Semiconductor device manufacturing method

By controlling the oxidation process and using a nitrogen-containing gas to form a silicon nitride oxide film with specific thickness ratios in SiC trench gate structures, the method addresses dielectric breakdown and enhances transistor performance in semiconductor devices.

JP7555467B2Active Publication Date: 2024-09-24ROHM CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023188783
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2008-12-26
Filing Date
2023-11-02
Publication Date
2024-09-24
Estimated Expiration
2029-12-24

AI Technical Summary

Technical Problem

Existing semiconductor devices using SiC trench gate structures face challenges in suppressing dielectric breakdown and maintaining efficient transistor operation due to uneven oxidation rates of gate trench surfaces, leading to potential electric field concentration and increased on-resistance.

Method used

The method involves forming a gate trench in a SiC semiconductor layer, where the inner surfaces are oxidized using a nitrogen-containing gas at controlled temperatures to create a silicon nitride oxide film with a specific thickness ratio, and incorporating a polysilicon source wiring with a titanium intermediate layer to improve channel mobility and connection reliability.

Benefits of technology

This approach effectively suppresses dielectric breakdown, enhances channel mobility, and improves connection reliability by maintaining optimal thickness ratios and reducing on-resistance in the semiconductor device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007555467000024
    Figure 0007555467000024
  • Figure 0007555467000008
    Figure 0007555467000008
  • Figure 0007555467000032
    Figure 0007555467000032
Patent Text Reader

Abstract

To provide a manufacturing method of a semiconductor device in which a SiC is used.SOLUTION: A manufacturing method of a semiconductor device contains: a first step of forming a carbon film 83 onto a front surface of an epitaxial layer 51 as a SiC semiconductor layer of a first conductive type having a body formation region and a source formation region on a SiC substrate 42; a second step of forming a body region 53 of a second conductive type on a front layer part of the SiC semiconductor layer, a source region 55 of the first conductive type on a front layer part of the body region, and a drain region 54 of the first conductive type on a back surface side of the SiC semiconductor layer to the source region of the first conductive type and the body region on the front layer part of the body region; and a third step of forming a gate insulation film so as to oxidize the SiC semiconductor layer as well as removing the carbon film. The first step contains a step of holding a temperature to a first temperature for a predetermined time. The second step contains a step of holding the temperature to a second temperature higher than the first temperature for the predetermined time.SELECTED DRAWING: Figure 5M
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a semiconductor device using SiC. [Background technology]

[0002] In recent years, the use of SiC (silicon carbide) has been considered as a next-generation power device material that will achieve high breakdown voltage and low on-resistance.

[0003] In addition, the trench gate structure is known as a structure for miniaturizing power devices and reducing on-resistance. For example, power MOSFETs that adopt the trench gate structure are becoming mainstream.

[0004] FIG. 11 is a schematic cross-sectional view of a semiconductor device having a conventional trench-gate type VDMOSFET using SiC.

[0005] The semiconductor device 201 has a structure in which unit cells of a trench-gate type VDMOSFET are arranged in a matrix.

[0006] The semiconductor device 201 is made of a N + The SiC substrate 202 is provided with an N-type SiC substrate 202. On the Si surface (silicon surface) of the SiC substrate 202, there is provided an N-type SiC substrate 202. The N-type SiC substrate 202 is provided with an N-type SiC substrate 202. The N-type SiC substrate 202 is provided with an N-type SiC substrate 202. - The epitaxial layer 203 is a N type epitaxial layer that is maintained in the same state as after epitaxial growth. - The epitaxial layer 203 has a P-type drain region 204 formed thereon. A P-type body region 205 is formed in contact with the drain region 204 in the epitaxial layer 203.

[0007] A gate trench 206 is formed in the epitaxial layer 203 by digging down from a surface 217 (Si surface) thereof. The gate trench 206 penetrates the body region 205 in the layer thickness direction, and its deepest part (bottom surface 216) reaches the drain region 204.

[0008] In the gate trench 206, a side surface 214 and a bottom surface 216 of the gate trench 206 are thermally oxidized to form a SiO 2 A gate insulating film 207 made of is formed on the entire inner surface of the gate trench 206 .

[0009] The inside of the gate insulating film 207 is filled with polysilicon doped with a high concentration of N-type impurities, thereby forming a gate electrode 208 in the gate trench 206 .

[0010] In the surface layer of the epitaxial layer 203, N + A source region 209 of a type is formed in the gate trench 206. The source region 209 extends in a direction along the gate width along the gate trench 206, and has a bottom portion in contact with the body region 205 from the surface 217 side of the epitaxial layer 203.

[0011] The epitaxial layer 203 has a P + A mold body contact region 210 is formed.

[0012] On the epitaxial layer 203, SiO 2 An interlayer insulating film 211 made of is laminated on the gate insulating film 207. A source wiring 212 is formed on the interlayer insulating film 211. The source wiring 212 has a nickel silicide layer 218 that is in contact with the source region 209 and the body contact region 210 via a contact hole 213 formed in the interlayer insulating film 211 and the gate insulating film 207, and an aluminum layer 219 formed on the nickel silicide layer 218.

[0013] A drain wiring 215 is formed on the back surface (carbon surface: C surface) of the SiC substrate 202. The drain wiring 215 has a nickel silicide layer 220 in contact with the SiC substrate 202, and an aluminum layer 221 formed on the nickel silicide layer 220.

[0014] When a predetermined voltage (a voltage equal to or higher than the gate threshold voltage) is applied to the gate electrode 208 while a predetermined potential difference is generated between the source wiring 212 and the drain wiring 215 (between the source and drain), a channel is formed in the body region 205 near the interface with the gate insulating film 207 due to an electric field from the gate electrode 208. As a result, a current flows between the source wiring 212 and the drain wiring 215, and the VDMOSFET is turned on. [Prior art documents] [Patent documents]

[0015] [Patent Document 1] JP 2007-258465 A Summary of the Invention [Means for solving the problem]

[0016] A method for manufacturing a SiC semiconductor device according to one embodiment of the present invention is a method for manufacturing a SiC semiconductor device in which a MOSFET is formed, the MOSFET having a front surface and a back surface, a gate trench formed on the front surface side of a SiC semiconductor layer of a first conductivity type, and a drain region of a first conductivity type formed on the back surface side of the SiC semiconductor layer, the method comprising the steps of: forming a body formation region in which second conductivity type ions are selectively implanted so that a part of the body formation region is exposed to an inner surface of the gate trench; and forming a source formation region in which first conductivity type ions are selectively implanted on the front surface side of the body formation region so that a part of the source formation region is exposed to an inner surface of the gate trench; the first step of forming a carbon film in a shape that conforms to the surface; a second step of forming a body region of a second conductivity type in the SiC semiconductor layer and a source region of a first conductivity type on the surface side of the body region by heating the SiC semiconductor layer on which the carbon film is formed and activating ions in the body formation region and the source formation region; a third step of forming a gate insulating film along the inner surface of the gate trench after removing the carbon film; and a step of embedding polysilicon in the gate trench, wherein the first step includes a step of holding at a first temperature for a predetermined time, and the second step includes a step of holding at a second temperature higher than the first temperature for a predetermined time. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view of a semiconductor device according to a first embodiment of the present invention. [Figure 2A] FIG. 2A is a schematic cross-sectional view for explaining a method for manufacturing the semiconductor device shown in FIG. [Figure 2B] FIG. 2B is a diagram showing the next step of FIG. 2A. [Figure 2C] FIG. 2C is a diagram showing the next step of FIG. 2B. [Figure 2D] FIG. 2D is a diagram showing the next step of FIG. 2C. [Figure 2E] FIG. 2E is a diagram showing the next step of FIG. 2D. [Figure 2F] FIG. 2F is a diagram showing the next step of FIG. 2E. [Figure 2G] FIG. 2G is a diagram showing the next step of FIG. 2F. [Figure 2H] FIG. 2H is a diagram showing the next step of FIG. 2G. [Figure 2I] FIG. 2I is a diagram showing the next step of FIG. 2H. [Figure 2J] FIG. 2J is a diagram showing the next step of FIG. 2I. [Figure 2K] FIG. 2K is a diagram showing the next step of FIG. 2J. [Figure 2L] FIG. 2L is a diagram showing the next step of FIG. 2K. [Figure 2M] FIG. 2M is a diagram showing the next step of FIG. 2L. [Figure 2N] FIG. 2N is a diagram showing the next step of FIG. 2M. [Diagram 3] 3(a) and (b) are schematic plan views of a semiconductor device according to a second embodiment of the present invention, with FIG. 3(a) showing an overall view and FIG. 3(b) showing an internal enlarged view. [Figure 4] FIG. 4 is a schematic cross-sectional view of a semiconductor device according to a second embodiment of the present invention, showing a cross section taken along line IV-IV in FIG. 3(b). [Figure 5A] FIG. 5A is a schematic cross-sectional view for explaining a method for manufacturing the semiconductor device shown in FIG. [Figure 5B] FIG. 5B is a diagram showing the next step of FIG. 5A. [Figure 5C] FIG. 5C is a diagram showing the next step of FIG. 5B. [Figure 5D] FIG. 5D is a diagram showing the next step of FIG. 5C. [Figure 5E] FIG. 5E is a diagram showing the next step of FIG. 5D. [Figure 5F] FIG. 5F is a diagram showing the next step of FIG. 5E. [Figure 5G] FIG. 5G is a diagram showing the next step of FIG. 5F. [Figure 5H] FIG. 5H is a diagram showing the next step of FIG. 5G. [Figure 5I] FIG. 5I is a diagram showing the next step of FIG. 5H. [Figure 5J] FIG. 5J is a diagram showing the next step of FIG. 5I. [Figure 5K] FIG. 5K is a diagram showing the next step of FIG. 5J. [Figure 5L] FIG. 5L shows the next step of FIG. 5K. [Figure 5M] FIG. 5M is a diagram showing the next step of FIG. 5L. [Figure 5N] FIG. 5N is a diagram showing the next step of FIG. 5M. [Figure 5O] FIG. 5O is a diagram showing the next step of FIG. 5N. [Figure 5P] FIG. 5P is a diagram showing the next step of FIG. 5N. [Figure 5Q] FIG. 5Q shows the next step of FIG. 5N. [Figure 5R] FIG. 5R is a diagram showing the next step of FIG. 5N. [Figure 5S] FIG. 5S is a diagram showing the next step of FIG. 5N. [Figure 5T] FIG. 5T is a diagram showing the next step of FIG. 5N. [Figure 5U] FIG. 5U shows the next step of FIG. 5N. [Figure 6] FIG. 6 is a graph showing the temperature change in a resistance heating furnace. [Figure 7] 5 is a schematic cross-sectional view for explaining a modification of the semiconductor device shown in FIG. [Figure 8] FIG. 8 is a schematic cross-sectional view of a planar gate type semiconductor device. [Figure 9A] FIG. 9A is a schematic cross-sectional view illustrating a method for manufacturing the semiconductor device of FIG. [Figure 9B] FIG. 9B is a schematic cross-sectional view showing the step subsequent to that of FIG. 9A. [Figure 9C] FIG. 9C is a schematic cross-sectional view showing the step subsequent to that of FIG. 9B. [Figure 9D] FIG. 9D is a schematic cross-sectional view showing the step subsequent to that shown in FIG. 9C. [Figure 9E] FIG. 9E is a schematic cross-sectional view showing the step subsequent to that of FIG. 9D. [Figure 9F] FIG. 9F is a schematic cross-sectional view showing the step subsequent to that of FIG. 9E. [Figure 9G] FIG. 9G is a schematic cross-sectional view showing the step subsequent to that of FIG. 9F. [Figure 9H] FIG. 9H is a schematic cross-sectional view showing the step subsequent to that of FIG. 9G. [Figure 9I] FIG. 9I is a schematic cross-sectional view showing the step subsequent to that of FIG. 9H. [Figure 9J] FIG. 9J is a schematic cross-sectional view showing the step subsequent to that of FIG. 9I. [Figure 9K] FIG. 9K is a schematic cross-sectional view showing the step subsequent to that of FIG. 9J. [Figure 9L] FIG. 9L is a schematic cross-sectional view showing the step subsequent to that of FIG. 9K. [Figure 10] 10(a), (b), and (c) are graphs in which the thickness of the oxide film is plotted against the supply time of the oxidizing gas, where (a) is a graph for Reference Example 1, (b) is a graph for Reference Example 2, and (c) is a graph for Reference Example 3. [Figure 11] FIG. 11 is a schematic cross-sectional view of a semiconductor device having a conventional trench-gate type VDMOSFET using SiC. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0019] FIG. 1 is a schematic cross-sectional view of a semiconductor device according to a first embodiment of the present invention.

