Insulating layer composition for lithium secondary battery and lithium secondary battery including same
The insulating layer composition for lithium secondary batteries, utilizing a conjugated diene copolymer and non-aqueous solvent, addresses heat resistance and processability issues, enhancing insulation and stability, thereby improving battery safety and manufacturing efficiency.
Patent Information
- Application Number
- JP2024523238
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-04
- Filing Date
- 2023-04-04
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-04
AI Technical Summary
Conventional separators in lithium secondary batteries face limitations in heat resistance and processability, leading to thermal runaway and decreased stability due to issues with binder adhesion, phase separation, and brittleness, which can cause short circuits and degrade battery performance.
An insulating layer composition for lithium secondary batteries using a conjugated diene copolymer, non-aqueous organic solvent, and emulsifier, with a high gel content and controlled particle size, to enhance insulation, processability, and storage stability, allowing simultaneous coating with the positive electrode mixture layer.
The composition provides excellent insulation, improved process efficiency, and enhanced storage stability by preventing short circuits and maintaining electrode integrity, thus improving battery safety and manufacturing efficiency.
Smart Images

Figure 2024539673000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an insulating layer composition for a lithium secondary battery and a lithium secondary battery including the same. [Background technology]
[0002] As technological development and demand for mobile devices increases, the demand for secondary batteries as an energy source is growing rapidly, and accordingly, much research is being conducted on batteries that can meet various needs.
[0003] One of the main research topics for such secondary batteries is to improve their safety. The main cause of safety-related accidents in batteries is the reaching of abnormally high temperatures due to short circuits between the positive and negative electrodes. In other words, under normal circumstances, a separator is located between the positive and negative electrodes to maintain electrical insulation, but in abnormal abuse situations such as when the battery is overcharged or overdischarged, internally short-circuited by dendritic growth of the electrode material or foreign matter, pierced by sharp objects such as nails or screws, or subjected to excessive deformation due to external forces, the conventional separator alone shows its limitations.
[0004] Generally, microporous membranes made of polyolefin resin are mainly used as separators, but their heat resistance is insufficient, with a temperature limit of about 120 to 160°C. Therefore, when an internal short circuit occurs, the separator shrinks due to the short circuit reaction heat, expanding the short circuit area, leading to a thermal runaway state in which a larger amount of reaction heat is generated. Therefore, various methods have been studied to reduce the possibility of cell deformation, external impact, or physical short circuit between the positive and negative electrodes.
[0005] For example, in order to prevent a short circuit caused by the electrode tab coming into contact with the upper end of the electrode assembly due to the movement of the electrode assembly in a completed battery, a method is used in which an insulating tape of a predetermined size is attached to the electrode tab adjacent to the upper end of the current collector. However, the winding of the insulating tape is very cumbersome, and when the insulating tape is wound to a length that extends slightly downward from the upper end of the current collector, such a portion may cause an increase in the thickness of the electrode assembly. Furthermore, there is a problem that the electrode tab is easily loosened when it is bent.
[0006] In addition, there is a method of forming an insulating layer on the tab portion of the positive electrode using a non-aqueous binder (such as PVDF) or an aqueous styrene butadiene copolymer (SBL). However, when a non-aqueous binder (such as PVDF) is used, there is a problem that the wet adhesion is reduced and the migration of lithium ions cannot be prevented in the overlay region of the electrode, resulting in the development of capacity. In particular, when the capacity is developed in the overlay region of the electrode, lithium ions may be precipitated, which may result in a decrease in the stability of the battery cell. In addition, when an aqueous styrene butadiene copolymer (SBL) binder is used, there is a process problem that the battery performance is decreased due to gelation of PVDF, which is an organic binder used as a positive electrode binder when simultaneously coated with a slurry for the positive electrode mixture layer, the boundary penetration of the positive electrode slurry into the insulating liquid, and side reactions due to moisture, and simultaneous coating of the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer is impossible. In addition, the non-aqueous binder (such as PVDF) or the aqueous styrene butadiene copolymer (SBL) insulating layer has a problem that phase separation occurs during storage, resulting in a decrease in storage stability.
[0007] Furthermore, carboxymethyl cellulose is often used as a thickener in insulating layer compositions for lithium secondary batteries, but such carboxymethyl cellulose has a problem of reducing processability during winding and cutting processes due to its brittleness.
[0008] Therefore, there is a high demand for the development of an insulating liquid that not only has excellent insulating properties, but also allows simultaneous coating of a slurry for a positive electrode mixture layer and a slurry for an insulating coating layer, is not brittle, has excellent processability, and has excellent storage stability. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Korean Patent No. 10-1586530 Summary of the Invention [Problem to be solved by the invention]
[0010] The present invention has been made in consideration of the above-mentioned problems, and an object of the present invention is to provide an insulating layer composition for a lithium secondary battery that not only has excellent insulating properties and processability, but also has excellent storage stability.
[0011] Another object of the present invention is to provide a method for manufacturing a positive electrode for a lithium secondary battery using the insulating layer composition for a lithium secondary battery.
[0012] Another object of the present invention is to provide a positive electrode for a lithium secondary battery comprising the insulating layer composition for a lithium secondary battery.
[0013] Another object of the present invention is to provide a lithium secondary battery including the positive electrode for lithium secondary batteries.
[0014] However, the objects of the present invention are not limited to those mentioned above, and other objects not mentioned will be clearly understood by a person having ordinary knowledge in the technical field to which this disclosure pertains (referred to as an "ordinary engineer" or "person skilled in the art") from the description in the claims. [Means for solving the problem]
[0015] In order to achieve the above object, according to one embodiment of the present invention, there is provided an insulating layer composition for a lithium secondary battery, comprising a conjugated diene copolymer as a binder polymer, a non-aqueous organic solvent, and an emulsifier, the gel content being 70 wt% or more based on the total weight of the conjugated diene copolymer, and the emulsifier content being 0.3 wt% or more based on the total weight of the conjugated diene copolymer.
[0016] The insulating layer composition for a lithium secondary battery may not contain carboxymethyl cellulose.
[0017] The conjugate diene copolymer may include a polymer of (a) a conjugate diene monomer or a conjugate diene polymer, (b) at least one monomer selected from the group consisting of acrylate monomers, vinyl monomers, and nitrile monomers, and (c) one or more monomers selected from the group consisting of unsaturated carboxylic acid monomers and hydroxyl group-containing monomers.
[0018] The conjugate diene monomer may be one monomer selected from the group consisting of 1,3-butadiene, isoprene, chloroprene, and piperylene, and the conjugate diene polymer may be a polymer of two or more monomers selected from the group consisting of 1,3-butadiene, isoprene, chloroprene, and piperylene, a styrene-butadiene copolymer, an acrylonitrile-butadiene copolymer, a styrene-isoprene copolymer, an acrylate-butadiene rubber, an acrylonitrile-butadiene-styrene rubber, an ethylene-propylene-diene polymer, or a polymer in which these polymers are partially epoxidized or brominated (Br), or a mixture thereof.
[0019] The acrylate monomer may be one or more monomers selected from the group consisting of methyl ethacrylate, methacryloxyethyl ethylene urea, β-carboxyethyl acrylate, aliphatic monoacrylate, dipropylene diacrylate, ditrimethylolpropane tetraacrylate, dipentaerythriol hexaacrylate, pentaerythriol triacrylate, pentaerythriol tetraacrylate, and glycidyl methacrylate.
