Coated steel sheet with excellent corrosion resistance and bendability and its manufacturing method
The Zn-Mg-Al plated steel sheet with a controlled Zn single phase structure addresses the challenges of corrosion resistance and bendability by optimizing the plating layer composition and manufacturing process, resulting in a steel sheet with improved adhesion and structural integrity.
Patent Information
- Application Number
- JP2024519265
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-30
- Filing Date
- 2022-09-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-09-27
AI Technical Summary
Existing zinc-based plated steel sheets face challenges in achieving both excellent corrosion resistance and bendability due to the formation of hard intermetallic compounds during bending, which cause cracks, and issues with plating adhesion due to dross formation and reduced reactivity with the steel sheet.
A plated steel sheet composition comprising a Zn-Mg-Al based plating layer with a controlled Mg and Al content, featuring a soft Zn single phase formed along the outer line of MgZn2 phases, and a controlled manufacturing process including specific plating bath conditions and cooling rates to ensure interfacial adhesion and bendability.
The solution provides a plated steel sheet with enhanced corrosion resistance, improved bendability, and superior plating adhesion by optimizing the plating layer composition and manufacturing process, ensuring a uniform and stable structure.
Smart Images

Figure 2024539570000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a highly corrosion-resistant plated steel sheet having excellent corrosion resistance and bendability, and a method for producing the same. [Background technology]
[0002] When exposed to a corrosive environment, zinc-based plated steel sheets have a sacrificial corrosion protection property in which zinc, which has a lower redox potential than iron, corrodes first, suppressing the corrosion of the steel material. In addition, as the zinc in the plated layer oxidizes, it forms a dense corrosion product on the surface of the steel material, insulating the steel material from the oxidizing atmosphere and improving the corrosion resistance of the steel material. Due to these advantageous properties, the range of applications of zinc-based plated steel sheets has recently been expanded to building materials, home appliances, and automotive steel sheets.
[0003] However, the corrosive environment is gradually worsening due to increased air pollution accompanying industrial advancement, and strict regulations on resources and energy conservation are creating a growing need for the development of steel materials with superior corrosion resistance to conventional galvanized steel materials.
[0004] In order to solve these problems, various researches are being conducted on the manufacturing technology of zinc alloy-plated steel sheets, which improve the corrosion resistance of steel materials by adding elements such as aluminum (Al) and magnesium (Mg) to the zinc plating bath. A representative example is Zn-Mg-Al zinc alloy-plated steel sheets, which further add Mg to the Zn-Al plating composition.
[0005] On the other hand, Zn-Mg-Al zinc alloy plated steel sheets are often used after processing, but they have the disadvantage that they contain a large amount of intermetallic compounds with high hardness in the plating layer, which causes cracks in the plating layer during bending, resulting in poor bending workability.
[0006] In addition, Zn-Mg-Al zinc alloy plated steel sheets have the problem that the adhesion of the plating may be reduced due to the adhesion of oxides such as dross during the plating process in the plating bath or due to weakening of the reactivity with the steel sheet.
[0007] Therefore, the reality is that no technology has been developed to date that can satisfy the high demand for excellent corrosion resistance, bendability, and plating adhesion. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean Patent Publication No. 2010-0073819 Summary of the Invention [Problem to be solved by the invention]
[0009] According to one aspect of the present invention, there are provided a plated steel sheet having excellent corrosion resistance and bendability, and a method for producing the same.
[0010] According to yet another aspect of the present invention, there are provided a plated steel sheet having excellent coating adhesion as well as corrosion resistance and bendability, and a method for producing the same.
[0011] The object of the present invention is not limited to the above. Anyone having ordinary skill in the art to which the present invention pertains will have no difficulty in understanding additional objects of the invention from the entire contents of the specification of the present invention. [Means for solving the problem]
[0012] One aspect of the present invention is A steel sheet comprising a base steel sheet and a Zn-Mg-Al-based coating layer provided on at least one surface of the base steel sheet, The present invention provides a plated steel sheet, in which the plating layer includes an MgZn2 phase and a Zn single phase formed along the outer line of the MgZn2 phase.
[0013] Another aspect of the present invention is Plating bath temperature (T B ) for T B +10℃~T BA step of immersing the base steel sheet in a coating bath containing, by weight%, 4.0 to 7.0% Mg, 11.0 to 19.5% Al, the balance being Zn and other unavoidable impurities, so as to satisfy a drawing temperature of +50°C, to perform hot-dip galvanizing; performing air wiping on the hot-dip galvanized steel sheet using an inert gas so as to satisfy the following Relational Formula 1; cooling the air-wiped steel sheet to the end of solidification temperature at an average cooling rate of 2 to 5°C / s. The present invention provides a method for producing a plated steel sheet, comprising the steps of: [Equation 1] 0.005≦P air / (W air ×T) (In the above Relational Formula 1, the above W air represents the distance between the air knives, in mm. air represents the pressure of the air knife in kPa. T represents the temperature of the supplied inert gas in °C. Effect of the Invention
[0014] According to one aspect of the present invention, it is possible to provide a plated steel sheet having excellent corrosion resistance and bendability, and a method for manufacturing the same.
[0015] According to another aspect of the present invention, it is possible to provide a plated steel sheet that is excellent not only in corrosion resistance and bendability but also in plating adhesion, and a method for producing the same.
[0016] The various yet significant advantages and effects of the present invention are not limited to the above, but can be more easily understood in the course of describing specific embodiments of the present invention. [Brief description of the drawings]
[0017] [Figure 1] 1 shows a photograph of the surface of the plated steel sheet obtained in Example 1, magnified 1,500 times, taken with a Field Emission Scanning Electron Microscope (hereinafter referred to as "FE-SEM"). [Diagram 2] 1 shows a photograph of the surface of the plated steel sheet obtained in Example 3, magnified 5,000 times, taken with a field emission scanning electron microscope (FE-SEM). [Diagram 3] 1 shows a photograph of the surface of the plated steel sheet obtained in Example 4, magnified 5,000 times, taken with a field emission scanning electron microscope (FE-SEM). [Figure 4] This is an enlarged view of the square portion shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The terms used in this specification are for the purpose of describing particular embodiments and are not intended to limit the present invention. Furthermore, the singular forms used in this specification also include the plural forms unless the related definition clearly indicates otherwise.
