A lithium ion conductive material with a crystalline LLZO phase and amorphous SiO2/P2O5 phase enhances dendrite stability, addressing dendrite formation issues in solid-state batteries, enabling high current density charging and preventing short circuits.
Patent Information
- Application Number
- JP2024525325
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-29
- Filing Date
- 2022-10-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-10-26
AI Technical Summary
Solid-state lithium-ion batteries face issues with dendrite formation during high current density charging, leading to short circuits, which existing separator materials fail to adequately address.
A lithium ion conductive material comprising a crystalline phase, such as Li-stable LLZO, combined with an amorphous phase containing specific glass formers like SiO2 and P2O5, is used to enhance dendrite stability, achieving a critical current density (CCD) of at least 0.5 mA/cm².
The material significantly increases the critical current density, preventing short circuits and enabling fast charging without compromising conductivity, thereby improving the safety and performance of solid-state lithium-ion batteries.
Smart Images

Figure 2024538271000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to lithium ion conducting materials, in particular glass-ceramics, with improved dendritic stability (stability against the formation of dendrites), and to methods of use and manufacture.
[0002] All-solid-state batteries (ASSB) are considered the future of energy storage technology / electromobility due to their high energy density and safety. The core of this innovation is the replacement of liquid electrolytes with solid ionically conductive separators, which allows the use of lithium metal as the anode material, especially if the separator itself is lithium-stable (e.g., when using lithium lanthanum zirconate (LLZO)). However, during charging, Li deposited on the anode can grow toward the separator and onto the cathode. This is called dendrite formation. When such dendrites form, a short circuit occurs. The higher the current density during charging, the more likely it is that undesirable dendrites will form. Therefore, it is necessary to provide separator materials that suppress the formation of dendrites even at high current densities, or that have a high critical current density (CCD).
[0003] It is therefore an object of the present invention to overcome the drawbacks of the prior art. This object is achieved by the subject matter of the claims. In particular, this object is to provide a lithium ion conducting material comprising a crystalline phase and an amorphous phase, the lithium ion conducting material having a current density of 0.5 mA / cm 2 This problem is solved by using lithium ion conducting materials with critical current densities of up to 1000 times higher.
[0004] The combination of a lithium ion conducting crystalline phase, such as Li-stable LLZO (especially Ta or Al doped), with an amorphous phase, especially at the grain boundaries of the sintered separator, allows a significant increase in the CCD compared to materials that do not contain such an amorphous phase, or that do not contain glass formers (pure Li2O), or that have a low content of glass formers relative to the total weight of the crystalline and amorphous phases, i.e., relative to the total weight of the lithium ion conducting material. The glass former content may advantageously be at least 0.05% by weight relative to the total weight of the lithium ion conducting material.
[0005] In particular, the amorphous phase comprises, in addition to Li2O (for Li-ion conductivity), at least one glass former (in particular selected from SiO2, Al2O3, B2O3, P2O5), where SiO2 and / or P2O5 are necessarily present and the proportion of SiO2 and P2O5 together in the total weight of the glass formers is at least 25% by weight, i.e. (SiO2+P2O5) / (SiO2+B2O3+Al2O3+P2O5)≧0.25, each in % by weight. This minimum content of SiO2 and / or P2O5 is favorable for the stabilization of the amorphous phase (also called glass phase). B2O3 is not preferred as the sole glass former, since it may lead to phase separation of the glass phase, in which case there is no positive effect on the CCD. Al2O3 is similarly not preferred as the sole glass former because small amounts of Al2O3 can dissolve in the crystalline phase, making it difficult to form an amorphous phase, and larger amounts of Al2O3 can form undesirable secondary phases.
[0006] Foreign glass formers such as Nb2O5, Ta2O5, PbO, Bi2O3, GeO2, SeO3, TeO3, Sb2O3 or As2O3 are not effective for the production of an amorphous phase in the sense of the present invention, because in the case of Nb2O5 and Ta2O5 they dissolve into the crystalline phase, and in the case of PbO, Bi2O3, GeO2, SeO3, TeO3, Sb2O3 and As2O3 they are multivalent and therefore reduced in contact with lithium metal, lowering the CCD. The amount of multivalent elements in the lithium ion conducting material, especially the glass ceramic, in particular the total proportion of PbO, Bi2O3, GeO2, SeO3, TeO3, Sb2O3 and As2O3, is preferably less than 0.5% by weight, for example at most 0.2% by weight or at most 0.1% by weight. The lithium ion conductive material may be free of, for example, PbO, Bi2O3, GeO2, SeO3, TeO3, Sb2O3, and / or As2O3.