[0020] The vinyl monomer may be one or more monomers selected from the group consisting of styrene, α-methylstyrene, β-methylstyrene, pt-butylstyrene, and divinylbenzene.
[0021] The nitrile monomer may be one or more monomers selected from the group consisting of acrylonitrile, methacrylonitrile, and allyl cyanide.
[0022] The unsaturated monocarboxylic acid monomer may be one or more monomers selected from the group consisting of maleic acid, fumaric acid, methacrylic acid, acrylic acid, glutaric acid, itaconic acid, tetrahydrophthalic acid, crotonic acid, isocrotonic acid, and nadic acid.
[0023] The hydroxy group-containing monomer may be one or more monomers selected from the group consisting of hydroxyacrylate, hydroxyethyl acrylate, hydroxybutyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate.
[0024] The conjugate diene copolymer may contain, based on the total weight, a polymer of 25 to 45% by weight of the (a) conjugate diene monomer or conjugate diene polymer, 50 to 70% by weight of the (b) one or more monomers selected from the group consisting of acrylate monomers, vinyl monomers, and nitrile monomers, and 1 to 20% by weight of the (c) one or more monomers selected from the group consisting of unsaturated carboxylic acid monomers and hydroxyl group-containing monomers.
[0025] The non-aqueous organic solvent may be at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol.
[0026] The conjugate diene copolymer can be a styrene-butadiene copolymer and the non-aqueous organic solvent can be N-methyl-pyrrolidone (NMP).
[0027] The insulating layer composition for a lithium secondary battery may have a moisture content of 10,000 ppm or less.
[0028] According to another embodiment of the present invention, there is provided a method for manufacturing a positive electrode for a lithium secondary battery, the method comprising: preparing a water-dispersible conjugated diene copolymer; adding a non-aqueous organic solvent to the water-dispersible conjugated diene copolymer and heating and reducing pressure to prepare a slurry for an insulating coating layer; coating a slurry for a positive electrode mixture layer, the slurry including a positive electrode active material, a non-aqueous binder, a conductive material, and a non-aqueous organic solvent, on one or both sides of a positive electrode current collector; coating the slurry for the insulating coating layer from a portion of an uncoated portion of the positive electrode current collector to cover a portion of the slurry for the positive electrode mixture layer coated on the current collector; and drying the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer coated on the positive electrode current collector.
[0029] The conjugated diene copolymer may be a conjugated diene latex.
[0030] The conjugate diene latex can be a styrene-butadiene latex and the non-aqueous organic solvent can be N-methyl-pyrrolidone (NMP).
[0031] According to another embodiment of the present invention, there is provided a positive electrode for a lithium secondary battery, comprising: a positive electrode current collector; a positive electrode tab protruding from the positive electrode current collector; and an insulating layer coated with an insulating material on the positive electrode tab, wherein the insulating material includes the insulating layer composition for a lithium secondary battery.
[0032] According to another embodiment of the present invention, there is provided a lithium secondary battery including the positive electrode for lithium secondary batteries. Effect of the Invention
[0033] The insulating layer composition for a lithium secondary battery according to an embodiment of the present invention does not contain carboxymethyl cellulose, and therefore is not brittle, and has excellent processability during winding and cutting processes.
[0034] In addition, the insulating layer composition for a lithium secondary battery according to one embodiment of the present invention replaces water, which is a dispersion solvent for the aqueous conjugate diene copolymer, with a non-aqueous organic solvent (e.g., N-methyl-pyrrolidone), so that the insulating liquid can be coated simultaneously with the positive electrode coating, and thus the processability in manufacturing the positive electrode for a lithium secondary battery is excellent.
[0035] In addition, the insulating layer composition for a lithium secondary battery according to an embodiment of the present invention has a high gel content and contains an emulsifier, and thus has excellent storage stability.
[0036] However, the effects of the present invention are not limited to those mentioned above, and other effects not mentioned will be clearly understood by a person having ordinary skill in the art in the technical field to which this disclosure pertains from the description in the claims. [Brief description of the drawings]
[0037] BRIEF DESCRIPTION OF THE DRAWINGS Non-limiting embodiments of the present invention will now be described with reference to the accompanying drawings, in which like reference numerals indicate like elements and in which: FIG.
[0038] [Figure 1] 13 is a diagram showing the state according to the moisture influence evaluation experiment of Experimental Example 3. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0039] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings, so that those skilled in the art can easily carry out the present invention. However, the present invention is provided by way of example only, and is not limited thereto, and the present invention is defined only by the scope of the claims that follow.
[0040] The terms or words used in this specification and the claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as having meanings or concepts that are consistent with the technical idea of the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to best describe his or her invention.
[0041] In this specification, terms such as "comprises" should be understood as open-ended terms that encompass the possibility of including other embodiments.
[0042] As used herein, "preferred" and "preferably" refer to embodiments of the invention that may provide certain advantages, under certain circumstances. However, other embodiments may also be preferred, under the same or different circumstances. Furthermore, reference to one or more preferred embodiments does not imply that other embodiments are not useful, and is not intended to exclude other embodiments from the scope of the invention.
[0043] In the present invention, the term "insulating coating layer" refers to an insulating member formed by coating and drying from at least a portion of the uncoated portion of the electrode current collector to at least a portion of the electrode mixture layer.
[0044] In the present invention, the term "metal test piece" refers to a space in which an insulating coating layer is formed, and may refer to a metal current collector used in manufacturing an electrode, and may be a metal current collector punched to have a predetermined width and length. For example, the metal test piece may be aluminum, copper, or an aluminum alloy.
[0045] 1. Insulating layer composition for lithium secondary batteries
[0046] According to one embodiment of the present invention, there is provided an insulating layer composition for a lithium secondary battery, comprising a conjugate diene copolymer as a binder polymer, a non-aqueous organic solvent, and an emulsifier, the gel content being 70 wt % or more based on the total weight of the conjugate diene copolymer, and the emulsifier content being 0.3 wt % or more based on the total weight of the conjugate diene copolymer.
[0047] Hereinafter, each component of the insulating layer composition for a lithium secondary battery will be described in detail.
[0048] An insulating layer composition for a lithium secondary battery according to an embodiment of the present invention includes a conjugated diene copolymer as a binder polymer.
[0049] The conjugated diene copolymer may comprise (a) a conjugated diene monomer or a conjugated diene polymer, (b) one or more monomers selected from the group consisting of acrylate monomers, vinyl monomers, and nitrile monomers, and (c) a polymer of one or more monomers selected from the group consisting of unsaturated carboxylic acid monomers and hydroxyl group-containing monomers.
[0050] The conjugated diene monomer may be one monomer selected from the group consisting of 1,3-butadiene, isoprene, chloroprene and piperylene.
[0051] The conjugated diene polymer may be, for example, a polymer of two or more monomers selected from the group consisting of 1,3-butadiene, isoprene, chloroprene, and piperylene, a styrene-butadiene copolymer, an acrylonitrile-butadiene copolymer, a styrene-isoprene copolymer, an acrylate-butadiene rubber, an acrylonitrile-butadiene-styrene rubber, an ethylene-propylene-diene polymer, a partially epoxidized or brominated polymer of these polymers, or a mixture thereof.
[0052] The acrylate monomer may be one or more monomers selected from the group consisting of methyl ethacrylate, methacryloxyethyl ethylene urea, β-carboxyethyl acrylate, aliphatic monoacrylate, dipropylene diacrylate, ditrimethylolpropane tetraacrylate, dipentaerythriol hexaacrylate, pentaerythriol triacrylate, pentaerythriol tetraacrylate, and glycidyl methacrylate.
