Nickel-Based Alloys
A nickel-based alloy with tailored composition and heat treatment achieves high-temperature resistance and fatigue life, addressing the limitations of existing alloys by ensuring compatibility with ring rolling and maintaining mechanical properties.
Patent Information
- Application Number
- JP2024536129
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-12-14
- Filing Date
- 2022-12-14
- Publication Date
- 2024-12-03
AI Technical Summary
Existing nickel-based alloys for aircraft engine turbine casings fail to maintain fatigue life and creep resistance at high temperatures exceeding 650°C, necessitating a compromise between grain size and temperature resistance, and lack compatibility with manufacturing methods like ring rolling.
A nickel-based alloy with specific compositions and controlled heat treatment processes, including γ' supersolvus and subsolvus treatments, to achieve intermediate grain sizes (ASTM 2-6) and stable γ' precipitates, enhancing creep resistance and fatigue life up to 800°C, compatible with ring rolling.
The alloy maintains mechanical integrity at high temperatures, supporting efficient manufacturing through ring rolling and extending component life without compromising fatigue resistance.
Smart Images

Figure 2024544718000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to nickel-based alloys, and more particularly, to nickel-based alloys that are specifically designed for application in turbine casings for aircraft engines. [Background technology]
[0002] The objective of ACARE is to challenge engine manufacturers to significantly improve the performance of new generation turbojet engines, especially while significantly reducing their intensity, in line with the European Union's European Green Deal and the requirements to reduce the cost of ownership imposed by aircraft manufacturers. This leads to the need to improve engine efficiency by reducing the ventilation of hot engine parts. As a result, materials have to withstand increasingly high service temperatures.
[0003] For example, in the case of low pressure turbine casings, certain areas are subject to both fatigue and creep at extremely high temperatures, with a peak at 850°C, with a target of 800°C in new generation engines. However, for a longer fatigue life, a fine grain size (around 10 according to the ASTM E112 standard, hereafter abbreviated as ASTM) is preferred, while the best creep resistance is obtained with a coarse grained microstructure (around ASTM 0). A compromise is therefore necessary between these two opposing properties.
[0004] Today, the main known alloys for aviation turbine casing applications are Inconel 718, 718 Plus and Waspaloy. Their maximum service temperatures are about 650°C, 704°C and 750°C, respectively. Moreover, their mechanical properties are reduced due to softening of their microstructure. Therefore, these alloys are not designed to withstand temperatures of about 800°C for extended periods of time.
[0005] Other alloys resulting from powder metallurgy, such as that described in EP1840232B1, make it possible to reach these high service temperatures. However, this alloy contains more than 43% by volume of γ' precipitates and its ductility is insufficient to consider ring roll forming, a technique used for the manufacture of components such as turbine casings for aeroengines. The current upper limit generally accepted is indeed around 40% γ' precipitates.
[0006] This is why Waspaloy, an alloy containing 25% by volume of γ' precipitates (nominal composition, by weight percent, is Cr 18.00-21.00, Co 12.00-15.00, Mo 3.50-5.00, Al 1.20-1.60, Ti 2.75-3.25, B 0.003-0.01, C 0.02-0.10, Zr 0.02-0.08, Fe 0-2.00, Mn 0-0.10, Si 0-0.15, P 0-0.015, S 0-0.015, and Cu 0-0.10), is currently the alloy that allows the best compromise between fatigue life and creep resistance at high temperatures. This compromise is achieved by obtaining an intermediate grain size (ASTM 2-6) throughout the component. However, again, this alloy was not designed to withstand service temperatures of 800° C. for very long periods of time.
[0007] Some alloys with 36 vol.% gamma prime precipitates, such as AD730TM or Rene65, may have better properties than Waspaloy, but are currently unable to achieve intermediate and uniform grain sizes across large parts. Their grain size, controlled by γ′, actually grows very rapidly when the temperature exceeds the γ′ solvus. Avoiding excessive grain growth requires precise control of the heat treatment temperature to the nearest degree throughout the part, which cannot be achieved in industrial furnaces.
