Method for preparing polyester polymers and polyester polymers obtained thereby

The ring-opening polymerization of cyclic polyester oligomers with furan units using plasticizers and zeolites addresses thermal degradation and impurity issues, facilitating efficient production of high-purity polyester polymers.

JP7551698B2Active Publication Date: 2024-09-17SULZER MANAGEMENT AG
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022106024
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-04-21
Filing Date
2022-06-30
Publication Date
2024-09-17
Estimated Expiration
2037-09-27

AI Technical Summary

Technical Problem

Existing methods for producing polyester polymers from cyclic polyester oligomers with furan units face challenges such as high melting points leading to thermal degradation, the need for complex and costly devolatilization equipment, and the presence of impurities that affect storage stability and polymerization behavior.

Method used

A method involving ring-opening polymerization of cyclic polyester oligomers in the presence of a plasticizer, combined with the use of zeolites for impurity removal and controlled reaction conditions, to lower melting points and improve polymerization efficiency.

Benefits of technology

This approach allows for the production of high-purity polyester polymers with reduced thermal degradation and improved molecular weight, enabling efficient and scalable polymerization processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007551698000049
    Figure 0007551698000049
  • Figure 0007551698000044
    Figure 0007551698000044
  • Figure 0007551698000052
    Figure 0007551698000052
Patent Text Reader

Abstract

A method for producing a polyester polymer by polymerizing a cyclic polyester oligomer composition comprising a cyclic polyester oligomer having furan units in the presence of a plasticizer, and the resulting polyester polymer are provided. [Solution] A composition containing (i) a plasticizer selected from the group consisting of optionally substituted phenyl ethers, ionic liquids, optionally substituted xylenes, polyethers, and mixtures thereof, (ii) a cyclic polyester oligomer having furan units, and (iii) either polyethylene furandicarboxylate or polytetramethylene furandicarboxylate.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a process for preparing polyester polymers from cyclic polyester oligomer compositions comprising cyclic polyester oligomers having furan units, and to the polymers obtained thereby. [Background technology]

[0002] Bio-based polymers with aromatic components are highly sought after today due to their environmental friendliness and good mechanical properties. A class of bio-based aromatic monomers that has attracted interest are furan-based compounds, such as furan-2,5-dicarboxylic acid (FDA), 5-(hydroxymethyl)furan-2-carboxylic acid (HMFA) and 2,5-bis(hydroxylmethyl)furan (BHMF), which can be prepared from intermediates such as furfural (2-furancarboxaldehyde) and 5-hydroxymethyl-2-furancarboxaldehyde (HMF), which can be produced by acid-catalyzed thermal dehydration of pentoses (C5) and hexoses (C6). The chemical similarity of the furan ring to the phenyl ring allows the replacement of phenyl-based polymers, such as polyethylene terephthalate (PET), with furan-based polymers.

[0003] The production of polyesters from furan components by polycondensation reaction involving heating a mixture of diols and diacids or diesters (monomers) at high temperatures in the presence of organometallic or acid catalysts is known, for example, from U.S. Pat. No. 2,551,731 and U.S. Pat. No. 8,143,355 B2. To drive this equilibrium reaction to polymer formation, the water or by-products formed, such as alcohols, must be removed, typically by reducing the pressure or gas flow at elevated temperatures during the process. Thus, complex and costly reaction and devolatilization equipment is required. As a result, if polycondensation and devolatilization are insufficient, high molecular weight polyesters with useful mechanical and other properties will not be produced. Moreover, high temperatures and long residence times often result in undesirable side reactions, such as degradation of monomers, oligomers or polymers, formation of intermolecular bonds that cause branching, and oxidation of the final product, resulting in color development.

[0004] Recently, new alternative raw materials have been developed to replace the diol and diacid or diester monomers traditionally used to prepare polyesters from furan building blocks in industrial-scale polymerization plants. WO 2014 / 139603(A1) discloses that cyclic polyester oligomers can be easily prepared by a process that includes reacting monomer components in a ring-closing oligomerization step under conditions of reaction temperature and reaction time sufficient to obtain cyclic polyester oligomers having furan units. Such cyclic polyester oligomers, as disclosed in WO 2014 / 139602A1, advantageously do not produce large amounts of water or alcohol by-products, and do not require complex reactions, equipment with high devolatilization capacity, or vigorous high-temperature reaction and devolatilization steps to drive the polymerization to completion.

[0005] Nevertheless, it was reported that in the cyclic polyester oligomers of WO 2014 / 139603 A1, there are low levels of diacid, diol and acidol monomers and / or dimers and / or oligomer species at equilibrium, which should be removed and may adversely affect the storage stability of the oligomers or the behavior of subsequent polymerization processes. It was disclosed that these undesirable impurities can be removed from the oligomer products by conventional methods, such as chromatography, selective precipitation, distillation, extraction and crystallization, as well as combinations of filtration and chromatography as taught in the examples. Although such purification methods are effective, it is nevertheless desirable to have methods that are as effective, and preferably more effective and selective, and that do not require large amounts of solvents, long times or complex combinations, especially in large-scale commercial production.

[0006] Although the production of polyester polymers from such cyclic oligomers by melt polymerization has been shown to be possible under milder thermal conditions (minimizing color and degradation) and with simpler equipment than the polycondensation reaction in WO 2014 / 139602 A1, some of the cyclic oligomer species nevertheless have very high melting points. For example, the predominant cyclic dimer often has a melting point of about 370° C. Thus, while such oligomer compositions can be readily polymerized at milder temperatures below 300° C., significantly higher temperatures and more aggressive conditions may be required to melt the raw materials prior to their polymerization, which may cause degradation and discoloration of some heat-sensitive aliphatic oligomers.

[0007] Consequently, it would be desirable to have improved methods for both producing such cyclic polyester oligomers as well as for polymerizing them. Summary of the Invention [Problem to be solved by the invention]

[0008] Starting from this state of the art, it is an object of the present invention to provide an improved process for the preparation of polyester polymers having furan units from cyclic polyester oligomer compositions comprising cyclic polyester oligomers having furan units, which process does not suffer from the above-mentioned drawbacks.A related object of the present invention is to provide an improved process for the preparation of such cyclic polyester oligomer compositions.

[0009] The first object is achieved by a method for preparing a polyester polymer comprising the ring-opening polymerization of a cyclic oligomer composition comprising a cyclic polyester oligomer having furan units, the ring-opening polymerization being carried out in the presence of a plasticizer. [Means for solving the problem]

[0010] In the present invention, "furan units" refers to furan derivatives, such as those based on the monomers FDA, HMFA, BHMF, and their partially or fully reacted monoester or diester derivatives. The presence of furan units means that fully or partially reacted derivatives of such monomers are incorporated into the polyester polymer or cyclic polyester oligomer.

[0011] According to the invention, a plasticizer is a compound capable of lowering the melting point and / or the viscosity of a cyclic polyester oligomer, preferably a cyclic dimer, having furan units.

[0012] The presence of a plasticizer has several beneficial effects. First, some of the cyclic species, such as cyclic dimers, have very high melting points, which are effectively lowered in the presence of a plasticizer. Thus, most cyclic oligomer compositions do not melt at the preferred temperatures below 300C, above which thermal degradation of both the oligomer and its polymeric product leads to significant coloration and reduction in the achieved molecular weight of the polymeric product. As a result, the plasticizer advantageously minimizes the thermal profile (temperature and / or time) of the reactant cyclic oligomer composition during the initial complete melting and any holding of the composition prior to melt polymerization. Furthermore, the plasticizer promotes polymerization of the cyclic oligomer composition at temperatures well below its melting point, and therefore under milder conditions.

[0013] Furthermore, many of the desirable polymerization catalysts are solids rather than liquids. Examples include cyclic stannoxanes, which readily yield high molecular weight polymers for commercial use, and metal oxides, such as Sb2O3 and Bi2O3, which yield polymer products with reduced color relative to those obtained with tin-based catalysts. Inert plasticizers facilitate polymerization by promoting intimate contact and mixing between the cyclic oligomer composition and these solid-state polymerization catalysts.

[0014] In a preferred embodiment, the amount of plasticizer during polymerization is sufficient to reduce the melting point of the initial unreacted cyclic oligomer composition by at least 10, preferably 25, more preferably 50, and most preferably about 75° C. In a preferred embodiment, the amount of plasticizer during polymerization is sufficient to reduce the initial melt viscosity of the reaction mixture containing the cyclic oligomer composition by at least 10, preferably 25, and more preferably 50%. In certain other preferred embodiments, the amount of plasticizer is 1 to 75, preferably 5 to 60, more preferably 10 to 50, and most preferably 15 to 40% by weight based on the weight of the initial cyclic polyester oligomer composition. Melt viscosity can be measured using a rheometer according to methods commonly known in the art.

[0015] In a specifically preferred embodiment, the plasticizer is one or more selected from the group consisting of supercritical fluids, optionally substituted phenyl ethers, ionic liquids, optionally substituted xylenes, polyethers, and mixtures thereof. In a more specifically preferred embodiment of the method, the supercritical fluid is carbon dioxide, or the polyether is glyme, preferably tetraethylene glycol dimethyl ether. In an alternative embodiment, the plasticizer is a polyester polymer of a cyclic polyester oligomer, preferably a PEF polymer, preferably having a molecular weight of about 15,000 to 30,000 g / mol (melting point about 220° C.), or a PEF oligomer, preferably having a molecular weight of about 1,000 to less than about 15,000 g / mol. The aforementioned molecular weights are measured by SEC against polystyrene standards. In yet another preferred embodiment, a mixture of any of the above-mentioned plasticizers is used.

[0016] In one embodiment of the present invention, ring-opening polymerization can also be carried out on known cyclic oligomer compositions, including cyclic polyester oligomers having furan units, such as those disclosed in EP 2 931 784 A1, in the presence of the plasticizers described above and disclosed in this application.

[0017] In yet another embodiment of the ring-opening polymerization, in the presence of the plasticizer described above and disclosed in this application, the polymerization is carried out in the presence of one or more antioxidants, such as derivatives of substituted phenols and phenylenediamines.Suitable antioxidants include IRGANOX 1098, a trade name for benzenepropanamide, N,N'-1,6-hexanediylbis[3,5-bis(1,1-dimethylethyl)-4-hydroxy; sterically hindered phenol antioxidants, such as IRGANOX 1076, having the formula octadecyl-3-(3,5-di-tert.butyl-4-hydroxyphenyl)-propionate.