[0053] The vinyl monomer may be at least one monomer selected from the group consisting of styrene, α-methylstyrene, β-methylstyrene, pt-butylstyrene, and divinylbenzene.
[0054] The nitrile monomer may be at least one monomer selected from the group consisting of acrylonitrile, methacrylonitrile, and allyl cyanide.
[0055] The unsaturated carboxylic acid monomer may be at least one monomer selected from the group consisting of maleic acid, fumaric acid, methacrylic acid, acrylic acid, glutaric acid, itaconic acid, tetrahydrophthalic acid, crotonic acid, isocrotonic acid, and nadic acid.
[0056] The hydroxy group-containing monomer may be one or more monomers selected from the group consisting of hydroxyacrylate, hydroxyethyl acrylate, hydroxybutyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate.
[0057] In the insulating layer composition for a lithium secondary battery according to the present invention, conjugated dienes copolymer particles having an average particle size of 50 nm to 500 nm exist as an independent phase.
[0058] Preferably, the conjugate diene copolymer may be a styrene-butadiene copolymer, more preferably, a styrene-butadiene latex, but is not limited thereto.
[0059] The method for producing the conjugate diene copolymer particles is not particularly limited, and may be a known method such as suspension polymerization, emulsion polymerization, or seed polymerization.
[0060] The mixture of monomers for producing the copolymer particles may contain one or more other components, such as polymerization initiators, crosslinking agents, coupling agents, buffer solutions, molecular weight regulators, emulsifiers, and the like.
[0061] Specifically, the copolymer particles may be produced by emulsion polymerization, and in this case, the average particle size of the copolymer particles may be adjusted by the amount of emulsifier, and generally, the particle size tends to become smaller as the amount of emulsifier increases, and the particle size tends to become larger as the amount of emulsifier decreases. The desired average particle size can be achieved by adjusting the amount of emulsifier used in consideration of the desired particle size, reaction time, reaction stability, etc. The polymerization temperature and polymerization time may be appropriately determined depending on the polymerization method, the type of polymerization initiator, etc., and for example, the polymerization temperature may be 10°C to 150°C, and the polymerization time may be 1 to 20 hours.
[0062] The polymerization initiator may be an inorganic or organic peroxide, for example, a water-soluble initiator including potassium persulfate, sodium persulfate, ammonium persulfate, etc., or an oil-soluble initiator including cumene hydroperoxide, benzoyl peroxide, etc. In addition, an activator may be further included to promote the initiation reaction of the peroxide together with the polymerization initiator, and the activator may be at least one selected from the group consisting of sodium formaldehyde sulfoxylate, sodium ethylenediaminetetraacetate, ferrous sulfate, and dextrose.
[0063] The crosslinking agent is a substance that promotes crosslinking of the binder, and examples of the crosslinking agent include amines such as diethylene triamine, triethylene tetramine, diethylamino propylamine, xylene diamine, and isophorone diamine, dodecyl succinic anhydride, and phthalic anhydride. Examples of suitable grafting agents include acid anhydrides such as aryl methacrylate, polyamide resins, polysulfide resins, phenolic resins, ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, 1,3-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, neopentyl glycol dimethacrylate, trimethylolpropane trimethacrylate, trimethylolmethane triacrylate, and glycidyl methacrylate. Examples of suitable grafting agents include aryl methacrylate (AMA), triaryl isocyanurate (TAIC), triarylamine (TAA), and diarylamine (DAA).
[0064] The coupling agent is a material for increasing the adhesive strength between the active material and the binder, and is characterized by having two or more functional groups, one of which reacts with a hydroxyl group or a carboxyl group on the surface of the silicon, tin or graphite-based active material to form a chemical bond, and the other functional group is a material that forms a chemical bond through a reaction with the nanocomposite according to the present invention, and is not particularly limited. For example, silane-based coupling agents such as triethoxysilylpropyl tetrasulfide, mercaptopropyl triethoxysilane, aminopropyl triethoxysilane, chloropropyl triethoxysilane, vinyltriethoxysilane, methacryloxypropyl triethoxysilane, glycidoxypropyl triethoxysilane, isocyanatopropyl triethoxysilane, and cyanatopropyl triethoxysilane may be used.
[0065] The buffer (buffering agent) may be, for example, one selected from the group consisting of NaHCO3, Na2CO3, K2HPO4, KH2PO4, Na2HPO4, NaOH and NH4OH.
[0066] As the molecular weight regulator, for example, mercaptans, terfins such as terpinolene, dipentene, and t-terpiene, and halogenated hydrocarbons such as chloroform and carbon tetrachloride can be used.
[0067] The conjugate diene copolymer may contain, based on the total weight, a polymer of (a) 20 to 45% by weight of the conjugated diene monomer or polymer, (b) 50 to 70% by weight of one or more monomers selected from the group consisting of acrylate monomers, vinyl monomers, and nitrile monomers, and (c) 1 to 20% by weight of one or more monomers selected from the group consisting of unsaturated carboxylic acid monomers and hydroxyl group-containing monomers. The other components such as the emulsifier, buffer, and crosslinker may be optionally contained within the range of 0.1 to 10% by weight.
[0068] When the content ratio between the monomers constituting the conjugate diene copolymer falls within the above-mentioned range, Tg can be -10°C or more and 40°C or less.
[0069] When the content ratio between the monomers constituting the conjugate diene copolymer falls within the above-mentioned range, the flexibility, insulating properties, and electrolyte resistance of the insulating layer can be significantly improved.
[0070] In the experimental examples of the present invention, it was confirmed that when the content ratio between each monomer constituting the conjugate diene copolymer falls within the above-mentioned range, both the initial adhesive strength and the insulating properties are excellent.
[0071] On the other hand, the average particle size of the copolymer may be 50 nm to 500 nm or less. If the average particle size of the copolymer is less than 50 nm or exceeds 500 nm, it is not preferable because the dispersion stability may decrease.
[0072] The insulating layer composition for a lithium secondary battery according to an embodiment of the present invention includes a non-aqueous organic solvent.
[0073] Meanwhile, when the copolymer particles in the composition according to the present invention exist as an independent phase, the effect of improving the adhesive strength is enhanced, so it is very important to prevent the occurrence of agglomeration between the particles. Therefore, the composition according to the present invention includes a dispersion solvent for dispersing the copolymer particles. In the present invention, a non-aqueous organic solvent is used as the dispersion solvent.
[0074] The non-aqueous organic solvent may be at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol.
[0075] Preferably, the non-aqueous organic solvent may be N-methyl-pyrrolidone (NMP), but is not limited thereto.
[0076] The insulating layer composition for a lithium secondary battery according to an embodiment of the present invention includes an emulsifier. By including an emulsifier, the insulating layer composition for a lithium secondary battery has excellent storage stability.
[0077] The emulsifier is a substance having both a hydrophilic group and a hydrophobic group. In one specific example, the emulsifier may be at least one selected from the group consisting of anionic emulsifiers and nonionic emulsifiers.
[0078] Nonionic emulsifiers, when used with anionic emulsifiers, can help control particle size and distribution and provide additional colloidal stabilization of the polymer particles through van der Waals forces in addition to the electrostatic stabilization of the ionic emulsifiers. Nonionic emulsifiers are not often used alone because they produce less stable particles than anionic emulsifiers.
