Liquid Wire
A gallium alloy composite with dispersed gallium oxide microstructures addresses the challenges of manufacturing stretchable conductors by providing high conductivity and resistance to oxidation, enabling reliable and scalable production for flexible electronic devices.
Patent Information
- Application Number
- JP2022135340
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-02-29
- Filing Date
- 2022-08-26
- Publication Date
- 2024-09-17
- Estimated Expiration
- 2037-02-27
AI Technical Summary
Existing manufacturing methods for stretchable conductors face challenges in achieving high conductivity and ease of processing, with high failure rates due to difficulties in sealing microfluidic channels and susceptibility to oxidation, leading to irreversibly leaking or breaking under fatigue conditions.
A novel composite material comprising a gallium alloy with dispersed gallium oxide microstructures, forming a Bingham plastic that is easily patterned and resistant to oxidation, maintaining conductivity even under strain, achieved by mixing gallium oxide into a gallium alloy with cross-linked nanostructures and submicron-scale particles.
The composite material exhibits high conductivity, low sheet resistance, and self-healing properties, allowing for reliable and scalable production of flexible conductive paths suitable for wearable devices and stretchable interconnects.
Smart Images

Figure 0007551050000004 
Figure 0007551050000017 
Figure 0007551050000023
Abstract
Description
CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of priority to the earlier filing date of U.S. Provisional Patent Application No. 62 / 301,622, filed February 29, 2016, which is specifically incorporated by reference in its entirety. [Technical field]
[0002] SUMMARY OF THE DISCLOSURE Embodiments herein relate to liquid wires, and more particularly to liquid wires having integral microstructures and comprising a gallium indium alloy. [Background technology]
[0003] There is growing interest in incorporating electronics into everyday objects, including clothing and fabrics, which are expected to be flexible and stretchable. Soft electronics could seamlessly interface with the human body, opening up many new applications for wearable devices, medical devices, and conformal robotics or "soft machines" candidates that can more safely interact with humans and delicate objects. (See, for example, Dickey, ACS Appl Mater Interfaces, 12 Nov 2014, Vol. 6, No. 21, pp. 18369-18379.)
[0004] Many alternative manufacturing methods, especially 3D printing, have been considered to produce these flexible electronic devices, but a major bottleneck is the lack of stretchable conductors that are both highly conductive and easily fabricated.
[0005] Many attempts have been made at stretchable conductors. One of the most successful examples was a microfluidic channel filled with room temperature liquid metal. Functional devices are created by etching micrometer-sized channels in polydimethylsiloxane (PDMS), sealing them, and then injecting metal alloys into the channels to create conductive pathways. These alloys have melting points as low as -19 °C, so they can remain fluid under normal conditions. Because metal conductors are fluids, they can deform to an extent limited only by the material that forms the channel that contains the conductor, and they can also fully recover. Furthermore, the change in resistance of a metal conductor is linear, since it is a purely mechanical function of the wire length and cross section. This offers the great advantage that the conductive pathways can also function as sensors.
[0006] However, fabricating devices with these microfluidic channels is very challenging. PDMS is the preferred substrate, but it is costly to form a suitable seal around the channels, and the layer containing the channels must be exposed to oxygen plasma to attach a cap layer to surround the channels. After fabrication, the channels must be filled via a two-syringe system, where one syringe injects the liquid alloy and the other evacuates the air already present. The failure rate during fabrication is very high. Based on individual cases, it has been reported that only about one successful attempt is made in 20 fabrication attempts. Thus, there is a demand for other "liquid" metals. [Brief description of the drawings]
[0007] Embodiments of the present invention will become readily understood from the following detailed description taken in conjunction with the accompanying drawings and claims, the embodiments being illustrated by way of example and not by way of limitation in the figures of the accompanying drawings.
[0008] [Figure 1A]FIG. 1A is a digital image of a scanning electron microscope (SEM) image showing various gallium containing formulations according to various embodiments. [Figure 1B] FIG. 1B is a digital image of a scanning electron microscope (SEM) image showing various gallium containing formulations according to various embodiments. [Figure 1C] FIG. 1C is a digital image of a scanning electron microscope (SEM) image showing various gallium containing formulations according to various embodiments. [Figure 1D] FIG. 1D is a digital image of a scanning electron microscope (SEM) image showing various gallium containing formulations according to various embodiments. [Figure 1E] FIG. 1E is a digital image of a scanning electron microscope (SEM) image showing various gallium containing formulations according to various embodiments.
[0009] [Figure 2A] FIG. 2A shows digital images of failed (FIGS. 2A, 2B) and successful (FIG. 2C) compression tests according to various embodiments. [Figure 2B] FIG. 2B shows digital images of failed (FIGS. 2A, 2B) and successful (FIG. 2C) compression tests according to various embodiments. [Figure 2C] FIG. 2C shows digital images of failed (FIGS. 2A, 2B) and successful (FIG. 2C) compression tests according to various embodiments.
[0010] [Diagram 3] FIG. 3 is a digital image of an initial observation of high fidelity contact transfer of a metal gel pattern.
[0011] [Figure 4A] 4A is a digital image of a test contact transfer pattern with particle-filled metal gel, the pattern having trace widths as fine as 0.5 mm and pitches as fine as 0.25 mm according to various embodiments. [Figure 4B]4B is a digital image of a test contact transfer pattern with particle-filled metal gel, the pattern having trace widths as fine as 0.5 mm and pitches as fine as 0.25 mm according to various embodiments. [Figure 4C] 4C is a digital image of a test contact transfer pattern with particle-filled metal gel, the pattern having trace widths as fine as 0.5 mm and pitches as fine as 0.25 mm according to various embodiments. [Figure 4D] 4D is a digital image of a test contact transfer pattern with particle-filled metal gel, the pattern having trace widths as fine as 0.5 mm and pitches as fine as 0.25 mm according to various embodiments.
[0012] [Diagram 5] FIG. 5 is a digital image of a patterned pressure sensor according to various embodiments.
[0013] [Figure 6] FIG. 6 is a graph of a strain test of an 8 inch trace of metal gel encapsulated in silicone, showing the linearity of resistance versus degree of strain.
[0014] [Figure 7] FIG. 7 illustrates variable resistance oriented to changes due to strain along the warp or weft directions.
[0015] [Figure 8] Figure 8 shows a simple 1x3 grid with 10 variable resistors and four analog output elements A, B, C, and D. Every unique pairing of the output elements produces a 6-element vector. By appropriately weighting the resistance range of each variable resistor, we can ensure that the output vector uniquely encodes all possible resistor combinations to any fidelity.
[0016] [Figure 9]FIG. 9 is a digital image of a 990 MHz antenna printed from metal gel according to embodiments disclosed herein.
[0017] [Figure 10] Figures 10A-10D are examples of trace patterns. Figure 10A is a simple line that acts as a variable resistance that changes with strain parallel to the path. Figure 10B has a return path that allows the signal to be read at i / o ports close to each other. The vertical connecting bars produce negligible resistance change for strain measured parallel to the main trace. In Figure 10C, the zigzag pattern adds resistance / strain feedback for strain perpendicular to the direction of the trace. Figure 10D is a trace with a return path and a resistance / strain feedback multiplier in the horizontal section. This trace is sensitive to strain parallel to its direction but not perpendicular to it.
[0018] [Figure 11] Figure 11 is a graph of measured insertion loss to 6 GHz for a 1.4 mil (35 μm) thick Cu reference trace and a 75 μm thick metal gel line. The insertion loss is increased for both materials from the skin effect.
[0019] [Figure 12] 12A-12D are schematic diagrams showing sealing of a line. FIG. 12A shows a standard parachute line with multiple cords surrounded by a sheath. In FIG. 12B, a metal gel (1) is housed within the sheath with nylon cords. In FIG. 12C, individual inner nylon cords may be coated with metal gel and sealed within an insulator such as thermosetting polyurethane to form multiple conductors within a single parachute line. Alternatively, in FIG. 12D, multiple metal gel conductors (3) may be housed within thermoplastic polyurethane and attached to the outside of the parachute line sheath.
[0020] [Figure 13]Figure 13 is a block diagram of a basic strain sensor using a pair of metal gel wires of length LS. The two wires have a combined resistance RS = RS1 + RS2 = VS / IS, where VS and IS are the DC voltage and current at the Wheatstone bridge sensing ports. The Wheatstone bridge has an output V0 proportional to RS which is fed to an ADC to generate a digital strain data output.