[0020] The semiconductor device 1 has a structure in which unit cells of a trench-gate type VDMOSFET are arranged in a matrix, of which only a part is shown in FIG.

[0021] The semiconductor device 1 includes a SiC substrate 2 that constitutes the base of the semiconductor device 1. The SiC substrate 2 contains a high concentration of N-type impurities (for example, 1e18 to 1e21 cm -3) is doped. The SiC substrate 2 has a front surface 21 (upper surface) which is a Si surface, and a rear surface (lower surface) which is a C surface.

[0022] The surface 21 of the SiC substrate 2 is made of SiC (silicon carbide) doped with N-type impurities at a lower concentration than the SiC substrate 2. - A type epitaxial layer 3 is laminated on the SiC substrate 2. The epitaxial layer 3 as a semiconductor layer is formed on the SiC substrate 2 by so-called epitaxial growth. The epitaxial layer 3 formed on the surface 21, which is a Si surface, is grown with the Si surface as the main growth surface. Therefore, the surface 31 of the epitaxial layer 3 formed by growth is a Si surface, similar to the surface 21 of the SiC substrate 2.

[0023] The epitaxial layer 3 has a C-face side (base layer) opposite to the Si-face side (surface layer), whose entire area remains in the same state as after epitaxial growth. - The N-type impurity concentration of the drain region 4 is, for example, 1e15 to 1e17 cm -3 It is.

[0024] On the other hand, a P-type body region 5 is formed in a surface portion of the epitaxial layer 3. The body region 5 contacts the drain region 4 from the surface 31 side (Si surface side) of the epitaxial layer 3. The P-type impurity concentration of the body region 5 is, for example, 1e16 to 1e19 cm -3 It is.

[0025] In the epitaxial layer 3, a gate trench 6 is formed by digging down from the surface 31. Although not shown in Fig. 1, a plurality of gate trenches 6 are formed at regular intervals, and they extend parallel to each other in the same direction (a direction perpendicular to the paper surface of Fig. 1; hereinafter, this direction may be referred to as "the direction along the gate width") to form, for example, a stripe structure.

[0026] The gate trenches 6 face each other with a gap therebetween, and each have a pair of planar side surfaces 7 perpendicular to the surface 31, and a bottom surface 8 having a portion parallel to the surface 31. The gate trenches 6 penetrate the body region 5 in the layer thickness direction, and their deepest part (bottom surface 8) reaches the drain region 4.

[0027] A gate insulating film 9 is formed on the inner surface of the gate trench 6 and on a surface 31 of the epitaxial layer 3 so as to cover the entire inner surface (side surface 7 and bottom surface 8) of the gate trench 6. The gate insulating film 9 is made of an oxide film containing nitrogen, for example, a silicon nitride oxide film formed by thermal oxidation using a nitrogen-containing gas. The nitrogen content (nitrogen concentration) in the gate insulating film 9 is, for example, 0.1 to 10%.

[0028] The gate insulating film 9 has a thickness T 2 However, the thickness T of the part on the side surface 7 (insulating film side portion 10) 1 Specifically, the thickness T of the insulating film side portion 10 is smaller than 1 Thickness T of the insulating film bottom 11 2 (the thickness T 2 / Thickness T of the insulating film side portion 10 1 ) is 0.3 to 1.0, preferably 0.5 to 1.0. The specific size of both thicknesses is, for example, the thickness T 1 is 300 to 1000 Å, and the thickness T 2 is 150~500Å.

[0029] The inside of the gate insulating film 9 is filled with a polysilicon material doped with a high concentration of N-type impurities, so that the gate electrode 12 is buried in the gate trench 6.

[0030] The surface layer of the body region 5 is provided with N +A source region 13 having a n-type impurity is formed in the drain region 4. The source region 13 is a region doped with a high concentration of n-type impurities, which is higher than the n-type impurity concentration of the drain region 4. The n-type impurity concentration of the source region 13 is, for example, 1e18 to 1e21 cm -3 The source region 13 extends in a direction parallel to the gate width at a position adjacent to the gate trench 6.

[0031] The epitaxial layer 3 has a P + A P-type body contact region 14 is formed in the body region 5. The body contact region 14 is a region doped with a P-type impurity at a high concentration, which is higher than the P-type impurity concentration of the body region 5. The P-type impurity concentration of the body contact region 14 is, for example, 1e18 to 1e21 cm -3 It is.

[0032] That is, the gate trenches 6 and the source regions 13 are alternately provided in a direction perpendicular to the gate width, and each extends in a direction along the gate width. A boundary between adjacent unit cells in a direction perpendicular to the gate width is set on and along the source region 13. At least one body contact region 14 is provided across two unit cells adjacent in a direction perpendicular to the gate width. The boundary between adjacent unit cells in the direction along the gate width is set so that the gate electrode 12 included in each unit cell has a constant gate width.

[0033] On the epitaxial layer 3, SiO 2 An interlayer insulating film 15 made of is laminated on the gate insulating film 9. In the interlayer insulating film 15 and the gate insulating film 9, contact holes 16 are formed to expose the surfaces of the source region 13 and the body contact region .

[0034] A source wiring 17 is formed on the interlayer insulating film 15. The source wiring 17 is in contact (electrically connected) with the source region 13 and the body contact region 14 through a contact hole 16. The source wiring 17 has a polysilicon layer 18 at a contact portion with the source region 13 and the body contact region 14, and has a metal layer 20 on the polysilicon layer 18.

[0035] The polysilicon layer 18 is a doped layer formed using doped polysilicon doped with impurities. 19 ~10 21 cm -3 It is preferable that the polysilicon layer 18 is a highly doped layer doped with an impurity at a high concentration of 10 ... s An N-type impurity such as arsenic (arsenic) or a P-type impurity such as boron (B) can be used. The polysilicon layer 18 fills the contact hole 16. The thickness of the polysilicon layer 18 varies depending on the depth of the contact hole 16, but is, for example, 5000 to 10000 Å.

[0036] The metal layer 20 is formed using, for example, aluminum (Al), gold (Au), silver (Ag), copper (Cu), alloys thereof, and metal materials containing these. The metal layer 20 forms the outermost layer of the source wiring 17, and is connected (bonded) with, for example, a metal wire. The thickness of the metal layer 20 is, for example, 1 to 5 μm.

[0037] In the source wiring 17, an intermediate layer 19 containing titanium is interposed between the polysilicon layer 18 and the metal layer 20. The intermediate layer 19 is made of a single layer containing titanium (Ti) or a plurality of layers including such a layer. The layer containing titanium can be formed using titanium, titanium nitride, or the like. The thickness of the intermediate layer 19 is, for example, 200 to 500 nm.

[0038] The source wiring 17 having the polysilicon layer 18, intermediate layer 19 and metal layer 20 as described above preferably has a laminated structure (Po-Si / Ti / TiN / Al) in which polysilicon (polysilicon layer 18), titanium (intermediate layer 19), titanium nitride (intermediate layer 19) and aluminum (metal layer 20) are laminated in this order.

[0039] A drain wiring 23 is formed on the back surface 22 of the SiC substrate 2. The drain wiring 23 is in contact (electrically connected) with the SiC substrate 2. The drain wiring 23 has a polysilicon layer 24 at a contact portion with the SiC substrate 2, and has a metal layer 26 on the polysilicon layer 24.

[0040] The polysilicon layer 24 can be formed using the same material as that constituting the above-mentioned polysilicon layer 18. The thickness of the polysilicon layer 24 is, for example, 1000 to 2000 Å.

[0041] The metal layer 26 can be formed using the same material as that of the above-mentioned metal layer 20. The metal layer 26 forms the outermost layer of the drain wiring 23, and is joined to the die pad when the SiC substrate 2 is bonded to the die pad of a lead frame, for example. The thickness of the metal layer 26 is, for example, 0.5 to 1 μm.

[0042] In the drain wiring 23, an intermediate layer 25 containing titanium is interposed between the polysilicon layer 24 and the metal layer 26. The intermediate layer 25 can be formed using the same material as that constituting the intermediate layer 19 described above.

[0043] A gate wiring 27 is in contact (electrically connected) with the gate electrode 12 via a contact hole (not shown) formed in the interlayer insulating film 15 .

[0044] With a predetermined potential difference being generated between the source wiring 17 and the drain wiring 23 (between the source and drain), a predetermined voltage (a voltage equal to or higher than the gate threshold voltage) is applied to the gate wiring 27, whereby an electric field from the gate electrode 12 forms a channel in the body region 5 near the interface with the gate insulating film 9. As a result, a current flows between the source wiring 17 and the drain wiring 23, turning the VDMOSFET on.

[0045] 2A to 2N are schematic cross-sectional views illustrating a method for manufacturing the semiconductor device shown in FIG.

[0046] First, as shown in Fig. 2A, a SiC crystal is grown on the surface 21 (Si surface) of the SiC substrate 2 while doping with impurities by epitaxial growth methods such as CVD (Chemical Vapor Deposition), LPE (Liquid Phase Epitaxy), and MBE (Molecular Beam Epitaxy). - A P-type epitaxial layer 3 is formed. Then, P-type impurities are implanted into the epitaxial layer 3 from a surface 31 of the epitaxial layer 3. The implantation conditions at this time vary depending on the type of P-type impurity, but for example, the acceleration energy is 200 to 400 keV.

[0047] 2B, a region where P-type impurities are implanted (P-type implant region 28) is formed in the surface layer portion of the epitaxial layer 3. By forming the P-type implant region 28, a drain region 4 is formed in the base layer portion of the epitaxial layer 3, which is separated from the P-type implant region 28 and maintains the state after epitaxial growth.

[0048] Next, as shown in FIG. 2C, SiO 2A mask 29 made of is formed. Subsequently, the mask 29 is etched via a photoresist (not shown) to be patterned into a pattern having openings 30 in regions where the body contact regions 14 are to be formed. After the openings 30 are formed, P-type impurities are implanted from a surface 31 of the epitaxial layer 3 into the interior of the epitaxial layer 3. The implantation conditions at this time vary depending on the type of P-type impurity, but for example, the acceleration energy is 30 to 200 keV. As a result, a region where the P-type impurity is implanted at a high concentration (P + A P-type implantation region 32 is formed. After the P-type impurity is implanted, the mask 29 is removed.

[0049] Next, as shown in FIG. 2D, SiO 2 is grown on the epitaxial layer 3 by a CVD (Chemical Vapor Deposition) method. 2 A mask 33 consisting of a mask 33 is then formed. The mask 33 is then etched via a photoresist (not shown) to be patterned into a pattern having an opening 34 in a region where the source region 13 is to be formed. After the opening 34 is formed, an N-type impurity is implanted from the surface 31 of the epitaxial layer 3 into the interior of the epitaxial layer 3. The implantation conditions at this time vary depending on the type of N-type impurity, but are, for example, an acceleration energy of 30 to 200 keV. After the N-type impurity is implanted, the mask 33 is removed. As a result, a region where the N-type impurity is heavily implanted (N + A mold implantation region 35) is formed.

[0050] 2E, the epitaxial layer 3 is heat-treated, for example, at 1400 to 2000° C. This activates the implanted N-type and P-type impurities to form a body region 5 in the surface layer portion of the epitaxial layer 3, and also forms a source region 13 and a body contact region 14 in the surface layer portion of the body region 5.

[0051] Next, as shown in FIG. 2F, SiO is formed on the entire surface 31 of the epitaxial layer 3 by a CVD method, a thermal oxidation method, or the like. 2 The mask 36 may be formed of SiN or the like by utilizing a CVD method.

[0052] Next, as shown in FIG. 2G, the mask 36 is etched through a photoresist (not shown) to be patterned into a pattern having openings 37 in areas where the gate trenches 6 are to be formed.

[0053] Then, as shown in FIG. 2H, SF6 (sulfur hexafluoride) and O 2 (Oxygen) containing mixed gas (SF6 / O 2 Gas) is incident on surface 31 of epitaxial layer 3 through opening 37. As a result, epitaxial layer 3 is dry etched from surface 31 (Si surface) to form gate trench 6 having bottom surface 8 with a portion (Si surface) parallel to surface 31 and side surface 7 perpendicular to the Si surface. After gate trench 6 is formed, mask 36 is removed.

