Alkali-dispersible hot melt pressure-sensitive adhesive

The hot melt adhesive composition with a thermoplastic block copolymer, metallocene olefin polymer, and tackifier resin addresses label retention and stringiness issues, ensuring effective adhesion and easy removal for recyclable PET bottles.

JP2024168981APending Publication Date: 2024-12-05HENKEL JAPAN
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023086123
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing alkali-dispersed hot melt adhesives used for labels on PET bottles and glass bottles face issues with insufficient label retention, adhesive residue, stringiness, and peeling due to carbon dioxide expansion, especially in the beverage industry, where labels lift and peel off during transportation and carbonation processes.

Method used

A hot melt adhesive composition comprising a thermoplastic block copolymer, metallocene olefin polymer, tackifier resin, and fatty acids or derivatives, with specific ratios and properties to enhance alkali dispersibility, label retention, and reduce stringiness.

Benefits of technology

The adhesive provides excellent label retention, minimal adhesive residue, and reduced stringiness, ensuring labels remain intact during transportation and easy removal in alkaline solutions, suitable for recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024168981000001
    Figure 2024168981000001
  • Figure 2024168981000002
    Figure 2024168981000002
  • Figure 2024168981000003
    Figure 2024168981000003
Patent Text Reader

Abstract

To provide an alkali-dispersible hot melt pressure-sensitive adhesive that has high alkali dispersibility, excellent label-holding strength, is less likely to cause the trouble of adhesive residue, capable of reducing stringiness, and furthermore ensures excellent adhesive strength between body-wrapping labels.SOLUTION: There is provided an alkali-dispersible hot melt pressure-sensitive adhesive, comprising: (A) a thermoplastic block copolymer that is a copolymer of vinyl aromatic hydrocarbons and conjugated diene compounds, (B) a metallocene olefin polymer, (C) a tackifying resin, and (D) at least one selected from a group consisting of fatty acids and derivatives thereof.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an alkali-dispersible hot-melt adhesive suitable as an adhesive for labels on glass bottles, PET (polyethylene terephthalate) bottles, etc., and in particular to an alkali-dispersible hot-melt adhesive effective as an adhesive used for bonding PET bottles and labels for carbonated beverages. [Background technology]

[0002] Aluminum cans, glass bottles, and polyethylene terephthalate (PET) bottles are commonly used as containers for medicines, foods, and beverages. Labels are attached to the surface of these containers with an adhesive strong enough that they cannot be peeled off by hand. For labels on beverage containers, roll labels made of polyethylene terephthalate (PET) film, biaxially oriented polypropylene film (OPP), and polylactic acid (PLA) film are often used.

[0003] When containers with labels attached are reused, the used containers must be collected at the factory, immersed in a heated alkaline aqueous solution, and the label and container must be separated. Therefore, the adhesive applied to the container label must have the property of swelling, softening, dispersing, or dissolving in the alkaline aqueous solution, allowing the label to be peeled off from the container in a short time (alkaline dispersibility).

[0004] Patent Documents 1 to 4 disclose alkali-dispersible hot melt adhesives containing a styrene block copolymer, a tackifier resin, and fats and oils. The hot melt adhesives in these documents contain modified rosin as a tackifier resin, and coconut oil, rice oil, sunflower oil, rapeseed oil, or the like as fats and oils.

[0005] Alkali-dispersible hot melt adhesives are required to have not only "alkali dispersibility" but also excellent adhesion (retention) between the label and the container. In the beverage industry in particular, in addition to "alkali dispersibility" and "retention," they are also required to leave no glue on the container after the label is peeled off, i.e., to have excellent removability.

[0006] When beverage manufacturers manufacture carbonated beverages, there is a process of filling PET bottles with the carbonated beverage, which have labels affixed thereto. If the PET bottles are left as they are after being filled with carbonated beverages, the carbon dioxide causes the PET bottle to expand slightly, which can cause the label to float and peel off from the bottle. However, the hot melt adhesives described in Patent Documents 1 and 2 are insufficient to solve the problems of label floating and peeling. In the beverage industry, there is a demand for an alkali dispersible hot melt adhesive with particularly excellent holding power.

[0007] In addition, alkali dispersion type hot melt adhesives are also required to reduce stringing during application. When applying hot melt adhesives, dedicated application devices such as hot melt applicators and labelers are often used. The hot melt adhesive is heated to about 120 to 190°C and applied to the adherend, which is a label, from the head of a dedicated application device. When the hot melt adhesive is applied to the label, thread-like matter of the hot melt adhesive may be generated between the tip of the head and the label. In addition, thread-like matter may be generated between a label that has been completely applied and a label that has not been completely applied. This thread-like matter is due to the stringing property of the hot melt adhesive, and stains the head or label. Therefore, the development of a hot melt adhesive with less stringing is an important responsibility for adhesive manufacturers. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2014-159563 A [Patent Document 2] JP 2016-204588 A [Patent Document 3] Patent Publication No. 2021-095443 [Patent Document 4] Patent Publication No. 2021-095448 Summary of the Invention [Problem to be solved by the invention]

[0009] In recent years, the demand for improved performance of hot melt pressure sensitive adhesives has become increasingly severe. In this situation, the hot melt pressure sensitive adhesives of Patent Documents 1 and 2 still lack sufficient improvement in stringiness. The hot melt pressure sensitive adhesives of Patent Documents 3 and 4 have improved stringiness, and in this respect meet the demands of the industry.

[0010] However, the problem of bottle-wrapped labels (made of biaxially oriented polypropylene film (OPP) etc.) peeling off due to vibration during transportation has become evident, and there is a demand to strengthen the adhesive strength of the film overlapping parts of the bottle-wrapped labels.

[0011] The present invention has been made to solve the above problems, and aims to provide an alkali-dispersible hot melt pressure-sensitive adhesive that has high alkali dispersibility, excellent label retention, is less likely to cause problems with residual glue, reduces stringiness, and has excellent adhesive strength between wrapped labels. [Means for solving the problem]

[0012] The present invention and preferred embodiments thereof are as follows.

[0013] 1. (A) a thermoplastic block copolymer which is a copolymer of a vinyl aromatic hydrocarbon and a conjugated diene compound; (B) Metallocene-based olefin polymer (C) a tackifying resin, and (D) at least one selected from the group consisting of fatty acids and derivatives thereof; Alkaline dispersible hot melt adhesive.

[0014] 2. The alkali dispersible hot melt pressure sensitive adhesive of embodiment 1, comprising 1 to 20 parts by mass of the metallocene olefin polymer (B) per 100 parts by weight of the total weight of the components (A) to (D).

[0015] 3. The alkali-dispersible hot melt pressure sensitive adhesive according to embodiment 1 or 2, wherein the metallocene olefin polymer (B) has a weight-average molecular weight polymer having a weight-average molecular weight of 12,000 or more.

[0016] 4. The alkali-dispersible hot-melt pressure-sensitive adhesive according to any one of Aspects 1 to 3, wherein the metallocene olefin polymer (B) comprises a copolymer of ethylene and an olefin having 3 to 20 carbon atoms.

[0017] 5. The alkali-dispersible hot-melt pressure-sensitive adhesive according to any one of aspects 1 to 4, wherein the thermoplastic block copolymer (A) comprises (A1) a styrene-based block copolymer having a styrene content of less than 40 mass %.

[0018] 6. The alkali-dispersible hot melt pressure sensitive adhesive of embodiment 5, comprising 70 parts by mass or more of (A1) a styrene block copolymer having a styrene content of less than 40% by mass, relative to 100 parts by mass of the total weight of components (A) to (D).

[0019] 7. The alkali dispersible hot melt pressure sensitive adhesive of any one of Aspects 1 to 6, wherein the (C) tackifier resin comprises a rosin ester and an α-methylstyrene resin.

[0020] 8. The alkali-dispersible hot-melt pressure-sensitive adhesive according to any one of Aspects 1 to 7, further comprising a Fischer-Tropsch wax.

[0021] 9. A label having an adhesive layer made of the alkali dispersible hot melt adhesive according to any one of embodiments 1 to 8.

[0022] 10. A body-wrapped label having an adhesive layer made of the alkali-dispersible hot-melt adhesive of any one of embodiments 1 to 8 in the overlapping portions of both ends of the film that are adhered to each other when wrapped around the body of a container.

[0023] 11. The label of embodiment 9 or 10, having a substrate made of polypropylene film.