[0079] The anionic emulsifier may be selected from the group consisting of phosphates, carboxylates, sulfates, succinates, sulfosuccinates, sulfonates and disulfonates. For example, the anionic emulsifier may be selected from the group consisting of sodium alkyl sulfate, sodium polyoxyethylene sulfate, sodium lauryl ether sulfate, sodium polyoxyethylene lauryl ether sulfate, sodium lauryl sulfate, sodium alkyl sulfonate, sodium alkyl ether sulfonate, sodium alkyl benzene sulfonate, sodium linear alkyl benzene sulfonate, sodium alpha olefin sulfonate, sodium alcohol polyoxyethylene ether sulfonate, sodium dioctyl sulfosuccinate, sodium perfluorooctane sulfonate, sodium perfluorobutane sulfonate, alkyl diphenyloxide disulfonate, sodium dioctyl sulfosuccinate (DOSS), sodium alkyl-aryl phosphate, alkyl ether phosate, and sodium lauryl sarcosinate. However, the anionic emulsifier is not limited to these, and all known anionic emulsifiers may be included in the scope of the present invention.
[0080] The nonionic emulsifier may be of the ester type, ether type, ester-ether type, etc. For example, it may be polyoxyethylene glycol, polyoxyethylene glycol methyl ether, polyoxyethylene monoallyl ether, polyoxyethylene bisphenol-A ether, polypropylene glycol, polyoxyethylene alkenyl ether, etc. However, it is not limited thereto, and all known nonionic emulsifiers may be included in the scope of the present invention.
[0081] Meanwhile, the content of the emulsifier is 0.3 wt% or more based on the total weight of the conjugate diene copolymer. Preferably, the content of the emulsifier may be 0.3 wt% or more and 5 wt% or less based on the total weight of the conjugate diene copolymer. If the content of the emulsifier is less than 0.3 wt%, the storage stability of the insulating layer composition for a lithium secondary battery may decrease, and if the content of the emulsifier is more than 5 wt%, the insulating properties of the insulating layer composition for a lithium secondary battery may deteriorate.
[0082] In the composition for a lithium secondary battery according to an embodiment of the present invention, the gel content is 70 wt % or more based on the total weight of the conjugate diene copolymer.
[0083] By containing a high gel content of 70 wt% or more, the insulating layer composition for lithium secondary batteries has excellent storage stability, and the initial adhesive strength can be appropriately adjusted so as not to be too high, which can prevent the electrodes from adhering to each other during the winding and slitting processes, thereby preventing deterioration of processability.
[0084] Meanwhile, the moisture content of the insulating layer composition for lithium secondary batteries may be 10,000 ppm or less, preferably 5,000 ppm or less, and more preferably 3,000 ppm or less. When the moisture content of the insulating layer composition for lithium secondary batteries is within the above range, the composition may be coated separately from the electrode (positive electrode) mixture layer, and the slurry for the electrode (positive electrode) mixture layer may be prevented from penetrating into the slurry for the insulating coating layer, thereby preventing deterioration of the physical properties of the electrode, such as failure to exhibit an insulating effect.
[0085] Meanwhile, the insulating layer composition for a lithium secondary battery according to an embodiment of the present invention may not contain carboxymethyl cellulose.
[0086] Carboxymethyl cellulose is sometimes used as a thickener in insulating layer compositions, but it has a problem of reducing processability in winding and cutting processes due to its brittleness. Therefore, the insulating layer composition for lithium secondary batteries according to the present invention does not contain carboxymethyl cellulose and is therefore not brittle, which can improve processability in winding and cutting processes.
[0087] 2. Manufacturing method of positive electrodes for lithium secondary batteries
[0088] Another example of the present invention provides a method for manufacturing a positive electrode for a lithium secondary battery, the method comprising the steps of: preparing a water-dispersible conjugated diene copolymer; adding a non-aqueous organic solvent to the water-dispersible conjugated diene copolymer, and heating and reducing pressure to prepare a slurry for an insulating coating layer; coating a slurry for a positive electrode mixture layer, the slurry including a positive electrode active material, a conductive material, a non-aqueous binder, and a non-aqueous organic solvent, on one or both sides of a positive electrode current collector; coating the slurry for the insulating coating layer from a portion of an uncoated portion of the positive electrode current collector to cover a portion of the slurry for the positive electrode mixture layer coated on the current collector; and drying the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer coated on the positive electrode current collector, the slurry for the insulating coating layer including an emulsifier.
[0089] First, a water-dispersible conjugated diene copolymer is prepared. The preparation method is the same as that disclosed in 1. Insulating layer composition for lithium secondary battery, so the detailed description is omitted.
[0090] Next, the water-dispersed conjugated dienes copolymer is mixed with a non-aqueous organic solvent, and the mixture is heated and reduced pressure.
[0091] At this time, water, which is the dispersion medium for the conjugate diene copolymer particles, is replaced with the non-aqueous organic solvent.
[0092] The method for producing a positive electrode for a lithium secondary battery of the present invention is extremely efficient in terms of the production process because the positive electrode can be produced by coating a slurry for a positive electrode mixture layer and a slurry for an insulating coating layer on a current collector, respectively, and then drying them together.
[0093] Preferably, the conjugated diene copolymer can be, but is not limited to, a conjugated diene latex.
[0094] Preferably, the conjugate diene latex can be, but is not limited to, a styrene-butadiene latex.
[0095] Preferably, the non-aqueous organic solvent may be, but is not limited to, N-methyl-pyrrolidone (NMP).
[0096] Preferably, the pressure can be reduced to less than 200 torr after the heating is performed to a setting temperature of 40° C. or more and 100° C. or less, thereby efficiently replacing water, which is the solvent of the water-dispersed conjugate diene latex, with a non-aqueous organic solvent.
[0097] Even after replacing the water, which is the dispersion medium of the conjugated diene latex particles, with a non-aqueous organic solvent, the conjugated diene latex particles maintain their particle shape. Whether or not the particle shape is maintained can be confirmed by particle size measurement. The particle size can be confirmed by, but is not limited to, a DLS particle size analyzer, a laser diffraction particle size analyzer, or an electron transmission microscope.
[0098] In addition, the insulating coating layer slurry contains an emulsifier. Since the insulating coating layer slurry contains an emulsifier, the insulating layer composition for a lithium secondary battery prepared using the same has excellent storage stability.
[0099] Next, a slurry for a positive electrode mixture layer containing a positive electrode active material, a non-aqueous binder, a conductive material, and a non-aqueous organic solvent is applied to one or both surfaces of the positive electrode current collector.
[0100] The positive electrode current collector may be one that does not induce chemical changes in the battery and has high conductivity. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. may be used, and in the case of aluminum or stainless steel, those that are surface-treated with carbon, nickel, titanium, silver, etc. may be used. For example, the current collector may be aluminum.
[0101] In addition, in the slurry for the positive electrode mixture layer, the positive electrode active material can be any positive electrode active material that is usually used in a positive electrode, and may be, but is not limited to, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or a lithium composite oxide that is a combination of these.
[0102] The non-aqueous binder may include one or more resins selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, and copolymers thereof. As an example, the binder may include polyvinylidene fluoride.
[0103] The conductive material is used to improve the performance of the positive electrode, such as electrical conductivity, and may be one or more selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, and carbon fiber. For example, the conductive material may include acetylene black.
[0104] The non-aqueous organic solvent may be one or more selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol, and may be, for example, N-methyl-2-pyrrolidone (NMP).