[0054] 2I, the SiC substrate 2 is carried into a diffusion furnace, and a nitrogen-containing gas is supplied into the diffusion furnace while the inside of the furnace is heated, whereby the inner surface (side surface 7 and bottom surface 8) of the gate trench 6 and the surface 31 of the epitaxial layer 3 are thermally oxidized. 2 O gas, NO gas, or the like can be used. The heater temperature (heating temperature) of the diffusion furnace is, for example, 1200 to 1350° C., and the supply time (oxidation time) of the nitrogen-containing gas is, for example, 3 to 5 hours. Since the gate trench 6 is formed in the epitaxial layer 3 made of SiC, the oxidation of the inner surface of the gate trench 6 proceeds under the condition that the oxidation rate of the bottom surface 8 having the Si surface and the oxidation rate of the side surface 7 which is a surface perpendicular to the Si surface satisfy the relational expression: oxidation rate of bottom surface 8 / oxidation rate of side surface 7<0. As a result, a gate insulating film 9 is formed in which the thickness of the portion on the bottom surface 8 (insulating film bottom portion 11) is smaller than the thickness of the portion on the side surface 7 (insulating film side portion 10).

[0055] 2J, a doped polysilicon material is deposited on the epitaxial layer 3 by a CVD method. The deposited polysilicon material is etched back until the etched back surface is flush with the surface 31 of the epitaxial layer. This removes the portion of the polysilicon material outside the gate trench 6, and a gate electrode 12 made of the polysilicon material remaining in the gate trench 6 is formed.

[0056] Next, as shown in FIG. 2K, SiO 2 Then, the interlayer insulating film 15 and the gate insulating film 9 are patterned to form contact holes 16 in the interlayer insulating film 15 and the gate insulating film 9, which expose the source region 13 and the body contact region 14.

[0057] Next, as shown in FIG. 2L, a polysilicon material 38 is deposited by CVD until the contact hole 16 is completely filled.

[0058] 2M, N-type or P-type impurities are implanted into the deposited polysilicon material 38. The implantation conditions at this time vary depending on the type of impurity, but for example, the acceleration energy is 10 to 100 keV. As a result, a polysilicon layer 18 doped with the impurity at a high concentration is formed.

[0059] Next, as shown in FIG. 2N, titanium and titanium nitride are deposited in this order on the surface of the polysilicon layer 18 by a method such as sputtering or vapor deposition to form an intermediate layer 19. Then, aluminum is deposited on the surface of the intermediate layer 19 by a method such as sputtering or vapor deposition to form a metal layer 20. Then, the metal layer 20, the intermediate layer 19, and the polysilicon layer 18 are patterned into a predetermined wiring pattern to form a source wiring 17. Then, a gate wiring 27 connected to the gate electrode 12 is formed. Then, a drain wiring 23 having a polysilicon layer 24, an intermediate layer 25, and a metal layer 26 is formed on the rear surface 22 of the SiC substrate 2 by the same method as the source wiring 17.

[0060] Through the above steps, the semiconductor device 1 shown in FIG. 1 is obtained.

[0061] As described above, in the semiconductor device 1, the gate trench 6 is formed by digging down from the surface 31 (Si surface) of the epitaxial layer 3 made of SiC. Therefore, the oxidation of the inner surface of the gate trench 6 proceeds under the condition that the oxidation rate of the bottom surface 8 having the Si surface and the oxidation rate of the side surface 7 which is a surface perpendicular to the Si surface satisfy the relation: oxidation rate of bottom surface 8 / oxidation rate of side surface 7<0.

[0062] In the above-mentioned manufacturing method, the oxidation of the inner surface of the gate trench 6 is performed by thermal oxidation using oxygen gas (dry oxidation) or water vapor (H 2 Unlike thermal oxidation (wet oxidation) using O gas, thermal oxidation is performed using a nitrogen-containing gas. Therefore, the ratio of the oxidation rate of the bottom surface 8 to the oxidation rate of the side surface 7 (oxidation rate of the bottom surface 8 / oxidation rate of the side surface 7) can be made larger than when the gate insulating film is formed by dry oxidation or wet oxidation.

[0063] The gate insulating film 9 thus formed has a thickness T 1 Thickness T of the insulating film bottom 11 2 (the thickness T 2 / Thickness T of the insulating film side portion 10 1) is in the range of 0.3 to 1.0.

[0064] The thickness T of the insulating film bottom 11 is set to a value sufficient to suppress dielectric breakdown. 2 Even if the thickness T 2 Since the lower limit of the thickness T1 of the insulating film side portion 10 is 0.3, the thickness T 1 On the other hand, since the upper limit is 1.0, the thickness T 2 When the thickness T of the insulating film side portion 10 is appropriately designed, 1 As a result, the thickness T of the insulating film bottom portion 11 is not excessively small. 2 By appropriately designing the thickness T of the insulating film side portion 10, 1 It is possible to suppress an increase in the dielectric breakdown of the insulating film bottom portion 11 while suppressing the dielectric breakdown.

[0065] Furthermore, since the gate insulating film 9 is made of a silicon oxynitride film formed by thermal oxidation using a nitrogen-containing gas, the channel mobility of the VDMOSFET can be improved.

[0066] 3(a) and (b) are schematic plan views of a semiconductor device according to a second embodiment of the present invention, with FIG. 3(a) showing an overall view and FIG. 3(b) showing an internal enlarged view.

[0067] The semiconductor device 41 is a trench-gate type power VDMOSFET (discrete element) using SiC, and has, for example, a square chip shape in a plan view. The chip-shaped semiconductor device 41 has a length of about several mm in the left-right (up-down) direction on the paper surface of FIG. 3(a).

[0068] The semiconductor device 41 has a SiC substrate 42 and a large number of unit cells 44 formed on the SiC substrate 42 and partitioned by gate trenches 43 having a lattice shape in plan view. That is, on the SiC substrate 42, rectangular parallelepiped unit cells 44 arranged in each window portion of the lattice-shaped gate trenches 43 are aligned in a matrix. Each unit cell 44 has a length of, for example, 10 μm or less in the left-right (up-down) direction on the paper surface of FIG. 3(b), and a source trench 45 having a square shape in plan view is formed in the center of the unit cell 44, which is dug down from the front surface side to the SiC substrate 42 side.

[0069] A source pad 46 is formed on the surface of the semiconductor device 41. The source pad 46 has a generally square shape in plan view with the four corners curved outward, and is formed so as to cover almost the entire surface of the semiconductor device 41. A removal region 47 is formed in the source pad 46, which is a region that has been partially removed and has a generally square shape in plan view, slightly to the left in the left-right direction on the paper surface of FIG.

[0070] A gate pad 48 is disposed in the removed region 47. A space is provided between the gate pad 48 and the source pad 46, and they are insulated from each other.

[0071] FIG. 4 is a schematic cross-sectional view of the semiconductor device according to the second embodiment of the present invention, showing a cross section taken along line IV-IV in FIG.

[0072] The cross-sectional structure of the semiconductor device 41 will be described with reference to FIG. + Type (for example, concentration is 1e18~1e21cm -3 The SiC substrate 42 has a front surface 49 (upper surface) which is a Si surface, and a rear surface 50 (lower surface) which is a C surface.

[0073] On the SiC substrate 42, a lower concentration of N is formed. - Type (for example, concentration is 1e15~1e17cm -3) is laminated on the SiC substrate 42. The epitaxial layer 51 as a semiconductor layer is formed on the SiC substrate 42 by so-called epitaxial growth. The epitaxial layer 51 formed on the surface 49 which is a Si face is grown with the Si face as the main growth surface. Therefore, the surface 52 of the epitaxial layer 51 formed by growth is a Si face, like the surface 49 of the SiC substrate 42.

[0074] A P-type body region 53 is formed in a wide area in the form of a well on the surface 52 side (Si surface side) of the epitaxial layer 51. The concentration of the P-type body region 53 is, for example, 1e16 to 1e19 cm -3 In the epitaxial layer 51, the region closer to the SiC substrate 42 (C-face side) than the body region 53 is maintained in the same state as after the epitaxial growth. - The n-type drain region 54 (drift region) is a n-type drain region 54.

[0075] In the body region 53, N is present in almost the entire area on the surface 52 side. + Type (for example, concentration is 1e18~1e21cm -3 ) source region 55, and P + Type (for example, concentration is 1e18~1e21cm -3 ) are formed in the body contact region 56. A large number of body contact regions 56 are formed in a matrix.

[0076] Then, the source trenches 45 are formed so as to penetrate each of the body contact regions 56 in the same number as the body contact regions 56, and the lattice-shaped gate trenches 43 are formed so as to surround each of the body contact regions 56 in which the source trenches 45 are formed. As a result, a large number of unit cells 44, each of which functions as a field effect transistor, are formed in the epitaxial layer 51. That is, in the unit cell 44, the body contact region 56 is formed so as to surround the source trench 45, and the body region 53 is formed so as to surround the body contact region 56. The side of the body region 53 opposite to the body contact region 56 side is exposed on the side surface of the gate trench 43. In the unit cell 44, the depth direction of the gate trench 43 is the gate length direction, and the circumferential direction of each unit cell 44 perpendicular to the gate length direction is the gate width direction.

[0077] Both the source trench 45 and the gate trench 43 extend from the surface 52 of the epitaxial layer 51 through the body region 53 to reach the drain region 54, and in this embodiment, they have the same depth. A distance D1 between a side surface 59 of the source trench 45 and a side surface 57 of the gate trench 43 is, for example, 0.5 to 3 μm. If the distance D1 is within this range, an increase in the resistance value (on-resistance) when each unit cell 44 is turned on can be suppressed, and the electric field applied to the bottom of the gate trench 43 can be alleviated.

[0078] The gate trench 43 has both end corners 61 in a direction perpendicular to the gate width at its bottom (opposing direction to the adjacent unit cell 44) curved toward the drain region 54, and has a U-shaped cross section in which the opposing side surfaces 57 and bottom surface 58 are continuous via the curved surfaces. Furthermore, like the gate trench 43, the source trench 45 also has a U-shaped cross section in which the opposing side surfaces 59 and bottom surface 60 are continuous via the curved surfaces. This allows the electric field applied to the both end corners 61 at the bottom of the gate trench 43 to be dispersed to parts other than the both end corners 61 when the unit cell 44 is turned off, thereby suppressing insulation breakdown in the part of the gate insulating film 63 on the bottom surface 58 (insulating film bottom portion 64) described later.

[0079] In the drain region 54, an implantation active layer 62 is formed as an implantation layer formed by implantation of P-type impurities (e.g., B (boron), Al (aluminum) etc.) in a portion from the bottom surface 58 of the gate trench 43 to the middle part in the thickness direction. The implantation active layer 62 is formed in a lattice shape overlapping the gate trench 43 in a plan view, and has a width narrower than the distance between adjacent unit cells 44. In this embodiment, the depth of the implantation active layer 62 is, for example, 0.1 to 0.5 μm.

[0080] The implantation active layer 62 is a high resistance layer having a resistance higher than that of the surrounding region (for example, the drain region 54) in the epitaxial layer 51, and the resistance value is, for example, several tens of kΩ / sq. The P-type impurity concentration of the implantation active layer 62 is, for example, 1e16 to 1e21 cm -3 It is.

[0081] A gate insulating film 63 is formed on the inner surface of the gate trench 43 so as to cover the entire area. The gate insulating film 63 is made of an oxide film containing nitrogen, for example, a silicon nitride oxide film formed by thermal oxidation using a gas containing nitrogen and oxygen. The nitrogen content (nitrogen concentration) in the gate insulating film 63 is, for example, 0.1 to 10%.

[0082] The gate insulating film 63 has a thickness T 4 However, the thickness T of the portion on the side surface 57 of the gate trench 43 (the insulating film side portion 65) 3 smaller than thickness T 3 for thickness T 4 Ratio of thickness T 4 / Thickness T 3 ) is 0.3 to 1.0, preferably 0.5 to 1.0. The specific size of both thicknesses is, for example, the thickness T 3 is 300-1000 Å, and the thickness T 4 The thickness T of the insulating film side portion 65 is 150 to 500 Å. 3 If is in the above range, the semiconductor device 41 can be operated with an appropriate gate-on voltage, and efficient transistor operation can be achieved.

[0083] The inside of the gate insulating film 63 is filled with a polysilicon material doped with a high concentration of N-type impurities, thereby embedding a gate electrode 66 in the gate trench 43 .

[0084] On the epitaxial layer 51, SiO 2 An interlayer insulating film 67 made of is laminated on the gate insulating film 63. In the interlayer insulating film 67 and the gate insulating film 63, a contact hole 68 is formed to expose the surfaces of the source trench 45 and the source region 55 of each unit cell 44.