[0024] 12. A container having the label of any one of embodiments 9 to 11 attached thereto. Effect of the Invention

[0025] The alkali dispersible hot melt adhesive of the present invention can be used to adhere labels to containers such as PET bottles, glass bottles, etc., and has excellent label retention. For example, when a label is adhered to a container such as a PET bottle filled with a carbonated drink using the alkali dispersible hot melt adhesive of the present invention, the label is less likely to shift or float even if the container expands.

[0026] The alkali-dispersible hot melt adhesive of the present invention has high alkali dispersibility, and when a container with a label attached thereto is immersed in an alkaline aqueous solution, the label can be peeled off cleanly without leaving any adhesive residue. Furthermore, the alkali-dispersible hot melt adhesive of the present invention allows the label to be peeled off again by hand or the like, and leaves little adhesive residue when the label is peeled off again.

[0027] The alkali dispersible hot melt pressure sensitive adhesive of the present invention is excellent in the above-mentioned properties and is therefore suitable for use in containers to be recycled.

[0028] The alkali dispersible hot melt pressure sensitive adhesive of the present invention is applied to labels and the like using a dedicated application device or the like, and can suppress the occurrence of stringiness during application.

[0029] In addition, the hot melt adhesive of the present invention has excellent adhesive strength between labels wrapped around the body, particularly shear strength, so that even if a label is affixed to a container and the labeled container is transported for a long period of time, the overlapping film portion of the label wrapped around the body will not peel off from the container due to vibrations during transport, etc. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] The alkali-dispersible hot melt pressure sensitive adhesive of the present invention contains all of four components: (A) a thermoplastic block copolymer which is a copolymer of a vinyl aromatic hydrocarbon and a conjugated diene compound; (B) a metallocene-based olefin polymer; (C) a tackifier resin; and (D) at least one component selected from the group consisting of fatty acids and derivatives thereof.

[0031] In this specification, these components may be referred to as "component (A)," "component (B)," "component (C)," and "component (D)," respectively, and the alkali-dispersible hot-melt pressure-sensitive adhesive of the present invention may be referred to simply as the "hot-melt pressure-sensitive adhesive."

[0032] <(A) Thermoplastic block copolymer> The "(A) thermoplastic block copolymer" is a copolymer in which a vinyl aromatic hydrocarbon and a conjugated diene compound are block copolymerized, and is usually a resin composition having a vinyl aromatic hydrocarbon block and a conjugated diene compound block.

[0033] Here, the term "vinyl aromatic hydrocarbon" refers to an aromatic hydrocarbon compound having a vinyl group, and specific examples thereof include styrene, o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 1,3-dimethylstyrene, α-methylstyrene, vinylnaphthalene, and vinylanthracene. Styrene is particularly preferred. These vinyl aromatic hydrocarbons can be used alone or in combination.

[0034] "Conjugated diene compound" means a diolefin compound having at least one pair of conjugated double bonds. Specific examples of "conjugated diene compound" include 1,3-butadiene, 2-methyl-1,3-butadiene (or isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, and 1,3-hexadiene. 1,3-butadiene and 2-methyl-1,3-butadiene are particularly preferred. These conjugated diene compounds can be used alone or in combination.

[0035] The thermoplastic block copolymer (A) used in the present invention may be either a non-hydrogenated product or a hydrogenated product.

[0036] A specific example of the "unhydrogenated" thermoplastic block copolymer (A) is one in which the block based on a conjugated diene compound is not hydrogenated. A specific example of the "hydrogenated thermoplastic block copolymer (A)" is one in which the block based on a conjugated diene compound is hydrogenated in whole or in part.

[0037] The hydrogenated ratio of the "hydrogenated product" of (A) thermoplastic block copolymer can be expressed as the "hydrogenation ratio". The "hydrogenation ratio" of the "hydrogenated product of (A) thermoplastic block copolymer" refers to the ratio of double bonds that have been hydrogenated and converted to saturated hydrocarbon bonds, based on the total aliphatic double bonds contained in the block based on the conjugated diene compound. This "hydrogenation ratio" can be measured by an infrared spectrophotometer, a nuclear magnetic resonance apparatus, or the like.

[0038] In one embodiment of the present invention, the thermoplastic block copolymer (A) is preferably a styrene-based block copolymer. The styrene-based block copolymer means a polymer having at least one styrene block. The styrene block means a segment having styrene as the main monomer, and is preferably a segment substantially composed of styrene only.

[0039] Specific examples of the "(A) unhydrogenated thermoplastic block copolymer" include styrene-isoprene-styrene block copolymer (also referred to as "SIS") and styrene-butadiene-styrene block copolymer (also referred to as "SBS"). Specific examples of the "(A) hydrogenated thermoplastic block copolymer" include hydrogenated styrene-isoprene-styrene block copolymer (also referred to as "SEPS"), hydrogenated styrene-butadiene-styrene block copolymer (also referred to as "SEBS"), and styrene-butylene-butadiene-styrene block copolymer (also referred to as "SBBS").

[0040] In the present invention, the weight average molecular weight (Mw) of the compound contained as component (A) is not particularly limited, but is preferably 1.0×10 4 ~3.0×10 5 It is preferable that the ratio is 5.0×10 4 ~2.0×10 5 It is more preferable that:

[0041] In this specification, the weight average molecular weight is determined by converting the molecular weight using gel permeation chromatography (GPC) with a calibration curve using polystyrene having a monodisperse molecular weight as a standard substance.

[0042] The alkali-dispersible hot melt pressure sensitive adhesive of the present invention contains the thermoplastic block copolymer (A), which gives it excellent cohesive strength, an excellent balance between label retention and adhesive residue, and improved shear strength at the adhesive joints between labels wrapped around the body.

[0043] In one embodiment of the present invention, (A) a thermoplastic block copolymer (component (A) preferably contains (A1) a styrene-based block copolymer having a styrene content of less than 40 mass% (sometimes referred to as "component (A1)"). The "styrene content" refers to the proportion of styrene contained in the thermoplastic block copolymer. The styrene content of component (A1) is preferably less than 40 mass%, more preferably less than 35 mass%, and even more preferably from 15 mass% to less than 35 mass%.

[0044] The hot melt pressure sensitive adhesive of the present invention contains component (A1) having a styrene content within the above range, thereby enabling the label to be stably held on a container such as a PET bottle, making the label less likely to float or shift.

[0045] In the hot melt pressure sensitive adhesive of the present invention, the content of component (A1) is preferably 70 parts by mass or more, more preferably 80 parts by mass or more, and may be 100 parts by mass, relative to 100 parts by mass of the total amount of component (A). When the content of component (A1) is within the above range, the holding power of the hot melt pressure sensitive adhesive of the present invention is further improved.

[0046] The thermoplastic block copolymer (A) may be used alone or in combination of two or more types, and in one embodiment, (A1) a styrene-based block copolymer having a styrene content of less than 40% by mass may be blended with a styrene-based block copolymer not corresponding to (A1). A styrene-based block copolymer not corresponding to (A1) means one having a styrene content of 40% by mass or more (hereinafter, sometimes referred to as "(A2) a styrene-based block copolymer having a styrene content of 40% by mass or more" or "component (A2)").

[0047] In the present invention, as the (A1) styrene-based block copolymer having a styrene content of less than 40% by mass, a commercially available product can be used. For example, Tufprene T420 (trade name), Tuftec P3000 (trade name), and Tuftec H1053 (trade name), manufactured by Asahi Kasei Chemicals Corporation; Quintac3460 (trade name), Quintac3433N (trade name), Quintac3520 (trade name), and Quintac3270 (trade name) manufactured by Zeon Corporation; Examples of such rubbers include Kraton D1160 (trade name), Kraton G1650 (trade name), Kraton G1652 (trade name), and Kraton G1657 (trade name).

[0048] It is preferable that component (A) is a triblock styrene-based block copolymer having a diblock content of 0 mass%, and in particular, when a triblock styrene-based block copolymer having a diblock content of 0 mass% is used as component (A1), the holding power of the hot melt pressure-sensitive adhesive becomes even better.

[0049] In this specification, the term "diblock" refers to a block copolymer having two blocks, and generally refers to a block copolymer having one each of a "vinyl aromatic hydrocarbon block", preferably a "styrene block", and a "conjugated diene compound block (which may be hydrogenated)", and can be represented, for example, by the following formula (1).

[0050] SE (1) (In formula (1), S is a styrene block, and E is a conjugated diene compound block.)

[0051] In this specification, the "diblock content" of component (A) refers to the proportion of a diblock copolymer (preferably a block copolymer having one styrene block and one conjugated diene compound block represented by formula (1)) contained in the thermoplastic copolymer of component (A).