[0018] According to the present invention, a related object is a method for preparing a cyclic polyester oligomer composition comprising a cyclic polyester oligomer having furan units, comprising the steps of: The following processes (I) Structure Y 1 in the presence of an optional catalyst and / or an optional organic base, in a ring-closing oligomerization step under conditions of reaction temperature and reaction time sufficient to obtain a cyclic polyester oligomer having furan units, 1 Or D 1 A step of reacting monomer component C 1 But the structure [ka] wherein each group A is an optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; and l is an integer from 1 to 100, preferably from 2 to 50, most preferably from 3 to 25; R1=OH, OR, halogen or OA-OH; R=optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; R2=H or [ka] is) Monomer component D 1 But the structure [ka] wherein A is an optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; each of the groups X is OH, halogen, or optionally substituted alkyloxy, phenoxy, or aryloxy; and when A is n-butyl, the group X is not OH. and a cyclic polyester oligomer having a furan unit, structure Y 1 but [ka] wherein m is an integer from 1 to 20, preferably from 2 to 15, and most preferably from 3 to 10. The above step (I), (II) Structure Y 2 in the presence of an optional catalyst and / or an optional organic base, in a ring-closing oligomerization step under conditions of reaction temperature and reaction time sufficient to obtain a cyclic polyester oligomer having furan units, 2 Or D 2 A step of reacting Monomer component C 2 But the structure [ka] wherein each group B is an optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl, l is an integer as defined above, and n' is an integer from 1 to 20, preferably from 2 to 10; R3 = OH, OR, halogen or O-(BO) n’ -H, R=optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; R4=H or [ka] is) Monomer component D 2 But the structure [ka] wherein each group X is OH, halogen, or optionally substituted alkyloxy, phenoxy or aryloxy; each group B is optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; and n' is an integer as defined above. and a cyclic polyester oligomer having a furan unit, structure Y2 but [ka] wherein each group B is an optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; n' is an integer as defined above; and m is an integer from 1 to 20, preferably from 2 to 15, most preferably from 3 to 10. The above step (II) Any of the steps of: a subsequent step (III) of separating and removing linear oligomeric polyester species having furan units from the cyclic oligomeric composition. Including, the step of reacting the monomer components C1 or D1 or C2 or D2 in the presence of an optional catalyst and / or an optional organic base in the ring-closing oligomerization step is carried out in the presence of a solvent, the solvent being selected from the group consisting of ionic liquids, optionally substituted naphthalenes, optionally substituted aromatic compounds and mixtures thereof, optionally carried out in the presence of a zeolite to absorb impurities on the zeolite, a subsequent step (III) of separating and removing linear oligomeric polyester species having furan units from the cyclic oligomeric composition, comprising the following substeps: A sub-step of adding zeolite and absorbing impurities on the zeolite; a sub-step of cooling the cyclic oligomer composition to precipitate cyclic polyester oligomers having furan units; a substep of adding an anti-solvent to precipitate the cyclic polyester oligomer having furan units; the sub-step of separating the zeolite having absorbed impurities from the cyclic oligomer composition; Contains one or more of This is achieved by the method.

[0019] Such cyclic polyester oligomer compositions are suitable for use in the polymerization process in the present invention in the presence of a plasticizer.

[0020] According to the present invention, another further object is first achieved by a cyclic polyester oligomer composition obtainable by said process, the composition containing less than 5 wt. %, preferably 3 wt. %, most preferably 1 wt. %, of linear oligomeric polyester species, based on the total weight of the composition.

[0021] The cyclic polyester oligomer composition is used in accordance with the present invention to produce a polyester polymer by polymerization in the presence of a plasticizer.

[0022] The present invention achieves some of these further objects and provides a compound having a furan unit and structure Y 1 Or Y 2 The present invention provides a solution to these problems by a method for preparing cyclic oligomer compositions comprising cyclic polyester oligomers having any of the following: Advantageously, these cyclic oligomers are readily prepared in high purity in a relatively simple, scalable manner at high conversions and with low content of linear monomeric or oligomeric species having alcoholic and / or acidic end groups.

[0023] These results are firstly and surprisingly achieved by carrying out the cyclization reaction in the presence of a solvent. The use of a solvent is highly favorable to the formation of cyclic oligomers, where the conversion level of the end groups in the dilute reaction system is much lower than that of the end groups in the bulk system. Without wishing to be bound by a particular mechanism, the inventors believe that this effect may be due to the presence of the solvent influencing the competition between two independent reversible reactions: step-growth polymerization and cyclization. High-boiling aromatic solvents have been found to show good solubility, but preferably more volatile ones, such as xylene, are chosen to facilitate subsequent removal.

[0024] The use of zeolites has been found to be particularly effective in removing linear monomeric and oligomeric species rather than cyclic species, since the structure of the linear species is more flexible and has a smaller cross-sectional area. In particular, zeolites offer the possibility of tuning the selectivity of linear species relative to cyclic species, and even with respect to various chain lengths. This aspect is particularly advantageous when the achieved purity is greater than 99%, thereby eliminating the need for anti-solvents and their subsequent removal. Furthermore, zeolites have been found to be more robust and physically and chemically stable absorption media in typical cyclization solvent systems than silica gel, especially at relatively high temperatures (e.g. 200° C.). Advantageously, zeolites can therefore be added at or near the end of the cyclization, or earlier than at an intermediate stage of the process. Zeolites can even be present in the initial monomer solution prior to its cyclization. Zeolite addition is preferred at the end of the cyclization process, for example after the weight fraction of cyclic oligomers and total oligomers reaches 0.6, preferably 0.7, more preferably 0.8, most preferably 0.9, and then when both the remaining unreacted monomers as well as the linear oligomers have been removed.

[0025] Cyclic oligomers tend to have lower solubility in the solvent than linear oligomers, or especially monomers, or other low molecular weight species (less than 100 g / mol) with acidic and / or alcoholic functional groups. Thus, the cyclic oligomers can additionally or alternatively be removed by cooling the reaction product mixture and / or adding an anti-solvent. Since most anti-solvents do not have a high selectivity for cyclic species over linear species, it is often preferable to cool the mixture so that the cyclic species precipitate early.

[0026] It is noted that in this application, "optionally substituted" refers to chemical substituents other than hydrogen, alkyl, aryl, or alkylaryl groups. Such optional substituents are generally considered to be inert during the ring-closing oligomerization process and may be, for example, halogens or ethers.

[0027] In the present invention, "catalyst" refers to an inorganic or metal-containing compound, such as an organometallic species or metal salt, while "organic base" refers to a non-metallic and basic organic species.

[0028] In another preferred embodiment of the method, any catalyst is either absent or present as one of metal alkoxides or metal carboxylates, preferably tin, zinc, titanium, calcium, iron, aluminum or mixtures thereof. The absence of a catalyst reduces raw material costs and simplifies purification and further use of the cyclic polyester oligomer. However, the inventors have found that some metal-based catalysts are highly effective in the method of the present invention, and thus allow the preparation of cyclic polyester oligomer compositions under relatively mild temperature and time conditions. This improves productivity and minimizes degradation and discoloration in the method. Furthermore, in some embodiments, non-metal catalysts are used. For example, non-metal catalysts, such as those used in lactide to PLA production, can be used. In certain embodiments, the non-metal catalyst may be selected from one or more of the group consisting of N-heterocyclic carbene (NHC); tris(pentafluorophenyl)borane (B(CF)); 1,3,4-triphenyl-4,5-dihydro-1H-1,2,4-triazol-5-ylidenecarbyne; and DMAP / DMAP.HX (wherein XH=CFSOH, CHSOH, HCl, (FCSO)NH) or DMAP / DMAPCHX (wherein X=I-, -PF).

[0029] In a specific preferred embodiment of the method, the optional organic base E is present in a stoichiometric ratio of 0.5 to 6, preferably 1 to 4, more preferably 2 to 3 moles per mole of all monomeric component species used as reactants in the method. It has been found that the use of such a charge of optional organic base allows the ring-closing oligomerization to be carried out under relatively mild temperature and time conditions while avoiding the catalysis of undesired side reactions during the process. Furthermore, contamination of the polyester oligomer composition with large amounts of unquenched residual catalyst, which may lead to degradation and / or discoloration during subsequent heat treatments, such as polymerization or extrusion or molding of the resulting polymer, is avoided. Also, an effective balance between catalyst cost and productivity is obtained.

[0030] In a preferred embodiment of the solvent of the present process, the ionic liquid is an ionic liquid whose cation does not contain an acidic proton, more preferably the ionic liquid is N-methyl-N-alkylpyrrolidinium bis(trifluoromethanesulfonyl)imide (PYR 1R TFSI).

[0031] In another preferred embodiment of the solvent of the present process, the optionally substituted naphthalene is selected from the group consisting of naphthalene, 1-methylnaphthalene and 2-methylnaphthalene.

[0032] In yet another preferred embodiment of the solvent of the present process, the optionally substituted aromatic compound is diphenyl ether, dichlorobenzene or xylene, preferably p-xylene.

[0033] In a preferred embodiment of the process, the zeolite is selected from either zeolite Y or zeolite B, and the absorbed impurities include one or more linear oligomeric polyester species having furan and / or alcohol units. Optionally, linear monomeric acid / ol, diacid, diester, or diol species, as well as other low molecular weight (<100 g / mol) impurities having acidic or alcoholic groups, are preferably also removed. In an even more preferred embodiment of the process, the silica to alumina (SiO2 / Al2O3, mol / mol) ratio of the zeolite is greater than 5, preferably greater than 20, and even more preferably greater than 40.

[0034] In the subsequent sub-step of step (III), in which the linear oligomeric polyester species having furan units are separated and removed from the cyclic oligomeric composition, the zeolite added and the impurities absorbed may be those described above.

[0035] The sub-step of cooling the cyclic oligomer composition to precipitate cyclic polyester oligomers having furan units is preferably carried out under temperature and time conditions of 50 to 125° C. and 5 to 180 minutes, preferably 60 to 110° C. and 30 to 120 minutes, more preferably 80 to 100° C. and 45 to 90 minutes.

[0036] The substep of adding an anti-solvent to precipitate the cyclic polyester oligomers having furan units is carried out by adding an anti-solvent selected from one or more hydrocarbons or monoesters in an amount of 5 to 95, preferably 25 to 75, more preferably 30 to 60 wt. %. In a preferred embodiment, the hydrocarbon is an alkane, preferably hexane, and the ester is a salicylic acid ester, preferably methyl salicylate.

[0037] The sub-step of separating the zeolites with adsorbed impurities from the cyclic oligomer composition is preferably carried out by one or more of the following methods: filtration, sedimentation and centrifugation. Alternatively, the zeolites are immobilized on a solid support and contacted with the solution, for example by packing them in a column and passing the solution through the column as a fluid phase.

[0038] Step (III), in which the linear oligomeric polyester species having furan units are separated and removed from the cyclic oligomer composition, may comprise one or more additional separation substeps of passing the cyclic oligomer composition in a mobile phase through a stationary phase, selective precipitation, distillation, extraction, crystallization or combinations thereof.

