Curable resin composition
The inclusion of curable polyisobutylene resin and antifoaming agents in the resin composition addresses microbubble formation issues, ensuring effective sealing and durability in fuel cells.
Patent Information
- Application Number
- JP2023084392
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-12-05
AI Technical Summary
Curable resin compositions used in fuel cells generate microbubbles due to a dehydrogenation reaction between residual silanol groups and hydrosilyl groups, leading to reduced sealing performance and damage to the sealant.
Incorporation of specific components such as curable polyisobutylene resin, antifoaming agents, and hydrosilylation catalysts in the resin composition to prevent microbubble formation and enhance sealing performance.
The composition maintains sealing integrity by preventing microbubble generation, ensuring low viscosity, low compression set, and high durability of the cured product.
Smart Images

Figure 2024168015000001 
Figure 2024168015000002 
Figure 2024168015000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a curable resin composition containing a component having a polyisobutylene skeleton. [Background technology]
[0002] In recent years, fuel cells have been attracting attention as a new energy system for automobiles and homes. A fuel cell is a power generation device that produces electricity by chemically reacting hydrogen and oxygen. In addition, fuel cells are clean, next-generation power generation devices because they have high energy efficiency when generating electricity and produce water by the reaction of hydrogen and oxygen. There are four types of fuel cells: polymer electrolyte fuel cells, phosphoric acid fuel cells, molten carbonate fuel cells, and solid oxide fuel cells. Among them, polymer electrolyte fuel cells have high power generation efficiency despite their relatively low operating temperature (around 80°C), and are therefore expected to be used as a power source for automobiles, home power generation devices, small power sources for electronic devices such as mobile phones, and emergency power sources.
[0003] Conventionally, solid packing such as rubber sealants for fuel cells has been used, but from the viewpoint of improving productivity, a sealant that is liquid under an atmosphere of 25°C and hardens after application is required. Since the hardened product has excellent hydrogen gas barrier properties, low moisture permeability, heat resistance, acid resistance, and flexibility, a thermosetting resin composition that contains a polyisobutylene skeleton and undergoes an addition reaction as described in Patent Document 1 is used, but it is required that the applied shape is accurately maintained and that there is no defect in the bead. However, when the hardening resin composition is stored at a constant temperature, although the exact cause is unknown, minute bubbles are generated, which are thought to be hydrogen generated by a dehydrogenation reaction between a silanol group and a hydrosilyl group, and the sealant after hardening shows a decrease in sealing property due to defects caused by the bubbles. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2005 / 095520 Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention has been made in consideration of the above-mentioned circumstances, and an invention has been found that overcomes the problem that when a curable resin composition is stored at a constant temperature, minute bubbles are generated, which are thought to be due to hydrogen being generated by a dehydrogenation reaction between residual silanol groups and hydrosilyl groups, although the exact cause is unknown. The bubbles cause defects in the sealant after curing, resulting in a decrease in sealing properties. [Means for solving the problem]
[0006] The gist of the present invention will now be described. A first embodiment of the present invention is a curable resin composition comprising the following components (A) and (B): (A) Component: Curable polyisobutylene resin Component (B): A defoaming agent containing the following components (B-1) and (B-2) Component (B-1): Defoamer consisting of a silicone-based polymer Component (B-2): Defoamer consisting of a vinyl polymer
[0007] A second embodiment of the present invention is the curable resin composition according to the first embodiment, which contains only the components (B-1) and (B-2) as the defoaming agent.
[0008] A third embodiment of the present invention is the curable resin composition according to the first embodiment, wherein the component (A) contains the following components (A-1) to (A-4): Component (A-1): Polyisobutylene having two or more allyl groups in one molecule Component (A-2): A compound having two or more hydrosilyl groups in one molecule Component (A-3): hydrosilylation catalyst (A-4) Component: Reaction inhibitor
[0009] A fourth embodiment of the present invention is the curable resin composition according to the second embodiment, wherein the component (A) further contains a vinyl ether compound and / or a polyalkylsiloxane having a vinyl group as a component (A-5).
[0010] A fifth embodiment of the present invention is the curable resin composition according to the first embodiment, further comprising a plasticizer as component (C).
[0011] A sixth embodiment of the present invention is the curable resin composition according to the first embodiment, further comprising a filler as component (D).
[0012] A seventh embodiment of the present invention is a sealant comprising the curable resin composition according to any one of the first to sixth embodiments.
[0013] An eighth embodiment of the present invention is a cured product obtained by heat-curing the curable resin composition according to any one of the first to sixth embodiments.
[0014] A ninth embodiment of the present invention is a cured product obtained by heat-curing the curable resin composition according to any one of the first to sixth embodiments together with an adherend by injection molding.
[0015] A tenth embodiment of the present invention is the cured product according to the eighth embodiment for use as a seal in a fuel cell.
[0016] An eleventh embodiment of the present invention is a fuel cell comprising at least one seal from the group consisting of a seal between two adjacent separators, a seal between a separator and a frame, a seal between a frame and an electrolyte membrane electrode assembly, and a seal between an electrolyte membrane and an electrode, the seal being made of the cured product according to the eighth embodiment. Effect of the Invention
[0017] Even when the curable resin composition according to the present invention is stored at a constant temperature, minute bubbles that are believed to be caused by hydrogen generation due to a dehydrogenation reaction between the remaining silanol groups and hydrosilyl groups do not occur, and the sealant after curing is free of defects due to bubbles. In addition, the curable resin composition has a low viscosity, and the cured product has a low compression set and high durability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The present invention will be described in detail below. In this specification, the expression "X to Y" means not less than X and not more than Y, with X and Y being the numerical values before and after the expression being included as the lower limit and upper limit, respectively.
[0019] The component (A) that can be used in the present invention is a curable polyisobutylene resin. The component (A) is liquid in an atmosphere at 25°C. The component (A) only needs to contain a component having a polyisobutylene skeleton, and can be composed of the components (A-1) to (A-5) described below. Here, the term "curable" refers to the fact that the component is crosslinked by energy rays or heat, polymerizes, and becomes a rubber-like solid at 25°C.