[0052] The triblock styrene-based block copolymer preferably has a structure represented by the following formula (2) and does not contain any other blocks.

[0053] SES (2) (In formula (2), S is a styrene block, and E is a conjugated diene compound block.)

[0054] In this specification, a triblock styrene-based block copolymer has a diblock content of 0 mass % and is distinguished from a diblock styrene-based block copolymer.

[0055] In the present invention, it is most desirable that component (A1) is a styrene-ethylene / butylene-styrene (SEBS) triblock copolymer. The hot melt pressure-sensitive adhesive of the present invention contains a styrene-ethylene / butylene-styrene (SEBS) triblock copolymer, which significantly improves the cohesive strength. As a result, when a label is adhered to a container using the hot melt pressure-sensitive adhesive, the label will not lift off the container or shift over a long period of time, and the label can maintain its adhesion.

[0056] (A2) Commercially available styrene-based block copolymers having a styrene content of 40% by mass or more include Asaprene T439 (trade name), Tufprene 125 (trade name), Tufprene A (trade name), Tuftec P2000 (trade name), Tuftec H1043 (trade name), and Tuftec H1051 (trade name), all of which are manufactured by Asahi Kasei Chemicals Corporation; TR2000 (product name), TR2250 (product name) manufactured by JSR; and SO1T6414 (trade name) manufactured by Enichem Co. These commercially available products may be used alone or in combination.

[0057] <(B) Metallocene-based olefin polymer> "(B) Metallocene-based olefin polymer" refers to a polymer obtained by polymerizing an olefin in the presence of a metallocene catalyst. The metallocene-based olefin polymer contains a chemical structure derived from the metallocene catalyst in the molecule. An example of the chemical structure derived from the metallocene catalyst is a chemical structure including the metallocene catalyst itself as shown in the following formula (I) or a modified product of formula (I).

[0058] [ka]

[0059] In formula (I), M represents a metal or a metal having a halogen atom or the like bonded thereto.

[0060] The viscosity of the (B) metallocene olefin polymer at 170°C is 10,000 mPa·s or less, more preferably 1000 to 10,000 mPa·s, and even more preferably 2000 to 8000 mPa·s. The viscosity of the (B) metallocene olefin polymer at 170°C is measured with a Brookfield RVT viscometer (spindle No. 27).

[0061] When the alkali dispersible hot melt adhesive of the present invention contains (B) a metallocene olefin polymer, when a label is adhered to a container with this hot melt adhesive, the label does not float or shift from the container for a long period of time. Furthermore, when a body-wrapped label is adhered to a container with the hot melt adhesive of the present invention, the film overlapping portion of the body-wrapped label does not peel off from the container due to vibration during transportation, etc., even if the labeled container is transported for a long period of time.

[0062] When olefin is polymerized using a metallocene catalyst, (B) metallocene-based olefin polymer is synthesized that has (i) crystallinity and (ii) a very narrow molecular weight distribution. (i) means that complete isotacticity and syndiotacticity can be controlled arbitrarily. Therefore, there is no bias in crystallinity, and a polymer with uniform arrangement and ratio of methyl groups is obtained, and there is a low possibility of low crystallinity sites causing a decrease in adhesive strength. Regarding (ii), the degree of molecular weight distribution of (B) metallocene-based olefin polymer is preferably 1.0 to 3.5 when expressed as polydispersity (Mw / Mn). Hot melt adhesives containing polyolefins with polydispersity of 1.0 to 3.5 have excellent adhesive strength. Molecular weight distribution is a concept that indicates the distribution of molecular weight of a synthetic polymer, and the ratio of weight average molecular weight (Mw) to number average molecular weight (Mn) (polydispersity: Mw / Mn) is used as a measure. In the present invention, the molecular weight distribution is measured by gel permeation chromatography (GPC).

[0063] The metallocene-based olefin polymer (B) may be either a homopolymer or a copolymer. Examples of the homopolymer include polyethylene and polypropylene.

[0064] In this specification, the copolymer refers to a copolymer of ethylene and a copolymerizable monomer that can be copolymerized with ethylene. Examples of the copolymerizable monomer include α-olefins such as propylene, 1-octene, and 1-butene; carboxylic acids (esters) having an ethylenic double bond such as vinyl acetate, (meth)acrylic acid, (meth)acrylic acid esters, maleic acid, and maleic acid esters; and carboxylic acid anhydrides having an ethylenic double bond such as maleic anhydride and phthalic anhydride. These copolymerizable monomers may be copolymerized with ethylene alone, or two or more types of copolymerizable monomers may be copolymerized.

[0065] That is, in the present invention, examples of the (B) metallocene-based olefin polymer include homopolymers of ethylene and propylene, and examples of the ethylene copolymer include ethylene / α-olefin copolymer, ethylene / carboxylic acid copolymer having an ethylenic double bond, ethylene / carboxylic acid ester copolymer having an ethylenic double bond, and ethylene / carboxylic anhydride copolymer having an ethylenic double bond. In this specification, acrylic acid and methacrylic acid are collectively referred to as "(meth)acrylic acid", and acrylic acid esters and methacrylic acid esters are collectively referred to as "(meth)acrylic acid esters". Examples of the ethylene / α-olefin copolymer include ethylene / propylene copolymer, ethylene / 1-octene copolymer, ethylene / 1-butene copolymer, and ethylene / propylene / 1-butene copolymer.

[0066] From the viewpoint of improving threadability and retention of a label wrapped around the body, the (B) metallocene-based olefin polymer is preferably a copolymer of ethylene and an olefin having 3 to 20 carbon atoms, more preferably a polymer based on polyethylene or polypropylene, particularly preferably an ethylene / propylene copolymer or an ethylene / octene copolymer, and most preferably an ethylene / propylene copolymer.

[0067] The hot melt adhesive of the present invention has excellent coatability and little stringiness, particularly when the metallocene olefin polymer (B) is an ethylene / propylene copolymer. Furthermore, even if a label is attached to a container with the hot melt pressure-sensitive adhesive of the present invention and the labeled container is transported for a long period of time, the film overlapping portion of the body-wrapped label will not peel off from the container due to vibration during transportation, etc.

[0068] In the present invention, the weight average molecular weight of the metallocene olefin polymer (B) is preferably 12,000 or more, particularly preferably 15,000 or more, more preferably 20,000 to 500,000, and most preferably 25,000 to 400,000. By having the weight average molecular weight of component (B) within the above range, the balance between adhesive residue and retention is maintained, and the film overlapping portion of the label becomes less likely to peel off from the container even when the labeled container is transported for a long period of time.

[0069] The weight average molecular weight (Mw) refers to a value measured by gel permeation chromatography (GPC). Specifically, the value can be measured using the following device and measurement method. A Waters RI is used as a detector. A Tosoh TSKGEL GMHHR-H(S)HT is used as a GPC column. The sample is dissolved in 1,2,4-trichlorobenzene and passed through at a flow rate of 1.0 ml / min and a measurement temperature of 145°C. The molecular weight is converted using a polypropylene calibration curve to determine the weight average molecular weight.

[0070] Since the number average molecular weight (Mn) is also determined by the same method, the molecular weight distribution is also calculated by GPC.

[0071] (B) Commercially available metallocene-based olefin polymers include: Examples of metallocene-based ethylene / propylene copolymers include Vistamax 8780 (trade name) and Vistamax 8880 (trade name) manufactured by ExxonMobil Corporation; Examples of metallocene-based ethylene / octene copolymers include Affinity GA1900 (trade name), Affinity GA1950 (trade name), Affinity GA1875 (trade name), Affinity GA1000R (trade name), Affinity EG8185 (trade name), Affinity EG8200 (trade name), Engage 8137 (trade name), Engage 8180 (trade name), and Engage 8400 (trade name), all of which are manufactured by The Dow Chemical Company; Metallocene-based ethylene / hexene copolymers, for example, Nipolon ZHM510R manufactured by Tosoh Corporation and Excellen FX402 manufactured by Sumitomo Chemical Co., Ltd.; Examples of metallocene-based propylene homopolymers include Elmodu S400 and Elmodu S600 manufactured by Idemitsu Kosan Co., Ltd.

[0072] <(C) Tackifying resin> The hot melt adhesive of the present invention can improve the retention of the label on the container by including a tackifier resin (component (C)). The "tackifier resin" is a resin that is commonly used in hot melt adhesives, and is not particularly limited as long as it can provide the hot melt adhesive of the present invention. In this specification, component (C) does not include the compound explained as component (A) above.