[0007] The composition of the amorphous phase can be selected so that undesirable interactions with the LLZO crystals (e.g., transformation of LLZO into a less conductive tetragonal form) do not occur. For example, too high a Li2O content in the amorphous phase can cause transformation from a cubic form to a less conductive tetragonal form of LLZO. Thus, the Li2O content of the amorphous phase can be limited, for example, to at most 5.00 wt%, at most 4.50 wt%, at most 4.00 wt%, or at most 3.50 wt%, based on the total weight of the lithium ion conductive material. The Li2O content of the amorphous phase can be, for example, at least 0.05 wt%, at least 0.20 wt%, at least 0.40 wt%, or at least 0.60 wt%, based on the total weight of the lithium ion conductive material. The Li2O content of the amorphous phase can be in the range of, for example, 0.05 to 5.00 wt%, 0.20 to 4.50 wt%, 0.40 to 4.00 wt%, or 0.60 to 3.50 wt%, based on the total weight of the lithium ion conductive material.
[0008] The glass former content of the amorphous phase can be, for example, at least 0.05% by weight, preferably at least 0.10% by weight, at least 0.15% by weight, at least 0.20% by weight, at least 0.25% by weight, at least 0.30% by weight, at least 0.35% by weight, at least 0.40% by weight, at least 0.45% by weight, or at least 0.50% by weight, based on the total weight of the lithium ion conducting material. The glass former content of the amorphous phase can be, for example, at most 4.00% by weight, at most 3.50% by weight, at most 3.00% by weight, at most 2.50% by weight, at most 2.00% by weight, at most 1.50% by weight, at most 1.00% by weight, at most 0.80% by weight, at most 0.75% by weight, or at most 0.70% by weight, based on the total weight of the lithium ion conducting material. The glass former content of the amorphous phase can be in the range of, for example, 0.05 to 4.00 wt %, 0.10 to 3.50 wt %, 0.15 to 3.00 wt %, 0.20 to 2.50 wt %, 0.25 to 2.00 wt %, 0.30 to 1.50 wt %, 0.35 to 1.00 wt %, 0.40 to 0.80 wt %, 0.45 to 0.75, or 0.50 to 0.70 wt %, based on the total weight of the lithium ion conductive material.
[0009] The glass former content of the lithium ion conducting material can be, for example, at least 0.05% by weight, preferably at least 0.10% by weight, at least 0.15% by weight, at least 0.20% by weight, at least 0.25% by weight, at least 0.30% by weight, at least 0.35% by weight, at least 0.40% by weight, at least 0.45% by weight, or at least 0.50% by weight, based on the total weight of the lithium ion conducting material. The glass former content of the lithium ion conducting material can be, for example, at most 4.00% by weight, at most 3.50% by weight, at most 3.00% by weight, at most 2.50% by weight, at most 2.00% by weight, at most 1.50% by weight, at most 1.00% by weight, at most 0.80% by weight, at most 0.75% by weight, or at most 0.70% by weight, based on the total weight of the lithium ion conducting material. The glass former content of the lithium ion conductive material can be in the range of, for example, 0.05 to 4.00 wt %, 0.10 to 3.5 wt %, 0.15 to 3.00 wt %, 0.20 to 2.50 wt %, 0.25 to 2.00 wt %, 0.30 to 1.50 wt %, 0.35 to 1.00 wt %, 0.40 to 0.80 wt %, 0.45 to 0.75, or 0.50 to 0.70 wt %, based on the total weight of the lithium ion conductive material.
