Piezoelectric material and piezoelectric device
The co-substitution of zinc oxide with rare earth elements and manganese in a specific range enhances the piezoelectric constant d33, addressing the lack of optimization in existing technologies and improving material performance for piezoelectric devices.
Patent Information
- Application Number
- JP2023085908
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-12-05
AI Technical Summary
Existing technologies have not explored the co-substitution of zinc in zinc oxide with rare earth elements and manganese to improve piezoelectric properties, particularly the piezoelectric constant d33, nor have they determined the optimal substitution range for enhanced performance.
A piezoelectric material is developed by co-substituting zinc oxide with rare earth elements and manganese, specifically formulated as Zn1-x(R0.5+δMn0.5-δ)O, where x is between 0.04 and 0.15, and |δ| is 0.1 or less, to enhance the piezoelectric constant d33.
The piezoelectric constant d33 is improved by more than 1.6 times, achieving values of 15 pC/N or more, with the material being chemically stable and easier to manufacture at lower film-forming temperatures, suitable for applications in piezoelectric devices.
Smart Images

Figure 2024168880000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to piezoelectric materials and piezoelectric devices. [Background technology]
[0002] It has been known that zinc oxide (ZnO)-based wurtzite oxides can be doped with at least one element selected from the group including rare earth elements and manganese (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2014-9384 A [Patent Document 2] JP 2013-103843 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, in Patent Documents 1 and 2, the piezoelectric properties (particularly the piezoelectric constant d 33 There has been no discussion at all about co-substitution of zinc in zinc oxide with rare earth elements and manganese in order to improve piezoelectric properties, nor about the range of substitution amounts that can improve the piezoelectric properties.
[0005] The present invention has been made to solve the above problems, and its object is to improve the piezoelectric properties (particularly the piezoelectric constant d 33 The present invention provides a piezoelectric material capable of improving the piezoelectric effect, and a piezoelectric device including the piezoelectric material. [Means for solving the problem]
[0006] A piezoelectric material according to one aspect of the present invention contains zinc, rare earth elements, and manganese as main components, and is represented by Zn for zinc, R for rare earth elements, and Mn for manganese. 1-x (R 0.5+ δMn 0.5- δ) x The rare earth is at least one element selected from rare earth elements, the substitution amount x is a value of 0.04 or more and 0.15 or less, and the variable amount δ is a value of 0.1 or less in absolute value.
[0007] A piezoelectric device according to another aspect of the present invention includes the above-described piezoelectric material, a pair of electrodes sandwiching the piezoelectric material, and a substrate supporting the piezoelectric material via one of the electrodes. Effect of the Invention
[0008] According to the present invention, the zinc in zinc oxide is co-substituted with a rare earth element and manganese in a range of a predetermined substitution amount, thereby improving the piezoelectric properties (particularly the piezoelectric constant d 33 ) can be improved. [Brief description of the drawings]
[0009] [Figure 1] FIG. 2 is an explanatory diagram illustrating a crystal structure of non-doped zinc oxide. [Diagram 2] FIG. 2 is an explanatory diagram illustrating a crystal structure of a wurtzite oxide contained in a piezoelectric material according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a cross-sectional view showing a schematic configuration of a BAW filter, which is an example of a piezoelectric device including the piezoelectric material. [Figure 4] FIG. 4 is a cross-sectional view showing another configuration of the BAW filter. [Diagram 5] FIG. 2 is an explanatory diagram showing the piezoelectric performance of each thin film of the examples and comparative examples. [Figure 6] 1 is a graph showing a representative XRD diffraction pattern of an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, exemplary embodiments of the present invention will be described with reference to the drawings.
[0011] [1. About Piezoelectric Materials] FIG. 1 is an explanatory diagram showing a schematic crystal structure of non-doped zinc oxide (hereinafter, zinc oxide is also referred to as ZnO), which is the premise of the piezoelectric material of this embodiment. Non-doped ZnO has a wurtzite crystal structure with a hexagonal unit lattice. In this crystal structure, zinc ions (Zn 2+ ) and oxygen ions (O 2- ) are stacked alternately in the c-axis direction. The O layers are positioned at a position shifted in the c-axis direction from the equidistant positions of the two Zn layers above and below them. In the above crystal structure, a polarization vector is generated in a direction parallel to the c-axis, even when no external electric field is applied.
[0012] The piezoelectric material of the present embodiment has a wurtzite oxide containing zinc, rare earths, and manganese as its main components. Here, "wurtzite oxide containing zinc, rare earths, and manganese as its main components" means that the wurtzite oxide of the present embodiment may contain components (impurities) other than zinc, rare earths, and manganese.
