Moisture-curable polyurethane hot melt adhesive composition

The formulation of a moisture-curable polyurethane hot melt adhesive with specific polyol and polyisocyanate components, along with a (meth)acrylic polymer and amorphous polyalphaolefin, addresses the lack of strength and impact resistance in existing adhesives, enabling effective bonding in electronic applications.

JP2024536120AActive Publication Date: 2024-10-04HENKEL KGAA
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024519087
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-09-28
Publication Date
2024-10-04
Estimated Expiration
2041-09-28

AI Technical Summary

Technical Problem

Existing moisture-curable polyurethane hot melt adhesives lack sufficient initial cross-tensile strength and impact resistance, making them unsuitable for structural bonding, particularly in electronic applications that require fast curing.

Method used

A moisture-curable polyurethane hot melt adhesive composition comprising a polyol mixture of polyester and polyether polyols, a polyisocyanate with at least two isocyanate groups, a (meth)acrylic polymer, and an amorphous polyalphaolefin with a softening point below 100°C, formulated to achieve high initial cross-tensile strength and excellent impact resistance.

Benefits of technology

The adhesive composition exhibits superior initial cross-tensile strength and impact resistance, suitable for bonding diverse substrates including glass, resin, and metal, particularly in electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536120000001
    Figure 2024536120000001
  • Figure 2024536120000002
    Figure 2024536120000002
  • Figure 2024536120000003
    Figure 2024536120000003
Patent Text Reader

Abstract

The present invention provides at least one polyurethane prepolymer obtained by reacting a reactant mixture comprising: (A) (A1) a polyol mixture comprising: (a) at least one polyester polyol; and (b) at least one polyether polyol; and (A2) at least one polyisocyanate having at least two isocyanate groups in one molecule; (B) at least one (meth)acrylic polymer present in an amount of 14% by weight or less, based on the total weight of the adhesive composition; and (C) at least one amorphous polyalphaolefin having a softening point less than 100° C., present in an amount of 20% by weight or less, based on the total weight of the adhesive composition; The present invention provides a moisture-curable polyurethane hot melt adhesive composition comprising:
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Technical Field The present invention relates to a moisture-curable polyurethane hot melt adhesive composition, a cured product thereof, and uses thereof. [Background technology]

[0002] 2. Background of the Invention Polyurethane hot melt adhesives have a long history and are widely used. In the context of industrial applications, polyurethane hot melt adhesives are solid at room temperature and melt into a viscous liquid when heated to a moderate temperature and applied to the substrate to be bonded. The molten adhesive composition then cools and solidifies, forming an initial bond with the substrate. It can further react with moisture to form crosslinked structures and achieve high final strength. Such adhesives consist of a polyol component and a difunctional or higher isocyanate component. These adhesives are preferred over other adhesives in many applications due to their excellent adhesive strength, flexibility, impact resistance, and fatigue resistance.

[0003] Although polyurethane hot melt adhesives have excellent adhesive strength in many fields of application, the adhesives known so far are not suitable for structural bonding of plastic and metal workpieces because they do not have sufficient impact toughness, and it is difficult for the cured adhesive to simultaneously achieve high initial tensile cross strength and good impact resistance, especially for the manufacture of electronic applications that require fast curing. This is probably because a large amount of crystalline polyester polyol is required to create high initial cross tensile strength, which reduces the impact resistance of the adhesive when cured. Summary of the Invention [Problem to be solved by the invention]

[0004] In view of the above, there remains a need for moisture-curable polyurethane hot melt adhesives that upon cure exhibit high initial cross tensile strength and excellent impact resistance. [Means for solving the problem]

[0005] Summary of the Invention According to a first aspect of the present invention, disclosed herein is a moisture-curable polyurethane hot melt adhesive composition comprising: (A) at least one polyurethane prepolymer obtained by reacting a reactant mixture comprising: (A1) A polyol mixture containing: (a) at least one polyester polyol, and (b) at least one polyether polyol, and (A2) at least one polyisocyanate having at least two isocyanate groups in one molecule; (B) at least one (meth)acrylic polymer present in an amount of 14% by weight or less, based on the total weight of the adhesive composition; and (C) at least one amorphous polyalphaolefin having a softening point less than 100° C., present in an amount of 20% by weight or less, based on the total weight of the adhesive composition.

[0006] According to a second aspect of the present invention, there is provided a method for preparing a moisture-curable polyurethane hot melt adhesive composition.

[0007] According to a third aspect of the present invention, provided herein is a laminate comprising a first substrate, a second substrate, and an adhesive layer sandwiched therebetween, wherein the first substrate and the second substrate are independently selected from glass, resin, and metal, and the adhesive layer is formed by curing an adhesive composition of the present invention.

[0008] According to a fourth aspect of the present invention, provided herein is an electronic device comprising a laminate of the present invention or manufactured using an adhesive composition according to the present invention.

[0009] According to a fifth aspect of the present invention, provided herein is the use of an adhesive composition according to the present invention or a laminate according to the present invention in the manufacture of an electronic device.

[0010] Other features and aspects of the subject matter are discussed in more detail below. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Detailed Description of the Invention Those skilled in the art should appreciate that the present invention has been described with reference to exemplary embodiments only, and is not intended to limit the broad scope of the present invention. Each aspect thus described may be combined with other aspects, unless expressly indicated to the contrary. In particular, any feature indicated as being preferred or advantageous may be combined with any other feature or features indicated as being preferred or advantageous.

[0012] Unless otherwise specified, in the context of the present invention, the terms used shall be construed in accordance with the following definitions.

[0013] As used herein, unless otherwise stated, the terms "a," "an," and "the" include singular and plural references.

[0014] As used herein, the terms "comprising" and "comprises" are synonymous with "including," "includes," or "containing," and "contains," and are inclusive or open-ended and do not exclude additional, unlisted members, elements, or process steps.

[0015] The terms "at least one" or "one or more" as used herein to define a component refer to the type of component and not the absolute number of molecules. For example, "one or more polyols" refers to one type of polyol or a mixture of multiple different polyols.

[0016] As used herein, the term "amorphous" means the absence of a melting transition as measured using differential scanning calorimetry (DSC).

[0017] As used herein, the term "crystalline" means having a melting transition as measured using differential scanning calorimetry (DSC).

[0018] As used herein, the term "room temperature" refers to a temperature of about 20°C to about 25°C, preferably about 25°C.

[0019] Unless otherwise specified, the recitation of numerical endpoints includes all numbers and fractions subsumed within the respective ranges, as well as the recited endpoints.

[0020] All documents cited herein are incorporated by reference in their entirety.

[0021] Molecular weights refer to number average molecular weights (Mn) unless otherwise stated. All molecular weight data refer to values ​​obtained by gel permeation chromatography (GPC), unless otherwise specified, e.g. according to DIN 55672.

[0022] In this context, the glass transition temperature (Tg) or melting point of a particular polymer is determined using DSC in accordance with DIN 53 765.

[0023] The softening points referred to in this specification are determined using the ring and ball method in accordance with DIN ISO 4625.

[0024] Unless otherwise defined, all terms used herein, including technical and scientific terms, have the meaning commonly understood by one of ordinary skill in the art to which this invention belongs.