[0010] The glass formers are present in the amorphous phase and not in the crystalline phase, so that the glass former content of the amorphous phase (relative to the total weight of the lithium ion conductive material) corresponds to the glass former content of the lithium ion conductive material (relative to the total weight of the lithium ion conductive material). Here, Al2O3 is an exception, as Al2O3 can also be present in the crystalline phase if the crystalline phase has a garnet structure, especially in the case of lithium lanthanum zirconate (LLZO). However, the solubility of Al2O3 in the crystalline phase with a garnet structure is limited. Depending somewhat on the composition and manufacturing process, the amount of Al2O3 per formula unit of LLZO is about 0.1 mol, i.e., Li 6.4 Al 0.2 La3Zr 12 O 12 This means that one or more divalent cations M II, one or more trivalent cations M III , one or more tetravalent cations M IV , one or more pentavalent cations M V This also applies to doped variants of this garnet, which are doped with Al2O3. Thus, when calculating the amorphous phase from the composition Al2O3, amounts up to 0.1 mol of Al2O3 per formula unit of garnet are assigned to the crystalline phase. Excess Al2O3, i.e., any amount above 0.1 mol of Al2O3 per formula unit of garnet, is assigned to the amorphous phase.
[0011] The amorphous phase can be produced by a manufacturing process via the melt, in which an amorphous phase, which in particular comprises and in particular consists of excess Li2O and glass formers, is also formed during solidification in addition to the crystalline LLZO. The glass formers mentioned do not "fit" into the crystalline structure of LLZO due to their small ionic radius. Furthermore, the amorphous phase can also be produced separately, for example by a melting process, and then added to and mixed with the crystalline phase. This can be achieved, for example, by grinding the crystalline and amorphous phases. Other manufacturing and mixing processes are also conceivable.
[0012] During sintering of glass ceramics, for example when or for use as separators, amorphous phases accumulate, especially at the grain boundaries.
[0013] The present invention provides a significantly increased CCD current, especially 0.5 mA / cm 2 greater than, for example, at least 1.0 mA / cm 2 or even higher CCD can be achieved. Complicated further process steps, such as the insertion of an intermediate layer between the negative electrode and the separator, can be avoided by the solution according to the invention.
[0014] The lithium-ion conducting materials according to the invention, in particular the glass ceramics or the lithium-ion conducting LLZO materials according to the invention, can be used alone or together with other battery materials, sintered, in inorganic ceramic electrolytes of rechargeable lithium-ion batteries, in particular solid-state lithium-ion batteries (ASSB). Here, on the one hand, the use as separators is also conceivable, which, when introduced between the electrodes, protect the electrodes against undesired short circuits and thus ensure the function of the entire system. Here, the separators according to the invention are characterized by an improved stability of the dendrites, which allows charging at high current densities without short circuits (fast charging). On the other hand, co-sintering with electrode materials is also conceivable, in which case the solid electrolyte transports the charge carriers (lithium ions) between the electrode material and the conductive electrode, depending on whether the battery is discharged or charged.
[0015] The material of the present invention is a lithium ion conducting material, in particular a glass ceramic. The conductivity is, for example, at least 1×10 -5 S / cm, at least 3×10 -5 S / cm, at least 7×10 -5 S / cm, at least 1×10 -4 S / cm, or at least 2×10 -4 The conductivity can be, for example, at most 1×10 -2 S / cm, maximum 5×10 -3 S / cm, maximum 4×10 -3 S / cm, maximum 3×10 -3 S / cm, or at most 2×10 -3 The conductivity can be, for example, 1×10 -5 S / cm~1×10 -2 S / cm, 3×10 -5 S / cm~5×10 -3 S / cm, 7×10 -5 S / cm~4×10 -3 S / cm, 1×10 -4 S / cm~3×10 -3 S / cm, or 2 x 10 -4S / cm~2×10 -3 The conductivity can be determined using impedance spectroscopy. For this purpose, the material is 50 = 1 μm in size and then pressed into a compact, which can be sintered at 1130 °C for 30 min. To avoid sample degradation due to contact with water, sample preparation can be performed anhydrous.
[0016] The lithium ion conductive material of the present invention includes a crystalline phase and an amorphous phase. The amorphous phase can in particular include Li2O and at least one glass former selected from SiO2, B2O3, Al2O3, P2O5 and a combination of two or more thereof, where the sum of the proportions of SiO2 and P2O5 relative to the total weight of the glass former is at least 25%, i.e., (SiO2+P2O5) / (SiO2+B2O3+Al2O3+P2O5)≧0.25, each in weight %. The sum of the proportions of SiO2 and P2O5 relative to the total weight of the glass former can be, for example, at least 30%, at least 40%, at least 50%, at least 60%, at least 70%, at least 80%, at least 90%, at least 95%, or even 100%. Thus, the lithium ion conductive material may not include B2O3 and Al2O3.
