Photoresponsive polymers

A photoresponsive polymer with an azomethine derivative structure addresses the limitations of azobenzene derivatives by providing enhanced toughness and color reproducibility, suitable for industrial applications.

JP7552133B2Active Publication Date: 2024-09-18KONICA MINOLTA INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020135376
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-07
Publication Date
2024-09-18
Estimated Expiration
2040-08-07

AI Technical Summary

Technical Problem

Azobenzene derivatives used in existing photoresponsive materials have low molecular weight, poor toughness, and yellow to orange coloring, limiting their application in industrial products like toners and adhesives due to insufficient fixability and color reproducibility.

Method used

A photoresponsive polymer containing a structural unit derived from an azomethine derivative, represented by a specific general formula, which becomes fluidized and reversibly non-fluidized by light irradiation, incorporating an aromatic hydrocarbon and aromatic heterocyclic structure with a hydrogen atom bonded to adjacent carbon atoms, enhancing toughness and color reproducibility.

Benefits of technology

The polymer achieves sufficient photoresponsiveness, improved fixing properties, and better color reproducibility, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007552133000060
    Figure 0007552133000060
  • Figure 0007552133000062
    Figure 0007552133000062
  • Figure 0007552133000061
    Figure 0007552133000061
Patent Text Reader

Abstract

To provide a photoresponsive polymer that sufficiently secures photoresponsiveness for being fluidized by light irradiation and reversibly non-fluidized, improves fixability, and further has good color reproducibility.SOLUTION: There is provided a photoresponsive polymer comprising a structural unit derived from an azomethine derivative represented by a general formula (1) in the figure, the photoresponsive polymer being fluidized by light irradiation and reversibly non-fluidized. In the formula, Z1 and Z2 are N or CH, provided that Z1≠Z2; R1 comprises an aromatic hydrocarbon structure; R2 comprises an aromatic heterocyclic structure; and a hydrogen atom is bonded to at least one carbon atom bonded adjacently to a carbon atom in the aromatic heterocyclic structure bonded to the Z2.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photoresponsive polymer that becomes fluid and reversibly non-fluid upon irradiation with light. [Background technology]

[0002] Photoresponsive materials are known as materials whose fluidity changes when irradiated with light. For example, the azobenzene compounds (azobenzene derivatives) described in Patent Documents 1 and 2 undergo a phase change in association with an isomerization reaction caused by irradiation with light.

[0003] It is believed that the change in molecular structure caused by this induces a phase transition from a solid state to a fluid state. In addition, if the material is exposed to light of a different wavelength, heated, or left in the dark at room temperature, a reverse reaction occurs and the material solidifies again. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-256155 A [Patent Document 2] International Publication No. 2013 / 081155 Summary of the Invention [Problem to be solved by the invention]

[0005] However, it has been found that the azobenzene derivatives described in Patent Documents 1 and 2 have a relatively low molecular weight, and therefore have low toughness as materials, and do not achieve sufficient fixability. In addition, it has been found that all of the azobenzene derivatives described in Patent Documents 1 and 2 are colored in yellow to orange, and therefore have a problem in that the desired color cannot be reproduced when applied to industrial products such as toners and adhesives.

[0006] Therefore, an object of the present invention is to provide a photoresponsive polymer that can be fluidized by irradiation with light and reversibly non-fluidized while having sufficient photoresponsiveness, improved fixability, and excellent color reproducibility. [Means for solving the problem]

[0007] The present inventors have conducted extensive research in view of the above problems. As a result, they have discovered a photoresponsive polymer that contains a structural unit derived from an azomethine derivative represented by the following general formula (1), which is fluidized and reversibly non-fluidized upon irradiation with light:

[0008] [ka]

[0009] The inventors have found that the above-mentioned problems can be solved by providing a compound in which Z1 and Z2 are N or CH, with the proviso that Z1 ≠ Z2, R1 contains an aromatic hydrocarbon structure, R2 contains an aromatic heterocyclic structure, and a hydrogen atom is bonded to at least one carbon atom that is bonded adjacent to a carbon atom in the aromatic heterocyclic structure that is bonded to Z2, and have thus completed the present invention. Effect of the Invention

[0010] According to the present invention, it is possible to provide a photoresponsive polymer that sufficiently ensures photoresponsiveness, in which the polymer is fluidized and reversibly non-fluidized upon irradiation with light, has improved fixability, and exhibits good color reproducibility. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram showing an image forming apparatus 100 used in an image forming method according to an embodiment of the present invention. [Diagram 2] 2 is a schematic configuration diagram of an irradiation unit 40 in the image forming apparatus 100. FIG. [Diagram 3] FIG. 2 is a schematic diagram of an apparatus used in the photoresponsive adhesion test of the Examples for measuring the change in adhesiveness of a polymer due to light irradiation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Preferred embodiments of the present invention will be described below. In this specification, the range "X to Y" means "X or more and Y or less." Furthermore, in this specification, unless otherwise specified, operations and measurements of physical properties are performed under the conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.

[0013] <Photoresponsive polymer> One embodiment of the present invention relates to a photoresponsive polymer that contains a structural unit derived from an azomethine derivative represented by the following general formula (1), and that is fluidized and reversibly non-fluidized upon irradiation with light:

[0014] [ka]

[0015] In the formula, Z1 and Z2 are N or CH, with the proviso that Z1≠Z2, R1 includes an aromatic hydrocarbon structure, R2 includes an aromatic heterocyclic structure, and a hydrogen atom is bonded to at least one carbon atom adjacent to the carbon atom in the aromatic heterocyclic structure bonded to Z2.

[0016] Here, the above general formula (1) will be explained using one of the following specific examples:

[0017] [ka]

[0018] As shown in the above, Z2 is bonded to a carbon atom in the aromatic heterocyclic structure, and at least one of the bonding sites adjacent to the carbon atom (i.e., the bonding site indicated by *) is a carbon atom (two carbon atoms in the above specific example), and a hydrogen atom (two hydrogen atoms in the above specific example) is bonded to the carbon atom (two carbon atoms in the above specific example). In this specification, the "photoresponsive polymer" may also be simply referred to as a "polymer". By using a photoresponsive polymer containing a structural unit derived from such an azomethine derivative, it is possible to provide a photoresponsive polymer that is fluidized by light irradiation and reversibly non-fluidized, has sufficient photoresponsiveness, improves fixability, and has good color reproducibility.

[0019] In this specification, "fluidized by light irradiation and reversibly non-fluidized" refers to a state in which the polymer changes from a non-fluid state to a fluid state by light irradiation and then returns to a non-fluid state. That is, the polymer of the present invention is in a non-fluid solid state at room temperature and normal pressure when not irradiated with light, and softens and changes to a fluid state by light irradiation. When the light irradiation is stopped and the polymer is left in a dark place at room temperature or under visible light irradiation, or is heated, the polymer returns to a non-fluid solid state. In this specification, "fluid state" refers to a state in which the polymer is deformed by a small external force.

[0020] The mechanism by which such technical effects are achieved is presumed to be as follows. However, the technical scope of the present invention is not limited to such a mechanism. That is, the conventional azobenzene compound having a long alkyl chain at the end is a material that absorbs light and softens from a solid state (photo-induced phase transition), and it is believed that this photo-induced phase transition occurs when the crystal structure collapses due to cis-trans isomerization. The azobenzene compounds described in Patent Documents 1 and 2 undergo a phase change in association with an isomerization reaction caused by light irradiation, but the present inventors have found that such azobenzene compounds have the problem of low toughness as a material. In addition, it is possible to obtain a material having n-π isomerization in the visible light region. * It has been found that, since it exhibits strong absorption due to transition and is colored orange, it is difficult to reproduce the desired color when applied to industrial products.

[0021] In the present invention, a polymer containing a structural unit derived from an azomethine derivative is used. This makes it possible to provide a polymer that is fluidized by light irradiation, reversibly non-fluidized, has high toughness, and is not significantly colored. Here, in a polymer containing a structural unit derived from an azomethine derivative, it is considered that the azomethine derivative absorbs light, and the heat energy released during the photoexcitation / deactivation process is transmitted to the repeating unit (structural unit) to which it is bonded (photothermal conversion), thereby inducing a reversible fluidization / non-fluidization phenomenon. In particular, if the polymer is a trans isomer, in addition to the above-mentioned photothermal conversion, trans-cis photoisomerization is more likely to occur by light irradiation, and a cis isomer with a low Tg is more likely to be produced. When a non-fluid trans isomer (E) is irradiated with light and isomerized to a cis isomer (Z), it is considered that the ordered structure is broken as many trans isomers (E) change to cis isomers (Z), which induces a phase transition change, i.e., a fluidization phenomenon. It is also considered that the return of the cis isomer (Z) to the trans isomer (E) causes an ordered structure to be formed again, which induces a non-fluidization phenomenon. This is believed to induce more efficient fluidization / defluidization phenomena. Therefore, in order to induce the fluidization phenomenon, it is considered preferable for many trans isomers (E) to be isomerized to cis isomers (Z). However, azomethine derivatives generally have a faster cis-trans isomerization rate than azobenzene derivatives, and it was predicted that azomethine derivatives with unsubstituted benzene rings attached to both ends of the C=N bond would be disadvantageous in inducing fluidization.

[0022] In the present invention, the polymer containing the azomethine derivative is made to have an aromatic hydrocarbon group and an aromatic heterocyclic group at both ends of the C=N moiety, and the polymer is made to have a cyclic structure in which a hydrogen atom is bonded to at least one of the carbons adjacent to the carbon bonded to the C=N moiety in the heterocycle, and it is possible to induce fluidization accompanying the photoisomerization reaction. This is believed to be because the introduction of the heterocycle reduces the cis-to-trans reaction rate, and further, in the cis form, the hydrogen atom on the carbon adjacent to the carbon bonded to the C=N moiety of the heterocycle and the aromatic hydrocarbon group form a CH-π interaction, stabilizing the cis form and producing more cis forms.

[0023] In one embodiment of the present invention, the photoresponsive polymer has a structural unit derived from the azomethine derivative represented by the general formula (1) having a polymerizable group.

[0024] In one embodiment of the present invention, the photoresponsive polymer has a structural unit derived from the azomethine derivative represented by the general formula (1) as a side chain in a repeating unit of the photoresponsive polymer.

[0025] In one embodiment of the present invention, the photoresponsive polymer contains at least one selected from the group consisting of a structure derived from a (meth)acrylic acid ester, a structure derived from an olefin, and a structure derived from a vinyl ester. In one embodiment of the present invention, the photoresponsive polymer contains a structure derived from a (meth)acrylic acid ester. This embodiment has the technical effect of facilitating polymerization.

[0026] In one embodiment of the present invention, the photoresponsive polymer has the general formula (2):

[0027] [ka]

[0028] The structural unit represented by In the general formula (2), r1 is a hydrogen atom or a methyl group; A is represented by general formula (1-1) to general formula (1-4):

[0029] [ka]

[0030] [ka]

[0031] [ka]

[0032] [ka]

[0033] Either * represents a bonding point, G is a divalent group, and R1, Z1, Z2, and R2 are the same as defined in the general formula (1). By adopting such an embodiment, the intended effect of the present invention can be efficiently achieved.

[0034] Here, the above general formula (1-2) will be explained using one of the following specific examples. Representatively, the formula is as follows:

[0035] [ka]

[0036] "R1-", "-Z1=Z2-", and "-R2" are as explained above, and G as a divalent group is an oxyalkylene group having 10 carbon atoms, which serves as the bonding point to the structural unit derived from a (meth)acrylic acid ester.

[0037] In one embodiment of the present invention, all of the atoms adjacent to and bonded to the carbon atom in the aromatic heterocyclic structure bonded to Z2 are carbon atoms, and all of the carbon atoms are bonded to a hydrogen atom. By adopting such an embodiment, the desired effects of the present invention, particularly fixability, are significantly improved.

[0038] General formulae (1) and (2) will be further explained below.

[0039] (Z1 and Z2) In one embodiment of the present invention, Z1 and Z2 are N or CH, as described above, with the proviso that Z1 ≠ Z2.

[0040] (R1 and R2) In one embodiment of the present invention, R1 comprises an aromatic hydrocarbon structure and R2 comprises an aromatic heterocyclic structure, as described above.

[0041] In one embodiment of the present invention, the aromatic hydrocarbon structure is not particularly limited, but is preferably an aromatic hydrocarbon having 6 to 30 carbon atoms, for example, derived from a structure such as benzene, naphthalene, anthracene, phenanthone, pyrene, biphenyl, etc. Among them, benzene, naphthalene, and phenanthrene are preferred from the viewpoints that packing between molecular chains is easily expressed, and that when trans-cis isomerization occurs, they exhibit high thermal motion and are easily induced to induce a fluidization phenomenon.

[0042] In one embodiment of the present invention, the aromatic hydrocarbon structure has a polycyclic structure such as naphthalene, anthracene, phenanthone, or pyrene.

[0043] In one embodiment of the present invention, the aromatic heterocyclic structure is not particularly limited, but preferably has a carbon number of 2 to 30. In addition, those having high electron donating properties are preferred, and examples thereof include those derived from structures such as thiophene, pyrrole, pyrazole, imidazole, pyridine, pyrimidine, pyrazine, triazine, benzothiophene, benzimidazole, indole, isoindole, quinoline, isoquinoline, quinazoline, quinoxaline, naphthyridine, acridine, a carbazole group, and dibenzothiophene.

[0044] In one embodiment of the present invention, when the photoresponsive polymer contains a structural unit represented by the general formula (2) and A is represented by the general formula (1-1) or (1-2), the aromatic hydrocarbon structure represented by R1 is a divalent group. That is, the aromatic hydrocarbon structure is an arylene group having 6 to 30 carbon atoms, such as a phenylene group, a naphthalenylene group, an anthracenylene group, a phenanthrenylene group, or a pyrenylene group. In one embodiment of the present invention, when the photoresponsive polymer contains a structural unit represented by the general formula (2) and A is represented by the general formula (1-3) or (1-4), the aromatic hydrocarbon structure represented by R1 is a monovalent group. That is, the aromatic hydrocarbon structure is an aryl group having 6 to 30 carbon atoms, such as a phenyl group, a biphenyl group, a naphthyl group, an anthracenyl group, a phenanthrenyl group, or a pyrenyl group.

[0045] In one embodiment of the present invention, when the photoresponsive polymer contains a structural unit represented by the general formula (2) and A is represented by the general formula (1-1) or (1-2), the aromatic heterocyclic structure represented by R2 is a monovalent group. That is, the aromatic heterocyclic structure is, for example, a thienyl group, a furanyl group, a pyrrolyl group, a pyrazolyl group, an imidazolyl group, a pyridyl group, a pyrimidinyl group, a pyrazinyl group, a triazinyl group, a benzothienyl group, a benzimidazolyl group, an indolyl group, an isoindolyl group, a quinolinyl group, an isoquinolinyl group, a quinazolinyl group, a quinoxalinyl group, a naphthyridinyl group, an acridinyl group, a carbazolyl group, a dibenzothienyl group, or the like. In one embodiment of the present invention, when the photoresponsive polymer contains a structural unit represented by the general formula (2) and A is represented by the general formula (1-3) or (1-4), the aromatic heterocyclic structure represented by R2 is a divalent group. That is, examples of the aromatic heterocyclic structure include divalent groups corresponding to the groups exemplified as the monovalent aromatic heterocyclic group above.

[0046] In one embodiment of the present invention, the aromatic hydrocarbon structure or aromatic heterocyclic structure may each have a substituent. The substituent is not particularly limited, but examples thereof include a halogen atom, a cyano group, a nitro group, an amino group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, an alkylamino group having 1 to 10 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms. Preferred are a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 19 carbon atoms, and an alkoxycarbonyl group having 2 to 19 carbon atoms. In this case, it is preferable that at least one of the above-mentioned substituents is a halogen atom, a cyano group, a nitro group, an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, a dialkylamino group having 2 to 10 carbon atoms, an acyl group having 2 to 18 carbon atoms, or an alkoxycarbonyl group having 2 to 18 carbon atoms. It is considered that such a structure makes it easier for cis-trans isomerization to proceed and makes it easier for fluidization to occur. Among these, it is more preferable that the alkyl group having 1 to 18 carbon atoms, the alkoxy group having 1 to 18 carbon atoms, or the dialkylamino group having 2 to 10 carbon atoms have high thermal mobility.