[0020] The (A-1) component that can be used in the present invention is a polyisobutylene having two or more allyl groups in one molecule. Polyisobutylene may have two or more -CH2C(CH3)2- units in one molecule, and may be copolymerized with a structural unit other than the -CH2C(CH3)2- unit. The (A-1) component is preferably unbranched and linear, and has allyl groups at both ends of the linear molecule. In that case, one molecule has two allyl groups. Also, it is preferable that at least one molecule contains 50% by mass or more of -CH2C(CH3)2- units, more preferably 70% by mass or more.
[0021] The component (A-1) is liquid under an atmosphere of 25°C, and its viscosity is preferably 10 to 5000 Pa·s in terms of coating properties such as bead coating and screen printing, more preferably 300 to 4500 Pa·s, and particularly preferably 500 to 4000 Pa·s. By having a polyisobutylene skeleton, the cured product is likely to have a low hardness but high strength and a rubber elastomer with low compression set. The molecular weight of the component (A-1) is not particularly limited, but the number average molecular weight is preferably 500 to 500,000 in terms of excellent durability, more preferably 1,000 to 100,000, and particularly preferably 3,000 to 50,000. The number average molecular weight can be calculated by gel permeation chromatography (GPC) or size exclusion chromatography (SEC), etc.
[0022] Specific examples of the (A-1) component include, but are not limited to, the EPION series manufactured by Kaneka Corporation, such as 200A, 400A, 450A, and 600A. In addition, the component may be used alone or in combination of multiple types.
[0023] The (A-2) component that can be used in the present invention is a compound having two or more hydrosilyl groups in one molecule. The hydrosilyl group is ≡Si-H. Examples include polyorganosiloxane compounds containing hydrosilyl groups in linear, branched, cyclic or network molecules. From the viewpoint of easily obtaining a rubber elastomer having a low compression set, the SiH value of the entire (A-2) component is preferably 0.1 to 10 mol / kg, more preferably 1 to 8 mol / kg, and particularly preferably 3 to 5 mol / kg.
[0024] Examples of commercially available products of component (A-2) include, but are not limited to, EPION series products such as CR300 and CR500 manufactured by Kaneka Corporation, HMS-013, HMS-151, and HMS-301 manufactured by Azmax Corporation, and SH1107 fluid manufactured by Dow Corning Toray Co., Ltd. In addition, the components may be used alone or in combination.
[0025] The amount of the (A-2) component is preferably 5 to 40 parts by mass, and more preferably 10 to 30 parts by mass, per 100 parts by mass of the (A-1) component. When the amount of the (A-2) component is 5 parts by mass or more, the curability can be maintained, and when the amount is 40 parts by mass or less, the flexibility of the cured product can be maintained.
[0026] The amount of hydrosilyl groups in the (A-2) component is 0.7 to 2.2 equivalents per mole of allyl groups in the (A-1) component. The amount is preferably 1.2 to 2.0 equivalents. If the amount of the (A-2) component added is more than 0.7 equivalents, the crosslink density tends to be high and the hydrogen gas barrier properties of the cured product tend to be improved, whereas if it is less than 2.2 equivalents, the problem of foaming of the cured product due to the generation of hydrogen gas by a dehydrogenation reaction tends to be avoided.
[0027] The component (A-3) that can be used in the present invention is a hydrosilylation catalyst. It is a catalyst that can cause an addition reaction between the allyl group of the component (A-1) and the hydrosilyl group of the component (A-2). It is sufficient that the catalyst can at least impart thermosetting properties to the curable resin composition. When the curable resin composition is to be cured by heating, preferred components of the component (A-3) include chloroplatinic acid, platinum alone, solid platinum supported on a carrier such as alumina, silica, or carbon black; complexes of chloroplatinic acid with alcohols, aldehydes, ketones, etc.; platinum-olefin complexes such as Pt(CH2=CH2)2Cl2; Pt n (ViMe2SiOSiMe2Vi) x , Pt[(MeViSiO)4] yand platinum-vinylsiloxane complexes such as Pt(PPh3)4 and Pt(PBu3)4; and platinum-phosphite complexes such as Pt(PPh3)4 and Pt(PBu3)4. Among these, chloroplatinic acid, platinum-olefin complexes, platinum-vinylsiloxane complexes, and the like are preferred from the viewpoint of excellent activity. Vi means a vinyl group. Examples of catalysts other than platinum compounds in component (A-3) include RhCl(PPh3)3, RhCl3, RuCl3, IrCl3, FeCl3, AlCl3, PdCl2·2H2O, NiCl2, TiCl4, and the like. These catalysts may be used alone or in combination of two or more kinds. In order to prevent a rapid reaction when component (A-3) is mixed with a composition of components (A-1) and (A-2), component (A-3) is preferably added in a state diluted with a solvent such as benzene, xylene, or ethylbenzene.
[0028] The amount of the (A-3) component is not particularly limited, but is added in the range of 0.001 to 1.0 part by mass, and more preferably 0.001 to 0.5 parts by mass, per 100 parts by mass of the (A-1) component. If the (A-3) component is 0.001 part by mass or more, curability is exhibited, and if it is 1.0 part by mass or less, storage stability can be maintained.
[0029] The component (A-4) that can be used in the present invention is a reaction inhibitor. The addition of the component (A-4) temporarily inhibits the crosslinking of the components (A-1) and (A-2) by the component (A-3). Examples of the component (A-4) include alkyne compounds, maleic acid compounds, organic phosphorus compounds, organic sulfur compounds, and nitrogen-containing compounds. These may be used alone or in combination of two or more.