[0025] In one aspect, the present disclosure is generally directed to a moisture-curable polyurethane hot melt adhesive composition comprising: (A) at least one polyurethane prepolymer obtained by reacting a reactant mixture comprising: (A1) A polyol mixture comprising: (a) at least one polyester polyol, and (b) at least one polyether polyol; and (A2) at least one polyisocyanate having at least two isocyanate groups per molecule; (B) at least one (meth)acrylic polymer present in an amount of 14% by weight or less, based on the total weight of the adhesive composition; and (C) at least one amorphous polyalphaolefin having a softening point less than 100° C., present in an amount of 20% by weight or less, based on the total weight of the adhesive composition.

[0026] (A) Polyurethane prepolymer According to the present invention, the moisture-curable polyurethane hot melt adhesive composition comprises: (A1) a polyol mixture comprising: (a) at least one polyester polyol; and (b) at least one polyether polyol; and (A2) at least one polyisocyanate having at least two isocyanate groups in one molecule. The polyurethane prepolymer comprises at least one polyurethane prepolymer obtained by reacting a reactant mixture comprising:

[0027] In some embodiments, the polyurethane prepolymer has a number average molecular weight (Mn) of 5,000 to 30,000 g / mol, preferably 8,000 to 20,000 g / mol.

[0028] In some embodiments, component (A) is preferably present in an amount of from 66% to 99% by weight, more preferably from 70% to 90% by weight, based on the total weight of the adhesive composition.

[0029] (A1) Polyol mixture In some embodiments, the polyol mixture (A1) used in the present invention comprises (a) at least one polyester polyol (a).

[0030] (a) Polyester polyol The polyester polyol used in the present invention can be selected from solid polyester polyols, liquid polyester polyols, and combinations thereof. The solid polyester polyols can be crystalline polyester polyols, amorphous polyester polyols, or combinations thereof.

[0031] In some embodiments, crystalline polyester polyols can be used in the present invention that can provide good adhesive strength to the adhesive composition.

[0032] Examples of such crystalline polyester polyols include those obtained by ring-opening polymerization of lactones such as ε-caprolactone, and / or those obtained from diols and diacids. Examples of diols useful in preparing preferred polyester polyols include ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and combinations thereof. Examples of diacids useful in preparing preferred polyester polyols include succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,12-dodecanedioic acid, dimer acid, and combinations thereof. Included in the range of useful diacids are various diacid derivatives such as carboxylic acid esters (especially methyl esters and ethyl esters), acid halides (such as acid chlorides), acid anhydrides, and combinations thereof.

[0033] Specific examples of suitable crystalline polyester polyols include poly(hexanediol adipate) polyol, poly(butanediol adipate) polyol, poly-epsilon-caprolactone polyol, poly(dodecanedioic acid hexanediol) polyol, poly(hexanediol adipate terephthalate) polyol, and combinations thereof.

[0034] Suitable commercially available crystalline polyester polyols are sold under the DYNACOLL 7300 series by Evonik Industries AG, which includes DYNACOLL 7360, 7361, 7362, 7363, 7380, 7390, and the like, and the CAPA series by Perstorp Polyols Inc., which includes caprolactone polyols such as CAPA 2201, 2205, 2209, 2302, 2304, 2402, and the like.

[0035] In some embodiments, amorphous polyester polyols can also be used in preparing the polyurethane prepolymers of the present invention.

[0036] The amorphous polyester polyol comprises a reaction product of a polyacid component (e.g., a polyacid, a polyanhydride, a polyacid ester, a polyacid halide) with a stoichiometric excess of a polyol. At least one of the polyacid component and the polyol comprises an aromatic group. Suitable polyacids include, for example, diacids (e.g., dicarboxylic acids), triacids (e.g., tricarboxylic acids), and higher acids, including aromatic dicarboxylic acids, their anhydrides and esters (e.g., terephthalic acid, isophthalic acid, dimethyl terephthalate, diethyl terephthalate, phthalic acid, phthalic anhydride, methyl-hexahydrophthalic acid, methyl-hexahydrophthalic anhydride, methyl-tetrahydrophthalic acid, methyl-tetrahydrophthalic anhydride, hexahydrophthalic acid, hexahydrophthalic anhydride, tetrahydrophthalic acid, etc.). , aliphatic dicarboxylic acids and their anhydrides (e.g., maleic acid, maleic anhydride, succinic acid, succinic anhydride, glutaric acid, glutaric anhydride, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, chlorendic acid, 1,2,4-butanetricarboxylic acid, decanedicarboxylic acid, octadecanedicarboxylic acid, dimer acid, dimerized fatty acid, trimer fatty acid, fumaric acid), and alicyclic dicarboxylic acids (e.g., 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, etc.), and mixtures thereof.Examples of suitable polyols include aliphatic polyols, such as ethylene glycol, propanediol (e.g., 1,2-propanediol, 1,3-propanediol, etc.), butanediol (e.g., 1,3-butanediol, 1,4-butanediol, 1,2-butanediol, etc.), 1,3-butenediol, 1,4-butenediol, 1,4-butynediol, pentanediol (e.g., 1,5-pentanediol), pentenediol, pentynediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, neopentyl glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, glycol, polyethylene glycol, propylene glycol, polypropylene glycol (e.g., dipropylene glycol and tripropylene glycol), 1,4-cyclohexanedimethanol, 1,4-cyclohexanediol, dimer diol, bisphenol A, bisphenol F, hydrogenated bisphenol A, hydrogenated bisphenol F, glycerol, tetramethylene glycol, polytetramethylene glycol, 3-methyl-1,5-pentanediol, 1,9-nonanediol, 2-methyl-1,8-octanediol, trimethylolpropane, pentaerythritol, sorbitol, glucose, and combinations thereof.

[0037] Specific examples of useful amorphous polyester polyols, when present, include poly(hexanediol phthalate) polyol, poly(neopentyl glycol adipate) polyol, poly(neopentyl glycol phthalate) polyol, poly(neopentyl glycol hexanediol phthalate) polyol, poly(diethylene glycol phthalate) polyol, poly(ethylene glycol adipate terephthalate) polyol, polyethylene terephthalate polyol, ethylene glycol, hexanediol, neopentyl glycol, random copolymer diols of adipic acid and terephthalic acid, and combinations thereof.

[0038] Useful amorphous polyester polyols are commercially available under a variety of trade names, including, for example, DYNACOLL 7110, 7130, 7140 and 7150 from Evonik Industries AG, and FLP PA-1000N from Xu Chuan Chemical (Suzhou) Co., Ltd.

[0039] In some embodiments, the polyester polyol used in the present invention can be liquid at room temperature, which provides wettability to the adhesive composition and impact resistance to the cured product. Therefore, the liquid polyester polyol preferably has a glass transition temperature (Tg) of 0° C. or less. If the Tg of the liquid polyester polyol is too high, it becomes difficult to be liquid.

