improve the removability of dirt, a technology is known for modifying the surface of the component by coating it with a protective layer, for example.

[0003] However, there have been problems with providing a protective layer on wet-area components, such as coloring of the surface of the components, or damage or peeling of the protective layer, which impairs the appearance of the components. To solve this problem, monomolecular films that chemically bond with wet-area components have been used. Since a monomolecular film is a thin layer that cannot be seen with the naked eye, the function of a monomolecular film can be imparted to the components without impairing their appearance by providing a monomolecular film. In addition, since the monomolecular film chemically bonds with wet-area components, the durability of the film is improved. For example, it is known that a monomolecular film containing a fluoroalkylsilane compound not only protects the surface of a component, but also has an antifouling effect. For example, JP 2005-206455 A (Patent Document 1) describes that a dirt-resistant ceramic product having wear resistance can be obtained by forming a film containing a fluoroalkylsilane compound on the surface of a tile.

[0004] On the other hand, it is difficult to completely prevent dirt from adhering to the surface of wet-area components, and dirt is removed by cleaning. For example, in the case of sanitary ware, attempts have been made to increase the smoothness of the surface to make it easier to remove dirt. However, the surface may become rough due to adhesion of dirt, and the hydrophilicity of the surface may decrease. There is still a demand for sanitary ware that can easily remove such adhered dirt. When removing adhered dirt or limescale, strong alkaline or strong acid detergents are used, the force required to wipe is increased, or the number of times of wiping is increased. In other words, wet-area components are placed in a high-stress environment. For this reason, thin films such as the monomolecular film containing the above-mentioned fluoroalkylsilane compound may lose their function early. In recent years, therefore, a technology has been proposed in which a compound containing a perfluoropolyether chain, which has superior adhesion and durability to wet-area components compared to fluoroalkylsilane compounds, is applied to the surface of the component.

[0005] For example, Japanese Patent Application Laid-Open No. 2011-021088 (Patent Document 2) describes the formation of an antifouling layer by applying an antifouling paint containing a base material made of perfluoropolyether and a solvent containing an alkane of a specific average molecular weight to the surface of sanitary ware having a glaze layer. According to Patent Document 2, perfluoropolyether contains CF 3 It contains side chains (paragraphs 0013-0014), and it is said that applying an antifouling paint containing this perfluoropolyether and an alkane with a specific average molecular weight forms an antifouling layer with excellent smoothness (paragraph 0016).

[0006] In addition, JP 2021-113323 A (Patent Document 3) describes that a hardened layer having good friction durability is formed by applying a surface treatment agent containing a perfluoropolyether group-containing compound to the surface of chemically strengthened glass. Specifically, the -(OC 6 F 12 ) a -(OC 5 F 10 ) b -(OC 4 F 8 )c -(OC 3 F 6 ) d -(OC 2 F 4 ) e -(OCF 2 ) f In the above, the e / f ratio must be 0.9 or more, which increases the water and oil repellency of the cured layer. On the other hand, if the e / f ratio is too low, the lubricity (surface slipperiness) of the cured layer decreases, and if the e / f ratio is too high, the dynamic friction coefficient of the cured layer increases, and sufficient friction durability cannot be obtained (paragraph 0039). More specifically, the e / f ratio is preferably 1.0 or more (paragraph 0039), and in the [Examples], it is described that the cured layers formed by applying the surface treatment agents of Examples 1, 2, and 3 containing perfluoropolyether group-containing compounds with e / f ratios of 1.08, 1.03, and 1.08, respectively, showed good results in the eraser abrasion resistance test. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2005-206455 A [Patent Document 2] JP 2011-021088 A [Patent Document 3] Patent Publication No. 2021-113323 Summary of the Invention [Problem to be solved by the invention]

[0008] The present inventors have confirmed that some sanitary ware containing perfluoropolyether chains on the surface, which are generally considered to have high durability, lose their functions when used under high-load environments. The present inventors have now found a new configuration of sanitary ware that combines good stain resistance with higher durability, especially sliding resistance. That is, the inventors have found that by providing the uneven surface inherent to sanitary ware with specific perfluoropolyether chains, adhesion of stains can be effectively prevented, and even stains that generally require cleaning under high-load environments can be easily removed, i.e., with a small cleaning load. Furthermore, the inventors have found that a sanitary ware having high durability, especially sliding resistance, against the cleaning load when removing stains can be obtained. The present invention is based on these findings. [Means for solving the problem]

[0009] The sanitary ware according to the present invention comprises: The sanitary ware has a base material for sanitary ware and a glaze layer provided on a surface of the base material, The glaze layer has an arithmetic mean roughness Ra of its surface of 0.03 μm or more and 2.5 μm or less, the surface of the sanitary ware contains perfluoropolyether chains, the ratio of the number of oxygen atoms in the perfluoropolyether chain to the number of all carbon atoms having C-F bonds in the perfluoropolyether chain, which is obtained by peak separation of a spectrum obtained by measuring the surface of the sanitary ware by X-ray photoelectron spectroscopy (XPS), is 0.1 or more and 1.0 or less; The number of C F bonds in the perfluoropolyether chain relative to the number of all carbon atoms having C F bonds in the perfluoropolyether chain obtained by the peak separation. 3 The ratio of the number of carbon atoms having bonds is 20 at % or less. Effect of the Invention

[0010] According to the present invention, by providing a specific perfluoropolyether chain on the surface of a glaze layer having a specific surface roughness, a sanitary ware is provided that has excellent durability against sliding force and can maintain good stain resistance even when used under high-stress environments (environments in which strong alkaline or strong acid detergents are used to remove stains, wiping is performed with strong force, or wiping is performed frequently, etc.). In addition, according to the present invention, a sanitary ware is provided that combines the above-mentioned good stain resistance and high durability while maintaining a beautiful appearance that makes use of the properties unique to sanitary ware (e.g., texture, gloss, hardness, etc.). [Brief description of the drawings]

[0011] [Figure 1] 1A and 1B are a schematic view and an enlarged view showing an example of sanitary ware according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a sanitary ware surface before and after a load is applied to the surface. [Diagram 3] FIG. 13 shows the results of XPS spectrum and peak separation of the surface of sanitary ware produced using treatment liquid a. [Figure 4] FIG. 13 shows the results of XPS spectrum and peak separation of the surface of sanitary ware prepared using treatment liquid b. [Diagram 5] FIG. 13 shows the results of the XPS spectrum and peak separation of the surface of sanitary ware prepared using treatment liquid c. [Figure 6] FIG. 13 shows the results of XPS spectrum and peak separation of the surface of sanitary ware produced using treatment liquid d. [Figure 7] FIG. 13 shows the results of XPS spectrum and peak separation of the surface of sanitary ware prepared using treatment liquid e. [Figure 8] FIG. 13 shows the results of XPS spectrum and peak separation of the surface of sanitary ware produced using treatment liquid f. [Figure 9] FIG. 13 shows the results of XPS spectrum and peak separation of the surface of sanitary ware produced using treatment liquid g. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Sanitary ware In the present invention, "sanitary ware" refers to ceramic products used in bathrooms, toilet spaces, dressing rooms, washrooms, kitchens, etc. Specifically, it refers to toilet bowls, urinals, toilet basins, toilet tanks, wash basins, hand washing basins, etc.

[0013] Fig. 1A is a schematic diagram showing the cross-sectional structure of sanitary ware according to the present invention, and Fig. 1B is an enlarged view of the circled portion in Fig. 1A. As shown in Fig. 1A, sanitary ware 10 according to the present invention comprises a base for sanitary ware 1 and a glaze layer 2. The sanitary ware 10 contains perfluoropolyether chains 3 on the surface of the glaze layer 2.

[0014] Base for sanitary ware In the present invention, the sanitary ware base 1 is not particularly limited, and it is possible to utilize a known sanitary ware base used for sanitary ware 10. The sanitary ware base 1 may be a conventionally known sanitary ware base obtained by preparing, shaping, and firing silica sand, feldspar, limestone, clay, or the like as raw materials.

[0015] In one embodiment of the present invention, an intermediate layer made of another base material having properties different from those of the sanitary ware base material 1 may be provided between the glaze layer 2 and the sanitary ware base material 1. This makes it possible to suppress air bubbles from penetrating from the ceramic base material into the glaze layer 2 during the firing process during production, and forms a glaze layer 2 that is not only excellent in appearance but also in cleanability.

[0016] Glaze layer In the present invention, the arithmetic mean linear roughness Ra of the surface of the glaze layer 2 is 0.03 μm or more and 2.5 μm or less. Preferably, the arithmetic mean linear roughness Ra of the surface of the glaze layer 2 is 0.03 μm or more and 1.5 μm or less. More preferably, the arithmetic mean linear roughness Ra of the surface of the glaze layer 2 is 0.03 μm or more and 1.0 μm or less. The arithmetic mean linear roughness Ra is obtained by using a stylus type surface roughness measuring device conforming to JIS-B0651 (2001) in accordance with "7. Method and procedure of evaluation using a stylus type surface roughness measuring device" of JIS-B0633 (2001). In the present invention, the arithmetic mean linear roughness Ra of the surface of the glaze layer 2 is considered to be the same as the arithmetic mean linear roughness Ra of the surface of the sanitary ware 10. Therefore, it is possible to obtain the arithmetic mean linear roughness Ra of the glaze layer 2 by measuring the arithmetic mean linear roughness Ra of the surface of the sanitary ware 10. This is because the perfluoropolyether chains 3 contained in the surface of the sanitary ware 10 have a height that does not affect the surface roughness of the glaze layer 2. Specifically, the perfluoropolyether chains 3 preferably have a height of 20 nm or less. In the present invention, the glaze layer 2 may have a composition that is generally understood by those skilled in the art as a glaze layer, so long as its surface satisfies the above Ra. According to one embodiment of the present invention, the glaze layer 2 has a composition calculated in terms of oxides as shown in Table 1 below.

[0017] [Table 1]

[0018] According to a further embodiment of the present invention, the glaze layer 2 contains, in addition to the components listed in Table 1 above, Fe 2 O 3 , TiO 2 , BaO, B 2 O 3 , Li 2 O, Sb 2 O 3 , CuO, MnO, NiO, CoO, MoO 3 , SnO 2, PbO, etc. The glaze layer 2 may also contain particles. The particles include crystalline particles contained in the glaze raw materials and crystalline particles precipitated by firing. The material of the particles may be zircon, quartz, diopside, anorthite, etc.