[0030] Specific examples of the component (A-4) include alkyne compounds such as 3-hydroxy-3-methyl-1-butyne, 3-hydroxy-3-phenyl-1-butyne, 3,5-dimethyl-1-hexyn-3-ol, and 1-ethynyl-1-cyclohexanol, maleic acid compounds such as maleic anhydride and dimethyl maleate, organic phosphorus compounds such as triorganophosphines, diorganophosphines, organophosphorus compounds, and triorganophosphites, organomercaptans, diorganosulfides, hydrogen sulfide, benzothiazole, thiazol-1, and the like. and organic sulfur compounds such as N,N,N',N'-tetramethylethylenediamine, N,N-dimethylethylenediamine, N,N-diethylethylenediamine, N,N-dibutylethylenediamine, N,N-dibutyl-1,3-propanediamine, N,N-dimethyl-1,3-propanediamine, N,N,N',N'-tetraethylethylenediamine, N,N-dibutyl-1,4-butanediamine, and 2,2'-bipyridine, but are not limited to these.
[0031] The amount of component (A-4) added is preferably 0.01 to 5.0 parts by mass, more preferably 0.5 to 3.0 parts by mass, and most preferably 0.8 to 2.0 parts by mass, per 100 parts by mass of component (A-1).The mass ratio of components (A-3) and (A-4) is preferably 1:10 to 1:1000.
[0032] The (A-5) component that can be used in the present invention is a vinyl ether compound and / or a polyalkylsiloxane having a vinyl group. However, the (A-1) component is excluded. The (A-5) component is used as a so-called reactive diluent, and the (A-5) component can crosslink with the (A-2) component and can reduce the viscosity of the (A) component. Specific examples include, but are not limited to, trimethylolpropane trivinyl ether, pentaerythritol tetravinyl ether, cyclohexane dimethanol divinyl ether, and polyalkylsiloxane having a vinyl group. It is most preferable to use a vinyl ether compound and a polyalkylsiloxane having a vinyl group in combination. As for the vinyl ether compound, it is preferable to use cyclohexane dimethanol divinyl ether, which has both dilution ability and reactivity. In addition, it may be used alone or in combination of multiple types.
[0033] The amount of the (A-5) component added is preferably 0.1 to 50 parts by mass, and more preferably 10 to 40 parts by mass, per 100 parts by mass of the (A-1) component. When the amount of the (A-5) component is 0.1 part by mass or more, the viscosity of the (A) component can be lowered to improve workability, and when the amount is 50 parts by mass or less, the curability can be maintained.
[0034] The (B) component that can be used in the present invention is a defoaming agent that contains a silicone-based polymer as the (B-1) component and a vinyl-based polymer as the (B-2) component. However, the (B) component does not contain the (A-1) to (A-5) components. In order to fully exert the defoaming effect, it is preferable that the (B) component contains only the (B-1) component and the (B-2) component.
[0035] The silicone polymer defoamer, which is the component (B-1), is a compound having a silicone structure. Specifically, the silicone defoamers include dimethyl silicone or modified silicone as an oil type, a combination of silicone and a solvent as a solution type (dispersion), a combination of silicone oil and silica as a compound type, a combination of silicone oil and silica or a combination of water-soluble silicone and a water-soluble organic substance (silicone emulsifier) as a self-emulsifying compound, and a combination of silicone compound, emulsifier, and water as an emulsion type. Modified silicones include silicones that contain fluorine in the skeleton, and silicones in which the terminal of dimethyl silicone is replaced with another organic group instead of a methyl group. When a diluting component such as a solvent or water is mixed as a component, the component (B-1) refers only to the active component as a defoamer.
[0036] Known examples of the (B-1) component include BYK-066N and BYK-141 manufactured by BYK Japan Co., Ltd., and the Dappo series SN-374 manufactured by San Nopco Ltd., but are not limited to these.
[0037] The defoaming agent made of vinyl-based polymer, which is the component (B-2), does not have a silicone structure and contains a vinyl compound as a starting material. Specifically, acrylic / vinyl ether copolymers, olefin oligomers, vinyl ether polymers, etc. are known, but are not limited to these. Here, the vinyl compound does not include a (meth)acryloyl compound. Also, a copolymer of a vinyl compound and a (meth)acryloyl compound corresponds to the component (B-2), but a (meth)acryloyl homopolymer, which is a polymer of one type of (meth)acryloyl compound, or a (meth)acryloyl copolymer, which is a polymer of two or more types of (meth)acryloyl compounds, is not included in the component (B-2). The component (B-2) refers to only the active ingredient, even if it is a mixture of solvent and water.
[0038] Known examples of the (B-2) component include the Dappo series manufactured by San Nopco Ltd., such as SN-510, SN-353, and SN-530, and the Flourene AC-380 manufactured by Kyoeisha Chemical Co., Ltd., but are not limited to these.
[0039] The amount of the (B-1) component added is preferably 0.01 to 5.0 parts by mass, more preferably 1.0 to 4.0 parts by mass, per 100 parts by mass of the (A) component. The amount of the (B-2) component added is preferably 0.01 to 5.0 parts by mass, more preferably 0.1 to 4.0 parts by mass, per 100 parts by mass of the (A) component. The amount of the (B) component added is preferably 0.1 to 7.0 parts by mass, more preferably 1.0 to 6.0 parts by mass, and most preferably 3.0 to 6.0 parts by mass, per 100 parts by mass of the (A) component.
[0040] The component (C) that can be used in the present invention is a plasticizer. Here, the plasticizer refers to a compound that is low in volatility and does not have a reactive functional group. Here, the reactive functional group refers to a vinyl group, a vinylsiloxane group, a hydrosilyl group, an alkoxysilyl group, an epoxy group, a (meth)acryloyl group, an isocyanate group, etc.
[0041] Specific examples of the (C) component include, but are not limited to, phthalate ester plasticizers, adipate ester plasticizers, trimellitate ester plasticizers, polyester plasticizers, epoxidized vegetable oil plasticizers, polyalphaolefin plasticizers, etc. From the viewpoint of reducing the compression set of the cured product of the present invention, polyalphaolefin plasticizers are preferred, and it is known that, for example, polyalphaolefin plasticizers are produced by polymerization reaction and hydrogenation treatment using α-olefins derived from ethylene as raw materials. Specific examples of polyalphaolefin plasticizers include, but are not limited to, the SpectraSyn series manufactured by ExxonMobil.
