Method for manufacturing connection structure and connection structure

By employing film-like solder connection materials with precise dimensions and a reflow oven process, the method addresses inefficiencies in solder placement between terminal rows, achieving high continuity reliability in surface mount device connections.

JP2024169309APending Publication Date: 2024-12-05DEXERIALS CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024050937
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-03-27
Publication Date
2024-12-05

AI Technical Summary

Technical Problem

Existing methods for mounting surface mount devices on rigid or flexible boards face challenges in efficiently placing solder particles between terminal rows, leading to short circuits and reduced continuity reliability.

Method used

A method involving the use of film-like solder connection materials with specific dimensions and arrangements to align and bond surface mount components, ensuring the relative standard deviation of solder thickness between terminals is less than 25%, and utilizing a reflow oven without mechanical load to achieve self-alignment and high continuity reliability.

Benefits of technology

The method efficiently aggregates solder particles onto electrodes, reducing variations in solder thickness and preventing short circuits, thereby enhancing continuity reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024169309000001_ABST
    Figure 2024169309000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a connection structure that efficiently arranges solder particles on an electrode and that can obtain high electrical conductivity reliability, and the connection structure.SOLUTION: A method includes a placement step of placing a surface mount component having a plurality of terminal rows on a wiring board via a film-like solder connection material having a rectangular portion corresponding to each terminal row, and a joining step of joining the surface mount component to the wiring board. The relative standard deviation of the solder thickness between the terminals of the surface mount component and terminals of the wiring board after the joining step is less than 25%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present technology relates to a manufacturing method of a connection structure for connecting, for example, surface mount components by using solder particles, and to the connection structure. [Background technology]

[0002] Mounting of surface mount devices (SMDs) onto rigid or flexible boards is generally performed by printing or temporarily attaching a solder paste or film to the board, placing the surface mount devices on top of it, and then performing a reflow process (see, for example, Patent Documents 1 to 3).

[0003] In the techniques described in Patent Documents 1 to 3, when a surface mount component having multiple terminal rows is mounted, some of the solder particles tend to be disposed between the terminal rows, making it difficult to efficiently dispose the solder particles on the electrodes (lines). This can cause short circuits (bridges) between adjacent terminals, making it difficult to obtain high electrical reliability. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2017-041442 A [Patent Document 2] JP 2016-219808 A [Patent Document 3] International Publication No. 2008 / 023452 Summary of the Invention [Problem to be solved by the invention]

[0005] The present technology is devised to solve the above-mentioned problems, and provides a method for manufacturing a connection structure that allows solder particles to be efficiently moved onto an electrode and high conductivity reliability to be obtained, and a connection structure. [Means for solving the problem]

[0006] As a result of intensive research, the present inventors have found that the following manufacturing method for a connection structure and the following connection structure can achieve the above object, and have completed the present technology.

[0007] [1] a placement step of placing a surface mount component having a plurality of terminal rows on a wiring board via a film-like solder connection material having rectangular portions corresponding to each of the terminal rows; a bonding step of bonding the surface mount component to the wiring board; A method for manufacturing a connection structure having the above structure. [2] The method for manufacturing a connection structure according to [1], wherein a relative standard deviation of the solder thickness between the terminal of the surface mount component and the terminal of the wiring board after the joining step is less than 25%. [3] the surface mount component includes a first terminal row and a second terminal row arranged in parallel; The method for manufacturing a connection structure according to [1] or [2], wherein in the placing process, a first film-like solder connecting material corresponding to the first terminal row and a second film-like solder connecting material corresponding to the second terminal row are placed, and the distance between the rectangular portion in the first film-like solder connecting material and the rectangular portion in the second film-like solder connecting material is set to 0 mm or more. [4] the surface mount component includes a first terminal row and a second terminal row arranged in parallel; The method for manufacturing a connection structure described in [3], wherein, in the arrangement process, the width W of the rectangular portion in the first film-shaped solder connection material and the width W of the rectangular portion in the second film-shaped solder connection material satisfy the following formula (1): W≦(2L+S) / 2 (1) In the above formula (1), L is the length of the terminals in the first terminal row and the second terminal row, and S is the distance between the first terminal row and the second terminal row. [5] The method for manufacturing a connection structure according to [1] or [2], wherein in the joining step, the surface mount component is joined to the wiring board without load using a reflow furnace. [6] The method for manufacturing a connection structure according to [1] or [2], wherein the pitch of the terminal rows of the surface mount component and the wiring board is 0.1 mm to 0.4 mm. [7] The method for manufacturing a connection structure according to [1] or [2], wherein the content of solder particles in the film-like solder connection material is 10 volume % to 60 volume % for a terminal row pitch of 0.1 mm to 0.4 mm of the surface mount component and the wiring board. [8] the surface mount component includes a first terminal row and a second terminal row arranged in parallel; In the arranging step, a first film-like solder connecting material corresponding to the first terminal row and a second film-like solder connecting material corresponding to the second terminal row are arranged, The method for manufacturing a connection structure according to [1] or [2], wherein a widthwise protrusion amount of the rectangular portion of the first film-like solder connection material relative to the first terminal row is 50% or less of the terminal length of the first terminal row, and a widthwise protrusion amount of the rectangular portion of the second film-like solder connection material relative to the second terminal row is 50% or less of the terminal length of the second terminal row. [9] the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and a third terminal row and a fourth terminal row arranged in parallel and perpendicular to the first terminal row and the second terminal row, The method for manufacturing a connection structure according to [1] or [2], wherein a widthwise protrusion amount of a rectangular portion corresponding to the first terminal row, the second terminal row, the third terminal row or the fourth terminal row from the terminal row is 50% or less of a terminal length of the corresponding first terminal row, the second terminal row, the third terminal row or the fourth terminal row.

[10] A connection structure comprising: a surface mount component having a plurality of terminal rows; a wiring board; and a cured film of a film-like solder connecting material provided for each of the terminal rows, joining the surface mount component and the wiring board, the film having a rectangular portion corresponding to each of the terminal rows.

[11] The connection structure according to

[10] , wherein the relative standard deviation of the solder thickness between the terminal of the surface mount component and the terminal of the wiring board is less than 25%.

[12] The connection structure according to

[10] or

[11] , wherein the pitch of the terminal rows of the surface mount component and the wiring board is 0.1 mm to 0.4 mm.

[13] the surface mount component includes a first terminal row and a second terminal row arranged in parallel; The connection structure according to

[10] or

[11] , wherein the widthwise protrusion amount of the rectangular portion of the first film-like solder connection material relative to the first terminal row is 50% or less of the terminal length of the first terminal row, and the widthwise protrusion amount of the rectangular portion of the second film-like solder connection material relative to the second terminal row is 50% or less of the terminal length of the second terminal row.

[14] the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and a third terminal row and a fourth terminal row arranged in parallel and perpendicular to the first terminal row and the second terminal row, The connection structure according to

[10] or

[11] , wherein a widthwise protrusion amount of a rectangular portion corresponding to the first terminal row, the second terminal row, the third terminal row or the fourth terminal row from the terminal row is 50% or less of a terminal length of the corresponding first terminal row, the second terminal row, the third terminal row or the fourth terminal row. Effect of the Invention

[0008] According to this technique, it is possible to efficiently move solder particles onto the electrodes, thereby obtaining high electrical conductivity reliability. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a plan view that shows a schematic state in which solder connection films are provided on a first terminal row and a second terminal row that are parallel to each other on a wiring board. [Diagram 2] FIG. 2 is a cross-sectional view that illustrates a state in which a solder connection film is provided on a first terminal row of a wiring board. [Diagram 3] FIG. 3 is a cross-sectional view that illustrates a state in which the first terminal row of the wiring board and the first terminal row of the surface mount component are aligned. [Figure 4] FIG. 4 is a cross-sectional view that typically shows a state in which the wiring board and the surface-mounted components are heated in a reflow furnace. [Diagram 5] FIG. 5 is a plan view illustrating an example of a wiring board. [Figure 6] FIG. 6(A) is a plan view showing a schematic example of a metal mask as an embodiment, and FIG. 6(B) is a plan view showing a schematic example of a solder paste film printed using the metal mask shown in FIG. 6(A). [Figure 7] FIG. 7(A) is a plan view showing a schematic example of a metal mask as a comparative example, and FIG. 7(B) is a plan view showing a schematic example of a solder paste film printed using the metal mask shown in FIG. 7(A). [Figure 8] FIG. 8(A) is a plan view showing a schematic example of a metal mask as a comparative example, and FIG. 8(B) is a plan view showing a schematic example of a solder paste film printed using the metal mask shown in FIG. 8(A). [Figure 9] FIG. 9 is a cross-sectional view showing an example of a plug and a receptacle in a vertical fitting type connector in the short side direction. [Figure 10] FIG. 10 is a cross-sectional view showing a schematic longitudinal direction of a connection structure in which a plug of a connector and a wiring board are connected. [Figure 11] FIG. 11 is a cross-sectional view that illustrates a schematic view in the short-side direction of a connection structure in which a plug of a connector and a wiring board are connected. [Figure 12] FIG. 12(A) is a photograph showing the state in which a solder connection film is temporarily attached to a printed wiring board for Example 1, FIG. 12(B) is a photograph showing the state in which a connector is mounted on a printed circuit board for Example 1, and FIG. 12(C) is an X-ray photograph showing the connection structure after reflow for Example 1. [Figure 13]FIG. 13(A) is a photograph showing the state in which a solder connection film has been temporarily attached to a printed wiring board for Comparative Example 1, FIG. 13(B) is a photograph showing the state in which a connector has been mounted on a printed circuit board for Comparative Example 1, and FIG. 13(C) is an X-ray photograph showing the connection structure after reflow for Comparative Example 1. [Figure 14] FIG. 14 is a photograph showing the sample of Example 13 after reflow. [Figure 15] FIG. 15 is a photograph showing the sample of Comparative Example 6 after reflow. [Figure 16] FIG. 16 is an X-ray photograph showing the sample of Example 15 after reflow. [Figure 17] FIG. 17 is an X-ray photograph showing the sample of Comparative Example 8 after reflow. [Figure 18] Figure 18(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape is temporarily attached to a wiring board for a plug connector as comparison example 9, Figure 18(A2) is a plan view showing a schematic shape of the anisotropic conductive film, Figure 18(B) is a photograph showing the state in which a plug connector is reflow-mounted on the wiring board for a plug connector, and Figure 18(C) is an X-ray photograph showing the plug connector structure after mounting. [Figure 19] Figure 19(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a plug connector as Example 16, Figure 19(A2) is a plan view showing a schematic view of the shape of the anisotropic conductive film, Figure 19(B) is a photograph showing the state in which a plug connector has been reflow-mounted on a wiring board for a plug connector, and Figure 19(C) is an X-ray photograph showing the plug connector structure after mounting. [Figure 20]Figure 20(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a plug connector as Example 17, Figure 20(A2) is a plan view showing a schematic shape of the anisotropic conductive film, Figure 20(B) is a photograph showing the state in which a plug connector has been reflow-mounted on a wiring board for a plug connector, and Figure 20(C) is an X-ray photograph showing the plug connector structure after mounting. [Figure 21] Figure 21(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a plug connector as Example 18, Figure 21(A2) is a plan view showing a schematic shape of the anisotropic conductive film, Figure 21(B) is a photograph showing the state in which a plug connector has been reflow-mounted on the wiring board for a plug connector, and Figure 21(C) is an X-ray photograph showing the plug connector structure after mounting. [Figure 22] Figure 22(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a receptacle connector as comparison example 10, Figure 22(A2) is a plan view showing a schematic view of the shape of the anisotropic conductive film, Figure 22(B) is a photograph showing the state in which a receptacle connector has been reflow-mounted on the wiring board for a receptacle connector, and Figure 22(C) is an X-ray photograph showing the receptacle connector structure after mounting. [Figure 23] Figure 23(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a receptacle connector as Example 19, Figure 23(A2) is a plan view showing a schematic view of the shape of the anisotropic conductive film, Figure 23(B) is a photograph showing the state in which a receptacle connector has been reflow-mounted on the wiring board for a receptacle connector, and Figure 23(C) is an X-ray photograph showing the receptacle connector structure after mounting. [Figure 24]Figure 24(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a receptacle connector as Example 20, Figure 24(A2) is a plan view showing a schematic view of the shape of the anisotropic conductive film, Figure 24(B) is a photograph showing the state in which a receptacle connector has been reflow-mounted on the wiring board for a receptacle connector, and Figure 24(C) is an X-ray photograph showing the receptacle connector structure after mounting. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present technology will be described in detail with reference to the drawings in the following order. 1. Method for manufacturing connection structure and connection structure 2. Solder connection film 3. First Example 4. Second Example 5. Third Example 6. Fourth Example