[0019] In the present invention, the color of the glaze layer 2 is not particularly limited as long as the composition of the glaze layer 2 is within the range of Table 1. Examples of the color of the glaze layer 2 include white, black, ivory, pink, gray, brown, beige, green, red, and blue.

[0020] In the present invention, the arithmetic mean linear roughness Ra (0.03 μm or more and 2.5 μm or less) of the surface of the glaze layer 2 may be such that the surface of the glaze layer 2 is processed so that Ra falls within the above-mentioned range, or the surface of the base 1 for sanitary ware may be processed so that the Ra of the glaze layer 2 thereon falls within the above-mentioned range.

[0021] In the present invention, a primer layer may be provided on the surface of the glaze layer 2. By providing a primer layer, it is possible to form perfluoropolyether chains at a high density on the surface of the glaze layer. The primer layer is preferably one that does not affect the Ra of the surface of the glaze layer 2, and the thickness thereof is preferably on the order of nanometers. Specifically, the thickness is 20 nm or less, and more preferably 10 nm or less. The primer layer is made of SiO 2 generated by hydroxyl groups present on the surface. 2 , TiO 2 , Al 2 O 3 It is preferable that the layer contains a metal oxide such as the above.

[0022] Sanitary ware manufacturing In the present invention, the sanitary ware 10 can be produced, for example, by first forming a glaze layer 2 on a base 1 for the sanitary ware, and then applying a treatment liquid containing a compound that includes a perfluoropolyether chain 3 to the surface of the glaze layer 2. Specifically, it can be produced by the following method.

[0023] First, a molded body is prepared as the base material 1 for the sanitary ware. This is made by casting a conventionally known sanitary ware slip prepared from raw materials such as silica sand, feldspar, limestone, clay, etc., into a mold made of plaster, etc. After drying, the molded body is glazed as described below.

[0024] The raw material of the glaze forming the glaze layer 2 is not particularly limited as long as it can make the arithmetic mean linear roughness Ra of the surface of the glaze layer 2 0.03 μm or more and 2.5 μm or less, but may be, for example, a material that can realize the composition of the glaze layer described in Table 1 above. In addition, as the glaze raw material, a mixture of natural mineral particles such as silica sand, feldspar, limestone, etc., pigments such as cobalt compounds and iron compounds, opacifiers such as zirconium silicate and tin oxide, etc. may be used. In one embodiment of the present invention, the composition of the glaze raw material may be, for example, 10 wt% to 30 wt% feldspar, 15 wt% to 40 wt% silica sand, 10 wt% to 25 wt% calcium carbonate, 10 wt% or less each of corundum, talc, dolomite, and zinc oxide, and 15 wt% or less in total of opacifiers and pigments. The glaze can be obtained, for example, by melting the glaze raw material as described above at a high temperature and then quenching it to vitrify it.

[0025] The above-mentioned glaze is applied to the dried molded body, and then dried and fired to form a glaze layer 2 on the sanitary ware base 1. The firing temperature can be, for example, a temperature of 1000°C or higher and 1300°C or lower at which the glaze softens.

[0026] The surface of the formed glaze layer 2 may be subjected to a surface treatment as necessary within a range in which Ra satisfies the above-mentioned range. For example, blasting or etching may be performed. In blasting, the surface of the glaze layer 2 with Ra satisfying the above-mentioned range can be obtained by controlling the material / shape / particle size of the media used, the processing time per unit area, whether the processing is dry or wet, and the like. In etching, the surface of the glaze layer 2 with Ra satisfying the above-mentioned range can be obtained by controlling the photomask pattern, the concentration / type / temperature of the etching solution, whether stirring is performed, and the like. This can improve the glossiness of the surface, or reduce the glossiness to give it a matte finish.

[0027] The surface of the formed glaze layer 2 may have micro-roughness in a range where Ra satisfies the above-mentioned range. For example, when observed using a scanning probe microscope (SPM), the arithmetic mean surface roughness Sa at a viewing angle of 5.0 μm × 5.0 μm is preferably 0.03 μm or less. The arithmetic mean surface roughness Sa of the surface of the glaze layer 2 is obtained using a three-dimensional measuring machine described in JIS-B0681-6 (2014) in accordance with JIS-B0681-2 (2018). When the perfluoropolyether chain 3 provided on the surface of the glaze layer 2 having such micro-roughness Sa is highly flexible, the chain 3 can not only follow the surface shape in a range where Ra satisfies the above-mentioned range, but also follow the surface shape having micro-roughness in a micro-region, and it is considered that a sanitary ware excellent in abrasion resistance and resistance to alkaline components contained in detergents and the like (hereinafter referred to as alkali resistance) can be obtained. It is also believed that the presence of microscopic roughness in the microscopic regions improves water repellency and provides better stain resistance.

[0028] In the present invention, in addition to the above-mentioned methods for manufacturing the base material and glaze layer for sanitary ware, for example, methods for manufacturing the base material and glaze layer for sanitary ware described in JP 2021-134133 A, JP 2020-147492 A, WO99 / 61392 A, etc. can be used. In this specification, by referring to the above publications, the methods for manufacturing the base material and glaze layer for sanitary ware described in these publications are incorporated into the description of this specification as methods for manufacturing the base material and glaze layer for sanitary ware that can be used in the present invention.

[0029] Next, a treatment liquid containing a compound containing a perfluoropolyether chain 3, which will be described later, is applied to the surface of the glaze layer 2 formed on the sanitary ware base 1. A known method can be used to apply the treatment liquid containing the compound containing the perfluoropolyether chain 3. For example, the treatment liquid containing the compound containing the perfluoropolyether chain 3 can be applied by dipping, spin coating, wiping, vacuum deposition, spray gun, or the like. After the treatment liquid containing the compound containing the perfluoropolyether chain 3 is applied to the surface of the glaze layer 2, it is dried and cured as necessary, and then, in some cases and preferably, the surface of each sanitary ware is washed with a neutral detergent and a sponge, and then thoroughly rinsed with ultrapure water, to obtain a sanitary ware 10 containing the perfluoropolyether chain 3 on the surface of the glaze layer 2.

[0030] In the present invention, a pretreatment may be performed to remove dirt present on the surface and activate the hydroxyl groups on the surface before applying a treatment liquid containing a compound containing a perfluoropolyether chain 3 to the surface of the glaze layer 2. As the pretreatment to activate the hydroxyl groups on the surface, ultrasonic cleaning using an alkaline solution or particle polishing using metal fine particles may be used.

[0031] In the present invention, a primer layer may be formed on the surface of the glaze layer 2, and after performing pretreatment as necessary, a treatment liquid containing a compound having a perfluoropolyether chain 3 may be applied. The primer layer may be formed by, for example, a sol-gel method, a physical vapor deposition method (PVD), a chemical vapor deposition method (CVD), or the like.

[0032] Any treatment solution containing a compound having a perfluoropolyether chain 3 can be used as long as it can produce the sanitary ware of the present invention. 2 O, C 2 F 4 O, C 3 F 6 O, C 4 F 8 Examples of the compound containing the perfluoropolyether chain 3 include a compound having a structure shown in the following formula 1. [ka] Here, p, q, r, and s are the numbers of repeating units, i.e., integers of 0 or more, and the sum of p, q, r, and s is 3 to 200. The repeating units in the formula may be randomly bonded to form a chain, or polymer chains each made of the repeating units may be bonded to each other. f1 represents a fluorine atom or an organic group having one or more carbon atoms that contains a carbon atom to which a fluorine atom is singly bonded, and R f2 represents an organic group having one or more carbon atoms that contains a carbon atom to which a fluorine atom is singly bonded.

[0033] Further specific examples of the compound containing the perfluoropolyether chain 3 include compounds containing the structures shown in the following formulas 2 to 6. [ka] (In the formula, l:m:n=23.2:22.3:0.4 (average value), and the repeating units in the formula are arranged randomly.) [ka] (wherein the average value of l is 22.9), [ka] (wherein the average value of l is 23.2), [ka] (wherein the average value of l is 18), [ka] (wherein the average value of l is 23.4).

[0034] The compound containing the perfluoropolyether chain 3 is preferably a compound containing the perfluoropolyether chain 3 and at least one Si atom. It is more preferable that the compound is a compound in which the perfluoropolyether chain 3 is bonded to at least one reactive silyl group. This makes it easier for the surface of the glaze layer 2 to be bonded to the perfluoropolyether chain 3. The Si atom of the reactive silyl group may be bonded to one end of the perfluoropolyether chain 3 or to both ends, but is preferably bonded to one end. The reactive silyl group is a functional group in which an organic group not containing a fluorine atom in the Si atom is bonded to a hydroxyl group or a hydrolyzable group. The hydrolyzable group is specifically an alkoxy group, a halogeno group, etc., and more specifically, -OCH 3 , -OCH 2 CH 3 , -OCOCH 3 , -Cl, etc.

[0035] The solvent used in the treatment liquid may be any solvent that is miscible with the perfluoropolyether chain 3, and examples thereof include fluorine-based solvents, hexane, chain ether compounds, and cyclic ether compounds.

[0036] Perfluoropolyether Chain The surface of the sanitary ware 10 according to the present invention contains a perfluoropolyether chain 3. The perfluoropolyether chain 3 is a chain containing, in its structure, a repeating carbon atom to which a fluorine atom is bonded and an ether bond in which the carbon atom is bonded via an oxygen atom, and for example, -[(CF 2 ) x -O]-(x is a natural number) repeating unit.2 )-O, (C 2 F 4 )-O, (C 3 F 6 )-O, (C 4 F 8 In the present invention, the total number of repeating units is preferably as large as possible, and more preferably 200 or less.

[0037] The presence of the perfluoropolyether chains 3 on the surface of the sanitary ware 10 can be identified, for example, by the following analysis method.

[0038] The presence of the perfluoropolyether chains 3 on the surface of the sanitary ware 10 can be identified by X-ray photoelectron spectroscopy (XPS) and time-of-flight secondary ion mass spectrometry (TOF-SIMS).