[0085] A source wiring 69 is formed on the interlayer insulating film 67. The source wiring 69 enters the source trenches 45 of all the unit cells 44 collectively through each contact hole 68, and in each unit cell 44, it contacts the drain region 54, the body contact region 56, and the source region 55 in that order from the bottom side of the source trench 45. That is, the source wiring 69 is a common wiring for all the unit cells 44. An interlayer insulating film (not shown) is formed on the source wiring 69, and the source wiring 69 is electrically connected to the source pad 46 (see FIG. 3(a)) through the interlayer insulating film (not shown). On the other hand, the gate pad 48 (see FIG. 3(a)) is electrically connected to the gate electrode 66 through a gate wiring (not shown) routed on the interlayer insulating film (not shown).

[0086] The source wiring 69 has, in this order from the contact side with the epitaxial layer 51 , a polysilicon layer 70 , an intermediate layer 71 , and a metal layer 72 .

[0087] The polysilicon layer 70 is a doped layer formed using doped polysilicon doped with impurities, and has a dopant concentration of, for example, 1e19 to 1e21 cm -3 The polysilicon layer 70 is a highly doped layer doped with impurities at a high concentration of 1000 Å. When forming the polysilicon layer 70 as a doped layer (including a highly doped layer), N-type impurities such as N (nitrogen), P (phosphorus), and As (arsenic) and P-type impurities such as Al (aluminum) and B (boron) can be used as impurities. The thickness of the polysilicon layer 70 is, for example, 5000 to 10000 Å.

[0088] In this embodiment, the polysilicon layer 70 is formed to cover the entire surface of the unit cell 44 exposed in the contact hole 68, and contacts the drain region 54, the body contact region 56, and the source region 55 in the source trench 45.

[0089] By using polysilicon for the contact layers of the source wiring 69 with the drain region 54, the body contact region 56, and the source region 55, the source wiring 69 can be made to have an ohmic junction with both the body contact region 56, which is a high-concentration impurity region, and the source region 55. On the other hand, with respect to the low-concentration drain region 54, a heterojunction junction with a junction barrier smaller than the diffusion potential of the body diode 73 (PN diode formed by the junction between the body region 53 and the drain region 54) present in the semiconductor device 41 can be formed.

[0090] Incidentally, when a current flows through the body diode 73 in the semiconductor device 41, holes that have moved from the body region 53 to the drain region 54 recombine with electrons in the drain region 54, and the resulting binding energy may cause defects in the SiC crystal in the epitaxial layer 51 to spread in-plane. Since these crystal defects have a high resistance, if the crystal defects spread toward the gate trench 43 side, they may interfere with normal transistor operation, causing an increase in on-resistance.

[0091] In contrast, as in this embodiment, if a heterojunction is formed by contact between the polysilicon layer 70 and the drain region 54, even if a reverse voltage is applied between the source and drain and a current flows through the body diode 73, the current can be made to flow preferentially to the heterojunction side rather than the body diode 73 side. As a result, the expansion of crystal defects in SiC can be prevented, and an increase in on-resistance can be suppressed.

[0092] The intermediate layer 71 is laminated on the polysilicon layer 70, and is made of a single layer containing Ti (titanium) or a plurality of layers including such a layer. The layer containing Ti can be formed using Ti, TiN (titanium nitride), etc. The thickness of the intermediate layer 71 is, for example, 200 to 500 nm.

[0093] The metal layer 72 is laminated on the intermediate layer 71, and is formed using, for example, Al (aluminum), Au (gold), Ag (silver), Cu (copper), Mo (molybdenum), alloys thereof, and metal materials containing these. The metal layer 72 forms the outermost layer of the source wiring 69. The thickness of the metal layer 72 is, for example, 1 to 5 μm.

[0094] A specific example of the combination of the polysilicon layer 70, intermediate layer 71, and metal layer 72 described above is a laminated structure (Poly-Si / Ti / TiN / Al) in which Poly-Si (polysilicon layer 70), Ti (intermediate layer 71), TiN (intermediate layer 71), and Al (metal layer 72) are laminated in this order.

[0095] A drain electrode 74 is formed to cover the entire back surface 50 of the SiC substrate 42. This drain electrode 74 is a common electrode for all the unit cells 44. An example of the drain electrode 74 is a laminated structure (Ti / Al) in which Ti and Al are laminated in this order from the SiC substrate 42 side.

[0096] When a predetermined voltage (a voltage equal to or higher than the gate threshold voltage) is applied to the gate pad 48 while a predetermined potential difference is generated between the source pad 46 (source wiring 69) and the drain electrode 74 (between the source and drain), a channel is formed in the body region 53 near the interface with the gate insulating film 63 due to the electric field from the gate electrode 66. As a result, a current flows between the source wiring 69 and the drain electrode 74, and the VDMOSFET is turned on.

[0097] 5A to 5U are schematic cross-sectional views illustrating a method for manufacturing the semiconductor device shown in FIG.

[0098] First, as shown in Fig. 5A, a SiC crystal is grown on a surface 49 (Si surface) of a SiC substrate 42 while doping with impurities by epitaxial growth such as CVD (Chemical Vapor Deposition), LPE (Liquid Phase Epitaxy), or MBE (Molecular Beam Epitaxy). - A mold epitaxial layer 51 is formed.

[0099] 5B, P-type impurities are implanted into the epitaxial layer 51 from the surface 52 of the epitaxial layer 51. The implantation conditions at this time vary depending on the type of P-type impurity, but for example, the acceleration energy is 200 to 3000 keV.

[0100] Next, as shown in FIG. 5C, SiO 2 A mask 75 made of is formed. Subsequently, the mask 75 is etched via a photoresist (not shown) to be patterned into a pattern having openings 76 in regions where the body contact regions 56 are to be formed. After the openings 76 are formed, P-type impurities are implanted from the surface 52 of the epitaxial layer 51 into the interior of the epitaxial layer 51. The implantation conditions at this time vary depending on the type of P-type impurity, but are, for example, an acceleration energy of 30 to 400 keV. After the implantation of the P-type impurity, the mask 75 is removed.

[0101] 5D, N-type impurities are implanted from the surface 52 of the epitaxial layer 51 into the epitaxial layer 51. The implantation conditions at this time vary depending on the type of N-type impurity, but for example, the acceleration energy is 30 to 400 keV.

[0102] Next, as shown in FIG. 5E, SiO 2 is formed on the entire surface 52 of the epitaxial layer 51 by a CVD method, a thermal oxidation method, or the like. 2A mask 77 made of, for example, SF6 (sulfur hexafluoride) and O is formed. The mask 77 may also be formed of SiN by utilizing a CVD method. The mask 77 is then etched via a photoresist (not shown) to be patterned into a pattern having openings 78 in the regions where the gate trench 43 and the source trench 45 are to be formed. After the openings 78 are formed, a mask made of, for example, SF6 (sulfur hexafluoride) and O 2 (Oxygen) containing mixed gas (SF6 / O 2 gas), SF6, O 2 and HBr (hydrogen bromide)-containing mixed gas (SF6 / O 2 / HBr gas) is incident on the surface 52 of the epitaxial layer 51 through the opening 78. As a result, the epitaxial layer 51 is dry-etched from the surface 52 (Si surface) to simultaneously form the gate trench 43 and the source trench 45. At the same time, a large number of unit cells 44 are formed in the epitaxial layer 51.

[0103] Then, as shown in FIG. 2 The inner surface of the gate trench 43 and the inner surface of the source trench 45 are oxidized by a thermal oxidation method (dry oxidation) using a gas. This forms a stopper film 79. Note that although the thickness of this stopper film 79 may not be uniform overall, for the sake of convenience, FIGS. 5F to 5I show a case in which the stopper film 79 has a uniform thickness.

[0104] Next, as shown in FIG. 5G, a material of a mask 77 (SiO 2 ) is deposited on epitaxial layer 51 until the entire surfaces of stopper film 79 and mask 77 are completely covered. As a result, protective mask 80 is formed on stopper film 79 and mask 77. The thickness of protective mask 80 is controlled to be, for example, 0.1 to 0.5 μm.

[0105] 5H, the protective mask 80 is etched back from above the epitaxial layer 51. The etch back is performed while the portion of the protective mask 80 on the bottom surface 60 of the source trench 45 is masked, and is continued until the etching is stopped by the stopper film 79 and the mask 77. As a result, only the portion of the protective mask 80 on the bottom surface 58 of the gate trench 43 is removed, and the portions of the protective mask 80 covering the side surface 57 of the gate trench 43 and the bottom surface 60 and side surface 59 of the source trench 45 remain.

[0106] 5I, P-type impurities are implanted into the epitaxial layer 51 from the bottom surface 58 of the gate trench 43 through the stopper film 79. The implantation conditions at this time vary depending on the type of P-type impurity, but for example, the acceleration energy is 30 to 400 keV.

[0107] Next, as shown in FIG. 5J, the protective mask 80 is removed by wet etching, and then the mask 77 and the stopper film 79 are removed.

[0108] 5K, an organic material film 81 is formed on the entire surface 52 of the epitaxial layer 51. The organic material film 81 is a material containing carbon, and for example, an organic material used as a photoresist (such as polyimide) can be used. Such an organic material film 81 is formed by using, for example, a spin coater.

[0109] After the organic material film 81 is formed, the SiC substrate 42 is loaded into a resistance heating furnace 82. There are no particular limitations on the resistance heating furnace 82 as long as it is an apparatus that can ensure airtightness inside the resistance heating furnace 82 in which the object to be heated is set and can introduce various gases into the resistance heating furnace 82, and the heating method thereof may be either a direct heating method or an indirect heating method.

[0110] Then, in a state where the SiC substrate 42 is set in the resistance heating furnace 82, an inert gas (for example, N2 , Ar, etc.) is introduced, and the resistance heating furnace 82 is subjected to temperature increase control (first temperature increase control).

[0111] In this first temperature rise control, as shown in Fig. 6, the heating temperature is controlled so as to rise from 100°C to 1000°C over, for example, 35 to 45 minutes, and after the rise, the heating temperature is held at 1000°C (first temperature hold) for, for example, 5 to 10 minutes. This temperature rise and temperature hold causes elements other than carbon in organic material film 81 to evaporate, and organic material film 81 is transformed into carbon film 83 as shown in Fig. 5L. Therefore, surface 52 of epitaxial layer 51 is entirely covered with carbon film 83.

[0112] Next, while the inside of the resistance heating furnace 82 is maintained in an inert atmosphere, the resistance heating furnace 82 is further subjected to temperature increase control (second temperature increase control).

[0113] In this second temperature rise control, as shown in Fig. 6, the heating temperature is controlled so as to rise from 1000°C to 1600°C over, for example, 30 to 60 minutes. After the rise, the heating temperature is held at 1600°C (second temperature hold) for, for example, 5 to 10 minutes. This temperature rise and temperature hold activates the individual N-type impurity and P-type impurity ions implanted into the surface layer portion of the epitaxial layer 51, and as shown in Fig. 5M, a body region 53, a source region 55, and a body contact region 56 are formed according to the implanted positions. Also, a drain region 54 that maintains the state after epitaxial growth is formed in the base layer portion of the epitaxial layer 51.

[0114] Next, while the inside of the resistance heating furnace 82 is maintained in an inert atmosphere, the temperature of the resistance heating furnace 82 is controlled to be lowered.

[0115] In the temperature drop control, as shown in FIG. 6, the heating temperature is limited (temperature drop limit) so as to drop from 1600°C to 1300°C over, for example, 15 to 30 minutes. After the temperature drop, while the heating temperature is held at 1300°C (third temperature hold), a nitrogen- and oxygen-containing gas is introduced into the resistance heating furnace 82 for, for example, 5 to 10 minutes. By introducing the nitrogen- and oxygen-containing gas, the carbon film 83 reacts with the oxygen in the gas and is oxidized and removed, as shown in FIG. 5N. The nitrogen- and oxygen-containing gas introduced contains at least N 2 A gas containing O (dinitrogen monoxide) can be used, and may also contain NO (nitric oxide). 2 The O gas is supplied at a flow rate ratio of 30% or less, preferably 1 to 30%, of the total flow rate of the introduced gases.

[0116] Thereafter, the heating temperature is held at 1300° C. for, for example, 200 to 240 minutes (fourth temperature holding) while introducing the nitrogen- and oxygen-containing gas into the resistance heating furnace 82 at the same flow rate. As a result, the surface 52 of the epitaxial layer 51 is oxidized to form a silicon nitride oxide film (gate insulating film 63) covering the entire surface 52, as shown in FIG. 5O.