[0011] <1. Method for producing connection structure and connection structure> The method for manufacturing a connection structure according to the present embodiment includes an arrangement step of arranging a surface mount component having a plurality of terminal rows on a wiring board via a film-like solder connection material having a rectangular portion whose longitudinal direction is the row direction of the terminal rows, and a joining step of joining the surface mount component to the wiring board. Here, when the surface mount component has a first terminal row and a second terminal row arranged in parallel, it is preferable that the protrusion amount of the solder connection film of the first terminal row or the second terminal row arranged between the first terminal row and the second terminal row is 50% or less of the terminal length in a direction perpendicular to the row direction of the first terminal row or the second terminal row. In addition, when the surface mount component includes a first terminal row and a second terminal row arranged in parallel, and a third terminal row and a fourth terminal row arranged in parallel and perpendicular to the first terminal row and the second terminal row, the protruding amount of the solder connection film of the first terminal row, the second terminal row, the third terminal row, or the fourth terminal row arranged between the first terminal row and the second terminal row is preferably 50% or less of the terminal length in the direction perpendicular to the row direction of the first terminal row, the second terminal row, the third terminal row, or the fourth terminal row. This makes it possible to prevent solder particles from remaining between the first terminal row and the second terminal row without agglomerating.

[0012] The connection structure according to the present embodiment includes a surface mount component having a plurality of terminal rows, a wiring board, and a cured film of a film-like solder connection material provided for each terminal row, which bonds the surface mount component to the wiring board and has a rectangular portion for each terminal row whose longitudinal direction is the row direction of the terminal row. Here, when the surface mount component includes a first terminal row and a second terminal row arranged in parallel, it is preferable that the protrusion amount of the cured film of the solder connection film of the first terminal row or the second terminal row arranged between the first terminal row and the second terminal row is 50% or less of the terminal length in a direction perpendicular to the row direction of the first terminal row or the second terminal row. In addition, when the surface mount component includes a first terminal row and a second terminal row arranged in parallel, and a third terminal row and a fourth terminal row arranged in parallel and perpendicular to the first terminal row and the second terminal row, the protrusion amount of the cured film of the solder connection film of the first terminal row, the second terminal row, the third terminal row, or the fourth terminal row arranged between the first terminal row and the second terminal row is preferably 50% or less of the terminal length in the direction perpendicular to the row direction of the first terminal row, the second terminal row, the third terminal row, or the fourth terminal row. This can prevent solder particles from remaining inside the first terminal row to the fourth terminal row without agglomerating.

[0013] In this embodiment, a film-like solder connection material having a rectangular portion with the row direction of the terminals as the longitudinal direction is provided for each terminal row, thereby restricting the movement of solder particles between the terminal rows due to the self-alignment effect in the joining process. This allows the solder particles in a predetermined rectangular portion to be aggregated for a predetermined terminal row, thereby obtaining high electrical reliability. The film-like solder connection material may be a solder connection film or a solder paste film on which solder paste is printed, as described later.

[0014] The film-like solder connection material may be continuous in a portion other than the rectangular portion corresponding to the terminal row. For example, when connecting a connector having a first terminal row and a second terminal row arranged in parallel, a film-like solder connection material may be used in which both ends in the longitudinal direction of two parallel rectangular portions are connected by a continuous portion. With such a film-like solder connection material, the continuous portions at both ends can further improve the adhesive strength.

[0015] Here, a connection structure refers to two materials or members electrically connected to each other. Furthermore, joining refers to joining two materials or members together. Furthermore, a terminal row refers to terminals (electrodes) lined up at a predetermined interval (pitch) in a predetermined direction. Furthermore, the predetermined direction in which the terminals are lined up is called the row direction of the terminal row, and the direction perpendicular to the row direction is called the width direction of the terminal row.

[0016] The surface mount component is not particularly limited as long as it has a plurality of terminal rows, and examples include a surface mount component having a first terminal row and a second terminal row arranged in parallel, a surface mount component having a first terminal row and a second terminal row arranged in parallel, and a third terminal row and a fourth terminal row arranged in parallel and perpendicular to the first terminal row and the second terminal row.

[0017] Specific examples of surface mount components include connectors, IC (Integrated Circuit) and LSI (Large Scale Integration) packages, LEDs (Light Emitting Diodes), and switches. For example, connectors include SMT (Surface Mount type) connectors having a first terminal row in which multiple pins (lead frames) extending outward on one side of the short side are arranged in the longitudinal direction, and a second terminal row in which multiple pins (lead frames) extending outward on the other side of the short side are arranged in the longitudinal direction. In addition, IC packages include surface mount lead type connectors such as SOP (Small Outline Package) and SOJ (Small Outline J-leaded) having terminal rows on two opposing sides of a rectangle, and QFP (Quad Flat Package) and QFN (Quad Flat No-leaded package) having terminal rows on four sides of a rectangle.

[0018] The wiring board is not particularly limited as long as it has wiring, and may be a rigid board or a flexible board (FPC: Flexible Printed Circuits) as long as it has electrodes on which surface-mounted components can be mounted, and may be broadly defined as a so-called printed wiring board (PWB). Examples of boards based on the type of base material include glass boards, ceramic boards, and plastic boards.

[0019] The upper limit of the pitch of the terminal rows of the surface mount components and the wiring board is preferably 2 mm or less, more preferably 1 mm or less, and even more preferably 0.5 mm or less, and the lower limit of the pitch of the terminal rows is preferably 0.06 mm or more, more preferably 0.08 mm or more, and even more preferably 0.1 mm or more.

[0020] The average thickness (height) of the solder between the terminals of the connection structure depends on the electrode area of ​​the wiring board and the surface mounted component, the content of the solder particles in the film-like solder connection material, etc., but the lower limit of the thickness is preferably 5 μm or more, more preferably 20 μm or more, and even more preferably 40 μm or more. The upper limit of the thickness is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less. This makes it possible to withstand the stress of the linear expansion difference between the surface mounted component and the wiring board due to thermal shock, and to obtain high conductive reliability.

[0021] In addition, the relative standard deviation (coefficient of variation, RSD (Relative Standard Deviation)) of the thickness (height) of the solder between the terminals after reflow is preferably less than 25%, more preferably 20% or less, and even more preferably 15% or less. A small rate of variation in the thickness (height) of the solder between the terminals can provide high conductivity reliability. In addition, the standard deviation (σ) of the thickness (height) of the solder between the terminals of the connection structure depends on the average thickness (height) of the solder between the terminals, but for example, when the average thickness (height) of the solder between the terminals is 5 μm or more and 200 μm, it is preferably 20 μm or less, more preferably 12 μm or less, and even more preferably 10 μm or less. A small rate of variation in the thickness of the solder between the terminals can provide high conductivity reliability.

[0022] Hereinafter, with reference to Figures 1 to 4, we will explain the process (A) of providing a solder connection film on multiple terminal rows of a wiring board, the process (B) of fixing surface mount components on the solder connection film, and the process (C) of joining the multiple terminal rows of the wiring board and the multiple terminal rows of the surface mount components using a reflow furnace.

[0023] [Process (A)] Fig. 1 is a plan view showing a state where a solder connection film is provided on each of parallel first and second terminal rows of a wiring board, and Fig. 2 is a cross-sectional view showing a state where a solder connection film is provided on the first terminal row of a wiring board. As shown in Fig. 1 and Fig. 2, in step (A), a rectangular first solder connection film 21 and a second solder connection film 22 containing solder particles 20 and having a longitudinal direction in the row direction of the terminal rows are provided on the first terminal row 11 and the second terminal row 12 of a wiring board 10.

[0024] Step (A) may be a temporary attachment step in which the first solder connection film 21 and the second solder connection film 22 are attached to the first terminal row 11 and the second terminal row 12 of the wiring board 10, respectively, at low temperature and low pressure, or may be a lamination step in which the first solder connection film 21 and the second solder connection film 22 are laminated onto the first terminal row 11 and the second terminal row 12 of the wiring board 10, respectively.

[0025] The width W of the first and second solder connection films 21, 22 is preferably 50% to 150% of the length L of the terminals 11a, 12a, and more preferably 75% to 125%. This allows the solder particles to aggregate on the terminals of the terminal row, thereby reducing the variation in the solder height on the terminals of the terminal row.

[0026] Moreover, the first and second solder connection films 21, 22 are preferably provided aligned with the outer end portions in the width direction of the first terminal row 11 and the second terminal row 12. Moreover, the protruding amount (WL) in the width direction of the rectangular portion of the first or second solder connection film arranged between the first and second terminal rows 11, 12 is preferably 50% or less, and more preferably 25% or less, of the length L of the terminals 11a, 12a. This makes it possible to prevent the solder particles 20 from remaining between the first terminal row 11 and the second terminal row 12 without agglomerating.

[0027] Moreover, it is preferable that the width W of the first and second solder connecting films 21, 22 satisfy the following formula (1). W≦(2L+S) / 2 (1) In the above formula (1), L is the length of the terminals 11a, 12a, and S is the distance between the first terminal row 11 and the second terminal row 12. There only needs to be a boundary between the first solder connection film 21 and the second solder connection film 22, and the distance (gap) S F may be zero.

[0028] The distance S between the first terminal row 11 and the second terminal row 12 is preferably 10 mm or less, more preferably 1 mm or less, and further preferably 0.5 mm or less. Even if the distance S between the first terminal row 11 and the second terminal row 12 is short, it is preferable that there is a boundary between the first solder connection film 21 and the second solder connection film 22, and the distance (gap) S F is preferably 0 mm or more, preferably 0.1 mm or more, and more preferably 0.2 mm or more. By having a boundary between the first solder connection film 21 and the second solder connection film 22, the movement of solder particles can be restricted, and the variation in the solder height on the terminals of the terminal row can be reduced.

[0029] [Process (B)] 3 is a cross-sectional view showing a state in which the first terminal row of the wiring board and the first terminal row of the surface mount component are aligned. As shown in FIG. 3, in step (B), the first and second terminal rows 11, 12 of the wiring board 10 are aligned with the first and second terminal rows 31, 32 of the surface mount component 30, and the surface mount component 30 is fixed onto the first solder connection film 21.

[0030] In step (B), the first and second terminal rows 11, 12 are aligned with the first and second terminal rows 31, 32 of the surface mount component 30 using, for example, a tool. The tool preferably has a suction mechanism for suctioning the surface mount component. In step (B), temporary pressure bonding may be performed by pressing the surface mount component 30 from the side using the tool.