[0019] The meaning of "comprise" as used in the specification is to specify a feature and does not exclude the presence or addition of other features.
[0020] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs. Dictionary-defined terms are to be interpreted as having a meaning consistent with the relevant technical literature and the presently disclosed content.
[0021] Hereinafter, a "plated steel sheet" according to one aspect of the present invention will be described in detail. In the present invention, the content of each element is expressed in percent by weight unless otherwise specified.
[0022] In conventional Zn-Mg-Al zinc alloy plated steel sheets, magnesium is added to improve corrosion resistance. However, if too much magnesium is added, there is a problem that more dross is generated floating in the plating bath, and the dross must be removed frequently, so the upper limit of magnesium addition was limited to 3%.
[0023] Therefore, research was conducted to further improve corrosion resistance by increasing the amount of Mg added beyond 3%. However, as the amount of Mg added increases, the plating layer contains a large amount of intermetallic compounds with high hardness, which causes cracks in the plating layer during bending, resulting in a decrease in bendability (or bending workability).
[0024] In addition to the bendability problem, Zn-Mg-Al zinc alloy plated steel sheets also have the problem of reduced coating adhesion due to the adhesion of Mg-based dross.
[0025] For this reason, it has been technically difficult with conventional techniques to provide a plated steel sheet that not only ensures corrosion resistance but also has excellent bendability and plating adhesion.
[0026] Therefore, the present inventors conducted extensive research in order to solve the above-mentioned problems and at the same time provide a plated steel sheet that is excellent not only in corrosion resistance but also in bendability and / or plating adhesion. As a result, they found that not only the composition of the plating layer but also the Zn single phase formed along the outer line of the MgZn2 phase formed in the plating layer is an important factor, and thus completed the present invention.
[0027] Therefore, the following will specifically describe the configuration of a plated steel sheet that has excellent corrosion resistance and, at the same time, excellent weldability and / or chemical conversion treatability.
[0028] First, the plated steel sheet according to the present invention includes a base steel sheet and a Zn-Mg-Al-based plating layer provided on at least one surface of the base steel sheet.
[0029] In the present invention, the type of base steel sheet is not particularly limited. For example, the base steel sheet may be an Fe-based base steel sheet used as a base steel sheet for ordinary zinc-based plated steel sheets, i.e., a hot-rolled steel sheet or a cold-rolled steel sheet, but is not limited thereto. Alternatively, the base steel sheet may be, for example, a carbon steel, an extra-low carbon steel, or a high manganese steel used as a material for construction, home appliances, or automobiles.
[0030] However, as an example, the above-mentioned base steel sheet has, by weight%, C: more than 0% (more preferably, 0.001% or more) and 0.18% or less, Si: more than 0% (more preferably, 0.001% or more) and 1.5% or less, Mn: 0.01 to 2.7%, P: more than 0% (more preferably, 0.001% or more) and 0.07% or less, S: more than 0% (more preferably, 0.001% or more) and 0.015% or less, Al: more than 0% (more preferably, It may have a composition including: Nb: more than 0% (more preferably, 0.001% or more) and 0.06% or less, Cr: more than 0% (more preferably, 0.001% or more) and 1.1% or less, Ti: more than 0% (more preferably, 0.001% or more) and 0.06% or less, B: more than 0% (more preferably, 0.001% or more) and 0.03% or less, and the balance being Fe and other unavoidable impurities.
[0031] Although not particularly limited, according to one embodiment of the present invention, at least one surface of the base steel sheet may be provided with a Zn-Mg-Al-based plating layer made of a Zn-Mg-Al-based alloy. The plating layer may be formed on only one surface of the base steel sheet, or may be formed on both surfaces of the base steel sheet. In this case, the Zn-Mg-Al-based plating layer refers to a plating layer that contains Mg and Al and mainly contains Zn (i.e., contains 50% or more Zn).
[0032] Although not particularly limited, according to one embodiment of the present invention, the thickness of the Zn-Mg-Al-based coating layer can be 5 to 100 μm, and more preferably 10 to 90 μm. If the thickness of the coating layer is less than 5 μm, the coating layer may become very thin locally due to an error caused by the thickness deviation of the coating layer, and the corrosion resistance may be poor. If the thickness of the coating layer exceeds 100 μm, the cooling of the hot-dip coating layer may be delayed, and there may be room for solidification defects such as sagging to occur on the surface of the coating layer, and the productivity of the steel sheet may decrease in order to solidify the coating layer.
[0033] Meanwhile, although not particularly limited, according to an embodiment of the present invention, an Fe-Al-based inhibition layer may be further included between the base steel sheet and the Zn-Mg-Al-based coating layer. The Fe-Al-based inhibition layer is a layer mainly containing (for example, 60% or more) an intermetallic compound of Fe and Al, and examples of the intermetallic compound of Fe and Al include FeAl, FeAl3, Fe2Al5, etc. In addition, a component derived from the coating layer such as Zn, Mg, etc. may be further included, for example, 40% or less. The inhibition layer is a layer formed by alloying Fe diffused from the base steel sheet at the initial coating stage with the coating bath components. The inhibition layer can play a role in improving the adhesion between the base steel sheet and the coating layer, and at the same time, can play a role in preventing Fe diffusion from the base steel sheet to the coating layer. In this case, the inhibition layer may be formed continuously or discontinuously between the base steel sheet and the Zn-Mg-Al-based coating layer. With respect to the inhibition layer, except for the above description, contents commonly known in the relevant technical field can be similarly applied.
