Circuit board and manufacturing method thereof
The circuit board design with a continuous and thicker bonding layer at the edge, combined with a protruding portion, addresses bonding reliability issues, enhancing both electrical and thermal durability.
Patent Information
- Application Number
- JP2023533899
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-01-04
- Publication Date
- 2024-09-24
- Estimated Expiration
- 2043-01-04
AI Technical Summary
Circuit boards used in power modules face challenges with bonding reliability between ceramic and metal plates due to defects such as peeling and voids, particularly at the edges, which affect heat cycle and electrical characteristics.
A circuit board design with a bonding layer that is formed continuously from the edge to the center of the metal plate, with a thicker thickness at the edge to ensure sufficient pressure and a protruding portion to alleviate thermal stress, and a manufacturing method that applies brazing material differently at the edge and center to enhance bonding reliability.
The design and manufacturing method improve bonding reliability, reduce defects, and enhance electrical and thermal durability of the circuit board.
Smart Images

Figure 0007555493000008 
Figure 0007555493000003 
Figure 0007555493000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a circuit board and a method for manufacturing the same. [Background technology]
[0002] As industrial equipment such as robots and motors become more sophisticated, power modules that control large currents and high voltages are being used. The circuit boards included in such power modules include a ceramic substrate and a copper plate, which are joined together via a brazing material containing an active metal. Such circuit boards are subject to the effects of heat generated by semiconductor elements mounted on the power modules.
[0003] Therefore, in Patent Document 1, in order to improve the TCT reliability evaluated by the TCT (Temperature Cycle Test), it is proposed to form a protruding portion in a part of the bonding layer bonding the ceramic substrate and the copper circuit plate. In Patent Document 2, a technique is proposed in which a second brazing material layer (a layer of Ag-Cu-Ti brazing material) is formed on both sides of the ceramic substrate so as to surround the periphery of a first brazing material layer (a layer of Ag-Ti brazing material), and the first brazing material layer is disposed between the ceramic substrate and the copper plate, and the second brazing material layer is disposed on the outer side of the copper plate. With such a technique, it is intended to prevent peeling of the brazing material solidified layer and improve the bonding reliability of the insulating circuit substrate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2015 / 019602 [Patent Document 2] JP 2020-107671 A Summary of the Invention [Problem to be solved by the invention]
[0005] It is expected that the environment in which circuit boards are used will become increasingly severe in the future. For this reason, it is considered that there will be a demand for circuit boards with even higher levels of reliability. In view of this, the present disclosure provides a circuit board having excellent bonding reliability between a ceramic plate and a metal plate, and a manufacturing method thereof. [Means for solving the problem]
[0006] A circuit board according to one aspect of the present disclosure includes a ceramic plate, a metal plate, and a bonding layer that bonds the ceramic plate and the metal plate, and when viewed in a cross section perpendicular to a main surface of the ceramic plate on which the bonding layer is provided and passing through a center of the metal plate, the bonding layer, and the ceramic plate, a thickness D of the bonding layer between an end of the metal plate and the ceramic plate is E The thickness of the bonding layer between the center of the metal plate and the ceramic plate D C and the bonding layer is formed continuously from between the end of the metal plate and the ceramic plate to between the center of the metal plate and the ceramic plate, thereby providing a circuit board.
[0007] In the bonding layer bonding the ceramic plate and the metal plate, when the portion bonding the center of the metal plate and the portion bonding the end of the metal plate are compared, the bonding layer bonding the end is more likely to have defects such as peeling and voids. If such defects occur, there is a concern that the heat cycle characteristics and electrical characteristics will deteriorate. The following, for example, are considered to be factors that make the bonding layer bonding the end of the metal plate more likely to have defects.
[0008] When a metal plate and a ceramic plate are laminated, for example, using a brazing material layer, if the metal plate and the ceramic plate are pressed in the lamination direction, the brazing material layer is sufficiently pressurized near the center of the metal plate and densely packed. On the other hand, near the ends of the metal plate, the brazing material moves so as to protrude outward from between the metal plate and the ceramic plate, and is therefore not sufficiently pressurized compared to the vicinity of the center. For this reason, the brazing material is less likely to be densely packed at the ends of the metal plate than near the center. Therefore, defects such as peeling and voids in the bonding layer tend to occur near the ends of the metal plate, and the bonding layer is more likely to be separated.