[0031] [Process (C)] FIG. 4 is a cross-sectional view showing a state in which the wiring board and the surface mount component are heated in a reflow furnace. As shown in FIG. 4, in step (C), the first and second terminal rows 11, 12 of the wiring board 10 and the first and second terminal rows 31, 32 of the surface mount component 30 are joined by solder 41 using a reflow furnace set at a temperature equal to or higher than the melting point of the solder particles 20, and the wiring board 10 and the surface mount component 30 are bonded by a binder 40 of the solder connection film. Here, since the first and second solder connection films 21, 22 containing the solder particles 20 are provided on the first and second terminal rows 11, 12 of the wiring board 10, respectively, the movement of the solder particles between the terminal rows due to the self-alignment effect is restricted during reflow. This allows only the solder particles 20 in the first and second solder connection films 21, 22 to be aggregated to the first and second terminal rows 11, 12, respectively.

[0032] Examples of reflow furnaces include atmospheric pressure reflow, vacuum reflow, atmospheric pressure ovens, and autoclaves (pressurized ovens). Among these, it is preferable to use vacuum reflow and autoclaves, which can eliminate air bubbles contained in the joints. A reflow furnace can heat and bond the components without mechanical pressure and without load, so damage to the wiring board 10 and the surface mount components 30 can be suppressed. Here, "without load" refers to a state in which no mechanical pressure is applied.

[0033] The lower limit of the peak temperature (maximum attained temperature) in the reflow furnace should be equal to or higher than the temperature at which the solder particles melt and the temperature at which the solder connection film starts to harden, and is preferably 150°C or higher, more preferably 180°C or higher, and even more preferably 200°C or higher. The upper limit of the peak temperature in the reflow furnace is 300°C or lower, more preferably 290°C or lower, and even more preferably 280°C or lower. This allows the first terminal row 11 of the wiring board 10 and the first terminal row 31 of the surface mount component 30 to be solder-bonded. In addition, when a thermosetting binder is used for the solder connection film, the parts other than the solder bonding parts in the terminals are bonded by the thermosetting binder. Here, solder bonding refers to connecting the terminals (electrodes) of the facing electronic components by melting the solder.

[0034] The average thickness (height) T of the solder 41 between the terminals after reflow depends on the electrode area of ​​the wiring board and the surface mounted component, the solder particle content of the solder connection film, etc., but the lower limit of the thickness is preferably 5 μm or more, more preferably 20 μm or more, and even more preferably 40 μm or more. The upper limit of the thickness T is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less. This makes it possible to withstand the stress of the linear expansion difference between the surface mounted component and the wiring board due to thermal shock, and to obtain high conductivity reliability.

[0035] In addition, the relative standard deviation (coefficient of variation, RSD (Relative Standard Deviation)) of the thickness (height) of the solder between the terminals after reflow is preferably less than 25%, more preferably 20% or less, and even more preferably 15% or less. A small rate of variation in the thickness (height) of the solder between the terminals can provide high conductivity reliability. In addition, the standard deviation (σ) of the thickness (height) of the solder between the terminals of the connection structure depends on the average thickness (height) of the solder between the terminals, but for example, when the average thickness (height) of the solder between the terminals is 5 μm or more and 200 μm, it is preferably 20 μm or less, more preferably 12 μm or less, and even more preferably 10 μm or less. A small rate of variation in the thickness of the solder 41 between the terminals can provide high conductivity reliability.

[0036] According to the above-mentioned method for manufacturing a connection structure, by providing a solder connection film for each terminal row, it is possible to limit the movement of solder particles between terminal rows due to the self-alignment effect during heating. Therefore, only the solder particles in a predetermined solder connection film can be aggregated for a predetermined terminal row, and high electrical reliability can be obtained.

[0037] In the above-mentioned method for manufacturing a connection structure, in step (C), a reflow furnace is used to join multiple terminal rows of a wiring board and multiple terminal rows of a surface-mounted component. However, this is not limited to this, and for example, joining may be performed using a heating and pressurizing tool as long as it does not prevent the solder particles from agglomerating onto the terminals.

[0038] The solder connection film may be shaped according to the electrode pattern of the wiring board. For example, the solder connection film may have a substantially rectangular first shaped portion corresponding to a predetermined terminal row, a second shaped portion connected to one end of the first shaped portion and corresponding to an electrode at one end of the predetermined terminal row, and a third shaped portion connected to the other end of the first shaped portion and corresponding to an electrode at the other end of the predetermined terminal row, and may have a shape in which the first shaped portion to the third shaped portion are combined. Also, for example, the solder connection film may have a substantially rectangular first shaped portion corresponding to the first terminal row, a substantially rectangular second shaped portion corresponding to the second terminal row, a third shaped portion connecting one end of the first shaped portion to one end of the second shaped portion and corresponding to a pair of electrodes at one end of the first terminal row and the second terminal row, and a fourth shaped portion connecting the other end of the first shaped portion to the other end of the second shaped portion and corresponding to a pair of electrodes at the other ends of the first terminal row and the second terminal row, and may have a shape in which the first shaped portion to the fourth shaped portion are combined.

[0039] As described above, the distance (gap) between the shaped portions corresponding to adjacent terminal rows is preferably 0 mm or more, more preferably 0.1 mm or more, and more preferably 0.2 mm or more. The presence of a boundary between the shaped portions corresponding to adjacent terminal rows can limit the movement of solder particles, and can reduce the variation in the solder height on the terminals of the terminal rows. A solder connection film of such a shape can be obtained by punching, slitting, or the like.

[0040] [Variations] In the above-mentioned method for manufacturing a connection structure, in step (A), a solder connection film is provided on the terminal row, but this is not limited thereto, and for example, a metal mask (stencil) may be used to print solder paste and provide a solder paste film on the terminal row. An example of a solder paste is one in which the polymer component is removed from the binder formulation of the solder connection film described below to reduce the viscosity.

[0041] Hereinafter, printing of solder paste using a metal mask will be described with reference to Figs. 5 to 8. Fig. 5 is a plan view showing an example of a wiring board. As shown in Fig. 5, a wiring board 50 includes a first terminal row 51 in which a plurality of terminals 51a, 51b, 51c, and 51d are arranged at a predetermined interval, and a second terminal row 52 in which a plurality of terminals 52a, 52b, 52c, and 52d are arranged at a predetermined interval. The row direction of the first terminal row 51 and the row direction of the second terminal row 52 are parallel, and the distance between the first terminal row 51 and the second terminal row 52 is preferably 10 mm or less, more preferably 1 mm or less, and further preferably 0.5 mm or less, as described above.

[0042] Fig. 6(A) is a plan view showing an example of a metal mask as an embodiment, and Fig. 6(B) is a plan view showing an example of a solder paste film printed using the metal mask shown in Fig. 6(A). Metal mask 53 shown in Fig. 6(A) has first openings 54 corresponding to first terminal row 51 and second openings 55 corresponding to second terminal row 52.

[0043] The method of printing the solder paste is to align and set the wiring board 50 under the metal mask 53, then move the squeegee downward from above the metal mask 53 while pressing it down, apply the solder paste to the specified locations through the openings of the metal mask 53, and then release the set wiring board 50. This allows a solder paste film with the same shape as the openings of the metal mask 53 to be transferred to the wiring board 50.

[0044] 6(B), in the wiring board 50, a first solder paste film 56 having the same shape as the first opening 54 is provided on the first terminal row 51, a second solder paste film 57 having the same shape as the second opening 55 is provided on the second terminal row 52, ​​and a gap is provided between the first solder paste film 56 and the second solder paste film 57. This makes it possible to restrict the movement of the solder particles between the terminal rows due to the self-alignment effect during heating, so that only the solder particles in a predetermined solder connection film can be aggregated for a predetermined terminal row, thereby obtaining high electrical connection reliability.

[0045] Similarly to the solder connection film described later, the thickness of the solder paste film printed on the wiring board 50 has a lower limit of preferably 0.6 or more, more preferably 0.8 or more, and even more preferably 0.9 or more, relative to the average particle size of the solder particles. The upper limit of the thickness is preferably 3.0 or less, more preferably 2.0 or less, and even more preferably 1.5 or less, relative to the average particle size of the solder particles. If the ratio of the average particle size of the solder particles to the thickness of the solder paste film is large, there is a risk that printing using a metal mask will become more difficult.

[0046] Here, the thickness of the solder paste film refers to the thickness of the binder resin layer only, and does not include the particle diameter. The thickness of the film-like solder paste can be measured using a known micrometer or digital thickness gauge (e.g., MDE-25M, minimum display 0.0001 mm, manufactured by Mitutoyo Corporation) that can measure thicknesses of 1 μm or less, preferably 0.1 μm or less. The film thickness can be determined by measuring at 10 or more points and averaging the measured thickness.

[0047] Fig. 7(A) is a plan view showing an example of a metal mask as a comparative example, and Fig. 7(B) is a plan view showing an example of a solder paste film printed using the metal mask shown in Fig. 7(A). Metal mask 58 shown in Fig. 7(A) has openings 59 corresponding to both first terminal row 51 and second terminal row 52.

[0048] When a solder paste film having the same shape as the openings of metal mask 58 is transferred to wiring board 50, solder paste film 60 having the same shape as openings 59 is provided on first terminal row 51 and second terminal row 52 on wiring board 50, as shown in Fig. 7(B). In this case, solder particles move between the terminal rows during heating and become unevenly distributed, resulting in a large degree of variation in the thickness (height) of the solder between the upper and lower terminals and making it difficult to obtain high conductivity reliability.

[0049] Fig. 8(A) is a plan view showing an example of a metal mask as a comparative example, and Fig. 8(B) is a plan view showing an example of a solder paste film printed using the metal mask shown in Fig. 8(A). Metal mask 61 shown in Fig. 8(A) has openings 62a, 62b, 62c, and 62d corresponding to the terminals of first terminal row 51, and openings 63a, 63b, 63c, and 63d corresponding to the terminals of second terminal row 52, ​​respectively.

[0050] When a solder paste film having the same shape as the opening of the metal mask 61 is transferred to the wiring board 50, as shown in Fig. 8(B), solder paste films 64a, 64b, 64c, 64d, 65a, 65b, 65c, and 65d having the same shapes as the openings 62a, 62b, 62c, 62d, 63a, 63b, 63c, and 63d are provided on the terminals 51a, 51b, 51c, and 51d of the first terminal row 51 and on the terminals 52a, 52b, 52c, and 52d of the second terminal row 52, ​​respectively. In this case, if the opening of the metal mask becomes smaller due to fine patterning, the solder paste remains in the opening, and for example, a situation occurs in which the solder paste is not transferred to the wiring board 50, as in the terminal 52b shown in Fig. 8(B).

[0051] [Connector assembly] In the following, a connector assembly using a vertical mating type connector will be described in detail as a specific example of a surface mount component. The connector is mainly a resin molded product having a mating part, and may be, for example, a resin molded product with multiple electrodes protruding in the longitudinal direction (a so-called centipede type connector) or one without protruding electrodes (a flip chip type connector).

[0052] Fig. 9 is a cross-sectional view showing an example of a plug and a receptacle in a short-side direction in a vertical mating type connector. The example of the connector shown in Fig. 9 is composed of a receptacle 70 to which receptacle terminals 71A, 71B are fixed by insulating resin, and a plug 80 to which plug terminals 81A, 81B are fixed by insulating resin. In addition, receptacle terminals 71A, 71B are formed at a predetermined pitch in the longitudinal direction of receptacle 70, and plug terminals 81A, 81B are formed at a predetermined pitch in the longitudinal direction of plug 80.