[0040] Examples of suitable liquid polyester polyols include those obtained by ring-opening polymerization of lactones such as ε-caprolactone and / or those obtained from diols and diacids. Examples of diols useful in preparing preferred polyester polyols include ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and combinations thereof. Examples of diacids useful in preparing preferred polyester polyols include succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,12-dodecanedioic acid, dimer acid, and combinations thereof. Included in the range of useful diacids are various diacid derivatives such as carboxylic acid esters (especially methyl esters and ethyl esters), acid halides (such as acid chlorides), acid anhydrides, and combinations thereof.

[0041] Specific examples of suitable liquid polyester polyols include poly(hexanediol adipate) polyol, poly(butanediol adipate) polyol, poly-epsilon-caprolactone polyol, poly(dodecanedioic acid hexanediol) polyol, poly(hexanediol adipate terephthalate) polyol, and mixtures thereof.

[0042] Suitable commercially available liquid polyester polyols are sold under trade names such as DYNACOLL 7210, 7230, 7231, 7250, and the DYNACOLL 7200 series by Evonik Industries AG; and Stepan PDP 70 by Stepan Corporation.

[0043] Preferably, a combination of at least one crystalline polyester polyol, at least one amorphous polyester polyol and at least one liquid polyester polyol can be used as reactant (a) in the present invention.

[0044] In a preferred embodiment, reactant (a) has a number average molecular weight (Mn) of 800 to 20,000 g / mol, preferably 1,000 to 10,000 g / mol, more preferably 1,000 to 5,000 g / mol.

[0045] Particularly preferably, reactant (a) may be present in an amount of from 30% to 70% by weight, more preferably from 35% to 65% by weight, based on the total weight of the adhesive composition.

[0046] (b) Polyether polyol In some embodiments, the polyol mixture (A1) used in the present invention comprises (b) at least one polyether polyol.

[0047] The polyether polyols used in the present invention are well known to those skilled in the art.These polyether polyols are obtained by copolymerizing at least one compound, such as ethylene oxide, propylene oxide, butylene oxide, tetrahydrofuran, and at least one compound having at least two active hydrogen atoms in average in one molecule, such as the above polyhydric alcohols, including ethylene glycol, propylene glycol, dipropylene glycol, glycerol, and combinations thereof.Other suitable polyhydric compounds include sucrose, ethylenediamine, propylenediamine, triethanolamine, 1,2-propanedithiol, and combinations thereof.

[0048] Preferred polyether polyols can be selected from polytetramethylene ether glycol, poly(oxypropylene) glycol, polyethylene oxide, polybutylene oxide, and ethylene oxide end-capped versions of any of the foregoing, and combinations thereof. Most preferred polyether polyols are polytetramethylene ether glycol, poly(oxypropylene) glycol, ethylene oxide end-capped poly(oxypropylene) glycol, and combinations thereof.

[0049] In a preferred embodiment, the polyether polyol has a number average molecular weight (Mn) of 200 to 8,000 g / mol, preferably 400 to 4,000 g / mol, more preferably 400 to 2,000 g / mol.

[0050] Commercially available products may be used in the present invention, examples of which include Voranol 2104, 2110, 2120, and 2140 from The Dow Chemical Company.

[0051] Particularly preferably, reactant (b) may be present in an amount of from 10% to 40% by weight, more preferably from 15% to 36% by weight, based on the total weight of the adhesive composition.

[0052] (A2) Polyisocyanate The moisture-curable polyurethane hot melt adhesive composition comprises (A1) a polyol mixture comprising: (a) at least one polyester polyol, and (b) at least one polyether polyol, and (A2) at least one polyisocyanate having at least two isocyanate groups per molecule. The polyurethane prepolymer comprises at least one polyurethane prepolymer obtained by reacting a reactant mixture comprising:

[0053] Polyisocyanates useful as reactant (A2) include any suitable isocyanate having at least two isocyanate groups per molecule, including, for example, aliphatic, cycloaliphatic, araliphatic, arylalkyl, aromatic isocyanates, and combinations thereof.

[0054] Preferred reactants (A2) are 4,4-diphenylmethane diisocyanate (MDI), hydrogenated MDI (H12MDI), partially hydrogenated MDI (H6MDI), xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), 4,4-diphenyldimethylmethane diisocyanate, dialkylenediphenylmethane diisocyanate, tetraalkylenediphenylmethane diisocyanate, 4,4-dibenzyl Diisocyanates, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, isomers of toluylene diisocyanate (TDI), 1-methyl-2,4-diisocyanatocyclohexane, 1,6-diisocyanato-2,2,4-trimethylhexane, 1,6-diisocyanato-2,4,4-trimethylhexane, 1-isocyanatomethyl-3-isocyanato-1,5,5-trimethylcyclohexane (IPDI), tetraisocyanatomethyl-3-isocyanato-1,5,5-trimethylcyclohexane (T ... Methoxybutane-1,4-diisocyanate, Naphthalene-1,5-diisocyanate (NDI), Butane-1,4-diisocyanate, Hexane-1,6-diisocyanate (HDI), Dicyclohexylmethane diisocyanate, 2,2,4-trimethylhexane-2,3,3-trimethylhexamethylene diisocyanate, Cyclohexane-1,4-diisocyanate, Ethylene diisocyanate, Methylenetriphenyl triisocyanate The polyisocyanate may be selected from the group consisting of bisisocyanatoethyl ester (MIT), phthalic acid, trimethylhexamethylene diisocyanate, 1,4-diisocyanatobutane, 1,12-diisocyanatododecane, and dimer fatty acid diisocyanates, lysine ester diisocyanates, 4,4-dicyclohexylmethane diisocyanate, 1,3-cyclohexane or 1,4-cyclohexane diisocyanate, and combinations thereof. The most preferred polyisocyanates are 4,4-diphenylmethane diisocyanate (MDI) and its isomers, chain extended MDI, and combinations thereof.

[0055] Useful commercially available polyisocyanates for use as reactant (A2) include DESMODUR 44C FUSED from Bayer, Desmodur 0118 I and Desmodur 44M from Covestro, Vannate MDI 100F from Wanhua Chemicals, Supresec 1809 from HUNTSMAN.

[0056] Particularly preferably, the reactant (A2) may be present in an amount of 10% to 25% by weight, preferably 10% to 20% by weight, based on the total weight of the adhesive composition.

[0057] (B) (Meth)acrylic polymer According to the present invention, the moisture-curable polyurethane hot melt adhesive composition comprises (B) at least one (meth)acrylic polymer in an amount of 14 wt. % or less, based on the total weight of the adhesive composition, which imparts to the adhesive composition excellent initial cross tensile strength when cured. The (meth)acrylic polymers used as component (B) in the present invention may be linear or branched and may consist of copolymerized alkyl-, acid-, or tertiary amine-functional (meth)acrylic monomers and may contain other functional groups that do not react rapidly with isocyanate functionality. Branching of the (meth)acrylic polymers can be induced by copolymerizing polyfunctional comonomers and / or by using polyfunctional chain transfer agents and / or polyfunctional initiators.