[0039] First, the surface of the sanitary ware is evaluated by X-ray photoelectron spectroscopy (XPS) to obtain the C1s and F1s spectra. In this spectrum, the peak of fluorine atoms having a C-F bond in F1s (peak position: 687 eV to 690 eV) and the peak of carbon atoms having a C-F bond in C1s (peak position: 289 eV to 297 eV) are obtained, which indicates that the surface of the sanitary ware contains C-F bonds. Examples of compounds containing C-F bonds include perfluoropolyether chain-containing compounds and fluoroalkylsilane compounds. The XPS measurement is performed by "Acquisition of XPS spectrum" using the "XPS measurement conditions" described below.

[0040] The surface of the sanitary ware is then evaluated using TOF-SIMS. The TOF-SIMS device that can be used is TOF.SIMS5 (ION-TOF). TOF-SIMS is an analytical technique that detects secondary ions generated from a sample surface when the sample surface is irradiated with pulsed primary ions emitted from a primary ion source. The type of secondary ions generated and the detection sensitivity vary depending on the composition and chemical structure of the sample surface. By visualizing the distribution of various secondary ions on the sample surface, the distribution of the composition and chemical structure on the sample surface can be estimated.

[0041] By evaluating the surface of sanitary ware with TOF-SIMS using the following measurement conditions, a secondary ion mass spectrum can be obtained, with the horizontal axis representing the mass number (m / z, i.e., the value obtained by dividing the mass m by the charge z) and the vertical axis representing the secondary ion intensity (number of counts). [TOF-SIMS measurement conditions] Primary ion source: Bi 3+ Primary ion acceleration voltage: 30 keV Primary ion current value: 0.2pA (at 10kHz) Primary ion punching: Yes Measurement range: 500μm×500μm Cycle time: 400μs Number of pixels: 128 x 128 pixels Vacuum degree: 9 -8 hPa Secondary ion: Negative Ion Neutralization gun: Yes

[0042] From the C1s and F1s peaks obtained by XPS, it can be determined whether or not the surface of the sanitary ware 10 contains CF bonds. If it is determined by XPS that the surface of the sanitary ware contains CF bonds, it is possible to confirm, based on this, that the surface of the sanitary ware 10 contains perfluoropolyether chains 3 from the secondary ion mass spectrum obtained by TOF-SIMS under the above measurement conditions. Specifically, if there are fragments that appear periodically at equal mass intervals on the high mass side of the m / z of the secondary ion mass spectrum obtained by TOF-SIMS, which is several hundred or more, the molecular formula of the repeating unit can be inferred from the mass intervals. A similar inference can be made when there are multiple repeating units. From the presence of CF bonds obtained by XPS and the degree of agreement of the exact mass and isotopes obtained by TOF-SIMS, it can be determined that the molecular formula of the repeating unit is C x F y O z When there is a repeating unit identified as (x, y, z are integers equal to or greater than 1, where y=2x), it is determined that the repeating unit contains perfluoroether. In addition, the total number of repeating units can be determined from fragments that appear periodically at equal mass intervals. From the above TOF-SIMS analysis, it is determined that when the repeating unit contains perfluoroether and the total number of repeating units is at least 3, the surface of the sanitary ware 10 contains perfluoropolyether chains 3.

[0043] The perfluoropolyether chain 3 is preferably bonded to the glaze layer via a Si atom. The perfluoropolyether chain 3 is more preferably bonded to the glaze layer via a plurality of Si atoms. This improves the adhesion between the perfluoropolyether chain 3 and the glaze layer 2. The Si atom is preferably bonded to the end of the perfluoropolyether chain 3. It is more preferable that the Si atom is bonded to the end of the perfluoropolyether chain 3. Although the Si atom may be bonded to both ends of the perfluoropolyether chain 3, it is more preferable that the Si atom is bonded to one end of the perfluoropolyether chain 3. The Si atom bonded to the perfluoropolyether chain 3 may be derived from a reactive silyl group bonded to the perfluoropolyether chain 3 contained in the raw material, or may be a Si atom generated by activating the surface of the glaze layer.

[0044] The hydroxyl group or hydrolyzable group contained in the reactive silyl group preferably functions as a bonding point with the glaze layer 2. In other words, the hydroxyl group contained in the reactive silyl group, or the hydroxyl group obtained by hydrolysis of the hydrolyzable group, or the hydrogen atom contained in the hydroxyl group undergoes dehydration condensation with a functional group (such as a hydrogen atom or a hydroxyl group) present on the surface of the glaze layer 2. This allows the perfluoropolyether chain 3 to bond to the surface of the glaze layer 2. The perfluoropolyether chain 3 is preferably bonded to the glaze layer 2 via a Si atom. In the present invention, the reactive silyl group preferably contains many hydroxyl groups or hydrolyzable groups. This improves the adhesion between the perfluoropolyether chain 3 and the glaze layer 2.

[0045] The fact that the perfluoropolyether chain 3 is bonded to the glaze layer 2 via a Si atom can be confirmed by, for example, surface-enhanced Raman spectroscopy (SERS), 19 It can be identified by methods such as Si-NMR and infrared spectroscopy (IR).

[0046] The ratio of the number of oxygen atoms to the number of carbon atoms in the perfluoropolyether chain In the present invention, the ratio of the number of oxygen atoms to the number of all carbon atoms having C-F bonds in the perfluoropolyether chain 3, which is obtained by peak separation of a spectrum obtained by measuring the surface of the sanitary ware by X-ray photoelectron spectroscopy (XPS), is 0.1 or more. The higher the O / C ratio, the higher the flexibility of the perfluoropolyether chain 3, which is preferable. Specifically, the O / C ratio is preferably 0.2 or more, more preferably 0.3 or more, and even more preferably 0.4 or more. This gives the perfluoropolyether chain 3 excellent flexibility. The reasons for this are considered to be as follows, but the present invention is not limited thereto. The perfluoropolyether chain 3 contains fluorine atoms, oxygen atoms, and carbon atoms, and it is considered that the fluorine atoms and oxygen atoms are bonded to the carbon atoms. In general, atoms bonded to carbon atoms are located at the vertices of a regular tetrahedral structure, and therefore can freely rotate around the carbon single bond. Therefore, it can take an infinite number of conformations. In the case of a perfluoropolyether chain containing an ether bond, the presence of an oxygen atom between the two carbon atoms bonded to the oxygen atom of the ether bond makes it difficult for the two carbon atoms to interact with each other, and there is almost no energy difference due to the position of the twist. Therefore, an organic chain containing an ether bond can rotate relatively freely around the carbon-oxygen single bond. For example, a perfluoropolyether chain having many ether bonds can change its shape with a high degree of freedom compared to a fluoroalkylsilane compound that does not have an ether bond. That is, it is considered to have excellent flexibility. And, due to the excellent flexibility of the perfluoropolyether chain 3, the sanitary ware according to the present invention can have high durability, especially abrasion resistance. The method of calculating the O / C ratio will be described later.

[0047] In the present invention, it is considered that the higher the O / C ratio, the more excellent the flexibility of the perfluoropolyether chain 3, so the higher the O / C ratio is, the better. However, if the flexibility is too high, the perfluoropolyether chain is likely to fall sideways, and the height of the perfluoropolyether chain is reduced. This increases the probability that water or alkaline components will reach the glaze layer surface from the area where the film is worn away due to the load caused by repeated use, making it easier for water stains to adhere and film wear to occur. Therefore, the O / C ratio, which is an index of flexibility, is preferably 1.0 or less, more preferably 0.9 or less, and even more preferably 0.8 or less.

[0048] CF relative to the number of all carbon atoms with CF bonds in the perfluoropolyether chain 3 Percentage of carbon atoms with bonds In the present invention, the ratio of CF to the number of all carbon atoms having CF bonds in the perfluoropolyether chain 3 is obtained by peak separation of a spectrum obtained by measuring the surface of the sanitary ware by X-ray photoelectron spectroscopy (XPS). 3 The ratio of the number of carbon atoms having bonds (hereinafter referred to as "CF 3 The ratio of the number of carbon atoms having bonds (also called "the ratio of the number of carbon atoms having bonds") is 20 at % or less. CF 3 It is believed that the excellent flexibility of the perfluoropolyether chain 3 is maintained by controlling the ratio of the number of carbon atoms having bonds to 20 at % or less. 3 It is believed that when the ratio of the number of carbon atoms having bonds exceeds 20 at %, the flexibility of the perfluoropolyether chain 3 decreases. 3 If the ratio of the number of carbon atoms having bonds exceeds 20 at%, the possibility of containing perfluoroalkyl chains in the side chains increases, which is likely to cause steric hindrance, reducing the degree of rotational freedom of the ether bonds contained in the perfluoropolyether chain, which is the main chain, and thus reducing flexibility.

[0049] It is believed that the sanitary ware according to the present invention has the following effects by containing the specific perfluoropolyether chains 3 described above on the surface of the glaze layer having a unique uneven shape.

[0050] In the sanitary ware of the present invention, the specific perfluoropolyether chains 3 have high flexibility, so that the perfluoropolyether chains 3 can follow the inherent uneven shape of the surface of the glaze layer 2. Therefore, even when used under a high-load environment, the sanitary ware has excellent sliding resistance and can exhibit antifouling properties for a long period of time. FIG. 2A is a cross-sectional view of an example of the sanitary ware of the present invention when a load is applied to the surface of the sanitary ware by a sponge or the like and after that. When removing dirt attached to the sanitary ware surface, the load applied to the sanitary ware surface by a sponge or the like is considered to be applied downward and laterally (left and right). The sanitary ware 10 of the present invention exhibits a unique action effect of dispersing or releasing the force of the load applied to the bond between the perfluoropolyether chains 3 and the glaze layer 2 due to its highly flexible surface structure. Therefore, it is possible to suppress (reduce) wear of the perfluoropolyether chains 3 and maintain the sliding resistance function for a long period of time. In particular, when a force applied laterally is concentrated on the convex parts of the uneven shape, the perfluoropolyether chains 3 can exhibit their excellent flexibility to the maximum. Furthermore, in an embodiment in which the perfluoropolyether chains 3 form a film, the flexibility is further enhanced, wear of the film is further suppressed, and the sliding resistance function is maintained for a longer period of time.

[0051] As described above, the sanitary ware of the present invention makes the most of its flexibility by containing specific perfluoropolyether chains 3 on the surface of the glaze layer 2 having a unique uneven shape. As a result, the sanitary ware of the present invention can exhibit excellent abrasion resistance.