[0039] Another aspect of the present invention relates to a cyclic polyester oligomer composition obtainable, preferably obtained, by the process according to the present invention, the composition (i) containing residual solvents at a concentration of less than 5, preferably 2, more preferably 1 wt.-%, selected from the group consisting of ionic liquids, optionally substituted naphtalenes, optionally substituted aromatics, and mixtures thereof; (ii) containing linear oligomeric polyester species having furan units and present at a concentration of less than 5, preferably 3, most preferably 1 wt.-%; and (iii) optionally containing zeolite at a concentration of less than 5, preferably 2, more preferably 1 wt.-%, the aforementioned percentages by weight being relative to the total weight of the cyclic polyester oligomer composition.

[0040] The linear oligomeric polyester species with furan units in the present invention typically contain 2 to 50, preferably 2 to 20, more preferably 2 to 10 monomer repeat units (the ester linkages being formed by the reaction of the diacid or diester monomers and diols in the present invention). Compositions containing such small amounts of linear species are advantageous in that subsequent polymerizations can be carried out efficiently and reproducibly. Large amounts and / or variable levels of linear species in the cyclic oligomer composition can alter the stoichiometry of the subsequent polymerizations and thus affect the molecular weight obtained during polymerization. Furthermore, acidic, alcoholic or ester end groups of linear oligomeric or monomeric species can react adversely and release volatile species during polymerization. Furthermore, reactive acidic species can act to quench base catalysts and / or be corrosive to process equipment.

[0041] In a preferred embodiment of the composition, the residual monomer components in the cyclic polyester oligomer composition, such as C 1 , D 1 , C 2 Or D 2 is less than 5 weight percent, preferably less than 3 weight percent, and most preferably less than 1 weight percent based on the total weight of the composition.

[0042] In a preferred embodiment of the cyclic polyester oligomer composition, the cyclic polyester oligomer composition contains halogenated impurities, preferably acid chlorides and / or their residues. Residues are defined herein as reaction products or by-products, such as halogen acids, for example HCl, or halogen salts, for example chloride salts. Such impurities are by-products of the use of reactants that are acid halides, for example acid chlorides, which have both favorable reaction rates and equilibria in the production of the oligomer composition than the reaction of alcohols with carboxylic acids. However, halogenated species are corrosive, thereby requiring specialized and expensive construction materials in the subsequent polymerization plant. Therefore, their content in the cyclic polyester oligomer composition of the present invention will preferably be kept low, for example by removal during subsequent separation and removal steps.

[0043] In another preferred embodiment of the cyclic polyester oligomer composition, the composition comprises a cyclic polyester oligomer having the structure Y 1 ' [ka] wherein m is an integer from 1 to 20, preferably from 2 to 15, and most preferably from 3 to 10. This embodiment is a suitable feedstock for the production of poly(2,5-ethylenefurandicarboxylate) (PEF) and therefore has the advantages previously described with respect to the method of producing this oligomeric composition.

[0044] In an alternative preferred embodiment of the cyclic polyester oligomer composition, the composition comprises the structure Y1″ [ka] wherein m is an integer from 1 to 20, preferably from 2 to 15, and most preferably from 3 to 10. This embodiment includes a specific cyclic polyester oligomer having furan units of the formula: This embodiment is a suitable feedstock for the production of poly(2,5-ethylenefurandicarboxylate) (PBF) and therefore has the advantages previously described with respect to the method of producing this oligomeric composition.

[0045] Another aspect of the present invention is a process for producing a polyester polymer comprising (i) the process of the present invention for preparing a cyclic oligomer composition comprising cyclic polyester oligomers having furan units, together with (ii) a subsequent polymerization step to produce a polyester polymer.

[0046] In a preferred embodiment of the method, the subsequent polymerization is carried out in the presence of a plasticizer. In an alternative embodiment of this aspect of the invention, the subsequent polymerization is carried out in the presence of a plasticizer on a cyclic oligomer composition obtainable, preferably obtained, by methods known in the art, preferably as disclosed in WO 2014 / 139603 as already discussed.

[0047] A related aspect of this invention is the use of the cyclic polyester oligomer compositions of the invention in the production of polyester polymers, which polymerization methods and uses advantageously take advantage of the desirable properties of the oligomer compositions as feedstocks in polymerization processes, such as favorable reaction rates, absence of corrosive acidic species, and absence of formation of significant amounts of volatile species during polymerization.

[0048] Those skilled in the art will understand that combinations of the subject matter of the various claims and embodiments of the present invention are possible without limiting the present invention to the extent that such combinations are technically feasible. In this combination, the subject matter of any one claim can be combined with one or more subject matter of other claims. In this combination of subject matter, the subject matter of any one method claim can be combined with one or more subject matter of other method claims, or with one or more subject matter of composition claims, or with one or more mixed subject matter of method claims and composition claims. By analogy, the subject matter of any one composition claim can be combined with one or more subject matter of other composition claims, or with one or more subject matter of method claims, or with one or more mixed subject matter of method claims and system claims. Those skilled in the art will also understand that combinations of the subject matter of the various embodiments of the present invention are also possible without limiting the present invention to the extent that such combinations are technically feasible.

[0049] The invention will be explained in more detail below with reference to various embodiments of the invention and figures. [Brief description of the drawings]

[0050] [Figure 1] FIG. 2 shows a reaction scheme for the synthesis of cyclic polyester oligomers having furan units, of structure Y1, from the reaction of monomer components C1 or D1 in a ring-closing oligomerization step. [Diagram 2] FIG. 2 shows a reaction scheme for synthesizing a cyclic polyester oligomer having furan units, of structure Y2, from the reaction of monomer components C2 or D2 in a ring-closing oligomerization step. [Diagram 3] FIG. 2 shows a reaction scheme for the synthesis of a particular cyclic polyester oligomer having furan units and of structure Y1′, useful for the production of PEF, from the reaction of particular monomer components C1′ or D1′ in a ring-closing oligomerization process. [Figure 4]FIG. 1 shows a reaction scheme for the synthesis of certain cyclic polyester oligomers having furan units and of structure Y1″, useful for PBF production, from the reaction of certain monomer components C1″ or D1″ in a ring-closing oligomerization process. [Diagram 5] FIG. 1 shows the effect of plasticization on the conversion of cyclic PEF dimer during ring-opening polymerization. [Figure 6] FIG. 1 shows HPLC results for the recovery procedure of cyclic PEF polyester oligomers. [Figure 7] FIG. 1 shows the results of thermal analysis of cyclic PEF polyester oligomer species and compositions by DSC (left) and TGA (right). [Figure 8] FIG. 1 shows a table of melting points of various cyclic PEF polyester oligomer and PEF polymer species and compositions. [Figure 9] FIG. 1 shows SEC traces of purified cyclic PEF polyester oligomers kept at 280 C (left) and conversion plots of cyclic PEF dimers kept with and without additives (right). [Figure 10] FIG. 1 shows the evolution of conversion and molecular weight of PEF ROP under different reaction conditions (50% plasticizer content). [Figure 11] FIG. 1 shows the extent to which tetraglyme (a plasticizer) is released from the reaction mixture upon evaporation by ROP operation near its boiling point. [Figure 12] FIG. 1 illustrates the conversion and molecular weight evolution for ROP producing PEF under different reaction conditions. [Figure 13] 13 shows a table of ROP selection results for the synthesis of PEF using a plasticizer amount of 50% by weight per mass of cyOEF. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0051] The claimed invention relates to a method for preparing polyester polymers from cyclic polyester oligomer compositions comprising cyclic polyester oligomers having furan units, such as those known from WO 2014 / 139603 A1, which is incorporated herein by reference. The invention also relates to such cyclic polyester oligomer compositions comprising cyclic polyester oligomers having furan units.

[0052] The present invention relates to a method for preparing a polyester polymer comprising the ring-opening polymerization of a cyclic oligomer composition comprising a cyclic polyester oligomer having furan units, the ring-opening polymerization being carried out in the presence of a plasticizer.

[0053] In one embodiment, the cyclic polyester oligomer composition has the structure [ka] (wherein m is typically an integer from 1 to 20). The composition comprises one or more cyclic polyester oligomers (cyOEF) having furan units, and the composition is used to produce a PEF polymer or copolymer.

[0054] In another embodiment, the cyclic polyester oligomer composition has the structure [ka] (wherein m is typically an integer from 1 to 20). and the composition comprises one or more cyclic polyester oligomers (cyOBF) having furan units, the composition being used to produce a PBF polymer or copolymer.

[0055] The use of plasticizers has been found to be highly advantageous in compositions having a higher content of high melting cyclic species, such as cyOEF or, in cyOEF, dimer species where m is 2. The amount of dimer species in the composition in various embodiments will be at least 40, 60 or 80% by weight.

[0056] In some embodiments, ring-opening polymerization will be used in the presence of a plasticizer to prepare higher molecular weight PEF or PBF polymers or copolymers, for example for the production of plastic bottles. In some such embodiments, the number average molecular weight Mn will be at least 25,000, preferably 30,000, more preferably 35,000 Daltons. In other such embodiments, the intrinsic viscosity will be at least 0.6, preferably 0.7, more preferably 0.85 dL / g.

[0057] In alternative embodiments, ring-opening polymerization may be used in the presence of a plasticizer to prepare lower molecular weight PEF or PBF polymers or copolymers, for example for the production of textiles, films, sheets, or tires. In some of such embodiments, the number average molecular weight Mn may be from about 10,000 to about 25,000, preferably from about 12,000 to about 22,000, more preferably from about 15,000 to about 20,000 Daltons. In other embodiments, the intrinsic viscosity may be in the range of 0.40 to 0.70, 0.72 to 0.98, 0.60 to 0.70, or 0.70 to 1.00 dL / g.

[0058] The reaction temperature for the ring-opening polymerization, in the presence of a plasticizer, will typically range from about 220 to about 300, preferably from about 230 to about 290, more preferably from about 240 to about 280° C.

[0059] The reaction time for the ring-opening polymerization will typically be less than 90, preferably 60, and more preferably less than 30 minutes in the presence of a plasticizer.