[0042] For the purpose of imparting flexibility to the cured product, the (C) component is preferably added in an amount of 1 to 100 parts by mass, more preferably 1 to 60 parts by mass, and most preferably 1 to 40 parts by mass, per 100 parts by mass of the (A) component. Also, it may be used alone or in combination of two or more kinds.
[0043] The component (D) that can be used in the present invention is a filler. To improve the elastic modulus, fluidity, etc. of the cured product, a filler may be added to an extent that does not impair storage stability. Specific examples include organic powders and inorganic powders. In order to improve the mechanical strength of the cured product, it is preferable to contain an inorganic powder. In this specification, the average particle size refers to the value of the particle size at 50% of the cumulative volume, which is determined by measuring the particle size distribution with a laser diffraction particle size distribution measuring device. When two or more types of component (D) are mixed, the 50% average particle size of the mixed powder is used.
[0044] Examples of inorganic powder fillers include metal powder, glass powder, fumed silica powder, silica powder, alumina powder, mica powder, calcium carbonate powder, aluminum nitride powder, and aluminum powder. In particular, silica powder is preferred and can be blended for the purpose of adjusting the viscosity of the curable resin composition or improving the mechanical strength of the cured product. The average particle size of the silica powder is preferably 1.0 to 10 μm. The particle size of the fumed silica powder as observed by an electron microscope is preferably 1 to 100 nm. Silica powder or fumed silica powder that has been hydrophobized with organochlorosilanes, polyorganosiloxane, hexamethyldisilazane, etc. can be used. Specific examples of silica powder include, but are not limited to, Nipsil series SS-70 manufactured by Tosoh Silica Corporation. Specific examples of fumed silica powder include, but are not limited to, the Aerosil series manufactured by Nippon Aerosil, such as R974, R972, R972V, R972CF, R805, R812, R812S, R816, R8200, RY200, RX200, RY200S, and R202.
[0045] Silicone rubber powder, the surface of which is coated with silicone resin, is also included. This is a core-shell powder, with the core being silicone rubber and the shell being silicone resin. Silicone rubber powder refers to a fine powder of silicone rubber with a linear polydimethylsiloxane structure. Silicone resin refers to a silicone rubber with a siloxane bond of (RSiO3 / 2) n Here, R represents an organic group, and the molecular weight and the modified organic group are not particularly limited, and n has a three-dimensional network-like crosslinked structure represented by an integer of 3 or more. From the viewpoint of low viscosity in the present invention, it is particularly preferable that the shape is spherical, and it may be used alone or two or more types may be mixed. The 50% average particle size is not particularly limited, but is preferably 0.1 μm or more, and more preferably 0.5 μm or more. By being 0.1 μm or more, the curable resin composition can be kept at a low viscosity. In addition, it is preferably 20 μm or less, more preferably 15 μm or less, and more preferably 10 μm or less. By being 15 μm or less, the compression set of the cured product is low and the cured product is excellent. Specific examples include KMP-601, KMP-600, KMP-605, etc., as the KMP series manufactured by Shin-Etsu Chemical Co., Ltd., but are not limited thereto.
[0046] Examples of organic powder fillers include particles of polyethylene, polypropylene, nylon, cross-linked acrylic, cross-linked polystyrene, polyester, polyvinyl alcohol, polyvinyl butyral, polycarbonate, and the like.
[0047] From the viewpoint of excellent compression set and durability, the content of the (D) component is preferably 5 to 80 parts by mass, more preferably 10 to 70 parts by mass, and most preferably 15 to 60 parts by mass, per 100 parts by mass of the (A) component. Also, the (D) component may be used alone or in combination.
[0048] <Optional ingredients> Additives such as allyl compounds other than the component (A-1), adhesion promoters, storage stabilizers, antioxidants, light stabilizers, heavy metal deactivators, flame retardants, polymerization inhibitors, and coupling agents can be used in the curable resin composition of the present invention as long as they do not impair the properties.
[0049] An allyl compound other than the component (A-1) can be added as a reactive diluent, except for the component (A-5). Specific examples include 2,4,6-tris(allyloxy)-1,3,5-triazine, trimethylolpropane diallyl ether, pentaerythritol triallyl ether, triallyl isocyanurate, diallyl isocyanurate, diallyl monoglycidyl isocyanurate, diallyl monobenzyl isocyanurate, diallyl monopropyl isocyanurate, diallyl phthalate, triallyl trimellitate, diethylene glycol bisallyl carbonate, trimethylolpropane diallyl ether, trimethylolpropane triallyl ether, pentaerythritol triallyl ether, and pentaerythritol tetraallyl ether. ether, 1,1,2,2-tetraallyloxyethane, diarylidene pentaerythritol, triallyl cyanurate, 1,4-butanediol diallyl ether, nonanediol diallyl ether, 1,4-cyclohexane dimethanol diallyl ether, triethylene glycol diallyl ether, diallyl ether of bisphenol S, 1,3-bis(allyloxy)adamantane, 1,3,5-tris(allyloxy)adamantane, bisphenol A diallyl ether, 2,5-diallylphenol allyl ether, and oligomers thereof, and allyl ether of novolak phenol, but are not limited thereto.
[0050] The antioxidant may be, but is not limited to, a phenol-based antioxidant, a hindered phenol-based antioxidant, an organic sulfur-based antioxidant, an amine-based antioxidant, or a benzotriazole-based antioxidant. The light stabilizer may be, but is not limited to, a hindered amine-based light stabilizer or a benzoate-based light stabilizer. Specific examples of the antioxidant and light stabilizer include the Sumilizer series manufactured by Sumitomo Chemical Co., Ltd., such as BHT, S, BP-76, MDP-S, GM, BBM-S, WX-R, NW, BP-179, BP-101, GA-80, TNP, TPP-R, and P-16, and the Adeka STAB series manufactured by ADEKA Corporation, such as AO-20, AO-30, AO-40, AO-50, AO-60, and AO- Examples of such polyvinyl chloride resins manufactured by Chiba Specialty Chemicals Co., Ltd. include, but are not limited to, 70, AO-80, AO-330, PEP-4C, PEP-8, PEP-24G, PEP-36, HP-10, 2112, 260, 522A, 329K, 1500, C, 135A, 3010, and the Tinuvin series manufactured by Chiba Specialty Chemicals Co., Ltd., such as 770, 765, 144, 622, 111, 123, and 292.