[0009] The bonding layer of the circuit board of the present disclosure is formed continuously from between the edge of the metal plate and the ceramic plate to between the center of the metal plate and the ceramic plate. This allows the metal plate and the ceramic plate to be firmly bonded. The thickness D of the bonding layer between the edge of the metal plate and the ceramic plate is E The thickness of the bonding layer between the center of the metal plate and the ceramic plate D C . Such a circuit board can be manufactured by making the brazing material layer between the end of the metal plate and the ceramic plate thicker than between the center of the metal plate and the ceramic plate. Therefore, the bonding layer between the end of the metal plate and the ceramic plate is also formed under sufficient pressure. This makes it possible to suppress defects such as peeling and voids in the bonding layer near the end of the metal plate. Therefore, the circuit board of the present disclosure has excellent bonding reliability between the ceramic plate and the metal plate. In addition, by suppressing the occurrence of defects in the bonding layer, the source of discharge where electric charges concentrate when a voltage is applied can be reduced, thereby improving electrical characteristics.
[0010] Above thickness D C The above thickness D E The ratio may be equal to or greater than 5. This can sufficiently reduce defects such as peeling of the bonding layer and voids near the ends of the metal plate, thereby further improving the bonding reliability between the ceramic plate and the metal plate.
[0011] In the circuit board of the present disclosure, when viewed in the cross section, the maximum area of the gap in the bonding layer between the ceramic plate and the metal plate is 1000 μm 2 Such a circuit board has better bonding reliability.
[0012] When viewed from the cross section, the bonding layer has a protruding portion formed so as to protrude outward from the lower end of the side surface of the metal plate, and the thickness of the bonding layer is D EThe ratio of the length L of the protruding portion to the length L may be 0.1 or more. Normally, the thermal expansion coefficients of the ceramic plate and the metal plate are different, so that thermal stress occurs due to heat cycles. Such thermal stress occurs in a concentrated manner in the bonding layer at the end of the metal plate. The protruding portion of the bonding layer has a sufficiently long length L, so that the thermal stress can be sufficiently alleviated. Such a circuit board has excellent durability against heat cycles.
[0013] When viewed in the cross section, the bonding layer may have a gradient portion in which the thickness increases from the center toward the end. When the ceramic plate and the metal plate are bonded with the brazing material, the brazing material that becomes the bonding layer flows smoothly from the center to the end of the metal plate and is spread evenly, forming such a bonding layer. This makes it possible to sufficiently reduce defects in the bonding layer not only at the end but also at the center. This makes it possible to further improve the bonding reliability of the circuit board.
[0014] When viewed in the cross section, the metal plate may have a convex shape, and the convex surface of the metal plate may be joined to the ceramic plate by a joining layer. This makes it possible to improve the appearance of the circuit board by suppressing the brazing material from flowing out onto the main surface of the circuit board while sufficiently improving the joining at the circuit end. The height of the convex portion on the convex surface may be 10 to 100 μm. This makes it possible to further improve the joining at the circuit end. In addition, it is possible to further improve the appearance of the circuit board by sufficiently suppressing the brazing material from flowing out onto the main surface of the circuit board.
[0015] A method for manufacturing a circuit board according to one aspect of the present disclosure includes the steps of applying a brazing filler metal to a main surface of a ceramic plate to provide a brazing filler metal layer, stacking the ceramic plate and the metal plate with the brazing filler metal layer sandwiched therebetween to produce a laminate, and heating the laminate to obtain a bonded body in which the ceramic plate and the metal plate are bonded with a bonding layer, wherein when providing the brazing filler metal layer, a second portion of the brazing filler metal layer that contacts an end of the metal plate is made thicker than a first portion of the brazing filler metal layer that contacts the center of the metal plate.
[0016] When a metal plate and a ceramic plate are laminated with a brazing material layer interposed therebetween, the brazing material is sufficiently pressurized and densely packed near the center of the metal plate when the metal plate and the ceramic plate are pressed in the lamination direction. On the other hand, near the ends of the metal plate, the brazing material moves so as to protrude outward from between the metal plate and the ceramic plate, and is not sufficiently pressurized. For this reason, the brazing material is less likely to be densely packed at the ends of the metal plate than near the center. Therefore, defects such as peeling and voids in the bonding layer bonding the metal plate and the ceramic plate tend to occur more easily near the ends of the metal plate.