[0060] The optimal or preferred amount of plasticizer used will depend somewhat on the type and composition of the plasticizer and the specific cyclic oligomer composition, and in particular on the content of high melting dimer and other cyclic polyester oligomer species that generally only melt at temperatures well above the minimum polymerization reaction temperature previously described and close to or even above the maximum polymerization temperature previously described. In one embodiment, the high melting species is one or more cyclic polyester oligomers having furan units and having a melting point of at least 270, 280, 340 or 360° C. Such species include C2, C3, C4 or C5 (m=2, 3, 4 or 5) cyOEF or cyOBF species. For compositions containing dimeric C2 (m=2) species, the use of plasticizer is particularly important. Nevertheless, a typical amount of plasticizer in the ring-opening polymerization will be about 25 to about 75, preferably about 35 to about 65, more preferably about 40 to 60 weight percent plasticizer based on the total weight of the cyclic polyester oligomers having furan units. In certain embodiments involving intimate contact of the cyclic polyester oligomer and catalyst, for example for reaction in an extruder, the typical amount of plasticizer may be lower, for example, at least 1, 25, or 40 wt. % plasticizer may be used, based on the total weight of the cyclic polyester oligomer having furan units.

[0061] It is noted that such large amounts of plasticizer may have undesirable effects on the physical properties of the resulting polyester polymer product. Thus, in some embodiments, the plasticizer will be at least partially removed by evaporation during the ring-opening polymerization and / or during one or more subsequent devolatilization steps. Liquid tetraglyme may be preferred as a plasticizer due to its relatively low boiling point. Other plasticizers having boiling points within the reaction temperature range of the ring-opening polymerization already described may also be useful in this respect. In some embodiments, at least 60%, preferably 90%, of the plasticizer present at the start of the ring-opening polymerization will be removed during or after the polymerization. In a detailed embodiment, the plasticizer content will be advantageously reduced to a level of less than 1,000, preferably 750, more preferably 500 ppm during or after the polymerization.

[0062] In one embodiment, the cyclic oligomer composition is milled, extruded, or otherwise processed with the catalyst prior to carrying out the ring-opening polymerization, so that the catalyst is uniformly dispersed and intimately contacted between the oligomer to be reacted and the catalyst. The intimate mixing of the method may be carried out in the presence of an added plasticizer or without an added plasticizer. In the absence of an added liquid plasticizer, plasticization will be carried out internally by the oligomeric or polymeric polyester species contained within the composition itself. Thus, the polyester polymer, for example PEF or PBF, may itself act as a plasticizer, and typically such polyester plasticizers will have a number average molecular weight Mn of about 1000 to about 50,000, preferably about 10,000 to about 40,000, more preferably about 15,000 to about 30,000 Daltons. Such polyester polymer plasticizers have the useful benefit that they are not believed to have a widespread adverse effect on the physical properties of the polyester polymer product, and therefore they may not need to be removed or devolatilized following ring-opening polymerization.

[0063] In one embodiment, the intimate mixing and ring-opening polymerization is carried out in one or more extruders, preferably in a reactive extrusion process.

[0064] The cyclic polyester oligomer composition of the present invention is not specifically limited, and has a furan unit and a structure Y 1 Or Y 2 and may also contain other components. For example, the cyclic polyester oligomer composition may further contain small amounts of one or more unreacted and / or unremoved reaction components, such as monomer components used in the preparation of the cyclic polyester oligomer (unreacted diacid, diol or acidol reagents), catalysts, templating agents, bases, catalyst quenching agents, solvents. The amount of these impurities in the cyclic polyester oligomer will preferably be less than 10 wt%, more preferably less than 5 wt%, even more preferably less than 3 wt%, and most preferably less than 1 wt%, based on the total weight of the cyclic polyester oligomer.

[0065] In addition, the cyclic polyester oligomer composition may further contain small amounts of impurities that are introduced as contaminants in one of the reaction components or that are formed due to side reactions during the ring-closing oligomerization process or any additional process, such as the subsequent devolatilization process. Examples of such impurities are linear oligomeric polyester species with furan units. Finally, the cyclic polyester oligomer composition may further contain additional components, such as typical monomer additives (e.g. stabilizers against oxidation, thermal degradation, light or UV irradiation) that are added during production or before use. Those skilled in the art will understand that blends with other monomers are also considered within the scope of the present invention in order to combine the preferred properties of various monomers.

[0066] In one embodiment, the content of diacid, diol or acidol monomers in the cyclic polyester oligomer composition is less than 5 wt%, preferably less than 3 wt%, more preferably less than 1 wt%. In this application, the content of diacid, diol or acidol monomers refers to their content as determined by extraction of soluble species followed by GC-MS analysis.

[0067] As shown in FIG. 1, the structure Y 1 The process of the present invention for preparing a cyclic oligomer composition comprising a cyclic polyester oligomer of the structure Y 1 in the presence of an optional catalyst and / or an optional organic base, in a ring-closing oligomerization step under conditions of reaction temperature and reaction time sufficient to obtain a cyclic polyester oligomer having furan units, 1 Or D 1 A step of reacting monomer component C 1 But the structure [ka] wherein each group A is an optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; and l is an integer from 1 to 100, preferably from 2 to 50, most preferably from 3 to 25; R1=OH, OR, halogen or OA-OH R=optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; R2=H or [ka] is) Monomer component D 1 But the structure [ka] wherein A is an optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl, and each of the groups X is OH, halogen, or optionally substituted alkyloxy, phenoxy or aryloxy, and when A is n-butyl, the group X is not OH. The method includes the above steps.

[0068] As shown in FIG. 2, the structure Y2 The process of the present invention for preparing a cyclic oligomer composition comprising a cyclic polyester oligomer of the structure Y 2 in the presence of an optional catalyst and / or an optional organic base, in a ring-closing oligomerization step under conditions of reaction temperature and reaction time sufficient to obtain a cyclic polyester oligomer having furan units, 2 Or D 2 A step of reacting monomer component C 2 But the structure [ka] wherein each group B is an optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; l is an integer as defined above; and n' is an integer from 1 to 20, preferably from 2 to 10. R3 = OH, OR, halogen or O-(BO) n’ -H, R=optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; R4=H or [ka] is) Monomer component D 2 But the structure [ka] wherein each group X is OH, halogen, or optionally substituted alkyloxy, phenoxy or aryloxy; each group B is optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; and n′ is Y 2 (which is an integer already defined for The method includes the above steps.

[0069] In step (III) after (I) or (II), the linear oligomeric polyester species having furan units are separated and removed from the cyclic oligomeric composition.

[0070] FIG. 3 shows a specific monomer component C in the ring-closing oligomerization process. 1 ' or D 1 ', which is useful for producing PEF and has a furan unit, structure Y 1 4 shows a reaction scheme for synthesizing a specific cyclic polyester oligomer of ', and FIG. 5 shows a reaction scheme for synthesizing a specific monomer component C in the ring-closing oligomerization process. 1 " or D 1 " reaction, which is useful for producing PBF, and has a furan unit, structure Y 1 3 shows a reaction scheme for synthesizing a particular cyclic polyester oligomer of formula (I) ", where in both figure examples l, m and n are as previously defined.

[0071] Unless specifically indicated, conventional ring-closing oligomerization processes and their various reagents, operating parameters and conditions, such as those known from WO 2014 / 139603 A1, are represented by the formula: 1 , Y 2 , Y 1’ Or Y 1’’ The process according to the invention can be used to prepare cyclic polyester oligomers having the formula:

[0072] In the ring-closing oligomerization step, the conditions of reaction temperature and reaction time sufficient to obtain a cyclic polyester oligomer having furan units are not specifically limited. In this specification, the term sufficient means that the reaction temperature and time are sufficient to cause the ring-closing reaction, and an oligomer having the value of m described in the claims is produced from the monomer components. Those skilled in the art will understand that the appropriate specific reaction temperature and reaction time may vary somewhat due to the mutual influence between reaction temperature and reaction time.

[0073] For example, increasing the reaction temperature allows the reaction to occur in a shorter time, or increasing the reaction time allows a lower reaction temperature to be used. Lower reaction temperatures and / or shorter reaction times may be appropriate if lower molecular weight cyclic polyester oligomers are to be produced and / or if a lower conversion of the monomeric components to oligomers can be tolerated. Alternatively, higher reaction temperatures and / or longer reaction times may be appropriate if higher molecular weight cyclic polyester oligomers are to be produced and / or if a higher conversion of the monomeric components is desired.

[0074] Furthermore, the use of more effective catalysts or bases, or higher concentrations of catalysts or organic bases, allows the use of milder reaction conditions (e.g., lower reaction temperatures and shorter reaction times). Conversely, the presence of impurities, particularly catalyst-quenching or chain-stopping impurities, can necessitate more aggressive reaction conditions.

[0075] In one embodiment, the cyclization reaction temperature is 100 to 350, preferably 150 to 300, and most preferably 180 to 280° C., and the reaction time is 30 to 600, preferably 40 to 400, and most preferably 50 to 300 minutes. In certain embodiments, a combination of various specific temperature and time ranges obtained by any combination of these disclosed ranges may be used. In more preferred embodiments, these temperature and / or time ranges are 1 Or C 2 together with the ring-closing oligomerization step.

[0076] In another embodiment, the cyclization reaction temperature is −10 to 150, preferably −5 to 100, and most preferably 0 to 80° C., and the reaction time is 5 to 240, preferably 10 to 180, and most preferably 15 to 120 minutes. In certain embodiments, a combination of various specific temperature and time ranges obtained by any combination of these disclosed ranges can be used. In more preferred embodiments, these temperature and / or time ranges are selected from the group consisting of monomer component D 1 Or D 2 together with the ring-closing oligomerization step.

[0077] In the practice of the present invention, any catalyst capable of catalyzing ring-closing oligomerization to form cyclic polyester oligomers can be used. Catalysts suitable for use in the present invention are those known in the art for the polymerization of cyclic esters, such as inorganic bases, preferably metal alkoxides, metal carboxylates, or Lewis acid catalysts. Lewis acid catalysts may be metal coordination compounds that contain metal ions with more than one stable oxidation state. Among this type of catalyst, tin- or zinc-containing compounds are preferred, of which alkoxides and carboxylates are more preferred, with tin octoate being the most preferred catalyst.

[0078] The ring-closing oligomerization step is preferably carried out in the presence of any organic base. The organic base is not specifically limited and may be an inorganic or organic base. In one embodiment, the organic base has the general structure E, and in another embodiment, it is an alkylamine, such as triethylamine or pyridine. In yet another embodiment, the organic base is a combination of E and an alkylamine. In this application, "catalyst" refers to an inorganic or metal-containing compound, such as an organometallic species or metal salt; whereas, "organic base" refers to non-metallic and organic base species.

[0079] Certain combinations of catalyst and base may be particularly effective and their use is preferred. In a preferred embodiment, the catalyst is a tin, zinc, titanium or aluminum alkoxide or carboxylate and the organic base is DABCO (CAS No. 280-57-9) or DBU (CAS No. 83329-50-4), preferably with triethylamine. The monomer components may be in a solid phase when mixed with the catalyst and / or organic base. However, it is preferred to use a solvent to bring the monomer components into a molten or liquid phase and then add the catalyst and / or organic base thereafter.