[0021] [Figure 14] 14 is a block diagram showing how a DC current IS can be forced through the strain sensor loop via Ld, while the RF signal is coupled into the loop by Cd and filtered out by C1 and C2. The inductor Ld also prevents the RF signal from being shorted out.
[0022] [Figure 15] Figures 15A-C show three ways to create a controlled impedance transmission line using metal gel. Figure 15A shows a coaxial interconnect with a metal gel center (1) conductor (which may be a coated nylon cord) covered with an insulating encapsulation layer metal gel outer layer (2) for a final outer encapsulation layer. Figure 15B shows two metal gel lines in a "parallel twin" (also called "two-wire") configuration. Figure 15C shows an outer metal gel layer applied to the structure in Figure 15B to allow for a lower impedance that reduces radiation and shields the two lines from electromagnetic interference (EMI). The first configuration (Figure 15A) has an outer conductor made of metal gel (2) formed around an insulating center conductor (1) to create an impedance coaxial transmission line in the range of 30 to 100 ohms. Detailed Description
[0023] In the following detailed description, reference is made to the accompanying drawings that form a part of this application, and in which is shown by way of illustration embodiments that may be practiced. It is to be understood that other embodiments may be utilized and structural or logical changes may be made without departing from the spirit or scope of the present disclosure. Therefore, the following detailed description is not to be taken in a limiting sense, and the scope of the embodiments is defined by the appended claims and their equivalents.
[0024] Unless otherwise stated, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the disclosed subject matter belongs. Definitions of commonly used words in chemical terms can be found in The McGraw-Hill Dictionary of Chemical Terms (1985), The Condensed Chemical Dictionary (1981). Unless otherwise stated, the methods and techniques disclosed herein are generally carried out by conventional methods well known in the art and as described in various general and more specific references cited and described throughout this specification. See, for example, Loudon, Organic Chemistry, 4th ed., New York: Oxford University Press, 2002, pp. 360-361 and 1084-1085; Smith and March, March's Advanced Organic Chemistry: Reactions, Mechanisms, and Structure, 5th ed., Wiley-Interscience, 2001; or Vogel, A Textbook of Practical Organic Chemistry, Including Qualitative Organic Analysis, 4th ed., New York: Longman, 1978.
[0025] Various operations may be described in sequence as multiple separate operations, which may be helpful in understanding the embodiments, however, the order of description should not be construed as implying that these operations are sequential.
[0026] In this description, relative descriptions such as above / below, back / front, and top / bottom may be used. Such descriptions are used for ease of description only and are not intended to limit the application of the disclosed embodiments.
[0027] The terms "coupled" and "connected," along with their derivatives, may be used. It should be understood that these terms are not used as synonyms for each other. Rather, in particular embodiments, "connected" may be used to indicate that two or more elements are in direct physical contact with each other. While "coupled" can mean that two or more elements are in direct physical contact, "coupled" can also mean that two or more elements are not in direct contact with each other, but still co-operate or interact with each other.
[0028] As used herein, singular terms include plural referents unless the context clearly dictates otherwise. Similarly, the word "or" is intended to include "and" unless the context clearly dictates otherwise. Also, as used herein, the term "comprising" means "including." Thus, "comprising A or B" means including A, including B, or including A and B.
[0029] Unless otherwise noted, all quantitative values are approximate, whether or not preceded by words such as "about" or "approximately." The materials, methods, and examples described herein are illustrative only and are not intended to be limiting. Any molecular weight or molecular mass values are approximate and are for illustration only.
[0030] In this description, the term "embodiments" may be used, which may each refer to one or more of the same or different embodiments. Furthermore, the terms "comprising," "including," "having," and the like, when used in reference to embodiments, are synonymous.
[0031] A. Overview Flexible conductors are needed for many applications in electronics. Wearable devices, compliant sensors, flexible displays, soft robotic actuators, and stretchable interconnects all require a conductive medium that can be both repeatedly bent and stretched. Ideally, a flexible conductor should maintain conduction through many cycles of stretching and bending while not offering significant resistance to the movement of the substrate to which it is attached. Ideally, a liquid conductor would be well suited for this task.
[0032] As briefly mentioned above, "liquid" metal conductors typically use eutectic alloys of gallium and tin mixed with indium, which are embedded within microfluidic channels. Typically, these alloys include gallium-indium (usually 75% gallium and 25% indium) and gallium-indium-tin (most commonly 68.5% gallium, 21.5% indium, and 10% tin). Gallium alloy fluids have low viscosity and high surface tension. Although these alloys can be good conductors, there are significant problems that prevent their widespread adoption. For example, the alloys themselves are difficult to process. In addition, microfluidic channels are prone to leaking or breaking irreversibly if the alloy substrate is embedded under fatigue conditions. Finally, the alloys form an oxide layer when exposed to air, which is not electrically conductive and can cause failure at the connection between the flexible wire and the rigid component. Thus, it would be a significant advancement to the art to provide a fluid that was easily processed, protected from oxidation, and had self-healing properties that allowed it to continue functioning even when its substrate began to wear. The present disclosure meets these needs.
[0033] Disclosed herein is a new composite material discovered by the inventors that includes a gallium alloy and a gallium oxide composition, the new composite material including dispersed microstructures formed from the gallium oxide within the bulk gallium alloy. In an embodiment, the microstructures are formed from sheets of gallium oxide formed on the surface of the bulk gallium to induce dispersed microstructures when mixed into the gallium alloy. The alloy binds to a crosslinked nanostructure of oxide ribbons that serves a similar purpose as the polymeric gelling agent in normal water-based gels. The gel is stabilized by using submicron scale particles to create a highly viscous, easily wetted, and leak-resistant Bingham plastic (a fluid that exhibits the properties of a solid until subjected to shear forces). This Bingham plastic can be patterned consistently on many surfaces at room temperature. When patterned, the result is a highly conductive fluid interconnect that does not affect the material properties of the substrate. The gel is fluid at room temperature and has a freezing point of -5°C. The final material can be 2-8×10 depending on the degree of stability required. 5With electrical conductivity on the scale of S / m, and the relative ease of patterning the conductors to thicknesses of 100 μm, the resulting sheet resistance is very low compared to other flexible conductors. The compositions disclosed herein generally form a paste-like material. The gallium oxide cooperates with the gallium alloy fluid to form micro- and nano-structures. These structures can withstand small amounts of force depending on their geometry. By dispersing a large number of irregularly shaped gallium oxide micro- and nano-structures in a large volume of gallium alloy fluid, a new and novel composite fluid can be created with high viscosity and non-Newtonian rheological properties. This fluid behaves similarly to a Bingham plastic and retains its structure until stress is applied. As disclosed herein, the creation and dispersion of these micro- and nano-structures can be achieved by multiple methods. In one embodiment, the creation and dispersion of gallium oxide micro-nanostructures is achieved by coating nano- and / or micro-particles in gallium-indium-tin wrapped gallium oxide and suspending them in a gallium-indium-tin fluid by applying shear through shaking or mixing.
[0034] B. Overview of Some Embodiments Aspects of the present disclosure relate to conductive compositions that utilize the structure provided by gallium oxide, e.g., having a paste-like viscosity, mixed into a eutectic gallium alloy to provide micro- or nano-structures that can alter the bulk material properties of the eutectic gallium alloy. In some embodiments, the conductive compositions can be characterized as conductive shear-thinning gel compositions or materials with Bingham plastic properties. In embodiments, compositions of the present disclosure have a viscosity ranging from about 10,000,000 centipoise to about 40,000,000 centipoise under low shear and a viscosity ranging from about 150 to about 180 centipoise under high shear. For example, under low shear conditions, the composition has a viscosity of about 10,000,000, about 15,000,000, about 20,000,000, about 25,000,000, about 30,000,000, about 45,000,000, or about 40,000,000 centipoise. Under high shear conditions, the composition has a viscosity of about 150, about 155, about 160, 165, about 170, about 175, or about 180 centipoise.