[0017] Therefore, in the above manufacturing method, when the brazing material is applied to the main surface of the ceramic plate to provide a brazing material layer, the thickness of the second portion of the brazing material layer that contacts the end of the metal plate is made larger than the thickness of the first portion of the brazing material layer that contacts the center of the metal plate. Therefore, when the metal plate and the ceramic plate are laminated so as to sandwich the brazing material layer, the second portion that contacts the end of the metal plate is also sufficiently pressed. This makes it possible to suppress defects such as peeling of the bonding layer and voids at the end of the metal plate when a circuit board is formed. Therefore, it is possible to manufacture a circuit board with excellent bonding reliability between the ceramic plate and the metal plate. Such a circuit board can reduce the discharge source where electric charges concentrate when a voltage is applied by suppressing the occurrence of defects in the bonding layer, thereby improving electrical characteristics.
[0018] The second portion may be formed by applying the brazing material more times than the first portion, thereby making it possible to smoothly form the second portion having a greater thickness than the first portion.
[0019] When the number of times the brazing material is applied to the first portion is n1, and the number of times the brazing material is applied to the second portion is n2, the brazing material layer may be provided by applying the brazing material so as to satisfy n2-n1≧2. With this manufacturing method, the thickness of the second portion and the difference in thickness between the first portion and the second portion can be made sufficiently large. Therefore, defects such as peeling and voids in the bonding layer near the end of the metal plate can be further reduced, and a circuit board with even more excellent bonding reliability can be manufactured.
[0020] The circuit board obtained by the above manufacturing method has a thickness D of the bonding layer between the end of the metal plate and the ceramic plate when viewed in a cross section perpendicular to the main surface of the ceramic plate and passing through the center of the metal plate, the brazing material layer, and the ceramic plate. E The thickness of the bonding layer between the center of the metal plate and the ceramic plate D C The bonding layer may be formed continuously from between the end of the metal plate and the ceramic plate to between the center of the metal plate and the ceramic plate. Such a circuit board has excellent bonding reliability between the ceramic plate and the metal plate. Effect of the Invention
[0021] The present disclosure can provide a circuit board having excellent bonding reliability between a ceramic plate and a metal plate, and a method for manufacturing the same. [Brief description of the drawings]
[0022] [Figure 1] FIG. 1 is a plan view of a circuit board. [Diagram 2] FIG. 2 is a cross-sectional view of the circuit board taken along line II-II of FIG. [Diagram 3] FIG. 3 is an enlarged cross-sectional view showing a part of the cross section of FIG. [Figure 4] FIG. 4 is a schematic cross-sectional view for explaining the method for manufacturing the circuit board. [Diagram 5] FIG. 5 is a SEM photograph of a cross section of the circuit board of Example 1. [Figure 6] FIG. 6 is a SEM photograph of a cross section of the circuit board of Example 1. [Figure 7] FIG. 7 is a SEM photograph of a cross section of the circuit board of Example 2. [Figure 8] FIG. 8 is an SEM photograph of a cross section of the circuit board of Comparative Example 1. [Figure 9] Fig. 9(A) is an optical electron microscope photograph of the circuit board of Example 1. Fig. 9(B) is an optical electron microscope photograph of the circuit board of Example 2. Fig. 9(C) is an optical electron microscope photograph of the circuit board of Comparative Example 1. [Figure 10]Fig. 10(A) is an image of ultrasonic testing (SAT) of the circuit board of Example 1. Fig. 10(B) is an image of ultrasonic testing (SAT) of the circuit board of Example 2. Fig. 10(C) is an image of ultrasonic testing (SAT) of the circuit board of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings as needed. However, the following embodiment is an example for explaining the present disclosure, and is not intended to limit the present disclosure to the following contents. In the description, the same elements or elements having the same functions are designated by the same reference numerals, and overlapping descriptions are omitted as the case may be. In addition, the positional relationship such as up, down, left, right, etc. is based on the positional relationship shown in the drawings unless otherwise specified. Furthermore, the dimensional ratio of each element is not limited to the ratio shown. When multiple components are exemplified, at least one of the multiple components may be included, or multiple components may be included in any combination, unless otherwise specified. A numerical range indicated by the symbol "~" includes a lower limit and an upper limit. That is, a numerical range indicated by "A~B" means A or more and B or less.