[0058] Suitable comonomers used to form the (meth)acrylic polymers of the present invention include, but are not limited to, C1-C12 esters of methacrylic and acrylic acids such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, n-hexyl methacrylate, n-octyl methacrylate, 2-ethylhexyl methacrylate, dodecyl (lauryl) methacrylate or the corresponding acrylates. Mixtures of compatible (meth)acrylate monomers can also be used. Methacrylic and acrylic comonomers based on esters of methacrylic and acrylic acids with poly(ethylene glycol) and / or poly(propylene glycol) and / or glycol ethers can also be used. Other vinyl comonomers that can be used include vinyl esters (vinyl acetate, vinyl propionate, etc.); vinyl ethers; esters of crotonic, maleic, fumaric, itaconic acid; styrene; alkyl styrenes; acrylonitrile; butadiene; and the like, and their comonomers. The particular monomer selected will depend largely on the end use for which the adhesive is intended.

[0059] Suitable acid-functional comonomers for use in forming the (meth)acrylic polymers of the present invention include, but are not limited to, methacrylic acid and acrylic acid.

[0060] Suitable hydroxyl-functionalized comonomers used to form the (meth)acrylic polymers of the present invention that can be incorporated include, but are not limited to, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, and 2-hydroxybutyl methacrylate or the corresponding acrylates.

[0061] Suitable amine-functionalized comonomers for use in forming the (meth)acrylic polymers of the present invention include, but are not limited to, dimethylaminoethyl methacrylate, diethylaminoethyl methacrylate, or the corresponding acrylates.

[0062] Component (B) can be prepared by free radical polymerization, with the molecular weight (Mn) being controlled by using chain transfer agents, e.g. catalytic chain transfer agents based on thiols or transition metal complexes, such as dodecyl mercaptan. Branched (meth)acrylic polymers are produced by copolymerizing polyfunctional monomers and / or by using polyfunctional chain transfer agents and / or by using polyfunctional initiators.

[0063] In a preferred embodiment, component (B) has a number average molecular weight (Mn) of 5,000 to 100,000 g / mol, preferably 5,000 to 80,000 g / mol, and more preferably 8,000 to 50,000 g / mol.

[0064] Useful components (B) are commercially available, for example Elvacite 2013 from Lucite International.

[0065] According to the invention, the (meth)acrylic polymer must be present in an amount of not more than 14% by weight, based on the total weight of the adhesive composition, otherwise a high content of (meth)acrylic polymer would be insoluble in the adhesive composition. Particularly preferably, component (B) can be present in an amount of 0.1% to 12% by weight, preferably 1% to 10% by weight, based on the total weight of the adhesive composition.

[0066] (C) Amorphous polyalphaolefin According to the present invention, the moisture-curable polyurethane hot melt adhesive composition comprises (C) at least one amorphous polyalphaolefin having a softening point of less than 100°C in an amount of 20% by weight or less, based on the total weight of the adhesive composition, which, when cured, imparts excellent initial cross tensile strength to the adhesive composition of the present invention.

[0067] According to the present invention, component (C) has a softening point of less than 100°C, which is equal to or lower than the reaction temperature when preparing the adhesive composition of the present invention. If the softening point of the amorphous polyalphaolefin is 100°C or higher, the amorphous polyalphaolefin precipitates during the reaction and forms granules in the adhesive composition. In a preferred embodiment, component (C) used in the present invention has a softening point of 70°C to 95°C.

[0068] In some embodiments, component (C) has a molecular weight (Mn) of less than 200,000 g / mol, preferably less than 100,000 g / mol.

[0069] In some embodiments, component (C) has a Brookfield viscosity at 190° C. of 50,000 mPa·s or less, preferably less than 30,000 mPa·s.

[0070] Useful amorphous polyalphaolefins used as component (C) in the present invention include polyalphaolefin homopolymers, copolymers, terpolymers, and combinations thereof. The amorphous polyalphaolefins used as component (C) may be random or block copolymers. The amorphous polyalphaolefins may be derived from various monomers, including, for example, propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 3-methyl-1-pentene, 4-methyl-1-pentene, 3-ethyl-1-pentene, 1-octene, 1-decene, 1-undecene, and combinations thereof.

[0071] Useful components (C) are commercially available as Vestoplast 508 and Vestoplast 520 from Evonik Industrials.

[0072] According to the present invention, component (C) is present in an amount of 20% by weight or less based on the total weight of the adhesive composition. In a preferred embodiment, component (C) used in the present invention is present in an amount of 1% by weight to 15% by weight, preferably 1% by weight to 8% by weight, based on the total weight of the adhesive composition. The use of component (C) having an amount in the above range is advantageous because such an amount of component (C) can impart excellent impact resistance performance to the adhesive composition while not reducing the initial cross tensile strength of the adhesive composition when cured.

[0073] (D)Catalyst Optionally, the moisture-curable polyurethane hot melt adhesive composition may also contain a catalyst (D) for promoting the reaction between (A1) the polyol and (A2) the polyisocyanate having at least two isocyanate groups per molecule.

[0074] Suitable components (D) are, for example, strongly basic amides, such as 2,3-dimethyl-3,4,5,6-tetrahydropyrimidine, tris-(dialkylaminoalkyl)-s-hexahydrotriazines, such as tris-(NN-dimethylaminopropyl)-s-hexahydrotriazine, or conventional tertiary amines, such as triethylamine, tributylamine, dimethylbenzylamine, N-ethyl-, N-methyl-, N-cyclohexylamine, dimethylcyclohexylamine, dimorpholinodiethyl ether, 2-(dimethylaminoethoxy)-ethanol, 1,4-diazabicyclo[2,2,2]octane, 1-azabicyclo[3,3,0]octane, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylbutanediamine, N,N,N',N'-tetramethylhexane-1,6-diamine, pentamethyldiethylenetriamine, tetramethyl dialkyltin(IV) dilaurate, dibutyltin(IV) dilaurate, dibutyltin(IV) maleate or dioctyltin(IV) diacetate, dibutyltin(IV) dimercaptide, or mixtures of two or more of the mentioned catalysts, and synergistic combinations of strongly basic amines and organometallic compounds.

[0075] When present, the catalyst is present in the adhesive composition in an amount of from 0.05% to 1% by weight, preferably from 0.05% to 0.5% by weight, based on the total weight of the adhesive composition.

[0076] (E) Additives Optionally, the moisture-curable polyurethane hot melt adhesive composition may contain at least one additive, such as colorants, antioxidants, and the like, which are commonly used in the art.

[0077] Examples of colorants include pigments that may be selected from metal oxide pigments, titanium dioxide, optionally surface-treated zirconium oxide or cerium oxide, zinc oxide, iron oxide (black, yellow, red), chromium oxide, manganese, and combinations thereof.

[0078] Examples of antioxidants include phenolics such as BHT (butylated hydroxytoluene), octadecyl-3,5-bis(1,1-dimethyl)-4-hydroxybenzenepropanoate, pyrogallol; phosphites such as triphenyl phosphite, tris(nonylphenyl) phosphite; or thioesters such as dilauryl thiodipropionate, and combinations thereof.

[0079] When present, the additives may be present in an amount of from 0.01% to 1% by weight, preferably from 0.05% to 0.5% by weight, based on the total weight of the adhesive composition.