[0035] In an embodiment, a composition according to the present disclosure includes a mixture of a eutectic gallium alloy and gallium oxide, the mixture having a weight percent (wt%) of about 59.9% to about 99.9%, e.g., about 67% to about 90%, of the eutectic gallium alloy and about 0.1% to about 2.0%, e.g., about 0.2 to about 1% of the gallium oxide. For example, compositions according to the present disclosure may have a molecular weight of about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92% , about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, or more, for example about 99.9%, eutectic gallium alloy, and about 0.1%, about 0.2%, about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.8%, about 0.9%, about 1.0%, about 1.1%, about 1.2%, about 1.3%, about 1.4%, about 1.5%, about 1.6%, about 1.7%, about 1.8%, about 1.9%, and about 2.0% gallium oxide.
[0036] In embodiments, the eutectic gallium alloy can include gallium-indium or gallium-indium-tin in any elemental ratio. In some embodiments, the eutectic gallium alloy includes gallium and indium. In some embodiments, the compositions disclosed herein include gallium-indium alloys having a weight percent of about 40% to about 95%, such as about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 95%, about 96%, about 97%, about 98%, about 99%, about 100%, about 101%, about 102%, about 103%, about 104%, about 105%, about 106%, about 107%, about 108%, about 109%, about 110%, about 111%, about 112%, about 113%, about 114%, about 115%, about 116%, about 117%, about 1 3%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, or about 95% gallium.
[0037] In some embodiments, the compositions disclosed herein are gallium-indium alloys having a weight percent of about 5% to about 60%, such as about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 13%, about 14%, about 15%, about 16%, about 17%, about 18%, about 19%, about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, or about 60% indium.
[0038] In some embodiments, the eutectic gallium alloy includes gallium and tin. In some embodiments, the compositions disclosed herein include eutectic gallium alloys that include gallium and tin in a weight percent range of about 0.001% to about 50%, such as about 0.001%, about 0.005%, about 0.01%, about 0.05%, about 0.1%, about 0.2%, about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.8%, about 0.9%, about 1%, about 1.5%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 13%, about 14%, about 15%, about 16%, about 17%, about 18%, about 19%, about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 68%, about 69%, about 70%, about , about 14%, about 15%, about 16%, about 17%, about 18%, about 19%, about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, or about 50% tin.
[0039] In an embodiment, one or more micro- or sub-micron-scale particles are mixed with the gallium alloy and gallium oxide. In an embodiment, these particles are suspended in the eutectic gallium alloy fluid, either coated with eutectic gallium alloy or gallium and sealed in gallium oxide, or uncoated as described above. These particles may range in size from nanometers to micrometers and may be suspended in gallium, gallium-indium alloy, or gallium-indium-tin alloy. The ratio of particles to alloy may be varied to alter fluid properties. In an embodiment, micro- and nano-structures are mixed in the mixture by sonication or other mechanical means. In an embodiment, the composition according to the present disclosure includes suspended colloids of micro- and nano-structures in the gallium alloy / gallium oxide mixture.
[0040] In an embodiment, the composition of the present disclosure further comprises one or more micro- or sub-micron-scale particles dispersed within the mixture. This can be done by suspending the particles within the eutectic gallium alloy fluid, either encapsulated within gallium oxide coated with either eutectic gallium alloy or gallium, or uncoated as previously described. The size of these particles can range from nanometers to micrometers and can be suspended within gallium, gallium-indium alloy, or gallium-indium-tin alloy. The ratio of particles to alloy can be varied to alter the fluid properties. Additionally, auxiliary materials are added to the suspended colloid or gallium alloy paste to enhance or modify its physical, electrical, or thermal properties. Dispersion of micro- and nano-structures within the eutectic gallium alloy can be achieved by sonication or other mechanical means without the addition of particles. In some embodiments, one or more microparticles or submicron particles are present in an amount ranging from about 0.001% to about 40.0%, e.g., about 0.001%, about 0.005%, about 0.01%, about 0.05%, about 0.1%, about 0.2%, about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.8%, about 0.9%, about 1%, about 1.5%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 12%, about 16%, about 18%, about 19%, about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about %, about 11%, about 12%, about 13%, about 14%, about 15%, about 16%, about 17%, about 18%, about 19%, about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, or about 40% by weight of microparticles.
[0041] In embodiments, the particles can be soda glass, silica, borosilicate glass, quartz, copper oxide, silver coated copper, non-oxidized copper, tungsten, supersaturated tin granules, glass, graphite, silver coated copper such as silver coated copper spheres or silver coated copper flakes, copper flakes, or copper spheres, or combinations thereof, or any other material that can be wetted by gallium. In certain embodiments, the one or more microparticles or submicron scale particles are in the shape of spheroids, rods, tubes, flakes, plates, cubes, prisms, pyramidal shapes, cages, and dendrimers. In certain embodiments, the one or more microparticles or submicron scale particles are from about 0.5 microns to about 60 microns, e.g., about 0.5 microns, about 0.6 microns, about 0.7 microns, about 0.8 microns, about 0.9 microns, about 1 micron, about 1.5 microns, about 2 microns, about 3 microns, about 4 microns, about 5 microns, about 6 microns, about 7 microns, about 8 microns, about 9 microns, about 10 microns, about 11 microns, about 12 microns, about 13 microns, about 14 microns, about 15 microns, about 16 microns, about 17 microns, about 18 microns, about 19 microns, about 20 microns, about 21 microns, about 22 microns, about 23 microns, about 24 microns, In the size range of about 25 microns, about 26 microns, about 27 microns, about 28 microns, about 29 microns, about 30 microns, about 31 microns, about 32 microns, about 33 microns, about 34 microns, about 35 microns, about 36 microns, about 37 microns, about 38 microns, about 39 microns, about 40 microns, about 41 microns, about 42 microns, about 43 microns, about 44 microns, about 45 microns, about 46 microns, about 47 microns, about 48 microns, about 49 microns, about 50 microns, about 51 microns, about 52 microns, about 53 microns, about 54 microns, about 55 microns, about 56 microns, about 57 microns, about 58 microns, about 59 microns, or about 60 microns.
[0042] Aspects of the present disclosure further relate to a method of making an electrically conductive shear thinning gel composition. In embodiments, the method comprises intermixing a surface oxide formed on the surface of a gallium alloy fluid with the bulk of the gallium alloy fluid by shear mixing at the interface between the surface oxide and the alloy to induce crosslinked microstructures in the surface oxide, thereby forming an electrically conductive shear thinning gel composition. In embodiments, a suspended colloid of microstructures is formed within the gallium alloy / gallium oxide mixture, for example, as gallium oxide particles and / or gallium oxide sheets.
[0043] In an embodiment, the surface oxide is mixed in a ratio of about 0.1% to about 2.0% (weight percent) gallium oxide to about 59.9% to about 99.9% (weight percent) eutectic gallium alloy. For example, the weight percent of gallium alloy mixed with gallium oxide is about 60%, 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, about 100%, about 101%, about 102%, about 103%, about 104%, about 105%, about 106%, about 107%, about 108%, about 109%, about 110%, about 111%, about 112%, about 113%, about 114%, about 115%, about 116%, about 117%, about 118%, about 119%, about 120%, about 121%, about 122%, about 123%, about 124%, about 125%, about 126%, about 127%, about 128%, about 129%, about 130%, about 131%, about 132%, about 133%, about 134%, about 135%, about 136%, about 137%, about 1 %, about 95%, about 96%, about 97%, about 98%, about 99%, or more, for example about 99.9%, with the weight percentage of gallium oxide being about 0.1%, about 0.2%, about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.8%, about 0.9%, about 1.0%, about 1.1%, about 1.2%, about 1.3%, about 1.4%, about 1.5%, about 1.6%, about 1.7%, about 1.8%, about 1.9%, and about 2.0% gallium oxide. In embodiments, the eutectic gallium alloy can include gallium-indium or gallium-indium-tin in any elemental ratio. In some embodiments, the eutectic gallium alloy includes gallium and indium. In certain embodiments, the weight percentage of gallium in the gallium-indium alloy is from about 40% to about 95%, e.g., about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, about 100%, about 101%, about 102%, about 103%, about 104%, about 105%, about 106%, about 107%, about 108%, about 109%, about 110%, about 111%, about 112%, about 113%, about 114%, about 115%, about 116%, about 117%, about 118%, about 119%, about 120%, about 121%, about 122%, about 123%, about 124%, about 125%, about 126%, about 127%, about 12 about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, or about 95%.In certain embodiments, the weight percentage of indium in the gallium-indium alloy is from about 5% to about 60%, for example, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 13%, about 14%, about 15%, about 16%, about 17%, about 18%, about 19%, about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, about 98%, about 99%, about 100 %, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, or about 60%. In some embodiments, the eutectic gallium alloy comprises gallium, indium, and tin. In certain embodiments, the weight percentage of tin in the gallium-indium-tin alloy is from about 0.001% to about 50%, e.g., about 0.001%, about 0.005%, about 0.01%, about 0.05%, about 0.1%, about 0.2%, about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.8%, about 0.9%, about 1%, about 1.5%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 13%, about 14%, about 15%, about 16%, about 17%, about 18%, about 19%, about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 75%, about 76%, about 77%, about 78%, about 79%, about %, about 13%, about 14%, about 15%, about 16%, about 17%, about 18%, about 19%, about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, or about 50%.