[0052] In the sanitary ware of the present invention, the specific perfluoropolyether chains 3 described above have high flexibility, so that the perfluoropolyether chains 3 can follow the inherent uneven shape of the surface of the glaze layer 2. This shows that the sanitary ware of the present invention is not only excellent in sliding resistance but also excellent in alkali resistance. Normally, even if a certain coating film provided on the surface of the glaze layer itself has alkali resistance, the glaze layer will dissolve when an alkaline component penetrates into the glaze layer, and as a result, the entire coating film provided on the surface of the glaze layer will disappear. However, by providing the perfluoropolyether chains 3 with high flexibility on the surface of the glaze layer, the perfluoropolyether chains 3 can follow the uneven shape of the glaze layer, improving the coverage of the surface. This makes it possible to prevent the alkaline component from penetrating into the glaze layer, and the alkali resistance function will be maintained for a longer period of time.

[0053] On the other hand, Figure 2B shows that CF 3 The cross-sectional view of sanitary ware containing perfluoropolyether chains with a ratio of the number of carbon atoms having bonds exceeding 20 at % and an O / C ratio of less than 0.1, i.e., low flexibility, is shown in Fig. 2B. As shown in Fig. 2B, the perfluoropolyether chains on the surface of the glaze layer having an uneven shape cannot withstand the force applied, especially in the lateral direction, and the perfluoropolyether chains are worn out, and it is considered that they cannot have sliding resistance.

[0054] In the sanitary ware of the present invention, when liquid is present on a sloping sanitary ware surface, the specific perfluoropolyether chain 3 described above has high flexibility, which improves the ability of the liquid to slide off. It is therefore believed that the amount of liquid remaining on the sloping sanitary ware surface can be reduced. In addition, the specific perfluoropolyether chain 3 described above has high flexibility, which makes it easier for liquid present on the sanitary ware surface to move to absorbent items such as tissue paper or dishcloths. It is therefore believed that the amount of liquid remaining on the sanitary ware surface when the liquid adhering to the sanitary ware surface is wiped off with an absorbent item can also be reduced.

[0055] In the case where a solid that is not dissolved in water or oily organic solvents is present on the inclined sanitary ware surface of the present invention, the specific perfluoropolyether chain 3 has high flexibility, and therefore the sliding property of the solid is improved. It is considered that this makes it easier to slide off solids present on the sanitary ware surface having an inclination angle of several degrees from the horizontal direction even when no external force is applied. In addition, even if a solid is strongly attached to the sanitary ware surface to the extent that it cannot be removed without mechanical force such as rubbing, the sliding property of the solid is improved due to the high flexibility of the specific perfluoropolyether chain 3, so it is considered that the solid can be removed, for example, with a much smaller mechanical force than when the solid is strongly attached to the sanitary ware surface not containing the specific perfluoropolyether chain. In other words, it is considered that the sanitary ware of the present invention, which contains the specific perfluoropolyether chain 3 on its surface, can remove solids while applying an efficient mechanical force.

[0056] The ratio of the number of fluorine atoms to the total number of carbon and oxygen atoms in the perfluoropolyether chain In the present invention, the ratio of the number of all fluorine atoms having C-F bonds to the total number of all carbon atoms having C-F bonds and oxygen atoms bonded thereto in the perfluoropolyether chain 3, which is obtained by peak separation of a spectrum obtained by measuring the surface of the sanitary ware by X-ray photoelectron spectroscopy (XPS), is preferably 1.1 or more and 1.7 or less. The F / (C+O) ratio is more preferably 1.1 or more and 1.5 or less. This gives the perfluoropolyether chain 3 excellent flexibility and excellent water repellency. The reasons for this are considered to be as follows, but the present invention is not limited thereto. The perfluoropolyether chain contains fluorine atoms, oxygen atoms, and carbon atoms, and it is considered that the fluorine atoms and oxygen atoms are bonded to the carbon atoms. In general, atoms bonded to carbon atoms are located at the vertices of a regular tetrahedral structure, and therefore can freely rotate around the carbon single bond. Therefore, it can take an infinite number of conformations. In the case of a perfluoropolyether chain containing an ether bond, the presence of an oxygen atom between the two carbon atoms bonded to the oxygen atom of the ether bond makes it difficult for the two carbon atoms to interact with each other, and there is almost no difference in energy due to the position of the twist. Therefore, an organic chain containing an ether bond can rotate relatively freely around the carbon-oxygen single bond. For example, a perfluoropolyether chain with many ether bonds can change its shape with a high degree of freedom compared to a fluoroalkyl chain that does not have an ether bond. In other words, it is considered to have excellent flexibility. In addition, the greater the ratio of fluorine atoms contained in the perfluoropolyether chain, the smaller the surface energy of the sanitary ware surface. In other words, it is considered to have excellent water repellency. The F / (C+O) ratio indicates the ratio of fluorine atoms to oxygen atoms, assuming that the number of carbon atoms is constant. Therefore, the higher the value of the F / (C+O) ratio, the higher the ratio of fluorine atoms, which means that the water repellency is excellent, and conversely, the lower the value of the F / (C+O) ratio, the higher the ratio of oxygen atoms, which means that the flexibility is excellent. For example, when the ratio of oxygen atoms present in the perfluoropolyether chain 3 is high, the ratio of fluorine atoms is correspondingly low, so that flexibility is increased but water repellency is decreased.Thus, the water repellency and flexibility of the perfluoropolyether chain are in a trade-off relationship, and it can be said that the balance between water repellency and flexibility is important for producing sanitary ware with high durability and high stain resistance. Therefore, due to the excellent water repellency and flexibility of the perfluoropolyether chain 3, the sanitary ware of the present invention can have high stain resistance and long-term durability, especially abrasion resistance. The method for calculating the F / (C+O) ratio will be described later.

[0057] In the present invention, the perfluoropolyether chain 3 is generally preferably one represented by the following formula 7. [ka] Here, p, q, r, and s are the numbers of repeating units, i.e., integers of 0 or more, and the sum of p, q, r, and s is 3 to 200. The repeating units in the formula may be randomly bonded to form a chain, or polymer chains each made of the repeating units may be bonded to each other. f1 and R f2 Each represents an organic chain containing carbon atoms in which hydrogen atoms are substituted with fluorine atoms. In addition, the repeating unit may be composed only of a straight chain or may include a side chain, but the straight chain is preferred.

[0058] More preferred examples of the perfluoropolyether chain 3 include perfluoropolyether chains represented by the following formulas 8 to 12. [ka] (wherein l:m:n=23.2:22.3:0.4 (average value), and the repeating units in the formula are arranged randomly.) [ka] (wherein the average value of l is 22.9), [ka] (wherein the average value of l is 23.2), [Chemical formula] (wherein the average value of l is 18.) [Chemical formula] (wherein the average value of l is 23.4).

[0059] XPS measurement method for sanitary ware surfaces In the present invention, the O / C ratio, the ratio of the number of carbon atoms having CF 3 bonds, and the F / (C + O) ratio are obtained by measuring the surface of the sanitary ware by X-ray photoelectron spectroscopy (XPS). Before performing the XPS measurement, it is preferable to clean the surface of the sanitary ware using a neutral detergent and a sponge, and then thoroughly rinse it with ultrapure water.

[0060] [Obtaining XPS spectrum] As the XPS apparatus, K-ALPHA (manufactured by thermo scientific) is used, and spectra of C1s, F1s, and O1s can be obtained by performing XPS measurement under the following XPS measurement conditions. When measuring a plurality of samples together, in order to avoid decomposition of the C—F bond due to X-ray irradiation, it is preferable to perform XPS measurement with each sample separated by at least 1 cm or more. Note that XPS is a technique for irradiating the sample surface with soft X-rays, capturing the photoelectrons emitted due to ionization of the sample surface, and performing energy analysis. Since the obtained spectrum shows the photoelectron peaks emitted from each electron orbit, the obtained photoelectron peaks are denoted by the element symbol and the electron orbit (for example, the photoelectron peak obtained from the 1s orbit of carbon is denoted as "C1s").

[0061] [XPS measurement conditions] X-ray conditions: Monochromatized AlKα ray, 30 W, 12 kV Analysis area: 200 μmφ Neutralization gun conditions: 0.1 V, 200 μA Photoelectron extraction angle: 90° Time Per Step: 50 ms Sweep: 5 times Pass energy: 55 eV Analysis elements (energy range, step size): C1s (278-308eV, 0.01eV), F1s (679-699eV, 0.03eV), O1s (523-543eV, 0.03eV) Inert gas species: Ar Sputtering voltage: 200V Sputtering area: 2mm x 2mm Sputter cycle: 1 second

[0062] In the spectrum obtained by XPS measurement of the surface of the sanitary ware, the type of bond state of the carbon atom contained in the perfluoropolyether chain 3 (hereinafter sometimes abbreviated as "bond type of carbon atom" or simply "bond type") is identified. The bond types of the carbon atom contained in the perfluoropolyether chain are five types (1) to (5) shown in Table 2 below. Table 2 shows each bond energy of C1s of bond types (1) to (5). However, the bond energy value of C1s of bond type (1) uses the literature value described in NIST Standard Reference Database 20, Version 4.1 (https: / / srdata.nist.gov / xps / ). The bond energy value of C1s described in the above database is shifted and set up with the bond energy value of C1s of CC bond as 284.8 eV. Therefore, in order to match the conditions of this XPS measurement, the bond energy value of C1s of an organic compound containing bond type (1) is corrected using the bond energy value of F1s contained in the organic compound, which is 688.5 eV, which is the same condition as the XPS measurement conditions of this XPS. For example, bond type (1) is a bond included in the reagent FOMBLIN Y in the NIST database, and the bond energy value of C1s is described as 295.2 eV. Here, since the bond energy value of F1s in FONBLIN Y is 689.1 eV, the literature value of the bond energy of this F1s is corrected to 688.5 eV. In other words, the bond energy value of this F1s is shifted by 0.6 eV to the lower energy side for correction. Accordingly, the bond energy value of C1s is also shifted by 0.6 eV to the lower energy side for correction, and the bond energy value of C1s of bond type (1) is obtained as 294.6 eV. This value is used as the bond energy value of C1s of bond type (1).

[0063] [Table 2]

[0064] In XPS, it is known that the binding energy of the photoelectrons obtained from the target atom (also called the "central atom") varies greatly (i.e., undergoes a chemical shift) depending on the bonding state between the target atom (also called the "central atom") and the atoms surrounding it (also called the "adjacent atoms"). Therefore, it is possible to identify which peak corresponds to which bond type in the obtained XPS spectrum from the C1s binding energies of bond types (1) to (5), i.e., to separate the peaks.