[0047] As for the number of carbon atoms of the substituent, the alkyl group is more preferably an alkyl group having 1 to 12 carbon atoms, and even more preferably an alkyl group having 4 to 8 carbon atoms. The alkoxy group is more preferably an alkoxy group having 1 to 12 carbon atoms, and even more preferably an alkoxy group having 4 to 8 carbon atoms. The dialkylamino group is more preferably a dialkylamino group having 2 to 8 carbon atoms, and even more preferably a dialkylamino group having 4 to 6 carbon atoms. The acyl group is more preferably an acyl group having 2 to 13 carbon atoms, and even more preferably an acyl group having 5 to 13 carbon atoms. The alkoxycarbonyl group is more preferably an alkoxycarbonyl group having 2 to 13 carbon atoms, and even more preferably an alkoxycarbonyl group having 5 to 13 carbon atoms. In this way, by introducing a long-chain substituent, the crystal is easily broken, the light melting property is improved, and the fixability is improved.

[0048] Examples of the alkyl group having 1 to 18 carbon atoms are not particularly limited, and include linear alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an isobutyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, an n-undecyl group, an n-dodecyl group, an n-tridecyl group, an n-tetradecyl group, an n-pentadecyl group, and an n-hexadecyl group; an isopropyl group, a sec-butyl group, a t Examples of branched alkyl groups include t-butyl, 1-methylpentyl, 4-methyl-2-pentyl, 3,3-dimethylbutyl, 2-ethylbutyl, 1-methylhexyl, t-octyl, 1-methylheptyl, 2-ethylhexyl, 2-propylpentyl, 2,2-dimethylheptyl, 2,6-dimethyl-4-heptyl, 3,5,5-trimethylhexyl, 1-methyldecyl, and 1-hexylheptyl groups.

[0049] Examples of alkoxy groups having 1 to 18 carbon atoms include linear alkoxy groups such as methoxy group, ethoxy group, n-propoxy group, n-butoxy group, n-hexyloxy group, n-heptyloxy group, n-octyloxy group, n-nonyloxy group, n-decyloxy group, n-undecyloxy group, n-dodecyloxy group, n-tridecyloxy group, n-tetradecyloxy group, n-pentadecyloxy group, and n-hexadecyloxy group; 1-methylpentyloxy group, 4-methyl-2-methylpentyloxy group, and 5-methyl-2-methylpentyloxy group. Examples of branched alkoxy groups include t-pentyloxy group, 3,3-dimethylbutyloxy group, 2-ethylbutyloxy group, 1-methylhexyloxy group, t-octyloxy group, 1-methylheptyloxy group, 2-ethylhexyloxy group, 2-propylpentyloxy group, 2,2-dimethylheptyloxy group, 2,6-dimethyl-4-heptyloxy group, 3,5,5-trimethylhexyloxy group, 1-methyldecyloxy group, and 1-hexylheptyloxy group.

[0050] Examples of alkylamino groups having 1 to 10 carbon atoms include methylamino groups, ethylamino groups, n-propylamino groups, n-butylamino groups, isobutylamino groups, n-hexylamino groups, n-heptylamino groups, n-octylamino groups, n-nonylamino groups, and n-decylamino groups.

[0051] Examples of the dialkylamino group having 2 to 10 carbon atoms include a dimethylamino group, a diethylamino group, a di-n-propylamino group, a di-n-butylamino group, a di-isobutylamino group, and a methylethylamino group.

[0052] Examples of the acyl group having 2 to 19 carbon atoms include saturated or unsaturated straight-chain or branched-chain acyl groups, such as an acetyl group, a propanoyl group (propionyl group), a butanoyl group (butyryl group), an isobutanoyl group (isobutyryl group), a pentanoyl group (valeryl group), an isopentanoyl group (isovaleryl group), a sec-pentanoyl group (2-methylbutyryl group), a t-pentanoyl group (pivalyl group), and the like. Examples of such groups include hexanoyl, heptanoyl, octanoyl, t-octanoyl (2,2-dimethylhexanoyl), 2-ethylhexanoyl, nonanoyl, isononanoyl, decanoyl, isodecanoyl, undecanoyl, lauroyl, myristoyl, palmitoyl, stearoyl, behenoyl, undecylenoyl, and oleoyl groups.

[0053] Examples of the alkoxycarbonyl group having 2 to 19 carbon atoms include linear or branched alkoxycarbonyl groups such as a methoxycarbonyl group, an ethoxycarbonyl group, an n-butoxycarbonyl group, an n-hexyloxycarbonyl group, an n-heptyloxycarbonyl group, an n-octyloxycarbonyl group, an n-nonyloxycarbonyl group, an n-decyloxycarbonyl group, an n-undecyloxycarbonyl group, an n-dodecyloxycarbonyl group, an n-tridecyloxycarbonyl group, an n-tetradecyloxycarbonyl group, an n-pentadecyloxycarbonyl group, and an n-hexadecyloxycarbonyl group; Examples of branched alkoxycarbonyl groups include branched alkoxycarbonyl groups such as a 4-methyl-2-pentyloxycarbonyl group, a 3,3-dimethylbutyloxycarbonyl group, a 2-ethylbutyloxycarbonyl group, a 1-methylhexyloxycarbonyl group, a t-octyloxycarbonyl group, a 1-methylheptyloxycarbonyl group, a 2-ethylhexyloxycarbonyl group, a 2-propylpentyloxycarbonyl group, a 2,2-dimethylheptyloxycarbonyl group, a 2,6-dimethyl-4-heptyloxycarbonyl group, a 3,5,5-trimethylhexyloxycarbonyl group, a 1-methyldecyloxycarbonyl group, and a 1-hexylheptyloxycarbonyl group.

[0054] (r1) In one embodiment of the present invention, as described above, r1 is a hydrogen atom or a methyl group. In this embodiment, r1 is preferably a hydrogen atom from the viewpoint of high fluidity and excellent fixability upon trans-cis isomerization.

[0055] (A) In one embodiment of the present invention, A is, as described above,

[0056] [ka]

[0057] [ka]

[0058] [ka]

[0059] [ka]

[0060] wherein * represents a bonding point, G is a divalent group, and R1, Z1, Z2, and R2 are as defined in general formula (1) above.

[0061] In one embodiment of the present invention, the G is not particularly limited as long as it is a divalent group, and is an alkylene group or an oxyalkylene group having 1 to 18 carbon atoms. This embodiment provides high thermal mobility and excellent light melting properties. In one embodiment of the present invention, the G is an alkylene group having 2 to 16 carbon atoms, an alkylene group having 3 to 14 carbon atoms, or an alkylene group having 4 to 12 carbon atoms. In one embodiment of the present invention, the oxyalkylene group is -(EO) nE is an alkylene group having 1 to 18 carbon atoms (2 to 16 carbon atoms, 3 to 14 carbon atoms, or 4 to 12 carbon atoms), and n is 1 to 3, and preferably 1.

[0062] In one embodiment of the present invention, examples of the alkylene group having 1 to 18 carbon atoms are preferably groups in which one hydrogen atom has been removed from the groups explained as examples of the alkyl group having 1 to 18 carbon atoms.

[0063] (Z2-R2) In one embodiment of the present invention, when A is represented by the general formula (1-1) or the general formula (1-2), the "Z2-R2" structure is as follows:

[0064] [ka]

[0065] wherein at least two of X, Y, P and Q are carbon atoms, and the rest are nitrogen, sulfur or oxygen atoms, provided that at least one of X and Y is a carbon atom, and R a , R b , R c and R d is an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, or a hydrogen atom, provided that R a and R b At least one of R is a hydrogen atom. a and R b And R c and R d may each independently form a condensed ring with a benzene ring or the like.

[0066] In one embodiment of the present invention, it is preferred that at least one of P and Q is a nitrogen atom, and more preferred that both of P and Q are nitrogen atoms.

[0067] In one embodiment of the present invention, R a and R bIt is preferable that each of these is a hydrogen atom.

[0068] In one embodiment of the present invention, R c and R d At least one of the groups is an alkyl group having 1 to 18 carbon atoms, an alkyl group having 1 to 12 carbon atoms, an alkyl group having 3 to 8 carbon atoms, or an alkyl group having 4 to 6 carbon atoms. In particular, by using an alkyl group having 4 or more carbon atoms, the desired effect of the present invention (particularly the effect of improving fixability when used in a toner) can be efficiently achieved.

[0069] (-R2-Z2) In one embodiment of the present invention, when A is represented by the general formula (1-3) or the general formula (1-4), the "-R2-Z2" structure is as follows:

[0070] [ka]

[0071] wherein at least two of X, Y, P and Q are carbon atoms, and the rest are nitrogen, sulfur or oxygen atoms, provided that at least one of X and Y is a carbon atom, and R a and R b is an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, or a hydrogen atom, provided that R a and R b At least one of R is a hydrogen atom. c and R d One of these is a structure derived from a polymerizable group such as a structural unit derived from a (meth)acrylic acid ester or a single bond bonded to the above G, and the other is an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, or a hydrogen atom.

[0072] In one embodiment of the present invention, it is preferred that at least one of P and Q is a nitrogen atom, and more preferred that both of P and Q are nitrogen atoms.

[0073] In one embodiment of the present invention, R a and R b It is preferable that each of these is a hydrogen atom.

[0074] In one embodiment of the present invention, R c and R d It is preferable that one of these is a structure derived from a polymerizable group such as a structural unit derived from a (meth)acrylic acid ester or a single bond bonding to G, and the other is a hydrogen atom.

[0075] By adopting such an embodiment, the desired effects of the present invention (particularly the effect of improving fixability) can be efficiently achieved.

[0076] In one embodiment of the present invention, A is represented by the general formula (1-1) or the general formula (1-2), and the "Z2-R2" structure is as follows:

[0077] [ka]

[0078] wherein at least two of X, Y, P and Q are carbon atoms, and the rest are nitrogen, sulfur or oxygen atoms, provided that at least one of X and Y is a carbon atom, and R a , R b , R c and R d is R a , R b , R c and R d are present according to the valences of X, Y, P, and Q, each independently represents an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, or a hydrogen atom, provided that R a and R b At least one of the atoms bonded to the carbon atom is a hydrogen atom, and R a and R b And R c and R dmay each independently form a condensed ring. By adopting such an embodiment, the intended effects of the present invention (particularly the effect of improving fixability) can be efficiently achieved.

[0079] In one embodiment of the present invention, the P and the Q are nitrogen atoms, the X and the Y are carbon atoms, and the R a and the above R b All of these are hydrogen atoms.

[0080] In one embodiment of the present invention, the P and the Q are nitrogen atoms, the X and the Y are carbon atoms, and the R a and the above R b are all hydrogen atoms, c and R d At least one of (any one of) is an alkyl group having a carbon number of 4 or more. By adopting such an embodiment, the desired effects of the present invention (particularly the effect of improving fixability) can be efficiently achieved.

[0081] In one embodiment of the present invention, A is represented by the general formula (1-3) or the general formula (1-4), and the “-R2-Z2” structure is as follows:

[0082] [ka]

[0083] wherein at least two of X, Y, P and Q are carbon atoms, and the rest are nitrogen, sulfur or oxygen atoms, provided that at least one of X and Y is a carbon atom, and R a and R b When present according to the valences of X, Y, P, and Q, each independently represents an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, or a hydrogen atom, provided that R a and R b At least one of the atoms bonded to the carbon atom is a hydrogen atom, and R c and R dOne of the groups is a structure derived from a polymerizable group or a single bond bonded to G, and the other group, when present according to the valence, is an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms, or a hydrogen atom. By adopting such an embodiment, the desired effects of the present invention (particularly the effect of improving fixability) can be efficiently achieved.

[0084] In one embodiment of the present invention, the P and the Q are nitrogen atoms, the X and the Y are carbon atoms, and the R a and the above R b are all hydrogen atoms, c and the above R d one of these is a structure derived from a polymerizable group or a single bond bonded to G, and the other is absent. By adopting such an embodiment, the desired effects of the present invention (particularly the effect of improving fixability) can be efficiently achieved.

[0085] <Method for producing photoresponsive polymer> One embodiment of the present invention relates to a photoresponsive polymer that contains a structural unit derived from an azomethine derivative represented by the following general formula (1), and that is fluidized and reversibly non-fluidized upon irradiation with light:

[0086] [ka]

[0087] The present invention provides a method for producing a compound in which Z1 and Z2 are N or CH, with the proviso that Z1≠Z2, R1 comprises an aromatic hydrocarbon structure, R2 comprises an aromatic heterocyclic structure, and a hydrogen atom is bonded to at least one carbon atom bonded adjacent to a carbon atom in the aromatic heterocyclic structure bonded to Z2.

[0088] In one embodiment of the present invention, the photoresponsive polymer can be obtained by preparing an azomethine derivative (monomer) having a polymerizable group and represented by general formula (1), and polymerizing it by a conventionally known method.

[0089] In one embodiment of the invention, the photoresponsive polymer has the following formula:

[0090] [ka]

[0091] [ka]

[0092] [ka]

[0093] [ka]

[0094] wherein J is a polymerizable group, and G, R1, Z1, Z2 and R2 are the same as defined in the general formula (1), and then polymerizing the same by a conventional method.

[0095] (Specific Example of Method for Preparing Azomethine Derivative Having Polymerizable Group) The azomethine derivative having a polymerizable group can be prepared by preparing an azomethine derivative represented by the general formula (1) and introducing a polymerizable group therein.

[0096] For example, in the case of preparing an azomethine derivative containing a pyrazole ring, in the first step, an aniline derivative is reacted with a pyrazole-carbaldehyde derivative as a compound having a pyrazole ring. In this case, if either the raw material aniline derivative or the pyrazole-carbaldehyde derivative has an OH group as a substituent, a polymerizable group can be easily introduced at the position of the OH group.

[0097] Specifically, 4-hydroxyaniline and 1-methyl-1H-pyrazole-4-carbaldehyde are treated (heated to reflux to react) in a solvent such as methanol (MeOH) or ethanol (EtOH), the reaction liquid is filtered, the resulting powder is washed with cooled ethanol, and recrystallized from methanol / ethanol to obtain the desired compound.

[0098] [ka]

[0099] Then, in the second step, a polymerizable group is introduced into the intermediate A. The method for introducing the polymerizable group is not particularly limited. For example, a linker, -OC 10 H 20 When introducing -, use a halogenated alcohol compound such as Cl-C 10 H 20 By reacting with -OH, intermediate B shown below is obtained.

[0100] The reaction conditions are not particularly limited, but for example, the reaction is preferably carried out in a solvent such as dimethylformamide (DMF) in the presence of potassium carbonate and potassium iodide at a temperature preferably within the range of 10° C. to 150° C., more preferably within the range of 50° C. to 140° C., and even more preferably within the range of 80° C. to 130° C. The order of addition of potassium carbonate and potassium iodide is preferably potassium carbonate first, and after potassium carbonate is added, stirring is preferably carried out within the range of 0° C. to 100° C., more preferably within the range of 0° C. to 60° C., and even more preferably within the range of 0° C. to 40° C. before adding potassium iodide.

[0101] [ka]

[0102] Then, in the third step, the intermediate B is reacted with a compound for forming a polymerizable group, for example, an acrylate or a methacrylate. As a result, the photoresponsive polymer contains a structural unit derived from a (meth)acrylate ester. In this case, the reaction conditions are not particularly limited. For example, it is preferable to carry out the reaction in a known organic solvent in the presence of a tertiary amine such as triethylamine or triethanolamine. Preferably, while keeping the mixed solution containing the intermediate B, the tertiary amine, and the solvent at 0 to 10°C, a compound for forming a polymerizable group, such as an acrylate or a methacrylate, is dropped into the mixed solution and mixed. Then, the mixed solution is reacted at room temperature for about 5 to 10 hours, for example, to obtain an azomethine derivative having a polymerizable group.

[0103] [ka]

[0104] In the first step, by changing the raw material used to another compound, it is possible to obtain an azomethine derivative having a desired substituent. Similarly, by changing the raw material aniline derivative to another aromatic hydrocarbon compound or aromatic heterocyclic compound having an amino group, it is possible to obtain an azomethine derivative having a different structure.

[0105] In addition, groups having polymerizable groups with different structures can be introduced by changing the compounds added in the second and third steps. A person skilled in the art can synthesize an azomethine derivative having a desired polymerizable group by appropriately making the above changes and selecting appropriate reaction conditions.

[0106] Furthermore, by appropriately selecting the raw materials used in the first step, it is also possible to introduce a polymerizable group into intermediate A without carrying out the second step.