[0017] SiO2 is a particularly preferred glass former of the present invention. The proportion of SiO2 to the total weight of the glass formers can be, for example, at least 25%, i.e., (SiO2) / (SiO2+B2O3+Al2O3+P2O5)≧0.25, each in weight %. The proportion of SiO2 to the total weight of the glass formers can be, for example, at least 30%, at least 40%, at least 50%, at least 60%, at least 70%, at least 80%, at least 90%, at least 95%, or even 100%. Thus, the lithium ion conductive material may be free of P2O5, B2O3 and Al2O3. In particular, the glass former can be SiO2. SiO2 is particularly advantageous for significantly increasing the critical current density.
[0018] The proportion of Li2O in the lithium ion conductive material of the present invention can be, for example, at least 10.0 wt%, at least 10.5 wt%, or at least 11.0 wt%. The proportion of Li2O in the lithium ion conductive material of the present invention can be, for example, at most 15.0 wt%, at most 14.5 wt%, or at most 14.0 wt%. The proportion of Li2O in the lithium ion conductive material of the present invention can be, for example, in the range of 10.0 to 15.0 wt%, 10.5 to 14.5 wt%, or 11.0 to 14.0 wt%.
[0019] The total proportion of rare earth oxides RE2O3, preferably La2O3, Gd2O3 and / or Y2O3 in the lithium ion conductive material of the present invention can be, for example, at least 45% by weight, at least 48% by weight, or at least 50% by weight. The total proportion of rare earth oxides RE2O3, preferably La2O3, Gd2O3 and / or Y2O3 in the lithium ion conductive material of the present invention can be, for example, at most 70% by weight, at most 65% by weight, or at most 60% by weight. The total proportion of rare earth oxides RE2O3, preferably La2O3, Gd2O3 and / or Y2O3 in the lithium ion conductive material of the present invention can be, for example, in the range of 45-70% by weight, 48-65% by weight, or 50-60% by weight.
[0020] The total proportion of ZrO2 and HfO2 in the lithium ion conductive material of the present invention can be, for example, at least 17% by weight, at least 18% by weight, or at least 19% by weight. The total proportion of ZrO2 and HfO2 in the lithium ion conductive material of the present invention can be, for example, at most 35% by weight, at most 33% by weight, or at most 31% by weight. The total proportion of ZrO2 and HfO2 in the lithium ion conductive material of the present invention can be, for example, in the range of 17 to 35% by weight, 18 to 33% by weight, or 19 to 31% by weight.
[0021] The proportion of SiO2 in the lithium ion conductive material of the present invention can be, for example, at least 0.05% by weight, preferably at least 0.10% by weight, at least 0.15% by weight, at least 0.20% by weight, at least 0.25% by weight, at least 0.30% by weight, at least 0.35% by weight, or at least 0.40% by weight. The proportion of SiO2 in the lithium ion conductive material of the present invention can be, for example, at most 2.00% by weight, at most 1.75% by weight, at most 1.50% by weight, at most 1.25% by weight, at most 1.00% by weight, at most 0.90% by weight, at most 0.85% by weight, or at most 0.80% by weight. The proportion of SiO2 in the lithium ion conductive material of the present invention can be in the range of, for example, 0.05 to 2.00 weight%, 0.10 to 1.75 weight%, 0.15 to 1.50 weight%, 0.20 to 1.25 weight%, 0.25 to 1.00 weight%, 0.30 to 0.90 weight%, 0.35 to 0.85 weight%, or 0.40 to 0.80 weight%.
[0022] The total proportion of Ta2O5, Nb2O5 and Al2O3 in the lithium ion conductive material of the present invention can be, for example, at least 0.5% by weight, at least 0.75% by weight, or at least 1% by weight. The total proportion of Ta2O5, Nb2O5 and Al2O3 in the lithium ion conductive material of the present invention can be, for example, at most 15% by weight, at most 13.5% by weight, or at most 12% by weight. The total proportion of Ta2O5, Nb2O5 and Al2O3 in the lithium ion conductive material of the present invention can be, for example, in the range of 0.5 to 15% by weight, 0.75 to 13.5% by weight, or 1 to 12% by weight.