[0080] The amount of catalyst and / or organic base in the method of the present invention is not specifically limited. In general, the amount of catalyst and / or organic base is sufficient to cause the ring-closing oligomerization process to occur for the selected reaction temperature and time, so that oligomers having the l value recited in the claims are produced from the monomer components. In one embodiment, the catalyst and / or organic base are present, the catalyst is present in an amount of 1 ppm to 1 wt%, preferably 10 to 1,000 ppm, more preferably 50 to 500 ppm, based on the total weight of the monomer components, and the organic base is present in a stoichiometric ratio of 0.5 to 6, preferably 1 to 4, more preferably 2 to 3 mol per mol of all monomer component species used as reactants in the method. The concentration of catalyst and organic base can be easily measured by the mass or mass flow rate of these reagents used relative to the mass or mass flow rate of the monomer components.

[0081] The method of preparing the cyclic polyester oligomer composition of the present invention is not specifically limited and can be carried out in batch, semi-continuous or continuous mode. The oligomerization method suitable for preparing the cyclic polyester oligomer composition of the present invention can be divided into two groups: solution oligomerization in the presence of a solvent, or oligomerization substantially free of a solvent, for example, melt oligomerization carried out at a temperature above the melting temperature of the monomeric components and oligomeric species.

[0082] Because the presence of significant amounts of unreacted monomeric components, such as linear oligomers, or other low molecular weight species in the cyclic polyester oligomer composition, especially those having acidic or other free OH groups, can adversely affect the storage stability and / or polymerization processing behavior of the oligomer composition, the cyclic polyester oligomer composition is subjected to a process in which the linear oligomeric polyester species, and optionally other impurities, such as low molecular weight (e.g., less than 100 g / mol) species having acidic and / or hydroxyl groups, are removed.

[0083] The process of separating and removing linear oligomeric polyester species having furan units, and possibly other impurities, from the cyclic polyester oligomer composition of the present invention is not specifically limited. Examples of other impurities may be unreacted starting materials, such as diacids or diols, or residual reagents, such as bases or their residues (e.g., amine residues). Separation and purification methods are well known in the art, for example, as disclosed in "Purification of Laboratory Chemicals", 6th Edition, WEArmarego and CLLChai, 2009, Elsevier, Oxford (ISBN-13:978-1856175678) and "The Molecular World, Separation, Purification and Identification", LESmart, 2002, the Royal Society of Chemistry, Cambridge (ISBN:978-1-84755-783-4).

[0084] Unless specifically indicated, conventional separation and purification processes, and their various equipment, operating parameters and conditions, are used in the methods of the present invention to prepare compounds of structure Y 1 , Y 2 , Y 1 ' or Y 1 " and compositions thereof.

[0085] In one embodiment, the separation step in which the linear oligomer species and optionally other impurities are removed comprises one or more separation sub-steps of passing a mobile phase, which is the cyclic oligomer composition, through a stationary phase, selective precipitation, distillation, extraction, crystallization, or combinations thereof.

[0086] In the product, which is the cyclic polyester oligomer composition obtained after the separation step, the linear oligomeric polyester species having furan units are generally present in an amount of less than 5% by weight, more specifically less than 3% by weight, and even more specifically less than 1% by weight, based on the total weight of the cyclic polyester oligomer composition. The content of the linear oligomeric polyester species having furan units in the cyclic polyester oligomer composition of the present invention can be easily measured by conventional methods. For example, the content of the linear oligomeric species can be measured by electrospray mass spectrometry, matrix-assisted laser desorption / ionization (MALDI) mass spectrometry, high performance liquid chromatography (HPLC) method combined with mass spectrometry, and gel filtration chromatography. In the present application and invention, the concentration of the linear oligomeric polyester species having furan units refers to the concentration measured by HPLC.

[0087] In a preferred embodiment of the composition, the residual monomer components in the cyclic polyester oligomer composition, such as C 1 , D 1 , C 2 Or D 2 The content of is less than 5 weight percent, preferably 3 weight percent, and most preferably 1 weight percent based on the total weight of the composition. The content of such residual monomer (or solvent) components can be measured by FTIR or NMR spectroscopic analysis of the composition. Alternatively, the content can be measured by chromatographic methods, such as HPLC or GC. In the present application and invention, the concentration of residual monomer (and solvent) components refers to the concentration measured by HPLC.

[0088] The present invention relates to a cyclic polyester oligomer composition comprising a cyclic polyester oligomer having a furan unit, the cyclic polyester oligomer having a furan unit having a structure of Y 1 Or Y 2 and the polyester polymer composition is obtained by the above process. The cyclic polyester oligomer composition is characterized in that the composition contains (i) residual solvent selected from the group consisting of ionic liquids, optionally substituted naphtalenes, optionally substituted aromatics, and mixtures thereof, at a concentration of less than 5, preferably 2, more preferably 1% by weight, (ii) linear oligomeric polyester species having furan units and present at a concentration of less than 5, preferably 3, most preferably 1% by weight, and (iii) optionally zeolite at a concentration of less than 5, preferably 2, more preferably 1% by weight, the percentages being based on the total weight of the cyclic polyester oligomer composition. Such oligomer composition can meet the majority of the requirements posed by current polymerization applications.

[0089] In another preferred embodiment, the composition contains halogenated impurities, preferably acid chlorides and / or their residues. Methods for detecting halogenated impurities in oligomers are well known and include combustion ion chromatography (IC), optical atomic spectroscopy and X-ray fluorescence spectrometry (XRF). However, halogenated species can be corrosive and therefore require special and expensive construction materials in the subsequent polymerization plant. Therefore, their content in the cyclic polyester oligomer composition of the present invention will preferably be kept low, for example by removal during the subsequent separation and removal steps.

[0090] In a preferred embodiment of the cyclic polyester oligomer composition, the specific cyclic polyester oligomer having furan units has the structure Y 1 ' or Y 1 " where m is an integer from 1 to 20, preferably from 2 to 15, and most preferably from 3 to 10.

[0091] Yet another aspect of the present invention is a method for producing a polyester polymer, comprising (i) the method of the present invention for preparing a cyclic oligomer composition comprising a cyclic polyester oligomer having furan units, together with (ii) a subsequent polymerization step to produce a polyester polymer. Suitable ring-opening polymerization catalysts, processing conditions, equipment and methods are those disclosed in the previously discussed WO 2014 / 139602, which is incorporated herein by reference. The aspect of using the cyclic polyester oligomer composition of the present invention is related to this aspect with respect to the production of a polyester polymer. A preferred embodiment of this method or use is the embodiment in which the polyester polymer is a PEF polymer or a PBF polymer.

[0092] Particularly preferred is a polyester polymer composition obtainable and preferably obtained by the ring-opening polymerization process of the present invention, the composition containing (i) a plasticizer selected from the group consisting of optionally substituted phenyl ethers, ionic liquids, optionally substituted xylenes, polyethers, and mixtures thereof, (ii) a cyclic polyester oligomer having furan units, and (iii) either (a) a PEF polymer or (b) a PBF polymer. The residual plasticizer is preferably present in an amount of less than 10, more preferably 5, even more preferably 2, and most preferably 1 wt. %. The plasticizer content in the polymer can be measured by conventional methods, such as those disclosed in Quantifying Polymer Plasticizer Content Through Direct Analysis of Tracer Compounds, IP.com Disclosure No.: IPCOM000246667D, Publication Date: June 24, 2016. The unreacted residual cyclic polyester oligomer having furan units is preferably present in an amount of less than 5, more preferably 2, and even more preferably 1 wt. %. In some embodiments, the content of residual plasticizer and unreacted cyclic oligomers are measured by separating them from the polymer by solvent extraction, high temperature distillation or column chromatography, followed by their identification by UV, NMR or IR spectroscopy and / or mass spectrometry.PEF and PBF polymers will often have a molecular weight of at least 10,000, preferably 15,000, more preferably 20,000 Daltons as measured by SEC against polystyrene standards. EXAMPLES

[0093] The following examples are set forth to provide those of ordinary skill in the art with detailed descriptions of how the claimed methods, polyester polymer compositions, and uses are evaluated, and they are not intended to limit the scope of what the inventors regard as their invention.

[0094] In these examples, the following characterization methods and parameters were used to characterize the cyclic polyester oligomer compositions prepared in the examples.

[0095] SEC-MALS Polyester conversion and molecular weight distribution were analyzed using multi-angle light scattering (SEC-MALS) on an Agilent 1100 GPC, a DAWN HELEOS II multi-angle laser light scattering (MALS) detector (Wyatt Technology Europe) using two PFG Linear M columns (PSS) in series connected to an Agilent 1100 VWD / UV detector operated at 290 nm, followed by size exclusion chromatography coupled to an Agilent 1100 RI detector. Samples were eluted in HFIP with 0.02 M K-TFAc at 1 mL / min at room temperature.

[0096] 1 H NMR The measurements were carried out on a Bruker AV300 spectrometer operating at a frequency of 300 MHz and using CDCl3 as the solvent.

[0097] HPLC-MS An Agilent 1200 Series HPLC with quaternary pump, autosampler and UV detector was equipped with an Agilent Eclipse XDB-C18, 5 m, 4.6 x 150 mm column. The eluent mixture consisted of (A) water stabilized with formic acid (1 mL / L) and (B) acetonitrile stabilized with formic acid (1 mL / L). The gradient was run at 1 mL / min for 60 min. The solvent ratio of B was changed linearly from 20% to 45.2% in 11 min, then from 45.2% to 80% in 29 min, followed by 97% in 10 min, and 20% in 10 min. Samples were dissolved at 1 mg / mL in HFIP / CHCl3 (15%). The injection volume was 10 μL and UV detection was performed at 280 nm. Peaks were characterized by online mass spectroscopy using an Agilent 1640 single quadrupole MS.

[0098] MALDI-TOF The matrix was T-2-[3-(4-t-butyl-phenyl)-2-methyl-2-propenylidene]malononitrile (DCTB)+Na mix 10:1, the instrument type was Bruker Daltonics Ultraflex II, and the collection mode was reflector.

[0099] (Example 1) Cyclic polyester oligomer composition (Y 1 'Embodiment of the Invention) In this example, the preparation of a cyclic polyester oligomer, shown in FIG. 3, is described, which can then be used to prepare PEF, i.e., poly(2,5-ethylene furan dicarboxylate). 40 g of me-FDCA was placed in a glass reactor equipped with a stirrer together with 20 mL of EG. The reaction was carried out under an inert atmosphere in the presence of 0.50 g of catalyst (Bu2SnO), at an initial temperature of 140° C., and gradually heated to a final temperature of 180° C. After 1 h, the reaction pressure was reduced to 700 mbar; after 40 min, the pressure was reduced again to 400 mbar, and after 30 min, it was further reduced to 200 mbar. Finally, the pressure was reduced stepwise to 10 mbar. The temperature was increased to 200° C., and the system was left under these conditions for 2 h. The system was cooled to room temperature, the solid product was removed, crushed and dried. The obtained prepolymer was characterized by HPLC and GPC, and its identity was confirmed to be C 1 ' was confirmed.