[0073] The alkali dispersible hot melt adhesive of the present invention contains a tackifier resin (C), which results in excellent compatibility between the individual components, an improved balance between label retention and adhesive residue, increased shear strength at the adhesive joints between labels wrapped around the body, and excellent stringiness reduction, resulting in an overall well-balanced adhesive.

[0074] Examples of tackifying resins include natural rosin, modified rosin, hydrogenated rosin, glycerol ester of natural rosin, glycerol ester of modified rosin, pentaerythritol ester of natural rosin, pentaerythritol ester of modified rosin, pentaerythritol ester of hydrogenated rosin, copolymers of natural terpene, three-dimensional polymers of natural terpene, hydrogenated derivatives of hydrogenated terpene copolymers, polyterpene resins, hydrogenated derivatives of phenol-based modified terpene resins, aliphatic petroleum hydrocarbon resins, hydrogenated derivatives of aliphatic petroleum hydrocarbon resins, aromatic petroleum hydrocarbon resins, hydrogenated derivatives of aromatic petroleum hydrocarbon resins, cyclic aliphatic petroleum hydrocarbon resins, and hydrogenated derivatives of cyclic aliphatic petroleum hydrocarbon resins.

[0075] Of these, component (C) preferably contains a tackifier resin having an acid value of 0 to 300 mgKOH / g, more preferably contains a rosin-based tackifier resin having an acid value of 50 to 300 mgKOH / g, even more preferably contains a rosin-based tackifier resin having an acid value of 100 to 300 mgKOH / g, and most preferably contains a rosin-based tackifier resin having an acid value of 100 to 250 mgKOH / g. When the acid value is within this range, the alkali dispersibility of the hot melt adhesive of the present invention is further improved.

[0076] In one embodiment of the present invention, the tackifier resin (C) preferably contains an α-methylstyrene resin in addition to the rosin-based tackifier resin. The α-methylstyrene resin enhances the cohesiveness of the hot melt adhesive and improves removability and holding power. As the α-methylstyrene resin, for example, an α-methylstyrene homopolymer or a styrene / α-methylstyrene copolymer is used.

[0077] In one embodiment of the present invention, the α-methylstyrene resin as component (C) is preferably a styrene / α-methylstyrene copolymer. The α-methylstyrene resin preferably has a softening point (measured by the ring and ball method specified in JIS K2207) of 65°C to 160°C, more preferably 85°C to 160°C. Specific examples of commercially available products include Crystallex 3085 (trade name), Crystallex 3100 (trade name), Crystallex 1120 (trade name), Crystallex 5140 (trade name), Endix 155, Plastri 290 manufactured by Eastman Chemical Co., and FTR-2120 (trade name) manufactured by Mitsui Chemicals, Inc.

[0078] These tackifier resins can be used alone or in combination of two or more. As the tackifier resin, a liquid type tackifier resin can also be used as long as it is colorless to pale yellow, substantially odorless, and has good thermal stability.

[0079] <(D) Fatty acids and their derivatives> The hot melt pressure-sensitive adhesive of the present invention contains at least one selected from the group consisting of (D) fatty acids and their derivatives (component (D)). By containing component (D), the hot melt pressure-sensitive adhesive of the present invention has excellent alkali dispersibility. Component (D) may contain one type of compound alone or two or more types.

[0080] In this specification, fatty acid refers to an aliphatic carboxylic acid having at least one carboxy group, and may have a hydroxy group. Fatty acids are broadly classified into saturated fatty acids and unsaturated fatty acids. Saturated fatty acids are acids that do not have a double bond or triple bond in the carbon chain. Unsaturated fatty acids are acids that have a double bond or triple bond in the carbon chain.

[0081] The saturated fatty acid may be any fatty acid that does not adversely affect the hot melt pressure sensitive adhesive of the present invention, preferably having 1 to 30 carbon atoms, more preferably having 3 to 26 carbon atoms, more preferably having 8 to 24 carbon atoms, even more preferably having 12 to 22 carbon atoms, and even more preferably having 14 to 22 carbon atoms. The saturated fatty acid may be either chain-like or cyclic, and is preferably chain-like. The chain-like saturated fatty acid may be either linear or branched, and is preferably linear saturated fatty acid. Specific examples of the saturated fatty acid include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, lauric acid, tridecylic acid, myristic acid, palmitic acid, stearic acid, tricosylic acid, and 12-hydroxystearic acid.

[0082] The unsaturated fatty acid may be any that does not adversely affect the hot melt pressure sensitive adhesive of the present invention, and preferably has 3 to 26 carbon atoms, more preferably has 4 to 22 carbon atoms, and even more preferably has 14 to 22 carbon atoms.

[0083] The unsaturated fatty acid preferably has 1 to 6 unsaturated bonds between carbon atoms, more preferably 1 to 3, and most preferably 1 or 2.

[0084] Examples of unsaturated fatty acids include crotonic acid, oleic acid, linoleic acid, docosahexaenoic acid, linoleic acid, and ricinoleic acid.

[0085] In this specification, the fatty acid derivative refers to a compound obtained by substitution of the above-mentioned fatty acid or other chemical reaction. Examples of the fatty acid derivative include fats and oils, hardened oils, fatty acid amides, fatty acid alkyl esters, monoglycerides, diglycerides, sorbitan fatty acid esters, diglycerin fatty acid esters, etc., with fats and oils and hardened oils being preferred, and hardened oils being more preferred. The "fat and oil" is mainly composed of triglycerides (triacylglycerols), which are esters of fatty acids and glycerin.

[0086] The hot melt adhesive of the present invention may contain fats and oils generally used as edible or industrial fats and oils. The fats and oils may be liquid or solid at room temperature (about 20 to 26°C), preferably liquid at room temperature, and preferably vegetable oils. Examples of fats and oils include corn oil, soybean oil, epoxidized soybean oil, sesame oil, linseed oil, olive oil, lettuce oil, fish oil, butter, lard, castor oil, rapeseed oil, sunflower oil, rice oil, and cottonseed oil, and one type of fats and oils may be used alone, or two or more types may be used in combination.

[0087] "Hydrogenated oil" is oil that is liquid at room temperature and is solidified at room temperature by hydrogenating the oil and fat and increasing the proportion of saturated fatty acids with higher melting points. "Hydrogenated oil" may be any oil that does not adversely affect the hot melt adhesive of the present invention, and specific examples include hydrogenated castor oil (i.e., hydrogenated castor oil), hydrogenated soybean oil, hydrogenated salad oil, etc.

[0088] The hot melt pressure-sensitive adhesive of the present invention contains (D1) a fatty acid derivative having a melting point of 40°C or higher (also referred to as "component (D1)" or "(D1) fatty acid derivative") as (D) a fatty acid or derivative thereof. The melting point of (D1) the fatty acid derivative is preferably 45 to 120°C, more preferably 50 to 100°C, and even more preferably 50 to 90°C. In one embodiment of the present invention, the hot melt pressure-sensitive adhesive preferably contains castor oil having a melting point of 50 to 100°C. The component (D1) may contain one type alone or two or more types.

[0089] The hot melt adhesive of the present invention has improved holding power due to the melting point of the fatty acid derivative (D1) being in the above range, making it suitable as a hot melt adhesive for labels. When a label is bonded to a PET bottle for carbonated drinks via the hot melt adhesive of the present invention, even if the PET bottle expands due to carbon dioxide gas, the label is retained on the PET bottle for a long period of time without shifting or floating. Furthermore, the alkali dispersible hot melt adhesive of the present invention has excellent shear strength at the bonded portion between the labels wrapped around the body and also has improved stringiness reduction properties, making it an adhesive with excellent overall balance.

[0090] In this specification, the melting point refers to a value measured by differential scanning calorimetry (DSC). Specifically, 10 mg of a sample is weighed into an aluminum container using a DSC6220 (trade name) manufactured by SII Nano Technology Co., Ltd., and the temperature at the top of the melting peak is referred to as the melting point, measured at a heating rate of 5°C / min.

[0091] The content of component (D1) is preferably 40 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 60 parts by mass or more, relative to 100 parts by mass of the total amount of component (D). In one embodiment of the present invention, in addition to component (D1), the composition may contain (D2) a fatty acid derivative having a melting point of less than 40°C (preferably an oil or fat having a melting point of less than 40°C).