[0034] Although not particularly limited, according to one embodiment of the present invention, the thickness of the inhibition layer can be 0.02 to 2.5 μm. The inhibition layer prevents alloying and ensures corrosion resistance, but since it is brittle, it may affect workability, and the thickness can be 2.5 μm or less. However, in order to fulfill the role of the inhibition layer, it is preferable to control the thickness to 0.02 μm or more. From the viewpoint of further improving the above-mentioned effect, the upper limit of the inhibition layer thickness can be preferably 1.8 μm. In addition, the lower limit of the inhibition layer thickness can be 0.05 μm. In this case, the thickness of the inhibition layer can mean the minimum thickness in a direction perpendicular to the interface of the base steel sheet.
[0035] On the other hand, although not particularly limited, according to one embodiment of the present invention, the Zn-Mg-Al-based plating layer may contain, by weight %, 4.0-7.0% Mg, 11.0-19.5% Al, the balance being Zn and other inevitable impurities. Each component will be specifically described below.
[0036] (Mg:4.0% or more and 7.0% or less) Mg is an element that plays a role in improving the corrosion resistance of plated steel materials, and in the present invention, the Mg content in the coating layer is controlled to 4.0% or more to ensure the desired excellent corrosion resistance. On the other hand, if Mg is added excessively, not only may dross be generated, but also a large amount of hard MgZn2 phase may be formed in the coating layer, causing cracks in the coating layer during bending, thereby reducing bendability, so the Mg content can be controlled to 7.0% or less.
[0037] (Al: 11.0% or more and 19.5% or less) Generally, when Mg is added at 1% or more, it is effective in improving corrosion resistance. However, when Mg is added at 2% or more, the oxidation of Mg in the plating bath increases the generation of floating dross in the plating bath, which requires frequent removal of the dross.
[0038] Due to these problems, in the prior art, 1.0% or more of Mg is added to Zn-Mg-Al zinc alloy plating to ensure corrosion resistance, but the upper limit of the Mg content is set to 3.0% and is in common use. However, in the present invention, in order to further improve corrosion resistance, it is necessary to increase the Mg content to 4% or more. However, if the coating layer contains 4% or more of Mg, there is a problem that dross is generated due to oxidation of Mg in the coating bath. In addition, there may be a problem that the coating adhesion is weakened due to the adhesion of oxides caused by dross or the reactivity with the base steel sheet is weakened, so it is necessary to add 11.0% or more of Al. However, if excessive Al is added to suppress dross, the melting point of the coating bath becomes high, and the operating temperature becomes too high, which may cause problems due to high-temperature work such as erosion of the coating bath structure and denaturation of the steel material. Therefore, it is preferable to control the upper limit of the Al content in the coating layer to 19.5%.
[0039] (The balance is Zn and other unavoidable impurities) In addition to the above-mentioned composition of the coating layer, the balance may be Zn and other inevitable impurities. The inevitable impurities may include any impurities that may be unintentionally mixed in the normal manufacturing process of a hot-dip galvanized steel sheet, and the meaning of the inevitable impurities can be easily understood by a person skilled in the relevant technical field.
[0040] In the coated steel sheet according to the present invention, the coating layer contains a MgZn2 phase as a microstructure. In addition, various phases such as a Zn single phase, an Al-Zn binary eutectic phase, a Zn-MgZn2-Al ternary eutectic phase, an Al single phase, etc. may also be contained in the coating layer. In this specification, the MgZn2 phase means a phase mainly composed of MgZn2, and the Zn single phase means a phase mainly composed of Zn and containing 85% or more of Zn by weight. In this case, the Zn single phase may contain additional components of Al and Mg in a range of 15% or less in addition to the Zn component. The Al single phase means a phase mainly composed of Al and containing 85% or more of Al by weight, but containing components such as Zn and Mg in addition to the Al component. The Zn-MgZn2-Al ternary eutectic phase refers to a ternary eutectic phase in which the Zn phase, MgZn2 phase, and Al phase are all mixed, and the Al-Zn binary eutectic phase refers to an arrangement in which the Al phase and the Zn phase are alternately arranged in a lamellar or irregular mixed form. At this time, it should be noted that the Zn phase contained in the ternary eutectic phase is not included in the Zn single phase formed along the outer line of the MgZn2 phase described later in this specification.
[0041] On the other hand, according to the present invention, the coating layer includes a Zn single phase formed along the outer line of the MgZn2 phase. Conventional Zn-Mg-Al coated steel sheets have a problem that when the Mg content is large, 4% or more, a large amount of hard MgZn2 phase is formed in the coating layer, which causes cracks in the coating layer during bending, thereby reducing bendability.
[0042] Therefore, the inventors conducted extensive research and discovered that by precisely controlling the plating composition and manufacturing conditions and forming a soft Zn single phase along the outer line of the hard MgZn2 phase in the plating layer, the soft Zn single phase can be made to function as a buffer between the MgZn2 phase and the Zn-MgZn2-Al ternary eutectic phase, thereby improving corrosion resistance while also ensuring bendability.
[0043] Furthermore, from the perspective of plating adhesion, it was discovered that by forming a soft Zn single phase along the outer line of the MgZn2 phase, the Zn-MgZn2-Al ternary eutectic phase and the MgZn2 phase are connected by the Zn single phase, thereby improving plating adhesion.
[0044] At this time, the Zn single phase formed along the outer line of the MgZn2 phase in the coating layer can be confirmed through a photograph of the surface of the coated steel sheet taken using an FE-SEM.
[0045] For example, a photograph taken at a magnification of 1,500 times using an FE-SEM to observe the surface structure of the plated steel sheet obtained in Example 1 of the present invention is shown in Fig. 1. As shown in Fig. 1, it can be confirmed that a single Zn phase is formed along the outer line of the MgZn2 phase mainly composed of MgZn2.
[0046] In addition, whether or not the phase formed along the outer line of the MgZn2 phase corresponds to a Zn single phase can be determined by utilizing the cross-sectional photograph taken by the FE-SEM described above, and at the same time, whether or not it is a phase mainly composed of Zn with a Zn content of 85% or more by EDS (Energy Dispersive spectroscopy) criteria. In this specification, the Zn single phase formed along the outer line of the MgZn2 phase is defined to include both the first Zn single phase and the second Zn single phase described below.