[0024] The circuit board according to one embodiment includes a ceramic plate, a metal plate, and a bonding layer that bonds the ceramic plate and the metal plate. The material of the ceramic plate is not particularly limited, and may be, for example, a nitride sintered body, a carbide sintered body, or an oxide sintered body. Specific examples include silicon nitride sintered body, aluminum nitride sintered body, aluminum oxide sintered body, and silicon carbide sintered body. There is no particular limitation as long as the ceramic plate has a plate shape. The thickness of the ceramic plate may be, for example, 0.2 to 2 mm, or 0.32 to 1.1 mm.
[0025] The metal plate may be, for example, a copper plate. The shape is not particularly limited as long as it is a plate. The thickness of the metal plate may be, for example, 0.1 to 1.2 mm, or 0.2 to 0.8 mm. The metal plate may have a plating film on the surface. The metal plate may have one and the other main surfaces that are convex. The metal plate may have a warp so that one main surface is convex and the other main surface is concave. In addition, at least one main surface of the metal plate may be a tapered surface such that the center protrudes more than the end portions.
[0026] The bonding layer may contain one or more metals selected from the group consisting of silver, copper, tin, and an active metal. The two or more metals may be an alloy. The active metal may include one or more metals selected from the group consisting of titanium, hafnium, zirconium, and niobium.
[0027] The bonding layer may contain at least one selected from the group consisting of silver, copper, and alloys thereof. The silver and copper contained in the bonding layer may be contained in the bonding layer as an alloy such as an Ag-Cu eutectic alloy. The silver content in the bonding layer may be 60 to 95 mass% in terms of Ag. The silver and copper contents in the bonding layer may be 75 to 100 mass%, 85 to 99 mass%, or 90 to 98 mass% in terms of Ag and Cu, respectively. This makes it possible to sufficiently reduce the residual stress in the bonding layer while improving the denseness of the bonding layer.
[0028] The content of the active metal in the bonding layer may be 0.5 to 5 parts by mass relative to 100 parts by mass of the total of Ag and Cu. By making the content of the active metal 0.5 parts by mass or more, the bonding strength between the ceramic plate and the bonding layer can be improved. On the other hand, by making the content of the active metal 5 parts by mass or less, the formation of a brittle alloy layer at the bonding interface can be suppressed.
[0029] The metal contained in the bonding layer may be contained as a nitride, oxide, carbide or hydride. As an example, the bonding layer may contain titanium nitride and / or titanium hydride (TiH2). This allows the bonding strength between the ceramic plate and the metal plate to be sufficiently high. The content of TiH2 relative to 100 parts by mass of Ag and Cu in total may be, for example, 1 to 8 parts by mass.
[0030] The titanium nitride phase contained in the bonding layer may be formed in a layered form on the contact surface of the bonding layer with the ceramic plate. The titanium nitride phase may be formed in a continuous layered form throughout the bonding layer. By forming the titanium nitride phase in a continuous layered form, the bonding strength between the ceramic plate and the metal plate can be further increased. The fact that the titanium nitride phase is continuous in a layered form can be confirmed by, for example, an electron probe microanalyzer (EPMA) of the cross section. Here, the cross section in the present disclosure is a cross section that is perpendicular to the main surface of the ceramic plate on which the bonding layer is provided, and passes through the center of the metal plate, the bonding layer, and the ceramic plate.
[0031] When viewed from the cross section, the thickness D of the bonding layer between the edge of the metal plate and the ceramic plate E The thickness of the bonding layer between the center of the metal plate and the ceramic plate D C Such a circuit board has excellent bonding reliability between the ceramic plate and the metal plate. E and thickness D C The measurement method will be described later.
[0032] FIG. 1 is a plan view showing an example of the circuit board of the present embodiment. The circuit board 100 has a ceramic plate 10 and a metal plate 21 bonded to the main surface 10A of the ceramic plate 10 via a bonding layer 31. In this example, two metal plates 21 are provided on the main surface 10A of the ceramic plate 10, but this is not limited thereto. For example, the number of metal plates may be one, or three or more. The shapes of the multiple metal plates may be the same or different from each other. In the plan view shown in FIG. 1, the bonding layer 31 has a protruding portion 31A formed along the outer edge of the metal plate 21 so as to surround the metal plate 21.