[0105] Simultaneously with or after the step of applying the slurry for the positive electrode mixture layer, the slurry for the insulating coating layer is applied from a portion of an uncoated portion of the positive electrode current collector to cover a portion of the slurry for the positive electrode mixture layer applied to the current collector.
[0106] Specifically, in the step of applying the slurry for the insulating coating layer to the current collector, the slurry for the insulating layer may be applied while the slurry for the positive electrode mixture layer is still wet, or the slurry for the positive electrode mixture layer and the slurry for the insulating layer may be applied simultaneously.
[0107] Next, the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer applied to the positive electrode current collector are dried.
[0108] The step of drying the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer may be performed by a drying method commonly known in the art, and the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer may be completely dried to remove the solvent.
[0109] In a specific example, the drying may be performed by changing a hot air method, a direct heating method, an induction heating method, etc. at a temperature at which the solvent is completely evaporated, but is not limited thereto. For example, the step of drying the insulating coating liquid may be performed by a hot air method.
[0110] At this time, the drying temperature may be in the range of 50° C. to 300° C., preferably 60 to 200° C., and more preferably 70 to 150° C. On the other hand, if the drying temperature of the insulating coating liquid is less than 50° C., the temperature may be too low to completely dry the insulating coating liquid, and if the drying temperature exceeds 300° C., the drying temperature may be too high to cause deformation of the electrodes.
[0111] As a result, a positive electrode mixture layer and an insulating coating layer are formed on the positive electrode current collector, and the resulting mixture is rolled to produce a positive electrode for a lithium secondary battery.
[0112] 3. Positive electrodes for lithium secondary batteries
[0113] According to another embodiment of the present invention, there is provided a positive electrode for a lithium secondary battery, comprising: a positive electrode current collector; a positive electrode tab protruding from the positive electrode current collector; and an insulating layer formed by coating an insulating material on the positive electrode tab, wherein the insulating material includes the insulating layer composition for a lithium secondary battery.
[0114] According to another embodiment of the present invention, the positive electrode for a lithium secondary battery includes an insulating layer containing the insulating layer composition for a lithium secondary battery on the positive electrode tab, and thus can be manufactured by simultaneously applying a slurry for a positive electrode mixture layer and a slurry for an insulating coating layer, which can significantly shorten the manufacturing process of the battery, ultimately reducing the manufacturing cost of the battery, and can further improve the safety of the battery by making the insulating area wider. In addition, the positive electrode for a lithium secondary battery includes an insulating layer containing the insulating layer composition for a lithium secondary battery on the positive electrode tab, and thus has an effect of not increasing the thickness of the electrode assembly, which is a problem that may occur when using a conventional insulating film or tape, that is, a very low possibility of detachment when bending the positive electrode tab for attachment to the corresponding area.
[0115] 4. Lithium secondary batteries
[0116] According to another embodiment of the present invention, there is provided a lithium secondary battery including the positive electrode for lithium secondary batteries.
[0117] More specifically, a lithium secondary battery according to another embodiment of the present invention may include a positive electrode, a negative electrode, a separator, and an electrolyte for a lithium secondary battery.
[0118] The lithium secondary battery may optionally further include a battery container that houses an electrode assembly including the positive electrode, the negative electrode, and a separator, and a sealing member that seals the battery container.
[0119] The negative electrode may include a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector.
[0120] The negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and examples thereof include copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, and aluminum-cadmium alloy. The negative electrode current collector may have a thickness of typically 3 μm to 500 μm, and like the positive electrode current collector, the current collector surface may be provided with fine irregularities to enhance the binding force of the negative electrode active material. For example, the negative electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, and nonwoven fabric.
[0121] The negative electrode active material layer may contain a negative electrode active material and, optionally, a binder and a conductive material.
[0122] The negative electrode active material may be a compound capable of reversible intercalation and deintercalation of lithium. Specific examples of the negative electrode active material include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, and Al alloys; and SiO. β(0<β<2), metal oxides capable of doping and dedoping lithium, such as SnO2, vanadium oxide, and lithium vanadium oxide, and composites containing the metallic compounds and carbonaceous materials, such as Si-C composites or Sn-C composites, can be used. A thin film of metallic lithium can also be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon can be used as the carbon material. Representative examples of low crystalline carbon include soft carbon and hard carbon, and representative examples of high crystalline carbon include amorphous, plate-like, flake-like, spherical or fibrous natural graphite or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, mesocarbon microbeads, mesophase pitches, and high-temperature fired carbon such as petroleum or coal tar pitch derived cokes.
[0123] The negative electrode active material is included in an amount of 80 to 99 parts by weight based on the total weight of the negative electrode active material layer.
[0124] The binder is a component that aids in bonding between the conductive material, active material, and current collector, and is usually added in an amount of 0.1 to 10 parts by weight based on the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0125] The conductive material is a component for further improving the conductivity of the negative electrode active material, and is added in an amount of 10 parts by weight or less, preferably 5 parts by weight or less, based on the total weight of the negative electrode active material layer. Such a conductive material is not particularly limited as long as it does not induce chemical changes in the battery and has conductivity, and examples of such conductive materials include graphite such as natural graphite and artificial graphite, carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, conductive fibers such as carbon fiber and metal fiber, metal powders such as carbon fluoride, aluminum, and nickel powder, conductive whiskeys such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and conductive materials such as polyphenylene derivatives.
[0126] The negative electrode active material layer may be prepared by coating a composition for forming a negative electrode active material layer, which is prepared by dissolving or dispersing a negative electrode active material, and optionally a binder and a conductive material in a solvent, on a negative electrode current collector and drying the composition. Alternatively, the composition for forming a negative electrode active material layer may be cast on a separate support, and then peeled off from the support to obtain a film, which may be laminated on the negative electrode current collector.
[0127] The separator separates the negative electrode and the positive electrode to provide a passage for lithium ions to move. Any separator that is generally used in lithium secondary batteries can be used without any particular limitation. In particular, a separator that has low resistance to electrolyte ion movement and excellent electrolyte humidification ability is preferred. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof is used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, etc., may be used. In addition, a coated separator containing a ceramic component or a polymeric material may be used to ensure heat resistance or mechanical strength, and is used in a single layer or multilayer structure.
[0128] Examples of the electrolyte include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries, but are not limited to these.
[0129] Specifically, the organic liquid electrolyte may include an organic solvent and a lithium salt.
[0130] The organic solvent is not particularly limited as long as it can function as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent may be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone, an ether solvent such as dibutyl ether or tetrahydrofuran, a ketone solvent such as cyclohexanone, an aromatic hydrocarbon solvent such as benzene or fluorobenzene, dimethylcarbonate (DMC), diethylcarbonate (DEC), methylethylcarbonate (MEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as polycarbonate (PC) and polycarbonate-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a hydrocarbon group having a linear, branched or cyclic structure with 2 to 20 carbon atoms, which may contain a double bond, an aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge / discharge performance of a battery and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) is more preferred. In this case, the performance of the electrolyte may be excellent if the cyclic carbonate and the chain carbonate are mixed in a volume ratio of about 1:1 to about 1:9.
[0131] The lithium salt is used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt may be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within the range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0132] In addition to the electrolyte components, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, and aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in battery capacity, and improving the discharge capacity of the battery. In this case, the additives may be contained in an amount of 0.1 to 5 parts by weight based on the total weight of the electrolyte.
[0133] Hereinafter, the present invention will be described in more detail with reference to the following examples, which are merely preferred examples of the present invention and are not intended to limit the scope of the present invention.