[0065] One of the factors of chemical shift is the difference in electronegativity of adjacent atoms. The more adjacent atoms with high electronegativity exist around the central atom, the more biased the charge is between the central atom (carbon atom in the present invention) and the adjacent atoms (fluorine atom, oxygen atom, carbon atom in the present invention). As a result, the binding energy of the photoelectron obtained from the central atom (binding energy of C1s in the present invention) shifts to the higher side. The constituent atoms of the perfluoropolyether chain are fluorine atom, oxygen atom, and carbon atom in order of increasing electronegativity, so the more fluorine atoms exist around the central atom, the carbon atom, the higher the binding energy of the binding type C1s. In addition, the binding energy of C1s decreases in the order of the adjacent atoms being oxygen atoms and carbon atoms. Based on this premise, the binding types (1) to (5) are arranged in order of increasing C1s binding energy, as follows: (1)>(2)>(3)>(4)>(5). The spectra of bond types (1) to (5) appear in the C1s binding energy region (289 eV to 298 eV), which is higher than the band of carbon and other atoms (around 285 eV).

[0066] In the obtained XPS spectrum, first, we confirm the influence of the peak due to potassium on the C1s spectrum. When the base and / or glaze layer for sanitary ware contains potassium, the K2p 1 / 2 However, depending on the height of the perfluoropolyether chains present on the surface of the glaze layer, even if the sanitary ware base and / or glaze layer contain potassium, the K2p peak may be present in the 296.8±1.0 eV region. 1 / 2In this case, the peak due to potassium may not be observed in the C1s spectrum, and the peak separation described below can be performed assuming that there is no influence of the peak due to potassium on the C1s spectrum.

[0067] K2p in the 296.8±1.0 eV region of the C1s spectrum 1 / 2 If the peak is confirmed, the following should be considered as the influence of potassium on the C1s spectrum. The peaks derived from potassium that affect the C1s spectrum are K2p 1 / 2 and K2p 3 / 2 These are derived from two types of electron orbitals. In general, K2p 3 / 2 The peak of K2p 1 / 2 The photoelectron binding energy is 2.8 eV lower than that of K2p 1 / 2 It is twice as large as K2p. 3 / 2 The peak of K2p exists at 294.0±1.0 eV, which overlaps with the peaks derived from the perfluoropolyether chains of bond types (2) and (3) listed in Table 2. 3 / 2 It is difficult to confirm the existence of the peak K2p 1 / 2 The peak of K2p is detected as a single peak in the photoelectron binding energy region away from the peaks derived from the perfluoropolyether chain. 1 / 2 If the presence of the peak is confirmed, 3 / 2 It is determined that there is a peak of K2p 1 / 2 From the binding energy and peak area of ​​K2p 3 / 2 It is possible to calculate the binding energy and the peak area of ​​K2p 3 / 2 It is assumed that the peak of is present in the C1s spectrum, and when performing peak separation of the C1s spectrum, this peak area is taken into consideration, and peak separation is performed excluding the influence of the peak derived from potassium. Therefore, even when the C1s spectrum is influenced by the peak derived from potassium, it is possible to calculate the composition ratio of each bond type contained in the perfluoropolyether chain.

[0068] <Peak separation> The obtained spectrum is subjected to peak separation using data analysis software Avantage (Version 5, Thermo Scientific). Peak separation refers to performing waveform separation by the detected peaks in the entire waveform of the obtained spectrum, and identifying the bond state corresponding to each obtained waveform. This peak separation makes it possible to calculate the ratio of different bond states contained in the perfluoropolyether chain, even though it is the same element (carbon atom in the present invention). The details of the peak separation method are described below. First, in the obtained F1s spectrum, the peak positions in the entire bond energy range of C1s, F1s, and O1s measured are corrected so that the F1s bond energy of the peak derived from the fluorine atom bonded to the carbon atom is 688.5 eV. In this state, peak separation is performed on the photoelectron spectrum of the bond types (1) to (5) present in the C1s spectrum. The specific method of peak separation of C1s is described below. First, in the range of 278 eV (start point) to 300 eV (end point) in the measurement range of C1s, the peak background is removed by the Shirley method. However, for the start and end points, the average value of the intensity in the range of ±0.25 eV with each point as the median is taken as the background intensity at that point. For example, at the start point of C1s at 278 eV, the average value of the intensity in the range of ±0.25 eV of the median value of 278 eV, that is, the range of 277.75 eV to 278.25 eV, is taken as the background intensity at the start point. Thereafter, the peak at 285 eV in the C1s binding energy is taken as the C-C bond or C-H bond, the peak at 286 eV in the C1s binding energy is taken as the C-O bond, the peaks at the C1s binding energy of the bond types (1) to (5) listed in Table 2 are taken as the respective bond types, and the peak at 296.8 ±1.0 eV in the C1s binding energy is taken as the K2p 1 / 2and add peaks. Other peaks suggested by the software are also added as necessary. The peak shape of the added peaks should follow the Gauss-Lorentz distribution. Then, fitting is performed using the peak fitting conditions below to obtain a spectrum for each bond type. If the fitting results do not meet the fitting completion criteria below, a peak is added at the position of the C1s binding energy that is the maximum among the positive maxima in the second derivative spectrum displayed on the screen, and fitting is performed again using the peak fitting conditions below. This operation is repeated until the fitting completion criteria below are met, and fitting is then completed. Next, K2p 1 / 2 If the peak of K is confirmed, the effect of the potassium peak is removed by the following procedure. First, the K2p peak determined by the above fitting is 1 / 2 The binding energy, peak height and full width at half maximum (FWHM) of the peak are specified on the software. 3 / 2 The binding energy of K2p 1 / 2 The binding energy of K2p is set to 2.8 eV smaller than the binding energy of 3 / 2 The half-width of K2p 1 / 2 Specify the value in the software as being equal to K2p 3 / 2 The peak area of ​​K2p 1 / 2 The peak height is adjusted on the software so that it is 1.95 to 2.05 times the peak area of ​​. Then, fitting is performed again using the peak fitting conditions below to obtain a spectrum for each bond type that takes into account the potassium peak. This completes the XPS peak separation. [Peak fitting conditions] Fitting Algorithm:Powell Maximum Iterations: 500 Convergence:1e-05 Gauss-Lorentz Mix:Product [Fitting completion criteria] Normalised Chi Square ≦ 10.0

[0069] <Calculation of the composition ratio of the bonding types of carbon atoms contained in the perfluoropolyether chain> From the spectra of the bonding types (1) to (5) identified by peak separation of XPS, the composition ratios of the bonding types (1) to (5) are calculated using data analysis software Avantage (Version 5, manufactured by Thermo Scientific). The ratio of the peak area intensity of each bonding type (1) to (5) to the total peak area intensity (Area Intensity) of the spectra of each bonding type (1) to (5) obtained by peak separation is defined as the composition ratio in the perfluoropolyether chain of each bonding type (1) to (5) and calculated in at% units.

[0070] <Calculation of the O / C ratio> From the composition ratios of the bonding types (1) to (5) obtained by peak separation, the O / C ratio contained in the perfluoropolyether chain is obtained. Since the number of carbon atoms and oxygen atoms contained in the perfluoropolyether chain cannot be directly obtained from the calculated composition ratios of the bonding types (1) to (5), the O / C ratio is calculated by the following method. Assume that the number of carbon atoms contained in the perfluoropolyether chain is 100, and the composition ratios of the carbon atoms of each of the bonding types (1) to (5) are also regarded as the number of carbon atoms as they are. Since the types of atoms bonded to each of the bonding types (1) to (5) are fixed, the number of oxygen atoms when the number of carbon atoms in the perfluoropolyether chain is 100 can be obtained. Thereby, the O / C ratio can be obtained.

[0071] For example, as the bonding types contained in the perfluoropolyether chain in the compound represented by the above formula (a), (2), (4), and (5) are detected, and the respective composition ratios are 34.0 at%, 56.0 at%, and 10.0 at%, the following conditions: · When C is bonded to the central carbon atom, this C is not counted in the number of carbon atoms · When O is bonded to the central carbon atom, this O is counted as 1 / 2 According to this, the number of carbon atoms is the sum of 34.0 for bond type (2), 56.0 for bond type (4), and 10.0 for bond type (5), which is a total of 100. Also, the number of oxygen atoms is the sum of 34.0×2×1 / 2 for bond type (2), 56.0×1×1 / 2 for bond type (4), and 10.0×0×1 / 2, which is a total of 62.0. Therefore, the O / C ratio is calculated to be 0.62. By rounding the second decimal place of this calculated O / C ratio, the O / C ratio of the present invention is obtained.

[0072] <Calculation of F / (C + O) ratio> From the composition ratios of bond types (1) to (5) obtained by peak separation, the F / (C + O) ratio contained in the perfluoropolyether chain is obtained. Since the number of carbon atoms, oxygen atoms, and fluorine atoms contained in the perfluoropolyether chain cannot be directly obtained from the calculated composition ratios of bond types (1) to (5), the F / (C + O) ratio is calculated by the following method. Assume that the number of carbon atoms contained in the perfluoropolyether chain is 100, and the composition ratios of the carbon atoms of each of bond types (1) to (5) are also regarded as the number of carbon atoms as they are. Since the types of atoms bonded to each of bond types (1) to (5) are fixed, the number of oxygen atoms and fluorine atoms when the number of carbon atoms in the perfluoropolyether chain is 100 can be obtained. Thereby, the F / (C + O) ratio can be obtained.

[0073] For example, as the bond types contained in the perfluoropolyether chain in the compound represented by the above formula (a), (2), (4), and (5) are detected, and when the respective composition ratios are 34.0 at%, 56.0 at%, and 10.0 at%, the following conditions: · When C is bonded to the central carbon atom, this C is not counted in the number of carbon atoms · When O is bonded to the central carbon atom, this O is counted as 1 / 2 · When F is bonded to the central carbon atom, this F is counted as one Accordingly, the number of carbon atoms is a total of 100, which is the sum of 34.0 for bond type (2), 56.0 for bond type (4), and 10.0 for bond type (5). Also, the number of oxygen atoms is a total of 62.0, which is the sum of 34.0×2×1 / 2 for bond type (2), 56.0×1×1 / 2 for bond type (4), and 10.0×0×1 / 2 for bond type (5). Further, the number of fluorine atoms is a total of 200.0, which is the sum of 34.0×2×1 for bond type (2), 56.0×2×1 for bond type (4), and 10.0×2×1 for bond type (5). Therefore, the F / (C + O) ratio is calculated to be 1.23. By rounding the second decimal place of this calculated F / (C + O) ratio, the F / (C + O) ratio of the present invention is obtained.