[0053] Fig. 10 is a cross-sectional view showing a schematic longitudinal direction of a connection structure in which a plug of a connector is connected to a wiring board, and Fig. 11 is a cross-sectional view showing a schematic transverse direction of a connection structure in which a plug of a connector is connected to a wiring board. That is, the longitudinal cross section shown in Fig. 10 is a Y cross section perpendicular to the transverse cross section shown in Fig. 11, and the transverse cross section shown in Fig. 11 is an X cross section perpendicular to the longitudinal cross section shown in Fig. 10.

[0054] As shown in Figures 10 and 11, the connector mounting body includes a plug 80 having plug terminals 81A as a first terminal row and plug terminals 81B as a second terminal row, a wiring board 90 having board terminals 91A, 91B corresponding to the plug terminals 81A, 81B, and an adhesive layer 100 joining the plug terminals 81A, 81B and the board terminals 91A, 91B with solder 101.

[0055] Plug 80 includes plug terminals 81A, 81B, connection pins 82A, 82B formed by bending a conductive metal continuous with plug terminals 81A, 81B, and insulating resin 83 that fixes plug terminals 81A, 81B and connection pins 82A, 82B.

[0056] The insulating resin 83 is made of, for example, polyamide or LCP (Liquid Crystal Polymer), and fixes the plug terminals 81A, 81B and the connection pins 82A, 82B by, for example, resin molding. Furthermore, leads are formed at the ends of the plug terminals 81A, 81B, respectively, and the plug terminals 81A, 81B constitute a surface mount type lead array.

[0057] The upper limit of the minimum value of the distance between adjacent terminals (space distance) in plug terminals 81A, 81B and board terminals 91A, 91B is preferably 0.8 mm or less, more preferably 0.3 mm or less, and even more preferably 0.2 mm or less. The lower limit of the minimum value of the distance between adjacent terminals in plug terminals 81A, 81B and board terminals 91A, 91B is preferably 50 μm or more, more preferably 60 μm or more, and even more preferably 70 μm or more. The surfaces of plug terminals 81A, 81B are preferably gold-plated.

[0058] The wiring board 90 has board terminals 91A, 91B on a base material corresponding to the plug terminals 81A, 81B. The wiring board 70 may be any board that can be broadly defined as a so-called printed wiring board (PWB), and may be either a rigid board or a flexible board (FPC: Flexible Printed Circuits). Examples of boards based on the type of base material include glass boards, ceramic boards, and plastic boards. In addition, the surfaces of the board terminals 91A, 91B are preferably gold-plated.

[0059] The adhesive layer 100 includes solder 101 that joins the plug terminals 81A, 81B and the board terminals 91A, 91B, and a hardened binder 102. The adhesive layer 80 is a hardened solder connection film described below, which joins the plug terminals 81A, 81B and the board terminals 91A, 91B with the solder 81, and is formed by hardening the binder of the solder connection film between the plug 80 and the wiring board 90.

[0060] <2. Solder connection film> The solder connection film according to the present embodiment contains a binder, solder particles, and a flux compound. Since the solder connection film has a film shape, not only can the amount of solder particles be made uniform, but also the film is easy to handle, which can increase the work efficiency.

[0061] The lower limit of the thickness of the solder connection film is preferably 0.6 or more, more preferably 0.8 or more, and even more preferably 0.9 or more, relative to the average particle size of the solder particles. The upper limit of the thickness of the solder connection film is preferably 3.0 or less, more preferably 2.0 or less, and even more preferably 1.5 or less, relative to the average particle size of the solder particles. If the ratio of the average particle size of the solder particles to the thickness of the solder connection film is large, the handling of the solder connection film may become difficult. Here, the thickness of the solder connection film refers to the thickness of only the binder resin layer, and does not include the particle size.

[0062] The thickness of the solder joint film can be measured using a known micrometer or digital thickness gauge (e.g., MDE-25M, minimum display 0.0001 mm, manufactured by Mitutoyo Corporation) capable of measuring 1 μm or less, preferably 0.1 μm or less. The film thickness can be determined by measuring at 10 or more locations and averaging the measured values. However, when the film thickness is thinner than the particle diameter, a contact-type thickness measuring device is not suitable, and therefore it is preferable to use a laser displacement meter (e.g., Keyence Corporation, spectral interference displacement type SI-T series, etc.).

[0063] The binder of the solder connection film may be either thermosetting or thermoplastic, but is preferably thermosetting, which can be melted and hardened by temperature control in a reflow process. The following describes thermosetting binders (insulating binders).

[0064] [Thermosetting binder] The thermosetting binder preferably has a heat generation peak temperature higher than the melting point of the solder particles, and preferably has a minimum melt viscosity temperature lower than the melting point of the solder particles. This allows the thermosetting binder to be melted by heating, and the solder particles to be aggregated on the terminals, and then the thermosetting binder can be hardened. Here, the heat generation peak temperature and the minimum melt viscosity temperature can be measured using, for example, a rotational rheometer (manufactured by Thermo Fisher Scientific) under the conditions of a measurement pressure of 1 N, a temperature range of 30 to 200°C, a heating rate of 10°C / min, a measurement frequency of 1 Hz, and a measurement plate diameter of 8 mm.

[0065] Examples of the thermosetting binder include a thermal radical polymerization type resin composition containing a (meth)acrylate compound and a thermal radical polymerization initiator, a thermal cationic polymerization type resin composition containing an epoxy compound and a thermal cationic polymerization initiator, and a thermal anionic polymerization type resin composition containing an epoxy compound and a thermal anionic polymerization initiator. A known pressure-sensitive adhesive composition may also be used. The (meth)acrylic monomer includes both acrylic monomers and methacrylic monomers.

[0066] In the following, a specific example will be described taking as an example a thermally polymerizable resin composition containing a solid epoxy resin, a liquid epoxy resin, and an epoxy resin curing agent.

[0067] The solid epoxy resin is not particularly limited as long as it is solid at room temperature and has one or more epoxy groups in the molecule, and may be, for example, a bisphenol A type epoxy resin, a biphenyl type epoxy resin, or the like. Among these, it is preferable to use a crystalline bisphenol A type epoxy resin with a low melt viscosity. A specific example of a crystalline bisphenol A type epoxy resin available on the market is a product name "YL6810" (crystalline BPA type epoxy resin) of Mitsubishi Chemical Corporation, which has a viscosity of 40 to 55 P by the Gardner-Holdt method. The solid epoxy resin may also be a phenoxy resin synthesized from bisphenols and epichlorohydrin. An example of the phenoxy resin is "YP-50" manufactured by Nippon Steel Chemical & Material Co., Ltd. This allows the film shape to be maintained. The room temperature is the range of 20°C ± 15°C (5°C to 35°C) specified in JIS Z 8703.

[0068] The liquid epoxy resin is not particularly limited as long as it is liquid at room temperature, and may be, for example, a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, hydrogenated bisphenol A glycidyl ether, or a urethane-modified epoxy resin. An example of the bisphenol F type epoxy resin is "YL983U" manufactured by Mitsubishi Chemical Corporation, and an example of the hydrogenated bisphenol A glycidyl ether is "YX8000" manufactured by Mitsubishi Chemical Corporation.

[0069] The amount of liquid epoxy resin is preferably 160 parts by mass or less, more preferably 140 parts by mass or less, and even more preferably 120 parts by mass or less, based on 100 parts by mass of solid epoxy resin. If the amount of liquid epoxy resin is large, it becomes difficult to maintain the film shape. In addition, if the amount of liquid epoxy resin is large, the cured physical properties after thermal curing generally become high elasticity due to high crosslink density, so that the stress relaxation ability becomes small.

[0070] The epoxy resin curing agent is not particularly limited as long as it is a heat curing agent that starts curing by heat, and examples thereof include anionic curing agents such as amines and imidazoles, and cationic curing agents such as sulfonium salts. The curing agent may be microencapsulated so as to be resistant to the solvent used in forming the film. Anionic curing agents include imidazole epoxy resin curing agents such as "2P4MHZ-PW" manufactured by Shikoku Kasei Co., Ltd.

[0071] [Solder particles] The solder particles can be appropriately selected from, for example, Sn-Pb, Pb-Sn-Sb, Sn-Sb, Sn-Pb-Bi, Bi-Sn, Sn-Cu, Sn-Pb-Cu, Sn-In, Sn-Ag, Sn-Pb-Ag, Pb-Ag, etc., as specified in JIS Z 3282-1999, depending on the electrode material, connection conditions, etc. Among these, the solder particles are preferably one or more selected from the group consisting of Sn-Bi-Cu alloy, Sn-Bi-Ag alloy, Sn-Bi alloy, Sn-Pb-Bi alloy, and Sn-In alloy. Specific examples of solder particles include Sn59.9Bi40Cu0.1, Sn30Bi0.5Cu, Sn30Bi, Sn40Bi, Sn50Bi, Sn58Bi, Sn40Bi0.1Cu, Sn43Pb14Bi, Sn20In, etc. This allows for excellent connection reliability.

[0072] The lower limit of the melting point of the solder particles is preferably 110°C or higher, more preferably 120°C or higher, and even more preferably 130°C or higher. The upper limit of the melting point of the solder particles may be 250°C or lower, preferably 200°C or lower, more preferably 180°C or lower, and even more preferably 160°C or lower. In addition, the solder particles may have a flux compound directly bonded to the surface for the purpose of activating the surface. Activating the surface can promote metal bonding with the electrode part.

[0073] The average particle size of the solder particles is preferably 0.5 times or less, more preferably 0.3 times or less, and even more preferably 0.2 times or less, of the minimum inter-terminal distance (space distance) between the terminal row of the surface-mounted component and the terminal row of the wiring board. Due to the relationship between the space distance and the average particle size of the solder particles, the terminal row of the surface-mounted component and the terminal row of the wiring board can be joined using a reflow furnace. If the average particle size of the solder particles is larger than 0.5 times the minimum inter-terminal distance between the terminal row of the surface-mounted component and the terminal row of the wiring board, the possibility of a short circuit occurring increases.

[0074] The lower limit of the average particle size of the solder particles is preferably 0.5 μm or more, more preferably 3 μm or more, and more preferably 5 μm or more, and the upper limit of the average particle size of the solder particles may be 50 μm or less, and is 30 μm or less, preferably 25 μm or less, and more preferably 20 μm or less. This makes it possible to obtain a good solder joint state and high reliability.

[0075] The average particle size is the average value of the major axis diameter of particles measured, for example, at N=20 or more, preferably N=50 or more, more preferably N=200 or more in an observation image using a metallurgical microscope, an optical microscope, an electron microscope such as a SEM (Scanning Electron Microscope), or the like, and in the case of a spherical particle, it is the average value of the diameter of the particles. In addition, the observed image may be a measured value measured using a known image analysis software ("WinROOF": Mitani Shoji Co., Ltd., "Azokun (registered trademark)": Asahi Kasei Engineering Co., Ltd., etc.), or a measured value (N=1000 or more) measured using an image type particle size distribution measuring device (for example, FPIA-3000 (Malvern Instruments)). The average particle size obtained from the observed image or the image type particle size distribution measuring device can be the average value of the maximum length of the particles. In addition, when preparing a solder connection film, the manufacturer's values ​​such as the particle size (D50) at which the cumulative frequency in the particle size distribution obtained simply by a laser diffraction / scattering method is 50%, the arithmetic mean diameter (preferably on a volume basis), etc. may be used.

[0076] The solder particles are preferably dispersed in a binder, and may be arranged randomly or according to a certain rule. Also, the solder particles may be in the form of aggregates in which a plurality of solder particles are aggregated.