[0100] Prepolymer C 1 ' was dissolved in 2-methylnaphthalene as a solvent at a concentration of 10 g / l, and the resulting solution was heated at 200° C. to obtain prepolymer C 1 ' to the cyclic oligomer Y 1The reaction was allowed to proceed for 3 hours under an inert atmosphere (without any additional catalyst added) to transform the mixture into '. Next, zeolite Y was added at a concentration of 10 g / l. HPLC analysis confirmed that the concentration of cyclic oligomers (m=2 to 5) remained essentially unchanged, while the linear species (l=1 to 8) were essentially removed from the solution. This confirms that the residual unreacted linear species can be easily removed from the reaction system by adsorption on the zeolite.

[0101] (Comparative Examples 1 and 2) Cyclic polyester oligomer compositions (Y 1’ ) lack of significant polymerization In this example, the cyclic oligomer Y1' (m=2) of Example 1 was reacted with tetra-glyme as plasticizer at a concentration of 60 uL of tetra-glyme per 180 mg of cyclic oligomer Y1' for 30 minutes under inert atmosphere at different temperatures between 260° C. and 320° C. No reaction occurred and the material remained unchanged.

[0102] In a second comparative example, the mixed cyclic oligomers Y1' (m=2 to 7) of Example 1 were reacted at a temperature of 280° C. for 60 minutes without the addition of a plasticizer or catalyst. GPC analysis confirmed little or no reaction of the generated m=2 cyclic oligomers. Thus, these comparative examples show that the typically most abundant species of low Mw cyclic oligomers (m=2) will generally not polymerize appreciably in a reasonable time without a catalyst or plasticizer.

[0103] (Example 2) Catalyzed Cyclic Polyester Oligomer Composition (Y 1’ ) to generate PEF In this example, the cyclic oligomer Y1' (m=2) of Example 1 was reacted as in Comparative Example 1, but in the presence of cyclic stannoxane as catalyst at a concentration of 0.1 mol % per mole of cyclic oligomer repeat unit. In this example, over 95% conversion was achieved within 20 minutes.

[0104] FIG. 5 shows data comparing the conversion of cyclic PEF dimer with both lower (1 / 3 v / m) and higher (2 / 3 v / m) concentrations of tetra-glyme plasticizer.

[0105] In carrying out other polymerizations, other metal oxide catalysts, such as Sb2O3 or Bi2O3, were compared to tin-based catalysts, and it was observed that the polymers prepared using Sb2O3 or Bi2O3 were more colorless and transparent in appearance than the slightly tan ones obtained with tin-based catalysts.

[0106] (Example 3) The uncatalyzed cyclic polyester oligomer composition (Y 1’ ) to generate PEF In this example, the cyclic oligomer Y1' (m=2) of Example 1 was reacted with tetra-glyme as plasticizer at a higher concentration of 240 uL of tetra-glyme per 180 mg of cyclic oligomer Y1' as in Comparative Example 1. In this example, over 95% conversion was achieved within 60 minutes at all temperatures.

[0107] (Example 4) Effect of reaction conditions on the formation of PEF from cyclic polyester oligomer compositions by ring-opening polymerization. In this example, high molecular weight PEF polymers were prepared from cyclic PEF oligomers (cyOEF) prepared as described in this application as well as previously described in WO 2014 / 139603 A1.

[0108] The following subsections outline the chemicals, equipment, and analytical devices used to demonstrate, by way of examples, the effect of various reaction conditions on the synthesis of PEF polymers from cyclic PEF oligomers (cyOEFs).

[0109] material Dibutyltin oxide (Bu2SnO, ≥ 98%), anhydrous ethylene glycol (EG, 99.8%), dimethyl 2,5-furandicarboxylate (meFDCA, 99%), tin(II) 2-ethylhexanoate (tin octoate, SnOct2, 95%), 1-dodecanol (98%), trifluoroacetic acid (TFA, 99%) and potassium trifluoroacetate (K-TFAc, 98%), 2-methylnaphthalene (95% or 97%), acetonitrile (ACN, ≥ 99. 7%), n-hexane (≧95%), toluene (≧99.7%), tetraethylene glycol dimethyl ether (tetraglyme, 99%), diethyl ether (Et2O, ≧99.8%), dichloromethane (DCM, 99.99%), hexafluoroisopropanol (HFIP, 99.9%), chloroform-d (CDCl3, ≧99.8%) and trifluoroacetic acid-d (TFA-d, 99.5%) were used as received from a laboratory supply store. The initiators 1-dodecanol and tetraglyme were stored in a glove box under nitrogen atmosphere. It is noted that these same materials were generally used in previous examples as well.

[0110] For benchmarking of the produced PEF examples against bottle-grade PET, the latter sample was obtained from a commercial PET plastic bottle. To verify the accuracy of the polymer molecular weight analysis, PET and PMMA standards were analyzed from PSS Polymer Standards Service, Germany.

[0111] analytical theory 1H NMR (300 MHz, 400 MHz) spectra were recorded on a Bruker Avance III spectrometer. 1H NMR spectra were referenced to residual solvent signals. Conversion (X), number-average and weight-average absolute molecular weight Mn and Mw values ​​of PET and PEF samples were determined by size-exclusion chromatography (SEC). An Agilent 1100 GPC / SEC unit equipped with two PFG Linear M columns (PSS) connected in series to an Agilent 1100 VWD / UV detector operated at 290 nm, a DAWN HELEOS II multi-angle laser light scattering (MALS) detector (Wyatt Technology Europe), followed by Wyatt's Optilab T-rEX RI detector was used. Samples were eluted in HFIP with 0.02 M K-TFAc at 1 mL / min at room temperature. Conversion was evaluated with PSS WinGPC Unichrom software as a fraction of the total PEF vs. UV signal area. Absolute molecular weights were evaluated using Wyatt ASTRA software and dn / dc values ​​based on our analytical settings (dn / dc(PEF)=0.227 mL / g, dn / dc(PET)=0.249 mL / g). Further absolute molecular weights were obtained from diffusion (DOSY) NMR measurements using 0.4 mg / mL samples of PET and PEF in TFA-d.

[0112] Analysis of cyOEF ring size composition and purity from residual linear was assessed on an Agilent 1100 HPLC with UV detector at 280 nm followed by an Agilent 1640 single quadrupole ESI-TOF mass spectrometer. Linear and cyclic species were clearly identified by this HPLC-MS setup and cyOEF purity was assessed as the HPLC area associated with the cyclic oligomer peaks versus the total HPLC area. The UV extinction coefficients of linear and cyclic species were assessed prior to these measurements to ensure an unbiased assessment and were found to be the same for all species. Samples were dissolved in 15% (v / v) HFIP / CHCl3 and eluted at 1 mL / min through an Eclipse XD8-C18 column (150 x 4.6 mm, 3.5 μm pore size) with a 20 / 80 to 80 / 20 acetonitrile / H2O gradient over 40 min. Formic acid 0.1% (v / v) was added as a stabilizer to both the organic and aqueous phases, Millipore water was used as the aqueous phase and acetonitrile as the organic phase, and the injection volume was kept constant at 10 μL.

[0113] Thermal property analysis was performed on a Mettler Toledo DSC Polymer machine calibrated with indium and zinc standards. The heating rate was 10°C / min under nitrogen flow. The cyclic oligomer melting point was calculated from the first heating curve, the glass transition temperature (Tg), and the PEF melting point (Tm) was calculated from the second heating curve after quenching in liquid nitrogen. Tg was recorded at the intermediate temperature. Thermal stability and degradation were analyzed on a Mettler Toledo TGA / SDTA 851 using a heating rate of 10°C / min under nitrogen flow.

[0114] Polarized optical microscopy (POM) images were acquired on an Olympus BX51 microscope equipped with a Linkam LTS350 temperature-controlled stage and a DP72 digital camera. Powder diffraction patterns were recorded on a Stoe&Cie STADI P powder diffractometer with Cu-K alpha 1 radiation focused on a Ge-monochromator and a Dectris Mythen silicon strip detector. ICP-OES analysis was performed on a Perkin Elmer Optima 8300. Gas permeability analysis of ROP-based PEF and PET films was performed on a MOCON Ox-Tran device using 35-45 μm thick films obtained from solution casting at 23 °C and 50% relative humidity. Films were prepared by solution casting of approximately 200 mg / mL PEF in HFIP on a heated glass plate at 70 °C to evaporate the HFIP, after which the thickness of the films was measured.

[0115] Preparation of cyclic stannoxane (cySTOX) initiator and its depolymerization to prepare cyclic oligoethylene furoate (cyOEF) 1,1,6,6-tetra-n-butyl-1,6-distanna-2,5,7,10-tetraoxacyclodecane, or commonly referred to as cyclic stannoxane (cySTOX), was synthesized using literature methods.

[0116] Cyclic PEF oligomers (cyOEF) were prepared according to the methods already described in this application and in WO 2014 / 139603 A1. In the depolymerization route, in detail, 400 g of dimethyl 2,5-furandicarboxylate (400 g, 2.17 mol, 1 eq.), ethylene glycol (270 g, 4.35 mol, 2 eq.) and Bu2SnO (2 g, 8 mmol, 0.004 eq.) were placed in a three-neck round-bottom flask equipped with a magnetic stirrer under N2 atmosphere. The solution was stirred at 200 °C and methanol was distilled as a condensation product and removed over 2 h. Excess ethylene glycol was removed under vacuum overnight to obtain a solid product. The PEF prepolymer (linOEF) was stored in a glove box and a 10 g batch of linOEF prepolymer was dissolved in 1 L of 2-methylnaphthalene (2-MN) in a 3-neck round bottom flask equipped with a magnetic stirrer under N2 atmosphere at 200 °C. The solution was stirred for 6 h, at which time the conversion of linOEF to cyOEF equilibrated at approximately 80%. The cyOEF / linOEF products were collected by precipitation on cooling and occasional addition of 1:1 v / v hexane followed by filtration.

[0117] cyOEF was purified from the linear species by elution through a short silica gel column with Et2O in DCM up to 7.5% v / v. The product was concentrated to give the cyclic species as a white powder with a purity of >99%. Individual cyclic species could also be fractionated by eluting the crude product in DCM through silica gel using Et2O / DCM (7.5 / 92.5 v / v) as the mobile phase. All purified products were collected and analyzed for purity by HPLC-MS, and they were characterized by 1H NMR.