[0080] Adhesive Composition In a particularly preferred embodiment, the moisture-curable polyurethane hot melt adhesive composition comprises, based on the total weight of the adhesive composition: 66% to 99% by weight, preferably 70% to 90% by weight, of at least one polyurethane prepolymer obtained by reacting a reactant mixture comprising: (A1) A polyol mixture comprising: (a) at least one polyester polyol, and (b) at least one polyether polyol; and (A2) at least one polyisocyanate having at least two isocyanate groups per molecule; 14% by weight or less, preferably 0.1% to 12% by weight, more preferably 1% to 10% by weight of at least one (meth)acrylic polymer; 20% by weight or less, preferably 1% to 15% by weight, more preferably 1% to 8% by weight, of at least one amorphous polyalphaolefin having a softening point below 100° C., 0.05% to 1% by weight, preferably 0.05% to 0.5% by weight, of at least one catalyst, and 0.01% to 1% by weight, preferably 0.05% to 0.5% by weight, of at least one additive.

[0081] Preparation method The moisture-curable polyurethane hot melt adhesive composition according to the present invention can be prepared by the following procedure to obtain the composition: (i) mixing reactant (A1), components (B) and (C) and optional component (E) at a temperature of 120°C to 140°C, followed by drawing a vacuum; (ii) decreasing the temperature from 80°C to 100°C, adding reactant (A2), and controlling the reaction temperature at 100°C to 110°C; and (iii) optionally, adding component (D) to the mixture and mixing uniformly.

[0082] The apparatus for mixing, stirring, dispersing, etc. is not particularly limited. An automatic mortar, a Henschel mixer, a three-roll mill, a ball mill, a planetary mixer, a bead mill, or the like equipped with a stirrer and a heater can be used. These apparatuses can also be used in appropriate combination. The method for preparing the moisture-curable polyurethane hot melt adhesive composition is not particularly limited as long as the composition is a homogeneous mixture of the above components.

[0083] Laminates and Electronics According to a third aspect of the present invention, provided herein is a laminate comprising a first substrate, a second substrate, and an adhesive layer sandwiched therebetween, wherein the first substrate and the second substrate are independently selected from glass, resin, and metal, and the adhesive layer is formed by curing an adhesive composition of the present invention.

[0084] The first substrate and / or the second substrate can be a single material and a single layer, or can include multiple layers of the same or different materials. The layers can be continuous or discontinuous.

[0085] The substrate of the articles described herein can have a variety of properties including rigidity (i.e., unable to bend using two hands or breaking when attempting to bend using two hands), flexibility (e.g., flexible substrate, i.e., substrate can be bent with less than two hands), porosity, electrical conductivity, lack of electrical conductivity, and combinations thereof.

[0086] The substrate of the article can be in a variety of forms including, for example, fibers, threads, yarns, woven fabrics, nonwoven fabrics, films (e.g., polymeric films, metallized polymeric films, continuous films, discontinuous films, and combinations thereof), foils (e.g., metal foils), sheets (e.g., metal sheets, polymeric sheets, continuous sheets, discontinuous sheets, and combinations thereof), and combinations thereof.

[0087] In a preferred embodiment, at least one of the substrates can be selected from metals such as metal fired pastes, aluminum, tin, molybdenum, silver, conductive metal oxides such as indium tin oxide (ITO), fluorine doped tin oxide, aluminum doped zinc oxide, glass such as ink filled glass, bare glass, resins such as polycarbonate, polybutylece terephthalate, polyamide, etc. Further suitable metals include copper, gold, palladium, platinum, aluminum, indium, silver coated copper, silver coated aluminum, tin, tin coated copper, etc. Preferably, both substrates are selected from any of the aforementioned materials.

[0088] The moisture-curable polyurethane hot melt adhesive composition of the present invention can be cured at room temperature in the range of 15° C. to 35° C. and a relative humidity of 50% for 1 to 7 days.

[0089] As will be appreciated, the time and temperature cure profile of each moisture curable polyurethane hot melt adhesive composition varies, and different compositions can be designed to provide a cure profile that is particularly suited to industrial manufacturing processes.

[0090] According to a fourth aspect of the present invention, provided herein is an electronic device comprising a laminate of the present invention or manufactured using an adhesive composition according to the present invention.

[0091] The moisture-curable polyurethane hot melt adhesive composition of the present invention can be applied to a substrate using any suitable application method including, for example, automated fine line application, jet application, slot die application, roll application, gravure application, transfer application, pattern application, screen printing, spray application, filament application, application by extrusion, air knife application, trailing blade application, brush application, dip application, doctor blade application, offset gravure application, gravure web application, and combinations thereof. The moisture-curable polyurethane hot melt adhesive composition can be applied as a continuous or discontinuous coating, in single or multiple layers, and combinations thereof.

[0092] use According to a fifth aspect of the present invention, provided herein is the use of an adhesive composition according to the present invention or a laminate according to the present invention in the manufacture of an electronic device.

[0093] Suitable electronic devices include, but are not limited to, wearable electronic devices (e.g., watches, eyeglasses), portable electronic devices (e.g., phones (e.g., cell phones, handheld smart phones), cameras, tablets, e-readers, monitors (e.g., monitors used in hospitals, medical professionals, athletes, and individuals), watches, calculators, mice, touchpads, joysticks), computers (e.g., desktop computers and laptop computers), computer monitors, televisions, media players, or other electronic components. EXAMPLES

[0094] Working Example The following examples are intended to help those skilled in the art to better understand and practice the present invention. The scope of the present invention is not limited by the examples, but is defined by the appended claims. All parts and percentages are by weight unless otherwise specified.

[0095] raw materials: VORANOL 2110 is a polyether polyol having a number average molecular weight (Mn) of 1,000 g / mol and is available from DOW.

[0096] Dynacoll 7360 is a crystalline polyester polyol with a number average molecular weight (Mn) of 3,500 g / mol and is available from Evonik Industries AG.

[0097] Dynacoll 7250 is a liquid polyester polyol with a number average molecular weight (Mn) of 5,500 g / mol and a glass transition temperature of -50°C, available from Evonik Industries AG.

[0098] Stepan PDP 70 is a liquid diethylene glycol-phthalic anhydride based modified polyester polyol with a number average molecular weight (Mn) of 1,600 g / mol, available from Stepan Corporation.

[0099] FLP PA-1000N is an amorphous polyester polyol with a number average molecular weight (Mn) of 1,000 g / mol and is available from Xu Chuan Chemical (Suzhou) Co., Ltd.

[0100] Vestoplast 708 is an amorphous polyalphaolefin with a softening point of 106±4° C. and is available from Evonik.

[0101] Vestoplast 408 is an amorphous polyalphaolefin with a softening point of 118±4° C. and is available from Evonik.

[0102] Vestoplast 520 is an amorphous polyalphaolefin with a softening point of 87±4° C. and is available from Evonik.

[0103] Vestoplast 508 is an amorphous polyalphaolefin with a softening point of 84±4° C. and is available from Evonik.

[0104] Elvacite 2013 is a (meth)acrylic polymer with a number average molecular weight (Mn) of 34,000 g / mol and is available from Lucite International.