[0047] Furthermore, although not particularly limited, according to one embodiment of the present invention, the average thickness of the Zn single phase formed along the outer line of the MgZn two phases can be selectively set to 2 to 7 μm.
[0048] If the average thickness of the Zn single phase formed along the outer line of the MgZn2 phase is less than 2 μm, the adhesion is weak due to the lack of the Zn single phase that can act as a buffer between the MgZn2 phase and the Zn-MgZn2-Al ternary eutectic phase, and problems may occur in bending workability and plating adhesion. On the other hand, if the average thickness of the Zn single phase formed along the outer line of the MgZn2 phase exceeds 7 μm, the Zn phase increases excessively and Mg is lacking, which may cause localized corrosion resistance problems. In order to further improve the above-mentioned effects, more preferably, the lower limit of the average thickness of the Zn single phase formed along the outer line of the MgZn2 phase may be 5.0 μm, or the upper limit of the average thickness of the Zn single phase formed along the outer line of the MgZn2 phase may be 6.9 μm.
[0049] At this time, the method for measuring the average thickness of the Zn single phase formed along the outer line of the MgZn2 phase is not particularly limited, but the average thickness of the Zn single phase formed along the outer line of the MgZn2 phase can be measured based on the length of the outer line of the MgZn2 phase, which is 5 μm or more, using surface photographs of the plating layer taken by FE-SEM and EDS.
[0050] Meanwhile, according to the present invention, two types of Zn single phases are formed along the outer line of the MgZn2 phase. First, a Zn single phase having a Mg solid solution rate of less than 4 wt% (hereinafter referred to as the "first Zn single phase") is formed primarily adjacent to the outer line of the MgZn2 phase. Secondarily, a Zn single phase having a high Mg solid solution rate of 4 wt% or more (hereinafter referred to as the "second Zn single phase") is formed adjacent to the above-mentioned first Zn single phase. To confirm this, FIG. 2 shows a photograph taken at a magnification of 5,000 times of the surface of the plated steel sheet obtained from Example 3 of the present invention. The region corresponding to A in FIG. 2 corresponds to the above-mentioned first Zn single phase formed adjacent to the outer line of the MgZn2 phase, and the region corresponding to B in FIG. 2 corresponds to the second Zn single phase formed adjacent to the above-mentioned first Zn single phase.
[0051] Therefore, when measuring the average thickness of the Zn single phase formed along the outer line of the MgZn2 phase, the above-mentioned "average thickness of the Zn single phase" is defined as the average distance from the outer line of the MgZn2 phase to the Zn single phase in which the Mg solid solution rate is high, that is, 4 wt% or more (for example, the average distance from the outer line of the MgZn2 phase to the region including region "B" in Figure 2) based on the length of the outer line of the MgZn2 phase of 5 μm or more, using the photograph taken with the FE-SEM described above.
[0052] On the other hand, although not particularly limited, according to one embodiment of the present invention, the ratio of the length of the Zn single phase formed along the outer edge of the MgZn2 phase to the length of the outer edge of the MgZn2 phase can be selectively set to 30 to 98%.
[0053] If the ratio of the length of the Zn single phase formed along the outer line of the MgZn2 phase to the outer line of the MgZn2 phase is less than 30%, a problem may occur in that the bendability and adhesion are not uniform throughout the steel sheet.On the other hand, if the ratio of the length of the Zn single phase formed along the outer line of the MgZn2 phase to the outer line of the MgZn2 phase exceeds 98%, a problem may occur in that the corrosion diffusion in the Zn single phase proceeds rapidly first, resulting in insufficient corrosion resistance.
[0054] From the viewpoint of further improving the above-mentioned effect, more preferably, the lower limit of the ratio of the length of the Zn single phase formed along the outer line of the MgZn2 phase to the outer line of the MgZn2 phase can be set to 60%, or the upper limit of the ratio of the length of the Zn single phase formed along the outer line of the MgZn2 phase to the outer line of the MgZn2 phase can be set to 90%.
[0055] There is no particular limitation on the method for measuring the ratio of the length of the Zn single phase formed along the outer line of the MgZn2 phase to the outer line of the MgZn2 phase. However, as an example, it can be obtained by measuring the ratio of the length of the Zn single phase having a Zn content of 85 wt% or more to the outer line of the MgZn2 phase, based on the length of the outer line of the MgZn2 phase that is 5 μm or more, using a photograph of the surface of the plated steel sheet taken with an FE-SEM. In this case, as described above, the Zn single phase includes both the first Zn single phase and the second Zn single phase.
[0056] On the other hand, although not particularly limited, the present inventors conducted intensive research to further improve the property of improving the adhesion between the phases, and as a result, confirmed that there are two types of Zn single phases formed along the outer line of the MgZn2 phase: a Zn single phase (first Zn single phase) with a Mg solid solution rate of less than 4% and a Zn single phase (second Zn single phase) with a Mg solid solution rate of 4% or more. However, through repeated research, the present inventors found that, among the Zn single phases formed along the outer line of the MgZn2 phase, 1) the Zn single phase with a Mg solid solution rate of 4% or more contributes to improving the adhesion with the Zn-MgZn2-Al ternary eutectic phase, and 2) the Zn single phase with a Mg solid solution rate of less than 4% contributes to improving the adhesion with the MgZn2 phase.
[0057] Specifically, although not particularly limited, according to one embodiment of the present invention, the area ratio of the Zn single phase (or the first Zn single phase) having a Mg solid solution rate of less than 4 wt% can be selectively set to 10 to 90% with respect to the entire area of the Zn single phase formed along the outer line of the MgZn2 phase. If the ratio of the Zn single phase having a Mg solid solution rate of less than 4 wt% is less than 10%, the effect of improving the connectivity with MgZn2 may be slight. On the other hand, if the ratio of the Zn single phase having a Mg solid solution rate of less than 4 wt% exceeds 1%, a problem may occur in that the connectivity between the phases is locally non-uniform. In order to further improve the adhesion between the Zn single phase and the MgZn2 phase, more preferably, the lower limit of the ratio of the Zn single phase having a Mg solid solution rate of less than 4 wt% may be 12%, or the upper limit of the ratio of the Zn single phase having a Mg solid solution rate of less than 4 wt% may be 75%.