[0044] In an embodiment, one or more microparticles or submicron scale particles are mixed with the gallium alloy and gallium oxide. In some embodiments, one or more microparticles or submicron particles are present in the composition at about 0.001% to about 40.0%, for example, about 0.001%, about 0.005%, about 0.01%, about 0.05%, about 0.1%, about 0.2%, about 0.3%, about 0.4%, about 0.5%, about 0.6%, about 0.7%, about 0.8%, about 0.9%, about 1%, about 1.5%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about The mixture can be combined to provide a wt% of microparticles of about 10%, about 11%, about 12%, about 13%, about 14%, about 15%, about 16%, about 17%, about 18%, about 19%, about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, or about 40%. In embodiments, the particles can be soda glass, silica, borosilicate glass, quartz, copper oxide, silver coated copper, non-oxidized copper, tungsten, supersaturated tin granules, glass, graphite, silver coated copper, such as silver coated copper spheres or silver coated copper flakes, copper flakes, or copper spheres, or combinations thereof, or any other material that can be wetted by gallium. In certain embodiments, the one or more microparticles or submicron scale particles are in the shape of spheroids, rods, tubes, flakes, plates, cubes, prisms, pyramidal shapes, cages, and dendrimers.In certain embodiments, the one or more microparticles or submicron scale particles are from about 0.5 microns to about 60 microns, e.g., about 0.5 microns, about 0.6 microns, about 0.7 microns, about 0.8 microns, about 0.9 microns, about 1 micron, about 1.5 microns, about 2 microns, about 3 microns, about 4 microns, about 5 microns, about 6 microns, about 7 microns, about 8 microns, about 9 microns, about 10 microns, about 11 microns, about 12 microns, about 13 microns, about 14 microns, about 15 microns, about 16 microns, about 17 microns, about 18 microns, about 19 microns, about 20 microns, about 21 microns, about 22 microns, about 23 microns, about 24 microns, In the size range of about 25 microns, about 26 microns, about 27 microns, about 28 microns, about 29 microns, about 30 microns, about 31 microns, about 32 microns, about 33 microns, about 34 microns, about 35 microns, about 36 microns, about 37 microns, about 38 microns, about 39 microns, about 40 microns, about 41 microns, about 42 microns, about 43 microns, about 44 microns, about 45 microns, about 46 microns, about 47 microns, about 48 microns, about 49 microns, about 50 microns, about 51 microns, about 52 microns, about 53 microns, about 54 microns, about 55 microns, about 56 microns, about 57 microns, about 58 microns, about 59 microns, or about 60 microns.
[0045] Aspects of the present disclosure relate to products including compositions of the present disclosure and methods of making such compositions. There is growing interest in incorporating electronics into everyday items, including clothing and fabrics, which are expected to be flexible and stretchable. Soft electronics can be smoothly coupled to the human body, opening up many new applications for wearable devices, medical devices, and conformal robotics or "soft machines" candidates that can interact more safely with humans and delicate objects.
[0046] In some embodiments, the product includes an electronic device. In some embodiments, the product includes a fabric, a plastic film, and / or a membrane. In some embodiments, the composition according to the present disclosure is integrated into a sensor, for example, a sensor used for strain detection and / or shear sensing. As an example, a deformed liquid wire having a composition according to the present disclosure can produce a measurable change in resistance, capacitance, inductance, impedance, or characteristic frequency depending on the geometric properties of the conductor. For example, the composition can be used as a sensor to detect strain and / or shear on any substrate. For example, the composition can be integrated into "geotextiles" used to reinforce road shoulders and embankments. In one such example, a long plastic-coated wire formed from a composition according to the present disclosure could detect slumping in a civil structure, providing early warning of collapse. In another example, the composition according to the present disclosure could be patterned on a parachute sling to provide real-time strain feedback that can be used to control a self-steerable parachute.
[0047] In some embodiments, the product includes a body wear comprising a substrate and one or more elements having a composition according to the present disclosure disposed thereon. In various embodiments, substrates, such as substrates for body gear, are disclosed that can use one or more elements having a composition according to the present disclosure disposed on the substrate and coupled to a surface of the substrate, such as an outer or inner surface facing the substrate. In one embodiment, the composition according to the present disclosure conducts electrical current between various other elements of the garment, such as a power source, such as a battery, and other integrated electronic devices, such as a sensor.
[0048] In some embodiments, the bodywear may include components coupled to the composition of the present disclosure for collecting information and / or processing collected information. For example, the bodywear may include components for monitoring one or more physical conditions of the wearer, such as heart rate, EKG, bodily vital signs such as pulse, temperature, and movement. In some embodiments, the composition of the present disclosure is configured as a pressure sensor.
[0049] Generally, sufficient surface area of the backing must be exposed to provide the desired backing function (e.g., stretch, drape, texture, breathability, moisture transmission, air permeability, and / or wicking). For example, if too little backing is exposed, properties such as moisture transmission and / or air permeability may be compromised disproportionately relative to the percentage of coverage.
[0050] In embodiments, the width of the conductive composition ranges from about 0.1 mm to about 10.0 mm, for example, about 0.1, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, or 10.0 mm (sometimes greater), or any value or range.
[0051] In some embodiments, the amount and / or placement of the conductive composition is selected to reduce cost and produce an aesthetically pleasing material, In embodiments, the thickness of the conductive composition ranges from about 0.05 mm to about 5 mm, e.g., about 0.05, about 0.1, about 0.5, about 1.0, about 1.5, about 2.0, about 2.5, about 3.0, about 3.5, about 4.0, about 4.5, about 5.0 mm, or any value or range, although lesser and greater thicknesses are contemplated.
[0052] According to various embodiments, the substrate may be part of any form of body wear, body gear such as a blanket, tent, rain fly, umbrella, or sunshade, or any material or device. As used herein, body wear includes, but is not limited to, athletic wear such as compression garments, outerwear such as jackets, pants, leggings, shirts, hats, etc., and footwear, etc. that is worn on the body.
[0053] In various embodiments, the amount and / or location of the conductive composition can be disposed on a backing having one or more desired properties or characteristics. For example, the backing can have properties such as breathability, moisture transmission, and / or wicking properties required for bodywear used in both indoor and outdoor applications. In some embodiments, the backing can have other desired attributes such as abrasion resistance, antistatic properties, antimicrobial activity, water repellency, flame resistance, hydrophilicity, hydrophobicity, wind resistance, sun protection, SPF protection, elasticity, stain resistance, wrinkle resistance, etc. In other embodiments, the amount of the conductive composition can be separated to allow the backing to have a desired drape, look, and / or texture. Suitable backings can include nylon, polyester, rayon, cotton, spandex, wool, silk, or blends thereof, or any other material having a desired look, feel, weight, thickness, weave, texture, or other desired properties.
[0054] In various embodiments, a single layer of fabric may be used to construct the fabric, while other embodiments may use a multi-layer fabric that includes a layer of fabric connected to one or more other layers.
[0055] In various embodiments, the arrangement, pattern, and amount of the conductive composition can vary. In various embodiments, the pattern and / or arrangement of the amount of the conductive composition can be symmetric, ordered, random, and / or asymmetric.
[0056] Aspects of the present disclosure further relate to methods of making products having the shear-thinning gel compositions disclosed above, in which the shear-thinning gel composition is printed onto at least one surface of the product.