[0107] One embodiment of the present invention relates to a photoresponsive polymer that contains a structural unit derived from an azomethine derivative represented by the following general formula (1), and that is fluidized and reversibly non-fluidized upon irradiation with light:

[0108] [ka]

[0109] Z1 and Z2 are N or CH, with the proviso that Z1≠Z2, R1 includes an aromatic hydrocarbon structure, R2 includes an aromatic heterocyclic structure, and a hydrogen atom is bonded to at least one carbon atom adjacent to a carbon atom in the aromatic heterocyclic structure bonded to Z2, except for azomethine derivatives (specifically disclosed in Tables 1 to 8) having the following structure: A polymer that contains a structural unit derived from an azomethine derivative having a polymerizable group and is reversibly fluidized / non-fluidized by light irradiation, and is represented by the following chemical formula (1): 10 A polymer represented in Table 1 below:

[0110] [ka]

[0111] Here, the "group having a polymerizable group" in Table 1 is a group represented by any one of the following formulas (i) to (iv), and R1 to R 10 Among these, the group corresponds to the group shown in "Polymerizable group position" in Table 1:

[0112] [ka]

[0113] In the formulas (i) to (iv), A1 is a hydrogen atom or a methyl group, A2 is an alkylene group having 1 to 18 carbon atoms, and A3 is an alkylene group having 1 to 6 carbon atoms.

[0114] A block copolymer that contains a polymer block containing a structural unit derived from an azomethine derivative having a polymerizable group represented by the above chemical formula (1), and that is reversibly fluidized / non-fluidized by light irradiation, wherein X, Y, Z1, Z2, R1 to R 10is a polymer represented by the following Table 2 (the group having a polymerizable group is the same as above): A polymer having a structural unit represented by the following general formula (1), which has a structural unit shown in Table 3, and which is fluidized and reversibly non-fluidized by light irradiation (r1 is a hydrogen atom or a methyl group, and r2 is an alkylene group having 1 to 18 carbon atoms):

[0115] [ka]

[0116] A is a group having an azomethine structure represented by the following general formula (2):

[0117] [ka]

[0118] [Table 1]

[0119] [Table 2]

[0120] [Table 3]

[0121] [Table 4]

[0122] [Table 5]

[0123] [Table 6]

[0124] [Table 7]

[0125] [Table 8]

[0126] [Table 9]

[0127] [Table 10]

[0128] [Table 11]

[0129] [Table 12]

[0130] (Other structural units) In one embodiment of the present invention, the photoresponsive polymer may contain a structural unit (another structural unit) other than the structural unit derived from the azomethine derivative represented by the general formula (1). When the photoresponsive polymer is a copolymer containing another structural unit, the arrangement of the repeating units of the copolymer is not particularly limited, and may be any of a random copolymer, a block copolymer, and an alternating copolymer.

[0131] The other structural units preferably do not contain structural units derived from the azomethine derivative represented by the general formula (1), and are more preferably structural units constituting a thermoplastic resin that is softened by heating.

[0132] The other structural unit is preferably one having a vinyl-based polymerizable group, since the copolymer can be easily synthesized. That is, in one embodiment of the present invention, the photoresponsive polymer further contains another structural unit derived from a monomer having a vinyl-based polymerizable group. Specifically, for example, a styrene derivative, a (meth)acrylic acid derivative, an olefin derivative, a vinyl ester derivative, a vinyl ether derivative, a vinyl ketone derivative, or the like is used, and the structural unit is preferably derived from a styrene derivative, a (meth)acrylic acid derivative, or an olefin derivative. That is, in one embodiment of the present invention, the monomer having a vinyl-based polymerizable group is at least one selected from the group consisting of a styrene derivative, a (meth)acrylic acid derivative, and an olefin derivative. By adopting such an embodiment, the desired effect of the present invention can be efficiently achieved.

[0133] Examples of styrene derivatives include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-phenylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, pt-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, and pn-dodecylstyrene.

[0134] Examples of (meth)acrylic acid derivatives include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylaminoethyl (meth)acrylate.

[0135] Examples of the olefin derivative include ethylene, propylene, n-butylene, isobutylene, n-pentene, 3-methyl-1-pentene, etc. The olefin derivative may be linear or branched, and the number of carbon chains is not particularly limited.

[0136] Examples of the vinyl ester derivatives include vinyl propionate, vinyl acetate, vinyl benzoate, etc. Examples of the vinyl ether derivatives include vinyl methyl ether, vinyl ethyl ether, etc. Examples of the vinyl ketone derivatives include vinyl methyl ketone, vinyl ethyl ketone, vinyl hexyl ketone, etc.

[0137] The content of the other structural units in the polymer is not particularly limited and can be appropriately selected, but is preferably 70% by mass or less, and more preferably 40% by mass or less, relative to 100% by mass of the total amount of all structural units constituting the polymer. In one embodiment of the present invention, the content of the other structural units in the polymer can be 5% by mass or more, or 15% by mass or more.

[0138] In one embodiment of the present invention, the number average molecular weight Mn of the photoresponsive polymer is not particularly limited, but is 3000 or more, 3500 or more, 4000 or more, 5000 or more, or 10000 or more. In one embodiment of the present invention, the number average molecular weight Mn of the photoresponsive polymer is not particularly limited, but is 100000 or less, 70000 or less, 50000 or less, 40000 or less, or 30000 or less. If the number average molecular weight of the polymer is 3000 or more, it is preferable because it has excellent toughness and when used as a toner, a toner image with excellent fixability can be more easily obtained. In addition, if the number average molecular weight is 100000 or less, it is preferable because the efficiency of isomerization and softening and melting is high.

[0139] The number average molecular weight of the polymer of the present invention can be measured by gel permeation chromatography (GPC), specifically, by the method described in the Examples below.

[0140] (Method of preparing polymer) The method for synthesizing the polymer of the present invention is not particularly limited, and a method of polymerizing an azomethine derivative represented by general formula (1) having a polymerizable group as a monomer using a known polymerization initiator, such as anionic polymerization, cationic polymerization, living radical polymerization, etc., may be used. A known chain transfer agent may be used as necessary.

[0141] As the polymerization initiator, for example, the following azo-based or diazo-based polymerization initiators and peroxide-based polymerization initiators can be used.

[0142] Examples of the azo or diazo polymerization initiator include azobisisobutyronitrile (AIBN) such as 2,2'-azobis-(2,4-dimethylvaleronitrile) and 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), and 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile.

[0143] Examples of the peroxide polymerization initiator include benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumene hydroperoxide, t-butyl hydroperoxide, di-t-butyl peroxide, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, 2,2-bis-(4,4-t-butylperoxycyclohexyl)propane, and tris-(t-butylperoxy)triazine.

[0144] Examples of the chain transfer agent include benzyl dithiobenzoate, 1-phenylethyl dithiobenzoate, 2-phenylprop-2-yl dithiobenzoate, 1-acetoxyethyl dithiobenzoate, hexakis(thiobenzoylthiomethyl)benzene, 1,4-bis(thiobenzoylthiomethyl)benzene, 1,2,4,5-tetrakis(thiobenzoylthiomethyl)benzene, 1,4-bis-(2-(thiobenzoylthio)prop-2-yl)benzene, 1-(4-methoxyphenyl)ethyl dithiobenzoate, benzyl dithioacetate; ethoxycarbonylmethyl dithioacetate, 2-(ethoxycarbonyl)prop-2-yl dithiobenzoate, 2-cyano prop-2-yl dithiobenzoate, t-butyl dithiobenzoate, 2,4,4-trimethylpent-2-yl dithiobenzoate, 2-(4-chlorophenyl)prop-2-yl dithiobenzoate, 3- and 4-vinylbenzyl dithiobenzoate, S-benzyl diethoxyphosphinyl dithioformate, t-butyl trithioperbenzoate, 2-phenylprop-2-yl 4-chlorodithiobenzoate, 2-phenylprop-2-yl 1-dithionaphthalate, 4-cyanopentanoic acid dithiobenzoate, dibenzyl tetrathioterephthalate, dibenzyl trithiocarbonate, carboxymethyl dithiobenzoate, and the like.

[0145] The polymerization temperature varies depending on the types of monomers and polymerization initiators used, but is preferably 50 to 100° C., and more preferably 55 to 90° C. The polymerization time varies depending on the types of monomers and polymerization initiators used, but is preferably, for example, 2 to 60 hours.

[0146] Regarding the copolymer containing structural units (other structural units) other than the structural unit containing a group having an azomethine structure represented by the above general formula (1), the preparation method thereof is not particularly limited.

[0147] For example, when preparing a random copolymer, the monomers for constituting the structural unit represented by the general formula (1) and the monomers for constituting the other structural units are mixed with a chain transfer agent, a polymerization initiator, etc. as raw material monomers to obtain a desired copolymer by carrying out a polymerization reaction. The specific form of the monomers for constituting the other structural units is as described above.

[0148] In one embodiment of the present invention, the photoresponsive polymer is The following general formula (3):

[0149] [ka]

[0150] It is expressed as Each α is independently a polymer block containing a structural unit represented by general formula (2), Each β is independently a polymer block containing a structural unit other than the structural unit represented by the general formula (2). In this embodiment, the azomethine derivative easily forms a domain in the polymer, and softening and melting can be efficiently induced, and a polymer having high toughness can be obtained by having a structural unit other than the structural unit represented by the general formula (2).

[0151] When the polymer of the present invention is polymerized, the azomethine structure absorbs light, and the heat energy released during the photoexcitation and deactivation process is transferred to the repeating units (structural units) to which it is bonded (photothermal conversion), which can cause melting or softening. In addition, by forming a block copolymer, the azomethine structure is more likely to form a domain within the polymer, which is thought to efficiently induce softening and melting. Therefore, the effects of the present invention can be obtained even more significantly.

[0152] The specific form of the structural unit represented by the general formula (1) constituting the polymer block α is as described above.

[0153] The structural unit constituting the polymer block β does not include the azomethine structure (R1-Z1=Z2-R2) in the general formula (1). Specifically, the above-described structural units other than the structural unit containing a group having an azomethine structure can be preferably used. In particular, from the viewpoint of application to the synthesis of a block copolymer by a living radical polymerization method such as the ATRP method, the ARGET-ATRP method, or the RAFT method, it is preferable that the structural unit has a vinyl-based polymerizable group. Specifically, for example, a styrene derivative, a (meth)acrylic acid derivative, an olefin derivative, a vinyl ester derivative, a vinyl ether derivative, a vinyl ketone derivative, or the like is used, and a styrene derivative, a (meth)acrylic acid derivative, or an olefin derivative is preferable. That is, in one embodiment of the present invention, the photoresponsive polymer is a polymer block in which the β contains at least one structural unit selected from the group consisting of a styrene derivative, a (meth)acrylic acid derivative, and an olefin derivative. This embodiment has the technical effect of obtaining a polymer with high toughness.

[0154] The number average molecular weight (total number average molecular weight) of the polymer block α contained in the polymer represented by the general formula (3) is not particularly limited, but is preferably 1000 or more, more preferably 1000 to 100,000, even more preferably 1000 to 70,000, even more preferably 1000 to 50,000, and particularly preferably 3000 to 50,000. If the total number average molecular weight of the polymer blocks α is 1000 or more, it is preferable because a toner image with excellent fixability can be more easily obtained when used as a toner. In addition, if the total number average molecular weight of the polymer blocks α is 100,000 or less, it is preferable because the efficiency of softening and melting is high. Here, the total number average molecular weight of the polymer blocks α refers to the number average molecular weight of the polymer block α when the polymer represented by the general formula (3) contains a single polymer block α, and refers to the sum of the number average molecular weights of the polymer blocks α when the polymer contains multiple polymer blocks α.

[0155] The number average molecular weight (total number average molecular weight) of the polymer block β contained in the polymer represented by the general formula (3) is not particularly limited, but is preferably 1000 or more, more preferably 1100 to 100000, even more preferably 1500 to 70000, even more preferably 2000 to 50000, and particularly preferably 3000 to 40000. If the total number average molecular weight of the polymer blocks β is 1000 or more, it is preferable because a toner image with excellent fixability can be more easily obtained when used as a toner. In addition, if the total number average molecular weight of the polymer blocks β is 100000 or less, it is preferable because the efficiency of softening and melting is high. Here, the total number average molecular weight of the polymer blocks β refers to the number average molecular weight of the polymer block β when the polymer represented by the general formula (3) contains a single polymer block β, and refers to the sum of the number average molecular weights of the polymer blocks β when the polymer represented by the general formula (3) contains multiple polymer blocks β.

[0156] The total number average molecular weight Mn of the polymer represented by the general formula (3) is preferably 3000 or more, more preferably 3200 to 100000, even more preferably 3300 to 70000, even more preferably 3400 to 50000, and particularly preferably 3450 to 50000. If the total number average molecular weight of the polymer represented by the general formula (3) is 3000 or more, it is preferable because a toner image with excellent fixability can be more easily obtained when used as a toner. If the total number average molecular weight is 100000 or less, it is preferable because the efficiency of softening and melting is high.

[0157] That is, in one embodiment of the present invention, the photoresponsive polymer has a number average molecular weight of α of 1,000 or more, a number average molecular weight of β of 1,000 or more, and a total number average molecular weight of 3,000 or more.

[0158] In the polymer represented by general formula (3), the ratio of the total number average molecular weight of the polymer blocks α to the total number average molecular weight of the polymer blocks β is not particularly limited, but from the viewpoints of ease of softening and melting and image strength, the ratio of the total number average molecular weight of the polymer blocks α to the total number average molecular weight of the polymer blocks β is preferably 1:20 to 20:1, and more preferably 1:15 to 15:1.

[0159] The total number average molecular weight of the polymer represented by formula (3) and the total number average molecular weight of the polymer blocks α and β can be measured by gel permeation chromatography (GPC), specifically, by the method described in the Examples below.

[0160] The method for synthesizing the block copolymer represented by the general formula (3) is not particularly limited, and known methods such as anionic polymerization, cationic polymerization, living radical polymerization, etc. can be used. Among them, as a simple synthesis method, a living radical polymerization method such as an atom transfer radical polymerization method (ATRP method), an ARGET-ATRP method, or a RAFT method can be preferably used.

[0161] Taking the ATRP method as an example, the method can be carried out by using a monofunctional, difunctional, trifunctional, or tetrafunctional compound containing a halogen element as an initiator as a starting material, and polymerizing a monomer that becomes a structural unit of the polymer block α or β in the presence of a catalyst.

[0162] In the step of polymerizing the monomer, for example, a macroinitiator is produced by polymerizing a monomer that will be a structural unit of either one of the polymer blocks α or β (the block that will be the core part of the block copolymer) in the presence of an initiator, a catalyst, and a ligand.

[0163] Examples of the initiator include, but are not limited to, 2-bromoisobutyrate butyl, 2-bromoisobutyrate ethyl, ethylene bis(2-bromoisobutyrate), 1,1,1-tris(2-bromoisobutyryloxymethyl)ethane, pentaerythritol tetrakis(2-bromoisobutyrate), α,α'-dibromo-p-xylene, ethyl bromoacetate, 2-bromoisobutyryl bromide, and mixtures thereof.

[0164] Examples of the catalyst include copper (I) catalysts and iron (II) catalysts, such as Cu(I)Cl, Cu(I)Br, Fe(II)Cl, Fe(II)Br, and mixtures thereof.

[0165] As the ligand, known ligands can be used, but one or more selected from the group consisting of 2,2'-bipyridyl, 4,4'-dimethyl-2,2'-bipyridyl, 4,4'-di-tert-butyl-2,2'-bipyridyl, 1,1,4,7,10,10-hexamethyltriethylenetetramine, N,N,N',N",N"-pentamethyldiethylenetriamine, cyclam (1,4,8,11-tetraazacyclotetradecane), 1,4,8,11-tetramethylcyclam (1,4,8,11-tetramethyl-1,4,8,11-tetraazacyclotetradecane), tris[2-(dimethylamino)ethyl]amine, and the like are preferred.

[0166] The amounts of the catalyst and ligand used are not particularly limited, and can be appropriately determined with reference to conventionally known knowledge.

[0167] Next, the macroinitiator obtained by the above polymerization is isolated and used as an initiator, and the monomer that is to become the structural unit of the polymer block α or β, which is not used in the synthesis of the macroinitiator, is polymerized again in the presence of a catalyst and a ligand. Alternatively, when the monomers have been almost completely consumed in the synthesis of the macroinitiator, the macroinitiator may be left as it is without isolating it, and the monomer that was not used in the synthesis of the macroinitiator may be added to continue the polymerization. By these operations, the desired block copolymer can be obtained.