[0051] The heavy metal deactivator may be a chelating agent. Specific examples of the heavy metal deactivator include, but are not limited to, the ADK STAB series manufactured by ADEKA CORPORATION, such as CDA-1, CDA-1M, CDA-6S, CDA-10, ZS-27, ZS-90, and ZS-91.
[0052] Coupling agents refer to compounds that contain hydrolyzable silyl groups such as trimethoxysilane, triethoxysilane, dimethoxymethylsilane, and diethoxymethylsilane in the molecule. If the coupling agent contains a vinyl group, it is classified as a coupling agent, and components (A) and (B) are excluded. Specific examples of coupling agents include 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, methacryloxyoctyltrimethoxysilane, vinyltrimethoxysilane, vinyltrichlorosilane, vinyltriethoxysilane, vinyl-tris(β-methoxyethoxy)silane, γ-chloropropyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. , γ-glycidoxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, γ-ureidopropyltriethoxysilane, hydroxyethyl methacrylate phosphate, methacryloxyoxyethyl acid phosphate, methacryloxyoxyethyl acid phosphate monoethylamine half salt, 2-hydroxyethyl methacrylic acid phosphate, etc. Among these, hydroxyethyl methacrylate phosphate, methacryloxyoxyethyl acid phosphate, methacryloxyoxyethyl acid phosphate monoethylamine half salt, 2-hydroxyethyl methacrylic acid phosphate, oligomeric reactive siloxane having hydrolyzable silyl group and vinyl group, etc. are listed, but are not limited to these. In addition, it is possible to use one or more kinds in combination. The coupling agent is contained in an amount of preferably 0.05 to 10 parts by mass, more preferably 0.5 to 10 parts by mass, and most preferably 1.0 to 5.0 parts by mass, per 100 parts by mass of the component (A).
[0053] The curable resin composition of the present invention can be produced by a conventionally known method, for example, by mixing predetermined amounts of each component using a mixing means such as a single-shaft mixer or a twin-shaft mixer at a temperature of preferably 10 to 70° C. for preferably 0.1 to 5 hours.
[0054] Since the curable resin composition is liquid at 25°C when used as a sealant, a known resin composition coating method is used as a method for coating the adherend. For example, methods such as dispensing using an automatic coater, spraying, inkjet, screen printing, gravure printing, dipping, and spin coating can be used. In addition, the curable resin composition of the present invention is preferably screen printed in view of its low viscosity.
[0055] The curing method of the curable resin composition of the present invention is not particularly limited, but it can be cured by heating. The curing temperature is not particularly limited, but is preferably 30 to 300° C., more preferably 50 to 200° C., and even more preferably 60 to 150° C. The curing time is not particularly limited, but when the temperature is 60 to 150° C., it is preferably 20 minutes or more and less than 5 hours, and even more preferably 40 minutes or more and less than 3 hours.
[0056] The curable resin composition of the present invention can be used in fields such as fuel cells, solar cells, dye-sensitized solar cells, lithium ion batteries, electrolytic capacitors, liquid crystal displays, organic EL displays, electronic paper, LEDs, hard disk drives, photodiodes, optical communications, optical fibers, optical isolators, laminates such as IC cards, sensors, substrates, medical devices, etc. Among these, fuel cells are suitable since the composition has both low viscosity and low compression set.
[0057] A fuel cell is a power generation device that produces electricity by chemically reacting hydrogen and oxygen. There are four types of fuel cells: polymer electrolyte fuel cells, phosphoric acid fuel cells, molten carbonate fuel cells, and solid oxide fuel cells. Among them, polymer electrolyte fuel cells have a relatively low operating temperature (around 80°C) yet high power generation efficiency, so they are used as a power source for automobiles, home power generation devices, small power sources for electronic devices such as mobile phones, and emergency power sources.
[0058] A typical solid polymer fuel cell cell is a structure that includes a membrane electrode assembly (MEA) in which a polymer electrolyte membrane is sandwiched between a fuel electrode and an air electrode, a frame that supports the MEA, and a separator in which a gas flow path is formed. When the solid polymer fuel cell is started up, fuel gas (hydrogen gas) and oxidizing gas (oxygen gas) are supplied through the fuel gas flow path and the oxidizing gas flow path. In addition, cooling water flows through the cooling water flow path to reduce heat generation during power generation. Several hundred of these cells are stacked and packaged together to form a cell stack.
[0059] When fuel gas (hydrogen gas) is supplied to the fuel electrode and oxidizing gas (oxygen gas) is supplied to the oxygen electrode, the following reactions occur at each electrode, with the overall reaction producing water (H2+1 / 2O2→H2O). In more detail, as shown below, protons (H+) produced at the fuel electrode diffuse through the solid polymer membrane and move to the oxygen electrode side, and water (H2O) produced by reacting with oxygen is discharged from the oxygen electrode side. Fuel electrode (anode electrode): H2 → 2H + +2e - Oxygen electrode (cathode electrode): 1 / 2O2+2H + +2e - →H2O
[0060] To start a polymer electrolyte fuel cell, it is necessary to supply a fuel gas containing hydrogen to the anode electrode and an oxidizing gas containing oxygen to the cathode electrode, separately and in isolation. If the isolation is insufficient and one gas mixes with the other, it may cause a decrease in power generation efficiency. For this reason, sealing agents are often used to prevent leakage of fuel gas, oxygen gas, etc. Specifically, sealing agents are used between adjacent separators, between the separator and the frame, between the frame and the electrolyte membrane or MEA, etc.
[0061] The polymer electrolyte membrane may be a cation exchange membrane having ion conductivity, and may preferably be a fluorine-based polymer having a sulfonic acid group, which is chemically stable and resistant to high-temperature operation. Commercially available products include Nafion manufactured by DuPont, Flemion manufactured by Asahi Kasei Corporation, and Aciplex manufactured by Asahi Glass Co., Ltd. Although polymer electrolyte membranes are generally difficult to bond, they can be bonded by using the curable resin composition of the present invention.