[0013] 2 is an explanatory diagram showing a schematic crystal structure of the wurtzite oxide of the present embodiment. The wurtzite oxide of the present embodiment is a crystal structure in which zinc is Zn, rare earth is R, and manganese is Mn. Zinc 1-x (R 0.5+ δMn 0.5- δ) x O (1) That is, the wurtzite oxide of the present embodiment is a ZnO crystal structure shown in FIG. 2+ is replaced with R, and at the same time, other Zn 2+has a structure in which R is replaced with Mn. In this way, the simultaneous replacement of some elements with multiple elements is called "co-substitution." Note that formula (1) indicates that the atomic concentration ratio of Zn to (R+Mn) is (1-x):x, and the atomic concentration ratio of R to Mn is (0.5+δ):(0.5-δ). Note that the atomic concentration ratio can also be interpreted as the molar ratio.
[0014] Here, the rare earth (R) is at least one element selected from the rare earth elements. The rare earth elements specifically refer to two elements, scandium (Sc) and yttrium (Y), and 15 elements of the lanthanoid series, totaling 17 elements. The 15 elements of the lanthanoid series are specifically lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), eurobium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu). The rare earth (R) may be one element selected from the above 17 elements, or may be multiple elements.
[0015] In the above formula (1), x is Zn 2+ x indicates the amount of substitution when R and Mn ions are co-substituted with each other. In other words, the amount of substitution x indicates the ratio of the total atomic concentration of R and Mn to all elements at the Zn site. In this embodiment, from the viewpoint of realizing the desired piezoelectric characteristics described later, the amount of substitution x is set to a value of 0.04 or more and 0.15 or less.
[0016] In the above formula (1), δ indicates the range (variance) of variation in the atomic concentrations of R and Mn that is permitted to achieve the desired piezoelectric characteristics described below. Specifically, the variable δ is set to a value of 0.1 or less in absolute value. In other words, -0.1≦δ≦0.1.
[0017] The valence of the above-mentioned Mn can be any value from divalent to heptavalent. Therefore, in FIG. 2, if the valence of Mn is m, m is any value from 2 to 7. On the other hand, the valence of rare earth (R) is mainly stable at trivalent, but in some cases it can be divalent or even tetravalent like Ce. Therefore, in FIG. 2, if the valence of R is n, n is 2 to 4.
[0018] As in this embodiment, some of the Zn included in the Zn site of the ZnO crystal structure 2+ By co-substitution of R and Mn, the charge balance of the crystal structure is greatly disrupted and the polarization becomes larger than that of non-doped ZnO. As a result, the piezoelectric properties (e.g., the longitudinal piezoelectric constant d 33 ) can be improved.
[0019] For example, the piezoelectric constant d of non-doped ZnO is 33 It is generally known that the piezoelectric constant d 33 It has been confirmed that a C / N of 15 pC / N or more can be obtained.
[0020] In particular, when the substitution amount x is a value between 0.04 and 0.15, the piezoelectric constant d 33 In addition, since the uncertainty δ is an absolute value of 0.1 or less, even if the atomic concentrations of R and Mn deviate from the target concentrations due to the deposition conditions during deposition of the piezoelectric material, the above piezoelectric constant d 33 It is possible to achieve this.
[0021] In addition, the piezoelectric material of this embodiment is an oxide mainly composed of ZnO. Therefore, compared to piezoelectric materials such as PZT (lead zirconate titanate), it can be formed at a lower film formation temperature and is easy to fabricate. In addition, the oxide is chemically stable even at elevated temperatures in an oxygen atmosphere such as the air, so it is also easy to fabricate in this respect.
[0022] Higher piezoelectric constant d 33 From the viewpoint of realizing the above, it is desirable that the substitution amount x is a value between 0.08 and 0.11. If the substitution amount x is a value within the above range, the piezoelectric constant d 33 It has been confirmed from the examples described below that the above can be realized.
[0023] The rare earth element is preferably Ce. It is generally known that, for example, in the case of trivalent ions of lanthanoid elements, the ionic radius becomes smaller as the atomic number increases. Among the lanthanoid elements, Ce, which has the second smallest atomic number, has an ionic radius of 1.01×10 -10 m, and the ionic radius of La, the element with the smallest atomic number, is 1.03×10 -10 m. In other words, among the lanthanide elements, Ce has the second largest ionic radius after La. Also, as mentioned above, Ce can be tetravalent among the rare earth elements. Therefore, by using Ce as a rare earth (rare earth element), it is easy to break the charge balance of the crystal structure and increase the polarization. As a result, the piezoelectric constant d 33 can be easily improved.