[0168] Each of the above reactions is preferably carried out in an inert atmosphere, such as nitrogen or a rare gas such as argon. Each of the above reactions can be carried out at a temperature of, for example, 25 to 160° C., preferably 35 to 130° C. Each of the above reactions may be carried out without using a solvent, or in a solvent such as an organic solvent such as anisole.

[0169] In the reaction for obtaining a macroinitiator by polymerizing a monomer that will become a structural unit of either one of the polymer blocks α or β, and the reaction for obtaining a block copolymer by reacting the macroinitiator with a monomer that will become a structural unit of the other polymer block, the conditions such as the type and amount of catalyst and ligand used, and the reaction temperature may be the same or different.

[0170] <Fluidization and reversible non-fluidization by light irradiation> The wavelength of the irradiated light when the polymer of the present invention is fluidized by light irradiation is preferably in the range of 280 nm to 480 nm, more preferably in the range of 300 nm to 420 nm, and even more preferably in the range of 330 nm to 420 nm. Within the above range, the crystals are easily broken (improved light melting property), and the fixability is improved. When fluidizing, in addition to light irradiation, heat or pressure may be applied to promote fluidization. By irradiating with light of the above wavelength, even when heat or pressure is applied, it is possible to fluidize with less heat or pressure. Therefore, by introducing the polymer of the present invention into a toner, fixation at the above wavelength is possible, and a toner with excellent fixability and high color reproducibility can be obtained.

[0171] The above wavelength range includes a part of visible light. Therefore, it is desirable that the polymer of the present invention does not become fluid only by being exposed to light such as sunlight (natural light) or fluorescent light, and that the polymer is made more fluid under low-cost conditions with as low an irradiation dose and irradiation time as possible. From this viewpoint, the irradiation conditions for the above-mentioned polymer to become fluid are preferably an irradiation dose of 0.1 J / cm. 2 More than 200J / cm 2 Within the range of 0.1 J / cm 2 More than 100J / cm 2 Within the range below, more preferably 0.1 J / cm 2 More than 50J / cm 2 It is within the following range.

[0172] When the compound is fluidized, the compound may be heated together with the light irradiation. This allows the compound to be fluidized with a lower irradiation dose. The heating temperature in this case is, for example, in the range of 20°C to 200°C, preferably in the range of 20°C to 150°C.

[0173] On the other hand, the conditions for immobilizing (resolidifying) the polymer of the present invention are preferably left at room temperature (within the range of 25±15° C.) (in a natural environment). In this case, it is preferable to leave it in a dark place, but it may be exposed to natural light or visible light such as fluorescent light. It is more preferable to apply heat during the immobilization process. Light may also be applied.

[0174] When the polymer is heated to make it non-fluid, the heating temperature is preferably in the range of 0°C or more and 200°C or less, more preferably in the range of 20°C or more and 150°C or less.

[0175] [Toner composition] One embodiment of the present invention is a toner containing the polymer of the present invention. That is, the present invention provides a toner containing the photoresponsive polymer as a binder resin. By introducing the polymer of the present invention into a toner, it is possible to obtain a toner that can be fixed by light irradiation, has excellent fixability, and has high color reproducibility. Note that the toner refers to toner base particles or an aggregate of toner particles. The toner particles are preferably toner base particles to which an external additive has been added, but the toner base particles can also be used as they are as toner particles. Note that in the present invention, when there is no particular need to distinguish between the toner base particles, the toner particles, and the toner, they are also simply referred to as "toner".

[0176] The content of the polymer in the toner depends on the type of the azomethine structure (R1-Z1=Z2-R2) and other structural units in general formula (1), but from the viewpoint of efficient fluidization and image strength, it is, for example, in the range of 5 to 95 mass % based on the total amount of the binder resin, colorant, release agent, and polymer of the present invention that constitute the toner.

[0177] (Other binder resins) The toner of the present invention may further contain other binder resins. In such an embodiment, the viscosity during fluidization can be adjusted, and image strength can be increased. The binder resin is a resin that does not have a structure derived from other azomethine derivatives, that is, a resin that does not contain an azomethine structure (R1-Z1=Z2-R2), and any resin that is generally used as a binder resin constituting a toner can be used without limitation. As the binder resin, for example, a styrene resin, an acrylic resin, a styrene-acrylic resin, a polyester resin, a silicone resin, an olefin resin, an amide resin, and an epoxy resin can be used. These binder resins can be used alone or in combination of two or more kinds.

[0178] Among these, from the viewpoint of having a low viscosity when melted and a high sharp melting property, the binder resin preferably contains at least one selected from the group consisting of styrene resin, acrylic resin, styrene-acrylic resin, and polyester resin, and more preferably contains at least one selected from the group consisting of styrene-acrylic resin and polyester resin. By adopting such an embodiment, the image strength can be increased.

[0179] (styrene acrylic resin) The styrene-acrylic resin in the present invention is a polymer containing at least a structural unit derived from a styrene monomer and a structural unit derived from a (meth)acrylic acid ester monomer. Here, the styrene monomer includes not only styrene represented by the structural formula CH2=CH-C6H5, but also structures having a known side chain or functional group in the styrene structure.

[0180] Examples of the styrene monomer include the same styrene monomers capable of forming the above-mentioned polymer.

[0181] Moreover, the (meth)acrylic acid ester monomer has a functional group having an ester bond in the side chain. Specifically, in addition to the acrylic acid ester monomer represented by CH2=CHCOOR (R is an alkyl group), it includes vinyl ester compounds such as the methacrylic acid ester monomer represented by CH2=C(CH3)COOR (R is an alkyl group). Note that (meth)acrylic acid in the (meth)acrylic acid ester monomer means acrylic acid and methacrylic acid.

[0182] Examples of (meth)acrylic acid ester monomers include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, dodecyl (meth)acrylate, phenyl (meth)acrylate, diethylaminoethyl (meth)acrylate, and dimethylaminoethyl (meth)acrylate.

[0183] The styrene monomer and the (meth)acrylic acid ester monomer can be used either alone or in combination of two or more kinds.

[0184] The content of the structural unit derived from the styrene monomer and the structural unit derived from the (meth)acrylic acid ester monomer in the styrene-acrylic resin is not particularly limited, and can be appropriately adjusted from the viewpoint of controlling the softening point and glass transition temperature of the binder resin. Specifically, the content of the structural unit derived from the styrene monomer is preferably 40 to 95 mass% and more preferably 50 to 90 mass% based on the total structural units constituting the styrene-acrylic resin. In addition, the content of the structural unit derived from the (meth)acrylic acid ester monomer is preferably 5 to 60 mass% and more preferably 10 to 50 mass% based on the total structural units.

[0185] The content of the styrene-acrylic resin is preferably 5 to 60 mass %, and more preferably 10 to 50 mass %, based on the total resin.

[0186] The styrene-acrylic resin may further contain structural units derived from other monomers than the styrene monomer and the (meth)acrylic acid ester monomer, if necessary. Examples of other monomers include vinyl monomers. Below, examples of vinyl monomers that can be used in combination when forming the styrene-acrylic copolymer of the present invention are shown, but the vinyl monomers that can be used in combination are not limited to those shown below.

[0187] (1) Olefins Ethylene, propylene, isobutylene, etc. (2) Vinyl esters Vinyl propionate, vinyl acetate, vinyl benzoate, etc. (3) Vinyl ethers Vinyl methyl ether, vinyl ethyl ether, etc. (4) Vinyl ketones Vinyl methyl ketone, vinyl ethyl ketone, vinyl hexyl ketone, etc. (5) N-vinyl compounds N-vinylcarbazole, N-vinylindole, N-vinylpyrrolidone, etc. (6)Other Vinyl compounds such as vinylnaphthalene and vinylpyridine, acrylic acid or methacrylic acid derivatives such as acrylonitrile, methacrylonitrile and acrylamide, and the like.

[0188] It is also possible to prepare a resin having a crosslinked structure by using a polyfunctional vinyl monomer. Furthermore, it is also possible to use a vinyl monomer having an ionic dissociation group in the side chain. Specific examples of the ionic dissociation group include a carboxyl group, a sulfonic acid group, and a phosphoric acid group. Specific examples of the vinyl monomer having these ionic dissociation groups are shown below.

[0189] Specific examples of vinyl monomers having a carboxyl group include acrylic acid, methacrylic acid, maleic acid, itaconic acid, cinnamic acid, fumaric acid, maleic acid monoalkyl esters, and itaconic acid monoalkyl esters.

[0190] When forming the styrene-acrylic resin used in the present invention, the contents of the styrene monomer and the (meth)acrylic acid ester monomer are not particularly limited, and can be appropriately adjusted from the viewpoint of controlling the softening point temperature and the glass transition temperature of the binder resin. Specifically, the content of the styrene monomer is preferably 40 to 95 mass% and more preferably 50 to 90 mass% based on the total monomers constituting the styrene-acrylic resin. In addition, the content of the (meth)acrylic acid ester monomer is preferably 5 to 60 mass% and more preferably 10 to 50 mass% based on the total monomers constituting the styrene-acrylic resin.

[0191] The method for forming the styrene-acrylic resin is not particularly limited, and may be a method of polymerizing a monomer using a known oil-soluble or water-soluble polymerization initiator. If necessary, a known chain transfer agent such as n-octyl mercaptan may be used. As the oil-soluble polymerization initiator, for example, the following azo-based or diazo-based polymerization initiator or peroxide-based polymerization initiator may be used.

[0192] Examples of the azo or diazo polymerization initiator include 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobisisobutyronitrile, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis-4-methoxy-2,4-dimethylvaleronitrile, and azobisisobutyronitrile.

[0193] Examples of the peroxide polymerization initiator include benzoyl peroxide, methyl ethyl ketone peroxide, diisopropyl peroxycarbonate, cumene hydroperoxide, t-butyl hydroperoxide, di-t-butyl peroxide, dicumyl peroxide, 2,4-dichlorobenzoyl peroxide, lauroyl peroxide, 2,2-bis-(4,4-t-butylperoxycyclohexyl)propane, and tris-(t-butylperoxy)triazine.

[0194] In addition, when forming styrene-acrylic resin particles by emulsion polymerization, a water-soluble radical polymerization initiator can be used. Examples of the water-soluble radical polymerization initiator include persulfates such as potassium persulfate and ammonium persulfate, azobisaminodipropane acetate, azobiscyanovaleric acid and its salts, and hydrogen peroxide.

[0195] The polymerization temperature varies depending on the types of monomers and polymerization initiators used, but is preferably 50 to 100° C., and more preferably 55 to 90° C. The polymerization time varies depending on the types of monomers and polymerization initiators used, but is preferably, for example, 2 to 12 hours.

[0196] The styrene-acrylic resin particles formed by emulsion polymerization can be made to have two or more layers made of resins with different compositions. In this case, the manufacturing method can be a multi-stage polymerization method in which a polymerization initiator and a polymerizable monomer are added to a dispersion of resin particles prepared by emulsion polymerization treatment (first stage polymerization) according to a conventional method, and this system is polymerized (second stage, third stage polymerization).

[0197] (polyester resin) The polyester resin is obtained by a polycondensation reaction between a divalent or higher carboxylic acid (a polyvalent carboxylic acid component) and a divalent or higher alcohol (a polyhydric alcohol component). The polyester resin may be amorphous or crystalline.

[0198] The valence of each of the polyvalent carboxylic acid component and the polyhydric alcohol component is preferably 2 to 3, and more preferably 2. That is, the polyvalent carboxylic acid component preferably contains a dicarboxylic acid component, and the polyhydric alcohol component preferably contains a dialcohol component.

[0199] Examples of the dicarboxylic acid component include saturated aliphatic dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid (dodecanedioic acid), 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,13-tridecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,16-hexadecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; and methylenesuccinic acid. unsaturated aliphatic dicarboxylic acids such as fumaric acid, maleic acid, 3-hexenedioic acid, 3-octenedioic acid, and dodecenylsuccinic acid; unsaturated aromatic dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, t-butylisophthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-phenylenediacetic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, and anthracenedicarboxylic acid; and lower alkyl esters and acid anhydrides of these may also be used. The dicarboxylic acid component may be used alone or in combination of two or more.

[0200] In addition, trivalent or higher polyvalent carboxylic acids such as trimellitic acid and pyromellitic acid, and their anhydrides or alkyl esters having 1 to 3 carbon atoms can also be used.

[0201] Examples of the diol component include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,20-eicosanediol, and neopentanediol. Examples of the diol component include saturated aliphatic diols such as ethyl glycol; unsaturated aliphatic diols such as 2-butene-1,4-diol, 3-butene-1,4-diol, 2-butyne-1,4-diol, 3-butyne-1,4-diol, and 9-octadecene-7,12-diol; and aromatic diols such as bisphenols such as bisphenol A and bisphenol F, and alkylene oxide adducts of bisphenols such as ethylene oxide adducts and propylene oxide adducts thereof, and derivatives thereof can also be used. The diol component may be used alone or in combination of two or more kinds.

[0202] The method for producing the polyester resin is not particularly limited, and the polyester resin can be produced by polycondensing (esterifying) the polyvalent carboxylic acid component and the polyhydric alcohol component using a known esterification catalyst.

[0203] Examples of catalysts that can be used in the production of polyester resins include alkali metal compounds such as sodium and lithium; compounds containing Group 2 elements such as magnesium and calcium; compounds of metals such as aluminum, zinc, manganese, antimony, titanium, tin, zirconium, and germanium; phosphorous compounds; phosphoric acid compounds; and amine compounds. Specifically, examples of tin compounds include dibutyltin oxide (dibutyltin oxide), tin octoate, tin dioctoate, and salts thereof. Examples of titanium compounds include titanium alkoxides such as tetra-normal-butyl titanate (Ti(On-Bu)4), tetraisopropyl titanate, tetramethyl titanate, and tetrastearyl titanate; titanium acylates such as polyhydroxytitanium stearate; and titanium chelates such as titanium tetraacetylacetonate, titanium lactate, and titanium triethanolamine. Examples of germanium compounds include germanium dioxide. Examples of aluminum compounds include polyaluminum hydroxide, aluminum alkoxide, and tributylaluminate. These may be used alone or in combination of two or more.

[0204] The polymerization temperature is not particularly limited, but is preferably 70 to 250° C. The polymerization time is also not particularly limited, but is preferably 0.5 to 10 hours. During the polymerization, the reaction system may be decompressed as necessary.

[0205] When the toner of the present invention contains a binder resin in addition to the polymer of the present invention, the content ratio of the polymer to the binder resin is not particularly limited.

[0206] From the viewpoints of fixability and heat-resistant storage stability, the glass transition temperature (Tg) of the toner is preferably 25 to 100° C., and more preferably 30 to 80° C. The glass transition temperature (Tg) of the toner can be adjusted by the molecular weight of the polymer, and when a structural unit other than a structural unit containing a group having an azomethine structure is contained, by the type and content of the structural unit. When the toner contains a binder resin, it can be further adjusted by the content ratio of the polymer and the binder resin, the type and molecular weight of the binder resin, etc.

[0207] The content of the polyester resin is preferably from 5 to 60% by mass, and more preferably from 10 to 50% by mass, based on the total resin.

[0208] The toner of the present invention may be particles having a single layer structure or particles having a core-shell structure. The types of binder resins used for the core particles and shell part of the core-shell structure are not particularly limited.

[0209] <Coloring agent> The toner of the present invention may further contain a colorant. Since the polymer of the present invention does not have a significant coloring, a toner having high color reproducibility of the colorant can be obtained. As the colorant, generally known dyes and pigments can be used.

[0210] Examples of colorants for obtaining black toner include carbon black, magnetic materials, iron-titanium composite oxide black, etc. Examples of carbon black include channel black, furnace black, acetylene black, thermal black, and lamp black, and examples of magnetic materials include ferrite and magnetite.

[0211] Colorants for obtaining yellow toners include dyes such as CI Solvent Yellow 19, 44, 77, 79, 81, 82, 93, 98, 103, 104, 112, and 162; and pigments such as CI Pigment Yellow 14, 17, 74, 93, 94, 138, 155, 180, and 185.

[0212] Colorants for obtaining magenta toner include dyes such as CI Solvent Red 1, 49, 52, 58, 63, 111, and 122; and pigments such as CI Pigment Red 5, 48:1, 53:1, 57:1, 122, 139, 144, 149, 166, 177, 178, and 222.

[0213] Colorants for obtaining cyan toner include dyes such as CI Solvent Blue 25, 36, 60, 70, 93, and 95; and pigments such as CI Pigment Blue 1, 7, 15, 15:3, 60, 62, 66, and 76.