[0058] Although not particularly limited, according to one embodiment of the present invention, the area ratio of the Zn single phase (or the second Zn single phase) having a Mg solid solution rate of 4 wt% or more can be selectively set to 10 to 90% with respect to the entire area of the Zn single phase formed along the outer line of the MgZn2 phase. If the area ratio of the Zn single phase having a Mg solid solution rate of 4 wt% or more is less than 10%, the effect of improving the connectivity with the Zn-MgZn2-Al ternary eutectic phase may be slight. On the other hand, if the area ratio of the Zn single phase having a Mg solid solution rate of 4 wt% or more exceeds 90%, a problem of locally non-uniform connectivity between the phases may occur. In order to further improve the adhesion between the Zn single phase and the Zn-MgZn2-Al ternary eutectic phase, more preferably, the lower limit of the area ratio of the Zn single phase having a Mg solid solution rate of 4 wt% or more can be 25%, or the upper limit of the area ratio of the Zn single phase having a Mg solid solution rate of 4 wt% or more can be 88%.
[0059] Therefore, according to one embodiment of the present invention, the Zn single phase formed along the outer line of the MgZn2 phase may selectively include, in area %, a first Zn single phase having a Mg solid solution rate of less than 4 wt%: 10-90% and a second Zn single phase having a Mg solid solution rate of 4 wt% or more: 10-90%. The first Zn single phase may be adjacent to the outer line of the MgZn2 phase, or the second Zn single phase may be adjacent to the first Zn single phase. The above description is similarly applicable to the first Zn single phase and the second Zn single phase.
[0060] In this specification, the above-mentioned Zn single phase with a Mg solid solution rate of 4 wt% or more and the Zn single phase with a Mg solid solution rate of less than 4 wt% can be distinguished by measuring the Mg content by weight relative to the Zn single phase at each point measured using FE-SEM and EDS.
[0061] Meanwhile, the method of measuring the area ratio of the Zn single phase with a Mg solid solution rate of 4 wt% or more and the area ratio of the Zn single phase with a Mg solid solution rate of less than 4 wt% is not particularly limited. For example, the surface of the coating layer may be measured by measuring the area ratio of the Zn single phase with a Mg solid solution rate of less than 4 wt% by FE-SEM and EDS. 2 It can be measured by calculating the area percentage of each Zn single phase relative to the total phase of the plating layer, based on the surface of the plating layer described above.
[0062] However, in the present invention, the Zn single phase having a Mg solid solution rate of 4 wt % or more may exist in a single connected form, or may exist in an island form separated from each other.
[0063] Therefore, 10 μm 2 Based on the surface area of the above plating layer, 1) when all Zn single phases (corresponding to area B) with a Mg solid solution rate of 4 wt% or more are present in a single connected shape as shown in Figure 2, the internal area from the outer line of the MgZn2 phase to the Zn single phase with a Mg solid solution rate of 4 wt% or more is regarded as the "Zn single phase formed along the outer line of the MgZn2 phase," and the area proportion of each Zn single phase (first Zn single phase and second Zn single phase) is measured.
[0064] On the other hand, 2) as shown in FIG. 3, when the Zn single phase with a Mg solid solution rate of 4 wt% or more exists in the form of islands separated from each other, a line of the shortest distance is drawn between two adjacent islands as shown in the square part of FIG. 3. A photograph of the square part is shown in FIG. 4, which shows the shortest line drawn between the two islands. Next, a line connecting the shortest line between the outer line of the Zn single phase with a Mg solid solution rate of 4 wt% or more and the above-mentioned islands is drawn as shown in FIG. 3. After this, the internal region from the outer line of the MgZn2 phase to the above-mentioned connecting line is regarded as the "Zn single phase formed along the outer line of the MgZn2 phase", and the area ratio of each Zn single phase (the first Zn single phase and the second Zn single phase) is measured. At this time, when two or more lines of the shortest distance exist between the above-mentioned islands with the same length, the area ratio of each Zn single phase is measured by the above-mentioned method, using the shortest line closest to the outer line of the MgZn2 phase as a reference.
[0065] Next, a "method for producing a plated steel sheet" according to another aspect of the present invention will be described in detail. However, this does not necessarily mean that the plated steel sheet of the present invention must be produced by the following method.
[0066] According to an embodiment of the present invention, the method may further include a step of preparing a base steel sheet, and the type of the base steel sheet is not particularly limited. The base steel sheet may be, but is not limited to, an Fe-based base steel sheet used as a base steel sheet for a typical hot-dip galvanized steel sheet, i.e., a hot-rolled steel sheet or a cold-rolled steel sheet. The base steel sheet may be, but is not limited to, a carbon steel, an extra-low carbon steel, or a high manganese steel used as a material for construction, home appliances, or automobiles. In this case, the above description may be similarly applied to the base steel sheet.
[0067] Next, the above-prepared base steel sheet is subjected to a plating bath temperature (T B ) for T B +10℃~T B The steel sheet is immersed in a plating bath containing, by weight, 4.0-7.0% Mg, 11.0-19.5% Al, the balance being Zn and other unavoidable impurities, so as to satisfy the drawing temperature of +50°C, and then hot-dip galvanizing is performed.
[0068] In this case, the reasons for adding the components in the coating bath and the reasons for limiting the contents thereof can be similarly applied to the explanation for the components of the coating layer described above, except for the small amount of Fe content that can flow in from the base steel sheet.