[0117] After the gate insulating film 63 is formed, an inert gas (for example, N2, Ar, etc.) is introduced again into the resistance heating furnace 82, and the heating temperature is controlled to drop from 1300° C. to 300° C. After the temperature drop, the SiC substrate 42 is removed from the resistance heating furnace 82.

[0118] 5P, a doped polysilicon material 84 is deposited by a CVD method from above the epitaxial layer 51. The deposition of the polysilicon material 84 is continued until at least the gate trench 43 and the source trench 45 are filled up.

[0119] Thereafter, as shown in FIG. 5Q, the deposited polysilicon material 84 is etched back until the etched back surface is flush with surface 52 of epitaxial layer 51.

[0120] 5R, only the polysilicon material 84 remaining in the source trench 45 is removed by dry etching. As a result, the gate electrode 66 made of the polysilicon material 84 remaining in the gate trench 43 is formed.

[0121] Next, as shown in FIG. 5S, SiO 2 An interlayer insulating film 67 made of is laminated.

[0122] Then, as shown in FIG. 5T, the interlayer insulating film 67 and the gate insulating film 63 are patterned in succession to form contact holes 68 in the interlayer insulating film 67 and the gate insulating film 63.

[0123] Next, as shown in FIG. 5U, a polysilicon material is deposited by a CVD method until the contact holes 68 are completely filled. After that, an N-type or P-type impurity is implanted into the deposited polysilicon material. The implantation conditions at this time vary depending on the type of impurity, but for example, the acceleration energy is 10 to 100 keV. Then, for example, impurity diffusion is performed at 900° C. for 20 minutes. As a result, a polysilicon layer 70 doped with impurities at a high concentration is formed. Then, Ti and TiN are deposited in this order on the surface of the polysilicon layer 70 by a method such as a sputtering method or a vapor deposition method, to form an intermediate layer 71. Then, a metal such as Al is deposited on the surface of the intermediate layer 71 by a method such as a sputtering method or a vapor deposition method, to form a metal layer 72. As a result, a source wiring 69 is formed. Then, a drain electrode 74 is formed on the rear surface 50 of the SiC substrate 42.

[0124] Thereafter, an interlayer insulating film (not shown), a source pad 46, a gate pad 48, etc. are formed, thereby obtaining the semiconductor device 41 shown in FIG.

[0125] As described above, according to the semiconductor device 41, similarly to the semiconductor device 1 of the first embodiment, the gate trench 43 is formed by digging down from the surface 52 (Si surface) of the epitaxial layer 51 made of SiC. Therefore, the oxidation of the inner surface of the gate trench 43 (see FIG. 5O) proceeds under the condition that the oxidation rate of the bottom surface 58 having the Si surface and the oxidation rate of the side surface which is a surface perpendicular to the Si surface satisfy the relation: oxidation rate of bottom surface 58 / oxidation rate of side surface 57<0.

[0126] In the above manufacturing method, the oxidation of the inner surface of the gate trench 43 is carried out by using O 2 Thermal oxidation using gas (dry oxidation) and H 2 The thermal oxidation is performed by using a nitrogen- and oxygen-containing gas, not by using O (water vapor) gas (wet oxidation). Furthermore, an implanted active layer 62 in which P-type impurities are implanted is formed directly below the bottom surface 58 of the gate trench 43. Therefore, the ratio of the oxidation rate of the bottom surface 58 to the oxidation rate of the side surface 57 (oxidation rate of the bottom surface 58 / oxidation rate of the side surface 57) can be made larger than when the gate insulating film 63 is formed by dry oxidation or wet oxidation.

[0127] The gate insulating film 63 thus formed has a thickness T 3 Thickness T of the bottom insulating film 64 4 Ratio of thickness T 4 / Thickness T 3 ) is in the range of 0.3 to 1.0.

[0128] In other words, the thickness T of the insulating film bottom 64 is set to a value sufficient to suppress dielectric breakdown. 4 Even if the thickness T 4 / Thickness T 3 Since the lower limit of the thickness T 3 On the other hand, since the upper limit is 1.0, the thickness T 4 When the thickness T of the insulating film side portion 65 is appropriately designed, 3 As a result, the thickness T4 By appropriately designing the thickness T 3 It is possible to suppress an increase in the dielectric breakdown of the insulating film bottom portion 64 while suppressing the dielectric breakdown.

[0129] Furthermore, since the gate insulating film 63 is made of a silicon oxynitride film formed by thermal oxidation using a nitrogen-containing gas, the channel mobility of the VDMOSFET can be improved.

[0130] In addition, since the implantation active layer 62 is formed directly below the gate trench 43, the energy barrier formed between the implantation active layer 62 and the epitaxial layer 51 can be made large. This makes it difficult for a current to flow through the implantation active layer 62. As a result, the electric field concentration on the bottom surface 58 of the gate trench 43 can be suppressed.

[0131] Furthermore, since the source trench 45 is formed in the center of each unit cell 44 surrounded by the gate trench 43, it is possible to suppress the concentration of equipotential lines near both end corners 61 of the gate trench 43. As a result, the electric field applied to both end corners 61 at the bottom of the gate trench 43 can be alleviated, so that the dielectric breakdown of the insulating film bottom 64 can be suppressed.

[0132] 7, the source trench 45 may be deeper than the gate trench 43. This makes it possible to further reduce the electric field applied to both end corners 61 at the bottom of the gate trench 43.

[0133] Furthermore, in the semiconductor device 41, the source wiring 69 has a polysilicon layer 70 at the contact portion with the source region 55 and the body contact region 56, so that the source wiring 69 can be made into an ohmic junction with both the body contact region 56 and the source region 55, which are high-concentration impurity regions.

[0134] Therefore, in manufacturing semiconductor device 41, unlike the case where a layer made only of a metal such as Al is in direct contact with an impurity region, the step of forming a Ni layer on surface 52 of epitaxial layer 51 can be omitted, and further the step of silicidating such a Ni layer can be omitted. Thus, the generation of a carbon layer on surface 52 of epitaxial layer 51 can be prevented.

[0135] As a result, it is possible to suppress layer peeling between the source wiring 69 and the epitaxial layer 51. This makes it possible to improve the connection reliability of the source wiring 69.

[0136] In addition, since the layer (polysilicon layer 70) that enters the source trench 45 and contacts the drain region 54, the body contact region 56, and the source region 55 is made of polysilicon with excellent coverage, it is possible to improve the coverage of the source wiring 69. As a result, it is possible to further improve the connection reliability of the source wiring 69.

[0137] In addition, an intermediate layer 71 having a laminated structure of a Ti layer and a TiN layer is interposed between the polysilicon layer 70 and the metal layer 72. Materials containing Ti have excellent adhesion to both polysilicon materials and metal materials. Therefore, it is possible to improve the adhesion between the polysilicon layer 70 and the metal layer 72. As a result, it is possible to further improve the connection reliability of the source wiring 69.

[0138] Furthermore, when the metal layer 72 contains Al, the TiN layer can be used as a barrier layer for preventing the diffusion of Al from the metal layer 72 to the polysilicon layer 70, thereby preventing excess Al from diffusing into the polysilicon layer 70. As a result, the impurity concentration of the polysilicon layer 70 can be stabilized, and therefore the resistance value of the polysilicon layer 70 can be stabilized.

[0139] Next, an embodiment of the invention of a method for manufacturing a SiC semiconductor device using a resistance heating furnace will be described.

[0140] FIG. 8 is a schematic cross-sectional view of a planar gate type semiconductor device.

[0141] The semiconductor device 101 has a structure in which unit cells of a planar gate type VDMOSFET are arranged in a matrix shape. Note that Fig. 8 shows only a part of the plurality of unit cells.

[0142] The semiconductor device 101 is made of a N + The SiC substrate 102 is provided with an N-type SiC substrate 102. The surface 121 of the SiC substrate 102 is provided with an N-type impurity layer 124 made of SiC (silicon carbide) doped with a lower concentration of N-type impurities than the SiC substrate 102. - A mold epitaxial layer 103 is laminated on the substrate 102. A surface 131 of the epitaxial layer 103 is formed of, for example, a (0001) plane of SiC.

[0143] The epitaxial layer 103 was formed of N - A drain region 104 of the type is formed.

[0144] Furthermore, a P-type body region 105 is formed in a surface layer portion of the epitaxial layer 103. Although not shown in Fig. 8, a plurality of body regions 105 are formed at regular intervals, and extend parallel to each other in the same direction (perpendicular to the paper surface of Fig. 8), and are arranged, for example, in a stripe shape or a matrix shape. Furthermore, the drain region 104 is exposed between the adjacent body regions 105.

[0145] The surface layer of the body region 105 is provided with N + A source region 106 of the type is formed.

[0146] A gate insulating film 107 is formed on the surface 131 of the epitaxial layer 103, and extends across the drain region 104, the body region 105, and the source region 106. The gate insulating film 107 is made of SiO 2 It consists of:

[0147] A gate electrode 108 made of polysilicon doped with a high concentration of N-type impurities is formed on the gate insulating film 107. The gate electrode 108 faces the drain region 104, the body region 105, and the source region 106 via the gate insulating film 107.

[0148] On the epitaxial layer 103, SiO 2 An interlayer insulating film 109 made of is laminated on the body region 105. A source wiring 111 is formed on the interlayer insulating film 109. The source wiring 111 is electrically connected to the body region 105 and the source region 106 via a contact hole 110 formed in the interlayer insulating film 109.

[0149] A gate wiring 112 is electrically connected to the gate electrode 108 via a contact hole (not shown) formed in the interlayer insulating film 109 .

[0150] A drain electrode 113 is formed on the back surface of the SiC substrate .

[0151] When the source wiring 111 is grounded and an appropriate positive voltage is applied to the drain electrode 113 while controlling the potential of the gate electrode 108, a channel can be formed in the body region 105 near the interface with the gate insulating film 107 due to the electric field from the gate electrode 108. This allows a current to flow between the source wiring 111 and the drain electrode 113.

[0152] 9A to 9L are schematic cross-sectional views illustrating a method for manufacturing the semiconductor device of FIG.

[0153] First, as shown in Fig. 9A, epitaxial layer 103 is formed on surface 121 of SiC substrate 102 by epitaxial growth. At this time, the main growth surface (surface 121) of SiC substrate 102 is the (0001) plane. Since surface 121 of SiC substrate 102 is the (0001) plane, epitaxial layer 103 formed by epitaxial growth on SiC substrate 102 is also formed with the (0001) plane as its main surface. Therefore, surface 131 of epitaxial layer 103 parallel to surface 121 of SiC substrate 102 is the (0001) plane.

[0154] Next, photoresist 114 having openings 115 in portions facing regions where body regions 105 are to be formed is formed on surface 131 of epitaxial layer 103 by known photolithography technology. Then, P-type impurity ions (e.g., boron ions) are incident on surface 131 of epitaxial layer 103 from above photoresist 114. As a result, the P-type impurity is implanted into the surface layer portion of epitaxial layer 103 exposed from opening 115, as shown in FIG. 9B.

[0155] Next, photoresist 116 having openings 117 in portions facing the regions where source regions 106 are to be formed is formed on surface 131 of epitaxial layer 103 by known photolithography techniques. Then, ions of N-type impurities (e.g., arsenic ions) are incident on surface 131 of epitaxial layer 103 from above photoresist 116. As a result, as shown in Fig. 9C, the N-type impurities are implanted into the surface layer portions (the surface 131 side of the implanted portions of the P-type impurities) of the portions exposed from openings 117 of epitaxial layer 103.

[0156] After the impurity ions are implanted into the surface layer of the epitaxial layer 103, an organic material film 118 is formed on the entire surface 131 of the epitaxial layer 103, as shown in Fig. 9D. The organic material film 118 is a material containing carbon, and for example, an organic material used as a photoresist (such as polyimide) can be used. Such an organic material film 118 is formed, for example, by using a spin coater.

[0157] After the organic material film 118 is formed, the SiC substrate 102 is loaded into a resistance heating furnace 122. The resistance heating furnace 122 is not particularly limited as long as it can ensure airtightness inside the resistance heating furnace 122 in which the object to be heated is set and can introduce various gases into the resistance heating furnace 122, and the heating method thereof may be either a direct heating method or an indirect heating method.

[0158] Then, in a state where the SiC substrate 102 is set in the resistance heating furnace 122, an inert gas (for example, N 2 , Ar, etc.) is introduced, and the resistance heating furnace 122 is subjected to temperature increase control (first temperature increase control).