[0008] For this reason, currently no alloy exists that combines better heat resistance than Waspaloy, the ability to be formed by ring rolling, and the ability to reach a uniform and intermediate grain size throughout the part through heat treatment to ensure the compromise between creep resistance and fatigue life required for the intended application.
[0009] Therefore, there is a need to have a new alloy that can meet the need for increased component service temperatures without reducing fatigue life compared to Waspaloy, while maintaining the ring rolling manufacturing process. [Prior art documents] [Patent documents]
[0010] [Patent Document 1] European Patent No. 1840232 Summary of the Invention [Problem to be solved by the invention]
[0011] It is therefore an object of the present invention to overcome at least one of the above mentioned disadvantages. [Means for solving the problem]
[0012] To this end, the present invention provides a nickel-based alloy comprising, in weight percent: 4.0-15.7% Cobalt, 15.3-19.5% chromium, 1.6-5.45% molybdenum, 1.65~2.5% aluminum, 2.8-4.3% titanium, 0.01~0.10% carbon, 0.003-0.02% boron, and 0.01-0.10% zirconium The present invention provides a nickel-base alloy comprising:
[0013] Other optional and non-limiting features are:
[0014] The nickel-based alloy contains, by weight percent: 0.02~0.06% carbon, 0.005-0.01% boron, and 0.02-0.06% zirconium may include.
[0015] The nickel-based alloy contains, by weight percent: 1.65 to 2.10% aluminum, and 2.8-3.45% titanium may include.
[0016] The nickel-based alloy contains, by weight percent: 4.0-13.2% Cobalt, 1.80 to 2.30% aluminum, and 3.5-4.0% titanium may include.
[0017] The nickel-based alloy contains, by weight percent: 4.0-11.0% Cobalt, 2.0 to 2.50% aluminum, and 4.05-4.4% titanium may include.
[0018] The nickel-base alloy may contain up to 6.0 wt. % iron, preferably up to 4.0 wt. % iron.
[0019] The nickel-base alloy may include up to 6.3 weight percent tungsten.
[0020] The nickel-base alloy may contain up to 0.4% by weight niobium.
[0021] The present invention further provides a method for processing such an alloy, comprising the steps of: - producing a billet having the same composition as the composition of the nickel-based alloy; Molding the part; - heat treating the part; The present invention provides a method comprising:
[0022] Other optional and non-limiting features are:
[0023] Producing a billet involves: - preparing an ingot, preferably by melting a material; - converting the ingot into a billet, preferably by cutting and then forging the ingot; may include.
[0024] Molding a part is - forging the billet, preferably by upset forging; - rolling the forged billet, preferably by ring rolling; may include.
[0025] Heat treating a part is - γ' supersolvus solution heat treatment, preferably at a temperature 10-40°C above the γ' solvus, and - γ' subsolvus solution heat treatment, preferably at a temperature 10-40°C lower than the γ' solvus The processing may include at least one of the following:
[0026] Heat treatment is Preferably, by heating to a temperature of 825 to 870°C, M 23 Tempering to precipitate C6 carbides, and Optionally, tempering to stabilize the population of γ' precipitates, preferably at temperatures between 760 and 825°C. It may further include.
[0027] The invention also proposes an aeronautical part, in particular a turbine casing, made of the above-mentioned alloy.
[0028] The nickel-base alloy according to the present invention is suitable for the manufacture of components intended to withstand temperatures of about 800°C in their hottest parts, and temperature spikes up to 850°C, while maintaining good fatigue resistance throughout the component.
[0029] This compromise is made possible by adjusting the grain size by heat treatment and forging, which makes it possible to obtain intermediate grain sizes between ASTM 2 and 6. The alloy is also suitable for vacuum casting and ring roll forming, techniques that make it possible to reduce production costs compared to other routes such as powder metallurgy or direct manufacturing.