[0033] Fig. 2 is a cross-sectional view of the circuit board of Fig. 1 taken along line II-II. That is, Fig. 2 shows a cross section perpendicular to the main surface 10A (main surface 10B) of the ceramic plate 10 on which the bonding layer 31 is provided, passing through the center 21C (center 22C) of the metal plate 21 (metal plate 22), the bonding layer 31 (bonding layer 32), and the ceramic plate 10. The bonding layer 31 is formed continuously from between the end 21E of the metal plate 21 and the ceramic plate 10 to between the center 21C of the metal plate 21 and the ceramic plate 10. That is, the bonding layer 31 is connected from the center 31C to the end 31E without being divided.
[0034] The circuit board 100 is also provided with a metal plate 22 on the main surface (main surface 10B) opposite to the main surface 10A of the ceramic plate 10. The metal plate 22 is also bonded to the main surface 10B of the ceramic plate 10 via a bonding layer 32, similar to the metal plate 21. In this example, the metal plate 22 is also provided on the main surface 10B, but is not limited to this. That is, a metal plate may be provided on only one of the main surfaces of the ceramic plate. The shapes, sizes, and numbers of the metal plates bonded to the main surface 10A and the main surface 10B may be the same as or different from each other.
[0035] 3 is an enlarged cross-sectional view showing an end 21E of the metal plate 21 and an end 31E of the bonding layer 31 in the cross section shown in FIG. Eis measured as follows. Using the lower end 70 (the boundary between the metal plate 21 and the bonding layer 31) of the side surface 21S of the metal plate 21 as a reference, an imaginary straight line VL1 perpendicular to the main surface 10A is drawn so that the distance from the lower end 70 is W (W=100 μm). At this time, the distance W is measured along the main surface 10A. The thickness of the bonding layer 31 along the imaginary straight line VL1 drawn in this way is called "thickness D E」 It becomes.
[0036] Thickness D E From the viewpoint of sufficiently increasing the bonding strength between the metal plate 21 and the ceramic plate 10, the thickness D may be, for example, 20 μm or more, 30 μm or more, or 40 μm or more. E From the viewpoint of saving expensive silver, the thickness D may be 100 μm or less, 80 μm or less, or 60 μm or less. E An example of the range is 20 to 100 μm. When multiple cross sections as shown in FIG. 2 (FIG. 3) are viewed, the thickness D E may be different for each cross section. E may be in the ranges described above.
[0037] The thickness D of the bonding layer 31 between the center portion 21C of the metal plate 21 and the ceramic plate 10 C is measured as follows. As shown in Fig. 2, an imaginary line VL2 is drawn from the center of the main surface 21A of the metal plate 21 so as to be perpendicular to the main surface 10A of the ceramic plate 10. The imaginary line VL2 in Fig. 2 and the imaginary line VL1 in Fig. 3 may be parallel to each other. The thickness of the bonding layer 31 along the imaginary line VL2 drawn in this way is called "thickness D C "
[0038] Thickness D C From the viewpoint of sufficiently increasing the bonding strength between the metal plate 21 and the ceramic plate 10, the thickness D may be, for example, 1 μm or more, 2 μm or more, or 3 μm or more. C From the viewpoint of shortening the melting time of the brazing material containing the powder, the thickness D may be 15 μm or less, 10 μm or less, or 8 μm or less. CAn example of the range is 1 to 15 μm. When multiple cross sections as shown in FIG. 2 (FIG. 3) are viewed, the thickness D C may be different for each cross section. C may be in the ranges described above.
[0039] Thickness D of the end 31E of the bonding layer 31 E The thickness D of the central portion 31C of the bonding layer 31 is C That is, D E >D C The bonding layer 31 is formed in such a state that it is sufficiently pressurized even in the vicinity of the end 31E. This makes it possible to prevent the metal plate 21 from peeling off at the end 31E and to prevent voids from occurring in the bonding layer 31. From the viewpoint of sufficiently preventing peeling and voids from occurring, the thickness D C Thickness D E Ratio of (D E / D C ) may be 5 or more, or may be 6 or more. On the other hand, from the viewpoint of maintaining the bonding strength in the central portion 31C of the bonding layer 31, the thickness D C Thickness D E Ratio of (D E / D C ) may be 20 or less, or may be 15 or less. C Thickness D E Ratio of (D E / D C An example of the range of is 5 to 20.