[0092] In the present invention, it is preferable that the fatty acid derivative (D1) contains a hardened oil. The melting point of the hardened oil as component (D1) is 40° C. or higher, preferably 50 to 100° C., and more preferably 50 to 90° C. By containing a hardened oil having a melting point of 40° C. or higher, the hot melt pressure-sensitive adhesive of the present invention remains solid without melting even at high temperatures, and the cohesive force with an adherend such as a label is improved, resulting in high holding power.

[0093] Examples of hardened oils include hydrogenated castor oil (i.e., hydrogenated castor oil), hydrogenated soybean oil, hydrogenated salad oil, hydrogenated rapeseed oil, hydrogenated palm oil, and beef tallow hardened oil. In particular, hydrogenated castor oil, hydrogenated soybean oil, and hydrogenated rapeseed oil are preferred, and hydrogenated castor oil is most preferred.

[0094] The hot melt pressure sensitive adhesive of the present invention has particularly excellent holding power when it contains hydrogenated castor oil having a melting point of 40° C. or higher. In one embodiment of the present invention, the hot melt pressure sensitive adhesive preferably contains hydrogenated castor oil having a melting point of 50 to 100° C. as component (D1).

[0095] In the present invention, as (D) the fatty acid or a derivative thereof, a commercially available product can be used.

[0096] (D1) Commercially available fatty acid derivatives include, for example, hydrogenated castor oil A (trade name), Technol MH (trade name), Technoroll ML98 (trade name), 12-hydroxystearic acid (trade name), hydrogenated soybean oil (trade name), hydrogenated rapeseed oil (trade name), hydrogenated palm oil (trade name), and rice wax SS-1 (trade name).

[0097] Examples of commercially available fatty acid derivatives other than component (D1) include: FS Oil (product name) and Prime Taste (product name) manufactured by Showa Sangyo Co., Ltd.; Rice oil (product name) and rice salad oil (product name) manufactured by Boso Oil Co., Ltd.; Cottonseed oil (product name) manufactured by Okamura Oil Co., Ltd. Rikemal (brand name) manufactured by Riken Vitamin Co., Ltd. Nonion (trade name) manufactured by NOF Corporation; and the like.

[0098] These commercially available fatty acid derivatives can be used alone or in combination.

[0099] The hot melt pressure sensitive adhesive of the present invention may contain a wax in addition to the components (A) to (D).

[0100] The "wax" is an organic substance that is solid at room temperature and becomes liquid when heated, and is a wax that is generally used in hot melt adhesives, and is not particularly limited as long as it can provide the hot melt adhesive of the present invention. Wax is generally a low polymer (i.e., an oligomer). In this specification, the wax is defined as a low polymer having a weight average molecular weight of less than 12,000. Specific examples of wax include synthetic waxes such as Fischer-Tropsch wax and polyolefin wax (polyethylene wax, polypropylene wax); petroleum waxes such as paraffin wax and microcrystalline wax; and natural waxes such as castor wax.

[0101] By including a wax in the hot melt adhesive of the present invention, when the label is peeled off from the container, less of the hot melt adhesive remains on the container.

[0102] In one embodiment of the present invention, the wax preferably comprises a Fischer-Tropsch wax, which is a wax fraction obtained by fractionating a wax having a narrow carbon number distribution from a wax having a relatively wide carbon number distribution in its component molecules. The Fischer-Tropsch wax reduces the adhesive residue of the hot melt adhesive when the label is peeled off from the container.

[0103] The hot melt pressure sensitive adhesive of the present invention may contain a plasticizer.

[0104] The plasticizer is blended for the purpose of reducing the melt viscosity of the hot melt pressure-sensitive adhesive, imparting flexibility, and improving wettability to the adherend, and is not particularly limited as long as it is compatible with other components and can provide the hot melt pressure-sensitive adhesive of the present invention. Examples of the plasticizer include paraffinic oil, naphthenic oil, and aromatic oil. In particular, paraffinic oil and / or naphthenic oil are preferred, and colorless, odorless paraffinic oil is most preferred.

[0105] Examples of commercially available plasticizers include White Oil Broom350 (trade name) manufactured by Kukdong Oil & Chem Co., Ltd., Diana Fresia S-32 (trade name), Diana Process Oil PW-90 (trade name), Daphne Oil KP-68 (trade name) manufactured by Idemitsu Kosan Co., Ltd., Enerper M1930 (trade name) manufactured by BP Chemicals Co., Ltd., Kaydol (trade name) manufactured by Crompton Co., Ltd., Primol 352 (trade name) manufactured by Exxon Corp., Process Oil NS-100 (trade name) manufactured by Idemitsu Kosan Co., Ltd., and DN4010 manufactured by PetroChina Co., Ltd. These can be used alone or in combination of two or more kinds.

[0106] The incorporation of a plasticizer improves the compatibility of the components (A) to (C) contained in the hot melt pressure-sensitive adhesive of the present invention, and also improves the compatibility with other components, resulting in improved tackiness, adhesion and coatability of the hot melt pressure-sensitive adhesive.

[0107] The hot melt pressure sensitive adhesive according to the present invention may further contain various additives, if necessary. Examples of such various additives include a stabilizer and a particulate filler.

[0108] The "stabilizer" is a compound that is blended to improve the stability of the hot melt pressure-sensitive adhesive by preventing the decrease in molecular weight, gelation, coloration, odor generation, etc., caused by heat, and is not particularly limited as long as it can provide the hot melt pressure-sensitive adhesive that is the object of the present invention. Examples of the "stabilizer" include antioxidants and ultraviolet absorbers.

[0109] Examples of the "antioxidant" include phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants. Examples of the "ultraviolet ray absorber" include benzotriazole-based ultraviolet ray absorbers and benzophenone-based ultraviolet ray absorbers. Furthermore, lactone-based stabilizers can also be added. These can be used alone or in combination. The following products can be used as commercially available antioxidants.

[0110] Specific examples include Sumilizer GM (trade name), Sumilizer TPD (trade name), and Sumilizer TPS (trade name) manufactured by Sumitomo Chemical Co., Ltd., Irganox 1010 (trade name), Irganox HP2225FF (trade name), Irgafos 168 (trade name), and Irganox 1520 (trade name), Tinuvin P, JF77 (trade name) manufactured by Johoku Chemical Co., Ltd., and Adeka STAB AO-60 (trade name) and Adeka STAB AO-412S (trade name) manufactured by ADEKA Corp. These stabilizers can be used alone or in combination.

[0111] The "ultraviolet absorber" is used to improve the light resistance of the hot melt adhesive. The "antioxidant" is used to prevent the hot melt adhesive from deteriorating due to oxidation.

[0112] The hot melt adhesive of the present invention may further contain a particulate filler. The particulate filler may be any commonly used one, and is not particularly limited as long as the hot melt adhesive of the present invention can be obtained. Examples of "particulate fillers" include mica, calcium carbonate, kaolin, talc, titanium oxide, diatomaceous earth, urea resin, styrene beads, calcined clay, starch, etc. The shape of these is preferably spherical, and the dimensions (diameter in the case of a spherical shape) are not particularly limited.

[0113] The hot melt adhesive of the present invention can be produced by blending components (A), (B), (C) and (D), preferably wax, a plasticizer and a stabilizer, and further various additives as necessary, using a commonly known method for producing a hot melt adhesive. The hot melt adhesive can be produced by blending the above-mentioned components in predetermined amounts and heating to melt them. As long as the desired hot melt adhesive can be obtained, the order of adding each component, the heating method, etc. are not particularly limited.

[0114] In the hot melt pressure sensitive adhesive of the present invention, the amount of component (A) is not particularly limited, but is preferably 10 to 30 parts by mass, more preferably 15 to 30 parts by mass, and even more preferably 15 to 25 parts by mass, per 100 parts by mass of the total mass of components (A), (B), (C) and (D).

[0115] By using the component (A) in the above range, the alkali dispersible hot melt pressure sensitive adhesive of the present invention has high cohesive strength, which makes it easier to attach the label to a container without shifting the label, and improves the shear strength of the adhesive portion between the labels wrapped around the body (e.g., between OPP films). Furthermore, the amount of the thermoplastic block copolymer (A) also contributes to reducing the stringiness of the hot melt pressure sensitive adhesive.

[0116] In the hot melt adhesive of the present invention, the amount of component (B) is not particularly limited, but is preferably 1 to 20 parts by mass, more preferably 3 to 15 parts by mass, and even more preferably 4 to 10 parts by mass, relative to 100 parts by mass of the total mass of components (A), (B), (C) and (D). By having the amount of component (B) within the above range, the hot melt adhesive of the present invention has an excellent balance between the retention power of the label and the adhesive residue. Furthermore, even if a labeled container having the hot melt adhesive of the present invention is transported for a long time, the film overlapping portion of the body-wrapped label is difficult to peel off from the container due to vibration during transportation, etc.