[0159] In this first temperature rise control, as shown in Fig. 6, the heating temperature is controlled so as to rise from 100°C to 1000°C over, for example, 35 to 45 minutes, and after the rise, the heating temperature is held at 1000°C (first temperature hold) for, for example, 5 to 10 minutes. This temperature rise and temperature hold causes elements other than carbon in the organic material film 118 to evaporate, and the organic material film 118 is transformed into a carbon film 119 as shown in Fig. 9E. Therefore, the entire surface 131 of the epitaxial layer 103 is covered with the carbon film 119.

[0160] Next, while the inside of the resistance heating furnace 122 is maintained in an inert atmosphere, the resistance heating furnace 122 is further subjected to temperature increase control (second temperature increase control).

[0161] In this second temperature rise control, as shown in Fig. 6, the heating temperature is controlled so as to rise from 1000°C to 1600°C over, for example, 30 to 60 minutes. After the rise, the heating temperature is held at 1600°C (second temperature hold) for, for example, 5 to 10 minutes. This temperature rise and temperature hold activates the ions of the N-type impurities and P-type impurities implanted in the surface layer portion of the epitaxial layer 103, and as shown in Fig. 9F, a body region 105 and a source region 106 are formed in the surface layer portion of the epitaxial layer 103. In addition, a drain region 104 is formed in the base layer portion of the epitaxial layer 103, which is separated from the body region 105 and maintains the state after epitaxial growth.

[0162] Next, while the inside of the resistance heating furnace 122 is maintained in an inert atmosphere, the temperature of the resistance heating furnace 122 is controlled to decrease.

[0163] In the temperature drop control, as shown in FIG. 6, the heating temperature is limited (temperature drop limit) so as to drop from 1600°C to 1300°C over, for example, 15 to 30 minutes. After the temperature drop, while the heating temperature is held at 1300°C (third temperature hold), an oxygen-containing gas is introduced into the resistance heating furnace 122 for, for example, 5 to 10 minutes. By introducing the oxygen-containing gas, the carbon film 119 reacts with the oxygen in the oxygen-containing gas and is oxidized and removed, as shown in FIG. 9G. However, it is preferable to use a gas containing oxygen and nitrogen as the oxygen-containing gas introduced into the resistance heating furnace 122, and specifically, NO (nitric oxide), N 2 Gases containing O (nitrous oxide) and the like can be used.

[0164] Thereafter, the heating temperature is held at 1300° C. for, for example, 200 to 240 minutes (fourth temperature holding) while an oxygen-containing gas is being introduced into resistance heating furnace 122. As a result, surface 131 of epitaxial layer 103 is oxidized, and oxide film 120 is formed to cover the entire surface 131, as shown in FIG.

[0165] After the oxide film 120 is formed, an inert gas (e.g., N 2Gas (such as Ar) is introduced again, and the heating temperature is controlled so as to drop from 1300° C. to 300° C. After the temperature drop, the SiC substrate 102 is removed from the resistance heating furnace 122.

[0166] Next, a conductive material is deposited by sputtering, and then the conductive material is patterned by known photolithography and etching techniques to form the gate electrode 108 on the oxide film 120, as shown in FIG.

[0167] Thereafter, an interlayer insulating film 109 is laminated on the epitaxial layer 103 by a CVD (Chemical Vapor Deposition) method, as shown in FIG. 9J.

[0168] 9K, a contact hole 110 is formed in the interlayer insulating film 109 and the oxide film 120 by known photolithography and etching techniques. The remaining portion of the oxide film 120 becomes the gate insulating film 107.

[0169] Next, a conductive material is deposited on the epitaxial layer 103 by sputtering. The conductive material is deposited so as to fill the contact holes 110 and form a thin film on the interlayer insulating film 109. Then, the conductive material on the interlayer insulating film 109 is patterned by known photolithography and etching techniques. As a result, a source wiring 111 is formed, as shown in FIG. 9L. Furthermore, a gate wiring 112 electrically connected to the gate electrode 108 is formed. Furthermore, a drain electrode 113 is formed on the back surface of the SiC substrate 102.

[0170] Through the above steps, the semiconductor device 101 shown in FIG. 8 is obtained.

[0171] According to the above manufacturing method, after the organic material film 118 is formed, the organic material film 118 in the resistance heating furnace 122 is heated by the first temperature rise control of the resistance heating furnace 122 and transformed into a carbon film 119, and the carbon film 119 is formed on the surface 131 of the epitaxial layer 103.

[0172] After the carbon film 119 is formed, while maintaining an inert atmosphere inside the resistance heating furnace 122, the epitaxial layer 103 is heated by a second temperature rise control of the resistance heating furnace 122, and the ions of the N-type impurities and P-type impurities in the epitaxial layer 103 are activated.

[0173] Then, while maintaining the inside of the resistance heating furnace 122 in an inactive state, a temperature drop control (for example, from 1600°C to 1300°C) is performed. Thereafter, while the heating temperature is maintained at 1300°C (third temperature maintenance), an oxygen-containing gas is introduced for, for example, 5 to 10 minutes. As a result, the carbon film 119 is oxidized and removed, and the surface 131 of the epitaxial layer 103 is exposed.

[0174] After removing carbon film 119, resistance heating furnace 122 is maintained at temperature (fourth temperature maintenance) while continuing to introduce oxygen-containing gas into resistance heating furnace 122, whereby exposed surface 131 is oxidized to form oxide film 120.

[0175] Prior to heating for ion activation (second temperature rise control), carbon film 119 is formed on surface 131 of epitaxial layer 103, so that it is possible to prevent Si from escaping from surface 131 when epitaxial layer 103 is heated. Therefore, it is possible to suppress roughness of surface 131 of epitaxial layer 103, and it is possible to maintain the flatness of surface 131. As a result, it is possible to smooth the interface between epitaxial layer 103 and gate insulating film 107, so that it is possible to improve the channel mobility of semiconductor device 101.

[0176] Furthermore, four steps consisting of a step of heating the organic material film 118 to change it into the carbon film 119 (first temperature rise control), a step of heating the epitaxial layer 103 to activate ions (second temperature rise control), a step of oxidizing and removing the carbon film 119 with an oxygen-containing gas (temperature drop limit control and third temperature maintenance), and a step of oxidizing the surface of the SiC layer to form an oxide film (fourth temperature maintenance) can be performed continuously in one resistance heating furnace 122. Since no separate device for removing the carbon film is required, an increase in the cost of the device can be suppressed. Moreover, since the resistance heating furnace 122 is used, the first temperature rise control, the second temperature rise control, the temperature drop limit control, the third temperature maintenance, and the fourth temperature maintenance can be performed precisely and simply.

[0177] Moreover, surface 131 of epitaxial layer 103 on which oxide film 120 is formed is a (0001) plane, and the oxygen-containing gas introduced into the heating furnace is a gas containing oxygen and nitrogen.

[0178] For example, O 2 Gas, H 2 O gas (water vapor) and N 2 When the (0001) surface of the SiC layer is oxidized with O gas to form an oxide film, the channel mobility of a MOSFET having the SiC layer is, for example, 1 to 5 cm 2 / V·s, 5~15cm 2 / V s and 15~25cm 2 / V s, N 2 The channel mobility is the best in the case of O gas.

[0179] In the semiconductor device 101 of this embodiment, the (0001) surface (surface 131) of the epitaxial layer 103 is heated with NO gas or N 2 Since the oxide film 120 is formed by oxidation with O gas, the channel mobility of the semiconductor device 101 can be further improved.

[0180] Although the embodiment of the present invention has been described above, the present invention can be embodied in other forms.

[0181] For example, it is possible to adopt a configuration in which the conductivity type of each semiconductor portion of the semiconductor device 1 is inverted. That is, in the semiconductor devices 1, 41, and 85, the P-type portions may be N-type, and the N-type portions may be P-type.

[0182] Furthermore, the source wirings 17, 69 and the drain wiring 23 (drain electrode 74) may have a laminated structure of a layer in which nickel (Ni) or titanium (Ti) is silicided and the above-mentioned metal layer.

[0183] In addition, various design modifications can be made within the scope of the claims.

[0184] In addition to the invention described in the claims, the following features can be extracted from the contents of the above-described embodiment.

[0185] For example, in FIG. 11, since a surface 217 of the epitaxial layer 203 is a Si surface, a bottom surface 216 of the gate trench 206 dug down from the surface 217 is also a Si surface.

[0186] Therefore, when the gate insulating film 207 is formed by dry oxidation or wet oxidation, the ratio of the oxidation rate of the bottom surface 216 to the oxidation rate of the side surface 214 (oxidation rate of the bottom surface 216 / oxidation rate of the side surface 214) is 0.2 or less. Therefore, in the gate insulating film 207, the thickness of the portion on the bottom surface 216 is smaller than the thickness of the portion on the side surface 214.

[0187] On the other hand, in semiconductor device 201, when the VDMOSFET is turned off, a high potential difference occurs between gate electrode 208 and drain wiring 215 (gate-drain), and an electric field is concentrated on bottom surface 216 of gate trench 206. In gate insulating film 207 having a small thickness above bottom surface 216 as described above, dielectric breakdown due to the concentration of the electric field is likely to occur.

[0188] To address this problem, a countermeasure has been considered in which the oxidation time during the formation of gate insulating film 207 is lengthened to increase the thickness of the portion above bottom surface 216. However, since the oxidation of side surface 214 progresses in parallel with the oxidation of bottom surface 216, the difference in oxidation rate causes the thickness of the portion above side surface 214 to become very large.

[0189] The purpose of the features described below is to provide a semiconductor device and a manufacturing method thereof that can suppress an increase in the thickness of the gate insulating film on the side surface of the gate trench while suppressing dielectric breakdown in the portion on the bottom surface of the gate trench. (Item 1) A semiconductor device comprising: a first conductive type semiconductor layer made of SiC and having a Si surface; a gate trench dug down from the surface of the semiconductor layer; a gate insulating film formed on a bottom surface and a side surface of the gate trench, the ratio of the thickness of the portion on the bottom surface to the thickness of the portion on the side surface being 0.3 to 1.0; and a gate electrode embedded in the gate trench via the gate insulating film.

[0190] According to this configuration, a gate trench is formed by digging down from a surface of a first conductivity type semiconductor layer made of SiC and having a Si surface. A gate insulating film is formed on the bottom and side surfaces of the gate trench. In addition, a gate electrode is embedded in the gate trench via the gate insulating film.

[0191] As a result, in this semiconductor device, a trench-gate MOSFET is formed having a MOS (Metal Oxide Semiconductor) structure in which a gate electrode (Metal) faces a semiconductor layer (Semiconductor) via a portion (Oxide) on the side surface of the gate trench in the gate insulating film.

[0192] In the MOSFET, the ratio of the thickness of the portion on the bottom surface to the thickness of the portion on the side surface in the gate insulating film is 0.3 to 1.0. Even if the thickness of the portion on the bottom surface is increased to a degree that can suppress dielectric breakdown, the lower limit of (thickness of the portion on the bottom surface / thickness of the portion on the side surface) is 0.3, so that excessive increase in the thickness of the portion on the side surface can be suppressed. On the other hand, since the upper limit is 1.0, when the thickness of the portion on the bottom surface is designed to be an appropriate size, the thickness of the portion on the side surface does not become excessively small. As a result, by appropriately designing the thickness of the portion on the bottom surface, it is possible to suppress dielectric breakdown in the portion on the bottom surface while suppressing an increase in the thickness of the portion on the side surface. (Item 2) The semiconductor device according to item 1, wherein the semiconductor layer includes a body region of a second conductivity type formed on a side of the gate trench and in contact with the gate insulating film on the side of the gate trench, and a source region of a first conductivity type formed adjacent to the gate trench in a surface portion of the body region, and the gate insulating film contains nitrogen.

[0193] In this configuration, a body region of a second conductivity type is formed on the side of the gate trench in the semiconductor layer, the body region being in contact with the gate insulating film on the side of the gate trench. A source region of a first conductivity type is formed adjacent to the gate trench in a surface layer of the body region. Therefore, in a trench-gate MOSFET in the semiconductor device, a portion of the body region near the interface with the gate insulating film is a channel portion where a channel is formed by an electric field from the gate electrode. In this semiconductor device, the gate insulating film contains nitrogen, so that the channel mobility of the MOSFET can be improved. (Item 3) The concentration of the second conductive type impurity in the body region is 1e19 cm -3 Item 3. The semiconductor device according to item 2, wherein:

[0194] The impurity concentration of the body region on the side of the gate trench is 1e19cm -3If the oxidation rate exceeds 100%, when the bottom and side surfaces of the gate trench are oxidized, the side surfaces of the trench are oxidized at a relatively high oxidation rate compared to the bottom surface of the trench, and the portions of the gate insulating film on the side surfaces become very thick.