[0077] The content of solder particles in the solder connection film can be appropriately determined based on the pitch of the terminal row of the surface mount component and the wiring board, and is preferably 10% to 60% by volume for a pitch of 0.1 mm to 0.4 mm of the terminal row of the surface mount component and the wiring board. For example, it is preferably 20% to 58% by volume when the pitch is 0.4 mm, 20% to 58% by volume when the pitch is 0.35 mm, 20% to 48% by volume when the pitch is 0.2 mm, 15% to 48% by volume when the pitch is 0.15 mm, and 10% to 38% by volume when the pitch is 0.1 mm. If the content of solder particles is too small, excellent conductivity, heat dissipation, and adhesion cannot be obtained, and if the content is too large, the anisotropy is easily impaired, making it difficult to obtain excellent conductivity reliability.

[0078] [Flux compounds] The flux compound removes foreign matter and oxide film on the electrode surface, prevents oxidation of the electrode surface, and reduces the surface tension of the molten solder. Examples of the flux compound include carboxylic acids such as levulinic acid, maleic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, and sebacic acid. Among these, it is preferable to use glutaric acid, which is excellent in removing oxide film.

[0079] [Other additives] In addition to the above-mentioned binder, solder particles, and flux compound, various additives that have been used as adhesives in the past can be blended into the solder connection film as long as they do not impair the effects of the present technology. The particle size of the additive is preferably smaller than the average particle size of the solder particles, but is not particularly limited as long as it does not impede the bonding between electrodes.

[0080] The above-mentioned solder connection film can be obtained, for example, by mixing an insulating binder, solder particles, and a flux compound in a solvent, applying the mixture to a release-treated film by a bar coater to a predetermined thickness, and then drying to volatilize the solvent. The mixture may also be applied to a release-treated film by a bar coater and then pressurized to a predetermined thickness. In order to increase the dispersibility of the solder particles, it is preferable to apply a high shear force while the film contains the solvent. For example, a known batch-type planetary stirring device can be used. The amount of residual solvent in the solder connection film is preferably 2% or less, more preferably 1% or less.

[0081] According to the solder connection film of the present embodiment, the removal of the oxide film by the flux compound is appropriately suppressed, and the solder is easily left in an appropriate range, so that the solder remaining area can be set in an appropriate range. In addition, since the solder remaining area is in an appropriate range, the moisture permeation resistance and mechanical strength are improved, and the decrease in the bonding strength and the increase in the resistance value can be suppressed. EXAMPLES

[0082] <3. First Example> In the first example, an anisotropic conductive film containing solder particles was produced as a form of a solder connection film. Then, a connector was mounted on a substrate having a first terminal row and a second terminal row using the anisotropic conductive film, and the connection structure after reflow was evaluated for bridge generation, conduction resistance, solder residue, and solder height.

[0083] [Preparation of anisotropic conductive film] A binder was prepared by mixing 45 parts by mass of phenoxy resin (YP-50, Nippon Steel Chemical & Material Co., Ltd.), 10 parts by mass of hydrogenated bisphenol A glycidyl ether (YX8000, Mitsubishi Chemical Co., Ltd.), 45 parts by mass of crystalline bisphenol A type epoxy resin (YL6810, Mitsubishi Chemical Co., Ltd.), 10 parts by mass of imidazole-based epoxy resin hardener (2P4MHZ-PW (2-phenyl-4-methyl-5-hydroxymethylimidazole), Shikoku Chemical Industry Co., Ltd.), and 8 parts by mass of glutaric acid (1,3-propanedicarboxylic acid, Tokyo Chemical Industry Co., Ltd.). A predetermined amount of solder particles (Sn59.9Bi40Cu0.1) with an average particle size of 20 μm was mixed with 118 parts by mass of the binder to prepare an anisotropic conductive film of a predetermined thickness.

[0084] [Fabrication of connection structure] A printed wiring board (having a first terminal row and a second terminal row, with a distance of 0.8 mm between the first terminal row and the second terminal row, the first terminal row and the second terminal row having a pitch of 0.35 mm (line / space = 0.18 / 0.17 mm, terminal length 0.8 mm), glass epoxy base material thickness 1.5 mm, copper pattern thickness 18 μm, surface OSP treatment) was prepared as the substrate.

[0085] The connectors prepared were a plug connector (Hirose BM23FR0.6-20DP, 10 pins on one side (20 pins on both sides), 0.35 mmP, line / space = 0.12 / 0.23 mm, terminal surface Au plated), and a receptacle connector (Hirose BM23FR0.6-20DS, 10 pins on one side (20 pins on both sides), 0.35 mmP, line / space = 0.12 / 0.23 mm, terminal surface Au plated).

[0086] The anisotropic conductive film was cut to a predetermined size and temporarily pressed onto the terminals of the board at 45°C, 1 MPa, and 1 second to temporarily attach the anisotropic conductive film to the terminals of the board. Next, connectors (plug connector and receptacle connector) were placed on the anisotropic conductive film and reflow was performed under the following reflow conditions to produce a connection structure. Reflow conditions: 150℃~260℃-100sec, peak top 260℃

[0087] [Evaluation of bridge occurrence] After reflow, the insulation resistance of the connection structure was measured when a voltage of 20 V was applied between adjacent terminals using a digital multimeter. 6 Ω or less was counted as the occurrence of solder bridging.

[0088] [Evaluation of conduction resistance] The connection structure after reflow was measured for its conduction resistance value when DC 10 mA was applied by the four-terminal method using a digital multimeter, and was evaluated based on the maximum resistance value. The evaluation criteria for A to C were as follows. A: Maximum resistance is 50mΩ or less B: Maximum resistance value is over 50mΩ and 90mΩ or less C: Maximum resistance value is over 90mΩ

[0089] [Evaluation of solder remaining] After reflow, the connection structure was X-rayed using an X-ray device to determine whether or not there was any solder remaining other than at the terminals.

[0090] [Solder height evaluation] For the connection structure after reflow, the cross section between the terminal of the first electronic component and the pin of the second component was observed using an electron microscope, the height (thickness) of the solder was measured, and the average value, standard deviation σ, and relative standard deviation (RSD) were calculated.

[0091] <Example 1> 118 parts by mass of binder was mixed with 460 parts by mass of solder particles to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.8 mm.

[0092] Fig. 12(A) is a photograph showing a state in which an anisotropic conductive film is temporarily attached to a printed wiring board in Example 1, Fig. 12(B) is a photograph showing a state in which a connector is mounted on a printed circuit board in Example 1, and Fig. 12(C) is an X-ray photograph showing a connection structure after reflow in Example 1. Anisotropic conductive films with a width of 0.8 mm were temporarily attached to the first terminal row and the second terminal row, respectively, and a gap with a width of 0.8 mm was provided between the first terminal row and the second terminal row, and the connector was mounted.

[0093] As shown in Table 1, the connection structure of Example 1 did not experience any bridges, was rated an A for conductive resistance, and had no solder residue as shown in the X-ray photograph of Fig. 12(C). The average solder height was 51 µm, the standard deviation was 6 µm, and the relative standard deviation was 12%.

[0094] <Example 2> A connection structure was produced in the same manner as in Example 1, except that 690 parts by mass of solder particles were mixed with 118 parts by mass of binder to produce an anisotropic conductive film having a thickness of 40 μm. As shown in Table 1, the connection structure of Example 2 did not produce bridges, was rated an A for conductive resistance, and had no solder residue. In addition, the average solder height was 60 μm, the standard deviation was 7 μm, and the relative standard deviation was 12%.

[0095] <Example 3> A connection structure was produced in the same manner as in Example 1, except that 1040 parts by mass of solder particles were mixed with 118 parts by mass of binder to produce an anisotropic conductive film having a thickness of 40 μm. As shown in Table 1, the connection structure of Example 3 did not produce bridges, was rated an A for conductive resistance, and had no solder residue. In addition, the average solder height was 71 μm, the standard deviation was 8 μm, and the relative standard deviation was 11%.

[0096] <Comparative Example 1> 118 parts by mass of binder was mixed with 300 parts by mass of solder particles to produce an anisotropic conductive film with a thickness of 40 μm, which was then cut to a width of 2.4 mm.

[0097] Fig. 13(A) is a photograph showing a state in which an anisotropic conductive film is temporarily attached to a printed wiring board for Comparative Example 1, Fig. 13(B) is a photograph showing a state in which a connector is mounted on a printed circuit board for Comparative Example 1, and Fig. 13(C) is an X-ray photograph showing a connection structure after reflow for Comparative Example 1. An anisotropic conductive film with a width of 2.4 mm was temporarily attached to the entire surface including the first terminal row and the second terminal row, and the connector was mounted.

[0098] As shown in Table 1, the connection structure of Comparative Example 1 did not experience any bridges, was rated B for conductive resistance, and had solder residue as shown in the X-ray photograph of Fig. 13(C). The average solder height was 48 µm, the standard deviation was 17 µm, and the relative standard deviation was 35%.

[0099] <Comparative Example 2> A connection structure was produced in the same manner as in Comparative Example 1, except that 460 parts by mass of solder particles were mixed with 118 parts by mass of binder to produce an anisotropic conductive film having a thickness of 40 μm. As shown in Table 1, the connection structure of Comparative Example 2 had bridges (3ch), was rated C for conduction resistance, and had solder residue. In addition, the average solder height was 74 μm, the standard deviation was 21 μm, and the relative standard deviation was 28%.

[0100] <Comparative Example 3> A connection structure was produced in the same manner as in Comparative Example 1, except that 460 parts by mass of solder particles were mixed with 118 parts by mass of binder to produce an anisotropic conductive film having a thickness of 30 μm. As shown in Table 1, the connection structure of Comparative Example 3 did not produce bridges, was rated B for conductive resistance, and had solder residue. The average solder height was 59 μm, the standard deviation was 23 μm, and the relative standard deviation was 39%.

[0101] <Comparative Example 4> A connection structure was produced in the same manner as in Comparative Example 1, except that 690 parts by mass of solder particles were mixed with 118 parts by mass of binder to produce an anisotropic conductive film having a thickness of 40 μm. As shown in Table 1, the connection structure of Comparative Example 4 had bridges (2ch), was rated C for conduction resistance, and had solder residue. In addition, the average solder height was 87 μm, the standard deviation was 25 μm, and the relative standard deviation was 29%.

[0102] [Table 1]

[0103] In Comparative Examples 1 to 4, an anisotropic conductive film was temporarily attached to the entire surface including the first and second terminal rows, so solder remained between the first and second terminal rows, and the standard deviation and relative standard deviation of the solder height were high. This is thought to be because the solder particles moved between the first and second terminal rows, and the solder particles did not efficiently aggregate on the terminals.

[0104] On the other hand, in Examples 1 to 3, since anisotropic conductive films were temporarily attached to the first and second terminal rows, respectively, no solder residue was generated between the first and second terminal rows, and the standard deviation and relative standard deviation of the solder height were low. This is believed to be because the solder particles did not move between the first and second terminal rows, and the solder particles efficiently aggregated on the terminals.

[0105] <4. Second Example> In the second example, an anisotropic conductive film was temporarily attached to a substrate having a first terminal row and a second terminal row, and reflow was performed, and the occurrence of bridging and the solder height were evaluated.

[0106] A printed wiring board (having a first terminal row and a second terminal row, with a distance of 0.8 mm between the first terminal row and the second terminal row, the first terminal row and the second terminal row having a pitch of 0.35 mm (line / space = 0.18 / 0.17 mm, terminal length 0.8 mm), glass epoxy base material thickness 1.5 mm, copper pattern thickness 18 μm, surface OSP treatment) was prepared as the substrate.