[0030] Other objects, features and advantages will become apparent from the following description when taken in conjunction with the drawings. [Brief description of the drawings]
[0031] [Figure 1] FIG. 1 is a diagram illustrating the steps of a method for manufacturing a component made from a nickel-based alloy according to the present invention. [Diagram 2] FIG. 2 is a diagram illustrating an example of a billet production sub-step of the method according to the invention. [Diagram 3] FIG. 3 is a diagram showing an example of an ingot preparation sub-process in the billet production process. [Figure 4] FIG. 4 is a diagram showing an example of a sub-process of converting an ingot into a billet in the billet production process. [Diagram 5] FIG. 5 illustrates an example of a part forming sub-step of the method according to the invention. [Figure 6] FIG. 6 shows a first example of the heat treatment substep of the method according to the invention. [Figure 7] FIG. 7 shows a second example of the heat treatment substep of the method according to the invention. [Figure 8] FIG. 8 shows a third example of the heat treatment substep of the method according to the invention. [Figure 9]FIG. 9 is a diagram showing grain boundaries and carbide precipitates in an alloy according to the present invention after treatment according to one of the treatment methods of FIGS. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The nickel-based alloy according to the present invention will now be described. Throughout the following, the composition of the alloy will always be given in weight percent.
[0033] The composition of such an alloy is presented in Table 1 below. Nickel is not specified. Generally speaking, the amount of nickel corresponds to the remainder to reach 100%. Moreover, as with any alloy composition, it is technically impossible to avoid residual impurities. Therefore, certain trace elements may be present, although not mentioned in the composition presented here. Those skilled in the art will be able to recognize whether an element is present as a trace element or whether the element was added intentionally. Indeed, it is recognized that trace forms of elements do not impart specific properties to the alloy or change any of the properties of the alloy.
[0034] [Table 1]
[0035] Thus, the present alloy comprises the elements cobalt, aluminum and titanium, which are intended to form strengthening γ′ precipitates of ordered structure L12 and composition (Ni,Co)3(Al,Ti).
[0036] In addition, cobalt contributes to enhancing the mechanical resistance to heat by solid solution hardening of the γ matrix, and the carbides of interest, MC (M=Ti, Mo) and M 23 It allows control of the stable domain of C6 (M=Cr, Mo).
[0037] The chromium content makes it possible, in particular, to promote the oxidation resistance of the alloy while reducing the precipitation of embrittlement-inducing TCP phases (Topologically Close Packed, also known as Frank-Kasper phases). In addition, chromium contributes to the oxidation resistance of the alloy. 23 Involved in the formation of C6 carbides.
[0038] Molybdenum contributes to the mechanical strengthening of the alloy against heat. Its content is optimized to maximize this strengthening while limiting the precipitation of the supposedly weakening σ or μ TCP phases. The σ TCP phase is an intermetallic compound with no defined stoichiometry and an electron / atom ratio of 6.2 to 7. The σ TCP phase has a basic unit cell of 30 atoms. The μ TCP phase has an ideal A6B7 stoichiometry. Furthermore, this element is present in the MC and M 23 It is part of the composition of C6 type carbides. The MC type carbides are intended to regulate the grain size by tightly pinning the grain boundaries during the γ' supersolvus treatment. Furthermore, as a first analogy, TCP phases have all the same effect, in particular the reduction of the ductility of the alloy by creating potential crack initiation sites. In addition, the formation of TCP phases also contributes to reducing the solid solution strengthening of the matrix, since they siphon off some of the atoms of the alloying elements.
[0039] Titanium is involved in the formation of MC type carbides.
[0040] Carbon is used to control grain growth through the precipitation of MC carbides, and M 23 It is present to enhance the heat resistance of grain boundaries by forming C6 carbides.
[0041] The elements boron and zirconium also make it possible to increase the strength of the grain boundaries over the entire service temperature range, especially up to 850°C.
[0042] The alloy may also contain up to 6.0% by weight of iron, or even up to 4.0% by weight of iron. Iron is a cheap element, making it possible to reduce the density of the alloy and its cost. Furthermore, taking the iron content into account when searching for a composition suitable for the intended application makes it possible to recycle iron-containing alloys for the manufacture of the nickel-based alloys of the present invention, thus expanding the range of available recycled resources.
[0043] The alloy may also contain up to 6.3% by weight of tungsten. Tungsten in addition to or as a replacement for molybdenum makes it possible to improve the mechanical behavior of the alloy at high temperatures, in particular by solid solution hardening of the γ matrix. The addition of molybdenum and tungsten in the alloy may also be between 2% and 5% atomic percent. This avoids promoting the precipitation of TCP phases, in this case M 23 In the formula of C6 type carbides, M=Cr, Mo, W.