[0074] <Ratio calculation of the number of carbon atoms having a <C-F bond to the number of carbon atoms having a CF 3 bond> In the present invention, when the composition ratio of bond type (3) obtained by peak separation is high, that is, exceeds 20 at%, it means that the perfluoropolyether chain has bond type (3). This means that the perfluoropolyether main chain is likely to have a side chain (-CF 3 )

[0075] Sputtering time by XPS depth profiling of sanitary ware surfaces In the present invention, in the profile obtained by the depth direction analysis of XPS described later, starting from the XPS measurement point on the surface of the sanitary ware, the peak area of fluorine atoms (A s ) at a certain measurement point with respect to the peak area of fluorine atoms (A a ) at this starting point, and the peak area of fluorine atoms (A b%) is 1.0 at % or less. In the present invention, the height of the perfluoropolyether chains 3 contained in the surface of the glaze layer can be specified using the sputtering time as an index, which is determined by XPS depth direction analysis of the surface of the sanitary ware.

[0076] The sputtering time of the sanitary ware surface by XPS depth direction analysis can be confirmed by a depth direction analysis by combining XPS measurement and sputtering using Ar ions. This depth direction analysis by combining XPS measurement and sputtering using Ar ions is referred to as "XPS depth direction analysis". In XPS depth direction analysis, first, the sanitary ware surface is cleaned with a neutral detergent, rinsed with ultrapure water, and the moisture is blown off with an air blower. When measuring multiple samples at once, it is preferable to perform XPS measurement with each sample at least 1 cm apart to avoid decomposition of C-F bonds due to X-ray irradiation. Then, XPS measurement of the sanitary ware surface is performed, and sputtering using Ar ions and XPS measurement are alternately repeated. The above-mentioned "XPS measurement conditions" can be used as the conditions for XPS measurement. The following conditions can be used as the conditions during sputtering (hereinafter also referred to as "sputtering conditions"). XPS measurement is performed for each "sputtering cycle" of the sputtering conditions. Spectral information is obtained by XPS depth direction analysis.

[0077] [Sputtering conditions] Inert gas species: Ar Sputtering voltage: 200V Sputtering area: 2mm x 2mm Sputter cycle: 1 second The sputtering voltage is the voltage applied to the Ar ion gun, the sputtering range is the range of the surface that is removed by sputtering, and the sputtering cycle is the time that Ar gas is continuously irradiated for each measurement in the depth direction, and the total sputtering cycle is the sputtering time.

[0078] In the profile obtained by the XPS depth direction analysis, the XPS measurement point on the sanitary ware surface (i.e., the perfluoropolyether chain) is taken as the starting point, and the peak area (A s ) versus the peak area of ​​fluorine atoms at a certain measurement point (A a ) and the peak area of ​​fluorine atoms at the measurement point one point before (A b The end point is the point where the absolute value of the difference from the measured value becomes 1.0 at% or less. End point: |A b -A a | / A s <=0.01

[0079] The sputtering time from the above-mentioned start point to the end point can be used as an index of the height of the perfluoropolyether chain.

[0080] In the present invention, the sputtering time from the start point to the end point is preferably within 60 seconds, more preferably within 30 seconds, and even more preferably within 20 seconds. The lower limit of the sputtering time is preferably 5 seconds or more. The preferred range of the sputtering time may be an appropriate combination of the above upper and lower limits.

[0081] The sanitary ware according to the present invention is preferably one in which a large number of perfluoropolyether chains 3 are formed in a film or layer on the surface of the glaze layer 2. The film containing the perfluoropolyether chains 3 is preferably a thin film. When the perfluoropolyether chains 3 are formed in a film or layer, the peak area (A s ) versus the peak area of ​​fluorine atoms at a certain measurement point (A a ) and the peak area of ​​fluorine atoms at the measurement point one point before (A b %) is 1.0 at % or less, can be used as an index of the thickness of the film or layer.

[0082] When the perfluoropolyether chain 3 is in the form of a film or layer, its height is preferably from 1 nm to 10 nm, and more preferably from 1 nm to 5 nm.

[0083] The perfluoropolyether chains contained in the surface of the sanitary ware of the present invention may contain two or more types of perfluoropolyether chains, or may contain a single type of perfluoropolyether chain.

[0084] The surface of the sanitary ware of the present invention may contain not only perfluoropolyether chains but also fluoroalkyl chains, but in order to obtain sufficient durability, the content is preferably low. Specifically, the content of fluoroalkyl chains relative to the total fluorine-based organic chains, such as perfluoropolyether chains and fluoroalkyl chains, contained in the surface of the sanitary ware is preferably less than 50 at%, more preferably 30 at% or less, and even more preferably 10 at% or less. EXAMPLES

[0085] The present invention will be described in more detail with reference to the following examples, although the present invention is not limited to these examples.

[0086] 1. Preparation of sanitary ware 1-1. Preparation of the base and glaze layer for sanitary ware <Preparation of base material for sanitary ware> A sanitary ware slip prepared from raw materials such as silica sand, feldspar, limestone, and clay was cast into a plaster mold to obtain a molded body. This molded body was then dried. The dried molded body was then fired in the firing process described below to produce the "sanitary ware base material."

[0087] <Preparation of glaze> A number of glaze raw materials having the compositions calculated as oxides and shown in Table 3 below were prepared. 600 g of each glaze raw material, 400 g of water, and 1 kg of alumina balls were placed in a 2-liter earthenware pot and ground in a ball mill for about 65 hours to obtain glazes.

[0088] [Table 3]

[0089] Glaze was applied to the dried molded body by spray coating, and the resulting product was fired at 1100 to 1200°C to produce a sanitary ware base material with a glaze layer. The surface of the resulting glaze layer was processed as necessary to produce substrates A to F with the arithmetic mean linear roughness Ra shown in Table 4 below. The arithmetic mean linear roughness Ra was measured using a stylus surface roughness measuring device conforming to JIS-B0651 (2001) in accordance with "7. Method and procedure of evaluation using a stylus surface roughness measuring device" of JIS-B0633 (2001). The color of each glaze layer is mainly due to the pigment. Substrate A was formed by applying a glaze having the composition shown in Table 3 to a sanitary ware base material, and then applying a glaze having the composition shown in Table 3 except for ZrO2 and pigment, and firing the substrate. Substrate B was obtained by applying a glaze having the composition shown in Table 3 to a base material for sanitary ware and firing it to form a glaze layer. Substrate C was obtained by wet blasting Substrate A using non-spherical alumina particles as an abrasive, selecting the particle size range of the abrasive from 1 μm to 100 μm, and appropriately selecting the compressed air supply pressure, projection distance, projection angle, and projection time. Substrate D was obtained by applying a glaze having an excess of 1 to 10 wt% of alkaline earth metal oxide from the composition shown in Table 3 to a base material for sanitary ware and firing it to form a glaze layer. Substrate E was obtained by dry blasting Substrate A using an abrasive with a particle size of #150 (median particle size 63 to 106 μm): Fuji Random A (manufactured by Fuji Manufacturing Co., Ltd.) under conditions of a compressor pressure of 0.6 MPa and a nozzle diameter of 5 mm. Substrate F was obtained by dry blasting substrate A using Fuji Random A (manufactured by Fuji Manufacturing Co., Ltd.) abrasive with grain size #150 (median grain size 63 to 106 μm) under conditions of a compressor pressure of 0.3 MPa and a nozzle diameter of 5 mm.

[0090] [Table 4]

[0091] 1-2.Pretreatment In order to remove dirt present on the surface of the glaze layer and to activate the hydroxyl groups present on the surface, pretreatment 1 or 2 described below was carried out.

[0092] <Pretreatment 1> First, the surface of the glaze layer was washed with a commercially available sponge I soaked in a neutral detergent (product name: Clean Ace, manufactured by AS ONE). Next, a small amount of ceria powder (manufactured by Treibacher Industrie AG) was sprinkled on the surface of the glaze layer, and the surface was washed with a commercially available sponge II. Next, the surface of the glaze layer was washed with ultrapure water while spraying it with running water, and the remaining ceria powder was removed with a commercially available sponge III (sponges I, II, and III were different, and each was used separately). The glaze layer was then immersed in an aqueous solution of alkaline detergent (product name: Semiclean, manufactured by Yokohama Yushi Kogyo Co., Ltd.) whose concentration was adjusted to 5 wt% with ion-exchanged water, and ultrasonically cleaned for 5 minutes. Next, ultrapure water was applied to the surface of the glaze layer to remove the alkaline detergent. The glaze layer was further immersed in ultrapure water and ultrasonically cleaned for 5 minutes. Next, ultrapure water was applied to the surface of the glaze layer again, and moisture was removed with an air duster.

[0093] <Pretreatment 2> First, the surface of the glaze layer was washed with a commercially available sponge i soaked in a neutral detergent (product name: Clean Ace, manufactured by AS ONE Co., Ltd.). Next, the surface of the glaze layer was washed with running water to remove the neutral detergent. The glaze layer was then immersed in an aqueous solution of alkaline detergent (product name: Semiclean, manufactured by Yokohama Yushi Kogyo Co., Ltd.) whose concentration was adjusted to 5 wt% with ion-exchanged water, and ultrasonically cleaned for 5 minutes. Next, ultrapure water was applied to the surface of the glaze layer to remove the alkaline detergent. The glaze layer was further immersed in ultrapure water and ultrasonically cleaned for 5 minutes. Next, ultrapure water was applied to the surface of the glaze layer again, and moisture was removed with an air duster.

[0094] 1-3. Formation of perfluoropolyether chain <Preparation of Reagents> The following reagents a to g were prepared, each of which contains a compound containing a perfluoropolyether chain or a compound containing a fluoroalkyl chain. In each of the reagents a to g, the partial structure containing a carbon atom to which fluorine is bonded is clearly indicated. In the structural formula of the active ingredient contained in each reagent, X Si means an organic group containing at least one Si atom and not containing a fluorine atom on the Si atom, and a hydroxyl group or a hydrolyzable group bonded to the organic group. The hydrolyzable group means an alkoxy group or a halogeno group. Specifically, -OCH 3 , -OCH 2 CH 3 , -Cl.