[0107] The anisotropic conductive film was cut to a specified size and temporarily pressed onto the terminals of the substrate at 45°C, 1 MPa, and 1 second. The anisotropic conductive film was temporarily attached to the terminals of the substrate, and reflow was performed under the reflow conditions listed below to produce a sample. Reflow conditions: 150℃~260℃-100sec, peak top 260℃

[0108] [Evaluation of bridge occurrence] After reflow, the insulation resistance of the sample was measured using a digital multimeter when a voltage of 20 V was applied between adjacent terminals. 6 A resistance of Ω or less was counted as the occurrence of solder bridging, and a test result in which no bridging occurred was rated "OK", and a test result in which bridging occurred was rated "NG".

[0109] [Solder height evaluation] The solder height (thickness) on the wiring of the sample after reflow was measured using a 3D measuring laser microscope (Olympus, LEXT OLS5000), and the average value, standard deviation σ, and relative standard deviation (RSD) were calculated.

[0110] [Preparation of anisotropic conductive film] A binder was prepared by mixing 45 parts by mass of phenoxy resin (YP-50, Nippon Steel Chemical & Material Co., Ltd.), 10 parts by mass of hydrogenated bisphenol A glycidyl ether (YX8000, Mitsubishi Chemical Co., Ltd.), 45 parts by mass of crystalline bisphenol A type epoxy resin (YL6810, Mitsubishi Chemical Co., Ltd.), 10 parts by mass of imidazole-based epoxy resin hardener (2P4MHZ-PW (2-phenyl-4-methyl-5-hydroxymethylimidazole), Shikoku Chemical Industry Co., Ltd.), and 8 parts by mass of glutaric acid (1,3-propanedicarboxylic acid, Tokyo Chemical Industry Co., Ltd.). A predetermined amount of solder particles (Sn59.9Bi40Cu0.1) with an average particle size of 20 μm was mixed with 118 parts by mass of the binder to prepare an anisotropic conductive film of a predetermined thickness.

[0111] <Example 4> 118 parts by mass of binder was mixed with 460 parts by mass of solder particles to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 1.2 mm. Anisotropic conductive films having a width of 1.2 mm were temporarily attached to the first terminal row and the second terminal row, respectively, and a gap of 0 mm was provided between the first terminal row and the second terminal row. As shown in Table 2, the sample of Example 4 was evaluated as OK for bridge generation, with an average solder height of 58.8 μm, a standard deviation of 8.4 μm, and a relative standard deviation of 14%.

[0112] <Example 5> 118 parts by mass of binder was mixed with 460 parts by mass of solder particles to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 1.0 mm. Anisotropic conductive films having a width of 1.0 mm were temporarily attached to the first terminal row and the second terminal row, respectively, and a gap of 0.4 mm was provided between the first terminal row and the second terminal row. As shown in Table 2, the sample of Example 5 was evaluated as OK for bridge generation, with an average solder height of 56.8 μm, a standard deviation of 5.8 μm, and a relative standard deviation of 10%.

[0113] <Example 6> 118 parts by mass of binder was mixed with 460 parts by mass of solder particles to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.8 mm. Anisotropic conductive films having a width of 0.8 mm were temporarily attached to the first terminal row and the second terminal row, respectively, and a gap of 0.8 mm was provided between the first terminal row and the second terminal row. As shown in Table 2, the sample of Example 6 was evaluated as OK for bridge generation, with an average solder height of 44.3 μm, a standard deviation of 5.3 μm, and a relative standard deviation of 14%.

[0114] <Example 7> 118 parts by mass of binder was mixed with 460 parts by mass of solder particles to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.6 mm. Anisotropic conductive films having a width of 0.6 mm were temporarily attached to the first terminal row and the second terminal row, respectively, and a gap of 1.2 mm was provided between the first terminal row and the second terminal row. As shown in Table 2, the sample of Example 7 was evaluated as OK for bridge generation, with an average solder height of 42.8 μm, a standard deviation of 3.8 μm, and a relative standard deviation of 9%.

[0115] <Example 8> 118 parts by mass of binder was mixed with 460 parts by mass of solder particles to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.4 mm. Anisotropic conductive films having a width of 0.4 mm were temporarily attached to the first terminal row and the second terminal row, respectively, and a gap of 1.6 mm was provided between the first terminal row and the second terminal row. As shown in Table 2, the sample of Example 8 was evaluated as OK for bridge generation, with an average solder height of 42.2 μm, a standard deviation of 8.5 μm, and a relative standard deviation of 20%.

[0116] <Comparative Example 5> A 40 μm thick anisotropic conductive film was prepared by mixing 118 parts by weight of binder with 460 parts by weight of solder particles, and the film was cut to a width of 2.4 mm. A 2.4 mm wide anisotropic conductive film was temporarily attached to the entire surface including the first terminal row and the second terminal row. As shown in Table 2, the sample of Comparative Example 5 was rated as NG for bridge generation, had an average solder height of 57.0 μm, a standard deviation of 14.0 μm, and a relative standard deviation of 25%.

[0117] [Table 2]

[0118] In Comparative Example 5, an anisotropic conductive film was temporarily attached to the entire surface including the first and second terminal rows, so bridges occurred and the standard deviation and relative standard deviation of the solder height were high. This is thought to be because the solder particles moved between the first and second terminal rows, and the solder particles did not efficiently aggregate on the terminals.

[0119] On the other hand, in Examples 4 to 8, since the anisotropic conductive film was temporarily attached to each of the first and second terminal rows, no bridges were generated, and the standard deviation and relative standard deviation of the solder height were low. In addition, in Examples 5 to 7, the protrusion amount of the rectangular parts in the width direction of the first and second anisotropic conductive films arranged between the first and second terminal rows, respectively, was 25% or less, so that the standard deviation and relative standard deviation of the solder height could be further reduced. This is considered to be due to efficient aggregation of the solder particles to the terminals.

[0120] <Example 9> 118 parts by mass of binder was mixed with 690 parts by mass of solder particles to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 1.2 mm. Anisotropic conductive films having a width of 1.2 mm were temporarily attached to the first terminal row and the second terminal row, respectively, and a gap of 0 mm was provided between the first terminal row and the second terminal row. As shown in Table 3, the sample of Example 9 was evaluated as OK for bridge generation, with an average solder height of 67.5 μm, a standard deviation of 9.7 μm, and a relative standard deviation of 14%.

[0121] <Example 10> 118 parts by mass of binder was mixed with 690 parts by mass of solder particles to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 1.0 mm. Anisotropic conductive films having a width of 1.0 mm were temporarily attached to the first terminal row and the second terminal row, respectively, and a gap of 0.4 mm was provided between the first terminal row and the second terminal row. As shown in Table 3, the sample of Example 10 was evaluated as OK for bridge generation, with an average solder height of 66.0 μm, a standard deviation of 7.9 μm, and a relative standard deviation of 12%.

[0122] <Example 11> 690 parts by mass of solder particles were mixed with 118 parts by mass of binder to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.8 mm. Anisotropic conductive films having a width of 0.8 mm were temporarily attached to the first terminal row and the second terminal row, respectively, and a gap of 0.8 mm was provided between the first terminal row and the second terminal row. As shown in Table 3, the sample of Example 11 was evaluated as OK for bridge generation, with an average solder height of 50.5 μm, a standard deviation of 6.4 μm, and a relative standard deviation of 13%.

[0123] <Example 12> 690 parts by mass of solder particles were mixed with 118 parts by mass of binder to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.6 mm. Anisotropic conductive films having a width of 0.6 mm were temporarily attached to the first terminal row and the second terminal row, respectively, and a gap of 1.2 mm was provided between the first terminal row and the second terminal row. As shown in Table 3, the sample of Example 12 was evaluated as OK for bridge generation, with an average solder height of 48.4 μm, a standard deviation of 4.7 μm, and a relative standard deviation of 10%.

[0124] <Example 13> 118 parts by mass of binder was mixed with 690 parts by mass of solder particles to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.4 mm. Anisotropic conductive films having a width of 0.4 mm were temporarily attached to the first terminal row and the second terminal row, respectively, and a gap of 1.6 mm was provided between the first terminal row and the second terminal row. As shown in Table 3, the sample of Example 13 was evaluated as OK for bridge generation, with an average solder height of 49.0 μm, a standard deviation of 8.1 μm, and a relative standard deviation of 17%.

[0125] Fig. 14 is a photograph showing a sample after reflow for Example 13. From the photograph in Fig. 14, it can be seen that there is no solder residue in the void portion, and a solder joint without bridge formation is formed. It can also be seen that a solder joint is formed in a part of the terminal to which the anisotropic conductive film is attached.

[0126] <Comparative Example 6> A 40 μm thick anisotropic conductive film was prepared by mixing 690 parts by mass of solder particles with 118 parts by mass of binder, and then cut to a width of 2.4 mm. A 2.4 mm wide anisotropic conductive film was temporarily attached to the entire surface including the first terminal row and the second terminal row. As shown in Table 3, the sample of Comparative Example 6 was rated as NG for bridge generation, had an average solder height of 88.2 μm, a standard deviation of 28.5 μm, and a relative standard deviation of 32%.

[0127] Fig. 15 is a photograph showing a sample after reflow for Comparative Example 6. From the photograph shown in Fig. 15, it can be seen that solder joints with bridges have been formed. It can also be seen that solder joints have been formed on all of the terminals to which the anisotropic conductive film was attached.

[0128] [Table 3]

[0129] In Comparative Example 6, an anisotropic conductive film was temporarily attached to the entire surface including the first and second terminal rows, which caused bridging and resulted in high standard deviation and relative standard deviation of the solder height. This is believed to be because the solder particles moved between the first and second terminal rows, and the solder particles did not efficiently aggregate on the terminals.

[0130] On the other hand, in Examples 9 to 13, since the anisotropic conductive film was temporarily attached to each of the first and second terminal rows, no bridges were generated, and the standard deviation and relative standard deviation of the solder height were low. In addition, in Examples 10 to 21, the protrusion amount of the rectangular parts in the width direction of the first and second anisotropic conductive films arranged between the first and second terminal rows, respectively, was 25% or less, so that the standard deviation and relative standard deviation of the solder height could be further reduced. This is considered to be due to efficient aggregation of the solder particles to the terminals.

[0131] <5. Third Example> In the third example, an anisotropic conductive film was temporarily attached to a substrate having a first terminal row to a fourth terminal row, and reflow was performed, and the occurrence of bridging and the solder height were evaluated.

[0132] A printed wiring board (the first to fourth terminal rows are arranged in a rectangular shape and wired on the outside, with no terminals inside the rectangle. The first to fourth terminal rows each have a 0.2 mm pitch (line / space = 0.1 / 0.1 mm, terminal length 0.6 mm), 40 pins (8 mm), glass epoxy base material thickness 1.5 mm, copper pattern thickness 18 μm, surface OSP treatment) was prepared as the substrate.

[0133] The anisotropic conductive film was cut to a specified size and temporarily pressed onto the terminals of the substrate at 45°C, 1 MPa, and 1 second. The anisotropic conductive film was temporarily attached to the terminals of the substrate, and reflow was performed under the reflow conditions listed below to produce a sample. Reflow conditions: 150℃~260℃-100sec, peak top 260℃

[0134] [Evaluation of bridge occurrence] After reflow, the insulation resistance of the sample was measured using a digital multimeter when a voltage of 20 V was applied between adjacent terminals. 6 A resistance of Ω or less was counted as the occurrence of solder bridging, and a test result in which no bridging occurred was rated "OK", and a test result in which bridging occurred was rated "NG".

[0135] [Solder height evaluation] The solder height (thickness) on the wiring of the sample after reflow was measured using a 3D measuring laser microscope (Olympus, LEXT OLS5000), and the average value, standard deviation σ, and relative standard deviation (RSD) were calculated.

