DRI induction heating

Induction heating of DRI and fines before briquetting addresses temperature imbalances in HBI production, ensuring uniform material properties and enabling the use of lower grade ores, thus improving yield and reducing costs.

JP2024536458AActive Publication Date: 2024-10-04ARCELORMITTAL TEXAS HBI LLC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024521351
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-10-07
Filing Date
2022-10-05
Publication Date
2024-10-04
Estimated Expiration
2042-10-05

AI Technical Summary

Technical Problem

Existing direct reduction processes for producing hot briquetted iron (HBI) face challenges in achieving uniform temperature control and material properties due to temperature imbalances and inefficiencies in the discharge system, leading to issues with briquetting density and increased fines generation.

Method used

The process involves using induction heating to adjust the temperature of directly reduced iron (DRI) and recirculated fines before briquetting, decoupling temperature control from the reactor conditions, allowing independent temperature selection for the briquetting process.

Benefits of technology

This approach results in more uniform HBI properties, reduced generation of particles and fines, increased yield, and the ability to use lower grade ores, thereby enhancing operational efficiency and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024536458000001_ABST
    Figure 2024536458000001_ABST
Patent Text Reader

Abstract

The present invention relates to a process for the production of hot briquetted iron (HBI) from direct reduced iron (DRI), characterized in that iron ore is directly reduced in a reactor with a reducing gas consisting of natural gas and / or hydrogen and / or carbon monoxide at elevated temperature, and the direct reduced iron is discharged to at least one briquetting device in which briquettes are pressed from the direct reduced iron, and the direct reduced iron is heated to a target briquetting temperature after leaving the reactor and before briquetting.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a process that produces hot briquetted iron (HBI) with more uniform properties and that allows for greater control of the temperature of the directly produced iron. [Background technology]

[0002] Due to environmental concerns, and in particular due to the emissions of carbon dioxide in conventional steelmaking processes, the avoidance of emitted carbon dioxide has become an increasing concern of the steel industry.

[0003] One focus is on the production of so-called direct reduced iron (DRI), which is produced from the direct reduction of iron ore by reducing gases or elemental carbon produced from natural gas or coal. The direct reduction of iron is a solid-state process that operates below the melting point of iron. An example is the direct reduction of iron ore in the presence of a reducing gas, the so-called synthesis gas, which is a mixture of hydrogen and carbon monoxide. This takes place at temperatures between 800 and 1200 °C.

[0004] These direct production processes can be divided into gas-based and coal-based processes, and in both cases, as in conventional steelmaking, the objective is to remove the oxygen contained in various forms as iron oxide.

[0005] In addition to avoiding carbon dioxide emissions, the direct reduction process is relatively energy efficient. For example, the DRI process requires significantly less fuel than a conventional blast furnace. By using the direct reduction process, it is possible to avoid a typical integrated steel plant. For shipping, handling and storage, the direct reduced iron can be in briquette form, which is usually done in a high-temperature process called hot briquetting, resulting in hot briquette iron (HBI). For the production of HBI, iron ore is reduced using hydrogen or natural gas, which is much more environmentally friendly than using coke. The reduction process takes place in a reduction tower. The tower is the core of the plant. The direct reduction process is quite complex and involves pelletizing the iron ore, or using pelletized iron ore and feeding them into a reactor. Natural gas is converted into reducing gas, which is then injected into the system and circulated in a closed system. The hot reducing gas is led through the iron ore from the bottom to the top of the reduction furnace using the counter-flow principle. The iron ore is reduced and sponge iron is produced. The sponge iron is then pressed into briquettes in a high temperature process, resulting in hot briquetted iron (HBI).

[0006] The temperature of the feed material to the briquette press is important to achieve the proper density and desired physical properties of the HBI. The temperature of the material arriving at the press is determined by the heat in the furnace above it, which is primarily influenced by the gas flow and temperature required for reduction. The amount of natural gas injected below the reduction zone cools the material and adds carbon. Oxygen can be injected to increase the temperature of the bed, but its use is limited by the temperature at which clustering of the material occurs. Carbon monoxide combined with natural gas injection injected at the bottom of the furnace can also be used to limit the temperature drop as carbon is added, but requires a complex flowsheet that includes hydrogen separation by methods such as pressure swing absorption (PSA), vacuum swing absorption (VSA), or other methods known in the art.