[0057] In some embodiments, the compositions disclosed herein are printed or transferred to a substrate. In some embodiments, printing includes screen printing. In some cases, printing is done by contact transfer using a 3D printing stamp mold, e.g., a silicone rubber and / or polyurethane rubber stamp. The parameters of the transfer contact are the surface energies of the material to be transferred, the contact pad, and the substrate. Fluids generally wet surfaces with higher energy than their own surface energy, and preferentially wet substrates with even higher energy. Silicone rubber (PDMS) has an unusually low surface energy and is often used as a transfer medium in contact transfer printing. In other embodiments, the compositions disclosed herein are transferred to a substrate by pressing a saturated sponge against a mask to transfer the material. For sponge methods, numerous polyurethane and PDMS foams are available.
[0058] The subject matter of the present disclosure is further illustrated by the following non-limiting examples. Example 1
[0059] Method of forming materials First, they experimented with a commercially available gallium-indium-tin (68.5, 21.5, 10) alloy (Galinstan) and observed that gallium-based alloys form an oxide layer very quickly in air. During the process of injecting liquid metal into the PDMS microfluidic channel, they were able to create a "clean" non-oxidized device by reducing the oxide layer on the sample with hydrochloric acid (HCL) and reducing the waste. During this process, they observed that the sample exhibited strange physical behavior when reduced by HCL. For example, the sample did not form the usual Galinstan, but instead produced a highly viscous material. This material could be obtained in small quantities from a commercially available Galinstan sample.
[0060] The first attempt synthesized a foam-like material from Galinstan by mixing it with 30 micron glass beads. In the presence of oxygen, Galinstan easily wets to glass through its oxide layer. The initial hope was that Galinstan would "wet" onto the glass beads in this way, forming a slurry of Galinstan and glass. This slurry would be highly viscous and easily moldable into any shape.
[0061] It has been previously reported that the only mechanism by which gallium-indium and related alloys wet to any non-metallic surface is through the deposition of an oxide layer and the resulting trapping of fluid beneath that layer. It was hypothesized that gallium-indium-tin wets like beads by a thin layer of fluid metal in direct contact with the glass, which is trapped in place by the oxide layer. Through mixing, the glass beads are repeatedly exposed to the atmosphere, forming successive layers of gallium-indium-tin oxide traps. When these structures are again immersed, it is believed that the shear forces from the mixing cause the destruction of the oxide layer, forming scattering structures, realizing suspended colloids of glass beads, and increasing the viscosity of the fluid.
[0062] The method worked well with micron beads and a variety of other sizes. This led to the discovery that a fine network of connected gallium-oxide structures provided the internal structure of the fluid that absorbed the gallium-indium alloy and increased its viscosity. The increased viscosity made the fluid more easily extrudable and could be reliably formed into conductive geometric configurations using traditional printing techniques such as nozzle deposition and stencil printing. The resulting high-viscosity fluid was variously called gallium-indium gel, gallium-indium alloy gel, metal gel, or simply gel. Example 2
[0063] Additive methods of material formation Gallium oxide microstructures were first produced by sonicating wet gallium-indium-tin on a flat glass surface. Sonication resulted in the formation of microstructures on the gallium-oxide surface. Subsequent sonication and mixing steps mixed these structures into the bulk of the fluid, ultimately resulting in a gel consisting of gallium-indium-tin and approximately .84% oxide. This gel was less likely to separate than the one produced using glass beads, and of course had a much higher bulk conductivity. Interestingly, hydrochloric acid, which is often used to reduce oxides on gallium alloys, reduced only the surface oxides on the gel produced in this way, leaving the internal structure intact. This is in contrast to gels produced using glass beads, which were completely reduced by HCL, resulting in complete separation of the beads from the gel and a drop in viscosity. Example 3
[0064] Additive methods of material formation A third successful example involves using a mixing bar partially immersed in a bath of gallium-indium or gallium-indium-tin and rotating it at very high RPM to generate a vortex. The vortex thus generated creates unstable thin walls of gallium-indium and its oxide layer around the mixing bar, extending several centimetres above the fluid surface. These walls give the vortex a large surface area, which causes a large amount of oxide to sublimate into the fluid. The fluid becomes rapidly viscous, necessitating annular mixing. The resulting fluid is not homogenous, with the lower viscosity gallium-indium alloy pooling at the bottom and a gallium-indium gel floating on the surface, mixed into air bubbles. The gel can be drained by placing it on an inclined surface, then collected and vacuum cycled out into air. The resulting gel is comparable to that produced by sonication. Example 4
[0065] Generation of stamp-transferable compositions Both gallium and indium are expensive. Their electrical conductivity is adequate, but much lower than that of copper or silver (58.5 x 10 6 3.46×10 for S / m 6 It was thought desirable to create a suspension of additives in the gel to increase conductivity while increasing cost. Several additives were tried.
[0066] Both microsphere and flake gels are resistant to displacement when subjected to pressure during sealing with adhesives or thermoplastic welding.
[0067] The innovation was that both flake gel and pure copper filled gel could be stamped. A regular lettering stamp could be coated with gel + additive material and then pressed against a suitable substrate, and the pattern on the stamp would be transferred with high fidelity. Features as small as 0.5 mm could thus be produced with pitches as small as 0.25 mm. Such deposits were very thin, about 25 micrometers. Example 5
[0068] Generation of stamp-transferable compositions Macro-contact printing has been performed but has not been successful so far for other gallium containing fluids. With regard to stamp lithography, attempts have also been made to transfer solid lines and solid rectangles onto elastomeric substrates using both flat and textured stamps, but without success. The transfer method is similar to previous existing approaches, but other groups have not been able to extend this technique to liquid phase gain alloys. For example, Galinstan does not wet the elastomer in some areas and coalesces into droplets in other areas. In the case of textured stamps, the droplets deposited in each recess do not coalesce uniformly. This uneven wetting may result from uneven wetting during "inking," when the stamp is first coated with Galinstan, or from uneven contact pressure during transfer.
[0069] These problems are overcome by the disclosed composition by incorporating low micron and nanoscale particles into the gallium alloy / oxide gel. Without being bound by theory, it is believed that the added particles stick to the oxide structure and do not float freely in the gallium metal. The reinforcing oxide ensures that the oxide breaks into larger chunks, generally trapping the flow in the system. Perhaps more importantly, if the splitting does not occur, the metal flow tends to entrap and transport the added particles + oxide, which inhibits the free flow. In some of the metal particles used, which can form unstable intermetallic compounds, interactions between gallium, indium or tin and silver or copper are also likely to occur, creating even more microstructure in the fluid and inhibiting its free flow.
[0070] Several loading schemes were tried for each additive. All were mechanically mixed into a pre-prepared gel at a constant addition rate. Loadings as high as 54% were tried, but the higher the metal loading, the harder the resulting mixture became, through an unknown process (thought to be the formation of an alloy or intermetallic compound).
[0071] It was found that loadings of silver-coated copper flakes between 10-30% by weight produced composites with a consistency similar to clay that spread into a very uniform flat sheet when deposited with a spatula or brush. Scanning electron microscope (SEM) images showed that the height of the sheet of deposited material was extremely uniform, although not precisely measured (see Figures 1A-1E). Figure 1A shows regular untreated gallium-indium-tin (note that it is blurry because it has a very low viscosity and vibrates from the impact of the electron beam). Figure 1B shows a stable flake gel on the micron scale (image width is 500 microns), Figure 1C shows an unstable gel (90 microns wide), Figure 1D shows an unstable gel formed into a standing shape, indicating its semi-solid nature (75 microns wide), and Figure 1E shows an unstable gel (field of view 250 microns).
[0072] When the sheet is sealed, it becomes fluid and spreads and reforms due to the forces of the sealing channels. Copper microspheres or flakes loaded 10-30% by weight produce a more viscous fluid, becoming somewhat solid and brittle near the higher end of the loading range.
[0073] To test compressibility, the new formulations were pressed between layers of “rescue tape,” a commercially available adhesive PDMS substrate, to confirm uniformity of flow upon compression.
[0074] Figures 2A and 2B show a failed (Figure 2A, 2B) and a successful (Figure 2C) compression test example side-by-side. Note that "sprue" erupted major portions of the failed compression examples. These are caused by unrestricted flow of gallium metal moving separately from the composite system. In contrast, the loaded particle additive in the successful tests forces the system to flow together and spreads evenly during compression. This is highly desirable for sealing the conductive gel using established industrial techniques such as heat welding a plastic film around the deposited pattern. During these compression tests, very high fidelity pattern transfer between the substrates upon peeling was observed (see Figure 3).