[0069] Meanwhile, in order to prepare the coating bath having the above composition, a composite ingot containing the desired Zn, Al, and Mg or a Zn-Mg or Zn-Al ingot containing individual components can be used. In order to replenish the coating bath consumed in hot dip coating, the ingot is further melted and supplied. In this case, a method of directly immersing the ingot in the coating bath and melting it can be selected, or a method of melting the ingot in a separate port and then replenishing the molten metal to the coating bath can be selected.
[0070] In addition, during the above hot dip galvanizing, the drawing temperature of the base steel sheet is the plating bath temperature (T B ) for T B +10℃~T B +50°C. At this time, although there is no particular limitation, the plating bath temperature (T B ) can be maintained in the range of 440 to 500° C. By setting the drawing temperature into the coating bath as described above, it is possible to improve the interfacial adhesion between the base steel sheet and the coating layer.
[0071] On the other hand, the drawing temperature of the above-mentioned base steel sheet is T B If the temperature is less than +10°C, the improvement in the interface adhesion is slight, and the problem of dross adhesion may occur. B If the temperature exceeds +50°C, the generation of zinc fumes will increase and they will be adsorbed onto the steel sheet, which may cause problems with the plating surface quality.
[0072] In this case, in order to further improve the above-mentioned effects, it is more preferable that the lower limit of the drawing temperature of the base steel sheet is T B +20℃, and the upper limit of the drawing temperature of the above-mentioned base steel sheet is T B It can be in the range of +45°C.
[0073] Next, the hot-dip galvanized steel sheet is air-wiped using an inert gas so as to satisfy the following relational expression 1. By controlling the air-wiping conditions so as to satisfy the following relational expression 1, the Zn single-phase structure formed along the outer line of the MgZn2 phase as specified in the present invention is ensured, and at the same time, smooth and uniform surface characteristics are ensured, thereby improving bendability. At this time, since the following relational expression 1 is an empirically obtained value, no particular unit can be specified, and the following defined W air The unit of is mm and P air It is sufficient to satisfy the units of kPa for pressure and the units of T for temperature. [Equation 1] 0.005≦P air / (Wair ×T) (In the above Relational Formula 1, the above W air represents the distance between the air knives, in mm. air represents the pressure of the air knife in kPa. T represents the temperature of the supplied inert gas in °C.
[0074] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the inert gas may be argon (Ar) gas, nitrogen (N2) gas, or a mixture of argon and nitrogen gas, and it is more preferable to use nitrogen gas.
[0075] Furthermore, according to one embodiment of the present invention, in the air wiping step, the air knife spacing may be in the range of 20 to 45 mm (more preferably, 30 to 40 mm). Alternatively, the air knife pressure may be in the range of 8 to 20 kPa (more preferably, 10 to 18 kPa). Alternatively, the temperature of the supplied gas may be in the range of 30 to 100°C (more preferably, 65 to 85°C). By adjusting the air wiping conditions so as to satisfy the above-mentioned ranges, a plated steel sheet having excellent corrosion resistance, bendability and plating adhesion can be produced.
[0076] Thereafter, the air-wiped steel sheet is cooled to the solidification end temperature at an average cooling rate of 2 to 5°C / s based on the surface temperature. If the average cooling rate in the cooling stage after the air wiping is less than 2°C / s, problems may occur in the productivity of the plated steel sheet, and if it exceeds 5°C / s, the Zn single-phase structure formed along the outer line of the MgZn two-phase defined in the present invention may not be formed.
[0077] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the cooling may be selectively performed in three stages, including a first cooling in which the air-wiped steel sheet is cooled in a temperature range of 420°C or more to 450°C or less at an average cooling rate of 1.0 to 2.0°C / s, a second cooling in which the primarily cooled steel sheet is cooled in a temperature range of 340°C or more to less than 420°C at an average cooling rate of 2.1 to 4.0°C / s, and a third cooling in which the secondarily cooled steel sheet is cooled in a temperature range of 150°C or more to less than 340°C at an average cooling rate of 5.0 to 7.0°C / s.
[0078] As a result of intensive research, the present inventors have found that slow cooling is performed, but by dividing the cooling rate into primary, secondary, and tertiary cooling sections and gradually increasing the cooling rate in each section, the bendability can be improved. Specifically, if the average cooling rate during the primary cooling is less than 1.0°C / s, problems with the productivity of the steel sheet may occur. On the other hand, if the average cooling rate during the primary cooling exceeds 2.0°C / s, problems with ensuring uniform interfacial adhesion between the base steel sheet and the coating layer may occur. Also, if the average cooling rate during the secondary cooling is less than 2.1°C / s, problems with the productivity of the steel sheet may occur. On the other hand, if the average cooling rate during the secondary cooling exceeds 4.0°C / s, problems with ensuring adhesion between the MgZn2 and Zn single phase in the coating layer may occur. Also, if the average cooling rate during the tertiary cooling is less than 5.0°C / s, a problem of the coating layer adhering to the top roll of the cooling tower may occur due to a delay in the completion of solidification of the steel sheet. On the other hand, if the average cooling rate during the tertiary cooling exceeds 7.0°C / s, problems may occur in the adhesion between the Zn single phase and the Zn-MgZn2-Al ternary eutectic phase in the coating layer.
[0079] Meanwhile, although not particularly limited, according to one embodiment of the present invention, the cooling can selectively further satisfy the following Relational Expression 2. By controlling the relationship between the average cooling rate during the tertiary cooling and the average cooling rates during the primary and secondary cooling as in the following Relational Expression 2, it is possible to promote improvement in adhesion between the MgZn2 phase and the Zn single phase and between the Zn-MgZn2-Al ternary eutectic phase and the Zn single phase, thereby further improving the bendability of the coating layer. [Equation 2] C1+C2≦C3≦1.5×(C1+C2) (In the above Relational Formula 2, C1 represents the average cooling rate [°C / s] during the first cooling, C2 represents the average cooling rate [°C / s] during the second cooling, and C3 represents the average cooling rate [°C / s] during the third cooling.)