[0044] The alloy may also contain up to 0.4% by weight of niobium. When the alloy contains niobium, the L12 ordered structure has the composition (Ni,Co)3(Al,Ti,Nb) instead of (Ni,Co)3(Al,Ti). Taking the niobium content into account when searching for a composition suitable for the intended application allows the alloys containing niobium to be recycled for the manufacture of the nickel-based alloys of the invention, thus expanding the range of available recycled resources. The maximum limit of the range, i.e. 0.4%, allows preferential stabilization of titanium carbides over niobium carbides.
[0045] Thus, the composition of the alloy according to the invention preferably follows Table 2, with nickel making up the balance.
[0046] [Table 2]
[0047] Such alloys have a higher heat resistance than Waspaloy, in particular due to the higher mole fraction of γ' precipitates. For this reason, for such compositions, this mole fraction is greater than 28%, in particular between 28 and 40%. Moreover, such compositions limit the mole fraction of γ' precipitates to 40%. Furthermore, the solvus temperature of γ' precipitates is limited to 1120 °C. This facilitates the forming of the alloy by ring rolling.
[0048] This composition also ensures that the sum of the atomic percentages of the elements Al, Ti and Nb is between 7 and 10 at%, which makes it possible to obtain a molar fraction of the γ' phase between 28% and 40%. Moreover, this composition ensures that the atomic ratio between the element Al on the one hand and the elements Ti and Nb on the other hand (Al / (Ti+Nb)) is between 0.85 and 1.2, which results in favoring the precipitation of the γ' phase over the η-Ni3Ti phase, the latter being undesirable from the standpoint of mechanical properties. In other words, the Ti content is optimized in the γ' phase, maximizing the mechanical strengthening of the alloy against heat, while avoiding any promotion of the formation of the η phase to the detriment of the γ' phase.
[0049] This composition is characterized by carbides at grain boundaries, especially M 23 It induces the precipitation of C6 type carbides and enhances the creep resistance of the alloy at high temperatures. In particular, the carbides have a discrete distribution at the grain boundaries. The carbides generally have a nodular shape smaller than 5 μm, advantageously smaller than 1 μm. The discrete distribution at the grain boundaries is made possible by combining the composition with an appropriate heat treatment as described below.
[0050] M 23 The amount of C6 carbides may be between 0.4 and 1 mol%, advantageously between 0.5 and 0.75 mol%, making it possible to obtain a sufficient carbide population to guarantee the desired hardening and to avoid saturation of the grain boundaries, which in fact promote undesirable intragranular precipitation.
[0051] Furthermore, M 23 The solvus of C6 carbides meets the following criteria: (γ'Solvus-M 23C6 Solvus)≧40℃
[0052] Compliance with this standard ensures that M 23 It is now possible to carry out a γ' subsolvus heat treatment without the risk of C6 carbide precipitation. In fact, above this temperature, M 23 Precipitation of C6-type carbides may occur preferentially on grain boundaries in the form of thin films or platelets, which adversely affects crack propagation resistance.
[0053] Furthermore, this composition has a M 23 It guarantees the solvus of C6 carbides, thus making it possible to avoid re-melting of the carbides during temperature spikes above 850°C during operation, which ultimately makes it possible to avoid deteriorating the mechanical aspects.
[0054] In addition, the alloy has an intermediate grain size between ASTM 2 and 6 that is an excellent compromise between the creep resistance at high temperatures promoted by a coarse grain size and the fatigue resistance promoted by a fine grain size.
[0055] This intermediate grain size is obtained in particular by the presence of a controlled population of MC carbides, which makes it possible to limit the enlargement of the grains during forging and during heat treatment above the γ' solvus. These carbides generally have a spherical, sometimes angular shape, and a size of less than 5 μm, in the presence of traces of nitrogen. Preferably, the molar amount of MC carbides is between 0.1 and 0.3% at a temperature above the solvus of the γ' phase, for example at the γ' solvus temperature of +40° C.
[0056] The presence of MC carbides allows the grain boundary 2 to be firmly anchored onto the MC carbides 3 during heat treatment (FIG. 9), which keeps the grain growth within the target values of ASTM 2-6.