[0095] Reagent a A reagent comprising the following components and containing a compound containing a perfluoropolyether chain represented by formula (a) as an active ingredient: [ka] (wherein l:m:n=23.2:22.3:0.4 (average value), and X Si means an organic group containing an average of 3.0 silicon atoms, the silicon atoms not containing fluorine atoms, and a hydroxyl group or a hydrolyzable group bonded to the organic group. The hydrolyzable group means an alkoxy group or a halogeno group. Specifically, -OCH 3 , -OCH 2 CH 3 , -Cl. The repeating units in the formula are arranged randomly. These values ​​were determined by liquid analysis of the reagent a using NMR. The number average molecular weight of the perfluoropolyether chain is 19 From the F-NMR results, Si The existence of 1 H-NMR and 29 This was confirmed by the Si-NMR detection spectrum.)

[0096] (component) Fluoroalkyl ether (CAS No. 163702-06-4) 30-40% Fluoroalkyl ether (CAS No. 163702-06-5) 40-50% 10-20% of a compound containing a perfluoropolyether chain of formula (a) (active ingredient)

[0097] Reagent B A reagent comprising the following components and containing a compound containing a perfluoropolyether chain represented by formula (b) as an active ingredient: [ka] (wherein the average value of l is 22.9. X Si X in formula (a) contains an average of 2.0 Si atoms. Si These values ​​were obtained by liquid analysis of the reagent b using NMR. The number average molecular weight of the perfluoropolyether chain is 19 From the F-NMR results, Si The existence of 1 H-NMR and 29 This was confirmed by the Si-NMR detection spectrum.)

[0098] (component) Ethyl nonafluorobutyl ether (CAS No. 163702-05-4) 25-35% Ethyl nonafluoroisobutyl ether (CAS No. 163702-06-5) 45-55% 15-25% of a compound containing a perfluoropolyether chain of formula (b) (active ingredient)

[0099] Reagent C A reagent comprising the following components and containing as an active ingredient a compound containing a perfluoropolyether chain represented by formula (c): [ka] (wherein the average value of l is 23.2. X Si X in formula (a) contains an average of 3.7 Si atoms. Si These values ​​were obtained by liquid analysis of reagent c using NMR. The number average molecular weight of the perfluoropolyether chain is 19 From the F-NMR results, Si The existence of 1 H-NMR and29 This was confirmed by the Si-NMR detection spectrum.)

[0100] (component) Ethyl nonafluorobutyl ether (CAS No. 163702-05-4) 25-35% Ethyl nonafluoroisobutyl ether (CAS No. 163702-06-5) 45-55% 15-25% of a compound containing a perfluoropolyether chain of formula (c) (active ingredient)

[0101] Reagent d A reagent comprising the following components and containing as an active ingredient a compound containing a perfluoropolyether chain represented by formula (d): [ka] (In the formula, the average value of l is 18, and this value was determined by liquid analysis of the reagent d by NMR. The number average molecular weight of the perfluoropolyether chain is 19 This was confirmed by the results of F-NMR. Si X in formula (a) contains an average of 5.0 Si atoms. Si is equivalent to

[0102] (component) 1,1,1,2,2,3,3,4,4,5,5,6,6-Tridecafluorooctane (CAS No. 80793-17-5) Over 99.5% Less than 0.5% of perfluoropolyether chain-containing silane compound (active ingredient) of formula (d)

[0103] Reagent e A reagent comprising the following components and containing as an active ingredient a compound containing a perfluoropolyether chain represented by formula (e): [ka] (In the formula, the average value of l is 23.4, and this value was obtained by liquid analysis of the reagent e by NMR. The number average molecular weight of the perfluoropolyether chain is 19This was confirmed by the results of F-NMR. Si X in formula (a) contains an average of 3.0 Si atoms. Si is equivalent to

[0104] (component) Ethyl nonafluorobutyl ether (CAS No. 163702-05-4) 25-35% Ethyl nonafluoroisobutyl ether (CAS No. 163702-06-5) 45-55% 15-25% of a compound containing a perfluoropolyether chain of formula (e) (active ingredient)

[0105] Reagent F : A perfluoropolyether chain (CF) represented by the formula (f) 3 A reagent containing a compound containing a side chain as an active ingredient. [ka] (In the formula, X Si X in formula (a) contains an average of 1.0 Si atom. Si is equivalent to

[0106] (component) Fluoroalkyl ether 80-85% The perfluoropolyether chain of formula (f) (CF 3 Compounds (active ingredients) containing side chains 15-20%

[0107] Reagent g A reagent containing a compound having a fluoroalkyl chain represented by formula (g) as an active ingredient. [ka] (In the formula, X Si X in formula (a) contains an average of 1.0 Si atom. Si is equivalent to

[0108] (component) Compounds containing a fluoroalkyl chain of formula (g) (active ingredient, CAS No. 83048-65-1) > 98.0%

[0109] <Preparation of processing solution> 206 μL of reagent a was dropped into 30 g of fluorine solvent (product name: NOVEC7200, 3M) and stirred gently to obtain treatment solution a, in which the concentration of the active ingredient of reagent a was approximately 0.1 wt%. Using a similar method, treatment solutions b, c, e, f, and g, each containing reagents b, c, e, f, and g, were obtained. Because reagent d had an active ingredient concentration of 0.1 wt%, it was used as is as treatment solution d without diluting it with a fluorine solvent.

[0110] <Application of processing liquid> Treatment liquid a was applied to the surface of base material A that had been subjected to pretreatment 1 using a spray gun at a pressure of 0.04 MPa, the surface was left to stand for 30 seconds, and then thermally dried for 30 minutes in a drying oven at 120° C. Thereafter, the surface was cured for 3 hours in a thermo-hygrostat set at a temperature of 80° C. and a humidity of 80%, and then for 17 hours at room temperature and atmospheric pressure, to obtain the sanitary ware of Example 1. In a similar manner, the sanitary ware of Examples 2 to 15 and Comparative Examples 1 to 10 were obtained using substrates A to F that had been pretreated as shown in Table 7 below and each of the treatment solutions.

[0111] 2.Analysis and Evaluation The sanitary wares produced as described above (Examples 1 to 15 and Comparative Examples 1 to 10) were subjected to the following analysis and evaluation.

[0112] 2-1.XPS analysis The surfaces of the sanitary ware of Examples 1 to 5 and Comparative Examples 1 and 2 were measured by X-ray photoelectron spectroscopy (XPS). Prior to the measurements, the surfaces of the sanitary ware were cleaned with a neutral detergent and a sponge, and then thoroughly rinsed with ultrapure water.

[0113] Using a K-ALPHA (made by Thermo Scientific) as the XPS device, measurements were taken on the surface of each sanitary ware under the following "XPS measurement conditions", and C1s, F1s, and O1s spectra were obtained. Note that if the treatment method using the treatment liquid is the same, it is self-evident that the structure of the compound formed will also be the same, and the results of this analysis can be interpreted as an analysis result that shows the structure of the compound itself, regardless of the pretreatment method.

[0114] [XPS measurement conditions] X-ray conditions: Monochromatic AlKα radiation, 30W, 12kV Analysis area: 200μmφ Neutralization gun conditions: 0.1V, 200μA Photoelectron take-off angle: 90° Time Per Step: 50 ms Sweep: 5 times Pass energy: 55 eV Analysis elements (energy range, step size): C1s (278-308eV, 0.01eV), F1s (679-699eV, 0.03eV), O1s (523-543eV, 0.03eV) Inert gas species: Ar Sputtering voltage: 200V Sputtering area: 2mm x 2mm Sputter cycle: 1 second

[0115] The types of bond states of carbon atoms contained in perfluoropolyether chains or fluoroalkyl chains contained in the surface of each sanitary ware (hereinafter simply referred to as "bond types") are seven types (1) to (7) shown in Table 5 below. The bond energies of C1s for each of bond types (1) to (7) are shown in Table 5 below. However, the bond energy values ​​of C1s for bond types marked with * (hereinafter referred to as "bond type *") were corrected as follows to the literature values ​​listed in NIST Standard Reference Database 20, Version 4.1. The bond energy values ​​of C1s listed in the above database were shifted and set up with the bond energy value of C1s of CC bonds as 284.8 eV. Therefore, in order to match the conditions of this XPS measurement, the bond energy values ​​of C1s of organic compounds containing bond type * were corrected using the bond energy value of F1s contained in the organic compounds, which is 688.5 eV, which is the same as the conditions of this XPS measurement.

[0116] [Table 5]

[0117] <Peak separation> For the obtained spectrum, peaks were separated using data analysis software Avantage (Version 5, Thermo Scientific). First, the peak positions in the entire binding energy range of C1s, F1s, and O1s measured were corrected so that the binding energy of the F1s peak derived from the fluorine atom bonded to the carbon atom in the obtained F1s spectrum was 688.5 eV. In this state, peak separation was performed on the photoelectron spectra of the bond types (1) to (7) present in the C1s spectrum. The specific method of peak separation for C1s is described below. First, the background of the peak was removed by the Shirley method in the range of 278 eV (start point) to 300 eV (end point) in the C1s measurement range. However, for the start point and end point, the average value of the intensity in the range of ±0.25 eV with each point as the median was used as the background intensity at that point. For example, at the start point of C1s at 278 eV, the average value of the intensity in the range of ±0.25 eV of the median value of 278 eV, that is, the range of 277.75 eV to 278.25 eV, was used as the background intensity at the start point. Then, the peak at 285 eV in the C1s binding energy was determined as a C-C bond or a C-H bond, the peak at 286 eV in the C1s binding energy was determined as a C-O bond, the peaks at the C1s binding energy of the bond types (1) to (7) listed in Table 5 were determined as each bond type, and the peak at 296.8 ± 1.0 eV in the C1s binding energy was determined as a K2p 1 / 2 and added peaks. Other peaks proposed by the software were also added as necessary. The added peaks were assumed to have a Gauss-Lorentz distribution in peak shape. Then, fitting was performed using the peak fitting conditions below to obtain spectra for each bond type. If the fitting results did not meet the fitting completion criteria below, a peak was added at the position of the C1s binding energy that was the maximum among the positive maxima in the second derivative spectrum displayed on the screen, and fitting was performed again using the peak fitting conditions below. This operation was performed until the fitting completion criteria below was met, and fitting was completed once. Next, K2p 1 / 2For the treated solutions a, b, d, e, f, and g in which the peaks of K were confirmed, the effects of the potassium peaks were removed by the following procedure. First, the K2p 1 / 2 The binding energy, peak height and full width at half maximum (FWHM) of K2p were specified on the software. 3 / 2 The binding energy of K2p 1 / 2 The binding energy of K2p is set to 2.8 eV smaller than the binding energy of 3 / 2 The half-width of K2p 1 / 2 The software specified the value as being equal to K2p 3 / 2 The peak area of ​​K2p 1 / 2 The peak height was adjusted on the software so that it was 1.95 to 2.05 times the peak area of ​​the above. Then, fitting was performed again using the following peak fitting conditions to obtain spectra for each bond type taking into account the potassium peak. This completes the XPS peak separation. [Peak fitting conditions] Fitting Algorithm:Powell Maximum Iterations: 500 Convergence:1e-05 Gauss-Lorentz Mix:Product [Fitting completion criteria] Normalised Chi Square≦10.0

[0118] The XPS spectra and peak separation results for the surfaces of each sanitary ware are shown in Figures 3 to 9.