[0105] GRK 830 is a carbon black paste available from Spectrum Dispersions.

[0106] DESMODUR 44C FUSED is MDI and is available from Bayer.

[0107] JEFFCAT DMDEE is a 2,2'-dimorpholinyl diethyl ether catalyst available from HUNTSMAN.

[0108] Preparation method: Example 1 (Ex.1) 19g VORANOL 2110, 18.6g Dynacoll 7250, 19.4g Dynacoll 7360, 6g Stepan PDP 70, 8g FLP PA-1000N, 10g Elvacite 2013, 1g Vestoplast 508 and 1g GRK 830 were added to the reactor and mixed at 130-140°C for 30 minutes, then the vacuum was reduced to less than 30mBar for 2.5 hours. The temperature of the mixture was then reduced to 95°C and 16.6g MDI was added and mixed at a temperature of 105°C to 115°C for another 80 minutes. Finally, 0.4g JEFFCAT DMDEE was added to the reactor and stirred for another 10 minutes. A homogeneous adhesive composition was obtained.

[0109] Example 2 (Ex.2) 19g VORANOL 2110, 18.6g Dynacoll 7250, 19.4g Dynacoll 7360, 6g Stepan PDP 70, 8g FLP PA-1000N, 10g Elvacite 2013, 5g Vestoplast 508 and 1g GRK 830 were added to the reactor and mixed at 130-140°C for 30 minutes, then the vacuum was reduced to less than 30mBar for 2.5 hours. The temperature of the mixture was then reduced to 95°C and 16.6g MDI was added and mixed at a temperature of 105°C to 115°C for another 80 minutes. Finally, 0.4g JEFFCAT DMDEE was added to the reactor and stirred for another 10 minutes. A homogeneous adhesive composition was obtained.

[0110] Example 3 (Ex.3) 19g VORANOL 2110, 18.6g Dynacoll 7250, 19.4g Dynacoll 7360, 6g Stepan PDP 70, 8g FLP PA-1000N, 10g Elvacite 2013, 3g Vestoplast 508 and 1g GRK 830 were added to the reactor and mixed at 130-140°C for 30 minutes, then the vacuum was reduced to less than 30mBar for 2.5 hours. The temperature of the mixture was then reduced to 95°C and 16.6g MDI was added and mixed at a temperature of 105°C to 115°C for another 80 minutes. Finally, 0.4g JEFFCAT DMDEE was added to the reactor and stirred for another 10 minutes. A homogeneous adhesive composition was obtained.

[0111] Example 4 (Ex.4) 19g VORANOL 2110, 18.6g Dynacoll 7250, 19.4g Dynacoll 7360, 6g Stepan PDP 70, 8g FLP PA-1000N, 10g Elvacite 2013, 3g Vestoplast 520 and 1g GRK 830 were added to the reactor and mixed at 130-140°C for 30 minutes, then the vacuum was reduced to less than 30mBar for 2.5 hours. The temperature of the mixture was then reduced to 95°C and 16.6g MDI was added and mixed at a temperature of 105°C to 115°C for another 80 minutes. Finally, 0.4g JEFFCAT DMDEE was added to the reactor and stirred for another 10 minutes. A homogeneous adhesive composition was obtained.

[0112] Example 5 (Ex.5) 19g VORANOL 2110, 18.6g Dynacoll 7250, 19.4g Dynacoll 7360, 6g Stepan PDP 70, 8g FLP PA-1000N, 8g Elvacite 2013, 5g Vestoplast 508 and 1g GRK 830 were added to the reactor and mixed at 130-140°C for 30 minutes, then the vacuum was reduced to less than 30mBar for 2.5 hours. The temperature of the mixture was then reduced to 95°C and 16.6g MDI was added and mixed at a temperature of 105°C to 115°C for another 80 minutes. Finally, 0.4g JEFFCAT DMDEE was added to the reactor and stirred for another 10 minutes. A homogeneous adhesive composition was obtained.

[0113] Comparative example 1 (CE.1) 19g VORANOL 2110, 18.6g Dynacoll 7250, 19.4g Dynacoll 7360, 6g Stepan PDP 70, 8g FLP PA-1000N, 11g Elvacite 2013 and 1g GRK 830 were added to the reactor and mixed at 130-140°C for 30 minutes, then the vacuum was reduced to less than 30mBar for 2.5 hours. The temperature of the mixture was then reduced to 95°C and 16.6g MDI was added and mixed at a temperature of 105°C to 115°C for another 80 minutes. Finally, 0.4g JEFFCAT DMDEE was added to the reactor and stirred for another 10 minutes. A homogeneous adhesive composition was obtained.

[0114] Comparative example 2 (CE.2) 19g VORANOL 2110, 18.6g Dynacoll 7250, 19.4g Dynacoll 7360, 6g Stepan PDP 70, 8g FLP PA-1000N, 10g Elvacite 2013, 25g Vestoplast 508 and 1g GRK 830 were added to the reactor and mixed at 130-140°C for 30 minutes, then the vacuum was reduced to less than 30mBar for 2.5 hours. The temperature of the mixture was then reduced to 95°C, 16.6g MDI was added and mixed at a temperature of 105°C to 115°C for another 80 minutes. Finally, 0.4g JEFFCAT DMDEE was added to the reactor and stirred for another 10 minutes. A homogeneous adhesive composition could not be obtained because the amorphous polyalphaolefins with weight percentages outside the range of the present invention were insoluble in the adhesive composition.

[0115] Comparative example 3 (CE.3) 19g VORANOL 2110, 18.6g Dynacoll 7250, 19.4g Dynacoll 7360, 6g Stepan PDP 70, 8g FLP PA-1000N, 10g Elvacite 2013, 3g Vestoplast 408 and 1g GRK 830 were added to the reactor and mixed at 130-140°C for 30 minutes, then the vacuum was reduced to less than 30mBar for 2.5 hours. The temperature of the mixture was then reduced to 95°C, 16.6g MDI was added and mixed at a temperature of 105°C to 115°C for another 80 minutes. Finally, 0.4g JEFFCAT DMDEE was added to the reactor and stirred for another 10 minutes. A homogeneous adhesive composition could not be obtained because amorphous polyalphaolefins having softening points outside the scope of the present invention precipitated during the reaction and formed granules in the adhesive composition.

[0116] Comparative example 4 (CE.4) 19g VORANOL 2110, 18.6g Dynacoll 7250, 19.4g Dynacoll 7360, 6g Stepan PDP 70, 8g FLP PA-1000N, 10g Elvacite 2013, 3g Vestoplast 708 and 1g GRK 830 were added to the reactor and mixed at 130-140°C for 30 minutes, then the vacuum was reduced to less than 30mBar for 2.5 hours. The temperature of the mixture was then reduced to 95°C, 16.6g MDI was added and mixed at a temperature of 105°C to 115°C for another 80 minutes. Finally, 0.4g JEFFCAT DMDEE was added to the reactor and stirred for another 10 minutes. A homogeneous adhesive composition could not be obtained because amorphous polyalphaolefins having softening points outside the scope of the present invention precipitated during the reaction and formed granules in the adhesive composition.