[0023] The lithium ion conductive material of the present invention may, for example, contain the following components in the indicated proportions (by weight %): [Table 1]
[0024] More preferably, the lithium ion conductive material of the present invention may contain, for example, the following components in the indicated proportions (by weight %): [Table 2]
[0025] Particularly preferably, the lithium ion conductive material of the present invention may contain, for example, the components shown below in the proportions (in weight %) shown: [Table 3]
[0026] Particularly preferably, the lithium ion conductive material of the present invention may contain, for example, the components shown below in the proportions (in weight %) shown: [Table 4]
[0027] Particularly preferably, the lithium ion conductive material of the present invention may contain, for example, the components shown below in the proportions (in weight %) shown: [Table 5]
[0028] Particularly preferably, the lithium ion conductive material of the present invention may contain, for example, the components shown below in the proportions (in weight %) shown: [Table 6]
[0029] In this disclosure, when a material is described as being free or free of a certain component, this means that this component may be present at most as an impurity. This means that this component is not added in a substantial amount. According to the present invention, an insubstantial amount is an amount of at most 0.05% by weight, or at most 0.04% by weight.
[0030] The proportion of the amorphous phase in the lithium ion conductive material corresponds in particular to the sum of the proportion of Li2O in the amorphous phase (relative to the total weight of the lithium ion conductive material) and the proportion of at least one glass former in the amorphous phase (relative to the total weight of the lithium ion conductive material). If the proportion of the amorphous phase in the lithium ion conductive material is too high, the lithium ion conductivity of the lithium ion conductive material may be impaired. It is therefore advantageous to limit the upper limit of the proportion of the amorphous phase in the lithium ion conductive material. Preferably, the proportion of the amorphous phase in the lithium ion conductive material is less than 5.0% by weight, in particular at most 4.9% by weight, at most 4.8% by weight, at most 4.7% by weight, at most 4.6% by weight, at most 4.5% by weight, at most 4.4% by weight, at most 4.3% by weight, at most 4.2% by weight, at most 4.1% by weight or at most 4.0% by weight. The proportion of the amorphous phase in the lithium ion conductive material can be, for example, at least 0.1 wt%, at least 0.15 wt%, at least 0.2 wt%, at least 0.3 wt%, at least 0.4 wt%, at least 0.5 wt%, at least 0.6 wt%, at least 0.7 wt%, at least 0.8 wt%, at least 0.9 wt%, or at least 1.0 wt%. The proportion of the amorphous phase in the lithium ion conductive material can be, for example, in the range of 0.1 to <5.0 wt%, 0.15 to 4.9 wt%, 0.2 to 4.8 wt%, 0.3 to 4.7 wt%, 0.4 to 4.6 wt%, 0.5 to 4.5 wt%, 0.6 to 4.4 wt%, 0.7 to 4.3 wt%, 0.8 to 4.2 wt%, 0.9 to 4.1 wt%, or 1.0 to 4.0 wt%.
[0031] The determination of the proportion of crystalline and amorphous phases in a lithium ion conducting material is made in particular on the basis of the composition of the lithium ion conducting material. For this purpose, the composition is converted from weight % to atomic % using the molecular formula of the crystalline phase. The elements that form a crystalline phase according to the molecular formula are then assigned to this phase (the same procedure is used for several crystalline phases). The amorphous phase is assigned the excess of Li, O and glass formers. This procedure is simplified if the composition in atomic % is normalized by one of the stoichiometric factors of the molecular formula of the crystalline phase. This is done by converting the composition in weight % to atomic % using the molecular formula of the crystalline phase Li 7-3x+y-z Al x M y II M 3-y III M 2-z IV M z V O 12 The following is an example of the composition in atomic percent: II +M III =3 (or M IV +M V = 2) to obtain the composition in pfu (parts per formula unit). This composition is divided into crystal-forming components and components that are not incorporated into the stoichiometric crystal: excess Li and O, as well as Si, P, B, and Al (Al has limited solubility in the garnet structure, so amounts up to 0.2 pfu are counted as crystal-forming components. If Al is present in excess, the difference from 0.2 pfu is assigned to the amorphous phase). The amorphous phase in pfu is then converted back to the weight % of the oxides present using their respective atomic weights. The weight percentage of the amorphous phase in the lithium ion conductive material is the sum of the weight percentages in weight % of the oxides in the amorphous phase (relative to the total weight of the lithium ion conductive material).