[0075] To further test the potential contact printing method, a stamp with "Celtic knot" patterning technology was used with various trace widths, pitches, and patterns. Figures 4A-4D show that initial trials with the stamp gave good results, producing patterns with trace widths as small as 0.5 mm and pitches as small as 0.25 mm.
[0076] The transfer process was highly dependent on how much metal gel was initially loaded into the stamp, how flat the substrate and stamp were, and how much pressure was applied.
[0077] Using these techniques, useful devices can be fabricated by stamp transfer. Figure 5 shows the encapsulation stamp with attached leads. This configuration acts as a pressure sensor. When pressure is applied, the pattern distorts and compresses, changing the measured resistance. Using a high fidelity transfer printing process and customized trace patterns, this could be made into a very cheap and very useful pressure sensor. The total manual assembly time was about 1 minute, including lead attachment and potting. This fabrication process is highly scalable, allowing for the rapid patterning of any trace geometry in two dimensions. Example 6
[0078] Strain detection using eutectic metal gel The disclosed formulations allow for the detection of large scale strains and deformations by using eutectic metal-gel composites that can be printed on various substrates similar to inks or paints to create conductive traces. The disclosed materials are amorphous room temperature fluids and can be deformed and stretched without fatigue. Thin traces placed on a plastic fabric liner can bend and stretch without affecting the tactile feel of the fabric. Encapsulating such traces with a second layer of fabric liner creates a sealed conductive path. These applications have already been shown for use in strain sensors and non-sensing thin stretchable wires for smart sports clothing.
[0079] The amorphous metallic structure of the disclosed material allows for sensing of linear resistance changes when stretched or otherwise deformed, as shown in Figure 6. When patterned on a parachute sling and integrated with a Wheatstone bridge and analog-to-digital converter, the resistance changes can be used to measure dynamic forces and strains during parachute deployment.
[0080] A piece of metal gel wire serves as a variable conductor whose dispersion value is a function of the strain parallel to the conductor. This allows the creation of many strain sensing patterns with various resolutions. In the simplest case, two traces could be patterned on each gore on the parachute, one running in the weft direction and the other in the warp direction (see Figure 7). By measuring the change in conductivity of both, a strain profile can be obtained for each individual parachute gore. With the correct patterning, some parts of the trace can have extremely large linear resistance changes in response to strain. For example, a zigzag pattern shows extremely large resistance changes when strained in an axis perpendicular to the path of the trace. Using this feature, multiple traces could be created to obtain strain information by appropriate patterning over the area of interest. This increases the resolution of the strain sensing across the gore, allowing the complete strain map to be estimated.
[0081] Extremely high resolution can be achieved by creating a mesh of interconnected metal gel traces. Each piece of this mesh is a variable resistor that depends on strain in either the weft or warp direction, depending on its orientation. Every unique pairing of output elements produces a six-element vector. By appropriately weighting the resistance range of each variable resistor, it is possible to ensure that the output vector uniquely encodes each possible combination of resistance values to any fidelity (see, for example, Figure 8).
[0082] Solving the resistance of a mesh of connected variable resistors based on a finite i / o vector is a well-known problem that is frequently encountered in the field of VLSI design and verification. Using the previously developed methodology, we can develop a mapping of resistance vs. i / o vector resistance that allows us to quickly and effectively measure the strain at each part of the parachute canopy surface traversed by a conductive gel strip. With this method, we have been able to obtain a resolution better than 1 cm2.
[0083] Data Acquisition
[0084] Since the metal gel does indeed act as a metal, electrical signals can be transmitted via wired connections formed from metal gel traces extending from the slings, or via broadcast. Each gore could be sewn into a small embedded system that reads the resistance and puts these into a standard broadcast format. These signals could be fed to a metal gel antenna printed on the canopy surface (see Figure 9). The antenna is stretchable, changing its operating frequency, but such changes are linear and can be matched. A low-resolution distortion map of the canopy surface could also be obtained, with the antenna pattern transmitting a unique ID. Data transfer and distortion detection via RF signals is possible, but not proposed in the Phase I proposal.
[0085] In any of the above methods, the strain can be measured directly on the canopy surface without the need for external illumination sources, remote sensing, etc. This not only allows for high-resolution measurements of the strain field without the computational overhead of image processing, but also allows for a field-deployable system that is less sensitive to varying light levels, adverse weather conditions, and payload / canopy misalignment.
[0086] Validation of current metal gel patterning and sealing methods for parachute canopy fabrics
[0087] The purpose is to adhere to the nylon material of the parachute canopy. It is not believed that the thin TPU traces or silicone adhesive will have a detrimental effect on the underlying material. However, tensile strength and fatigue testing will be performed to ensure there are no detrimental effects. An evaluation will be performed to apply a silicone based adhesive such as Dow Corning 7091 directly to the parachute fabric, then pattern a metal gel on the cured sealant, and adhere the TPU sealant metal gel traces to the canopy fabric.
[0088] Characterization of metal gel traces on parachute canopy fabrics
[0089] Strain testing of sealed metal gel traces against parachute fabric is performed to measure the strain-resistance feedback relationship in the weft and warp directions. Various standard trace patterns in the weft and warp directions are measured over the desired strain range of .2-25%. The characterized eutectic metal gel variable resistance values are used.
[0090] Using the output of feature analysis to model two-dimensional variable resistive strain sensing
[0091] Using commercially available simulation tools such as MatLab and LabView, several 2D strain gauge topologies are modeled. Of particular interest are variable resistor mesh networks. By simulating these networks with real values obtained as described below, a mapping of a high-dimensional surface network of connected linear variable resistors to an output vector that can take on values in a continuous range is generated. Such mappings are stored in a look-up table that can be used to analyze the variable resistor network output in larger scale experiments.
[0092] Characterizing small-scale parachutes using variable resistance topology in wind tunnels
[0093] A small-scale parachute, less than 3 feet long with a single gore, will be patterned using two eutectic metal gel strain sensors, one for the weft direction and one for the warp direction. The system will be deployed in a wind tunnel and the results will be characterized.
[0094] Repeated wind tunnel testing with improved sensor resolution
[0095] Increasingly higher resolution sensing networks on a simple parachute are constructed, tested, and verified using previous tests. Data from the strain sensor canopy is used to verify the output data from the four sensor test, which is then used to verify data from progressively more complex and higher resolution patterns.
[0096] Examining current metal gel patterning and sealing techniques for parachute canopy fabrics
[0097] A variable resistance trace is prepared on the inside of a TPU membrane. These membranes are attached to a 1' x 3" swatch of parachute canopy material. A silicone adhesive, such as Dow Corning 7091 adhesive / encapsulant, is then applied directly to the parachute canopy, a metal gel is patterned on the adhesive, and a second encapsulation layer is placed. The result of this task is the best possible means of depositing the metal gel onto the parachute canopy material.
[0098] Characterization of metal gel traces on parachute canopy fabrics
[0099] The above prepared swatches are fatigued in an Instron 3365 for 350 cycles and strained to failure. Results are compared to a control swatch of canopy fabric without the metal gel trace to ensure that there is no adverse effect on the canopy fabric. The results of these tests are used to perform a deeper characterization of the strain / resistance relationship for different trace geometric configurations. With the integral metal gel trace, strain ε = ΔL S / L S Normalized resistance change ΔR S / R S By measuring L in both the weft and warp directions, S = Gauge factor (GF) for a 0.5 meter canopy fabric swatch Characterize JPEG0007551050000001.jpg1428.
[0100] To obtain the data for calculating GF, a swatch of the canopy material with an integral strain sensing trace was mounted on an Instron 3365 test fixture equipped with a 2kN load cell and LVDT to measure the displacement ΔL. S Quasi-static strain tests are performed from 0 to 20% strain in 0.25% increments. Dynamic strain tests are performed over the range 0-20% for 350 cycles on each specimen. Displacement data is collected in Labview for all tests.
[0101] A Wheatstone bridge is used to generate an analog output voltage V0 that is a function of the resistance change at the input, ΔRS is measured. In this application, the input “strain” resistor has a length L S The two metal gel wires form a resistor R S1 and R S2 If R S =V S / I S These two wires represent the two conductors in the strain sensing topology shown in Figures 10A-10D. The analog output voltage V0 is converted to digital data using a National Instruments ADC (analog-to-digital converter) for analysis in Labview, where it is represented as R S The ADC has a target spatial resolution sufficient to detect 0.25% voltage change at a sampling rate of 1000Hz. The nominal zero distortion resistance R S0 Resistance change rate ΔR S divided by the strain ε gives GF. In fact, this system can be attached to a microcontroller to dynamically view the strain during parachute deployment in real time. During this task, multiple conductive patterns are tested in the latitudinal and longitudinal directions. These patterns contain trace widths from 1 to 4 mm in .5 mm increments in various geometric configurations.