[0134] Example 1
[0135] 5 parts by weight of styrene-butadiene seed latex with a particle size of 55 nm was placed in a reactor and heated to 80°C, and then 35 g of 1,3-butadiene as a monomer, 62 g of styrene, 3 g of itaconic acid, 30.5 g of NaHCO3 as a buffer, 1 g of sodium polyoxyethylene lauryl ether sulfate as an emulsifier, 1 g of dodecyl mercaptan as a molecular weight regulator, and 1 g of potassium persulfate as a polymerization initiator were added to the reactor for 4 hours, and the mixture was reacted for another 4 hours while maintaining the temperature at 80°C to produce a styrene-butadiene copolymer latex with a solid content of 50%. At this time, the pH was adjusted to neutral (7) using sodium hydroxide. After polymerization, the size of the copolymer particles was analyzed using a Submicron particle sizer (Nicomp TM 380), and the average particle size of the polymerized copolymer particles was 150 nm and the gel content was 85%.
[0136] 100g of the prepared styrene butadiene copolymer latex was placed in a reactor, 700g of NMP (N-methyl-pyrrolidone) was added, mixed, and heated to 90°C. The pressure was then reduced to 15 torr within 3 hours to replace the water, which was the dispersion solvent for the styrene butadiene copolymer particles, with NMP, to prepare a composition containing a styrene butadiene copolymer dispersed in NMP. At this time, the final moisture content was 10,000ppm or less, and after checking the solid content, NMP was added so that the final solid content was 7.6%. The moisture content of the final product was measured using a Karl Fischer moisture meter.
[0137] Example 2
[0138] In Example 1, 30 g of 1,3-butadiene, 60 g of styrene, 5 g of methyl methacrylate, 2 g of acrylonitrile, 1 g of hydroxyacrylate, and 3 g of itaconic acid were used as monomers, and alkyldiphenyloxide disulfonate was used as an emulsifier instead of sodium polyoxyethylene lauryl ether sulfate. 1 g of alkyldiphenyloxide was further added before NMP substitution, and then a composition containing a styrene-butadiene copolymer dispersed in NMP was produced in the same manner as in Example 1.
[0139] Example 3
[0140] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that dodecyl mercaptan was not used as a molecular weight regulator, 0.4 g of sodium polyoxyethylene lauryl ether sulfate was used as an emulsifier, and 450 g of NMP was used.
[0141] Example 4
[0142] A composition containing a styrene-butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that 2 g of sodium lauryl sulfate was added as an emulsifier before adding NMP.
[0143] Example 5
[0144] A composition containing a styrene butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that 5 g of sodium lauryl sulfate was added as an emulsifier before adding NMP.
[0145] Comparative Example 1
[0146] In Example 1, 2.3 g of dodecyl mercaptan was used as a molecular weight regulator, and the amount of NMP used was increased to 1000 g. In the same manner as in Example 1, a composition containing a styrene-butadiene copolymer dispersed in NMP was prepared.
[0147] Comparative Example 2
[0148] A composition containing a styrene butadiene copolymer dispersed in NMP was prepared in the same manner as in Example 1, except that the amount of sodium polyoxyethylene lauryl ether sulfate used as an emulsifier was reduced to 0.1 g.
[0149] Comparative Example 3
[0150] PVDF (polyvinylidene fluoride) was dissolved in NMP to prepare a composition with a solid content of 8%.
[0151] Comparative Example 4
[0152] Hydrogenated nitrile rubber with 0% gel content was dissolved in NMP to prepare an 8% solids composition.
[0153] Comparative Example 5
[0154] Styrene-butadiene synthetic rubber with 0% gel content was dissolved in NMP to prepare a composition with 8% solids content.
[0155] Comparative Example 6
[0156] A styrene-butadiene copolymer latex having a solid content of 50% was produced in the same manner as in Example 2.
[0157] 100g of the prepared styrene-butadiene copolymer latex was placed in a reactor, 530g of NMP (N-methyl-pyrrolidone) was added, mixed, and heated to 85℃, and the pressure was reduced to 180 torr for 1 hour to replace the water, which is the dispersion solvent for the styrene-butadiene copolymer particles, with NMP to prepare a composition containing a styrene-butadiene copolymer dispersed in NMP. NMP was added so that the final solid content was 8%, and the final moisture content was 50,010ppm. The moisture content of the final product was measured using a Karl Fischer moisture meter.
[0158] Comparative Example 7
[0159] A styrene-butadiene copolymer latex having a solid content of 50% was produced in the same manner as in Example 2.
[0160] 100g of the prepared styrene-butadiene copolymer latex was placed in a reactor, 530g of NMP (N-methyl-pyrrolidone) was added, mixed, and heated to 90°C, and the pressure was reduced to 100 torr for 7 hours to replace the water, which is the dispersion solvent for the styrene-butadiene copolymer particles, with NMP to prepare a composition containing a styrene-butadiene copolymer dispersed in NMP. At this time, NMP was added to make the final solid content 8%, and the final moisture content was 12,201ppm. The moisture content of the final product was measured using a Karl Fischer moisture meter.
[0161] Comparative Example 8
[0162] To compare with a composition containing styrene-butadiene latex without solvent replacement, the styrene-butadiene latex prepared in Example 2 was mixed with carboxymethyl cellulose in a weight ratio of 9:1 without solvent replacement to prepare a composition. Carboxymethyl cellulose is used as a thickener to improve the coatability of styrene-butadiene latex without solvent replacement.
[0163] Experimental Example 1
[0164] For the compositions prepared in Examples 1 to 5 and Comparative Examples 1 to 7, the water content, viscosity, gel content and total emulsifier amount were measured according to the methods described in the following Experimental Examples 1-1, 1-2, 1-3 and 1-4, and the results are shown in the following Table 1. The following total emulsifier amount (%) is based on the total solid content of the composition.
[0165] [Table 1]
[0166] Experimental Example 1-1: Measurement of moisture content
[0167] For the compositions prepared in Examples 1 to 5 and Comparative Examples 1 to 7, the moisture content was measured by weighing 0.1 to 0.4 g of the sample at 220° C. using a Metrohm 899 Coulometer connected to an 860 KF Thermoprep oven.
[0168] Experimental Example 1-2: Viscosity measurement
[0169] The viscosity of the compositions prepared in Examples 1 to 5 and Comparative Examples 1 to 7 was measured 1 minute after rotating at 12 rpm using a Brookfield LV viscometer with a No. 63 spindle at a temperature of 25° C. When the viscosity was outside the measurement range, the rpm was lowered and the measurement was continued.
[0170] Experimental Example 1-3: Measurement of gel content
[0171] The gel content was measured for the compositions prepared in Examples 1 to 5 and Comparative Examples 1 to 7. 10 g of the obtained sample was dried at 135° C. for 30 minutes, and then a thin film was made and cut into a width of 2 mm×2 mm. A dish was made with 200 mesh and weighed on a precision balance, and the weight was indicated as A. 0.3 to 0.4 g of the cut film was placed in the dish, and the weight of the film was measured and indicated as B. The dish was placed in a 100 ml glass bottle, 75 ml of tetrahydrofuran was added, and the dish and glass bottle were sealed, and the dish was placed in a water bath type ultrasonic device and sonicated for 3 hours, and then the dish was taken out, washed with 50 ml of tetrahydrofuran, and dried in an oven at 135° C. for 30 minutes, and the weight was measured and indicated as C. During sonication, the temperature of the water bath should not exceed 50° C. The final gel content (%) was calculated according to the following formula.