[0032] The lithium ion conductive material of the present invention has a current density of 0.5 mA / cm 2 The critical current density is, for example, at least 0.6 mA / cm 2 , at least 0.7mA / cm 2, at least 0.8mA / cm 2 , at least 0.9mA / cm 2 , or at least 1.0 mA / cm 2 The critical current density can be, for example, at most 20 mA / cm 2 , maximum 18mA / cm 2 , maximum 16mA / cm 2 , maximum 14mA / cm 2 , maximum 12mA / cm 2 , or at most 10mA / cm 2 The critical current density can be, for example, >0.5 to 20 mA / cm 2 , 0.6~18mA / cm 2 , 0.7~16mA / cm 2 , 0.8~14mA / cm 2 , 0.9~12mA / cm 2 , or 1.0 to 10mA / cm 2 In some embodiments, the critical current density can be in the range of at most 7.5 mA / cm 2 , maximum 5.0mA / cm 2 , maximum 4.0mA / cm 2 , maximum 3.0mA / cm 2 , maximum 2.0mA / cm 2 , or at most 1.2mA / cm 2 It is.
[0033] The critical current density can be measured by contacting lithium with two opposing faces of a disk-shaped sintered body (diameter 8.5 mm, height 1 mm). 2 The current density is 50μA / cm 2 The current density is increased by 1000 ds and the voltage is recorded. One cycle is performed for each current density, and the charge / discharge process is performed for 30 minutes each. The critical current density is defined as the current density at which the cell shorts out. At this current density, the voltage no longer follows the current density according to Ohm's law and an immediate voltage drop occurs. To produce the sintered body, the lithium ion conductive material is d 50= 1 μm in size and then pressed into a compact, which can be sintered at 1130 °C for 30 min. To avoid sample degradation due to contact with water, sample preparation can be performed anhydrous.
[0034] The lithium ion conducting material of the present invention may in particular be a glass-ceramic.
[0035] Glass-ceramics within the meaning of the present invention are materials produced from a homogeneous melt of the components by cooling and spontaneous crystallization or by cooling and a subsequent controlled ceramization process. The forming or grinding steps can be carried out before, during or after cooling.
[0036] The lithium ion conductive material of the present invention comprises a crystalline phase and an amorphous phase. The crystalline phase can comprise a predominant crystalline phase. The predominant crystalline phase is the crystalline phase that has the highest proportion by weight of the crystalline phase of the lithium ion conductive material. The predominant crystalline phase in particular has a proportion of at least 50% by weight, for example more than 50% by weight, at least 60% by weight, at least 70% by weight, at least 80% by weight, at least 90% by weight, at least 95% by weight, or even 100% by weight of the crystalline phase of the lithium ion conductive material. Thus, the crystalline phase of the lithium ion conductive material can consist of the predominant crystalline phase.
[0037] The main crystalline phase may in particular have a garnet structure. However, the main crystalline phase may also have a rock salt structure, a perovskite structure, an inverse perovskite structure or a NASICON structure. The main crystalline phase may, for example, be in the cubic system. The main crystalline phase may, for example, comprise or consist of lithium lanthanum zirconate (LLZO).
[0038] The main crystalline phase of the lithium ion conductive material is, in particular, a crystalline phase having the molecular formula Li 7-3x+y-z Al x M y II M 3-y III M2-z IV M z V O 12±δ where M II contains one or more divalent cations, M III contains one or more trivalent cations, M IV contains one or more tetravalent cations, M V contains one or more pentavalent cations, x+z>0, y<1 and δ<0.5. Particularly preferred is M III contains one or more lanthanides and / or yttrium. Particularly preferred is M IV contains zirconium or hafnium. Particularly preferably, M V contains niobium or tantalum. Particularly preferably, M III contains one or more lanthanides and / or yttrium, M IV contains zirconium or hafnium, M V contains niobium or tantalum.
[0039] The lithium ion conducting material of the present invention comprises a crystalline phase and an amorphous phase. The crystalline phase can be present, for example, in the form of crystallites separated by grain boundaries in the lithium ion conducting material. The amorphous phase can in particular be present at the grain boundaries (FIG. 1). The amorphous phase can be present, for example, at least 1.5 g / cm. 3 The density of the powder may be 0.01 to 0.01.