[0080] As described above, by precisely controlling the coating composition and manufacturing conditions, it is possible to effectively provide a plated steel sheet that is excellent not only in corrosion resistance but also in one or more of the properties of bendability and coating adhesion. EXAMPLES
[0081] (Example) The present invention will be described in more detail with reference to the following examples. However, it should be noted that the following examples are for illustrative purposes only and are not intended to limit the scope of the present invention. The scope of the present invention is determined by the matters described in the claims and matters reasonably inferred therefrom.
[0082] (Experimental Example 1) A base steel plate having a thickness of 2 mm and a width of 1300 mm and having a composition of C: 0.018%, Si: 0.01%, Mn: 0.2%, P: 0.009%, S: 0.005%, Al: 0.1%, Nb: 0.02%, Cr: 0.2%, Ti: 0.02%, B: 0.015%, the balance being Fe and impurities, is prepared.
[0083] The prepared base steel sheet was immersed in a coating bath under the conditions shown in Table 1 below to perform hot-dip galvanization. The hot-dip galvanized steel sheet was then subjected to air wiping treatment using nitrogen (N2) gas under the conditions shown in Table 1 below, and then cooled under the conditions shown in Table 2 below.
[0084] [Table 1]
[0085] [Table 2] C*: Average cooling rate to the end of solidification temperature [℃ / s]
[0086] Test pieces of the plated steel sheets obtained by the methods in Tables 1 and 2 above were prepared, and the plated layers were dissolved in a hydrochloric acid solution. The dissolved liquid was then analyzed by a wet analysis (ICP) method to determine the compositions of the plated layers, which are shown in Table 3 below (the remainder corresponds to Zn and impurities).
[0087] In addition, cross-sectional test pieces were prepared by cutting the steel sheet in the thickness direction (i.e., the direction perpendicular to the rolling direction) so that the interface between the coating layer and the base steel sheet could be observed, and the cross sections were photographed using an SEM. It was confirmed that an Fe-Al-based inhibitory layer having a thickness of 0.1 to 1 μm was formed between the base steel sheet and the Zn-Mg-Al-based coating layer.
[0088] In addition, the surface of the steel sheet was photographed at a magnification of 1,500 times using FE-SEM and EDS, and the presence or absence of a Zn single phase formed along the outer line of the MgZn two phases was indicated by presence or absence [○ / ×] in Table 3 below.
[0089] In this case, the Zn single phase was determined based on whether the Zn content (wt%) was 85% or more, using surface photographs taken with FE-SEM and EDS.
[0090] In addition, the average thickness of the Zn single phase formed along the outer line of the MgZn2 phase was measured using a FE-SEM based on the outer line length of 5 μm of the MgZn2 phase, and is shown in Table 3 below.
[0091] [Table 3] ○: Zn single phase formed along the outer line of MgZn2 phase ×: No Zn single phase formed along the outer line of the MgZn2 phase
[0092] The characteristics of each of the examples and comparative examples were evaluated according to the following criteria, and the evaluation results of each characteristic are shown in Table 4 below.
[0093] <Corrosion resistance> In order to evaluate the corrosion resistance, a salt spray tester (SST) was used in accordance with the test method of ISO14993, and the evaluation was performed according to the following criteria. ○: The time it takes for red rust to appear is 30 to 40 times longer than that of Zn plating of the same thickness. △: The time it takes for red rust to appear is 20 to 30 times longer than that of Zn plating of the same thickness. ×: The time it takes for red rust to appear is less than 20 times longer than that for Zn plating of the same thickness.
[0094] <Bending property> To evaluate cracks at the bent portion, the material was cut into a piece of 30 mm x 100 mm, and the number of cracks that occurred within a length of 10 mm after 3t bending was observed using FE-SEM. The bendability was evaluated according to the following criteria. ◎: Less than 5 ○: 5 or more but less than 10 △: 10 or more but less than 20 ×: 20 or more
[0095] <Plating adhesion> To evaluate the plating adhesion, the material was cut to 30 mm x 100 mm, and each plated steel material was bent 180° (OT bending). Each bent test piece was taped, and the peeled area of the test piece was measured and the plating adhesion was evaluated according to the following criteria. The evaluation criteria for plating adhesion are as follows: ◎: No peeling area ○: Peeling area over 0% and less than 3% △: Peeling area 3-10% ×: Peeling area 10% or more
[0096] [Table 4]
[0097] As can be seen from the experimental results in Table 4 above, it was confirmed that in Examples 1 to 5, which satisfy the plating composition and manufacturing conditions specified in the present invention, the corrosion resistance, bendability, and plating adhesion are excellent.
[0098] On the other hand, in the case of Comparative Examples 1 to 14, which do not satisfy one or more of the plating composition and manufacturing conditions specified in the present invention, it was confirmed that one or more of the properties of corrosion resistance, bendability, and plating adhesion were inferior to those of Examples 1 to 5.
[0099] (Experimental Example 2) A plated steel sheet was produced in the same manner as in Experimental Example 1 described above, except that hot-dip galvanizing and air wiping treatment were performed under the conditions in Table 5 below, and then three-stage cooling was performed by controlling the average cooling rate in the first, second and third stages under the conditions in Table 6 below.
[0100] At this time, analysis was carried out in the same manner as in Experimental Example 1, and it was confirmed that an Fe-Al-based inhibiting layer having a thickness of 0.3 µm was formed between the base steel sheet and the Zn-Mg-Al-based coating layer.
[0101] Meanwhile, the coating layer composition, the presence or absence of the Zn single phase formed along the outer line of the MgZn two phase, and the average thickness were measured in the same manner as described above in Experimental Example 1, and are shown in Table 7 below.
[0102] Additionally, the proportion of the Zn single phase formed along the outer line of the MgZn2 phase within a 10 μm outer line length of the MgZn2 phase was measured using FE-SEM and EDS in the same manner as described above in the specification, and the results are shown in Table 7 below.