[0040] As shown in FIG. 2 and FIG. 3, the bonding layer 31 may have a gradient portion 35 in which the thickness of the bonding layer 31 increases from the center 31C toward the end 31E. The bonding layer 31 having such a gradient portion 35 is formed by sufficiently smoothly flowing the brazing material that becomes the bonding layer 31 from the center 31C toward the end 31E when the ceramic plate 10 and the metal plate 21 are bonded using the brazing material. The bonding layer 31 is formed by sufficiently spreading the brazing material evenly. Therefore, defects of the bonding layer 31 can be sufficiently reduced not only near the end 31E of the bonding layer 31 but also near the center 31C. As shown in FIG. 2, the bonding layer 31 may have a gradient portion 35 closer to the end 31E than the center 31C. This can further suppress the occurrence of defects at the end 31E.
[0041] As shown in FIG. 2 and FIG. 3, the bonding layer 31 of the circuit board 100 has a protruding portion 31A formed to protrude outward from the lower end 70 of the metal plate 21. The protruding portion 31A may be expanded in a skirt shape toward the main surface 10A of the ceramic plate 10. By having such a protruding portion 31A, it is possible to alleviate the concentration of thermal stress occurring at the end of the bonding layer 31 due to the difference in thermal expansion coefficient between the ceramic plate 10 and the metal plate 21. From the viewpoint of sufficiently alleviating the concentration of thermal stress, the length L of the protruding portion 31A may be 5 μm or more, 10 μm or more, 30 μm or more, or 50 μm or more. The length L of the protruding portion 31A may be, for example, 500 μm or less, or 300 μm or less, depending on the size of the ceramic plate 10. An example of the range of the length L of the protruding portion 31A is 5 to 500 μm.
[0042] The length L of the protruding portion 31A is measured as follows. As shown in FIG. 3, an imaginary line VL3 is drawn that passes through an end point E1 of the protruding portion 31A on the main surface 10A of the ceramic plate 10 and is perpendicular to the main surface 10A. The imaginary line VL3 is parallel to the imaginary line VL1. The shortest distance between the lower end 70 (the boundary between the metal plate 21 and the bonding layer 31) of the side surface 21S of the metal plate 21 and the imaginary line VL3 is the "length L". When multiple cross sections as shown in FIG. 2 (FIG. 3) are viewed, the length L of the protruding portion 31A may differ from cross section to cross section. In any cross section, the length L may be within the above-mentioned range.
[0043] Thickness D of the bonding layer 31 E The ratio of the length L of the protruding portion 31A to the length D E ) may be 0.1 or more, 0.5 or more, or 1 or more. Since such a bonding layer 31 has a protruding portion 31A with a sufficiently long length L, it is possible to sufficiently relieve thermal stress. Such a circuit board 100 has excellent durability against heat cycles. E Ratio of length L to length (L / D E ) may be 10 or less, 5 or less, or 3 or less, depending on the size of the ceramic plate 10. E Ratio of length L to length (L / D E An example of the range of is 0.1 to 10.
[0044] It is preferable that the voids in the bonding layer 31 are small, and it is preferable that the bonding layer 31 has no voids. The voids become unbonded areas between the ceramic plate 10 and the metal plate 21. Therefore, if the voids become large, the ceramic plate 10 and the metal plate 21 are more likely to peel off from each other, decreasing the bonding reliability. From the viewpoint of improving the bonding reliability of the circuit board 100, the maximum area of the voids is 1000 μm 2 may be less than or equal to 500 μm 2 may be less than or equal to 300 μm 22 and 3, the area of the voids is measured in a cross section perpendicular to the main surface 10A of the ceramic plate 10 and passing through the center 21C of the metal plate 21, the bonding layer 31, and the ceramic plate 10. Specifically, the area of the voids may be obtained by observing the cross section with a SEM (scanning electron microscope) and performing image processing on the region including the voids.
[0045] When viewed in the cross section of FIG. 2, the metal plates 21, 22 have a convex shape. One of the main surfaces of the metal plates 21, 22 is a convex surface, and the convex surface is in contact with the bonding layers 31, 32. That is, the convex surfaces of the metal plates 21, 22 are bonded to the ceramic plate 10 by the bonding layers 31, 32. The height of the convex portion on the convex surface may be 10 to 100 μm. By making the height of the convex portion 10 μm or more, it is possible to prevent the brazing material from becoming excessive when the brazing material is applied multiple times to the portion in contact with the end of the metal plates 21, 22. This sufficiently prevents the brazing material from flowing out to the main surfaces 10A, 10B, and sufficiently improves the appearance of the circuit board 100. By making the height of the convex portion 100 μm or less, it is possible to avoid a shortage of the brazing material in the portion in contact with the end of the metal plates 21, 22, and sufficiently improve the bondability of the end (circuit end) of the metal plates 21, 22. The height of the convex portion is a thickness D E and thickness D C Difference (D E -D C That is, the height of the protrusions is measured based on the height of the outer edges of the metal plates 21 and 22.