[0118] Synthesis of polyethylene furoate (PEF) by ROP For every batch of molten ring-opening polymerization (ROP), an amount of cyOEF was weighed in a Schlenk tube reactor equipped with a magnetic stirrer in a glove box. The tube was transferred to a heating block and dried under vacuum. The reactor was removed from the heater and the vacuum was released with nitrogen. The temperature was set to the desired value and the Schlenk tube was reintroduced into the heating block. The initiator was added neat or in the form of a suspension with a plasticizer (tetraglyme). The initiator suspension was preheated to 70° C. with stirring, and it was observed that, especially for cySTOX, which is a powder at room temperature unlike SnOct2, the solubility was increased and therefore the homogeneity of the initiator solution was improved at higher temperatures. The initiator was injected at a concentration of 0.01 to 0.03 M in tetraglyme after 5 min of temperature equilibration in the case of the cyclic dimer or before heating to the reaction temperature. Samples were taken during the reaction. Visual appearance and discoloration were qualitatively analyzed during sampling. After the desired reaction time, the product was quenched by immersion in ice water, followed by dissolution in pure HFIP and precipitation in THF. The product was collected either by filtration of the mixture or by centrifugation of the mixture and removal of the solvent by decantation. The solid was dried under vacuum at 80° C. to give a white or brown powder, depending on the reaction conditions, which was characterized by 1H NMR, as discussed later.

[0119] The results of these additional examples illustrate the effect of reaction parameters on the formation of initial cyclic PEF oligomers (cyOEFs), and subsequently representative final PEF polymers, and are shown in FIG.

[0120] FIG. 6 illustrates an embodiment of the recovery procedure after cyOEF preparation. Upon cooling to 100° C., the cyclic dimer C2 precipitates first. Further cooling precipitates more cyclic dimers, but not trimer C3 and linear chains (linOEF). Using an anti-solvent, C3 can be precipitated as well. Such selective precipitation methods allow the preparation of cyOEF materials of different compositions. Purification via silica gel allows the removal of residual linOEF, which may limit the ultimately achievable molecular weight during subsequent ROP.

[0121] FIG. 7 shows DSC (left) and TGA (right) traces of isolated cyclic dimers C2, C3, cyOEF and PEF polymers with a full range of ring sizes after hexane precipitation with C3 removed by precipitation upon cooling. These plots demonstrate that the C2 dimer, which is the major component in cyOEF and usually results from cyOEF synthesis, e.g., depolymerization, has two temperature transitions. The first one at 290° C. is recrystallized as evident by powder diffraction and POM analysis, and the second one at 370° C. is the actual melting point. The melting points of cyOEF species and mixtures of different compositions and PEF polymers evaluated by DSC are summarized in the table shown in FIG. 8, and literature values ​​for cyclic PET oligomers of given ring sizes and linear PET polymers are also shown for comparison.

[0122] The extremely high melting point of the C2 cyOEF dimer is in the thermal range of both the PEF polymer and the cyOEF degradation (see TGA on the right of the figure). Therefore, the ROP of the PEF cyclic oligomer needs to be carried out at a temperature well below this temperature in order to obtain a satisfactory polymer product with good color. This optimized result can be achieved by plasticization, as shown in the following sub-examples.

[0123] Figure 9 shows the SEC traces of purified cyOEF(-) after 20, 60, 240 and 666 min, respectively, held neat without additives at 280°C, represented by the dashed lines with increasing punctuation. The corresponding molecular weights of the polymers (PEF peaks) formed during the reaction were Mn=33.8, 40.5, 24.8 and 13.8 kg / mol, respectively. These results illustrate that C3 and higher cyclic species react with PEF within 1 h, but the complete conversion of C2 requires more than 10 h, as its degradation results in substantially less PEF molecular weight being achieved.

[0124] Figure 10 illustrates the effect of plasticization (right). The conversion of purified cyOEF kept neat without additives (□) at 280°C was compared to ROP using 66% tetraglyme without initiator (△), 0.1% cySTOX initiator ground into cyOEF without plasticizer (◇), the same ground with 33% tetraglyme added (◆), and premixed with initiator and tetraglyme as plasticizer by stirring without grinding (○). These results show that homogenization of the initiator into the cyOEF feedstock by grinding (such as in an industrial scale extruder) substantially increases the reaction rate, leading to higher molecular weights, albeit very non-uniformly, and longer reaction times leading to discoloration. Optimal results in terms of conversion and discoloration are achieved by using tetraglyme as a plasticizer and as a promoter of uniform dispersion of the initiator.

[0125] Figure 11 shows how much tetraglyme is released from the reaction mixture along the reaction path by evaporation from the ROP operation near its boiling point (275 °C) at different plasticizer loadings ranging from 0% (○), 25% (△), 33% (◇) to 100% (□).

[0126] FIG. 12 illustrates the evolution of conversion and molecular weight for PEF ROP under different reaction conditions. The plasticizer content was 50% in all cases. Subplot A demonstrates the feasibility of complete (95%) conversion of the most resistant and highest melting cyclic species, cyOEF C2 species, to PEF by ROP. The reaction conditions were 280° C. temperature using 0.1% (+) and 0.2% (×) SnOct2 and 0.07% (○) and 0.15% (△) cySTOX as initiator. Subplot B shows the effect of reaction temperature using purified cyOEF with predominantly C2 and C4 and less C3, C5, C6, C7. The reaction conditions were 0.1% cySTOX as initiator with reaction temperatures of 240° C. (○), 260° C. (□), and 280° C. (◇). Subplot C shows the optimization of initiator content for ROP. The reaction conditions were a temperature of 260°C using different cySTOX loadings, namely 0.05% (○), 0.1% (□), 0.2% (◇) and 0.3% (△). The dashed lines in Figure 13 should draw attention to the partial living behavior (linear tendency of Mn at X) before degradation becomes significant. At 260°C, 0.1% cySTOX as initiator represents the optimal condition in these examples, reaching the highest molecular weight in less than 20 minutes before molecular weight degradation becomes significant.

[0127] Figure 13 shows the results of ROP selection for the synthesis of PEF using 50% by weight of plasticizer per mass of cyOEF. The purity of cyclic oligomers is shown as HPLC area fraction of cyOEF relative to the total area. X is the conversion quantified as SEC area fraction of PEF versus total area. Mn and Mw are absolute molecular weights from SEC-MALS.

[0128] Table entries 1 and 2 show that purified cyOEF can often react very slowly, sometimes taking more than 10 hours to reach 80% conversion, and therefore complete conversion at bottle grade molecular weights is generally not readily feasible without the addition of initiators and plasticizers.

[0129] Table entries 3-7 show the feasibility of converting C2, the highest melting and extremely reaction resistant cyclic species, to PEF. Two initiators were used: SnOct2 and cyclic stannoxane (cySTOX). SnOct2 often only allows for the production of lower molecular weight PEF polymers due to the alcohol required to activate SnOc2, which adds additional end groups to the system, thereby reducing the achievable molecular weight. cySTOX is therefore the preferred initiator in these examples in terms of achievable molecular weight and reaction rate.

[0130] Table entries 8-10 show the effect of cyOEF purity. The lower the purity, the lower the molecular weight of the polymer produced. Without wishing to be bound by any mechanism, we conclude that a purity of about 98-99% is required to achieve high molecular weight of the polymer.

[0131] Table entries 11-12 show the effect of temperature using cySTOX initiator. Going from 280°C to 260°C slowed the reaction rate but limited thermal degradation, allowing for the production of higher molecular weights. The temperature of 240°C was too low in these particular examples, slowing the reaction too much, and the long reaction times exposed the product to potential degradation for too long.

[0132] Table entries 13-15 show the optimization of the initiator content after the reaction temperature was optimized to 260°C for the specific reaction conditions in this particular example and the reaction equipment used. A higher initiator content means a faster reaction and lower molecular weight due to the increased number of end groups and chains in the system. The optimal concentration in these particular examples was found to be around 0.1 mol% of cySTOX (relative to the cyOEF repeats).

[0133] Table entries 16-19 show data for ROP reactions selected to evaluate the effect of various parameters on the polymer discoloration. Polymerizations 16 and 17 were carried out at high and low temperatures using a lower purity (95%) cyOEF for the same reaction time, with the higher temperature resulting in significant visual discoloration of the PEF polymer product, while the lower T showed no coloration but also poor conversion, outlining the effect of temperature (only qualitative results here). Polymerizations 18 and 19 show the effect of purity on the reaction. Identical conditions were applied to batches with different cyOEF purity (97% vs. 99%), giving a lower molecular weight brown polymer product and a higher molecular weight PEF product with much less discoloration, respectively.

[0134] Table entries 20-24 show intermediate results using various non-tin initiators under non-optimized conditions, which also demonstrate the feasibility of ROP for PEF using them. Sb2O3 is antimony(III) oxide, Bi2O3 is bismuth(III) oxide, FeAc is iron acetate, and Ca(MeO)2 is calcium methoxide.

[0135] It should be noted that the results and conclusions in this example apply to the specific reaction compositions evaluated under the specific reaction conditions carried out in the specific reactor system of this example, but that other reaction compositions, conditions and reactor systems may produce somewhat different results.