[0117] In the hot melt adhesive of the present invention, the amount of component (C) is not particularly limited, but is preferably 40 to 80 parts by mass, more preferably 50 to 75 parts by mass, and most preferably 60 to 71 parts by mass, relative to 100 parts by mass of the total mass of components (A), (B), (C) and (D). By having the amount of component (C) within the above range, the hot melt adhesive of the present invention becomes stable as an adhesive and has an excellent balance of holding power, reduced adhesive residue, and reduced stringiness. Furthermore, even if a labeled container having the hot melt adhesive of the present invention is transported for a long time, the film overlapping portion of the body-wrapped label becomes difficult to peel off from the container due to vibration during transportation, etc.

[0118] In the hot melt adhesive of the present invention, the amount of component (D) is not particularly limited, but is preferably 5 to 18 parts by mass, more preferably 7 to 15 parts by mass, and more preferably 9 to 13 parts by mass, based on 100 parts by mass of the total mass of components (A), (B), (C) and (D). By including component (D) in the above range, the hot melt adhesive of the present invention has improved alkali dispersibility, and while maintaining holding power, can reduce adhesive residue on the adherend when peeled off, which also contributes to reducing stringiness. Furthermore, even if a labeled container having the hot melt adhesive of the present invention is transported for a long time, the film overlapping portion of the body-wrapped label becomes difficult to peel off from the container due to vibration during transportation, etc.

[0119] In the hot melt pressure-sensitive adhesive of the present invention, the total content of components (A), (B), (C) and (D) relative to the total mass of the hot melt pressure-sensitive adhesive is not particularly limited, but is preferably 50 parts by mass or more, more preferably 60 to 85 parts by mass, and even more preferably 65 to 75 parts by mass.

[0120] In the hot melt pressure sensitive adhesive of the present invention, the amount of wax to be blended is not particularly limited and may be 0 part by mass relative to 100 parts by mass of the total mass of components (A), (B), (C) and (D), but is preferably 1 to 10 parts by mass, more preferably 2 to 8 parts by mass, and even more preferably 2.5 to 6 parts by mass.

[0121] In one embodiment of the present invention, the hot melt pressure sensitive adhesive preferably contains a Fischer-Tropsch wax. The amount of the Fischer-Tropsch wax relative to the total amount of wax is not particularly limited, but is preferably 50 mass% or more, more preferably 65 mass% or more, and may be 100 mass%.

[0122] In a preferred embodiment of the present invention, the hot melt pressure sensitive adhesive has a viscosity (or melt viscosity) at 160°C of preferably 4000 mPa·s or less, more preferably 3000 mPa·s or less, and even more preferably 2000 mPa·s or less. By having a viscosity at 160°C within the above range, the hot melt pressure sensitive adhesive becomes more suitable for coating. In this specification, the viscosity (or melt viscosity) at 160°C means a value measured with a Brookfield viscometer using a No. 27 rotor.

[0123] The label according to the present invention has a substrate and an adhesive layer made of the hot melt adhesive. Specific examples of the substrate include paper, processed paper (paper that has been subjected to aluminum deposition processing, aluminum lamination processing, varnishing processing, resin processing, etc.), synthetic paper, organic compound film, inorganic compound film, metal film, etc.

[0124] The substrate for the label is preferably an organic compound film such as polypropylene, polyethylene terephthalate (PET), polylactic acid (PLA), etc., which are often subjected to alkaline cleaning. As the polypropylene film, biaxially oriented polypropylene (OPP) film is particularly preferable.

[0125] The adhesive layer may be formed on the entire back surface of the label or on a part of the back surface of the label. For example, in the case of a body-wrapped label, an adhesive layer may be formed on the overlapping portions of both ends of the film that are adhered to each other when the film is wrapped around the body of a container.

[0126] The adhesive layer can be formed by applying a hot melt adhesive to the surface of the substrate. Coating methods include the open wheel method, the closed gun method, and the direct coat method. The open wheel method and the direct coat method are preferred because they do not leave any adhesive on the PET bottle when the label is removed.

[0127] The container according to the present invention has the above-mentioned label attached to its surface. Examples of such containers include glass containers such as glass bottles used for soft drinks, seasonings, detergents, shampoos, edible oils, cosmetics, medicines, etc.; plastic containers such as PET (polyethylene terephthalate) bottles; and metal cans such as aluminum cans. Of the above-mentioned containers, PET bottles are particularly preferred in the present invention. Examples of PET bottles to which the label of the present invention is attached include a PET bottle with a label attached to a part of the body of the bottle, and a bottle with a "body wrap label" wrapped around the body of the bottle, which is attached to the bottle in a circumferential manner, as one embodiment of the present invention. The hot melt adhesive of the present invention has excellent holding power, so that even if the container expands due to the fact that the container, such as a PET bottle, is filled with a carbonated drink, the label can be prevented from shifting or floating.

[0128] The hot melt adhesive of the present invention is preferably used for adhesion of a body-wrapped label. A biaxially oriented polypropylene (OPP) film may be used as the base material of the body-wrapped label. The label to which the hot melt adhesive of the present invention is applied may or may not be printed. When a printed label is used, the hot melt adhesive of the present invention may be applied not only to the unprinted side but also to the printed side.

[0129] An example of a type of device for attaching a label to a PET bottle using the hot melt adhesive of the present invention is an open wheel type device. With the open wheel type device, the hot melt adhesive is melted at 120 to 190°C and applied to the back side of the label. This label is attached to a PET bottle to produce the container of the present invention.

[0130] A container with a label attached with the hot melt adhesive of the present invention is easily peeled off from the container when immersed in a hot alkaline solution, making the container suitable for reuse, etc. The method for peeling off the label with a hot alkaline solution is not particularly limited, but an example of the method is to cut a labeled container into small pieces to form pellets, place the pellets in a hot alkaline aqueous solution (e.g., a sodium hydroxide aqueous solution having a temperature of 80°C to 90°C and a concentration of 0.5 to 5.0% by mass) and stir for about 1 to 20 minutes.

[0131] In addition, containers to which a label has been affixed using the hot melt adhesive of the present invention have sufficient adhesion so that the label does not peel off from the container during normal use, and when the label is to be removed after use of the container, for example, it can be peeled off by hand without leaving any glue residue, and has excellent removability.

[0132] Furthermore, even if this labeled container is transported for a long period of time, the overlapping film portion of the body-wrapped label will not peel off from the container due to vibrations or the like during transport. EXAMPLES

[0133] EXAMPLES Hereinafter, the present invention will be described in more detail and specifically with reference to examples, but these examples are not intended to limit the present invention in any way.

[0134] In the examples and comparative examples, the components blended in the hot melt pressure sensitive adhesive are shown below.

[0135] (A) Thermoplastic block copolymer (A1) A styrene-based block copolymer having a styrene content of less than 40% by mass (A1-1) Styrene-ethylene / butylene-styrene triblock copolymer (Kraton G-1652 (trade name) manufactured by Kraton Corporation, styrene content 30% by mass, diblock content 0% by mass, weight average molecular weight 72,000) (A1-2) Styrene-ethylene / butylene-styrene triblock copolymer (Kraton G-1650 (trade name) manufactured by Kraton Corporation, styrene content 30% by mass, diblock content 0% by mass, weight average molecular weight 92,000) (A1-3) Styrene-ethylene / butylene-styrene block copolymer (Kraton G-1726 (trade name) manufactured by Kraton Corporation, styrene content 31% by mass, diblock content 73% by mass, weight average molecular weight 43,000) (A1-4) Styrene-ethylene / butylene-styrene block copolymer (Kraton G-1657 (trade name) manufactured by Kraton Corporation, styrene content 15% by mass, diblock content 33% by mass, weight average molecular weight 106,000)

[0136] (A2) A styrene-based block copolymer having a styrene content of 40% by mass or more (A2-1) Styrene-ethylene / butylene-styrene triblock copolymer (Tuftec H1043 (product name) manufactured by Asahi Kasei Chemicals Corporation, styrene content 68% by mass, diblock content 0% by mass, weight average molecular weight 53,000) (A2-2) Styrene-butadiene / butylene-styrene triblock copolymer (Tuftec P2000 (trade name) manufactured by Asahi Kasei Chemicals Corporation, styrene content 68% by mass, diblock content 0% by mass, weight average molecular weight 54,000) (A2-3) Styrene-butadiene-styrene block copolymer (Asahi Kasei Chemicals Corporation's Asaprene T-439 (trade name), styrene content 46% by mass, diblock content 69% by mass, weight average molecular weight 63,000) (A2-4) Styrene-isoprene-styrene triblock copolymer (Kraton D-1162P (trade name) manufactured by Kraton Corporation, styrene content 41% by mass, diblock content 0% by mass, weight average molecular weight 82,000)