[0040] The present invention also relates to a method for producing a lithium ion conducting material, in particular a lithium ion conducting material according to the invention, which method may in particular comprise the following steps: Melting the starting material; Cooling the melt.
[0041] The starting materials (also called raw materials) can be melted, for example, in a skull crucible (especially open at the top). Preferably, the raw materials are mixed and the resulting mixture is preheated. In particular, burner heating can be used for this. The lowest conductivity can be achieved by preheating. Once the so-called coupling temperature is reached, further heating and homogenization of the melt can be achieved by high-frequency coupling, in particular through an induction coil. To improve the homogenization of the melt, it can be stirred, in particular with a water-cooled stirrer. After complete homogenization, for example, a sample can be taken directly from the melt (fast cooling), while the rest of the melt can be cooled slowly by switching off the high-frequency.
[0042] The materials thus produced can be converted into lithium-ion conducting, especially glass-ceramic, materials with a garnet-like predominant crystalline phase by either solidifying directly from the melt or by quenching and then by temperature treatment (ceramization). Samples taken directly from the melt show spontaneous crystallization independent of cooling, making it possible to dispense with the subsequent ceramization step.
[0043] The present invention also relates to the use of the lithium ion conductive material of the present invention in solid-state lithium ion batteries, in particular as a separator. The lithium ion conductive material can also be used in the negative and / or positive electrodes, in particular after co-sintering with an electrode material.
[0044] The present invention also relates to a solid-state lithium-ion battery comprising the lithium-ion conducting material of the present invention. [Brief description of the drawings]
[0045] [Figure 1] Electron micrographs of sintered separators made with the materials of a) Example 1 and b) Example V1. The SiO2-rich amorphous phase of Example 1 accumulates at the grain boundaries (dark areas).
[0046] Working Example Table 1 below shows Example 1 according to the invention and two comparative examples V1 and V2.
[0047] [Table 7-1] [Table 7-2]
[0048] The raw materials were mixed according to the composition in Table 1 and charged into an open-top skull crucible, where an excess of about 5% was used relative to the amount of Li2O to compensate for the evaporation of Li2O. The mixture first had to be preheated to achieve a certain minimum conductivity. For this purpose, burner heating was used. After reaching the coupling temperature, further heating and homogenization of the melt was achieved by high-frequency coupling through an induction coil. Stirring was performed with a water-cooled stirrer to improve the homogenization of the melt. After complete homogenization, a sample was taken directly from the melt (quenching), while the rest of the melt was cooled slowly by switching off the high-frequency.
[0049] The materials thus produced can be transformed into glass-ceramic materials with a predominant garnet-like crystalline phase by either solidifying directly from the melt or by quenching and then temperature treatment (ceramization). Samples taken directly from the melt showed spontaneous crystallization independent of cooling, making it possible to dispense with the subsequent ceramization step. From the glass-ceramics thus obtained, samples were prepared for impedance spectroscopy to measure the conductivity and CCD (critical current density). For this purpose, the materials were d 50 = 1 μm in size and then pressed into compacts, which were sintered at 1130 °C for 30 min. Sample preparation was carried out anhydrous to avoid sample degradation due to contact with water.
[0050] The compositions of the crystalline and amorphous phases are given in parts per formula unit (pfu) of lithium lanthanum zirconate. The amorphous phase is oxidizing, so oxygen (O 2- ) to balance the charge of the elements / cations. For this, the composition in weight percent is first converted to the composition in atomic percent. The composition in atomic percent is then normalized to La=3 to obtain the composition in pfu. This composition is separated into the LLZO forming components Li, La, Zr, Hf, Ta, and O, and the amorphous phase (components that are not incorporated into the stoichiometric LLZO crystal, namely Si, as well as excess Li and O). Here, the composition of the stoichiometric LLZO crystal is Li 7-x La3Zr 2-x-y Ta x Hf y O 12±δ This composition division is based on the assumption that all elements that can form stoichiometric LLZO crystals also exist as LLZO crystals, and elements that cannot be incorporated or are present in excess exist as amorphous phases. The amorphous phase in pfu is then converted back to weight percent using the respective atomic weights to determine the percentage of oxides in weight percent of the total weight of the lithium ion conductive material.
[0051] The weight of the amorphous phase (Table 2) is the sum of the oxides in the amorphous phase from Table 1 in weight percent.