[0007] For example, the reactor zone temperature in the reduction furnace is about 850° C., and the HDRI temperature after natural gas injection and cooling is about 650-680° C. After natural gas injection and cooling, multiple feed channels distribute the material to the briquetting machine.

[0008] The prior art addresses various issues such as temperature non-uniformity that can result in each briquetting machine receiving material at different temperatures. The pellet quality impacts the briquetting and therefore the final HBI quality. Also, the maximum temperature of the feed material is tied to furnace operation. Summary of the Invention [Problem to be solved by the invention]

[0009] It is an object of the present invention to provide a process which produces hot briquetted iron with more uniform properties and allows for better control of the temperature of the directly produced iron. A further object is to allow for uniform material properties prior to feeding into the hot briquetting process. [Means for solving the problem]

[0010] These objects are achieved by means of the process described in claim 1.

[0011] Advantageous features are claimed in the dependent claims.

[0012] The inventors have found that flow problems in the discharge system result in temperature imbalances that have an impact on briquetting: some parts of the material may have a very low temperature, which creates problems in the briquetting density, resulting in a lot of fines and chips.

[0013] Also, recirculation of the hot fines to the briquetting machine significantly cools the DRI through the screening operation.

[0014] The inventors also recognized the problem that in future operations with partial hydrogen use, the carbon formed in the reduction zone itself will be greatly reduced due to thermodynamic conditions. This limits the amount of carbon that can be added to the product in combination with the endothermic reduction reaction that cools the bed, as the maximum amount of carbon that can be added by natural gas injection in the lower furnace zone is limited by the temperature required for briquetting. A small amount of carbon in the product is important for downstream EAF operations to ensure a foamy slag, and therefore it is desirable to have a residual carbon content in the product, especially when using a reducing gas containing hydrogen.

[0015] Furthermore, the inventors have considered that there is no way to independently control the temperature of the material in the reactor and the temperature of the material going from the reactor to the briquette press. If it is necessary to increase the temperature of the material arriving at the briquette press, according to the prior art, the temperature of the entire reactor must be increased. However, this increases the risk of clustering in the furnace and reduces energy efficiency.

[0016] Therefore, the inventors have found it advantageous to elevate the temperature of the DRI before it reaches the briquette press, thereby eliminating the need for temperature adjustments within the reactor. Additionally, the inventors have identified the need for a means to balance the temperature between the feed channels and a means to elevate the temperature of the recirculated fines before they enter the briquette press.

[0017] To achieve the above and to avoid the shortcomings in the prior art, the feeding channel and / or the hot fine powder are modified such that induction heating of these materials is performed in the feeding channel to control the temperature before entering the briquette press.

[0018] This temperature control decouples the DRI temperature from the temperature in the reactor, thereby allowing the reactor to operate at the optimum conditions for direct reduction. The hot briquetting temperature can be selected independently according to the optimum temperature for this process.

[0019] The temperature of the DRI is monitored and adjusted during the induction process, thereby allowing a controlled increase in the DRI temperature to a target temperature regardless of the particular feed channel, so the briquette press is fed with DRI at the same temperature, resulting in uniform briquette properties.

[0020] It has been found that by increasing the temperature of the DRI by 25°C, HDI chip and fine generation can be reduced by several percent, which translates into increased yields and higher value for customers.

[0021] As a notable side effect, it has been found that operating at higher briquetting temperatures allows the use of greater amounts of lower grade ore, which may become more important in the future. The use of lower grade ore provides further cost savings.

[0022] Additionally, since the DRI can be reheated, additional carbon can be added in the transition zone from natural gas and / or other carbon-containing gases such as biogas, thereby compensating for both carbon losses in the reactor and cooling due to hydrogen use.