[0137] (B) Metallocene-based olefin polymer (B1) Metallocene-based ethylene / propylene copolymer (Vistamax 8780 (trade name) manufactured by Exxon Mobil Corporation, weight average molecular weight: 30,000, ethylene content: 12% by mass) (B2) Metallocene-based ethylene / propylene copolymer (Vistamax 8880 (trade name) manufactured by ExxonMobil Corporation, weight average molecular weight: 25,000, ethylene content: 6.0 mass%, melting point: 97°C, melt viscosity at 190°C: 1200 mPa·s) (B3) Metallocene-based ethylene / propylene copolymer (Affinity GP1570 (trade name) manufactured by Dow Chemical Company, weight average molecular weight: 35,000, melt viscosity at 177°C: 12,500 mPa·s,) (B4) Metallocene-based ethylene / octene copolymer (Affinity GA1900 (trade name) manufactured by Dow Chemical Company, weight average molecular weight: 30,000, 1-octene content: 35 to 37 mass%, melt flow rate: 1000 g / 10 min) (B5) Metallocene-based ethylene / octene copolymer (Engage 8137 (trade name) manufactured by Dow Chemical Company, weight average molecular weight: 200,000, 1-octene content: 13% by weight, melt flow rate: 13 g / 10 min) (B6) Metallocene-based ethylene / octene copolymer (Infuse 9808 (trade name) manufactured by The Dow Chemical Company, weight average molecular weight: 200,000, melt flow rate: 15 g / 10 min) (B7) Metallocene-based ethylene / hexene copolymer (Kernel KJ604T (product name) manufactured by Japan Polyethylene Co., Ltd., weight average molecular weight: 130,000, melt flow rate: 30 g / 10 min, melting point: 58° C.) (B8) Metallocene-based propylene homopolymer (Elmodu S400 (trade name) manufactured by Idemitsu Kosan Co., Ltd., weight average molecular weight 450,000, melting point 75°C, polydispersity index 2.0) (B9) Metallocene-based propylene homopolymer (Elmodu S600 (trade name) manufactured by Idemitsu Kosan Co., Ltd.), Heavy Weight average molecular weight: 70,000 Melting point: 80°C Polydispersity: 2.0 (B10) Metallocene-based ethylene / 1-butene copolymer (Tafmer DF7350 (trade name) manufactured by Mitsui Chemicals, Inc., weight average molecular weight: 120,000, melt flow rate: 35 g / 10 min, melting point: 55° C.)

[0138] (B'11) Ziegler-Natta propylene homopolymer (Eastflex P1010PL (trade name) manufactured by Eastman Chemical Co., weight average molecular weight: 260,000, melt viscosity at 190°C: 1000 mPa s, softening point: 155°C, density: 0.87 g / cm 3 ) (B'12) Ziegler-Natta ethylene / propylene copolymer (Eastman Chemical Company's Eastflex E1016 (trade name), weight average molecular weight: 380,000) (B'13) Ziegler-Natta ethylene / propylene / butene copolymer (Bestplast 708 (trade name) manufactured by Evonik, weight average molecular weight: 78,000, melt flow rate: 450 g / 10 min, melting point: 124°C, melt viscosity at 190°C: 2700 mPa·s)

[0139] (C) Tackifying resin (C1) Hydrogenated alicyclic / aromatic copolymer hydrocarbon resin (T-REZ HC103 (product name) manufactured by ENEOS Corporation, softening point 103°C) (C2) Hydrogenated alicyclic hydrocarbon resin (T-REZ HA103 (product name) manufactured by ENEOS Corporation, softening point 103°C) (C3) Hydrogenated alicyclic hydrocarbon resin (T-REZ HA125 (product name) manufactured by ENEOS Corporation, softening point 125°C) (C4) Hydrogenated rosin ester (KOMOTAC KHR75 (trade name) manufactured by GUANGDONG KOMO Co., Ltd., acid value 170 mg KOH / g, softening point 80°C) (C5) Hydrogenated rosin ester (ForalAX-E (trade name) manufactured by Eastman Chemical Company, acid value 160 mg KOH / g, softening point 80°C) (C6) Water-added rosin ester (Foral 85E (trade name) manufactured by Eastman Chemical Company, acid value 9 mg KOH / g, softening point 85°C) (C7) Rosin ester (KOMOTAC K107 (trade name) manufactured by GUANGDONG KOMO Co., Ltd., acid value 155 mg KOH / g, softening point 80°C) (C8) Rosin ester (KOMOTAC KB90H (product name) manufactured by GUANGDONG KOMO Co., Ltd., acid value 15 mg KOH / g, softening point 90°C) (C9) α-methylstyrene resin (Crystalex 3070 (trade name) manufactured by Eastman Chemical Company, softening point 70°C) (C10) α-methylstyrene resin (Crystalex 3085 (trade name) manufactured by Eastman Chemical Company, softening point 85°C) (C11) α-methylstyrene resin (Crystalex 3100 (trade name) manufactured by Eastman Chemical Company, softening point 100°C)

[0140] (D) at least one selected from the group consisting of fatty acids and derivatives thereof (D1) Fatty acid derivatives with a melting point of 40°C or higher (D1-1) Castor hydrogenated oil (castor hydrogenated oil A (trade name) manufactured by Ito Oil Mills, melting point 85.5°C) (D1-2) Monohydroxystearic acid hydrogenated castor oil (Technol MH (trade name) manufactured by Yokoseki Oils and Fat Co., Ltd., melting point 58.0°C) (D1-3) Hydrogenated castor oil with lauric acid (Technol ML98 (trade name) manufactured by Yokoseki Oils and Fat Co., Ltd., melting point 51.0°C) (D1-4) Castor hydrogenated fatty acid (NOF Corporation's 12-hydroxystearic acid (trade name), melting point 69.0°C) (D1-5) Beef tallow hardened oil (51° beef tallow hardened oil HO (trade name) manufactured by NOF Corp., melting point 51.0° C.) (D1-6) Extremely hardened soybean oil (Hydrogenated soybean oil (product name) manufactured by Yamakei Sangyo Co., Ltd., melting point 68.2°C) (D1-7) Rice wax rapeseed hardened oil (Rice wax SS-1 (trade name) manufactured by BOSO Oil & Fat Co., Ltd., melting point 79.0°C)

[0141] (D2) Fatty acid derivatives with a melting point of less than 40°C (D2-1) Castor oil (Toyokuni Oil Mill's industrial No. 1 castor oil (product name), no melting point (freezing point -22°C) (D2-2) Rice oil (Rice salad oil (product name) made by BOSO Oil & Fat, no melting point (freezing point -10 to -5°C)) (D2-3) Sunflower oil (High Oleic Sunflower Oil (product name) manufactured by Yamakei Sangyo Co., Ltd., no melting point (freezing point -18 to -16°C))

[0142] (E) Wax (E1) Fischer-Tropsch wax (Sasol C80 (trade name) manufactured by Sasol, weight average molecular weight: 620, melting point 80°C, penetration 7) (E2) Fischer-Tropsch wax (Sasol H1 (trade name) manufactured by Sasol, weight average molecular weight: 880, melting point 108°C, penetration 2) (E3) Ethylene-vinyl acetate copolymer wax (AC400 (trade name) manufactured by Honeywell, weight average molecular weight: 400, melting point 92°C) (E4) Polyethylene wax (Hiwax 320P (product name) manufactured by Mitsui Chemicals, Inc., weight average molecular weight: 3000, melting point 109°C, penetration 7) (E5) Polypropylene wax: Hiwax NP105 (trade name) manufactured by Mitsui Chemicals, Inc., weight average molecular weight: 10,000, melting point 140 / 148°C, penetration 1) (E6) Paraffin wax (Paraffin wax 150F (product name) manufactured by Nippon Seiro Co., Ltd., weight average molecular weight: 400, melting point 66°C, needle penetration 12) (E7) Maleic anhydride modified polypropylene wax (Licosene PPMA6252 (trade name) manufactured by Clariant, weight average molecular weight: 4000, melting point 140°C)

[0143] (F) Plasticizer (oil) (F1) Paraffin oil (Daphne Oil KP-68 (product name) manufactured by Idemitsu Kosan Co., Ltd.) (F2) Paraffin oil (Diana Process Oil PW90 (product name) manufactured by Idemitsu Kosan Co., Ltd.) (F3) Polybutene (Nippon Oil Polybutene HV-300 (product name) manufactured by Nippon Oil Corporation) (F4) Naphthenic oil (DN4010 (product name) manufactured by PetroChina)

[0144] (G) Stabilizers (antioxidants) (G1) Hindered phenol-based antioxidant (Adeka STAB AO-60 (product name) manufactured by Adeka Corporation) (G2) Phosphorus-based antioxidant (Irgafos 168 (product name) manufactured by BASF Japan)

[0145] Components (A) to (G) were blended in the blending ratios shown in Tables 1 and 2, and melt-mixed using a universal mixer at about 145°C for about 3 hours to produce the hot melt pressure sensitive adhesives of Examples 1 to 16 and Comparative Examples 1 to 4. All numerical values ​​relating to the compositions (blends) of the hot melt pressure sensitive adhesives shown in Table 1 are in parts by mass.