[0214] The colorants for obtaining the toner of each color may be used alone or in combination of two or more kinds for each color.

[0215] The content of the colorant in the toner particles (toner base particles) before addition of external additives is preferably 0.5 to 20% by mass, and more preferably 2 to 10% by mass.

[0216] <Release agent> The toner according to the present invention may further contain a release agent. By incorporating a release agent into the toner, a toner having superior fixability and color reproducibility can be obtained when thermal fixing is performed together with light irradiation.

[0217] The release agent used is not particularly limited, and various known waxes can be used. Examples of the wax include polyolefins such as low molecular weight polypropylene, polyethylene, or oxidized low molecular weight polypropylene, polyethylene, paraffin wax, and synthetic ester wax. Among them, it is preferable to use paraffin wax from the viewpoint of improving the storage stability of the toner.

[0218] The content of the release agent in the toner base particles is preferably 1 to 30% by mass, and more preferably 3 to 15% by mass.

[0219] <Charge control agent> The toner according to the present invention may contain a charge control agent. The charge control agent used is a substance capable of imparting positive or negative charge by frictional charging, and is colorless, and is not particularly limited. Any of various known positively and negatively chargeable charge control agents can be used.

[0220] The content of the charge control agent in the toner base particles is preferably 0.01 to 30% by mass, and more preferably 0.1 to 10% by mass.

[0221] <External additives> In order to improve the fluidity, chargeability, cleaning properties, etc. of the toner, external additives such as a fluidizing agent, a cleaning aid, etc., which are so-called post-treatment agents, may be added to the toner base particles to form the toner according to the present invention.

[0222] Examples of the external additive include inorganic oxide particles such as silica particles, alumina particles, and titanium oxide particles, inorganic stearic acid compound particles such as aluminum stearate particles and zinc stearate particles, and inorganic titanic acid compound particles such as strontium titanate particles and zinc titanate particles. If necessary, these inorganic particles may be hydrophobized. These may be used alone or in combination of two or more.

[0223] Among these, preferred external additives are, for example, sol-gel silica particles, silica particles whose surfaces have been hydrophobized (hydrophobic silica particles), or titanium oxide particles (hydrophobic titanium oxide particles), and it is more preferred to use at least two or more types of external additives among these.

[0224] The number average primary particle size of the external additive is preferably within the range of 1 to 200 nm, more preferably 10 to 180 nm. When two or more types of external additives are used in combination, it is particularly preferable that at least one of the external additives has a size of 30 nm or more and 180 nm or less.

[0225] The amount of these external additives added is preferably 0.05 to 5% by mass, and more preferably 0.1 to 3% by mass, in the toner.

[0226] In one embodiment of the present invention, the amount of these external additives added is preferably 0.5 to 5% by mass, and more preferably 0.1 to 3% by mass, based on the toner base particles.

[0227] <Average particle size of toner> The average particle size of the toner (and the average particle size of the toner base particles) is preferably 4 to 20 μm, more preferably 5 to 15 μm, in terms of volume-based median diameter (D50). When the volume-based median diameter (D50) is within the above range, the transfer efficiency is increased, and the image quality of halftones and fine lines, dots, etc. is improved.

[0228] The volume-based median diameter (D50) can be measured and calculated using a measuring device consisting of a "Coulter Counter 3" (Beckman Coulter, Inc.) connected to a computer system (Beckman Coulter, Inc.) equipped with the data processing software "Software V3.51."

[0229] Specifically, 0.02 g of the measurement sample (toner or toner base particles) is added to 20 mL of surfactant solution (a surfactant solution prepared by diluting, for example, a neutral detergent containing surfactant components 10 times with pure water in order to disperse toner particles), and after mixing, ultrasonic dispersion is performed for 1 minute to prepare a dispersion liquid. This dispersion liquid is then pipetted into a beaker containing an "ISOTON II" (manufactured by Beckman Coulter, Inc.) in the sample stand until the concentration indicated on the measuring device reaches 8%.

[0230] Here, by setting the display concentration within the above range, it is possible to obtain reproducible measurement values. In the measurement device, the number of measured particles is set to 25,000, the aperture diameter is set to 50 μm, the measurement range of 1 to 30 μm is divided into 256 parts to calculate the frequency value, and the particle size with the largest volume cumulative fraction of 50% is set as the volume-based median diameter (D50).

[0231] [Toner manufacturing method] The method for producing the toner of the present invention is not particularly limited. For example, when the toner is made from only the polymer of the present invention, a production method including pulverizing the polymer using an apparatus such as a hammer mill, a feather mill, or a counter jet mill, and then classifying the polymer to a desired particle size using a dry classifier such as a spin air sieve, a classifier, or a micron classifier can be used. When a toner further containing a colorant is produced, the polymer and the colorant are dissolved in a solvent in which both the polymer of the present invention and the colorant are soluble to obtain a solution, the solvent is removed, and then the solution is pulverized and classified in the same manner as above.

[0232] In particular, the toner containing the polymer of the present invention and, if necessary, a binder and a colorant is preferably produced by a production method utilizing an emulsion aggregation method, which allows easy control of particle size and shape.

[0233] Such a manufacturing method is as follows: (1A) A binder resin particle dispersion preparation step of preparing a binder resin particle dispersion as required. (1B) A step of preparing a polymer particle dispersion liquid for preparing a dispersion liquid of the polymer particles of the present invention (1C) A colorant particle dispersion preparation step of preparing a colorant particle dispersion as required. (2) An association step in which a flocculant is added to an aqueous medium in which polymer particles, and if necessary, binder resin particles and colorant particles are present, to promote salting out and simultaneously cause aggregation and fusion to form associated particles. (3) Aging process to form toner base particles by controlling the shape of aggregated particles (4) A filtering and washing process for filtering the toner base particles from the aqueous medium and removing surfactants and the like from the toner base particles. (5) A drying process for drying the washed toner base particles. (6) Additive addition step of adding additives to the dried toner base particles It is preferable that the method includes each of the steps of:

[0234] The steps (1A) to (1C) are described below.

[0235] (1A) Binder resin particle dispersion preparation process In this process, resin particles are formed by a conventional emulsion polymerization or the like, and the resin particles are aggregated and fused to form binder resin particles. As an example, polymerizable monomers constituting the binder resin are introduced into an aqueous medium, dispersed therein, and polymerized by a polymerization initiator to prepare a dispersion of binder resin particles.

[0236] As a method for obtaining a binder resin particle dispersion, in addition to the above-mentioned method of polymerizing a polymerizable monomer in an aqueous medium by a polymerization initiator, for example, a method of performing a dispersion treatment in an aqueous medium without using a solvent, or a method of dissolving a crystalline resin in a solvent such as ethyl acetate to prepare a solution, emulsifying and dispersing the solution in an aqueous medium using a disperser, and then performing a solvent removal treatment, can be mentioned.

[0237] In this case, if necessary, a release agent may be added to the binder resin in advance. For dispersion, it is also preferable to carry out the polymerization in the presence of a known surfactant (for example, an anionic surfactant such as polyoxyethylene (2) dodecyl ether sodium sulfate, sodium dodecyl sulfate, or dodecylbenzenesulfonic acid).

[0238] The volume-based median diameter of the binder resin particles in the dispersion is preferably 50 to 300 nm. The volume-based median diameter of the binder resin particles in the dispersion can be measured by a dynamic light scattering method using "Microtrac UPA-150" (manufactured by Nikkiso Co., Ltd.).

[0239] (1B) Polymer particle dispersion preparation process The polymer particle dispersion preparation step is a step of dispersing the polymer of the present invention in the form of fine particles in an aqueous medium to prepare a dispersion of the polymer particles.

[0240] In preparing the dispersion of the polymer particles, first, an emulsion of the polymer is prepared. For example, the emulsion of the polymer is prepared by dissolving the polymer in an organic solvent and then emulsifying the obtained solution in an aqueous medium.

[0241] The method for dissolving the polymer in the organic solvent is not particularly limited, and examples thereof include a method of adding the polymer to the organic solvent and stirring and mixing the polymer so as to dissolve it. The amount of the polymer added is preferably 5 parts by mass or more and 100 parts by mass or less, more preferably 10 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the organic solvent.

[0242] Next, the obtained solution of the polymer is mixed with an aqueous medium and stirred using a known dispersing machine such as a homogenizer, whereby the polymer becomes droplets and is emulsified in the aqueous medium to prepare an emulsion of the polymer.

[0243] The amount of the polymer solution added is preferably 10 parts by mass or more and 110 parts by mass or less with respect to 100 parts by mass of the aqueous medium.

[0244] The temperatures of the polymer solution and the aqueous medium when the polymer solution and the aqueous medium are in a temperature range below the boiling point of the organic solvent, and are preferably from 20° C. to 80° C., more preferably from 30° C. to 75° C. When the polymer solution and the aqueous medium are mixed, the temperatures of the polymer solution and the aqueous medium may be the same or different, and are preferably the same.

[0245] Regarding the stirring conditions of the dispersing machine, when the capacity of the stirring vessel is 1 to 3 L, for example, the rotation speed is preferably 7000 rpm or more and 20000 rpm or less, and the stirring time is preferably 10 minutes or more and 30 minutes or less.

[0246] The dispersion of the polymer particles is prepared by removing the organic solvent from the polymer emulsion. Examples of the method for removing the organic solvent from the polymer emulsion include known methods such as blowing air, heating, reducing pressure, or a combination of these.

[0247] As an example, the polymer emulsion is heated, for example, in an inert gas atmosphere such as nitrogen, preferably at 25° C. to 90° C., more preferably at 30° C. to 80° C., until, for example, about 80% by mass to 95% by mass of the initial amount of organic solvent is removed (for example, for 20 to 150 minutes), thereby removing the organic solvent. As a result, the organic solvent is removed from the aqueous medium, and a dispersion of the polymer particles in which the polymer particles are dispersed in the aqueous medium is prepared.

[0248] The mass average particle diameter of the polymer particles in the dispersion of the polymer particles is preferably 90 nm or more and 1200 nm or less. The mass average particle diameter can be set within the above range by appropriately adjusting the viscosity when the polymer is mixed with an organic solvent, the mixing ratio of the polymer solution to the aqueous medium, the stirring speed of a dispersing machine when preparing the polymer emulsion, and the like. The mass average particle diameter of the polymer particles in the dispersion of the polymer particles can be measured using a Microtrac UPA-150 (manufactured by Nikkiso Co., Ltd.) or an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).

[0249] <Organic solvent> The organic solvent used in this step is not particularly limited as long as it can dissolve the polymer.Specific examples of the organic solvent include esters such as ethyl acetate and butyl acetate, ethers such as diethyl ether, diisopropyl ether, and tetrahydrofuran, ketones such as acetone and methyl ethyl ketone, saturated hydrocarbons such as hexane and heptane, and halogenated hydrocarbons such as dichloromethane, dichloroethane, and carbon tetrachloride.

[0250] Such organic solvents can be used alone or in combination of two or more kinds. Among these organic solvents, ketones and halogenated hydrocarbons are preferred, and methyl ethyl ketone and dichloromethane are more preferred.

[0251] <Aqueous medium> The aqueous medium used in this step may be water, or an aqueous medium containing water as the main component and water-soluble solvents such as alcohols and glycols, and optional components such as surfactants and dispersants. The aqueous medium used is preferably a mixture of water and a surfactant.

[0252] Examples of the surfactant include cationic surfactants, anionic surfactants, and nonionic surfactants. Examples of the cationic surfactant include dodecyl ammonium chloride, dodecyl ammonium bromide, dodecyl trimethyl ammonium bromide, dodecyl pyridinium chloride, dodecyl pyridinium bromide, and hexadecyl trimethyl ammonium bromide. Examples of the anionic surfactant include fatty acid soaps such as sodium stearate and sodium dodecanoate, sodium dodecyl benzene sulfonate, and sodium dodecyl sulfate. Examples of the nonionic surfactant include polyoxyethylene dodecyl ether, polyoxyethylene hexadecyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene dodecyl ether, polyoxyethylene sorbitan monooleate ether, and monodecanoyl sucrose.

[0253] Such surfactants can be used alone or in combination of two or more. Among the surfactants, anionic surfactants are preferred, and sodium dodecylbenzenesulfonate is more preferred.

[0254] The amount of the surfactant added is preferably 0.01 to 10 parts by mass, more preferably 0.04 to 1 part by mass, in terms of solid content, relative to 100 parts by mass of the aqueous medium.

[0255] (1C) Colorant particle dispersion preparation process The colorant particle dispersion preparation step is a step of dispersing a colorant in the form of fine particles in an aqueous medium to prepare a colorant particle dispersion.

[0256] The colorant can be dispersed by utilizing mechanical energy. The median diameter based on the number of colorant particles in the dispersion is preferably 10 to 300 nm, and more preferably 50 to 200 nm. The median diameter based on the number of colorant particles can be measured using an electrophoretic light scattering photometer "ELS-800" (manufactured by Otsuka Electronics Co., Ltd.).

[0257] The steps from (2) association step to (6) external additive addition step can be carried out according to various conventionally known methods.

[0258] The flocculant used in the (2) association step is not particularly limited, but is preferably selected from metal salts. Examples of metal salts include monovalent metal salts such as salts of alkali metals such as sodium, potassium, and lithium; divalent metal salts such as calcium, magnesium, manganese, and copper; and trivalent metal salts such as iron and aluminum. Specific examples of metal salts include sodium chloride, potassium chloride, lithium chloride, calcium chloride, magnesium chloride, zinc chloride, copper sulfate, magnesium sulfate, and manganese sulfate. Among these, it is particularly preferable to use divalent metal salts because they can promote flocculation with a smaller amount. These can be used alone or in combination of two or more.

[0259] [Developer] The toner according to the present invention can be suitably used in various cases, including when it contains a magnetic material and is used as a one-component magnetic toner, when it is mixed with a so-called carrier and used as a two-component developer, and when it is used alone as a non-magnetic toner.

[0260] As the magnetic material, for example, magnetite, γ-hematite, or various ferrites can be used.

[0261] The carrier contained in the two-component developer may be magnetic particles made of conventionally known materials such as metals such as iron, steel, nickel, cobalt, ferrite, and magnetite, and alloys of these metals with metals such as aluminum and lead.

[0262] The carrier may be a coated carrier in which the surface of the magnetic particles is coated with a coating agent such as a resin, or a resin-dispersed carrier in which magnetic powder is dispersed in a binder resin. The resin for coating is not particularly limited, but for example, olefin resin, acrylic resin, styrene resin, styrene-acrylic resin, silicone resin, polyester resin, or fluororesin is used. The resin for constituting the resin-dispersed carrier particles is not particularly limited, and known resins can be used, for example, acrylic resin, styrene-acrylic resin, polyester resin, fluororesin, phenolic resin, etc. can be used.

[0263] The volume-based median diameter of the carrier is preferably 20 to 100 μm, and more preferably 25 to 80 μm. The volume-based median diameter of the carrier can be measured typically by a laser diffraction particle size distribution measuring device "HELOS" (manufactured by SYMPATEC) equipped with a wet disperser.

[0264] The mixing amount of the toner with respect to the carrier is preferably 2 to 10% by mass, with the total mass of the toner and carrier being 100% by mass.

[0265] [Image forming method] The toner of the present invention can be used in various known electrophotographic image forming methods. For example, it can be used in monochrome image forming methods and full-color image forming methods. In the full-color image forming method, it can be applied to any image forming method, such as a four-cycle image forming method that is composed of four types of color developing devices for yellow, magenta, cyan, and black, and one photoconductor, and a tandem image forming method that is equipped with image forming units having color developing devices and photoconductors for each color, respectively.

[0266] That is, an image forming method according to one embodiment of the present invention includes a step of 1) forming a toner image made of the toner of the present invention on a recording medium, and a step of 2) irradiating the toner image with light to soften the toner image. This embodiment provides excellent fixability and high image quality.

[0267] Regarding step 1) In this process, a toner image made of the toner of the present invention is formed on a recording medium.

[0268] (Recording medium) The recording medium is a member for holding a toner image. Examples of the recording medium include plain paper, high-quality paper, art paper, coated printing paper such as coated paper, commercially available Japanese paper and postcard paper, resin films for overhead projectors or packaging materials, and cloth.

[0269] The recording medium may be in the form of a sheet (foliage) having a predetermined size, or may be in the form of a long piece that is wound up in a roll after the toner image is fixed thereon.

[0270] As described later, the toner image can be formed, for example, by transferring the toner image on the photoconductor onto a recording medium.