[0023] It is preferred to use sustainable energy sources for the derivation process, such as wind and / or solar energy and / or energy from solid oxide fuel cells. In periods when sustainable energy is insufficient, stored hydrogen may be used for these fuel cells and for the direct reduction of iron ore.

[0024] In one embodiment, an induction heating device is positioned around each feed channel.

[0025] In an advantageous embodiment, it is recommended that the system or induction heating device for each supply channel is designed to allow a heating of the DRI material up to 100° C. Typically, a heating of the DRI material of 20° C. is used.

[0026] In a further advantageous embodiment, the induction heating device for each system of each supply channel is designed for a specific energy input of between 2 and 18 kWh / t HBI, preferably between 2 and 8 kWh / t HBI during conventional operation with higher grade ores and between 8 and 18 kWh / t HBI when operating with lower grade ores or during a hybrid operating mode using hydrogen.

[0027] In particular, the present invention relates to a process for the production of hot briquette iron (HBI) from direct reduced iron (DRI), in which iron ore is directly reduced at elevated temperature in a reactor by a reducing gas consisting of natural gas and / or hydrogen and / or carbon monoxide, and the direct reduced iron is discharged to at least one briquetting device, where briquettes are pressed from the direct reduced iron, and the direct reduced iron is heated to a target briquetting temperature after leaving the reactor and prior to briquetting.

[0028] In one embodiment, the post-briquetting fines are collected downstream of the briquetting press and heated to the target briquetting temperature before being reintroduced into the briquetting press.

[0029] In one embodiment, the DRI and / or fines are heated by induction heating.

[0030] In one embodiment, the DRI and fines are heated separately or mixed and then heated together after mixing.

[0031] In one embodiment, the induction heater is positioned around a duct or channel that carries the DRI and / or fines to the briquette press.

[0032] In one embodiment, the DRI and / or fines are heated to a temperature above 700° C., preferably between 700° C. and 800° C., prior to briquetting.

[0033] In one embodiment, a sustainable energy source is used for the induction process, preferably energy from wind energy or solid oxide fuel cells, and the hydrogen used for these fuel cells is from the same source as the hydrogen used for the direct reduction of iron ore.

[0034] In one embodiment, the induction heating unit is designed to input energy to the material between 2 and 18 kWh / t HBI, preferably between 2 and 8 kWh / t HBI when processing higher grade materials, and between 8 and 18 kWh / t HBI when processing lower grade ores or operating in a hybrid mode of operation with hydrogen.

[0035] Therefore, for a reduction furnace with a production capacity of 2 million tons per year and seven feed legs, a nominal material input power of 75 to 700 kW per feed leg is required.

[0036] In one embodiment, the induction heating device for each feed channel is designed to allow heating of the DRI material of at least 100°C or more, preferably between 20-50°C when processing high grade ores in a conventional process, and 50-100°C when processing lower grade materials or operating in a hybrid mode of operation with hydrogen.

[0037] The present invention will now be described with reference to examples and the accompanying drawings. [Brief description of the drawings]

[0038] [Figure 1] FIG. 13 illustrates feed channel temperature in degrees Fahrenheit as a function of briquette density. [Diagram 2] FIG. 1 shows the relative strength of briquettes as a function of temperature. [Diagram 3] FIG. 13 illustrates the reduced temperature of materials with higher carbon content. [Figure 4] FIG. 13 is a schematic diagram showing a modified supply channel. [Diagram 5] FIG. 13 shows the percentage of chips and fines in HBI as a function of feed channel temperature. [Figure 6a] FIG. 1 shows briquette density in correlation with Fe content in the pellets before reduction at 700° C. [Figure 6b] FIG. 1 shows briquette density in correlation with Fe content in the pellets before reduction at 800° C. [Figure 7] FIG. 1 shows a comparison of the prior art with 100% natural gas, compared to hydrogen natural gas operation with reduced carbon content, and hydrogen natural gas operation with the desired carbon content in a hydrogen / natural gas operation according to the present invention. [Figure 8] FIG. 1 shows a possible installation location for a briquetting plant, where fines resulting from the briquetting process are sent back to the DRI. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0039] In Figure 1, the feed channel temperature in degrees Fahrenheit and the 5t / m 3 From this chart it can be derived that the higher the feed channel temperature the denser the briquettes are, and that the increase in density is not linear and can be significantly reduced by a 30° F. increase in temperature. Also in FIG. 2 the relative strength of the briquettes is plotted as a function of the feed channel temperature, showing that higher temperatures result in higher relative strength.