[0117] Comparative example 5 (CE.5) 19g VORANOL 2110, 18.6g Dynacoll 7250, 19.4g Dynacoll 7360, 6g Stepan PDP 70, 8g FLP PA-1000N, 3g Vestoplast 508 and 1g GRK 830 were added to the reactor and mixed at 130-140°C for 30 minutes, then the vacuum was reduced to less than 30mBar for 2.5 hours. The temperature of the mixture was then reduced to 95°C and 16.6g MDI was added and mixed at a temperature of 105°C to 115°C for another 80 minutes. Finally, 0.4g JEFFCAT DMDEE was added to the reactor and stirred for another 10 minutes. A homogeneous adhesive composition was obtained.

[0118] Comparative example 6 (CE.6) 19g VORANOL 2110, 18.6g Dynacoll 7250, 19.4g Dynacoll 7360, 6g Stepan PDP 70, 8g FLP PA-1000N, 15g Elvacite 2013, 3g Vestoplast 508 and 1g GRK 830 were added to the reactor and mixed at 130-140°C for 30 minutes, then the vacuum was reduced to less than 30mBar for 2.5 hours. The temperature of the mixture was then reduced to 95°C, 16.6g MDI was added and mixed at a temperature of 105°C to 115°C for another 80 minutes. Finally, 0.4g JEFFCAT DMDEE was added to the reactor and stirred for another 10 minutes. A homogeneous adhesive composition could not be obtained because the (meth)acrylic polymer with a weight percentage outside the range of the present invention was insoluble in the adhesive composition.

[0119] Test Method: Initial cross tensile strength: Sample preparation: I. First, a polycarbonate substrate containing 20% ​​glass fiber by weight, measuring 101.6x25.4x1mm, and an ink glass substrate measuring 101.6*25.4*3mm were prepared. The substrates were washed with isopropanol and left to idle for a few minutes at ambient conditions to ensure that the surfaces were completely dry. The polycarbonate substrate and the ink glass substrate were arranged in a cross shape, and an adhesive layer was sandwiched between the overlapping areas.

[0120] II. Next, two spacers with a diameter of 0.127 mm were placed to control the thickness of the adhesive layer. Before dispersing the adhesive composition, the spacers were placed on the edge of the ink glass at a distance of 3 mm from the edge of the overlapping portion.

[0121] III. The adhesive composition was then heated to 110°C for 30 minutes with a Loctite 400D dispenser. A 21# size needle was used to apply the adhesive composition to the surface of the ink glass. During the dispensing process, two bond lines were formed by the adhesive beads dispensed from the needle. The two bond lines were applied in parallel, and the distance of each bond line to the edge of the overlapping part of the two substrates was 1-1.5 mm. Furthermore, the distance between each adhesive bead was controlled to be 8 mm, and the distance from the adhesive bead to the edge of the overlapping part of the two substrates was also 8 mm.

[0122] IV. After dispensing, the polycarbonate substrates loaded with 20% glass fiber by weight were pressed to form a sandwich structure of overlapping parts, leaving two free ends of each substrate. Then, the laminate was prepared.

[0123] V. A 2 kilogram weight was applied to the overlapping sandwich structure for 15 seconds, after which the weight was removed and the resulting sample was placed at 23° C. and 50% relative humidity for 1 hour to allow the adhesive composition to cure.

[0124] Testing of samples: To measure the initial cross tensile strength at the time of adhesive layer breakage, the cross tensile strength of the samples was measured with an INSTRON tensile tester at a test speed of 10 mm / min. If the initial cross tensile strength is greater than 2.5 MPa, the adhesive composition is suitable for use in electronic devices.

[0125] DuPont Impact Energy Test: The impact resistance of the cured adhesive compositions was evaluated by DuPont impact energy using a lap shear assembly.

[0126] Sample preparation: I. First, we prepared a polycarbonate substrate with 20% glass fiber by weight, measuring 101.6 x 25.4 x 1 mm, a magnesium aluminum alloy substrate with a width of 1 inch and length of 4 inches with a 10 mm diameter hole in the center, and a polyethylene terephthalate (PET) film with a thickness of 0.12 mm with a 12 mm diameter hole in the center. The PET film has tape on one side for adhering to the magnesium aluminum alloy substrate to control the width and thickness of the adhesive layer. The substrates were washed with isopropanol and left to idle for a few minutes at ambient conditions to ensure that the surfaces were completely dry.

[0127] II. The PET film was attached to the magnesium aluminum alloy substrate so that the position of the central hole of the PET film was aligned with the position of the central hole of the magnesium aluminum alloy substrate. The diameter of the magnesium aluminum alloy substrate was 2 mm larger than that of the PET film, forming a circular ring area with a width of 1 mm.

[0128] III. The adhesive composition was discharged into the circular ring region of the magnesium aluminum alloy substrate, and a polycarbonate substrate was placed horizontally so as to cover the central hole of the magnesium aluminum alloy substrate, and an adhesive layer having a width of 1 mm and a thickness of 0.12 mm was formed by sandwiching the overlapping portion, i.e., the circular ring region.

[0129] IV. The test specimens were cured for 72 hours at 23°C and 60% humidity.

[0130] V. The test specimen was fixed to a holder at the bottom of a DuPont testing machine (BGD301) and subjected to the test.

[0131] Sample test: As a starting point, a 50g weight was dropped onto the test specimen from a height of 2cm. If the magnesium aluminum alloy substrate did not peel off from the polycarbonate substrate three times, the weight was raised to a height 2cm higher than the previous height and dropped again. If the magnesium aluminum alloy substrate did not peel off from the polycarbonate substrate using the 50g weight at a height of 50cm, the test was performed using a 60g weight. DuPont impact energy was calculated using the following formula:

[0132] E=m*g*h*0.01,

[0133] Here, E is the impact energy (mJ), m is the weight (g) when the substrates are peeled off, h is the height (cm) of the weight that is loosened when the substrates are peeled off, and g is 9.8 m / s 2 DuPont impact energy values ​​below 350 mJ are considered unacceptable impact resistance.

[0134] The test results are shown in Table 1.

[0135] TIFF2024536120000001.tif44160

[0136] As can be seen from Table 1, the moisture-curable polyurethane hot melt adhesive compositions of the present invention exhibited excellent impact resistance and initial cross tensile strength when cured, whereas the comparative compositions exhibited unsatisfactory performance.

[0137] While several preferred embodiments have been described, many modifications and variations can be made thereto in light of the above teachings, and it is therefore to be understood that the invention can be practiced otherwise than as specifically described without departing from the scope of the appended claims.

Claims

1. (A) at least one polyurethane prepolymer obtained by reacting a reactant mixture comprising: (A1) A polyol mixture comprising: (a) at least one polyester polyol, and (b) at least one polyether polyol; and (A2) at least one polyisocyanate having at least two isocyanate groups in one molecule; (B) at least one (meth)acrylic polymer present in an amount of 14% by weight or less, based on the total weight of the adhesive composition; and (C) at least one amorphous polyalphaolefin having a softening point less than 100° C., present in an amount of 20% by weight or less, based on the total weight of the adhesive composition; A moisture-curable polyurethane hot melt adhesive composition comprising:

2. 2. The moisture-curable polyurethane hot melt adhesive composition of claim 1, wherein the reactant (a) is selected from solid polyester polyols, liquid polyester polyols, and combinations thereof, preferably selected from crystalline polyester polyols, amorphous polyester polyols, liquid polyester polyols, and combinations thereof.