[0195] In contrast, the impurity concentration in the body region is 1e19cm -3 If the ratio is less than the above, when the bottom and side surfaces of the gate trench are oxidized, the ratio of the oxidation rate of the trench side surface to the oxidation rate of the trench bottom surface can be maintained at an appropriate value, thereby suppressing an increase in the thickness of the gate insulating film on the side surfaces. (Item 4) The semiconductor device according to any one of items 1 to 3, further comprising an implantation layer formed by implanting impurities in a portion of the semiconductor layer from the bottom surface of the gate trench to a middle portion of the semiconductor layer in a thickness direction.

[0196] By forming an implantation layer directly below the bottom surface of the gate trench, when oxidizing the bottom and side surfaces of the gate trench after the implantation layer is formed, the bottom surface of the trench can be oxidized at a relatively high oxidation rate compared to the trench side surfaces, making it possible to set the ratio of the thickness of the portion of the gate insulating film on the bottom surface to the thickness of the portion on the side surfaces to 0.3 to 1.0. (Item 5) The semiconductor device according to item 3, wherein the implantation layer is formed by implantation of the second conductive type impurity.

[0197] If the implantation layer is formed by implanting a second conductivity type impurity different from the conductivity type of the semiconductor layer, the energy barrier formed between the implantation layer and the semiconductor layer can be made larger. This makes it difficult for current to flow through the implantation layer. As a result, the electric field concentration at the bottom of the gate trench can be suppressed. (Item 6) The semiconductor device according to any one of items 1 to 5, wherein the gate insulating film has a thickness of 2000 Å or less at a portion on the side surface of the gate trench.

[0198] If the thickness of the portion on the side surface of the gate trench exceeds 2000 Å, it becomes necessary to operate the semiconductor device at a high gate-on voltage (for example, about 20 V), and efficient transistor operation may not be possible.

[0199] In contrast, if the thickness of the portion on the side surface of the gate trench is 2000 Å or less, the semiconductor device can be operated with an appropriate gate-on voltage, and efficient transistor operation can be achieved. (Item 7) The semiconductor device according to any one of items 1 to 6, wherein an end portion of the bottom of the gate trench in a direction perpendicular to the gate width is curved outward.

[0200] In this configuration, by curving the end of the bottom of the gate trench where the electric field is likely to concentrate during turn-off, the electric field applied to the end can be dispersed to parts other than the end, thereby suppressing dielectric breakdown of the part above the bottom surface of the gate insulating film. (Item 8) The semiconductor device according to item 2, further comprising a source wiring formed on the semiconductor layer and in contact with the source region, the source wiring having a polysilicon layer at a contact portion with the source region and a metal layer on the polysilicon layer.

[0201] For example, in the semiconductor device 201 shown in FIG. 11, to form the source wiring 212, first, Ni is deposited by sputtering on the surface (surface of the source region 209 and the body contact region 210) of the region doped with impurities (impurity region) in the epitaxial layer 203. Next, in order to form an ohmic junction between Ni and the impurity region, a high-temperature (for example, about 1000° C.) heat treatment is performed to react Si and Ni in SiC to convert Ni into a silicide. This forms a nickel silicide layer 218. Thereafter, Al is deposited on the nickel silicide layer 218 by sputtering. This forms an aluminum layer 219, and the source wiring 212 is formed.

[0202] However, during the formation of the nickel silicide layer 218, residual carbon (C) in SiC precipitates on the surface of the nickel silicide layer 218 and in the vicinity of the interface with the impurity region in the nickel silicide layer 218, forming a carbon layer containing a large amount of C. Since the carbon layer has poor adhesion to metal and SiC, peeling is likely to occur between the aluminum layer 219 and the nickel silicide layer 218 and between the nickel silicide layer 218 and the impurity region.

[0203] Therefore, in the configuration of item 8, the source wiring that contacts the source region has a polysilicon layer at the contact portion with the source region, and has a metal layer on the polysilicon layer.

[0204] Polysilicon can form a good ohmic junction with a region in SiC doped with impurities (impurity region). Therefore, silicidation, which is essential for a structure in which a metal layer is in direct contact with a source region, can be omitted. This makes it possible to prevent the generation of a carbon layer on the surface of the polysilicon layer and in the vicinity of the interface between the polysilicon layer and the source region. As a result, it is possible to suppress layer peeling between the polysilicon layer and the metal layer and between the polysilicon layer and the source region. This makes it possible to improve the connection reliability of the source wiring. (Item 9) The semiconductor device according to item 8, wherein an intermediate layer containing Ti is interposed between the polysilicon layer and the metal layer.

[0205] Materials containing titanium have excellent adhesion to both polysilicon materials and metal materials. Therefore, in a semiconductor device having a structure in which a layer containing titanium is interposed between a polysilicon layer and a metal layer, the adhesion between the polysilicon layer and the metal layer can be improved. As a result, the connection reliability of the source wiring can be further improved. (Item 10) The semiconductor device according to item 9, wherein the metal layer has a layer containing Al, and the intermediate layer has a structure in which a Ti layer and a TiN layer are stacked in this order from the polysilicon layer side.

[0206] Al can be used as an impurity to impart conductivity to the polysilicon layer. However, if an appropriate amount of Al is not mixed into the polysilicon layer, the resistance value of the polysilicon layer used as the source wiring may become unstable.

[0207] Therefore, in the configuration of item 10, a TiN layer is interposed between the layer containing Al and the polysilicon layer as a barrier layer to prevent the diffusion of Al into the polysilicon layer. This prevents excess Al from diffusing into the polysilicon layer, stabilizing the impurity concentration of the polysilicon layer. As a result, the resistance value of the polysilicon layer can be stabilized. (Item 11) A method for manufacturing a semiconductor device, comprising: forming a gate trench that is dug down from a surface of a first conductive type semiconductor layer made of SiC and having a Si surface; forming a gate insulating film on the bottom and side of the gate trench by oxidizing the bottom and side of the gate trench at a heat treatment temperature of 1200 ° C. or more in a gas containing nitrogen and oxygen; and forming a gate electrode on the gate insulating film so as to fill the gate trench.

[0208] By oxidizing the bottom and side surfaces of the gate trench under the conditions (atmospheric gas and heat treatment temperature) of this method, the ratio of the thickness of the portion on the bottom surface of the gate insulating film to the thickness of the portion on the side surfaces can be set to 0.3 to 1.0.

[0209] In the step of forming the gate insulating film, (item 12) includes at least N 2 It is preferable that the bottom surface and the side surface of the gate trench are oxidized in a gas containing O, and further, N 2 As for O gas, (item 13), it is preferable to supply the O gas at a flow rate ratio of 30% or less with respect to the total flow rate of the gases to be supplied.

[0210] The step of forming the gate insulating film may include the steps of loading the semiconductor layer into a resistance heating furnace, introducing a gas containing nitrogen and oxygen into the resistance heating furnace to create a nitrogen- and oxygen-containing gas atmosphere, and controlling the heating temperature of the resistance heating furnace to 1200°C or higher while maintaining the gas atmosphere.

[0211] For example, the following findings are known as background art relating to heating of a semiconductor layer made of SiC (for example, Japanese Patent Application Laid-Open No. 2003-318388).

[0212] Specifically, a known example of a semiconductor device that employs SiC is a MOSFET having a MOS (Metal Oxide Semiconductor) structure that includes a SiC layer having an activated ion region in a surface portion thereof, a gate oxide film formed on the surface of the SiC layer, and a gate electrode formed on the gate oxide film and facing the ion region via the gate oxide film.

[0213] To fabricate such a MOS structure, for example, first, impurity ions are implanted into the surface layer of the SiC layer. Next, the SiC layer is heated in a resistance heating furnace to activate the implanted ions. After the ion activation, a gate oxide film is formed on the surface of the SiC layer by supplying an oxygen-containing gas in a CVD (Chemical Vapor Deposition) device. Then, a gate electrode is formed on the gate oxide film by a sputtering method. In this way, a layer structure (MOS structure) of gate electrode (metal)-gate oxide film (oxide)-SiC layer (semiconductor) is fabricated.

[0214] To activate the ions in the SiC layer, for example, annealing at a temperature of 1600 to 1700°C is necessary. In a resistance heating furnace, the heating time to reach the high temperature range is long, so during the heating for ion activation, silicon sublimes from the surface of the SiC layer, which is called silicon loss, and the surface of the SiC layer becomes rough. As a result, the interface between the SiC layer and the gate oxide film becomes uneven, and the channel mobility of the MOSFET decreases.

[0215] Therefore, a method has been adopted in which a high-frequency induction heating furnace is used to shorten the heating time to a high temperature range, thereby suppressing surface roughness of the SiC layer, and then a gate oxidation furnace is used to form a gate oxide film.

[0216] However, this method requires two separate devices, a high-frequency induction heating furnace and a gate oxidation furnace, which increases the cost of the devices.

[0217] As another method, it has been proposed to form a carbon film on the surface of the SiC layer prior to ion activation, and to maintain the flatness of the SiC layer surface by using this carbon film to prevent silicon loss.

[0218] The carbon film is formed, for example, by forming a film containing carbon on the surface of a SiC layer and heating the carbon-containing film in a high-frequency induction heating furnace to evaporate elements other than carbon from the film.

[0219] However, after extensive research, the inventors of the present invention found that the heating temperature for forming a carbon film is about 1000° C., which is lower than the temperature for activating ions (1600 to 1700° C.). Therefore, the heating temperature needs to be controlled in two stages, but it is difficult to precisely control the temperature of a high-frequency induction heating furnace.

[0220] Furthermore, after the ions are activated, the carbon film becomes unnecessary. This unnecessary carbon film is oxidized and removed by an oxidizing gas in a device separate from the high-frequency induction heating furnace. It has been considered to introduce an oxidizing gas into the high-frequency induction heating furnace and remove the carbon film following the activation of the ions, but since the heating element of the high-frequency induction heating furnace uses a carbon material, the carbon material will be oxidized when the oxidizing gas is supplied. Therefore, a separate carbon film removal device is necessary, and it has been found that an increase in the cost of the device is unavoidable.

[0221] Therefore, in order to achieve the object of providing a manufacturing method for a semiconductor device that can suppress roughness of the SiC layer surface by simple temperature control without increasing the cost of the equipment, the following invention has been made.

[0222] Specifically, the invention is a method for manufacturing a semiconductor device including the steps of: forming an organic material film on a surface of a SiC layer having ions implanted into a surface layer portion; after forming the organic material film, heating the organic material film in a resistance heating furnace to transform the organic material film into a carbon film; activating ions in the SiC layer by heating the SiC layer on which the carbon film has been formed in the resistance heating furnace in the resistance heating furnace; oxidizing and removing the carbon film by introducing an oxygen-containing gas into the resistance heating furnace; and, after removing the carbon film, continuing in the resistance heating furnace, oxidizing the surface of the SiC layer with the oxygen-containing gas to form an oxide film.

[0223] According to this manufacturing method, after the organic material film is formed, the organic material film is heated in a resistance heating furnace, whereby the organic material film is transformed into a carbon film, and a carbon film is formed on the surface of the SiC layer. After the carbon film is formed, the SiC layer is heated to activate ions in the SiC layer. Then, an oxygen-containing gas is introduced into the resistance heating furnace, whereby the carbon film is oxidized and removed. After the carbon film is removed, the surface of the SiC layer is oxidized by the oxygen-containing gas in the resistance heating furnace to form an oxide film.

[0224] Since a carbon film is formed on the surface of the SiC layer prior to heating for ion activation, it is possible to prevent Si from being removed from the surface of the SiC layer when the SiC layer is heated. Therefore, roughness of the surface of the SiC layer can be suppressed, and the flatness of the surface of the SiC layer can be maintained. As a result, the interface between the SiC layer and the oxide film can be made smooth, and the channel mobility of the semiconductor device can be improved.

[0225] Furthermore, the four steps of heating the organic material film to transform it into a carbon film, heating the SiC layer to activate ions, oxidizing and removing the carbon film with an oxygen-containing gas, and oxidizing the surface of the SiC layer to form an oxide film can be performed continuously in one resistance heating furnace. Since no separate device for removing the carbon film is required, the increase in equipment costs can be suppressed. Moreover, since a resistance heating furnace is used, the heating temperature for forming the carbon film and the heating temperature for activating the ions can be precisely and easily controlled.