[0119] <Calculation of the composition ratio of bond types of carbon atoms contained in perfluoropolyether chains or fluoroalkyl chains> From the spectra of the bond types (1) to (7) identified by peak separation, the composition ratios of the bond types (1) to (7) were calculated using the data analysis software Avantage (Version 5, manufactured by Thermo Scientific). Specifically, the ratio of the peak area intensity of the spectra of each bond type (1) to (7) to the total peak area intensity of all the spectra of the bond types (1) to (7) obtained by XPS measurement and peak separation was defined as the composition ratio in the perfluoropolyether chain or fluoroalkyl chain of each bond type (1) to (7), and was calculated in units of at%. The results are shown in Table 6.

[0120]

Table 6

[0121] < CF to the number of carbon atoms with CF bonds 3 Calculating the percentage of carbon atoms with bonds > The composition ratio of the bond type (3) in the perfluoropolyether chain was calculated. The obtained results are shown in Table 7 below.

[0122] <Calculation of O / C ratio> From the composition ratios of the bond types (1) to (7) obtained by peak separation, the O / C ratio of the perfluoropolyether chain or fluoroalkyl chain was calculated using the method already described. The results are shown in Table 7 below.

[0123] <Calculation of F / (C + O) ratio> From the composition ratios of the bond types (1) to (7) obtained by peak separation, the F / (C + O) ratio of the perfluoropolyether chain or fluoroalkyl chain was calculated using the method already described. The results are shown in Table 7 below.

[0124] 2-2. Confirmation of sputtering time by XPS depth profile analysis of sanitary ware surface An XPS depth profile analysis was carried out on the surface of the sanitary ware. After XPS measurement of the sanitary ware surface, sputtering using Ar ions and XPS measurement were alternately repeated using the aforementioned "XPS measurement conditions" and "sputtering conditions." XPS measurement was carried out for each "sputtering cycle" of the sputtering conditions. Spectral information was obtained by XPS depth profile analysis. The XPS measurement point on the surface of each sanitary ware was set as the starting point, and the peak area (A s ) versus the peak area of ​​fluorine atoms at a certain measurement point (A a ) and the peak area of ​​fluorine atoms at the measurement point one point before (A b The point where the absolute value of the difference between the sputtering start point and the end point became 1.0 at % or less was taken as the end point, and the sputtering time from the start point to the end point was calculated. The results are shown in Table 7.

[0125] 2-3. Evaluation of water stain removal performance For each piece of sanitary ware, an evaluation of limescale removability was carried out after the following durability test 1 or durability test 2.

[0126] Durability test 1: Sliding test 1 to 2 mL of ion-exchanged water was dropped onto the surface of the sanitary ware, and the nonwoven fabric part of the sponge (Scotch-Brite (registered trademark) hybrid laminated sponge, manufactured by 3M Japan) was subjected to a load of 50 g / cm. 2 The sponge was then pressed against the surface and then moved back and forth 20,000 times.

[0127] Durability test 2: Sliding test after alkali immersion Each sanitary ware was immersed in an alkaline cleaning agent (Kabikira, Johnson & Johnson) maintained at 40°C for 16 hours. After that, the sanitary ware was taken out and exposed to running water, then to ultrapure water, and the moisture was removed with an air duster. Then, the above-mentioned durability test 1 (sliding test) was conducted.

[0128] Durability test 3: Sliding test after alkali immersion Each piece of sanitary ware was immersed in an alkaline cleaning agent (Kabikira, Johnson & Johnson Co., Ltd.) maintained at 25°C for 1.6 hours. After that, each piece of sanitary ware was taken out and rinsed with running water, then with ultrapure water, and the moisture was removed with an air duster. Next, 1 to 2 mL of ion-exchanged water was dropped onto the surface of each piece of sanitary ware, and the nonwoven fabric part of a sponge (Scotch-Brite (registered trademark) hybrid laminated sponge, 3M Japan) was applied with a load of 50 g / cm. 2 The sponge was then pressed against the surface and then moved back and forth 6,000 times.

[0129] Limescale cleaning performance evaluation Commercially available water containing 9.0-10.0 mg of silica (Si), 1.0-2.0 mg each of sodium (Na), calcium (Ca), and magnesium (Mg), and 0-1.0 mg of potassium per 100 mL of water was diluted 5.5 times with ion-exchanged water to prepare test water. 200 μL of this test water was dropped onto the sanitary ware surface after durability test 1, the sanitary ware surface after durability test 2, or the sanitary ware surface after durability test 3, and dried for 16 hours in a constant temperature and humidity chamber set at a temperature of 25°C and a humidity of 70% under atmospheric pressure to form limescale on the surface.

[0130] A bathroom sponge (Scotch-Brite (registered trademark) Bath Shine antibacterial sponge (with special abrasive particles), manufactured by 3M Japan) was soaked in ion-exchanged water, and then a single push (approximately 1 mL) of bathroom detergent (Magiclean Bath Foaming Spray, manufactured by Kao) was sprayed onto the sponge surface to create a foam of the detergent. The sponge surface was then placed under a load of 200 g / cm on the surface of a sanitary ware surface on which limescale had formed. 2 The sample was pressed against the plate and slid back and forth five times.

[0131] After the sliding, the surface of the sanitary ware was visually inspected to see if the limescale had been completely removed. If it had been completely removed, it was judged as ○, and if even a small amount of limescale remained, it was judged as ×. The results are shown in Table 7 below.

[0132] [Table 7] [Explanation of symbols]

[0133] 1. Base for sanitary ware 2 Glaze layer 3 Perfluoropolyether chain 10 Sanitary ware

Claims

1. A sanitary ware comprising a base for sanitary ware and a glaze layer provided on a surface of the base, The glaze layer has an arithmetic mean linear roughness Ra of its surface of 0.03 μm or more and 2.5 μm or less, the surface of the sanitary ware contains perfluoropolyether chains, the ratio of the number of oxygen atoms in the perfluoropolyether chain to the number of all carbon atoms having C—F bonds in the perfluoropolyether chain, which is obtained by peak separation of a spectrum obtained by measuring a surface of the sanitary ware by X-ray photoelectron spectroscopy (XPS), is 0.1 or more and 1.0 or less; The number of C—F bonds in the perfluoropolyether chain relative to the number of all carbon atoms having C—F bonds in the perfluoropolyether chain obtained by the peak separation 3 1. A sanitary ware comprising: a sanitary ware body having a ratio of the number of carbon atoms having bonds to 20 at % or less.

2. 2. The sanitary ware according to claim 1, wherein the glaze layer has a surface having an arithmetic mean linear roughness Ra of 0.03 μm or more and 1.5 μm or less.

3. 3. The sanitary ware according to claim 2, wherein the glaze layer has a surface having an arithmetic mean linear roughness Ra of 0.03 μm or more and 1.0 μm or less.

4. The sanitary ware according to any one of claims 1 to 3, wherein a ratio of the number of oxygen atoms in the perfluoropolyether chain to the number of all carbon atoms having C-F bonds in the perfluoropolyether chain, obtained by the peak separation, is 0.2 or more and 1.0 or less.

5. The sanitary ware according to claim 4, wherein the ratio of the number of oxygen atoms in the perfluoropolyether chain to the number of all carbon atoms having C—F bonds in the perfluoropolyether chain, obtained by the peak separation, is 0.4 or more and 1.0 or less.

6. In the profile obtained by the XPS depth direction analysis, the XPS measurement point on the surface of the sanitary ware is set as the starting point, and the peak area (A s ) to the peak area (A a ) and the peak area of ​​fluorine atoms at the measurement point one point before that (A b 4. The sanitary ware according to claim 1, wherein the sputtering time until the end point at which the ratio of the absolute value of the difference between the average sputtering temperature and the average sputtering temperature is 1.0 at % or less is 60 seconds or less.

7. In the profile obtained by the XPS depth direction analysis, the XPS measurement point on the surface of the sanitary ware is set as the starting point, and the peak area (A s ) to the peak area (A a ) and the peak area of ​​fluorine atoms at the measurement point one point before that (A b 5. The sanitary ware according to claim 4, wherein the sputtering time until the end point at which the percentage of the absolute value of the difference between the average sputtering temperature and the average sputtering temperature is 1.0 at % or less is 60 seconds or less.

8. In the profile obtained by the XPS depth direction analysis, the XPS measurement point on the surface of the sanitary ware is set as the starting point, and the peak area (A s ) to the peak area (A a ) and the peak area of ​​fluorine atoms at the measurement point one point before that (A b 6. The sanitary ware according to claim 5, wherein the sputtering time until the end point at which the percentage of the absolute value of the difference between the average sputtering temperature and the average sputtering temperature is 1.0 at % or less is 60 seconds or less.

Citation Information

Patent Citations

  • Stainproof ceramic product and production thereof

    JP1992240171A

  • Water-repellent glass article and its production

    JP1996319137A

  • Sanitary ware

    JP2000272988A

  • Ceramic formed body

    JP2002211989A

  • Thin film manufacturing method, optical component manufacturing method, and film deposition apparatus

    JP2005187936A