[0136] [Preparation of anisotropic conductive film] A binder was prepared by mixing 45 parts by mass of phenoxy resin (YP-50, Nippon Steel Chemical & Material Co., Ltd.), 10 parts by mass of hydrogenated bisphenol A glycidyl ether (YX8000, Mitsubishi Chemical Co., Ltd.), 45 parts by mass of crystalline bisphenol A type epoxy resin (YL6810, Mitsubishi Chemical Co., Ltd.), 10 parts by mass of imidazole-based epoxy resin hardener (2P4MHZ-PW (2-phenyl-4-methyl-5-hydroxymethylimidazole), Shikoku Chemical Industry Co., Ltd.), and 8 parts by mass of glutaric acid (1,3-propanedicarboxylic acid, Tokyo Chemical Industry Co., Ltd.). A predetermined amount of solder particles (Sn59.9Bi40Cu0.1) with an average particle size of 20 μm was mixed with 118 parts by mass of the binder to prepare an anisotropic conductive film of a predetermined thickness.

[0137] <Example 14> 204 parts by mass of solder particles were mixed with 118 parts by mass of binder to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.6 mm and a length of 8 mm. Anisotropic conductive films having a width of 0.6 mm were temporarily attached to the first to fourth terminal rows. As shown in Table 4, the sample of Example 14 was evaluated as OK for bridge generation, had an average solder height of 24.5 μm, a standard deviation of 4.0 μm, and a relative standard deviation of 17%.

[0138] <Comparative Example 7> 204 parts by mass of solder particles were mixed with 118 parts by mass of binder to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 9.2 mm and a length of 9.2 mm. An anisotropic conductive film having a size of 9.2 mm×9.2 mm was temporarily attached to the entire surface including the first to fourth terminal rows. As shown in Table 4, the sample of Comparative Example 7 was evaluated as NG for bridge generation, had an average solder height of 17.7 μm, a standard deviation of 6.0 μm, and a relative standard deviation of 34%.

[0139] <Example 15> 225 parts by mass of solder particles were mixed with 118 parts by mass of binder to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 0.6 mm and a length of 8 mm. Anisotropic conductive films having a width of 0.6 mm were temporarily attached to the first to fourth terminal rows. As shown in Table 4, the sample of Example 15 was evaluated as OK for bridge generation, had an average solder height of 26.3 μm, a standard deviation of 4.4 μm, and a relative standard deviation of 17%.

[0140] Fig. 16 is an X-ray photograph showing the sample after reflow for Example 15. From the photograph shown in Fig. 16, it can be seen that there is no solder remaining in the void portion, and a solder joint without bridging has been formed.

[0141] <Comparative Example 8> 225 parts by mass of solder particles were mixed with 118 parts by mass of binder to prepare an anisotropic conductive film having a thickness of 40 μm, which was then cut to a width of 9.2 mm and a length of 9.2 mm. An anisotropic conductive film having a size of 9.2 mm×9.2 mm was temporarily attached to the entire surface including the first to fourth terminal rows. As shown in Table 4, the sample of Comparative Example 8 was evaluated as NG for bridge generation, had an average solder height of 28.1 μm, a standard deviation of 16.1 μm, and a relative standard deviation of 57%.

[0142] Fig. 17 is an X-ray photograph showing the sample after reflow for Comparative Example 8. From the photograph shown in Fig. 17, it can be seen that there is residual solder in the void portion, and a solder joint with bridge generation has been formed.

[0143] [Table 4]

[0144] In Comparative Examples 7 and 8, anisotropic conductive film was temporarily attached to the entire surface including the first to fourth terminal rows, so bridges occurred and the standard deviation and relative standard deviation of the solder height were high. This is thought to be because the solder particles moved between the first and second terminal rows, and the solder particles did not efficiently aggregate on the terminals.

[0145] On the other hand, in Examples 14 and 15, anisotropic conductive films were temporarily attached to the first to fourth terminal rows, respectively, so that no bridging occurred and the standard deviation and relative standard deviation of the solder height were low.

[0146] <6. Fourth Example> In the fourth example, a connection structure was produced using an anisotropic conductive film of a predetermined shape, and solder residue, where solder particles exist outside the terminal portion, was observed and evaluated by X-ray photography.

[0147] [Preparation of anisotropic conductive film] A binder was prepared by mixing 45 parts by mass of phenoxy resin (YP-50, Nippon Steel Chemical & Material Co., Ltd.), 10 parts by mass of hydrogenated bisphenol A glycidyl ether (YX8000, Mitsubishi Chemical Co., Ltd.), 45 parts by mass of crystalline bisphenol A type epoxy resin (YL6810, Mitsubishi Chemical Co., Ltd.), 10 parts by mass of imidazole-based epoxy resin hardener (2P4MHZ-PW (2-phenyl-4-methyl-5-hydroxymethylimidazole), Shikoku Chemical Industry Co., Ltd.), and 8 parts by mass of glutaric acid (1,3-propanedicarboxylic acid, Tokyo Chemical Industry Co., Ltd.). 300 parts by mass of solder particles (Sn59.9Bi40Cu0.1) with an average particle size of 20 μm were mixed with 118 parts by mass of the binder (28 Vol%) to prepare an anisotropic conductive film with a thickness of 30 μm.

[0148] [Fabrication of connection structure] (Plug connector structure) As the substrate, a wiring substrate for a plug connector (a first terminal row and a second terminal row are formed in parallel, and a pair of electrodes are formed at both ends of the first terminal row and the second terminal row at a distance smaller than the distance between the first terminal row and the second terminal row. The distance between the first terminal row and the second terminal row is 0.8 mm. The first terminal row and the second terminal row have a pitch of 0.35 mm (line / space = 0.18 / 0.17 mm, terminal length 0.8 mm), glass epoxy base material thickness 1.5 mm, copper pattern thickness 18 μm, surface OSP treatment) was prepared.

[0149] A plug connector (terminal row 10 pins on one side (20 pins on both sides), 0.35 mmP, line / space = 0.12 / 0.23 mm, 2 pins + 1 pin on both ends on one side, terminal surface Au plated) was prepared.

[0150] (Receptacle connector structure) As the substrate, a wiring board for a receptacle connector (a first terminal row and a second terminal row are formed in parallel, and electrodes spanning between the first terminal row and the second terminal row are formed at both ends of the first terminal row and the second terminal row. The distance between the first terminal row and the second terminal row is 0.8 mm. The first terminal row and the second terminal row have a pitch of 0.35 mm (line / space = 0.18 / 0.17 mm, terminal length 0.8 mm), glass epoxy base material thickness 1.5 mm, copper pattern thickness 18 μm, surface OSP treatment) was prepared.

[0151] The connector prepared was a receptacle connector (10 pins on one side (20 pins on both sides), 0.35 mmP, line / space = 0.12 / 0.23 mm, 2 pins + 1 pin on both ends on one side, Au-plated terminal surface).

[0152] The anisotropic conductive film was cut into a predetermined shape and temporarily pressed onto the terminals of the substrate at 45°C, 1 MPa, and 1 second to temporarily attach the anisotropic conductive film to the terminals of the substrate. Next, a connector (plug connector or receptacle connector) was placed on the anisotropic conductive film of the predetermined shape and reflowed under the following reflow conditions to produce a connection structure.

[0153] Reflow conditions: 150℃~250℃-100sec, peak top set at 250℃, heating rate 3.0℃ / sec

[0154] Figure 18(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape is temporarily attached to a wiring board for a plug connector as comparison example 9, Figure 18(A2) is a plan view showing a schematic shape of the anisotropic conductive film, Figure 18(B) is a photograph showing the state in which a plug connector is reflow-mounted on the wiring board for a plug connector, and Figure 18(C) is an X-ray photograph showing the plug connector structure after mounting.

[0155] As shown in Figures 18(A1) to 18(C), in Comparative Example 9, a rectangular anisotropic conductive film was temporarily attached to the entire surface including the first terminal row, the second terminal row, and the pair of electrodes at both ends, and a plug connector was mounted. As shown in Figures 18(A1) and 18(A2), as a result of using an anisotropic conductive film with no gap between the first terminal row and the second terminal row, solder residue was observed between the first terminal row and the second terminal row in the X-ray photograph shown in Figure 18(C), and also a solder joint with a bridge larger than the terminal width was observed.

[0156] Figure 19(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a plug connector as Example 16, Figure 19(A2) is a plan view showing a schematic view of the shape of the anisotropic conductive film, Figure 19(B) is a photograph showing the state in which a plug connector has been reflow-mounted on a wiring board for a plug connector, and Figure 19(C) is an X-ray photograph showing the plug connector structure after mounting.

[0157] As shown in Figures 19(A1) to 19(C), in Example 16, an anisotropic conductive film having a substantially rectangular first shaped portion 161 corresponding to the first terminal row, a substantially rectangular second shaped portion 162 corresponding to the second terminal row, a third shaped portion 163 that connects one end of the first shaped portion to one end of the second shaped portion 162 and is attached to one longitudinal end of the plug connector, and a fourth shaped portion 164 that connects the other end of the first shaped portion to the other end of the second shaped portion and is attached to the other longitudinal end of the plug connector, was temporarily attached to mount the plug connector.

[0158] As shown in Figures 19(A1) and 19(A2), when an anisotropic conductive film having a gap between the first terminal row and the second terminal row was used, the amount of solder residue was dramatically improved compared to Comparative Example 9, and almost no solder residue was observed in the X-ray photograph shown in Figure 19(C).

[0159] Figure 20(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a plug connector as Example 17, Figure 20(A2) is a plan view showing a schematic shape of the anisotropic conductive film, Figure 20(B) is a photograph showing the state in which a plug connector has been reflow-mounted on a wiring board for a plug connector, and Figure 20(C) is an X-ray photograph showing the plug connector structure after mounting.

[0160] As shown in Figures 20(A1) to 20(C), in Example 17, a first anisotropic conductive film was temporarily attached, the first anisotropic conductive film having a substantially rectangular first shaped portion 171 corresponding to the first terminal row, a second shaped portion 172 that is continuous with one longitudinal end of the first shaped portion 171 and is adapted to bond one longitudinal end of the plug connector, and a third shaped portion 173 that is continuous with the other longitudinal end of the first shaped portion 171 and is adapted to bond the other longitudinal end of the plug connector, and a second anisotropic conductive film was temporarily attached, the fourth anisotropic conductive film having a substantially rectangular fourth shaped portion 174 corresponding to the second terminal row, a fifth shaped portion 175 that is continuous with one longitudinal end of the fourth shaped portion 174 and is adapted to bond one longitudinal end of the plug connector, and a sixth shaped portion 176 that is continuous with the other longitudinal end of the fourth shaped portion 174 and is adapted to bond the other longitudinal end of the plug connector, was temporarily attached, and the plug connector was mounted. In a state in which the first anisotropic conductive film and the second anisotropic conductive film are temporarily attached, the distances between the first shape portion 171 to the third shape portion 173 and the distances between the fourth shape portion 174 to the sixth shape portion 176 are substantially the same.

[0161] As shown in Figures 20(A1) and 20(A2), a first anisotropic conductive film and a second anisotropic conductive film were used that were shaped to bond both longitudinal ends of the plug connector, and a gap was provided between the first anisotropic conductive film and the second anisotropic conductive film.As a result, almost no solder residue was observed in the X-ray photograph shown in Figure 20(C), and in particular, the solder residue at both longitudinal ends of the plug connector was improved.

[0162] Figure 21(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a plug connector as Example 18, Figure 21(A2) is a plan view showing a schematic view of the shape of the anisotropic conductive film, Figure 21(B) is a photograph showing the state in which a plug connector has been reflow-mounted on the wiring board for a plug connector, and Figure 21(C) is an X-ray photograph showing the plug connector structure after mounting.