[0146] The hot melt adhesives of the Examples and Comparative Examples were evaluated for alkali dispersibility, holding power, adhesive residue, stringiness, and shear strength of the adhesive portion between the labels wrapped around the body. The measurement and evaluation methods are described below.

[0147] <Alkaline dispersibility> The hot melt adhesive of each Example and Comparative Example was applied to an OPP film to a thickness of 20 to 25 μm, and a label (25 mm × 50 mm) of the OPP film with the hot melt adhesive was prepared. This label was pressed against an empty PET bottle at 100 ° C for 5 seconds to adhere to the bottle, and a test sample was prepared. The mass of this test sample (mass of the test sample before cleaning) was measured, and the test sample was placed in a 1.5 mass % sodium hydroxide aqueous solution at 85 ° C and stirred (cleaned) for 15 minutes. After 15 minutes, the test sample was taken out and thoroughly air-dried. The mass of the test sample after air drying (mass of the test sample after cleaning) was measured, and the alkali dispersion ratio was calculated from the mass before and after cleaning. The alkali dispersion ratio was calculated from the following formula, and the alkali dispersibility was evaluated from the calculated value.

[0148] Alkali dispersion rate (%) = {(mass of test sample before cleaning - mass of test sample after cleaning) / (mass of hot melt adhesive used)} x 100

[0149] The evaluation results are shown in Table 3. The evaluation criteria are as follows. ◎: Alkaline dispersion rate is higher than 90% ○: Alkaline dispersion rate is 60% or more and 90% or less ×: Alkaline dispersion rate is less than 60%, or the film does not adhere and a test sample cannot be prepared, so measurement is not possible.

[0150] <Retention power (label floating and shifting when PET bottle expands)> A hot melt adhesive was applied to an OPP film to a thickness of 20 to 25 μm to prepare an OPP label (25 mm × 50 mm) with hot melt adhesive. The label was then pressed against an empty PET bottle at 100°C for 5 seconds to adhere the label to a test sample.

[0151] The PET bottles were then filled with carbonated beverages, and the test samples containing the carbonated beverages were stored for one week in an atmosphere at 40°C. Another test sample containing a carbonated beverage was also stored for three days in an atmosphere at -10°C, and the label lifting and label misalignment of each test sample were checked.

[0152] The evaluation results are shown in Table 3. The evaluation criteria are as follows. ◎: No label lift, label misalignment less than 2mm Good: No label lifting, label misalignment is 2mm or more, less than 4mm △: No label lifting, label misalignment between 4mm and 7mm ×: Label is floating or the label is misaligned by 7mm or more

[0153] <Glue residue> A hot melt adhesive was applied to an OPP film to a thickness of 20 to 25 μm to prepare an OPP label (25 mm x 50 mm) with hot melt adhesive. The label was pressed against an empty PET bottle at 100°C for 5 seconds to adhere to the bottle, preparing a test sample. After storing the test sample at 0°C for 7 days, the label was peeled off the bottle by hand, and the state of adhesion of the hot melt adhesive to the bottle was visually confirmed. Another test sample containing a carbonated drink was also stored in an atmosphere at 40°C for 7 days, the label was peeled off the bottle by hand, and the state of adhesion of the hot melt adhesive to the bottle was visually confirmed.

[0154] The evaluation results are shown in Table 3. The evaluation criteria are as follows. ◎: The interface was peeled off, and the hot melt adhesive was not adhered. Good: A small amount of hot melt adhesive attached. ×: Cohesive failure, most of the hot melt adhesive remains in the PET bottle.

[0155] <Stringiness> The hot melt adhesive was intermittently applied vertically to the adherend 20 cm away from the tip of the hot melt gun. The state of the fallen matter between the hot melt gun and the adherend was visually observed and the stringiness was evaluated. The measurement conditions were as follows:

[0156] Temperature settings: Tank temperature, hose temperature, and nozzle temperature are all 160°C. Nozzle diameter: 14 / 1000 inch Nozzle: Single nozzle Dispensing pressure: 0.3MPa Number of coating shots: 90 shots / 3 minutes

[0157] The evaluation results are shown in Table 3. The evaluation criteria are as follows. ○: The object falls away from the nozzle (no stringing). ×: Falling objects adhere to the area around the nozzle (stringing occurs).

[0158] <Shear strength of the adhesive part between the labels wrapped around the body (OPP / OPP)> The hot melt adhesive was applied to an OPP film to a thickness of 20 to 25 μm, and the OPP film was then cut to 25 mm × 50 mm. Another OPP film was then placed on top so that the adhesive surface was 25 mm × 25 mm, and the film was pressed at 100°C for 3 seconds to bond the films together, producing a sample.

[0159] After storing the film for 1 day under a 23°C, 55% humidity atmosphere, a tensile test was carried out on the film in the shear direction to measure the shear strength.

[0160] The evaluation results are shown in Table 3. The evaluation criteria are as follows. ◎: Shear strength is 10kg / cm 2 Greater than 〇: Shear strength is 5kg / cm 2 More than 10kg / cm 2 below △: Shear strength is 3kg / cm 2 More than 5kg / cm 2 below ×: Shear strength is 3kg / cm 2 Less than

[0161] [Table 1]

[0162] [Table 2]

[0163] [Table 3]

[0164] As shown in Tables 1 and 2, the alkali-dispersible hot melt adhesives of Examples 1 to 16 had excellent alkali dispersibility and holding power, reduced glue residue and stringiness, and improved the shear strength of the adhesive joints between the labels wrapped around the body, and all other performance characteristics were excellent.

[0165] On the other hand, the hot melt pressure sensitive adhesives of Comparative Examples 1 to 4 all had a rating of x for the shear strength of the adhesive portion between the labels wrapped around the body, and also had a rating of x for all other performance properties.

[0166] These results confirm that the hot melt adhesive containing components (A), (B), (C), and (D) has high alkali dispersibility, excellent label retention, little glue residue, reduced stringiness, and excellent shear strength at the adhesive joints between labels wrapped around the body. [Industrial Applicability]

[0167] The present invention can provide an alkali dispersible hot melt adhesive, a label coated with the hot melt adhesive, and a container with the label affixed thereto.

Claims

1. (A) a thermoplastic block copolymer which is a copolymer of a vinyl aromatic hydrocarbon and a conjugated diene compound; (B) a metallocene-based olefin polymer, (C) a tackifier resin, and (D) at least one selected from the group consisting of fatty acids and derivatives thereof; Alkaline dispersible hot melt adhesive.

2. 2. The alkali dispersible hot melt pressure sensitive adhesive according to claim 1, comprising 1 to 20 parts by mass of the metallocene olefin polymer (B) per 100 parts by weight of the total weight of the components (A) to (D).

3. The alkali dispersible hot melt pressure sensitive adhesive according to claim 1 or 2, wherein the metallocene olefin polymer (B) has a weight average molecular weight of 12,000 or more.

4. A label having an adhesive layer comprising the alkali dispersible hot melt adhesive according to claim 1.

5. A container having the label of claim 4 attached thereto.

Citation Information

Patent Citations

  • Alkali dispersion type hot-melt adhesive

    JP2014159563A

  • Hot-melt adhesive and plastic label with hot-melt adhesive

    JP2016204588A

  • Alkali dispersion type hot-melt adhesive

    JP2021095443A

  • Alkali dispersion type hot-melt adhesive

    JP2021095448A