[0040] In processes where natural gas is introduced and hydrogen is partially used, the amount of carbon formed in the reduction zone itself will be greatly reduced due to thermodynamic conditions: this, combined with the endothermic reduction reactions cooling the bed, will limit the amount of carbon that can be added to the product, since the maximum amount of carbon that can be added by the natural gas injected into the lower furnace zone will be limited by the temperature required for briquetting.

[0041] In FIG. 3 it can be clearly seen that the higher the carbon content the lower the material temperature in the feed channel, which is lower than the values ​​shown in FIGS. 1 and 2 for sufficient density and sufficient relative strength of the briquettes.

[0042] The present invention aims to solve the problem of different temperatures resulting from, on the one hand, operating in an optimal mode a DRI reactor operated with a higher hydrogen content in the reducing gas and the introduction of carbon by injection of natural gas, and, on the other hand, operating the briquetting in such a way that briquettes can be formed with sufficient strength and density.

[0043] According to FIG. 4, this is accomplished by induction heating of the DRI or sponge iron in the feed channel to the briquetting machine, where the sponge iron or DRI can be conditioned to an ideal temperature, typically above 1300° Fahrenheit.

[0044] As can be seen in Figure 5, the amount of chips and fines in the resulting briquettes can be significantly reduced by increasing the temperature by only 25°C. This is due to the fact that increasing the temperature can increase the density and strength of the briquettes.

[0045] The pellet grade limits at current feed channel temperatures are shown in comparison to higher feed channel temperatures according to the present invention. As an added benefit, iron ore with an Fe content in the ore pellets prior to reduction of about 66.5% can be reduced by 1 m 3 It was found that this produces a required briquette density of 5 tons per tonne. This is normally achieved at a briquetting temperature of 700°C (1292°F) (Figure 6a). It was found that the same density could be achieved with iron ore having a significantly lower Fe content by increasing the briquetting temperature by 100°C to 800°C (1472F) (Figure 6b), thereby allowing the use of larger amounts of lower grade ore, which could be important in the future, providing cost advantages.

[0046] In Figure 7, three different operating systems for operating the reactor are shown. On the left side, the current situation is shown where 100% natural gas is used for reforming to produce synthesis gas for reduction in the reactor. As can be seen, the product has a carbon content of about 1.5 wt% and the operating temperature of the DRI is about 670-700 °C. In the middle, a hydrogen / natural gas blend operation with maximum carbon content is shown, with the DRI temperature kept at a minimum value of about 670 °C. In this case, the product has a carbon content of less than 1 wt%.

[0047] On the right, a hydrogen / natural gas blended operation is shown. The operating conditions are shown in the middle, but the carbon content must be kept at the required product, about 1.5 wt%. The operating conditions shown in the middle diagram do not achieve a high enough carbon content. Achieving a carbon content of about 1.2-1.5 wt% is possible at a DRI temperature of 600 °C, which is too low for briquetting.

[0048] According to the invention, the operating route shown on the right side can be selected so as to obtain a product with sufficient carbon content. The lower output temperature from the reactor is compensated for according to the invention by induction heating of the DRI before briquetting. In a preferred embodiment, induction heating of the DRI is performed in the feed channel from the reactor to the briquetting machine. It is advantageous to design the induction heating system to allow a temperature increase of at least 100°C of the DRI material. It may be sufficient to allow a temperature increase of up to 100°C of the DRI material. During typical operation, a material temperature increase of 20°C is expected to be sufficient.

[0049] In order to heat the DRI sufficiently, the temperature of the DRI can be monitored before it reaches the induction heating zone and increased to a predetermined temperature if necessary, allowing all material in all feeding channels to arrive at the briquetting machine at a predetermined temperature.