[0046] The structure and shape of the bonding layer 32 and metal plate 22 provided on the main surface 10B side of the ceramic plate 10 are the same as those of the bonding layer 31 and metal plate 21 provided on the main surface 10A side. When the circuit board 100 is mounted on a power module, the metal plates 21 and 22 may function as a circuit board having a function of transmitting an electric signal, or as a heat sink having a function of transmitting heat. The metal plates 21 and 22 may also have both a function of transmitting heat and a function of transmitting an electric signal. In a modified example, the structure and shape of the bonding layer and metal plate provided on each of the pair of main surfaces may be different from each other.
[0047] A method for manufacturing a circuit board according to one embodiment includes the steps of applying a brazing filler metal to a main surface of a ceramic plate to provide a brazing filler metal layer, stacking the ceramic plate and the metal plate with the brazing filler metal layer in between to produce a laminate, and heating the laminate to obtain a bonded body in which the ceramic plate and the metal plate are bonded with a bonding layer.
[0048] Each step will be described in detail. First, a slurry containing an inorganic compound powder, a binder resin, a sintering aid, a plasticizer, a dispersant, a solvent, and the like is molded to prepare a green sheet. Examples of inorganic compounds include aluminum nitride (AlN), silicon nitride (Si3N4), silicon carbide, and aluminum oxide. Examples of sintering aids include rare earth metals, alkaline earth metals, metal oxides, fluorides, chlorides, nitrates, and sulfates. These may be used alone or in combination of two or more. The use of a sintering aid can promote the sintering of the inorganic compound powder. Examples of binder resins include methyl cellulose, ethyl cellulose, polyvinyl alcohol, polyvinyl butyral, and (meth)acrylic resins.
[0049] Examples of the plasticizer include purified glycerin, glycerin trioleate, diethylene glycol, phthalic acid plasticizers such as di-n-butyl phthalate, and dibasic acid plasticizers such as di-2-ethylhexyl sebacate. Examples of the dispersant include poly(meth)acrylate and (meth)acrylic acid-maleic acid copolymer. Examples of the solvent include organic solvents such as ethanol and toluene.
[0050] Examples of the method for forming the slurry include a doctor blade method and an extrusion molding method. Next, the green sheet obtained by molding is degreased and sintered. The degreasing may be performed, for example, by heating at 400 to 800°C for 0.5 to 20 hours. This makes it possible to reduce the amount of residual organic matter (carbon) while suppressing oxidation and deterioration of the inorganic compound. The sintering may be performed by heating at 1700 to 1900°C in a non-oxidizing gas atmosphere such as nitrogen, argon, ammonia, or hydrogen. This makes it possible to obtain, for example, a ceramic plate 10. If necessary, the ceramic plate may be laser processed to cut the edges or provide a scribe line on the main surface of the ceramic plate.
[0051] The above-mentioned degreasing and sintering may be performed in a state where a plurality of green sheets are laminated. When the green sheets are laminated and degreasing and sintering are performed, a release layer made of a release agent may be provided between the green sheets in order to facilitate separation of the base material after firing. For example, boron nitride (BN) may be used as the release agent. The release layer may be formed by applying a slurry of boron nitride powder by a method such as spraying, brushing, roll coating, or screen printing. The number of green sheets to be laminated may be, for example, 8 to 100 sheets, or 30 to 70 sheets, from the viewpoint of efficiently mass-producing ceramic plates while sufficiently advancing degreasing.
[0052] A brazing material is applied to the main surface of the ceramic plate thus obtained. The brazing material contains, for example, Ag, Cu, Sn, an active metal, a metal compound containing these as constituent elements, an organic solvent, a binder, and the like. The viscosity of the brazing material (20°C) may be, for example, 5 to 20 Pa s. The content of the organic solvent in the brazing material may be, for example, 5 to 25 mass %, and the content of the binder may be, for example, 2 to 15 mass %.