[0103] In addition, the area of 25 μm was photographed using FE-SEM and EDS. 2 Using the surface of the plating layer as a reference, the area percentage of the Zn single phase with a Mg solid solution rate of 4 wt% or more and the area percentage of the Zn single phase with a Mg solid solution rate of less than 4 wt% were measured in the same manner as described above in this specification, and these values are shown in Table 7 below.
[0104] In addition, for the plated steel sheets obtained in each of the Examples and Comparative Examples, the corrosion resistance, bendability and plating adhesion were evaluated in the same manner as in Experimental Example 1, and the results are shown in Table 8 below.
[0105] [Table 5]
[0106] [Table 6] Primary cooling*: Cooling in the temperature range below 450℃ and above 420℃ Secondary cooling*: Cooling in the temperature range of 340℃ or more and less than 420℃ Tertiary cooling*: Cooling in the temperature range of 150℃ or more but less than 340℃
[0107] [Table 7]
[0108] [Table 8]
[0109] As can be seen from the experimental results in Table 8 above, it was confirmed that in the cases of Examples 6 to 10, which satisfy the plating composition and manufacturing conditions specified in the present invention, the corrosion resistance, bendability, and plating adhesion are excellent.
[0110] In particular, it was confirmed that, among the above examples, in the case of Examples 8 to 10 in which the three-stage cooling defined in the present invention was performed, the bendability was further improved compared to Examples 6 and 7. This is presumed to be because the occupancy rate and average thickness of the MgZn2 phase relative to the Zn single phase formed along the outer line is large in the above Examples 8 to 10, and a large amount of soft Zn single phase is formed around the hard MgZn2 phase, resulting in further excellent bendability. It is also presumed that the Zn single phase with a Mg solid solution rate of 4% or more contributes to improving interphase adhesion with the Zn-MgZn2-Al ternary eutectic phase, and the Zn single phase with a Mg solid solution rate of less than 4% contributes to improving interphase adhesion with the MgZn2 phase, ultimately contributing to improving plating adhesion.
[0111] On the other hand, in the case of Comparative Examples 15 and 16, which do not satisfy all of the plating composition and manufacturing conditions specified in the present invention, it was confirmed that one or more of the properties of corrosion resistance, bendability, and plating adhesion were inferior to those of Examples 6 to 10.
Claims
1. Base steel sheet, and A Zn-Mg-Al-based plating layer is provided on at least one surface of the base steel sheet, The plating layer is MgZn 2 phase, and the MgZn 2 and a Zn single phase formed along an outer line of the phase.
2. The plated steel sheet according to claim 1, wherein the plating layer contains, by weight percent, 4.0 to 7.0% Mg, 11.0 to 19.5% Al, and the balance being Zn and other inevitable impurities.
3. The plated steel sheet according to claim 1, further comprising an Fe-Al-based inhibiting layer provided between the base steel sheet and the Zn-Mg-Al-based plating layer.
4. The MgZn 2 The Zn single phase formed along the outer line of the phase is the MgZn 2 The plated steel sheet according to claim 1, wherein the proportion of the length of the phase occupying the outer line is 30 to 98%.
5. The MgZn 2 The plated steel sheet according to claim 1, wherein the average thickness of the Zn single phase formed along the outer line of the phase is 2 to 7 μm.
6. The MgZn 2 6. The plated steel sheet according to claim 5, wherein the Zn single phase formed along an outer line of the phase includes, in area %, a first Zn single phase having a Mg solid solution rate of less than 4 wt %: 10 to 90% and a second Zn single phase having a Mg solid solution rate of 4 wt % or more: 10 to 90%.
7. The first Zn single phase is the MgZn 2 The plated steel sheet of claim 6 adjacent an outer line of the phase.
8. Plating bath temperature (T B ) for T B +10℃~T B A step of immersing the base steel sheet in a coating bath containing, by weight%, 4.0 to 7.0% Mg, 11.0 to 19.5% Al, the balance Zn and other inevitable impurities, so as to satisfy a drawing temperature of +50°C, to perform hot-dip galvanizing; performing air wiping on the hot-dip galvanized steel sheet using an inert gas so as to satisfy the following Relational Formula 1; and cooling the air-wiped steel sheet to a solidification end temperature at an average cooling rate of 2 to 5° C. / s. A method for producing a plated steel sheet, comprising: [Relationship 1] 0.005≦P air / (W air ×T) (In the above-mentioned relational expression 1, the W air represents the distance between the air knives, and is expressed in mm. air represents the pressure of the air knife, in kPa. T represents the temperature of the supplied inert gas, in °C.
9. The cooling step includes: a primary cooling step of cooling the air-wiped steel sheet to a temperature range of 450°C to 420°C at an average cooling rate of 1.0 to 2.0°C / s; Secondary cooling of the primarily cooled steel sheet in a temperature range of 340°C or more but less than 420°C at an average cooling rate of 2.1 to 4.0°C / s; and The secondarily cooled steel sheet is then subjected to a third cooling step of cooling the steel sheet to a temperature range of 150°C or more but less than 340°C at an average cooling rate of 5.0 to 7.0°C / s. The method for producing a plated steel sheet according to claim 8, comprising:
10. The method for producing a plated steel sheet according to claim 9 , wherein the cooling step satisfies the following Relational Expression 2: [Relationship 2] C 1 +C 2 ≦C 3 ≦1.5×(C 1 +C 2 ) (In the above-mentioned relational formula 2, C 1 represents the average cooling rate during the first cooling [°C / s], and C 2 represents the average cooling rate during secondary cooling [°C / s], C 3 indicates the average cooling rate during the tertiary cooling [℃ / s].)
Citation Information
Patent Citations
Hot dip zn-al-mg coated steel sheet excellent in corrosion resistance and external surface appearance, and its production
JP1998306357A
Hot dip high al-containing zn-al-mg base metal coated steel sheet
JP2001295015A
Plated steel, and method for producing plated steel
JP2021004403A
Hot-dip zinc plating bath providing excellent corrosion resistance, high formability and appearance, and steel plate plated with the same
KR1020120076111A
Plated steel
WO2018139619A1