[0062] The fuel electrode is called a hydrogen electrode or anode, and a known one is used. For example, a catalyst such as platinum, nickel, or ruthenium is supported on carbon. The air electrode is called an oxygen electrode or cathode, and a known one is used. For example, a catalyst such as platinum or an alloy is supported on carbon. A gas diffusion layer may be provided on the surface of each electrode. A known gas diffusion layer is used, and examples of the gas diffusion layer include carbon paper, carbon cloth, and carbon fiber.
[0063] The separator has fine uneven channels through which the fuel gas and oxidizing gas pass and are supplied to the electrodes. The separator is made of aluminum, stainless steel, titanium, graphite, carbon, etc.
[0064] The frame supports and reinforces the thin electrolyte membrane or MEA to prevent it from breaking. Examples of frame materials include thermoplastic resins such as polyvinyl chloride, polyethylene naphthalate (PEN), polyethylene terephthalate (PET), polypropylene (PP), and polycarbonate.
[0065] The fuel cell of the present invention is a fuel cell that is characterized by being sealed with the curable resin composition of the present invention. Examples of components in a fuel cell that require sealing include a separator, a frame, an electrolyte membrane, a fuel electrode, an air electrode, and an MEA. More specific examples of sealed locations include adjacent separators, adjacent separators and frames, adjacent frames and electrolyte membranes, and adjacent frames and MEAs. The main purpose of sealing adjacent separators and frames, adjacent frames and electrolyte membranes, and adjacent frames and MEAs is to prevent gas mixing and leakage, and the purpose of sealing between adjacent separators is to prevent gas leakage and leakage of cooling water from the cooling water flow path to the outside.
[0066] The curable resin composition of the present invention is preferably used as a sealant. A sealant is applied to the gap of one adherend or two or more adherends to keep the inside sealed, and is used for the purpose of preventing leakage and preventing moisture from entering from the outside, that is, for sealing. Hereinafter, a composition containing the curable resin composition for this purpose before curing is called a sealant, a cured product obtained by curing the curable resin composition for sealing purposes is called a seal, and a method of curing is called a sealing method.
[0067] The sealing method using the curable resin composition of the present invention is not particularly limited, but examples thereof include FIPG (formed-in-place gasket), CIPG (cured-in-place gasket), MIPG (molded-in-place gasket), etc. Among them, CIPG and MIPG are preferred from the viewpoint of obtaining low compression set.
[0068] The FIPG in the present invention is a method for sealing at least two members selected from the group consisting of a separator, a frame, an electrolyte, a fuel electrode, an air electrode, and an electrolyte membrane electrode assembly, which are components constituting a fuel cell, and is a sealing method carried out in the following order of steps 1 to 3. Step 1: Applying a curable resin composition to the sealing surface of one of the components Step 2: The part from step 1 is attached to the sealing surface of the other part. Step 3: Heating and curing the curable resin composition
[0069] The CIPG in the present invention is a method for sealing at least two members selected from the group consisting of a separator, a frame, an electrolyte, a fuel electrode, an air electrode, and an electrolyte membrane electrode assembly, which are components constituting a fuel cell, and is a sealing method carried out in the following order of steps 1 to 3. Step 1: Applying a curable resin composition to the sealing surface of one of the components Step 2: Heating and curing the curable resin composition Step 3: Press the part from step 2 against the sealing surface of the other part to secure it in place.
[0070] In the present invention, MIPG refers to a case where a mold is pressed against the sealing surface of a member and the composition is pressure-fed into the mold cavity and applied to the sealing surface in step 1 of the FIPG or CIPG. In step 2, in the case of FIPG, the mold is released from the sealing surface before hardening, whereas in the case of CIPG, the composition is hardened while the mold is pressed against the sealing surface, and it is preferable to apply a fluorine-based, silicone-based or other mold release agent to the inner surface of the mold in advance to make it easier to remove the seal from the mold. EXAMPLES
[0071] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Hereinafter, the curable resin composition will be simply referred to as the composition.
[0072] The following components were used to prepare Examples 1-12 and Comparative Examples 1-12. (A) Component: Curable polyisobutylene resin Component (A-1): Polyisobutylene having two or more allyl groups in one molecule Polyisobutylene having allyl groups at both ends, with a molecular weight of 2750 Pa·s at 25°C and a number average molecular weight of 15350 (EPION 450A, manufactured by Kaneka Corporation) Component (A-2): A compound having two or more hydrosilyl groups in one molecule Hydrosilyl group-containing compound (EPION CR500, manufactured by Kaneka Corporation) Component (A-3): hydrosilylation catalyst Platinum divinyltetramethyldisiloxane complex, 3% by mass in xylene / ethylbenzene solution (Pt-VTSC-3.0X, Umicore Precious Metals Japan, Inc.) (A-4) Component: Reaction inhibitor Dimethyl maleate (reagent) Component (A-5): vinyl ether compound and / or polyalkylsiloxane having a vinyl group Cyclohexanedimethanol divinyl ether (CHDEV, manufactured by Nippon Carbide Industries Co., Ltd.) Polymethylsiloxane with vinyl groups (XF40-A1987 Momentive Performance Materials Japan LLC) (B) Component: Defoamer Component (B-1): Defoamer consisting of a silicone-based polymer Additives for paints, coatings, and inks Organically modified and alkyl-modified polysiloxane with antifoaming properties (active ingredient: 0.7% by mass) (BYK-066N BYK Japan Co., Ltd.) Additives for paints, coatings, and inks Organically modified and alkyl-modified polysiloxane with antifoaming properties (active ingredient: 3.2% by mass) (BYK-141 BYK Japan Co., Ltd.) Fluorosilicone (active ingredient: 100% by weight) (Dappo SN-374, San Nopco Ltd.) Component (B-2): Defoamer consisting of a vinyl polymer Vinyl polymer (active ingredient: 30% by weight) (Dappo SN-510, San Nopco Ltd.) Vinyl polymer (active ingredient: 40% by weight) (Dappo SN-353, San Nopco Ltd.) Vinyl polymer (active ingredient: 20% by weight) (Dappo SN-530, San Nopco Ltd.) Acrylic / vinyl copolymer (active ingredient: 100% by mass) (Floren AC-380, Kyoeisha Chemical Co., Ltd.) Component (B'): a defoaming agent other than components (B-1) and (B-2) Additives for paints, coatings, and inks Acrylic polymer with anti-fogging effect (active ingredient: 52% by mass) (BYK-392 BYK Japan Co., Ltd.) Acrylic copolymer mixture (active ingredient: 40% by weight) (Dappo SN-348, San Nopco Ltd.) Acrylic copolymer mixture (active ingredient: 38% by weight) (Dappo SN-354, San Nopco Ltd.) (C) Component: Plasticizer Polyalphaolefin plasticizer (SpectraSyn4 ExxonMobil) (D) Component: Filler Hydrophobic silica powder with an average particle size of 5.3 μm (Nipsil SS-70 Tosoh Silica Corporation) Coupling Agent Oligomeric reactive siloxane with vinyl groups (containing methoxysilane groups) (Dynasylan 6490, EVONIC) 3-Glycidoxypropyltrimethoxysilane (KBM-403 Shin-Etsu Chemical Co., Ltd.)