[0024] The thickness of the piezoelectric material is preferably 0.1 μm or more and 10 μm or less. Piezoelectric materials in this thickness range are suitable for application to piezoelectric devices. As an example of a piezoelectric device, an elastic wave filter (frequency filter) such as a BAW (Bulk Acoustic Wave) filter can be considered.
[0025] [2. About Piezoelectric Devices] 3 is a cross-sectional view showing the configuration of a BAW filter 10, which is an example of a piezoelectric device according to this embodiment. The BAW filter 10 is formed by laminating a lower electrode 2, a piezoelectric thin film 3, and an upper electrode 4 in this order on a substrate 1 to form a resonator.
[0026] The substrate 1 is composed of a semiconductor substrate made of, for example, single crystal Si (silicon). A cavity 1a is formed in the substrate 1. This allows the piezoelectric thin film 3 to vibrate without being bound by the substrate 1. The lower electrode 2 is composed of, for example, platinum (Pt), but may be composed of a metal such as gold (Au), aluminum (Al), iridium (Ir), or ruthenium (Ru) instead of Pt. The upper electrode 4 is also composed of a metal such as Pt or Au like the lower electrode 2, but may be composed of a metal different from the lower electrode 2.
[0027] 3, the piezoelectric thin film 3 is composed of one layer 3a. The layer 3a is made of a piezoelectric material having the wurtzite oxide described in this embodiment. That is, the piezoelectric material of this embodiment described above is applied to the piezoelectric thin film 3.
[0028] Thus, the BAW filter 10 as a piezoelectric device comprises the piezoelectric material (piezoelectric thin film 3) of the present embodiment described above, a pair of electrodes (lower electrode 2 and upper electrode 4) that sandwich the piezoelectric material, and a substrate 1 that supports the piezoelectric material via one of the electrodes (lower electrode 2).
[0029] When a high-frequency signal is applied to the piezoelectric thin film 3 by a pair of electrodes, an elastic wave is excited that propagates in the thickness direction according to the direction of spontaneous polarization of the piezoelectric material. Then, vibration (resonance) occurs in the thickness direction at a frequency according to the film thickness and composition of the piezoelectric thin film 3. In the piezoelectric thin film 3, mechanical vibrations are converted into electrical signals due to the piezoelectric effect of the piezoelectric material. In other words, by resonating the piezoelectric thin film 3, a signal in a specific frequency range can be extracted as an electrical signal.
[0030] For example, when communicating with a mobile device such as a mobile phone or a smartphone, it is necessary to extract radio waves of a required frequency from radio waves received by an antenna. In addition, the fifth generation mobile communication system, called 5G, uses frequencies in the 3.7 GHz, 4.5 GHz, and 28 GHz bands. The BAW filter 10 of this embodiment can extract high-frequency signals by increasing the resonant frequency by thinning the piezoelectric thin film 3. Therefore, the BAW filter 10 of this embodiment is particularly suitable for mobile devices that use 5G communication systems.
[0031] FIG. 4 is a cross-sectional view showing another configuration of the BAW filter 10. The BAW filter 10 in FIG. 4 has the same configuration as the BAW filter 10 shown in FIG. 3, except that the piezoelectric thin film 3 is formed by stacking a plurality of layers 3a. In FIG. 4, the number of layers 3a is two, but it may be three or more. Each layer 3a is made of the wurtzite oxide of this embodiment. Here, if the substitution amount x is the same in each layer 3a, each layer 3a can be regarded as one layer as a whole, so in FIG. 4, the substitution amount x in each layer 3a is different from each other. For example, the BAW filter 10 in FIG. 4 can be constructed by selecting any two of the four piezoelectric materials shown in Examples 1 to 4 described later and stacking them as each layer 3a. Note that when the piezoelectric thin film 3 is composed of three or more layers 3a, it is sufficient that the substitution amount x of at least two layers 3a is different.
[0032] In this way, the piezoelectric material constituting the piezoelectric thin film 3 of this embodiment may have multiple layers of the wurtzite oxide of this embodiment (multiple layers 3a), and the substitution amount x in each layer may be different from each other. In this case, the polarization state such as the polarization value and polarization direction will differ for each layer depending on the substitution amount x, and a piezoelectric device (BAW filter 10) can be realized in which the frequency of the entire piezoelectric thin film 3 is increased by a multiple of the number of layers. The polarization direction can also be configured by inverting the polarization of only some of the layers by a strong electric field.