[0226] In addition, the oxygen-containing gas may be a gas containing oxygen and nitrogen. If the oxygen-containing gas for forming the oxide film is a gas containing oxygen and nitrogen, the channel mobility of the semiconductor device can be further improved.

[0227] Examples of gases containing oxygen and nitrogen include NO (nitric oxide), N 2 Gases containing O (nitrous oxide) and the like can be used.

[0228] Moreover, the surface of the SiC layer is preferably a (0001) plane, that is, a Si plane.

[0229] As described above, the present inventors have made an invention relating to heating of a semiconductor layer made of SiC, which uses a resistance heating furnace.

[0230] Therefore, when the step of forming the gate insulating film includes the steps of loading the semiconductor layer into a resistance heating furnace, introducing a gas containing nitrogen and oxygen into the resistance heating furnace to create a nitrogen- and oxygen-containing gas atmosphere, and controlling the heating temperature of the resistance heating furnace to 1200°C or higher while maintaining the gas atmosphere, in addition to the effects of the present invention, the effects of the invention using the above-mentioned resistance heating furnace can be enjoyed. EXAMPLES

[0231] Next, the present invention will be described based on Reference Examples, however, the present invention is not limited to the following Reference Examples. Reference example 1 (N 2 O oxidation) First, an epitaxial layer made of SiC was formed on the Si surface of a wafer-shaped SiC substrate (manufactured by Cree) by growing SiC crystals while doping with N-type impurities. Next, a SiO 2 Form a mask and then SiO 2 Through the Mask, Sci-Fi 6 / O 2 The trenches were formed by injecting gas onto the surface of the epitaxial layer.

[0232] Next, the SiC substrate was placed in a diffusion furnace, and the inside of the furnace was heated to 1275°C. 2 O gas was supplied for 3 hours, which oxidized the inner surface of the trench to form an oxide film.

[0233] Also, N 2 Oxide films were also formed in the same manner as above when the O gas supply time (oxidation time) was 8 hours and 12 hours. Reference Example 2 (Dry oxidation) The same steps as in Reference Example 1 were performed up to the step of forming the trench. After the trench was formed, the SiC substrate was carried into a diffusion furnace, and the inside of the diffusion furnace was heated to 1150° C., and O 2 The gas was supplied for four hours, thereby oxidizing the inner surface of the trench to form an oxide film.

[0234] Also, O 2 Oxide films were also formed in the same manner as above when the gas supply time (oxidation time) was 6 hours and 8 hours. Reference Example 3 (Wet oxidation) The same steps as those in Reference Example 1 were performed up to the step of forming the trench. After the trench was formed, the SiC substrate was carried into a diffusion furnace, and water vapor (H 2 O gas was supplied for 15 minutes, which oxidized the inner surface of the trench to form an oxide film.

[0235] Also, H 2 Oxide films were also formed in the same manner as above when the O gas supply time (oxidation time) was set to 25 minutes and 35 minutes. 1) Oxide film thickness measurement The thickness of each oxide film formed in Reference Examples 1 to 3 was measured for each portion on the side surface and bottom surface of the trench. The results are shown in Figures 10(a) to 10(c) (Figure 10(a): Reference Example 1, Figure 10(b): Reference Example 2, Figure 10(c): Reference Example 3). 2) Oxide film thickness ratio Using the thicknesses of the oxide films shown in Figures 10(a) to (c), the ratio of the thickness of the bottom surface of the oxide film to the thickness of the side surface of the oxide film (bottom surface / side surface) was calculated. The results are shown in Figures 10(a) to (c).

[0236] According to FIG. 10(a), the ratio of the thickness of the part on the bottom of the oxide film to the thickness of the part on the side (bottom / side) was confirmed to be approximately 0.54 (3 hours), 0.46 (8 hours), and 0.48 (12 hours) for each supply time.

[0237] Furthermore, according to FIG. 10(b), the ratio of the thickness of the part of the oxide film on the bottom to the thickness of the part on the side (bottom / side) was confirmed to be approximately 0.20 (4 hours), 0.20 (6 hours), and 0.19 (8 hours) for each supply time.

[0238] Furthermore, according to FIG. 10(c), the ratio of the thickness of the part on the bottom of the oxide film to the thickness of the part on the side (bottom / side) was confirmed to be approximately 0.23 (15 min), 0.21 (25 min), and 0.22 (35 min) for each supply time. [Explanation of symbols]

[0239] 1 Semiconductor device 3 Epitaxial layer 5. Body Region 6 Gate trench 9 Gate insulating film 10 Insulating film side 11 Bottom of insulating film 12 Gate electrode 13 Source Area 18 Polysilicon layer 25 Middle Class 26 Metal Layer 41 Semiconductor Devices 43 Gate Trench 51 Epitaxial layer 53 Body Region 55 Source Region 61 Corner 62 Implant active layer 63 Gate insulating film 64 Insulating film bottom 65 Insulating film side 66 Gate electrode 69 Source wiring 70 Polysilicon layer 71 Middle Class 72 Metal Layer 85 Semiconductor Devices

Claims

1. 1. A method for manufacturing a SiC semiconductor device including a MOSFET including a SiC semiconductor layer of a first conductivity type having a front surface and a back surface, the MOSFET having a gate trench on the front surface side and a drain region of the first conductivity type on the back surface side, the method comprising: a first step of forming a carbon film in a shape that conforms to the gate trench and the surface of the SiC semiconductor layer, the gate trench having at least a portion of an inner surface defined by the drain region, a body formation region in which second conductivity type ions are selectively implanted into the surface side of the drain region, and a source formation region in which first conductivity type ions are selectively implanted into the surface side of the body formation region; a second step of heating the SiC semiconductor layer on which the carbon film is formed to activate ions in the body formation region and the source formation region, thereby forming a body region of a second conductivity type in the SiC semiconductor layer and a source region of a first conductivity type on the front surface side of the body region; a third step of forming a gate insulating film along an inner surface of the gate trench after removing the carbon film; and filling the gate trench with polysilicon; The first step includes a step of maintaining the first temperature for a predetermined time, The second step includes a step of maintaining the second temperature higher than the first temperature for a predetermined time, The method for manufacturing a SiC semiconductor device, wherein the temperature is changed from the first temperature to the second temperature over 30 minutes or more.

2. 1. A method for manufacturing a SiC semiconductor device including a MOSFET including a SiC semiconductor layer of a first conductivity type having a front surface and a back surface, the MOSFET having a gate trench on the front surface side and a drain region of the first conductivity type on the back surface side, the method comprising: a first step of forming a carbon film in a shape that conforms to the gate trench and the surface of the SiC semiconductor layer, the gate trench having at least a portion of an inner surface defined by the drain region, a body formation region in which second conductivity type ions are selectively implanted into the surface side of the drain region, and a source formation region in which first conductivity type ions are selectively implanted into the surface side of the body formation region; a second step of heating the SiC semiconductor layer on which the carbon film is formed to activate ions in the body formation region and the source formation region, thereby forming a body region of a second conductivity type in the SiC semiconductor layer and a source region of a first conductivity type on the front surface side of the body region; a third step of forming a gate insulating film along an inner surface of the gate trench after removing the carbon film; filling the gate trench with polysilicon; forming a source contact wiring that is in ohmic contact with the source region; The first step includes a step of maintaining the first temperature for a predetermined time, The second step includes a step of maintaining the second temperature higher than the first temperature for a predetermined time, the step of forming the source contact wiring includes a step of forming a polysilicon layer at a junction with the source region; A method for manufacturing a SiC semiconductor device, further comprising, before the step of forming the carbon film, a step of forming a source trench penetrating the SiC semiconductor layer from a surface through the source formation region and the body formation region.

3. 1. A method for manufacturing a SiC semiconductor device including a MOSFET including a SiC semiconductor layer of a first conductivity type having a front surface and a back surface, the MOSFET having a gate trench on the front surface side and a drain region of the first conductivity type on the back surface side, the method comprising: a first step of forming a carbon film in a shape that conforms to the gate trench and the surface of the SiC semiconductor layer, the gate trench having at least a portion of an inner surface defined by the drain region, a body formation region in which second conductivity type ions are selectively implanted into the surface side of the drain region, and a source formation region in which first conductivity type ions are selectively implanted into the surface side of the body formation region; a second step of heating the SiC semiconductor layer on which the carbon film is formed to activate ions in the body formation region and the source formation region, thereby forming a body region of a second conductivity type in the SiC semiconductor layer and a source region of a first conductivity type on the front surface side of the body region; a third step of forming a gate insulating film along an inner surface of the gate trench after removing the carbon film; and filling the gate trench with polysilicon; The first step includes a step of maintaining the first temperature for a predetermined time, The second step includes a step of maintaining the second temperature higher than the first temperature for a predetermined time, the third step includes a step of oxidizing and removing the carbon film by an oxygen-containing gas and oxidizing the SiC semiconductor layer to form the gate insulating film, A method for manufacturing a SiC semiconductor device, comprising the steps of: successively performing the first step, the second step, and the third step in one heating furnace without removing the SiC semiconductor layer from the heating furnace.

4. 4. The method for manufacturing a SiC semiconductor device according to claim 1, wherein the third step includes a step of forming the gate insulating film thinner than the carbon film.

5. 5. The method for manufacturing a SiC semiconductor device according to claim 1, wherein the first step includes a step of forming the carbon film having an upper surface located lower than the surface of the SiC semiconductor layer in a central portion away from a side surface of the gate trench.

6. The method for manufacturing a SiC semiconductor device according to any one of claims 1 to 5, wherein the third step includes a step of forming the gate insulating film such that a ratio (first thickness / second thickness) of a first thickness of a portion on a bottom surface of the gate trench to a second thickness of a portion on a side surface of the gate trench is 0.3 to 1.

0.

7. 7. The method for manufacturing a SiC semiconductor device according to claim 1, further comprising the step of etching back the polysilicon until the front surface side of the polysilicon becomes flush with a surface of the SiC semiconductor layer.

8. 4. The method for manufacturing a SiC semiconductor device according to claim 2, wherein the temperature is changed from the first temperature to the second temperature over 30 minutes or more.

9. The step of forming the gate insulating film may include using NO or N 2 The method for producing a SiC semiconductor device according to any one of claims 1 to 8, wherein the method is carried out in a gas containing O.

10. 10. The method for manufacturing a SiC semiconductor device according to claim 1, wherein the first step includes a step of forming an organic material film on a surface of the SiC semiconductor layer, and heating the organic material film to the first temperature to transform the organic material film into the carbon film.

11. The method for manufacturing a SiC semiconductor device according to claim 10, wherein polyimide is used as the organic material film.

12. forming a source contact wiring that is in ohmic contact with the source region; 4. The method for manufacturing a SiC semiconductor device according to claim 1, wherein the step of forming the source contact wiring includes the step of forming a polysilicon layer at a junction with the source region.

13. The method for manufacturing a SiC semiconductor device according to claim 12 , further comprising, before the step of forming the carbon film, a step of forming a source trench penetrating the SiC semiconductor layer from a surface through the source formation region and the body formation region.

14. 14. The method for manufacturing a SiC semiconductor device according to claim 2, wherein the step of forming the source contact wiring includes the step of burying the polysilicon layer in the source trench.

15. The method for manufacturing a SiC semiconductor device according to any one of claims 12 to 14, further comprising the step of implanting an impurity of a first conductivity type or a second conductivity type into the polysilicon layer.

16. The method for manufacturing a SiC semiconductor device according to any one of claims 1 to 15, wherein the step of forming the gate insulating film includes a step of forming a gate insulating film containing nitrogen at a concentration of 0.1 to 10%.

17. the third step includes a step of oxidizing and removing the carbon film by an oxygen-containing gas and oxidizing the SiC semiconductor layer to form the gate insulating film, 3. The method for manufacturing a SiC semiconductor device according to claim 1, wherein the first step, the second step, and the third step are successively performed in one heating furnace without removing the SiC semiconductor layer from the heating furnace.

Citation Information

Patent Citations

  • Method of manufacturing gate oxidized film of insulating gate-type semiconductor device

    JP2002222945A

  • Mos device

    JP2002261275A

  • Silicon carbide-oxide laminate, manufacturing method therefor, and semiconductor device

    JP2005136386A

  • Semiconductor device

    JP2007258465A

  • Method of manufacturing silicon carbide semiconductor device

    JP2007281005A