[0172] Gel content (%) = (CA) / B*100
[0173] Experimental Example 1-4: Total emulsifier amount measurement
[0174] The total amount of emulsifier was measured for the compositions prepared in Examples 1 to 5 and Comparative Examples 1 to 7. Acetonitrile / methanol was added to 0.5 g of the obtained sample to precipitate the polymer component. After stirring for 1 hour, the polymer was precipitated using a centrifuge, and the supernatant was filtered and the amount of emulsifier was measured using HPLC / PDA / MS. The total amount of emulsifier was converted into the ratio of the emulsifier content to the total weight of solids and is shown in Table 1.
[0175] Experimental Example 2
[0176] Experiments to evaluate the initial adhesive strength, storage stability, and insulating properties of the compositions prepared in Examples 1 to 5 and Comparative Examples 1 to 5 were carried out according to the methods described in Experimental Examples 2-1, 2-2, and 2-3 below, and the results are shown in Table 2 below.
[0177] [Table 2]
[0178] Experimental Example 2-1: Initial Tackiness Evaluation
[0179] The compositions prepared in Examples 1 to 5 and Comparative Examples 1 to 5 were coated on aluminum metal foil and dried at 130° C. to prepare metal samples having an insulating coating layer of about 10 μm in thickness. The metal samples were cut to a size of 2 cm×12 cm and laminated on SUS plates (SUS plates), and the 90° adhesive strength was measured. The results are shown in Table 2 below.
[0180] As can be seen from Table 2, it was confirmed that all of the compositions of Examples 1 to 5 had low initial adhesion. If the initial adhesion is low, there is little possibility that the composition will adhere to the electrode or current collector during the winding and slitting process, thereby deteriorating the processability. On the other hand, Comparative Example 1, which has a gel content of less than 70 wt%, and Comparative Examples 4 and 5, which have no gel content, have too high initial adhesion, which may cause the electrodes to adhere to each other during the winding and slitting process, thereby deteriorating the processability.
[0181] Experimental Example 2-2: Storage stability evaluation
[0182] The compositions prepared in Examples 1 to 5 and Comparative Examples 1 to 5 were each placed in a 250 ml glass bottle (200 ml) and sealed. The bottles were then stored in an oven at 100° C. for 7 days, and then removed and stored at room temperature for 1 day. The solid content of the upper layer was then measured, and the reduction rate of the solid content relative to the base solid content was measured. The results are shown in Table 2.
[0183] The composition of Comparative Example 1, which has a low gel content, and the composition of Comparative Example 2, which has a low emulsifier content, have a higher solid content reduction rate than the compositions of Examples 1 to 5, and therefore it is expected that phase separation will occur over time, resulting in a significant decrease in storage stability.
[0184] Experimental example 2-3: Insulation characteristics evaluation
[0185] LiNi as the positive electrode active material 0.8 Co 0.2Mn 0.2 96 parts by weight of O2, 2 parts by weight of PVdF as a binder, and 2 parts by weight of carbon black as a conductive material were weighed and mixed in N-methylpyrrolidone (NMP) solvent to prepare a slurry for a positive electrode mixture layer. The slurry for the mixture layer was applied to an aluminum foil, dried, and then rolled to prepare a positive electrode having a positive electrode mixture layer with a thickness of 60 μm.
[0186] Thereafter, the insulating liquid, which was the composition produced in Examples 1 to 5 and Comparative Examples 1 to 5, was applied onto the positive electrode mixture layer and then dried to form a positive electrode insulating layer having a thickness of 10 μm.
[0187] A coin-type half cell was manufactured using the above positive electrode, a lithium foil as the negative electrode, and an electrolyte containing 1M LiPF4 in a solvent of EC:EMC=3:7. The coin-type half cell was stored in an oven at 60°C for 15 days, and then the discharge capacity of the half cell was measured to confirm the insulating effect of the insulating layer. For comparison, a half cell was manufactured using a positive electrode without an insulating coin layer, and the 0.1C discharge capacity was set as 100. The discharge capacity ratio of the positive electrodes having insulating coating layers formed with the compositions of Examples 1 to 5 and Comparative Examples 1 to 5 was calculated, and the results are shown in Table 2 below.
[0188] As can be seen from Table 2, the compositions of Comparative Examples 3 to 5 were found to have a higher 0.1C discharge capacity ratio than the compositions of Examples 1 to 5. This is because the insulating layer swelled or detached, decreasing the insulating performance and resulting in partial expression of the positive electrode capacity below the insulating layer. In the case of Example 5, which has an emulsifier content of 5.39%, which is slightly higher than Examples 1 to 4, it was found that the excess emulsifier slightly reduced the wet adhesive strength in the electrolyte, resulting in partial expression of the positive electrode capacity.
[0189] Experimental example 3: Moisture effect evaluation
[0190] LiNi as the positive electrode active material 0.8 Co 0.2 Mn 0.296 parts by weight of O2, 2 parts by weight of PVdF as a binder, and 2 parts by weight of carbon black as a conductive material were weighed and mixed in an N-methylpyrrolidone (NMP) solvent to produce a slurry for a positive electrode mixture layer.
[0191] The slurry for the positive electrode mixture layer and the slurry for the insulating coating layer, which are the compositions prepared in Example 2 and Comparative Examples 6 to 8, were simultaneously applied to a current collector using a doctor blade so as to be overlaid. The state of the current collector was observed immediately after application and 1 minute after application, and the results are shown in FIG.
[0192] As can be seen from Figure 1, a comparison was made immediately after application and one minute after application, and the composition of Example 2 maintained the initial coated state without penetration into the overlay both immediately after application and one minute after application, but the compositions of Comparative Examples 6 to 8, which have a higher water content than Example 2, had the electrode slurry penetrate into the insulating layer and were unable to reliably maintain the coating boundary. In particular, in the case of Comparative Example 8, where the dispersion solvent was not replaced, the area where the positive electrode slurry and insulating liquid come into contact immediately after application was coagulated by water, and it was confirmed that the aqueous insulating liquid without solvent replacement could not be simultaneously coated with the positive electrode slurry.
[0193] This can be interpreted as follows: if the moisture content of the positive electrode insulating coating layer slurry exceeds 10,000 ppm, when the positive electrode mixture layer slurry and the insulating layer slurry are simultaneously coated, the positive electrode mixture layer slurry permeates into the positive electrode insulating coating layer slurry, making it difficult to exhibit the expected insulating effect.
[0194] Experimental Example 4: Carboxymethylcellulose effect evaluation
[0195] The compositions prepared in Example 2 and Comparative Example 8 were coated on a substrate to a final thickness of 20 μm, dried at 130° C., cut into 2 cm widths, and then measured for brittleness. The samples were folded in half at room temperature, pressed once with a 1 kg roller, and then unfolded, and the coating film was visually checked for cracks or tears, and the results are shown in FIG. 2 below. In the case of Example 1, the film did not crack or tear, but in the case of Comparative Example 8, the film was torn. The composition of Comparative Example 8 is a composition in which the styrene-butadiene latex prepared in Example 2 was mixed with carboxymethyl cellulose in a weight ratio of 9:1 without performing a separate solvent replacement. This is because even a small amount of carboxymethyl cellulose, a thickener, is highly brittle and affects the coating film, so even if styrene-butadiene latex is coated separately without performing simultaneous coating, the insulating layer may be broken or detached during the winding and slitting process for this reason.