[0033] 3. Examples Next, specific examples of the piezoelectric material of this embodiment will be described. A dual-target sputtering system using two targets, zinc oxide (ZnO) and cerium manganate (CeMnO3), was used to fabricate Zn with different substitution amounts x. 1-x (Ce,Mn) x The ZnO thin film was formed by sputtering on a Si substrate with a Pt electrode (lower electrode) heated to 300°C. A mixture of 75% argon (Ar) and 25% oxygen (O2) was used as the sputtering gas. The pressure in the film formation device (vacuum chamber) was 1 Pa. In addition, the ZnO thin film was formed by sputtering on a Si substrate with a Pt electrode (lower electrode) heated to 300°C. 1-x (Ce,Mn) x The O thin film was formed to a thickness of 300 nm on a Si substrate with a thickness of 525 μm.
[0034] The input power to the ZnO target was 100 W, and the input power to the CeMnO3 target was the value shown in Fig. 5. The substitution amount x was adjusted by changing the input power to the CeMnO3 target as shown in Fig. 5.
[0035] 5 shows the piezoelectric performance of each of the thin films of Examples 1 to 4 and Comparative Examples 1 and 2 together with the substitution amount x. Note that Comparative Example 1 is a thin film with a substitution amount x of zero (i.e., a non-doped ZnO thin film), and Comparative Example 2 is a ZnO thin film with a substitution amount x of 0.17. 1-x (Ce,Mn) x In Examples 1 to 4, the substitution amount x is 0.04, 0.08, 0.11, and 0.15, respectively. 1-x (Ce,Mn) x The piezoelectric performance of the thin film (piezoelectric constant d 33 ) was evaluated by forming a 100 nm thick Pt electrode (upper electrode) on top of the thin film by sputtering, and detecting the charge generated when stress was applied to the thin film in the thickness direction via the upper electrode.
[0036] The crystal structure of the deposited thin film was confirmed to be a c-axis oriented film with a wurtzite crystal structure by 2θ / θ measurement using X-ray diffraction (XRD). Since almost the same XRD diffraction patterns were obtained in Examples 1 to 4 and Comparative Examples 1 and 2, the XRD diffraction pattern of the piezoelectric thin film of Example 2 is shown in FIG. 6 as a representative example. It can be seen from FIG. 6 that the thin film of Example 2 is a piezoelectric thin film oriented along the (002) axis, i.e., the c-axis. This makes it easy to understand that the other piezoelectric thin films such as Example 1 are also c-axis oriented films in accordance with FIG. 6. Furthermore, energy dispersive X-ray spectroscopy (EDX) was used to determine the chemical composition of the thin film, revealing that Zn 1-x (Ce,Mn) x It was confirmed that the composition was O.
[0037] From the results in FIG. 5, when the substitution amount x is in the range of 0.04 to 0.15, the piezoelectric constant d 33 is 15 pC / N or more (see Examples 1 to 4), and the piezoelectric constant d 33 It was confirmed that the piezoelectric constant d 33 is 18 pC / N or more (see Examples 2 and 3), and the piezoelectric constant d 33 was confirmed to be improved by more than two times.
[0038] In addition, when the ratio of the standard atomic concentrations of Ce and Mn is 1:1 when Zn is co-substituted with Ce and Mn, the absolute value of the variable δ is 0.1 or less (specifically, the absolute value is 0.01 to 0.05), and it is found that Ce and Mn are present in the thin film at a ratio close to the standard atomic concentration ratio. In other words, even when Zn is co-substituted with Ce and Mn, it is found that the piezoelectric performance is improved with small variations from the standard atomic concentrations of Ce and Mn.
[0039] [4. Supplementary Information] In this embodiment and the examples, Zn 1-x(R,Mn) x In the wurtzite oxide represented by O, an example in which Ce is used as the rare earth (R) has been described. However, it is expected that the same effect as in this embodiment can be obtained even when one or more rare earth elements other than Ce are used to co-substitute Zn together with Mn.
[0040] In this embodiment and the examples, the content of lithium (Li) in the wurtzite oxide mainly composed of ZnO is zero. In this embodiment, since the wurtzite oxide contains Mn, the electrical insulation can be improved without containing Li. In other words, by using Mn instead of Li, the electrical insulation can be improved while the piezoelectric constant d 33 can be improved.