[0052] To measure the critical current density (CCD), lithium is placed in contact with two opposing faces of a disk-shaped sintered body (diameter 8.5 mm, height 1 mm). 2 The current density is 50μA / cm 2 The cells are cycled at increasing current densities and the voltage is recorded. One cycle is performed for each current density, and the charge / discharge process is carried out for 30 minutes each. The critical current density is defined as the current density at which the cell shorts out. At this current density, the voltage no longer follows Ohm's law current density and an immediate voltage drop occurs.
[0053] Table 2 below shows the percentage of amorphous phase and the critical current density CCD of Example 1 and the two comparative examples V1, V2.
[0054] [Table 8]
[0055] In Example 1, the glass former SiO2 was added as required, thereby making it possible to significantly increase the proportion of the amorphous phase and the critical current density compared to Comparative Examples V1 and V2.
[0056] In comparative example V2, the proportion of the amorphous phase was increased by about 10 times compared to comparative example V1 by increasing the proportion of Li2O in the raw material composition. Nevertheless, the CCD of V2 did not change compared to V1. Therefore, increasing the proportion of glass formers, particularly preferably SiO2, is particularly advantageous for further increasing the CCD.
Claims
1. A lithium ion conducting material comprising a crystalline phase and an amorphous phase, the lithium ion conducting material having a current density of 0.5 mA / cm 2 A lithium ion conducting material with a critical current density of .
2. The amorphous phase is Li 2 O and SiO 2 , B 2 O 3 , Al 2 O 3 , P 2 O 5 and a combination of two or more thereof, wherein the content of the glass former relative to the total weight of the lithium ion conductive material is at least 0.05 wt %, and the content of SiO relative to the total weight of the glass former is at least 0.05 wt %. 2 and P 2 O 5 2. The lithium ion conductive material according to claim 1, wherein the total proportion of is at least 25% by weight.
3. The SiO based on the total weight of the glass former 2 3. The lithium ion conductive material according to claim 2, wherein the proportion of is at least 25% by weight.
4. 4. The lithium ion conducting material according to claim 1, wherein the lithium ion conducting material is a glass ceramic.
5. 5. The lithium ion conductive material according to claim 1, wherein the crystalline phase comprises a predominant crystalline phase, the predominant crystalline phase having a proportion of the crystalline phase of at least 50% by weight, and the predominant crystalline phase is present in a cubic system.
6. 6. The lithium ion conductive material according to claim 1 , wherein the crystalline phase comprises a predominant crystalline phase, the predominant crystalline phase having a proportion of the crystalline phase of at least 50% by weight, and the predominant crystalline phase has a garnet structure.
7. 7. The lithium ion conducting material of claim 5 or 6, wherein the predominant crystalline phase comprises lithium lanthanum zirconate (LLZO).
8. The main crystalline phase has the molecular formula Li 7-3x+y-z A x M y II M 3-y III M 2-z IV M z V O 12±δ M II contains one or more divalent cations, M III contains one or more trivalent cations, M IV contains one or more tetravalent cations, M V 8. The lithium ion conductive material according to claim 5, wherein x+z>0, y<1 and δ<0.
5.
9. Li in the amorphous phase 2 9. The lithium ion conductive material according to claim 1, wherein the proportion of O is 0.05 to 5.00% by weight based on the total weight of the lithium ion conductive material.
10. 10. The lithium ion conductive material according to claim 1 , wherein the proportion of the amorphous phase in the lithium ion conductive material is less than 5% by weight.
11. A method for producing a lithium ion conductive material according to any one of claims 1 to 10, comprising the steps of: Melting the starting materials; cooling the melt A method comprising:
12. 11. Use of a lithium ion conducting material according to any one of claims 1 to 10 in a solid-state lithium ion battery, in particular as a separator.
Citation Information
Patent Citations
Surface coated and modified lithium lanthanum zirconium oxygen-based solid electrolyte material and preparation method and application thereof
CN110265709A
Lithium ion conductive solid electrolyte and method of manufacturing the same
JP2009227474A
Lithium ion conductive inorganic solid composite
JP2014229579A
Method for producing glass-ceramic ion conductor
JP2016117637A
Ion-conducting glass ceramics with a garnet-type crystal structure
JP2017511781A