[0271] Regarding step 2) In this process, the formed toner image is irradiated with light to soften the toner image, which allows the toner image to adhere to a recording medium.

[0272] The wavelength of the irradiated light is not particularly limited as long as it can sufficiently soften the toner image by photothermal conversion by the polymer in the toner, but is preferably 280 nm or more and 480 nm or less. If it is in the above range, the toner image can be softened more efficiently. From the same viewpoint, the amount of light irradiation is preferably 0.1 to 200 J / cm. 2 , more preferably 0.1 to 100 J / cm 2 , and more preferably 0.1 to 50 J / cm 2 It is.

[0273] As described later, the light irradiation can be performed using a light source such as a light emitting diode (LED) or a laser light source. In addition, as described later, heating may be further performed in addition to the light irradiation.

[0274] After the step 2), if necessary, a step 3) of pressing the softened toner image may be further carried out. This embodiment improves the fixing property.

[0275] Regarding step 3) In this process, the softened toner image is pressed.

[0276] The pressure when pressing the toner image on the recording medium is not particularly limited, but is preferably 0.01 to 5.0 MPa, and more preferably 0.05 to 1.0 MPa. By setting the pressure to 0.01 MPa or more, the deformation amount of the toner image can be increased, so that the contact area between the toner image and the recording paper S increases, and it is easy to further improve the fixability of the image. In addition, by setting the pressure to 5.0 MPa or less, shock noise during pressing can be suppressed.

[0277] The pressurizing step may be carried out before or simultaneously with the step of irradiating light and softening the toner image (step 2) described above), but it is preferable to carry it out after the light irradiation, since this allows pressure to be applied to the toner image that has already been softened, thereby further improving the fixability of the image.

[0278] In addition, in the pressurizing step, the softened toner image may be further heated. That is, the pressurizing step may be performed while heating the toner image. The temperature at that time (for example, the temperature of the pressing member) is preferably 15°C or higher, more preferably 20°C or higher, even more preferably more than 20°C, even more preferably 30°C or higher, and even more preferably 40°C or higher. This embodiment significantly improves the fixability. There is no particular upper limit, but it is, for example, 200°C or lower, 150°C or lower, or 100°C or lower.

[0279] The heating temperature of the toner image (the surface temperature of the toner image during heating) is preferably (Tg+20) to (Tg+100)° C., and more preferably (Tg+25) to (Tg+80)° C., where Tg is the glass transition temperature of the toner. If the surface temperature of the toner image is (Tg+20)° C. or higher, the toner image is easily deformed by pressure, and if it is (Tg+100)° C. or lower, hot offset is easily suppressed. Note that hot offset refers to a phenomenon in which part of the toner is transferred to a pressure member such as a roller during the fixing process, causing the toner layer to break up.

[0280] Furthermore, before the step 2), a step 4) of heating the toner image in advance may be further carried out as necessary. By carrying out the step 4) of heating the toner image in advance before the step 2), the sensitivity of the polymer of the present invention to light can be further increased. This makes it easy to promote melting or softening of the toner image by light irradiation, since the sensitivity to light is unlikely to be impaired even in the case of a polymer.

[0281] The image forming method of the present invention can be carried out by using, for example, the following image forming apparatus.

[0282] Fig. 1 is a schematic diagram showing an image forming apparatus 100 used in an image forming method according to an embodiment of the present invention. However, the image forming apparatus used in the present invention is not limited to the following form and illustrated example. Fig. 1 shows an example of a monochrome image forming apparatus 100, but the present invention can also be applied to a color image forming apparatus.

[0283] The image forming apparatus 100 is an apparatus for forming an image on a recording paper S as a recording medium, and is equipped with an image reading device 71 and an automatic document feeder 72, and performs image formation on the recording paper S transported by a paper transport system 7 using an image forming unit 10, an irradiation unit 40, and a pressing unit 9.

[0284] Furthermore, while image forming apparatus 100 uses recording paper S as a recording medium, the medium on which an image is formed may be something other than paper.

[0285] An original d placed on the platen of the automatic document feeder 72 is scanned and exposed by the optical system of the scanning exposure device of the image reading device 71 and read into the image sensor CCD. An analog signal photoelectrically converted by the image sensor CCD is subjected to analog processing, A / D conversion, shading correction, image compression processing, etc. in the image processing unit 20, and then input to the exposure device 3 of the image forming unit 10.

[0286] The paper transport system 7 includes a plurality of trays 16, a plurality of paper feed units 11, transport rollers 12, a transport belt 13, etc. The trays 16 each store recording paper S of a predetermined size, and operate the paper feed unit 11 of the specified tray 16 in response to an instruction from the control unit 90 to supply the recording paper S. The transport rollers 12 transport the recording paper S sent out from the tray 16 by the paper feed unit 11 or the recording paper S brought in from the manual paper feed unit 15 to the image forming unit 10.

[0287] The image forming unit 10 is configured by arranging a charger 2, an exposure unit 3, a developing unit 4, a transfer unit 5 and a cleaning unit 8 in this order around the photoreceptor 1 along the direction of rotation of the photoreceptor 1.

[0288] The photoconductor 1, which is an image carrier, is an image carrier having a photoconductive layer formed on its surface, and is configured to be rotatable in the direction of the arrow in Fig. 1 by a driving device (not shown). A thermo-hygrometer 17 that detects the temperature and humidity inside the image forming apparatus 100 is provided near the photoconductor 1.

[0289] The charger 2 uniformly charges the surface of the photoreceptor 1, thereby uniformly charging the surface of the photoreceptor 1. The exposure unit 3 is equipped with a beam emission source such as a laser diode, and irradiates the charged surface of the photoreceptor 1 with a beam of light, thereby dissipating the charge in the irradiated area and forming an electrostatic latent image on the photoreceptor 1 according to the image data. The development unit 4 supplies the toner contained therein to the photoreceptor 1, and creates a toner image on the surface of the photoreceptor 1 based on the electrostatic latent image.

[0290] The transfer unit 5 faces the photoreceptor 1 via the recording paper S, and transfers the toner image onto the recording paper S. The cleaning unit 8 includes a blade 85. The blade 85 cleans the surface of the photoreceptor 1 to remove developer remaining on the surface of the photoreceptor 1.

[0291] The recording paper S onto which the toner image has been transferred is transported by a transport belt 13 to a pressing unit 9. The pressing unit 9 may be installed arbitrarily, and performs a fixing process on the recording paper S onto which the toner image has been transferred by applying pressure alone or heat and pressure with pressure members 91 and 92, thereby fixing the image onto the recording paper S. The recording paper S onto which the image has been fixed is transported by transport rollers to a paper discharge unit 14, and is discharged from the paper discharge unit 14 to the outside of the machine.

[0292] In addition, the image forming apparatus 100 is equipped with a paper inversion section 24, so that the recording paper S that has been subjected to the heat fixing process is transported to the paper inversion section 24 just before the paper discharge section 14, and the recording paper S is either inverted and discharged, or the inverted recording paper S is transported again to the image forming section 10, so that images can be formed on both sides of the recording paper S.

[0293] <Irradiation unit> FIG. 2 is a schematic diagram of the irradiation unit 40 in the image forming apparatus 100. As shown in FIG.

[0294] An image forming apparatus 100 according to an embodiment of the present invention includes an irradiation section 40. The irradiation section 40 includes a light source 41 and a heating member 93. Examples of devices constituting the light source 41 include a light emitting diode (LED) and a laser light source.

[0295] The light source 41 irradiates the toner image formed on the recording medium with light to soften the toner image. The conditions of the light irradiation are not particularly limited as long as they melt and fluidize the composition of the present invention contained in the toner of the developer. The wavelength of the light irradiated to the toner image may be sufficient to sufficiently fluidize the composition, and is preferably in the range of 280 nm to 480 nm, more preferably in the range of 300 nm to 420 nm, and even more preferably in the range of 330 nm to 420 nm. The amount of light irradiated by the light source 41 may also be sufficient to sufficiently fluidize the composition, and is, for example, 0.1 J / cm. 2 More than 200J / cm 2 Within the range below, preferably 0.1 J / cm 2 More than 100J / cm 2 Within the range of 0.1 J / cm 2 More than 50J / cm 2 It is within the following range.

[0296] When the toner image is softened by irradiating the toner image with light from the light source 41, the toner image may be heated by the heating member 93 in addition to the light irradiation. This allows the toner image to be softened and melted more efficiently. The heating temperature at this time is, for example, in the range of 20° C. to 200° C., and preferably in the range of 20° C. to 150° C.

[0297] The softened toner image can be solidified and fixed to the recording medium by leaving it at room temperature (within the range of 25±15° C.), heating it, or irradiating it with visible light. As described below, the fixing step preferably further includes a step of applying pressure to the softened toner image. In the pressurizing step, it is preferable to further heat the softened toner image.

[0298] Light source 41 irradiates light toward a first surface of recording paper S holding a toner image, which is on the photoreceptor side, and is disposed on the photoreceptor side with respect to the surface of recording paper S nipped between photoreceptor 1 and transfer roller 5, which is a transfer section. A heating member 93 is disposed on the opposite side of light source 41 with respect to the surface of recording paper S. Light source 41 and heating member 93 are disposed along the transport direction of recording paper S (paper transport direction).

[0299] The light source 41 and the heating member 93 are disposed downstream of the nip position between the photoconductor 1 and the transfer roller 5 in the paper transport direction and upstream of the pressure bonding unit 9 in the paper transport direction.

[0300] According to an image forming method according to an embodiment of the present invention, the photoconductor 1 is charged by applying a uniform potential to it using the charger 2, and then the photoconductor 1 is scanned with a light beam irradiated by the exposure device 3 based on original image data to form an electrostatic latent image. Next, the developing unit 4 supplies a developer having a toner containing the composition of the present invention onto the photoconductor 1.

[0301] When the recording paper S is transported from the tray 16 to the image forming unit 10 in time with the rotation of the photoconductor 1 causing the toner image carried on the surface of the photoconductor 1 to reach the position of the transfer roller 5, which is the transfer unit, the toner image on the photoconductor 1 is transferred onto the recording paper S, which is nipped between the transfer roller 5 and the photoconductor 1, by the transfer bias applied to the transfer roller 5.

[0302] The transfer unit 5 also functions as a pressure member, and can reliably bring the toner image into close contact with the recording paper S while transferring the toner image from the photoreceptor 1 to the recording paper S.

[0303] After the toner image is transferred onto the recording paper S, the blade 85 of the cleaning unit 8 removes the developer remaining on the surface of the photoconductor 1 .

[0304] In the process in which the recording paper S onto which the toner image has been transferred is transported by the transport belt 13 to the pressing unit 9, the light source 41 irradiates light onto the toner image transferred onto the recording paper S. By irradiating light onto the toner image on the first side of the recording paper S from the light source 41, the toner image can be melted more reliably, and the fixability of the toner image to the recording paper S can be improved.

[0305] When the recording paper S carrying the toner image reaches the pressing unit 9 by the conveyor belt 13, the pressure members 91 and 92 press the toner image onto the first side of the recording paper S. Before the toner image is fixed by the pressing unit 9, the toner image is softened by being irradiated with light by the light source 41, so that it is possible to save energy in pressing the image onto the recording paper S. Furthermore, in the process of solidifying the toner image and fixing it to the recording medium, the toner image is pressed by the pressure members 91 and 92, so that the fixability of the toner image onto the recording paper S is further improved.

[0306] The pressure when pressing the toner image is as described above. The pressing step may be performed before, simultaneously with, or after the step of softening the toner image by irradiating light. From the viewpoint of being able to pressurize a toner image in a pre-softened state and facilitating the enhancement of image strength, it is preferable to perform the pressing step after the light irradiation.

[0307] In addition, the pressure member 91 can heat the toner image on the recording paper S when the recording paper S passes between the pressure members 91 and 92. The toner image softened by the light irradiation is further softened by this heating, and as a result, the fixability of the toner image to the recording paper S is further improved.

[0308] The heating temperature of the toner image is as described above. The heating temperature of the toner image (surface temperature of the toner image) can be measured by a non-contact temperature sensor. Specifically, for example, a non-contact temperature sensor may be installed at a position where the recording medium is discharged from the pressure member, and the surface temperature of the toner image on the recording medium may be measured.

[0309] The toner image pressed by the pressure members 91 and 92 is solidified and fixed onto the recording paper S.

[0310] In one embodiment of the present invention, the fixing device has a pressing section equipped with a pressure member.

[0311] In one embodiment of the present invention, the pressure member includes a heating means.

[0312] In one embodiment of the present invention, the temperature of the pressure member is preferably 15° C. or higher, more preferably 20° C. or higher, even more preferably more than 20° C., even more preferably 30° C. or higher, and even more preferably 40° C. or higher. There is no particular upper limit, but it is, for example, 200° C. or lower, 150° C. or lower, or 100° C. or lower.

[0313] <Photoresponsive adhesives, photoswitching materials> Since the polymer of the present invention becomes fluid when irradiated with light and becomes non-fluid reversibly, it is possible to prepare a photoresponsive adhesive (photosensitive adhesive) or photoswitching material that can be used repeatedly using the polymer of the present invention. For example, it is possible to apply the polymer to various adhesion techniques as a photoresponsive adhesive that can be repeatedly attached and detached by light in response to changes in viscosity (friction coefficient). That is, one embodiment of the present invention is a photoresponsive adhesive or photoswitching material that includes the polymer of the present invention.

[0314] The light-responsive adhesive of the present invention can be used for temporary fixing that allows repeated use, and is also suitable for recycling, but is not limited thereto. EXAMPLES

[0315] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.

[0316] <Synthesis of azomethine derivative monomer 12>

[0317] [ka]

[0318] 4-Aminophenol (5 g, 0.046 mol), 1-methyl-1H-pyrazole-4-carbaldehyde (5.1 g, 0.046 mol), and 100 ml of ethanol were added to a 100 ml four-neck flask and heated and stirred. The reaction solution was suction filtered, and the resulting powder was washed with cooled ethanol. Further, recrystallization was performed with methanol / ethanol to obtain target product 1.

[0319] [ka]

[0320] Next, in a 200 ml four-neck flask, the target product 1 (4.6 g, 0.023 mol) obtained above was dissolved in 25 ml of dimethylformamide (DMF). To this, 4.88 g (0.035 mol) of potassium carbonate was added, and the mixture was stirred while maintaining the temperature at 30°C. To this, 10.2 mg (0.06 mmol) of potassium iodide and 10-chloro-1-decanol (5.0 g, 0.026 mol) were added, and the mixture was reacted at 110°C. This was cooled to room temperature, added to 650 g of ice, and then filtered. The crystals were dispersed in 400 ml of water, stirred overnight, washed, filtered, and dried. Furthermore, recrystallization was performed with ethanol to obtain target product 2.

[0321] [ka]

[0322] Next, the target product 2 (3.6 g, 0.01 mol) obtained above, 1.34 ml (0.01 mol) of triethylamine, and 30 ml of dichloromethane were added to a 100 ml four-neck flask. At this time, the raw materials were in a dispersed state. While maintaining the internal temperature at 0°C, a solution of 1.0 g (0.011 mol) of acrylic acid chloride dissolved in 10 ml of dichloromethane was added dropwise while maintaining the internal temperature at 0 to 5°C. As the mixture was added dropwise, the raw materials dissolved.

[0323] After the dropwise addition, the reaction solution was returned to room temperature and stirred. After the reaction was completed, dichloromethane was removed by concentration, and the solution was dissolved in ethyl acetate and washed with dilute hydrochloric acid, aqueous sodium bicarbonate solution, and saturated saline. The organic layer was dried over magnesium sulfate and then concentrated. The orange crystals obtained were purified using a silica gel column (ethyl acetate / heptane=1 / 5) to obtain azomethine derivative monomer 12.

[0324] <Synthesis of azomethine derivative monomer 1> The azomethine derivative monomer 1 was synthesized by replacing 1-methyl-1H-pyrazole-4-carbaldehyde with 5-methylthiophene-2-carboxaldehyde.

[0325] <Synthesis of azomethine derivative monomer 2> Azomethine derivative monomer 2 was synthesized by changing 1-methyl-1H-pyrazole-4-carbaldehyde to 5-hexylthiophene-2-carboxaldehyde and 10-chloro-1-decanol to 6-chloro-1-hexanol.