[0050] Figure 8 shows different installation possibilities of induction heating shown for a briquetting plant where fines are fed back to the briquetting machine. Due to the difference in temperature between the DRI (temperature T1) and the fines (temperature T2), the resulting DRI / fines mixture temperature (temperature T3) depends on the relative amount of recirculated fines and the temperatures of both the incoming DRI and fines. In the first example, only the temperature of the DRI is adjusted (2) to control the temperature of the DRI and fines mixture fed to the briquetting press. In the second example, an additional heating source (5) is installed in the fines recirculation line to allow independent control of the DRI and fines temperatures.

[0051] Induction heating has a high degree of efficiency, making it the preferred heating method. Furthermore, high mass flows of DRI or sponge iron material can be processed very efficiently. The power required for this induction heating can be derived from sustainable energy sources, so that the overall process is already more environmentally friendly than conventional steelmaking.

[0052] For example, the same hydrogen source as for the reduction can be used for the generation of electrical energy for induction heating, or electrical energy from wind energy, etc. Also, the supply channel pipe can be easily adapted for an induction heating process by placing an induction coil on the pipe, which is much easier to achieve and safer than, for example, heating with a combustible energy source.

[0053] The expected energy input into the material for the required temperature increase can range from 2-18 kWh / t HBI, with an expected range of between 2-8 kWh / t HBI when processing higher grade material, and 8-18 kWh / t HBI when processing lower grade ores or operating in a mixed hydrogen / natural gas mode of operation.

Claims

1. A process for the production of hot briquetted iron (HBI) from direct reduced iron (DRI), comprising: iron ore being directly reduced in a reactor by a reducing gas consisting of natural gas and / or hydrogen and / or carbon monoxide at an elevated temperature, and discharging the direct reduced iron to at least one briquetting device where briquettes are pressed from the direct reduced iron; 1. A process for the production of direct reduced iron, characterized in that after leaving the reactor, the direct reduced iron is heated to a target briquetting temperature prior to briquetting.

2. 2. The process according to claim 1, characterized in that the fines after briquetting are recovered downstream of the briquetting press and heated to the target briquetting temperature before being reintroduced into the briquetting press.

3. 3. The process according to claim 1 or 2, characterized in that the DRI and / or the fines are heated by induction heating.

4. A process according to any one of claims 1 to 3, characterised in that the DRI and the fines are heated separately or mixed and heated together after mixing.

5. A process according to any one of claims 1 to 4, characterised in that the induction heating is positioned around a duct or channel which conveys the DRI and / or the fines to the briquetting press.

6. 6. The process according to any one of claims 1 to 5, characterized in that the DRI is heated to a temperature above 700°C, preferably between 700-750C when processing higher grade ores during conventional operation and between 750-800C when using lower grade feedstock or operating in a hybrid mode of operation using hydrogen.

7. 7. The process according to any one of claims 1 to 6, characterized in that for the induction process a sustainable energy source is used, preferably wind and / or solar energy and / or energy from solid oxide fuel cells, and the hydrogen used in these fuel cells is from the same source as the hydrogen used for the direct reduction of iron ore.

8. The process according to any one of claims 1 to 7, characterized in that the induction heating device is designed for an energy input to the DRI of about 2 to 18 kWh / t HBI.

9. 9. The process according to any one of claims 1 to 8, characterized in that the induction heating device for each supply channel is designed to allow a heating of the DRI material of at least 100°C or more, preferably for a heating of the DRI material of 20°C when processing higher grade material and for a heating of 50-100°C when processing lower grade ores or operating in a hybrid operation mode using hydrogen.

Citation Information

Patent Citations

  • Method and device for preparing binder-free hot briquet

    JP1984025936A

  • Efficient application method of carbonaceous resource

    JP2005042142A

  • Method for manufacturing reduced iron molded material, and method for producing pig iron

    JP2009079292A

  • Molded body of small iron oxide carrier bonded to bentonite

    JP2013525605A

  • Method for producing molten iron and manufacturing plant

    JP2013531733A