[0102] Construction of gauge factor model for simulation
[0103] Using the measured GF, a simulation model is generated in either MatLab or LabView. The model consists of a list of variable resistors with strain percentage as input and resistance change appropriate to the metal gel pattern as output. This list of known characterized metal gel traces is used below.
[0104] Modeling Multiple 2-D Variable Resistor Strain Sensing
[0105] Circuit simulations are created for various variable resistor topologies using MatLab or Labview. With the generated list of variable resistor models, accurate simulation of the distortion of the canopy fabric can be performed by varying the values on the simulated variable resistor network. These simulations can be used to design and test new topologies to achieve high resolution designs. Of particular note are variable resistor grid patterns, which are easy to fabricate with high density of distortion sensors. However, this does not exclude other unconnected or sparsely connected variable resistor networks for high resolution sensing. The result of this task is a set of modeling patterns that can be formed on the canopy system specimen.
[0106] Characterizing small-scale parachutes using variable resistance topology in wind tunnels
[0107] A small parachute is purchased and two metal gel traces are attached to one gore, one in the latitudinal direction and one in the longitudinal direction. These traces are wired to a Wheatstone bridge to an ADC circuit attached to a computer running LabView to record the strain results in real time. The assembly is then placed in the tunnel. Real-time data is acquired as the parachute deploys in the wind tunnel.
[0108] Repeated wind tunnel testing with improved sensor resolution
[0109] Using the data collected above for validation, two additional patterns with higher resolution are tested. These patterns are based on simulations and serve to validate the model. One pattern is expected to be a grid of variable resistance with output vectors as described in Figure 8. The other pattern is an unconnected network of trace geometries across the parachute surface that increases the output providing higher resolution by having independent latitudinal and longitudinal traces across multiple portions of the canopy surface with dedicated i / o lines so that deciphering the distortion feedback is trivial. Example 7
[0110] Application of nylon fiber to parachute sling cord The eutectic metal gel can be applied directly to nylon fiber parachute sling cord at room temperature without the need for intermediate chemical processing. A flexible, stretchable binder, such as a two-part polyurethane resin or silicone elastomer, can be used to permanently seal the gel to the nylon cord, preventing displacement during normal handling and packing of the parachute sling and control line system. This process is not believed to alter the ultimate tensile strength and flexibility of the parachute line.
[0111] Importantly, the amorphous metal structure of the disclosed composition ensures that when stretched or otherwise deformed, it produces linear and repeatable resistance changes that can be used for sensing. When patterned onto standard parachute cord such as PIA-C-5040 and integrated into a Wheatstone bridge using an analog-to-digital converter, these linear and repeatable resistance changes can be used to measure dynamic forces and strains during parachute deployment.
[0112] Tests were conducted to demonstrate the feasibility of coating the inner cord from a MIL-C-5040H parachute line. The metallic gel provided good wetting with nylon, producing a low resistance trace with negligible weight increase.
[0113] The resistance of liquid wire conductors can be set by adjusting thickness and width to the order of 1 to 100 ohms per meter. This resistance is high enough to give a good signal to noise ratio in a Wheatstone bridge, making it ideal for applications that require measuring resistance versus elongation. Making the resistance higher, as for CNT-based conductive coatings, results in very small currents that are easily corrupted by electromagnetic interference (EMI). Similarly, copper has a low resistance, so the voltage drop over a few meters of line is too small to be practical, and there are EMI issues as well. Typical resistances for a 6-foot-long MIL-C-5040H control line coated with metallic gel are 2 to 20 ohms, depending on the deposition thickness.
[0114] A typical conductivity change can be seen in Figure 6, which shows the strain response for a metal gel wire encapsulated in silicone rubber. The samples were tested using an adjustable jig that could be stretched in 1.5 mm increments and an ESR meter that accurately measured the sub-1 ohm resistance of the sample during quasi-static strain testing.
[0115] Metal gel conductors are not as conductive as copper, but are still effective for transmitting high speed data. Tests on flat traces for clothing applications have shown that the material is suitable for transmitting signals up to 6 GHz and above, allowing the interconnects to be directly integrated into general purpose radio frequency or microwave frequency transmission systems. Figure 11 shows the measured insertion loss for a 50 ohm microstrip line made from copper and metal gel. Other organic conductor solutions have resistances of several kiloohms, making them impractical for sending RF signals over distances of more than a few inches.
[0116] Testing metal gel gauge factor for strain sensing
[0117] The gauge factor (GF) of a 0.5 meter nylon cord with an integral metal gel trace is characterized for axial strain sensing by measuring the normalized resistance change (ΔR / R) with respect to strain (ΔL / L).
[0118] RF Signal Transmission Capability
[0119] The goal of this exercise is to test different types of transmission lines formed from metal gel to characterize their RF signal transmission capabilities. This includes controlling the transmission line characteristic impedance. The transmission lines are designed to fit standard parachute line cord form factors.
[0120] Electromagnetic interference (EMI) shielding
[0121] To prevent EMI from being radiated by the metal gel line (radiated emissions) or received by it (radiated susceptibility), it will probably be necessary to use some sort of conductive shield. This shield will completely or perhaps only partially surround the metal gel line. The purpose is to test the feasibility of using a carbon black filled polyurethane or silicone, or a metal gel, as a shielding layer formed on an insulator coating the inner conductor or a conductor formed from metal gel.
[0122] The effect of eutectic metal gels and seals on sling line durability.
[0123] The parachute line must have flexibility and durability that are not substantially altered by the addition of the eutectic metal gel. The ultimate tensile strength of the coated line is measured and compared to that of the uncoated one. Similarly, the conductive metal gel coating must be able to withstand the same requirements of flexibility and durability imposed on the sling line. For this purpose, the dynamic strain feedback is tested by repeatedly straining the line for 350 cycles. The objective is to avoid the development of defects in the conductor or any part of the parachute sling line.
[0124] Application of Metal Gel to PIA-C-5040 Parachute Line
[0125] In this task, known forming methods used for flat surfaces such as those found in clothing fabrics are applied and modified as necessary to the cylindrical surface of the nylon inner cord from the parachute sling line. This is followed by sealing of the coated cord with both silicone and two-part polyurethane. In addition, known methods of sealing metal gels in TPU membranes are used to create large, extremely flexible and stretchable, low-profile strain sensors that can be attached to the exterior of the nylon control line or between the parachute sling line and the core and sleeve cords of the control line. This approach also has the added advantage of being applicable to parachute canopy materials, since the same low-profile TPU sealing interconnects can be attached to the control line and canopy. Some of the possible methods are shown in Figures 12A-12D. In evaluating the methods, a total of four types of strain-sensing parachute lines are considered to be created. one with all eight inner cords unsealed and sealed with a sheath (Figure 12B), one with two polyurethane sealed metal gel coated nylon inner cords providing the output and return signal lines (Figure 12C), a similar configuration sealed in silicone rubber, and one with a separate TPU sensing ribbon running the length of the parachute line (Figure 12D). Multiple lines of each type may be made to facilitate testing.
[0126] Tensile Strength and Strain Range Test
[0127] The PIA-C-5040 parachute line with integral strain sensing traces is mounted on an Instron 3364 testing machine equipped with a 5kN load cell and strained to its breaking point. The tests are compared to a stock parachute line without the integral strain sensing traces. The linear range of strain feedback from the conductive traces is evaluated over all extensions from 0% to breaking (expected to be 30%). Data is generated on the effect of this method on the ultimate tensile strength of the parachute line.
[0128] Metal gel gauge factor for strain sensing
[0129] The goal of this task is to find the strain ε = ΔL S / L S Normalized resistance change ΔR S / R S By measuring the L S = Gauge factor GF for 0.5 meter nylon cord The aim is to characterize JPEG0007551050000002.jpg1222.