[0041] In this embodiment, Zn 1-x (R,Mn) x Although the BAW filter 10 has been described as an example of a piezoelectric device to which the wurtzite oxide represented by O can be applied, the wurtzite oxide of this embodiment can also be applied to a SAW (surface acoustic wave) filter.
[0042] Piezoelectric devices to which the piezoelectric material of this embodiment is applied are not limited to frequency filters such as BAW filters and SAW filters. For example, the piezoelectric material described in this embodiment can also be applied to actuators (piezoelectric actuators) of inkjet heads, piezoelectric sensors (vibration sensors, gyro sensors, ultrasonic sensors), infrared sensors, non-volatile memories, etc.
[0043] [5. Notes] The piezoelectric material and the piezoelectric device described in the above embodiment can be expressed as follows.
[0044] The piezoelectric material in Appendix (1) is The main components are zinc, rare earths, and manganese, with zinc as Zn, rare earths as R, and manganese as Mn, and Zn 1-x (R 0.5+ δMn 0.5-δ) x O, The rare earth is at least one element selected from rare earth elements, The substitution amount x is a value of 0.04 or more and 0.15 or less, The uncertainty δ is an absolute value of 0.1 or less.
[0045] The piezoelectric material of appendix (2) is the piezoelectric material according to appendix (1), The longitudinal piezoelectric constant d along the c axis 33 However, it is more than 15 pC / N.
[0046] The piezoelectric material of supplementary note (3) is the piezoelectric material according to supplementary note (1) or (2), The substitution amount x is a value not less than 0.08 and not more than 0.11.
[0047] The piezoelectric material of appendix (4) is the piezoelectric material according to appendix (3), The longitudinal piezoelectric constant d along the c axis 33 However, it is more than 18 pC / N.
[0048] The piezoelectric material of supplementary note (5) is the piezoelectric material according to any one of supplementary notes (1) to (4), The rare earth is cerium.
[0049] The piezoelectric material of supplementary note (6) is the piezoelectric material according to any one of supplementary notes (1) to (5), The film thickness is 0.1 μm or more and 10 μm or less.
[0050] The piezoelectric material of appendix (7) is the piezoelectric material according to any one of appendix (1) to (6), The wurtzite oxide has multiple layers, The substitution amount x in each layer is different from each other.
[0051] The piezoelectric device in Appendix (8) is A piezoelectric material according to any one of appendices (1) to (7), A pair of electrodes sandwiching the piezoelectric material; and a substrate supporting the piezoelectric material via one of the electrodes.
[0052] Although the embodiment of the present invention has been described above, the scope of the present invention is not limited to this, and the invention can be expanded or modified without departing from the spirit of the invention. [Industrial Applicability]
[0053] The piezoelectric material of the present invention can be used in piezoelectric devices such as acoustic wave filters. [Explanation of symbols]
[0054] 1 Board 2 Lower electrode (electrode) 3. Piezoelectric thin film (piezoelectric material) 3a layer 4 Upper electrode 10 BAW filter (piezoelectric device)
Claims
1. The main components are zinc, rare earth elements, and manganese, with zinc as Zn, rare earth elements as R, and manganese as Mn, and 1-x (R 0.5+ δMn 0.5- δ) x O, The rare earth is at least one element selected from rare earth elements, The substitution amount x is a value of 0.04 or more and 0.15 or less, A piezoelectric material, wherein the uncertainty δ is an absolute value of 0.1 or less.
2. The longitudinal piezoelectric constant d along the c-axis 33 The piezoelectric material according to claim 1 , wherein the piezoelectric constant is 15 pC / N or more.
3. The piezoelectric material according to claim 1 , wherein the substitution amount x is a value not less than 0.08 and not more than 0.
11.
4. The longitudinal piezoelectric constant d along the c-axis 33 The piezoelectric material according to claim 3 , wherein the piezoelectric constant is 18 pC / N or more.
5. The piezoelectric material of claim 1 , wherein the rare earth is cerium.
6. The piezoelectric material according to claim 1 , having a film thickness of 0.1 μm or more and 10 μm or less.
7. The wurtzite oxide has multiple layers, The piezoelectric material of claim 1 , wherein the substitution amount x in each layer is different from each other.
8. A piezoelectric material according to any one of claims 1 to 7; A pair of electrodes sandwiching the piezoelectric material; A piezoelectric device comprising: a substrate that supports the piezoelectric material via one of the electrodes.
Citation Information
Patent Citations
Inorganic crystal film and manufacturing method therefor
JP2013103843A