[0196] Although the above describes a preferred embodiment of the present invention, the present invention is not limited thereto, and can be embodied in various modified forms within the scope of the claims, the detailed description of the invention, and the accompanying drawings, which of course also fall within the scope of the present invention.
[0197] Accordingly, the true scope of the invention should be defined by the appended claims and their equivalents.
Claims
1. Conjugated dienes as binder polymers; A non-aqueous organic solvent; an emulsifier, The gel content is 70% by weight or more based on the total solids weight, The content of the emulsifier is 0.3% by weight or more based on the total solid content weight. An insulating layer composition for a lithium secondary battery.
2. The insulating layer composition for a lithium secondary battery does not contain carboxymethyl cellulose. The insulating layer composition for a lithium secondary battery according to claim 1 .
3. The conjugate diene copolymer comprises a polymer of (a) a conjugated diene monomer or a conjugated diene polymer, (b) at least one monomer selected from the group consisting of an acrylate monomer, a vinyl monomer, and a nitrile monomer, and (c) at least one monomer selected from the group consisting of an unsaturated carboxylic acid monomer and a hydroxyl group-containing monomer. The insulating layer composition for a lithium secondary battery according to claim 1 .
4. the conjugated diene monomer is one monomer selected from the group consisting of 1,3-butadiene, isoprene, chloroprene, and piperylene; The conjugated diene polymer is a polymer of two or more monomers selected from the group consisting of 1,3-butadiene, isoprene, chloroprene and piperylene, a styrene-butadiene copolymer, an acrylonitrile-butadiene copolymer, a styrene-isoprene copolymer, an acrylate-butadiene rubber, an acrylonitrile-butadiene-styrene rubber, an ethylene-propylene-diene polymer, a partially epoxidized or brominated polymer of these polymers, or a mixture thereof. The insulating layer composition for a lithium secondary battery according to claim 3 .
5. The acrylate monomer is at least one monomer selected from the group consisting of methyl ethacrylate, methacryloxyethyl ethylene urea, β-carboxyethyl acrylate, aliphatic monoacrylate, dipropylene diacrylate, ditrimethylolpropane tetraacrylate, dipentaerythriol hexaacrylate, pentaerythriol triacrylate, pentaerythriol tetraacrylate, and glycidyl methacrylate. The insulating layer composition for a lithium secondary battery according to claim 3 .
6. The vinyl monomer is at least one monomer selected from the group consisting of styrene, α-methylstyrene, β-methylstyrene, pt-butylstyrene, and divinylbenzene. The insulating layer composition for a lithium secondary battery according to claim 3 .
7. The nitrile monomer is one or more monomers selected from the group consisting of acrylonitrile, methacrylonitrile, and allyl cyanide. The insulating layer composition for a lithium secondary battery according to claim 3 .
8. The unsaturated carboxylic acid monomer is at least one monomer selected from the group consisting of maleic acid, fumaric acid, methacrylic acid, acrylic acid, glutaric acid, itaconic acid, tetrahydrophthalic acid, crotonic acid, isocrotonic acid, and nadic acid. The insulating layer composition for a lithium secondary battery according to claim 3 .
9. The hydroxy group-containing monomer is one or more monomers selected from the group consisting of hydroxyacrylate, hydroxyethyl acrylate, hydroxybutyl acrylate, hydroxypropyl acrylate, hydroxyethyl methacrylate, hydroxypropyl methacrylate, and hydroxybutyl methacrylate. The insulating layer composition for a lithium secondary battery according to claim 3 .
10. The conjugate diene copolymer comprises, based on the total weight, a polymer of (a) 20 to 45% by weight of a conjugated diene monomer or a conjugated diene polymer, (b) 50 to 70% by weight of at least one monomer selected from the group consisting of an acrylate monomer, a vinyl monomer, and a nitrile monomer, and (c) 1 to 20% by weight of one or more monomers selected from the group consisting of an unsaturated carboxylic acid monomer and a hydroxyl group-containing monomer. The insulating layer composition for a lithium secondary battery according to claim 3 .
11. The non-aqueous organic solvent is at least one selected from the group consisting of N-methyl-pyrrolidone (NMP), dimethylformamide (DMF), dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), ethylene carbonate (EC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dimethyl carbonate (DMC), propylene carbonate (PC), dipropyl carbonate (DPC), butylene carbonate (BC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), acetonitrile, dimethoxyethane, tetrahydrofuran (THF), gamma-butyrolactone, methyl alcohol, ethyl alcohol, and isopropyl alcohol; The insulating layer composition for a lithium secondary battery according to claim 1 .
12. Conjugate diene copolymer particles having an average particle size of 50 nm to 500 nm are present as an independent phase; The insulating layer composition for a lithium secondary battery according to claim 1 .
13. The copolymer is a styrene-butadiene copolymer, and the non-aqueous organic solvent is N-methyl-pyrrolidone (NMP). The insulating layer composition for a lithium secondary battery according to claim 1 .
14. The conjugate diene copolymer is a styrene-butadiene copolymer latex, and the non-aqueous organic solvent is N-methyl-pyrrolidone (NMP). The insulating layer composition for a lithium secondary battery according to claim 1 .
15. The moisture content is 10,000 ppm or less. The insulating layer composition for a lithium secondary battery according to claim 1 .
16. preparing a water-dispersed conjugated dienes copolymer; mixing the water-dispersed conjugated dienes copolymer with a non-aqueous organic solvent, and heating and reducing pressure to prepare a slurry for an insulating coating layer; applying a slurry for a positive electrode mixture layer, the slurry including a positive electrode active material, a non-aqueous binder, a conductive material, and a non-aqueous organic solvent, to one or both surfaces of a positive electrode current collector; applying the slurry for the insulating coating layer to a portion of an uncoated portion of the positive electrode current collector so as to cover a portion of the slurry for the positive electrode mixture layer applied to the current collector; and drying the slurry for the positive electrode mixture layer and the slurry for the insulating coating layer applied to the positive electrode current collector. The insulating coating layer slurry contains an emulsifier. A method for producing a positive electrode for a lithium secondary battery.
17. The step of preparing a slurry for the insulating coating layer includes replacing water, which is a dispersion medium for the conjugate diene copolymer particles, with a non-aqueous organic solvent; The method for producing a positive electrode for a lithium secondary battery according to claim 16.
18. The conjugate diene copolymer particles maintain their particle shape even after the dispersion solvent is replaced with a non-aqueous organic solvent. The method for producing a positive electrode for a lithium secondary battery according to claim 17.
19. The conjugate diene copolymer is a conjugate diene latex. The method for producing a positive electrode for a lithium secondary battery according to any one of claims 16 to 18.
20. the conjugate diene copolymer is a styrene-butadiene latex; The non-aqueous organic solvent is N-methyl-pyrrolidone (NMP). The method for producing a positive electrode for a lithium secondary battery according to claim 16.
21. A positive electrode current collector; a positive electrode tab protruding from the positive electrode current collector; an insulating layer coated with an insulating material on the positive electrode tab; The insulating material comprises the composition of claim 1. Positive electrode for lithium secondary batteries.
22. The positive electrode for a lithium secondary battery according to claim 21 is provided. Lithium secondary battery.
Citation Information
Patent Citations
Method of manufacturing lithium ion secondary battery, electrode and battery
JP2001176517A
Binder composition for electricity storage devices, slurry for electricity storage device electrodes, electricity storage device electrode, slurry for forming protective film, protective film, and electricity storage device
WO2013187188A1
Cathode comprising insulating layer on cathode tab and secondary battery comprising the same
KR101586530B1