[0057] The mole fraction of MC carbides limited to 0.3% makes it possible to avoid the reduction in fatigue life due to the formation of coarser carbides and carbonitrides (i.e., larger than 5 μm in size) associated with manufacturing by casting and forging.
[0058] Another way to limit the formation of coarse carbides is to have the solvus temperature of the MC carbides lower than the solidus of the alloy, which is made possible by this composition.
[0059] A preferred composition is according to Table 3 below, or Table 4 if the amounts of Fe, W and Nb are taken into account.
[0060] [Table 3]
[0061] [Table 4]
[0062] These compositions ensure that the sum of the atomic percentages of the elements Al, Ti and Nb is between 7 and 8.25 at.%.
[0063] Another preferred composition is according to Table 5 below, or Table 6 if the amounts of Fe, W and Nb are taken into account.
[0064] [Table 5]
[0065] [Table 6]
[0066] These compositions ensure that the sum of the atomic percentages of the elements Al, Ti and Nb is between 8.5 and 9% at.
[0067] Yet another preferred composition is according to Table 7 below, or Table 8 if the amounts of Fe, W and Nb are taken into account.
[0068] [Table 7]
[0069] [Table 8]
[0070] These compositions ensure that the sum of the atomic percentages of the elements Al, Ti and Nb is between 9.25 and 10 at.%. Moreover, these compositions correspond to the compositions giving the highest molar content of γ' precipitates, up to 40%.
[0071] A method for manufacturing a component made from a nickel-based alloy as described above will now be described with reference to Figures 1-8.
[0072] The method includes a step 100 of producing a billet having a composition similar to that of the nickel-based alloy, a step 200 of forming a part, and a step 300 of heat treating the part (FIG. 1).
[0073] The step 100 of manufacturing a billet can in particular include a step 110 of making an ingot and a step 120 of converting the ingot into a billet (FIG. 2). The step 110 of making an ingot can be achieved by a step 111 of melting the materials selected to obtain the composition of the nickel-based alloy as described above (FIG. 3). This first step in making an ingot can in particular be carried out by vacuum induction melting (VIM). The step 110 of making an ingot can also include one or more remelting processes 112. For example, this step includes electroslag remelting (ESR) and / or vacuum arc remelting (VAR) (FIG. 3). These additional steps make it possible to improve the overall cleanliness of the ingot and to minimize macrosegregation.
[0074] The conversion of the ingot into a billet, step 120, may be carried out by forging, step 121 of cutting the ingot, in particular by the successive performance of step 122 of upsetting the nickel-base alloy to refine the solidification structure of the nickel-base alloy, and step 123 of drawing (FIG. 4).
[0075] Forming the part 200 may include forging the billet 210, particularly by upset forging the nickel-based alloy forming the billet. Forming the part may also include post-forging rolling 220, particularly ring rolling (FIG. 5).
[0076] In particular, the process 300 of heat treating the component includes at least one of a gamma prime supersolvus solution heat treatment 310 and a gamma prime subsolvus solution heat treatment 320 (FIGS. 6-8).
[0077] The gamma prime supersolvus solution heat treatment 310 allows the grains to grow to a desired size, in particular between ASTM 2 and 6, such as ASTM 4. For example, the gamma prime supersolvus solution heat treatment 310 is carried out by heating at a temperature between 10 and 40° C. above the gamma prime solvus, in particular for a period between 1 and 8 hours.
[0078] The gamma '-subsolvus solution heat treatment 320 makes it possible to refine the size of the gamma '-precipitates and improve the mechanical strength of the alloy. This solution heat treatment is followed by a quench. For example, the gamma '-subsolvus solution heat treatment 320 is carried out by heating at a temperature between 10 and 40 °C below the gamma '-solvus, in particular for a period between 1 and 8 hours. The gamma '-subsolvus solution heat treatment 320 can be carried out immediately after the step 200 of forming the part, when the desired grain size has already been reached during forging.