[0326] <Synthesis of azomethine derivative monomer 3> By changing 1-methyl-1H-pyrazole-4-carbaldehyde to 5-methylfuran-2-carboxaldehyde and 4-aminophenol to 4-aminobenzenehexanol, azomethine derivative monomer 3 was synthesized. (This synthesis method omits the step of obtaining target product 2.) <Synthesis of azomethine derivative monomer 4> The azomethine derivative monomer 4 was synthesized by replacing 1-methyl-1H-pyrazole-4-carbaldehyde with 2-formyl-1-methylpyrrole and 10-chloro-1-decanol with 8-chloro-1-octanol.

[0327] <Synthesis of azomethine derivative monomer 5> Azomethine derivative monomer 5 was synthesized by replacing 1-methyl-1H-pyrazole-4-carbaldehyde with 1-methyl-1H-pyrazole-3-carboxaldehyde.

[0328] <Synthesis of azomethine derivative monomer 6> The azomethine derivative monomer 6 was synthesized by replacing 1-methyl-1H-pyrazole-4-carbaldehyde with 1-methylpyrazole-5-carboxaldehyde.

[0329] <Synthesis of azomethine derivative monomer 7> Azomethine derivative monomer 7 was synthesized by replacing 1-methyl-1H-pyrazole-4-carbaldehyde with 1-methylimidazole-4-carboxaldehyde.

[0330] <Synthesis of azomethine derivative monomer 8> The azomethine derivative monomer 8 was synthesized by replacing 1-methyl-1H-pyrazole-4-carbaldehyde with 1-methylimidazole-5-carboxaldehyde.

[0331] <Synthesis of azomethine derivative monomer 9> Azomethine derivative monomer 9 was synthesized by changing 1-methyl-1H-pyrazole-4-carbaldehyde to 5-butylthiophene-2-carboxaldehyde, 4-aminophenol to 6-aminonaphthalen-2-ol, and 10-chloro-1-decanol to 6-chloro-1-hexanol.

[0332] <Synthesis of azomethine derivative monomer 10> Azomethine derivative monomer 10 was synthesized by changing 1-methyl-1H-pyrazole-4-carbaldehyde to 1-methyl-1H-pyrazole-3-carboxaldehyde, 4-aminophenol to 4-hydroxy-4'-aminobiphenyl, and 10-chloro-1-decanol to 4-chloro-1-butanol.

[0333] <Synthesis of azomethine derivative monomer 11> The azomethine derivative monomer 11 was synthesized by replacing 1-methyl-1H-pyrazole-4-carbaldehyde with 3-formyl-1-methylpyrrole and 10-chloro-1-decanol with 8-chloro-1-octanol.

[0334] <Synthesis of azomethine derivative monomer 13> The azomethine derivative monomer 13 was synthesized by changing 1-methyl-1H-pyrazole-4-carbaldehyde to 1-butyl-1H-pyrazole-4-carbaldehyde and 10-chloro-1-decanol to 6-chloro-1-hexanol.

[0335] <Synthesis of azomethine derivative monomer 14> The azomethine derivative monomer 14 was synthesized by changing 4-aminophenol and 1-methyl-1H-pyrazole-4-carbaldehyde to 5-methyl-2-thienylamine and 4-hydroxy-2,6-dimethylbenzaldehyde, and by changing 10-chloro-1-decanol to 6-chloro-1-hexanol.

[0336] <Synthesis of azomethine derivative monomer 15> Azomethine derivative monomer 15 was obtained in the same manner as azomethine derivative monomer 12, except that acrylic acid chloride was changed to methacrylic acid chloride.

[0337] <Synthesis of azomethine derivative monomer 16> The azomethine derivative monomer 16 was synthesized by changing 4-aminophenol and 1-methyl-1H-pyrazole-4-carbaldehyde to 5-hydroxythiophene-2-carboxaldehyde and 2-aminonaphthalene, and by changing 10-chloro-1-decanol to 4-chloro-1-butanol.

[0338] <Synthesis of azomethine derivative monomer 17> The azomethine derivative monomer 17 was synthesized by changing 4-aminophenol and 1-methyl-1H-pyrazole-4-carbaldehyde to 5-hydroxythiophene-2-carboxaldehyde and 2-phenanthrenamine, and by changing 10-chloro-1-decanol to 6-chloro-1-hexanol.

[0339] <Synthesis of azomethine derivative monomer 18> Azomethine derivative monomer 18 was synthesized by changing 4-aminophenol to 4-butoxy-1,1′-biphenyl-4-amine, 1-methyl-1H-pyrazole-4-carbaldehyde to 1-hydroxypyrazole-4-carbaldehyde, and 10-chloro-1-decanol to 6-chloro-1-hexanol.

[0340] <Synthesis of azomethine derivative monomer 19> Comparative Example Azomethine derivative monomer 19 was synthesized in the same manner as azomethine derivative monomer 12, except that 4-aminophenol was changed to 1,3-dimethyl-1-pyrrol-2-amine, 1-methyl-1H-pyrazole-4-carbaldehyde was changed to 4-hydroxybenzaldehyde, and 10-chloro-1-decanol was changed to 6-chloro-1-hexanol.

[0341] <Synthesis of azobenzene derivative monomer> Comparative Example The following comparative compound 1 (number average molecular weight Mn: 2870) was obtained by the method described in paragraphs 0217 to 0227 of JP2014-191078A.

[0342] [ka]

[0343] <Polymer 1> In a 100 ml four-neck flask, 1.8 g (4.21 mmol) of the azomethine derivative monomer 1 obtained above, 5 mg (0.023 mmol) of 4-cyanopentanoic acid dithiobenzoate, and 1 mg (0.006 mmol) of AIBN were dissolved in 4 ml of anisole.

[0344] Then, after the mixture was frozen and degassed to create an argon gas atmosphere, it was heated to 75°C and stirred for 8 hours to polymerize. 40 ml of methanol was gradually added dropwise to the obtained polymer solution, and then THF was added to remove unreacted azomethine derivative monomer 1. The separated polymer solution was dried in a vacuum drying oven at 40°C for 24 hours to obtain azomethine derivative-containing polymer 1. The number average molecular weight Mn of the obtained polymer 1 was measured by GPC and found to be 15,000.

[0345] The molecular weight distribution was measured by GPC as follows.

[0346] That is, using the apparatus "HLC-8220" (manufactured by Tosoh Corporation) and the column "TSKguardcolumn + TSKgelSuperHZM-M triple series" (manufactured by Tosoh Corporation), while maintaining the column temperature at 40 ° C., tetrahydrofuran (THF) as a carrier solvent was flowed at a flow rate of 0.2 mL / min, and the measurement sample was dissolved in tetrahydrofuran to a concentration of 1 mg / mL under dissolution conditions of processing for 5 minutes using an ultrasonic disperser at room temperature (25 ° C.), and then processed with a membrane filter with a pore size of 0.2 μm to obtain a sample solution, 10 μL of this sample solution was injected into the apparatus together with the above carrier solvent, detected using a refractive index detector (RI detector), and the molecular weight distribution of the measurement sample was calculated using a calibration curve measured using monodisperse polystyrene standard particles. As a standard polystyrene sample for calibration curve measurement, a molecular weight of 6 × 10 2 , 2.1×10 3 , 4×10 3 , 1.75×10 4 , 5.1×10 4 , 1.1×10 5 , 3.9×10 5 , 8.6×10 5 , 2×10 6 , 4.48×10 6 A calibration curve was created by measuring 10 standard polystyrene samples using a refractive index detector.

[0347] The number average molecular weight Mn was calculated from a chromatogram showing the molecular weight distribution measured by GPC as described above.

[0348] <Preparation of polymer particle dispersion 1> 80 parts by mass of dichloromethane and 20 parts by mass of the polymer 1 obtained above were mixed and stirred while being heated at 50° C. to obtain a solution containing polymer 1. A mixed liquid of 99.5 parts by mass of distilled water heated to 50° C. and 0.5 parts by mass of a 20% by mass aqueous solution of sodium dodecylbenzenesulfonate was added to 100 parts by mass of the obtained solution. Thereafter, the mixture was emulsified by stirring at 16,000 rpm for 20 minutes using a homogenizer (manufactured by Heidolph) equipped with a shaft generator 18F to obtain an emulsion of polymer 1.

[0349] The obtained emulsion was charged into a separable flask, and the organic solvent was removed by heating and stirring at 40° C. for 90 minutes while supplying nitrogen into the gas phase, to obtain polymer particle dispersion 1. The particle size of the polymer particles in polymer particle dispersion 1 was measured using Microtrac UPA-150 (manufactured by Nikkiso Co., Ltd.) and found to be 185 nm in mass average particle size.

[0350] (Preparation of Black Colorant Particle Dispersion (Bk-1)) 90 parts by mass of sodium n-dodecyl sulfate was added to 1600 parts by mass of ion-exchanged water. While stirring this solution, 320 parts by mass of carbon black "Regal 330R" (manufactured by Cabot Corporation) was gradually added to the solution, and then the solution was dispersed using a stirring device "Clearmix" (manufactured by M Technique Co., Ltd.) to prepare a black colorant particle dispersion (Bk-1). The volume-based median diameter of the colorant particles in the black colorant particle dispersion (Bk-1) was 110 nm.

[0351] (Preparation of Toner 1) Into a reaction vessel equipped with a stirrer, a temperature sensor, and a cooling tube, 480 parts by mass (solid content equivalent) of the particle dispersion of polymer 1 and 2000 parts by mass of ion-exchanged water were added. Then, while stirring at 150 rpm, a 5 mol / L aqueous sodium hydroxide solution was added to adjust the pH (25°C equivalent) to 10.

[0352] After that, 24 parts by mass (solid content equivalent) of colorant particle dispersion (Bk-1) was added, and then an aqueous solution in which 60 parts by mass of magnesium chloride was dissolved in 60 parts by mass of ion-exchanged water was added over 10 minutes at 30°C while stirring at 150 rpm. After leaving this system for 3 minutes, the temperature was raised to 70°C over 60 minutes while stirring at 200 rpm, and the particle growth reaction was continued while maintaining the temperature at 70°C. In this state, the particle size of the associated particles was measured using a Coulter Multisizer 3 (manufactured by Coulter Beckman), and the volume-based median diameter (D 50 When the particle size reached 6.1 μm, an aqueous solution of 20 parts by weight of sodium chloride dissolved in 80 parts by weight of ion-exchanged water was added to stop particle growth. After stirring at 70°C for 1 hour, the temperature was further increased, and the particles were heated and stirred at 75°C to promote fusion of the particles. The mixture was then cooled to 30°C to obtain a dispersion of toner base particles.

[0353] Next, the toner cake was subjected to solid-liquid separation, and the dehydrated toner cake was redispersed in ion-exchanged water and subjected to solid-liquid separation, which was repeated three times for washing, and then dried at 40° C. for 24 hours to obtain toner base particles.

[0354] To the obtained toner base particles, 1.5% by mass of hydrophobic silica (number average primary particle size: 12 nm) was added, and mixed using a Henschel mixer (registered trademark), toner 1 was obtained.

[0355] (Toner 2-19) Polymers 2 to 19 having the molecular weights shown in the table below were synthesized by using the azomethine derivative monomers shown in the table below and appropriately adjusting the polymerization conditions. In the table below, the structure of A refers to A in the structural unit shown in the general formula (2). Each polymer has a structural unit in which, in the general formula (2), A has the structure shown in the table below, and r1 is a hydrogen atom in polymers 1 to 14 and 16 to 19, and r1 is a methyl group.

[0356] Thereafter, in the same manner as for Toner 1, Toners 2 to 19 were obtained.

[0357] (Toner 20-23) Polymer 20 Polymer 20 was obtained in the same manner as in the synthesis of Polymer 1, except that the amount of azomethine derivative monomer 12 was 1.2 g and the amount of styrene monomer was 0.6 g.

[0358] Polymer 21-23 In the synthesis of Polymer 20, 0.6 g of styrene monomer was changed to 0.6 g of ethyl acrylate, 0.6 g of n-butyl methacrylate, and 0.3 g / 0.3 g of styrene monomer / methyl acrylate, respectively, to obtain Polymers 21 to 23.

[0359] Toner 20-23 Toners 20 to 23 were obtained in the same manner as in Toner 1 using Polymers 20 to 23.

[0360] (Toner 24~31) Polymer 24 <Synthesis of macroinitiator 24> In a 100 ml eggplant flask, 2,2'-bipyridyl (230 mg, 1.47 mmol) was added, and in a glove box under a nitrogen atmosphere, Cu(I)Br (95 mg, 0.66 mmol), styrene (15 g, 144 mmol), and ethyl 2-bromoisobutyrate (35 mg, 0.18 mmol) were added and sealed. This was heated and stirred in an oil bath at 100°C. Then, an appropriate amount of tetrahydrofuran was added, and the mixture was passed through a neutral alumina column. This was purified by reprecipitation with methanol and centrifugation to obtain macroinitiator 24. The number average molecular weight (β Mn) of the obtained macroinitiator 24 was measured by GPC method and found to be 5000.

[0361] <Synthesis of polymer 24> In a 100 ml eggplant flask, the above-obtained azomethine derivative monomer 12 (20 g, 47 mmol) and the above-mentioned macroinitiator 24 (0.92 g, 0.18 mmol) were placed, and in a glove box under a nitrogen atmosphere, Cu(I)Cl (29 mg, 0.29 mmol), 1,1,4,7,10,10-hexamethyltriethylenetetramine (136 mg, 0.59 mmol), and anisole (4.9 g, 41.1 mmol) as a solvent were added and sealed. Then, the mixture was heated and stirred in an oil bath at 80°C. Then, an appropriate amount of chloroform was added, and the mixture was passed through a basic alumina column. The mixture was purified by reprecipitation with methanol and centrifugation to obtain polymer 24. The total number-average molecular weight Mn of the obtained polymer 24 was measured by GPC method and found to be 17,000. From this, the number-average molecular weight (α Mn) of the structural unit derived from the azomethine derivative was determined to be 12,000.

[0362] Toner 24 Toner 24 was prepared in the same manner except that Polymer 24 was used in place of Polymer 1.

[0363] Polymer 25 In the preparation of macroinitiator 24, ethyl 2-bromoisobutyrate was changed to α,α'-dibromo-p-xylene to obtain macroinitiator 25. Polymer 25 was obtained in the same manner as in the synthesis of polymer 24, except that macroinitiator 24 was changed to macroinitiator 25.

[0364] Polymer 26 Macroinitiator 26 was obtained in a similar manner, except that ethyl 2-bromoisobutyrate was changed to ethylene bis(2-bromoisobutyrate), 2,2'-bipyridyl was changed to 1,1,4,7,10,10-hexamethyltriethylenetetramine, styrene was changed to azomethine derivative monomer 12, and anisole was further added.

[0365] Polymer 26 was obtained in the same manner as in the synthesis of polymer 24, except that macroinitiator 24 was changed to macroinitiator 26, 1,1,4,7,10,10-hexamethyltriethylenetetramine was changed to 2,2'-bipyridyl, azomethine derivative monomer 12 was changed to styrene, and anisole was omitted.

[0366] Polymer 27 Macroinitiator 27 was obtained in the same manner as in the synthesis of macroinitiator 24, except that ethyl 2-bromoisobutyrate was changed to 1,1,1-tris(2-bromoisobutyryloxymethyl)ethane.

[0367] Polymer 27 was obtained in the same manner as in the synthesis of Polymer 24, except that macroinitiator 24 was changed to macroinitiator 27.

[0368] Polymer 28 Macroinitiator 28 was obtained in the same manner as in the synthesis of macroinitiator 26, except that ethylene bis(2-bromoisobutyric acid) was changed to 1,1,1-tris(2-bromoisobutyryloxymethyl)ethane.

[0369] Polymer 28 was obtained in the same manner as in the synthesis of Polymer 26, except that macroinitiator 26 was changed to macroinitiator 28.

[0370] Polymer 29 Macroinitiator 29 was obtained in the same manner as in the synthesis of macroinitiator 24, except that ethyl 2-bromoisobutyrate was changed to pentaerythritol tetrakis(2-bromoisobutyrate).

[0371] Polymer 29 was obtained in the same manner as in the synthesis of Polymer 24, except that macroinitiator 24 was changed to macroinitiator 29.

[0372] Polymer 30 Macroinitiator 30 was obtained in the same manner as in the synthesis of macroinitiator 26, except that ethylene bis(2-bromoisobutyric acid) was changed to pentaerythritol tetrakis(2-bromoisobutyrate).

[0373] Polymer 30 was obtained in the same manner as in the synthesis of Polymer 26, except that macroinitiator 26 was changed to macroinitiator 30.

[0374] Polymer 31 Macroinitiator 31 was obtained in the same manner as in the synthesis of macroinitiator 25, except that styrene was changed to methyl acrylate. Polymer 31 was obtained in the same manner as in the synthesis of polymer 25, except that macroinitiator 25 was changed to macroinitiator 31.