[0073] To prepare Examples 1 to 12 and Comparative Examples 1 to 12, the compositions are prepared as follows. The components (A-1), (A-2), (A-4) and (A-5) are weighed into a stirring vessel and stirred for 30 minutes under a 25°C atmosphere, and the components (B) (or (B')), (C), (D), coupling agent and other components are weighed into a stirring vessel and stirred for another 30 minutes under a 25°C atmosphere. Finally, the component (A-3) is weighed and vacuum degassed while being checked for another 30 minutes under a 25°C atmosphere. The detailed amounts of the preparations are shown in Table 1, and all values are expressed in parts by mass.
[0074] For Examples 1 to 12 and Comparative Examples 1 to 12, initial foaming was confirmed, and the results are also summarized in Table 1.
[0075] [Short-term foaming confirmed] The composition is applied to one glass plate in a bead shape with a height of 5 mm and a length of 30 mm, and the composition is crushed by the other glass plate, maintaining a gap of 0.5 mm between the two glass plates. In this state, the mixture is left in a 25°C atmosphere for 1 minute, and the occurrence of bubbles is visually confirmed through the glass plate based on the following evaluation criteria, which is regarded as "short-term foaming." Evaluation criteria ○: No foaming at all △: 1 or 2 bubbles ×: 3 or more bubbles
[0076] [Table 1]
[0077] Examples 1 to 12 contain the (B-1) component and the (B-2) component, Comparative Examples 1 to 5 contain only the (B-1) component, and Comparative Examples 6 to 12 contain the (B-1) component and the (B') component (an antifoaming agent other than the (B-1) component or the (B-2) component). When short-term foaming was confirmed, when the (B-1) component and the (B-2) component were contained, the results were "○" or "△", which shows that there was no residual foam in the early stages and there was a low risk of failure as a sealant.
[0078] For Example 2 and Comparative Example 1, the differences between the initial state immediately after preparation of the composition and after one year of storage in an atmosphere at 10°C were confirmed. The test items were appearance check, specific gravity measurement, viscosity measurement, hardness measurement, tensile strength measurement, elongation measurement, tensile shear adhesive strength measurement, compression set measurement, curing speed check, and long-term foaming check. The initial results and those after one year in an atmosphere at 10°C are summarized in Table 2.
[0079] [External appearance check] The color was visually confirmed and was taken as "appearance".
[0080] [Specific gravity measurement] The specific gravity is measured using a density cup.
[0081] [Viscosity measurement] The "viscosity (Pa s)" of the composition at 25°C was measured using a rheometer (HAAKE MARSIII) under the following measurement conditions. Taking into account the ejection properties, the upper limit of the viscosity is preferably 600 to 900 Pa s, and more preferably 700 to 800 Pa s. Measurement conditions Preshare condition 20(1 / s)30sec Geometry C20 / 1 Shear rate: 0.01 to 100 1 / s (reading value is 1.0 1 / s) Temperature 25±2℃
[0082] [Hardness measurement] A polytetrafluoroethylene frame measuring 2 mm thick x 50 mm long x 50 mm long is placed on a polytetrafluoroethylene plate and the composition is applied. The polytetrafluoroethylene plate is heated in a hot air drying oven at 130°C for 1 hour and 30 minutes to harden the composition into a sheet. Three sheets of the hardened material are stacked to form a test piece. The pressure surface of an A-type durometer (hardness tester) is pressed with a force of 10 N while keeping it parallel to the test piece, so that the pressure surface and the sample are in close contact. The maximum value is read during measurement and is defined as the "A hardness". Details are in accordance with JIS K 6253 (2012). It is preferable that the hardness is A30 or less from the viewpoint of following the distortion and shape deformation of the adherend.
[0083] [Tensile strength measurement] A polytetrafluoroethylene frame measuring 2 mm thick x 100 mm long x 200 mm long is placed on a polytetrafluoroethylene plate and the composition is applied. The polytetrafluoroethylene plate is heated in a hot air drying oven at 130°C for 1 hour and 30 minutes to harden the composition into a sheet. The hardened product is punched out with a cutter for a No. 3 dumbbell to prepare a test piece. Both ends of the test piece are fixed to the chuck so that the long axis of the test piece and the center of the chuck are in a straight line. The test piece is pulled at a tensile speed of 500 mm / min until it breaks, and the maximum load is measured and calculated from the cross-sectional area to obtain the "tensile strength (MPa)". Details are in accordance with JIS K 6251 (2010). The tensile strength is preferably 1.0 MPa or more to prevent the bead from breaking.