[0136] While various embodiments have been described for purposes of illustration, the above description is not intended to limit the scope of the present specification. Accordingly, various modifications, adaptations and alternatives may occur to those skilled in the art without departing from the spirit and scope of the present specification. One embodiment of the present invention will be described below, but the present invention is not limited thereto. [Invention 1] 1. A method for preparing a polyester polymer comprising the steps of: Ring-opening polymerization of cyclic oligomer compositions containing cyclic polyester oligomers having furan units wherein the ring-opening polymerization is carried out in the presence of a plasticizer. [Invention 2] The method according to claim 1, wherein the plasticizer is one or more selected from the group consisting of supercritical fluids, optionally substituted phenyl ethers, ionic liquids, optionally substituted xylenes, polyethers, and mixtures thereof. [Invention 3] 3. The method according to claim 2, wherein the supercritical fluid is carbon dioxide or the polyether is glyme, preferably tetraethylene glycol dimethyl ether. [Invention 4] The process according to any one of claims 1 to 3, wherein the polymerization step is carried out in the presence of a catalyst, preferably the catalyst is selected from cyclic dibutyltin compounds, Sb2O3, and SnOct2, more preferably the cyclic dibutyltin compound is 1,1,6,6-tetra-n-butyl-1,6-distanna-2,5,7,10-tetraoxyacyclodecane. [Invention 5] A polyester polymer composition obtainable, preferably obtained, by the process according to any one of claims 1 to 4, (i) a plasticizer selected from the group consisting of optionally substituted phenyl ethers, ionic liquids, optionally substituted xylenes, polyethers, and mixtures thereof; (ii) cyclic polyester oligomers having furan units, and (iii)(a) Structure [C1] JPEG0007551698000019.jpg1654 or (b) Structure [C2] JPEG0007551698000020.jpg1969 PBF polymer containing (wherein n is an integer from 10 to 100,000, preferably from 100 to 10,000). Either A composition comprising: [Invention 6] A cyclic polyester oligomer composition comprising a cyclic polyester oligomer having a furan unit, comprising the steps of: ·(I) Structure Y 1 in the presence of an optional catalyst and / or an optional organic base, in a ring-closing oligomerization step under conditions of reaction temperature and reaction time sufficient to obtain a cyclic polyester oligomer having furan units, 1 Or D 1 A step of reacting monomer component C 1 But the structure [C3] JPEG0007551698000021.jpg1676 wherein each group A is an optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; and l is an integer from 1 to 100, preferably from 2 to 50, most preferably from 3 to 25; R 1 =OH, OR, halogen or OA-OH; R=optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; R 2 =H or [C4] JPEG0007551698000022.jpg1738 is) Monomer component D 1 But the structure [5] JPEG0007551698000023.jpg1772 wherein A is an optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; each of the groups X is OH, halogen, or optionally substituted alkyloxy, phenoxy, or aryloxy; and when A is n-butyl, the group X is not OH. and a cyclic polyester oligomer having a furan unit, structure Y 1 but, Y 1 wherein m is an integer from 1 to 20, preferably from 2 to 15, and most preferably from 3 to 10. The process of or (II) Structure Y 2 in the presence of an optional catalyst and / or an optional organic base in a ring-closing oligomerization step under conditions of reaction temperature and reaction time sufficient to obtain a cyclic polyester oligomer having furan units, 2 Or D 2 A step of reacting monomer component C 2 But the structure [6] JPEG0007551698000024.jpg1672 wherein each group B is an optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl, l is an integer as defined above, and n' is an integer from 1 to 20, preferably from 2 to 10; R 3 =OH, OR, halogen or O-(BO) n’ -H, R=optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; R 4 =H or [7] JPEG0007551698000025.jpg1738 is) Monomer component D 2 But the structure [8] JPEG0007551698000026.jpg1682 wherein each group X is OH, halogen, or optionally substituted alkyloxy, phenoxy or aryloxy; each group B is optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; and n' is an integer as defined above. and a cyclic polyester oligomer having a furan unit, structure Y 2 but [9] JPEG0007551698000027.jpg2369 wherein each group B is an optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; n' is an integer as defined above; and m is an integer from 1 to 20, preferably from 2 to 15, most preferably from 3 to 10. A process that is Any of the steps of: a subsequent step (III) of separating and removing linear oligomeric polyester species having furan units from the cyclic oligomeric composition. Including, In the ring-closing oligomerization step, monomer component C1 or D1 or C 2 Or D 2 is carried out in the presence of a solvent, the solvent being selected from the group consisting of ionic liquids, optionally substituted naphtalenes, optionally substituted aromatic compounds, and mixtures thereof, and is optionally carried out in the presence of a zeolite to absorb the impurities onto the zeolite; a subsequent step (III) of separating and removing linear oligomeric polyester species having furan units from the cyclic oligomeric composition, comprising the following substeps: a sub-step of adding zeolite and absorbing the impurities on the zeolite; a sub-step of cooling the cyclic oligomer composition to precipitate cyclic polyester oligomers having furan units; a substep of adding an anti-solvent to precipitate the cyclic polyester oligomer having furan units; the sub-step of separating the zeolite having absorbed impurities from the cyclic oligomer composition; Contains one or more of 6. The method according to any one of claims 1 to 5, which is prepared by the method. [Invention 7] The method according to claim 6, wherein the method is any one of the following: (I) The monomer component is C 1 A is an optionally substituted linear, branched or cyclic alkyl; l is an integer from 3 to 25; and m is an integer from 3 to 10; or The monomer component is D 1 A is an optionally substituted linear, branched or cyclic alkyl, X is halogen or an optionally substituted alkyloxy or phenoxy, m is as previously defined in the present invention, and the structure of the cyclic polyester oligomer having furan units is Y 1 The structure is or (II) The monomer component is C 2 where B is an optionally substituted linear, branched or cyclic alkyl, l and m are integers as defined above, and n' is an integer from 2 to 10; or The monomer component is D 2 wherein X is OH, halogen, or optionally substituted alkyloxy, phenoxy, or aryloxy; B is an optionally substituted linear, branched, or cyclic alkyl, or phenyl; n′ and m are integers as previously defined in the present invention; and the structure of the cyclic polyester oligomer having furan units is Y 2 This is the structure. [Invention 8] The method according to claim 6 or 7, wherein the method is any one of the following: The monomer component is C 1 A is an optionally substituted linear, branched or cyclic C 1 From C 6 alkyl, l is an integer from 3 to 25, and m is an integer from 3 to 10; The monomer component is D 1 A is an optionally substituted linear, branched or cyclic C 1 From C 6 alkyl, X is halogen, or optionally substituted alkyloxy or phenoxy, and m is an integer as defined above; The monomer component is C 2 where B is an optionally substituted linear, branched or cyclic C 1 From C 6 alkyl, l and m are integers as defined above, and n' is an integer from 2 to 10; or The monomer component is D 2 X is halogen, or an optionally substituted alkyloxy, phenoxy or aryloxy; B is an optionally substituted linear, branched or cyclic C 1 From C 6 alkyl or phenyl, and n' and m are integers as defined in invention 2. [Invention 9] Monomer component is C 1 Or C 2 and the reaction temperature is from 100 to 350, preferably from 150 to 300, and most preferably from 180 to 280° C., and the reaction time is from 30 to 600, preferably from 40 to 400, and most preferably from 50 to 300 minutes; or Monomer component is D 1 Or D 2 the reaction temperature is from -10 to 150, preferably from -5 to 100, most preferably from 0 to 80°C, and the reaction time is from 5 to 240, preferably from 10 to 180, most preferably from 15 to 120 minutes; 9. The method according to any one of claims 6 to 8. [Invention 10] Monomer component C 1 However, certain structures [C10] JPEG0007551698000028.jpg1676 or monomer component D 1 However, certain structures [C11] JPEG0007551698000029.jpg1682 and a cyclic polyester oligomer having a furan unit, structure Y 1 However, for a particular structure Y 1 ’ [C12] JPEG0007551698000030.jpg2266 where: R 5 =OH, OR, halogen or O-CH 2 CH 2 -OH, R=optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; R 6 =H or [C13] JPEG0007551698000031.jpg1641 That is, A method according to any one of claims 6 to 9, comprising: X, l and m are defined as indicated in the invention(s). method. [Invention 11] Monomer component C 1 However, in the case of a specific structure C 1 ” [C14] JPEG0007551698000032.jpg1991 or monomer component D 1 However, for a specific structure D 1 ” [C15] JPEG0007551698000033.jpg1688 and a cyclic polyester oligomer having a furan unit, structure Y 1 However, for a particular structure Y 1 ” [C16] JPEG0007551698000034.jpg2482 and R 7 =OH, OR, halogen or O-CH 2 CH 2 CH 2 CH 2 -OH, R=optionally substituted linear, branched or cyclic alkyl, phenyl, aryl or alkylaryl; R 8 =H or [C17] JPEG0007551698000035.jpg1641 That is, A method according to any one of claims 6 to 10, comprising: X, l and m are defined as indicated in the invention(s). method. [Invention 12] An optional organic base E is present, the organic base E being a monoamine compound or a compound of the structure [C18] JPEG0007551698000036.jpg1957 (In the formula, the group R 9 From R 12 is hydrogen, optionally substituted alkyl, phenyl, aryl or alkaryl, and each of the groups R 9 From R 12 can optionally be bonded together in any cyclic organic base E by a single or double bond group as part of a cyclic substituent. 12. The method according to any one of claims 6 to 11, wherein the compound has the formula: [Invention 13] Any organic base E is present, and the organic base E is (i) Structure [C19] JPEG0007551698000037.jpg1926 DABCO, which has or (ii) Structure

[20] JPEG0007551698000038.jpg1932 DBU having 13. The method according to any one of claims 6 to 12, wherein DABCO or DBU is optionally used together with an alkylamine, more preferably triethylamine. [Invention 14] the absence or presence of any catalyst, the catalyst being a metal alkoxide or metal carboxylate, preferably one of tin, zinc, titanium or aluminium; or The optional organic base E is present in a stoichiometric ratio of 0.5 to 6, preferably 1 to 4, more preferably 2 to 3 moles per mole of all monomeric component species used as reactants in the process; 14. The method according to any one of claims 6 to 13. [Invention 15] 15. The method according to any one of claims 6 to 14, wherein step (III) of separating and removing linear oligomeric polyester species having furan units from the cyclic oligomer composition comprises one or more additional separation sub-steps of passing the mobile phase, which is the cyclic oligomer composition, through a stationary phase, selective precipitation, distillation, extraction, crystallization or combinations thereof.

Claims

1. 1. A polyester polymer composition comprising: (i) a plasticizer which is tetraethylene glycol dimethyl ether; (ii) cyclic polyester oligomers having furan units, and (iii) (a) Structure [Formula 1] or (b) Structure [chemical 2] PBF polymer comprising (wherein n is an integer from 10 to 100,000). Either A composition comprising:

2. 2. The polyester oligomer composition of claim 1, wherein n is an integer from 100 to 10,000.

3. The furan unit [C3] (wherein m is an integer from 1 to 20). The polyester oligomer composition according to claim 1 or 2,

4. The polyester oligomer composition of claim 3 , wherein m is an integer from 2 to 15.

5. The polyester oligomer composition of claim 3 , wherein m is an integer from 3 to 10.

6. The furan unit [C4] (wherein m is an integer from 1 to 20). The polyester oligomer composition according to claim 1 or 2,

7. 7. The polyester oligomer composition of claim 6, wherein m is an integer from 2 to 15.

8. 7. The polyester oligomer composition of claim 6, wherein m is an integer from 3 to 10.

Citation Information

Patent Citations

  • Process for preparing polyarylate resin containing furan ring

    JP2008308578A

  • Polyester resin, its producing method, composition for shaped article, and shaped article

    JP2009197110A

  • Process for preparing a polyester polymer composition comprising a polyester polymer having furan units, and the resulting polyester polymer composition and uses thereof

    JP2016510084A

  • Method for preparing cyclic oligomers and cyclic oligomers obtained thereby

    JP2016512811A

  • Polyester resin, method of producing the same, composition for molded article and molded article