[0375] Toner 24-31 Polymer 1 was replaced with Polymers 24-31, and toners 24-31 were obtained in the same manner.

[0376] (Toner 32) (Preparation of Styrene Acrylic Resin Particle Dispersion) A 5 L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device was charged with 5.0 parts by mass of sodium lauryl sulfate and 2,500 parts by mass of ion-exchanged water, and the internal temperature was raised to 80° C. while stirring at a stirring speed of 230 rpm under a nitrogen stream.

[0377] Next, an aqueous solution of 15.0 parts by mass of potassium persulfate (KPS) dissolved in 300 parts by mass of ion-exchanged water was added, and the liquid temperature was again adjusted to 80°C. Then, a monomer mixture consisting of 840.0 parts by mass of styrene (St), 288.0 parts by mass of n-butyl acrylate (BA), 72.0 parts by mass of methacrylic acid (MAA), and 15 parts by mass of n-octyl mercaptan was added dropwise over 2 hours. After the dropwise addition was completed, polymerization was carried out by heating and stirring at 80°C for 2 hours, and a dispersion a1 of styrene-acrylic resin A1 particles having a volume-based median diameter of 120 nm was prepared.

[0378] The styrene acrylic resin A1 had a glass transition temperature (Tg) of 52.0° C. and a weight average molecular weight (Mw) of 28,000.

[0379] Toner 32 Toner 32 was obtained in the same manner as in the preparation of toner 1, except that 480 parts by mass (solid content equivalent) of the particle dispersion of polymer 1 was changed to 336 parts by mass (solid content equivalent) of the particle dispersion of polymer 12 and 144 g (parts by mass) (solid content equivalent) of the dispersion a1 of styrene acrylic resin A1 particles.

[0380] (Toner 33) <Preparation of amorphous polyester resin dispersion> Monomers of the following composition and 0.25 parts by mass of tin dioctylate per 100 parts by mass of the monomers of the following composition were added to a reaction vessel equipped with a stirrer, a thermometer, a condenser, and a nitrogen gas inlet tube. The mixture was reacted at 235°C for 6 hours under a nitrogen gas flow, then cooled to 200°C and reacted for 1 hour. The mixture was heated to 220°C over 5 hours and polymerized under a pressure of 10 kPa until the desired molecular weight was reached, to obtain a pale yellow transparent amorphous polyester resin (B1). The weight average molecular weight of the amorphous polyester resin (B1) was 18000 and the acid value was 17.8 mgKOH / g.

[0381] Bisphenol A ethylene oxide 2 mole adduct 50.2 parts by mass Bisphenol A propylene oxide 2 mole adduct 249.8 parts by mass Terephthalic acid 82.5 parts by mass Fumaric acid 32.0 parts by mass.

[0382] 72 parts by mass of the amorphous polyester resin (B1) was added to 72 parts by mass of methyl ethyl ketone and dissolved by stirring at 30° C. for 30 minutes. 2.1 parts by mass of a 25% by mass aqueous sodium hydroxide solution was added to this oil phase liquid and placed in a reaction vessel equipped with a stirrer. While stirring the oil phase liquid, 252 parts by mass of 30° C. ion-exchanged water was added dropwise over 70 minutes and mixed. During the dropwise addition, the liquid in the vessel became cloudy, and after the entire amount was added dropwise, a uniformly emulsified emulsion was obtained.

[0383] This emulsion was heated to 60°C using a diaphragm vacuum pump V-700 (manufactured by BUCHI) and stirred for 3 hours under a reduced pressure of 15 kPa (150 mbar) to distill off the methyl ethyl ketone, preparing an amorphous polyester resin particle dispersion (B1).

[0384] Toner 33 Toner 33 was obtained in the same manner as in the preparation of toner 1, except that 480 parts by mass (solid content equivalent) of the particle dispersion of polymer 1 was changed to 336 parts by mass (solid content equivalent) of the particle dispersion of polymer 12 and 144 g (parts by mass) (solid content equivalent) of the dispersion B1 of amorphous polyester resin B1 particles.

[0385] (Comparative Example 1 Toner) Comparative toner 1 was obtained in the same manner except that azomethine derivative monomer 19 was used instead of azomethine derivative monomer 1.

[0386] (Comparative Example 2 Toner) Comparative toner 2 was obtained in the same manner except that the azomethine derivative monomer 1 was changed to an azobenzene derivative monomer.

[0387] (Preparation of developer) For the toners 1 to 33 and the toners of Comparative Examples 1 and 2 prepared above, ferrite carrier particles having a volume average particle size of 30 μm coated with a copolymer resin of cyclohexane methacrylate and methyl methacrylate (monomer mass ratio 1:1) were mixed so that the toner particle concentration was 6 mass%, thereby obtaining developers 1 to 33 and the developers of Comparative Examples 1 and 2. Mixing was performed for 30 minutes using a V-type mixer.

[0388] [Evaluation: Photoresponsive adhesion test of polymers] The change in adhesiveness of polymers 1 to 33 prepared in each example with light irradiation was evaluated by the following photoresponsive adhesive test using the apparatus shown in the figure. As shown in the figure, 2 mg of polymer was placed on a 18 mm square cover glass 1 within a radius of 6 mm from the center of the glass, and a cover glass 2 of the same size was placed at a position shifted about 4 mm in a parallel direction to the cover glass 1 so as to completely cover the polymer. This was heated to melt the sample, and the cover glass 1 and the cover glass 2 were bonded together. Each of the obtained samples was subjected to the following non-fluidity → fluidity test, and then the following fluidity → non-fluidity (return) test.

[0389] <Testing for non-liquidity → liquidity> Part (A) shown in Figure 3 was fixed to the stand with cellophane tape, and a 30 cm long vinyl string with a 100 g weight attached was fixed to part (C) with cellophane tape. Part (B) was irradiated with 365 nm light at a dose of 20 J / cm. 2 It was confirmed whether cover glass 2 peeled off from cover glass 1, and the peeling was judged according to the following evaluation criteria.

[0390] - Evaluation criteria for non-liquidity to liquidity testing - ○: Cover glass 2 was completely peeled off from cover glass 1 △: Cover glass 2 is displaced ×: The cover glass 2 did not move.

[0391] <Test for fluidity → non-fluidity (return)> After the non-fluidity → fluidity test was completed, the following experiment was performed on the samples in which the cover glass 2 had been completely peeled off and on the samples in which it had shifted. For the shifted samples, the cover glasses 1 and 2 were peeled off by hand. Five minutes after the end of the light irradiation in the non-fluidity → fluidity test (the sample was left in a natural environment, i.e., in a dark room at room temperature, for five minutes), a cover glass 3 (same size as cover glasses 1 and 2) was placed so as to cover the sample portion (part (B)) of the cover glass 1 used in the above test, and it was confirmed whether the cover glass 1 and cover glass 3 were adhered to each other, and a judgment was made according to the following evaluation criteria.

[0392] -Evaluation criteria for fluidity to non-fluidity (return) tests- 〇: Did not adhere (had become non-fluid) △: Partially adhered (partially maintained in a fluid state) ×: Adhered (fluid state was maintained).

[0393] It should be noted that, for the polymers prepared in the examples which were evaluated as ◯ in the above-mentioned fluidity → non-fluidity (reversion) test, it was confirmed that all of them re-solidified after the non-fluidity → fluidity test was carried out.

[0394] [Evaluation: Fixation test] Fixing tests were carried out under normal temperature and humidity conditions (temperature 20°C, relative humidity 50% RH) using the above-obtained developers 1 to 33 and the developers of Comparative Examples 1 and 2. The developer was placed on one side, and paper (Mondi color copy paper, basis weight: 120 g / m2) was placed on the other side as a recording medium. 2 The developer is placed between a pair of parallel flat plate (aluminum) electrodes with a magnetic force, and the gap between the electrodes is 0.5 mm. The DC bias and AC bias are set to a toner adhesion amount of 5 g / m 2 The toner was developed under the above conditions, a toner layer was formed on the surface of the plain paper, and the toner was fixed by each fixing device to obtain a print (image formation). The 1 cm square toner image on the print was rubbed 15 times with a "JK Wiper (registered trademark)" (manufactured by Nippon Paper Crecia Co., Ltd.) at a pressure of 50 kPa to evaluate the fixation rate of the image. A fixation rate of 60% or more was considered to be acceptable. The fixation rate of the image is a numerical value obtained by measuring the reflection density of the image after printing and the image after rubbing with a fluorescent spectrodensitometer "FD-7" (manufactured by Konica Minolta, Inc.), and dividing the reflection density of the solid image after rubbing by the reflection density of the solid image after printing, expressed as a percentage.

[0395] The fixing devices used were the following four types of fixing devices configured by appropriately modifying the device shown in FIG. 2: No. 1: There was no pressure bonding portion 9 in FIG. 2, heating was not performed by the heating member 93, the wavelength of the ultraviolet light irradiated from the light source 41 was 365 nm (light source: LED light source with an emission wavelength of 365 nm±10 nm), and the irradiation amount was 12 J / cm 2 is; No. 2: The pressing unit 9 in FIG. 2 is included, heating is not performed by the heating member 93, the temperature of the pressure member 91 is 20° C., and the pressure during pressing is 0.2 MPa. The light source and the irradiation amount of the irradiation unit 40 are the same as those of No. 1; 2, no heating was performed by the heating member 93, the temperature of the pressure member 91 was 50° C., and the pressure during pressing was 0.2 MPa. The light source and the irradiation amount of the irradiation unit 40 were the same as those of No. 1.

[0396] No. 4: There is no pressure bonding portion 9 in FIG. 2, the temperature of the heating member 93 is 50° C., and the wavelength and irradiation amount of the light source 41 are the same as those of No. 1. [Color reproducibility evaluation] The color reproducibility of the images of the examples and comparative examples obtained above was evaluated by visual evaluation by 10 monitors according to the following evaluation criteria. Specifically, a toner was prepared in which all of the polymer 1 was replaced with a styrene acrylic resin as a sample for evaluation comparison. A developer was prepared using this in the same manner as above, and the image was developed in the same manner as in the image formation in the fixing property test above, and fixing was performed using the fixing device No. 5 described below.

[0397] Fixing device No. 5: The pressing unit 9 in FIG. 2 was included, heating was not performed by the heating member 93, the temperature of the pressure member 91 was 150° C., the pressure during pressing was 0.2 MPa, and light irradiation was not performed.

[0398] The 10 monitors were shown the sample for evaluation and the images obtained in the above-mentioned Examples and Comparative Examples in turn, and asked whether the colors of the two images were clearly different. The results of the evaluation based on the following color reproducibility evaluation criteria are shown in Table 3 below.

[0399] -Evaluation criteria for color reproducibility- ◎: Less than 2 people answered that it was clearly different ○: 3 to 4 people answered that it was clearly different △: 5 to 7 people answered that it was clearly different ×: Eight or more people answered that it was clearly different.

[0400] [Table 13-1]

[0401] [Table 13-2]

[0402] [Table 14-1]

[0403] [Table 14-2]

[0404] [Table 14-3]

[0405] [Table 15-1]

[0406] [Table 15-2] [Explanation of symbols]

[0407] 1 photoreceptor, 2 Charger, 3 Exposure device, 4 Development section, 5 Transcription unit, 7 Paper transport system, 8 Cleaning section, 9 Crimping part, 10 Image forming unit, 11 Paper feed section, 12 Transport roller, 13 conveyor belt, 14 Paper ejection section, 15 Manual feed unit, 16 trays, 17 Thermohygrometer, 20 Image processing unit, 24 Paper reversing section, 40 Irradiation unit, 41 light source, 71 Image reading device, 72 Automatic document feeder, 85 blades, 90 control section, 91, 92 Pressurizing member, 93 Heating member, 100 Image forming apparatus, d manuscript, S Recording paper.

Claims

1. A photoresponsive polymer which contains a structural unit derived from an azomethine derivative represented by the following general formula (2), and which becomes fluid and reversibly non-fluid upon irradiation with light: [Formula 1] In the general formula (2), r 1 is a hydrogen atom or a methyl group; A is represented by the following general formula (1-1) or the following general formula (1-2): [chemical 2] [C3] In the formula, * represents a bonding point, G is a divalent group, and Z 1 and Z 2 is N or CH, with the proviso that Z 1 ≠Z 2 and R 1 contains an aromatic hydrocarbon structure, R 2 contains an aromatic heterocyclic structure; The "Z 2 -R 2 " structure is as follows: [C4] In this case, at least two of X, Y, P and Q are carbon atoms, and the rest are nitrogen atoms, sulfur atoms or oxygen atoms, provided that at least one of X and Y is a carbon atom, and R a , R b , R c and R d , when present according to the valences of X, Y, P and Q, are each independently an alkyl group having 1 to 18 carbon atoms, an alkoxy group having 1 to 18 carbon atoms or a hydrogen atom, provided that at least one of R a and R b bonded to a carbon atom is a hydrogen atom, and R a and R b , as well as R c and R d , may each independently form a fused ring.

2. 2. The photoresponsive polymer according to claim 1, wherein G is an alkylene group or an oxyalkylene group having 1 to 18 carbon atoms.

3. Said Z 23. The photoresponsive polymer according to claim 1 , wherein all of the atoms bonded adjacent to the carbon atom in the aromatic heterocyclic structure bonded to the group represented by the formula (I) are carbon atoms, and all of the carbon atoms are bonded to a hydrogen atom.

4. the P and the Q are nitrogen atoms, The X and the Y are both carbon atoms, and the R a and the R b are all hydrogen atoms, The R c and R d 4. The photoresponsive polymer according to claim 1, wherein at least one of the above is an alkyl group having 4 or more carbon atoms.

5. The photoresponsive polymer according to any one of claims 1 to 4, having a number average molecular weight Mn of 3,000 or more.

6. The photoresponsive polymer according to any one of claims 1 to 5, further comprising another structural unit derived from a monomer having a vinyl-based polymerizable group.

7. The photoresponsive polymer according to claim 6 , wherein the monomer having a vinyl-based polymerizable group is at least one selected from the group consisting of styrene derivatives, (meth)acrylic acid derivatives, and olefin derivatives.

8. The following general formula (3): [C9] It is expressed as Each α is independently a polymer block containing a structural unit represented by general formula (2), The photoresponsive polymer according to any one of claims 1 to 7, wherein each β is independently a polymer block containing a structural unit other than the structural unit represented by the general formula (2).

9. The number average molecular weight of the α is 1000 or more, The number average molecular weight of β is 1000 or more, The photoresponsive polymer according to claim 8 , having a total number average molecular weight of 3,000 or more.

10. The photoresponsive polymer according to claim 8 or 9, wherein the β is a polymer block containing at least one structural unit selected from the group consisting of styrene derivatives, (meth)acrylic acid derivatives, and olefin derivatives.

11. The photoresponsive polymer according to any one of claims 1 to 10, wherein the wavelength of the light in the light irradiation is 280 nm or more and 480 nm or less.

12. A toner comprising the photoresponsive polymer according to any one of claims 1 to 11 as a binder resin.

13. The toner according to claim 12, further comprising another binder resin.

14. The toner according to claim 13, wherein the other binder resin comprises at least one selected from the group consisting of a styrene-acrylic resin and a polyester resin.

15. forming a toner image on a recording medium, the toner image being made of the toner according to any one of claims 12 to 14; irradiating the toner image with light to soften the toner image; An image forming method comprising:

16. The image forming method according to claim 15, wherein the wavelength of the light is 280 nm or more and 480 nm or less.

17. 17. The image forming method according to claim 15, further comprising a step of pressing the toner image.

18. The image forming method according to claim 17, further comprising the step of: further heating the toner image in the step of pressing.

19. The image forming method according to claim 18, wherein the heating temperature is higher than 20°C.

20. 18. The image forming method according to claim 15, wherein in the step of irradiating the toner image with light to soften the toner image, the toner image is heated in addition to being irradiated with light.

21. A photoresponsive adhesive comprising the photoresponsive polymer according to any one of claims 1 to 11.

22. A light switching material comprising the photoresponsive polymer according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Carbazole ring-containing monomer, carbazole ring-containing polymer and production thereof

    JP1993323298A

  • Liquid crystal polymer and its production

    JP1996092324A

  • Optical film, polarizing plate and liquid crystal display device

    JP2002107539A

  • Photoresponsive liquid crystal compound

    JP2011256155A

  • Toner for electrostatic charge image development and manufacturing method of the same