[0084] [Elongation measurement] A polytetrafluoroethylene frame measuring 2 mm thick x 100 mm long x 200 mm long is placed on a polytetrafluoroethylene plate and the composition is applied. The polytetrafluoroethylene plate is heated in a hot air drying oven at 130°C for 1 hour and 30 minutes to harden the composition into a sheet. The hardened product is punched out with a cutter for a No. 3 dumbbell to prepare a test piece, and marks are drawn on the test piece at intervals of 20 mm. Both ends of the test piece are fixed to the chuck so that the long axis of the test piece and the center of the chuck are in a straight line. When pulled at a tensile speed of 500 mm / min, the test piece stretches and the spacing between the marks widens, so the spacing between the marks is measured with a caliper until the test piece breaks. The percentage of stretch based on the initial spacing between the marks is taken as the "elongation rate (%)". The elongation rate is preferably 200% or more from the viewpoint of following the distortion and shape deformation of the adherend.
[0085] [Lateral shear adhesive strength measurement] The composition is applied to the bonding surface between two pieces of aluminum (A1050P) measuring 25 mm wide x 100 mm long x 1 mm thick, and fixed with a fixture so that the bonding area is 25 mm x 10 mm, and any protruding parts are wiped off. A test piece is made by heating for 1 hour and 30 minutes in a 130°C atmosphere. Both ends of the test piece are fixed to the chuck of a universal testing machine, and the test piece is pulled in the shear direction at 50 mm / sec. The "shear adhesive strength (MPa)" is calculated from the strength at the maximum load. For details, follow JIS K 6850. The shear adhesive strength is preferably 1.0 MPa or more to prevent the material from falling off from the adherend.
[0086] [Compression set test] The composition is applied to a steel substrate of 80 mm long x 50 mm wide x 5 mm thick, with a bead width of 2 mm, bead thickness of 1 mm, and length of 50 mm, and then left in a hot air drying oven at 130°C for 65 minutes to harden the composition. After removing it once and returning it to room temperature, the cured product is taken out after 96 hours at 90°C with another substrate at a compression ratio of 25%, and the compression set is calculated from the bead height after returning to room temperature, and this is called "compression set (%)". The calculation is made according to the formula below, and the test method is in accordance with JIS K 6262 (2013). Compression set of 30% or less is preferable.
[0087]
number
[0088] [Check curing time] Using a rheometer (HAAKE MARSIII), the viscosity is measured as it changes over time under the following measurement conditions. As the temperature rises, the composition polymerizes, so the viscosity starts to rise, and at a certain temperature the viscosity stops increasing. The time at which the tangent when the viscosity increases and the tangent when the viscosity stops increasing is read as the intersection point, and this is taken as the "curing time (seconds)." Considering workability, the curing time is preferably 500 to 1000 seconds. Measurement conditions Heating rate: 10℃ / min Temperature range: 25~130℃ Oscillation: 1Hz
[0089] [Bubble confirmation] The composition is applied to a glass plate in a bead shape with a height of 5 mm and a length of 50 mm, and cured in this state for 30 minutes at 130°C. The presence or absence of bubbles is then visually confirmed through the glass plate from the opposite side of the bead (check 1), and then the cross section of the bead is cut in one place with a cutter and the presence or absence of bubbles on the cross section is visually confirmed (check 2), and the "bubble confirmation" is judged according to the following evaluation criteria. Considering the breakage of the bead, it is preferable that the bubble confirmation is "○". Evaluation criteria ○: No foaming in either Confirmation 1 or Confirmation 2 ×: There is foaming in either Check 1 or Check 2
[0090] [Table 2]
[0091] In the above short-term foaming, Example 2 was rated "○" and Comparative Example 1 was rated "×". Although the exact reason is not clear, it is believed that the foaming confirmed in the initial stage of foaming in Comparative Example 1 was removed by heating. However, foaming was not confirmed in Example 2 at the initial stage or after one year, whereas foaming was confirmed after one year in Comparative Example 1. In other words, in Example 2, the combination of the (B) component, which is an antifoaming agent, gave good results with the (B-1) component and the (B-2) component. Furthermore, no significant difference was observed in the physical properties of the cured product when the (B) component was changed between Example 2 and Comparative Example 1. [Industrial Applicability]
[0092] Even when the curable resin composition according to the present invention is stored at a constant temperature, no minute bubbles are generated, which are believed to be due to hydrogen being generated by a dehydrogenation reaction between the residual silanol groups and hydrosilyl groups, and the sealant after curing is free of defects due to bubbles, has low compression set and high durability, and can therefore be used as a sealant for various purposes, making it industrially useful.
Claims
1. A curable resin composition comprising the following components (A) and (B): Component (A): Curable polyisobutylene resin Component (B): a defoaming agent containing the following components (B-1) and (B-2) Component (B-1): Defoaming agent made of silicone polymer Component (B-2): Defoamer consisting of vinyl polymer
2. The curable resin composition according to claim 1, comprising only the components (B-1) and (B-2) as the defoaming agent.
3. The curable resin composition according to claim 1, wherein the component (A) comprises the following components (A-1) to (A-4): Component (A-1): Polyisobutylene having two or more allyl groups in one molecule Component (A-2): a compound having two or more hydrosilyl groups in one molecule Component (A-3): Hydrosilylation catalyst Component (A-4): Reaction inhibitor
4. The curable resin composition according to claim 2, wherein the component (A) further comprises a component (A-5) of a vinyl ether compound and / or a polyalkylsiloxane having a vinyl group.
5. The curable resin composition according to claim 1 , further comprising a plasticizer as component (C).
6. The curable resin composition according to claim 1 , further comprising a filler as component (D).
7. A sealant comprising the curable resin composition according to any one of claims 1 to 6.
8. A cured product obtained by heat-curing the curable resin composition according to any one of claims 1 to 6.
9. A cured product obtained by heat-curing the curable resin composition according to any one of claims 1 to 6 together with an adherend by injection molding.
10. The cured product according to claim 8, which is used as a seal for a fuel cell.
11. 9. A fuel cell comprising at least one seal made of the cured product according to claim 8, the seal being between two adjacent separators, a seal between a separator and a frame, a seal between a frame and an electrolyte membrane electrode assembly, and a seal between an electrolyte membrane and an electrode.
Citation Information
Patent Citations
Curing composition and sealing method
WO2005095520A1