[0163] As shown in Figures 21(A1) to 21(C), in Example 18, a first anisotropic conductive film was temporarily attached, the first anisotropic conductive film having a substantially rectangular first shaped portion 181 corresponding to the first terminal row, a second shaped portion 182 that is continuous with one longitudinal end of the first shaped portion 181 and is attached to one longitudinal end of the plug connector, and a third shaped portion 183 that is continuous with the other longitudinal end of the first shaped portion 181 and is attached to the other longitudinal end of the plug connector, and a second anisotropic conductive film was temporarily attached, the fourth anisotropic conductive film having a substantially rectangular fourth shaped portion 184 corresponding to the second terminal row, a fifth shaped portion 185 that is continuous with one longitudinal end of the fourth shaped portion 184 and is attached to one longitudinal end of the plug connector, and a sixth shaped portion 186 that is continuous with the other end of the fourth shaped portion 184 and is attached to the other longitudinal end of the plug connector, was temporarily attached, and the plug connector was mounted. When the first anisotropic conductive film and the second anisotropic conductive film are temporarily attached, the distance between the first shape portion 181 and the fourth shape portion 184 is greater than the distance between the second shape portion 182 and the fifth shape portion 185 and the distance between the third shape portion 183 and the sixth shape portion 186.

[0164] As shown in Figures 21(A1) and 21(A2), a first anisotropic conductive film and a second anisotropic conductive film shaped to bond both longitudinal ends of the plug connector were used, and the gap distance between the first shaped portion 181 and the fourth shaped portion 184 was made larger than that of Example 17.As a result, almost no solder residue was observed in the X-ray photograph shown in Figure 21(C), and in particular, the solder residue in the first terminal row and the second terminal row was improved.

[0165] Figure 22(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a receptacle connector as comparison example 10, Figure 22(A2) is a plan view showing a schematic view of the shape of the anisotropic conductive film, Figure 22(B) is a photograph showing the state in which a receptacle connector has been reflow-mounted on the wiring board for a receptacle connector, and Figure 22(C) is an X-ray photograph showing the receptacle connector structure after mounting.

[0166] As shown in Figures 22(A1) to 22(C), in Comparative Example 10, a rectangular anisotropic conductive film was temporarily attached to the entire surface of the receptacle connector, including both longitudinal ends, and the receptacle connector was then mounted. As shown in Figures 22(A1) and 22(A2), when an anisotropic conductive film with no gap between the first terminal row and the second terminal row was used, solder residue was observed between the first terminal row and the second terminal row in the X-ray photograph shown in Figure 22(C), and a solder joint with a bridge larger than the terminal width was also observed.

[0167] Figure 23(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a receptacle connector as Example 19, Figure 23(A2) is a plan view showing a schematic view of the shape of the anisotropic conductive film, Figure 23(B) is a photograph showing the state in which a receptacle connector has been reflow-mounted on the wiring board for a receptacle connector, and Figure 23(C) is an X-ray photograph showing the receptacle connector structure after mounting.

[0168] As shown in Figures 23(A1) to 23(C), in Example 19, an anisotropic conductive film having a rectangular gap having a width greater than the distance between the first terminal row and the second terminal row and the length of the terminal row portion of the receptacle connector was temporarily attached to the center of a rectangle including both longitudinal ends of the receptacle connector, and the receptacle connector was mounted.

[0169] As shown in Figures 23(A1) and 23(A2), when an anisotropic conductive film having a gap between the first terminal row and the second terminal row was used, the amount of solder residue was dramatically improved compared to Comparative Example 10, and almost no solder residue was observed in the X-ray photograph shown in Figure 23(C).

[0170] Figure 24(A1) is a photograph showing the state in which an anisotropic conductive film of a predetermined shape has been temporarily attached to a wiring board for a receptacle connector as Example 20, Figure 24(A2) is a plan view showing a schematic view of the shape of the anisotropic conductive film, Figure 24(B) is a photograph showing the state in which a receptacle connector has been reflow-mounted on the wiring board for a receptacle connector, and Figure 24(C) is an X-ray photograph showing the receptacle connector structure after mounting.

[0171] As shown in Figs. 24(A1) to 24(C), in Example 20, a first anisotropic conductive filter includes a first shaped portion 201 having a substantially rectangular shape corresponding to a first terminal row, a second shaped portion 202 that is continuous with one end of the first shaped portion 201 in the longitudinal direction and to which one end of the receptacle connector in the longitudinal direction is bonded, and a third shaped portion 203 that is continuous with the other end of the first shaped portion 201 in the longitudinal direction and to which the other end of the receptacle connector in the longitudinal direction is bonded. The first anisotropic conductive film was temporarily attached, and a second anisotropic conductive film having a substantially rectangular fourth shaped portion 204 corresponding to the second terminal row, a fifth shaped portion 205 that is continuous with one end of the fourth shaped portion 204 in the longitudinal direction and to which one end of the receptacle connector in the longitudinal direction is bonded, and a sixth shaped portion 206 that is continuous with the other end of the fourth shaped portion 204 and to which the other end of the receptacle connector in the longitudinal direction is bonded was temporarily attached, thereby mounting the receptacle connector. In a state in which the first anisotropic conductive film and the second anisotropic conductive film are temporarily attached, the distance between the first shaped portion 201 and the fourth shaped portion 204 is greater than the distance between the second shaped portion 202 and the fifth shaped portion 205 and the distance between the third shaped portion 203 and the sixth shaped portion 206.

[0172] As shown in Figures 24(A1) and 24(A2), a first anisotropic conductive film and a second anisotropic conductive film were used that were shaped to bond both longitudinal ends of the receptacle connector, and a gap was provided between the first anisotropic conductive film and the second anisotropic conductive film.As a result, almost no solder residue was observed in the X-ray photograph shown in Figure 24(C), and in particular, the solder residue at both longitudinal ends of the receptacle connector was improved. [Explanation of symbols]

[0173] 10 wiring board, 11 first terminal row, 11a terminal, 12 second terminal row, 12a terminal, 20 solder particles, 21 first solder connection film, 22 second solder connection film, 30 surface mount component, 31 first terminal row, 32 second terminal row, 40 binder, 41 solder, 50 wiring board, 51 first terminal row, 51a to 51d terminal, 52 second terminal row, 52a to 52d terminal, 53 metal mask, 54 first opening, 55 second opening, 556 first solder paste film, 57 second solder paste film, 58 metal mask, 59 opening, 60 solder paste film, 61 metal mask, 62a to 62d opening, 63a to 63d opening, 64a to 64d Solder paste film, 65a to 65d solder paste film 70 receptacle, 71A, 71B receptacle terminal, 80 plug, 81A, 81B plug terminal, 82A, 82B connection pin, 83 insulating resin, 90 wiring board, 91A, 91B board terminal, 100 adhesive layer, 101 solder, 102 binder hardened product

Claims

1. a placement step of placing a surface mount component having a plurality of terminal rows on a wiring board via a film-like solder connection material having rectangular portions corresponding to each of the terminal rows; a bonding step of bonding the surface mount component to the wiring board; A method for manufacturing a connection structure having the above structure.

2. 2. The method for manufacturing a connection structure according to claim 1, wherein a relative standard deviation of the solder thickness between the terminal of the surface mount component and the terminal of the wiring board after the joining step is less than 25%.

3. the surface mount component includes a first terminal row and a second terminal row arranged in parallel; 3. A method for manufacturing a connection structure as described in claim 1 or 2, wherein in the arrangement process, a first film-like solder connection material corresponding to the first terminal row and a second film-like solder connection material corresponding to the second terminal row are arranged, and the distance between the rectangular portion in the first film-like solder connection material and the rectangular portion in the second film-like solder connection material is set to 0 mm or more.

4. the surface mount component includes a first terminal row and a second terminal row arranged in parallel; The method for manufacturing a connection structure described in claim 3, wherein, in the arrangement process, the width W of the rectangular portion in the first film-shaped solder connection material and the width W of the rectangular portion in the second film-shaped solder connection material satisfy the following formula (1). W≦(2L+S) / 2 (1) In the above formula (1), L is the length of the terminals in the first terminal row and the second terminal row, and S is the distance between the first terminal row and the second terminal row.

5. 3. The method for manufacturing a connection structure according to claim 1, wherein in the bonding step, the surface mount component is bonded to the wiring board without load using a reflow furnace.

6. 3. The method for manufacturing a connection structure according to claim 1, wherein the pitch of the terminal rows of the surface mount components and the wiring board is 0.1 mm to 0.4 mm.

7. 3. The method for manufacturing a connection structure according to claim 1 or 2, wherein the content of solder particles in the film-like solder connection material is 10% by volume to 60% by volume for a pitch of 0.1 mm to 0.4 mm of the terminal rows of the surface mount components and the wiring board.

8. the surface mount component includes a first terminal row and a second terminal row arranged in parallel; In the arranging step, a first film-like solder connecting material corresponding to the first terminal row and a second film-like solder connecting material corresponding to the second terminal row are arranged; 3. A method for manufacturing a connection structure as described in claim 1 or 2, wherein the widthwise protrusion amount of the rectangular portion of the first film-like solder connection material relative to the first terminal row is 50% or less of the terminal length of the first terminal row, and the widthwise protrusion amount of the rectangular portion of the second film-like solder connection material relative to the second terminal row is 50% or less of the terminal length of the second terminal row.

9. the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and a third terminal row and a fourth terminal row arranged in parallel and perpendicular to the first terminal row and the second terminal row, 3. The method for manufacturing a connection structure according to claim 1 or 2, wherein the amount of protrusion in the width direction of the rectangular portion corresponding to the first terminal row, the second terminal row, the third terminal row or the fourth terminal row from the terminal row is 50% or less of the terminal length of the corresponding first terminal row, the second terminal row, the third terminal row or the fourth terminal row.

10. A connection structure comprising: a surface mount component having a plurality of terminal rows; a wiring board; and a cured film of a film-like solder connecting material provided for each of the terminal rows, joining the surface mount component and the wiring board, the film having a rectangular portion corresponding to each of the terminal rows.

11. 11. The connection structure according to claim 10, wherein the relative standard deviation of the solder thickness between the terminal of the surface mount component and the terminal of the wiring board is less than 25%.

12. 12. The connection structure according to claim 10, wherein the pitch of the terminal rows of the surface mount component and the wiring board is 0.1 mm to 0.4 mm.

13. the surface mount component includes a first terminal row and a second terminal row arranged in parallel; A connection structure as described in claim 10 or 11, wherein the widthwise protrusion amount of the rectangular portion of the first film-like solder connection material relative to the first terminal row is 50% or less of the terminal length of the first terminal row, and the widthwise protrusion amount of the rectangular portion of the second film-like solder connection material relative to the second terminal row is 50% or less of the terminal length of the second terminal row.

14. the surface mount component comprises a first terminal row and a second terminal row arranged in parallel, and a third terminal row and a fourth terminal row arranged in parallel and perpendicular to the first terminal row and the second terminal row, 12. A connection structure as described in claim 10 or 11, wherein the amount of widthwise protrusion of the rectangular portion corresponding to the first terminal row, the second terminal row, the third terminal row or the fourth terminal row from the terminal row is 50% or less of the terminal length of the corresponding first terminal row, the second terminal row, the third terminal row or the fourth terminal row.

Citation Information

Patent Citations

  • Method for manufacturing connection structure

    JP2016219808A

  • Conductive material and connection structure

    JP2017041442A

  • Adhesive tape, joint structure, and semiconductor package

    WO2008023452A1