[0130] To obtain the data for calculating GF, an Instron 3385 test machine equipped with a 2kN load cell and LVDT was fitted with a parachute line with an integral strain sensing trace to measure the displacement ΔL. S The resistance change ΔR is measured using a Wheatstone bridge which generates an analog output voltage V0, which is a function of the resistance change at the input. S In this application, the input “strain” resistor has a length L S The two metal gel wires form a resistor R S1 and R S2 13, R S =V S / I SThese two wires represent the two conductors in the strain sensing topology shown in Figures 12C and 12D. The analog output voltage V0 is converted to digital data using a National Instruments ADC (analog-to-digital converter) for analysis in Labview, where it is represented as R S The ADC has a target spatial resolution sufficient to detect 0.25% voltage change at a sampling rate of 1000Hz. The nominal zero distortion resistance R S0 Resistance change rate ΔR S Dividing by the strain ε gives GF. In fact, by attaching this system to a microcontroller, we can dynamically view the strain during parachute deployment in real time.
[0131] RF signal propagation capability
[0132] In this task, the transmission of an RF signal along a metal-gel strain sensing line is demonstrated. In Figure 11, preliminary data shows that above 6 GHz the insertion loss of an RF signal in a microstrip line made from metal-gel is not much worse than that of copper. This finding is extended to design a transmission line structure that fits the standard parachute line form factor. To be able to transmit an RF signal along the metal-gel strain sensing wire, a system as shown in Figure 14 is constructed. This is done by feeding a direct current I S A diplexer is added to pass R S1 and R S2 In order to be able to measure the inductor L d A capacitor C dThe block diagram of FIG. 3 is similar to that of FIG. 3, except that the inductor acts as a DC block and allows an RF signal to enter the loop from the RF data source shown. The inductor prevents the RF signal from shorting out, and at the far end of the loop the RF signal exits the loop through capacitors C1 and C2. To transmit the RF signal along the interconnect system, it is desirable to control the characteristic impedance. To control the impedance, it is possible to evaluate interconnection schemes such as those shown in FIG. 15A-15C. The second structure (B) uses a pair of adjacent conductors (3) to create a "parallel bilinear" interconnect with an impedance on the order of 100 to 300 ohms. The exact impedance is a function of the metal gel dimensions, the spacing of the lines, and the dielectric constant of the encapsulation material. The third structure (C) is similar to (B), except that an outer shield (4) is added to lower the impedance value and reduce radiation and EMI. The test structure is simulated and measured to characterize its insertion loss and characteristic impedance over frequency. Simulation results and completed transmission line structures are the outcome of this task.
[0133] EMI shielding
[0134] A proof of concept transmission line or lines will be fabricated by covering the signal lines with a rubber jacket containing conductive material to provide EMI shielding as shown in Figure 15A and Figure 15C. The feasibility of using carbon black filled polyurethane or silicone will be tested with a shielding layer consisting of a metal gel formed on an insulating seal coating an inner layer of sensing / transmitting gel. Simulations will be performed using a 3D electromagnetic simulator such as ANSYS HFSS to model the behavior. Data from the simulation and a prototype line will be the outcome of this task.
[0135] Embedded Systems Design
[0136] Design and build a prototype embedded system to read the variable resistance values and convert these to strain percentages that can be sent via SPI or I2C for processing elsewhere. A Wheatstone bridge designed to generate a variable voltage ranging from 250mV to 2500mV will be integrated onto a board with a 12-bit ADC, a low-power microcontroller, and a power supply. Designing and building the prototype board does not involve unknown science or new engineering and will require approximately two months of time depending on working with an assembler. Programming the embedded system is expected to take another month. The raw voltage values from the Wheatstone bridge, read through the ADC, will need to be converted to strain percentages based on the experiments done in task 3 that will give the approximate GF. A more uncertain goal is the package design that will firmly bond the metal gel conductors to the contacts on the board. The conductive lines running the length of the parachute cord need to contact solid metal so that the metal gel traces are sealed to prevent displacement or contamination of the metal gel. The most successful packaging method is to bond brass wires to the variable resistor transmission line at the termination, encapsulate the connection points with potting compound, and then solder the wires to terminals on the PCB. We believe that by using wires of sufficient length with some slack and stitching them into ripstop fabric at the parachute sling line termination, we can limit enough strain from the connection points to operate through multiple deployments. The completed system can be verified by mounting the parachute line in an Instron 3364 and subjecting the line to precise, known strains while reading data from the embedded system. The outcome of this task is a completed prototype of the parachute sling line with strain-sensing metal gel attached to an embedded system that can generate data in the form of strain percentages through either the SPI or I2C data lines.
[0137] EMI shield prototyping and testing
[0138] We physically test prototype lines consisting of shielding layers of either metal gel or carbon black impregnated elastomer, and a sense / transmit gel to create a coaxial cable or a shielded twin line as shown in Figures 15A and 15C, respectively. We test both systems as transmission lines and test their radiated emissions using an anechoic chamber.
Claims
1. A stretchable substrate; a stretchable conductor disposed on the stretchable substrate; and an encapsulant material, the stretchable conductor comprises a metal gel composition; The metal gel composition comprises: (a) a eutectic gallium alloy and a quantity of gallium oxide distributed within a bulk of the eutectic gallium alloy, the bulk mixture of the eutectic gallium alloy and the gallium oxide having between 59.9% and 99.9% by weight (wt%) of the eutectic gallium alloy; (b) the metal gel composition is stabilized by the gallium oxide microstructure; the encapsulation material is configured to encapsulate the stretchable conductor with the stretchable substrate; The metal gel composition has electrical characteristics that have a substantially linear response that is linear within a margin of ±1.5% when the metal gel composition is stretched.
2. further comprising a circuit operably coupled to the stretchable conductor; The electronic system of claim 1 , wherein the circuitry is configured to determine the electrical characteristic and to output a signal based on the electrical characteristic.
3. The electronic system of claim 1 , wherein the electrical property is resistance.
4. 2. The electronic system of claim 1, wherein the electrical characteristic is one of resistance, impedance, capacitance, inductance, or frequency.
5. The electronic system of claim 1 , wherein the metal gel composition is printed onto the stretchable substrate.
6. The electronic system of claim 5 , wherein the metal gel composition is printed onto a surface of the stretchable substrate.
7. 3. The electronic system of claim 2, wherein the circuitry includes an analog-to-digital converter configured to output the signal.
8. the stretchable conductor forms a sensor; The electronic system of claim 1 , wherein the electrical characteristic is indicative of an output of the sensor.
9. The electronic system of claim 8 , wherein the sensor is one of a strain sensor, a pressure sensor, a shear sensor, a deformation sensor, or a compression sensor.
10. 1. A method of manufacturing an electronic system, comprising: disposing a stretchable conductor on a stretchable substrate; applying an encapsulant to encapsulate the stretchable conductor with the stretchable substrate; the stretchable conductor comprises a metal gel composition; The metal gel composition comprises: (a) the metal gel composition has electrical properties when stretched that have a substantially linear response that is linear within a margin of ±1.5%; (b) a eutectic gallium alloy and a quantity of gallium oxide distributed within a bulk of the eutectic gallium alloy, the bulk mixture of the eutectic gallium alloy and the gallium oxide having between 59.9% and 99.9% by weight percent (wt %) of the eutectic gallium alloy.
11. operably coupling a circuit to the stretchable conductor; The method of claim 10 , wherein the circuitry is configured to determine the electrical characteristic and to output a signal based on the electrical characteristic.
12. The method of claim 10 , wherein the electrical property is resistance.
13. The method of claim 10, wherein the electrical property is one of resistance, impedance, capacitance, inductance and frequency.
14. 11. The method of claim 10, wherein disposing the metal gel composition is accomplished by printing the metal gel composition onto the stretchable substrate.
15. 15. The method of claim 14, wherein the metal gel composition is printed onto a surface of the stretchable substrate.
16. The method of claim 11 , wherein the circuitry includes an analog-to-digital converter configured to output the signal.
17. the stretchable conductor forms a sensor; The method of claim 10 , wherein the electrical characteristic is indicative of an output of the sensor.
18. The method of claim 17 , wherein the sensor is one of a strain sensor, a pressure sensor, a shear sensor, a deformation sensor, or a compression sensor.
Citation Information
Patent Citations
Liquid metal paste
EP2058081A2
Flexible strain gage
JP1988225103A
Artificial skin and elastic strain sensor
JP2014528079A
Strain sensor
US20100132476A1