3. 3. The moisture-curable polyurethane hot melt adhesive composition according to claim 1 or 2, wherein reactant (a) has a number average molecular weight (Mn) of 800 to 20,000 g / mol, preferably 1,000 to 10,000 g / mol, more preferably 1,000 to 5,000 g / mol.

4. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 1 to 3, wherein the reactant (b) is selected from polytetramethylene ether glycol, poly(oxypropylene) glycol, polyethylene oxide, polybutylene oxide, and any of the aforementioned ethylene oxide end-capped types, and combinations thereof, and is preferably selected from polytetramethylene ether glycol, poly(oxypropylene) glycol, ethylene oxide end-capped poly(oxypropylene) glycol, and combinations thereof.

5. The reactant (A2) is 4,4-diphenylmethane diisocyanate (MDI), hydrogenated MDI (H12MDI), partially hydrogenated MDI (H6MDI), xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), 4,4-diphenyldimethylmethane diisocyanate, dialkylene diphenylmethane diisocyanate, tetraalkylene diphenylmethane diisocyanate, 4,4-dibenzyl diisocyanate, 1,3- Phenylene diisocyanate, 1,4-phenylene diisocyanate, isomers of toluylene diisocyanate (TDI), 1-methyl-2,4-diisocyanatocyclohexane, 1,6-diisocyanato-2,2,4-trimethylhexane, 1,6-diisocyanato-2,4,4-trimethylhexane, 1-isocyanatomethyl-3-isocyanato-1,5,5-trimethylcyclohexane (IPDI), tetramethoxybutane-1,4-diisocyanate, Naphthalene-1,5-diisocyanate (NDI), butane-1,4-diisocyanate, hexane-1,6-diisocyanate (HDI), dicyclohexylmethane diisocyanate, 2,2,4-trimethylhexane-2,3,3-trimethylhexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, ethylene diisocyanate, methylenetriphenyl triisocyanate (MIT), phthalic acid bisisocyanatoethyl ester , trimethylhexamethylene diisocyanate, 1,4-diisocyanatobutane, 1,12-diisocyanatododecane, and dimer fatty acid diisocyanate, lysine ester diisocyanate, 4,4-dicyclohexylmethane diisocyanate, 1,3-cyclohexane or 1,4-cyclohexane diisocyanate, and combinations thereof. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 1 to 4.

6. Component (B) has a number average molecular weight (Mn) of 5,000 to 100,000 g / mol, preferably 5,000 to 80,000 g / mol, more preferably 8,000 to 50,000 g / mol. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 1 to 5.

7. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 1 to 6, wherein component (C) has a softening point of 70°C to 95°C.

8. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 1 to 7, wherein component (C) has a molecular weight (Mn) of less than 200,000 g / mol, preferably less than 100,000 g / mol.

9. The adhesive composition may be prepared by mixing a strong basic amide, triethylamine, tributylamine, dimethylbenzylamine, N-ethyl-, N-methyl-, N-cyclohexylmorpholine, dimethylcyclohexylamine, dimorpholinodiethyl ether, 2-(dimethylaminoethoxy)-ethanol, 1,4-diazabicyclo[2,2,2]octane, 1-azabicyclo[3,3,0]octane, N,N,N'. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 1 to 8, further comprising at least one catalyst (D) selected from N'-tetramethylethylenediamine, N,N,N',N'-tetramethylbutanediamine, N,N,N',N'-tetramethylhexane-1,6-diamine, pentamethyldiethylenetriamine, tetramethyldiaminoethyl ether, bis-(dimethylaminopropyl)-urea, N,N'-dimethylpiperazine, 1,2-dimethylimidazole, di-(4-N,N-dimethylaminocyclohexyl)-methane, organometallic compounds, and combinations thereof.

10. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 1 to 9, wherein the adhesive composition further comprises (E) at least one additive.

11. 11. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 1 to 10, wherein component (A) is present in an amount of from 66% to 99% by weight, more preferably from 70% to 90% by weight, based on the total weight of the adhesive composition.

12. 12. The moisture-curable polyurethane hot melt adhesive composition according to any of the preceding claims, wherein reactant (a) is present in an amount of from 30% to 70% by weight, more preferably from 35% to 65% by weight, based on the total weight of the adhesive composition.

13. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 1 to 12, wherein reactant (b) is present in an amount of from 10 wt% to 40 wt%, more preferably from 15 wt% to 36 wt%, based on the total weight of the adhesive composition.

14. 14. The moisture-curable polyurethane hot melt adhesive composition according to any of the preceding claims, wherein reactant (A2) is present in an amount of 10 wt.-% to 25 wt.-%, preferably 10 wt.-% to 20 wt.-%, based on the total weight of the adhesive composition.

15. 15. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 1 to 14, wherein component (B) is present in an amount of preferably 0.1 wt% to 12 wt%, more preferably 1 wt% to 10 wt%, based on the total weight of the adhesive composition.

16. 16. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 1 to 15, wherein component (C) is present in an amount of 1 wt.% to 15 wt.%, preferably 1 wt.% to 8 wt.%, based on the total weight of the adhesive composition.

17. 17. The moisture-curable polyurethane hot melt adhesive composition according to any one of claims 9 to 16, wherein component (D) is present in an amount of 0.05 wt% to 1 wt%, preferably 0.05 wt% to 0.5 wt%, based on the total weight of the composition.

18. (i) mixing reactant (A1), components (B) and (C), and optional component (E) at a temperature of 120° C. to 140° C., followed by drawing a vacuum; (ii) decreasing the temperature to 80°C to 100°C, adding reactant (A2), and controlling the reaction temperature to 100°C to 110°C; and (iii) optionally, adding component (D) to the mixture and mixing uniformly. A method for preparing the hot melt adhesive composition of any one of claims 1 to 17, comprising:

19. A laminate comprising a first substrate, a second substrate, and an adhesive layer sandwiched therebetween, the first substrate and the second substrate being independently selected from glass, resin, and metal, and the adhesive layer being formed by curing the adhesive composition according to any one of claims 1 to 17.

20. An electronic device comprising the laminate of claim 19 or produced using the adhesive composition of any one of claims 1 to 17.

21. Use of the adhesive composition according to any one of claims 1 to 17 or the laminate according to claim 19 in the manufacture of an electronic device.

Citation Information

Patent Citations

  • Polyurethane hot melt adhesive for bonding non-polar material and preparation method thereof

    CN111234768A

  • Polyurethane hot melt adhesive for bonding low-surface-energy base material and preparation method thereof

    CN113025261A

  • Polyolefin modified reactive polyurethane hot melt adhesive and preparation method thereof

    CN113322043A

  • Polyurethane hot melt adhesive with acrylic copolymer and thermoplastic resin

    JP2003531271A

  • Moisture reactive hot melt adhesive

    JP2004339469A