[0079] The step of heat treating the component 300, particularly after the gamma prime supersolvus solution heat treatment 310 and / or the gamma prime subsolvus solution heat treatment 320, may further comprise the steps of: 23 It may further include tempering 330 to precipitate C6 carbides. 23 This tempering 330 for precipitating C6 carbides is carried out by heating to a temperature between 825° C. and 870° C., preferably between 840° C. and 860° C., for example to a temperature of about 850° C., in particular for a period of 4 to 8 hours.
[0080] The step 300 of heat treating the component may further comprise a tempering 340 for stabilizing the population of γ' precipitates, typically after tempering 330 for precipitation, particularly at a temperature close to the targeted service temperature, for example between 760° C. and 825° C. (FIG. 6), preferably between 790° C. and 810° C., for example at about 800° C. For example, this tempering 340 for stabilization is performed by heating between 760° C. and 825° C., particularly for a period of 4 to 16 hours.
[0081] Thus, the process of heat treating the part may in particular include the following combinations (see identifying numbers in reference numbers 310, 320, 330 and 340): 1+3, 1+4, 2+3, 2+4, 1+2+3, 1+2+4, 1+3+4, 2+3+4, 1+2+3+4. EXAMPLES
[0082] Table 9 gives the mass composition of 24 examples according to the invention (Examples 1 to 24) and a comparative example (Example C1). Table 10 gives the characteristics for these examples.
[0083] [Table 9]
[0084] [Table 10]
[0085] In the table, P1 is the atomic ratio Al / (Ti+Nb), P2 is the sum of the atomic percentages of the elements Al, Ti and Nb, and P3 is the M determined at 850°C. 23 is the mole percent of C6 carbides, P4 is the γ' solvus (°C), and P5 is the M 23 C6 type carbide solvus (℃), P6 is the γ' solvus and M 23 P5 is the difference from the solvus of C6 carbides (°C), P6 is the mole percentage of MC carbides that is 40°C above the γ' solvus temperature, P7 is the solvus of MC carbides (°C), and P8 is the solidus (°C).
Claims
1. A nickel-based alloy comprising, in weight percent: 4.0 to 15.7% cobalt, 15.3 to 19.5% chromium, 1.6 to 5.45% molybdenum, 1.65 to 2.5% aluminum, 2.8 to 4.3% titanium, 0.01 to 0.10% carbon, 0.003 to 0.02% boron, 0.01 to 0.10% zirconium, 0-6.0% iron, 0 to 6.3% tungsten, and 0 to 0.4% niobium, The balance up to 100% is equivalent to nickel Nickel-based alloys, including
2. In weight percent, 0.02 to 0.06% carbon, 0.005 to 0.01% boron, and 0.02 to 0.06% zirconium The nickel-base alloy of claim 1 , comprising:
3. In weight percent, 1.65 to 2.10% aluminum, and 2.8-3.45% titanium The nickel-base alloy of claim 2 , comprising:
4. In weight percent, 4.0 to 13.2% cobalt, 1.80 to 2.30% aluminum, and 3.5-4.0% titanium The nickel-base alloy of claim 2 , comprising:
5. In weight percent, 4.0 to 11.0% cobalt, 2.0 to 2.50% aluminum, and 4.05-4.4% titanium The nickel-base alloy of claim 2 , comprising:
6. A method of manufacturing a component made from a nickel-based alloy according to any one of claims 1 to 5, comprising the steps of: producing a billet having the same composition as the nickel-based alloy; Molding the part; heat treating the component; A method comprising:
7. The step of heat treating the component comprises: a gamma-prime supersolvus solution heat treatment, preferably at a temperature 10-40° C. above the gamma-prime solvus; and γ' subsolvus solution heat treatment, preferably at a temperature 10-40°C lower than the γ' solvus The method of claim 6 , further comprising at least one of the steps:
8. The heat treatment is Preferably, by heating to a temperature of 825 to 870° C., M 23 C 6 Tempering to precipitate carbides; and Optionally, tempering to stabilize the population of gamma prime precipitates, preferably at a temperature between 760 and 825°C. The method according to any one of claims 6 to 7, further comprising:
9. An aeronautical component, in particular a turbine casing, made from an alloy according to any one of claims 1 to 5.
Citation Information
Patent Citations
Nickel-based alloy
EP1840232A1