[0053] A brazing material is applied to the main surface of the ceramic plate by a roll coater method, a screen printing method, a transfer method, or the like to provide a brazing material layer. When providing the brazing material layer, the thickness of a second portion of the brazing material layer that contacts the end portion of the metal plate is made thicker than the thickness of a first portion of the brazing material layer that contacts the center portion of the metal plate. The thickness of the brazing material layer may be changed by changing the application conditions to provide a first portion and a second portion having different thicknesses. The first portion and the second portion may be provided with different thicknesses by changing the number of times the brazing material is applied. That is, the second portion may be formed by applying the brazing material more times than the first portion. This makes it possible to easily provide a first portion and a second portion having different thicknesses on the main surface of the ceramic plate.
[0054] 4 is a schematic cross-sectional view for explaining an example of a method for manufacturing a circuit board. In this example, a brazing material is applied to the main surfaces 10A and 10B of a ceramic plate 10 to form a first portion 81 and a second portion 82. In the first portion 81, the brazing material is applied only once to form a first brazing material layer 41. On the other hand, in the second portion 82, the brazing material is applied three times to provide a second brazing material layer 42 and a third brazing material layer 43 in this order on the first brazing material layer 41. The number of laminations of the brazing material layers in the first portion 81 and the second portion 82 is not particularly limited. For example, the first portion 81 may have a two-layer structure, and the second portion 82 may have a four-layer structure.
[0055] The metal plates 21 and 22 are laminated to the main surfaces 10A and 10B of the ceramic plate 10 on which the brazing material layers are provided. The main surfaces 21B and 22B of the metal plates 21 and 22 are tapered (convex) surfaces that are convex with respect to the main surfaces 10A and 10B of the ceramic plate 10. Therefore, the thicknesses of the end portions 21E and 22E of the metal plates 21 and 22 are smaller than the thicknesses of the central portions 21C and 22C of the metal plates 21 and 22. The method is not limited to using such metal plates 21 and 22, and for example, metal plates that are warped so that the main surfaces 21B and 22B facing the ceramic plate 10 are convex may be used.
[0056] The metal plates 21 and 22 are pressed in a direction toward the ceramic plate 10 (in the direction of the arrow in FIG. 4) to obtain a laminate. With the pressing, the brazing material layer spreads smoothly, and a laminate in which the ceramic plate and the metal plates 21 and 22 are well bonded by the brazing material layer is obtained. The obtained laminate is heated in a heating furnace to bond the ceramic plate 10 and the metal plates 21 and 22 to obtain a bonded body. The heating temperature may be, for example, 700 to 900° C. The atmosphere in the furnace may be an inert gas such as nitrogen, and may be performed under reduced pressure below atmospheric pressure or under vacuum. The heating furnace may be a continuous type that continuously produces a plurality of bonded bodies, or may be a batch type that produces one or a plurality of bonded bodies. Heating may be performed while pressing the bonded body in the stacking direction of the laminate.
[0057] When the laminate is heated, each brazing material layer flows and reacts with the metal plate to form a bonding layer. In this way, when viewed in a cross section perpendicular to the main surface of the ceramic plate and passing through the center of the metal plate, the bonding layer, and the ceramic plate, the thickness D at the end is E The thickness D at the center C A bonding layer larger than the thickness of the metal plate is formed. After that, a surface treatment such as forming a plating film on the metal plate may be performed. At this time, cutting or the like may be performed to adjust the shape of the bonding layer. In this manner, for example, the circuit board 100 can be manufactured.
[0058] In the above manufacturing method, when the number of times the brazing material is applied to the first portion is n1 and the number of times the brazing material is applied to the second portion is n2, the brazing material may be applied so as to satisfy n2-n1≧2 to provide a brazing material layer. This allows the thickness D of the bonding layer between the end of the metal plate and the ceramic plate to be increased. E is the thickness D of the bonding layer between the center of the metal plate and the ceramic plate. C can be significantly larger than
[0059] Although the embodiment of the present disclosure has been described above, the present disclosure is not limited to the above embodiment. For example, when a plurality of bonding layers and a metal plate are provided on a ceramic plate, it is not necessary for all the bonding layers to have the above-mentioned structure. In at least one bonding layer, the thickness D of the end portion is E The thickness of the center is D C Any combination of the upper and lower limit values specifically described in each embodiment above is also included in the present disclosure. In addition, the present disclosure also includes a numerical range in which the upper and / or lower limit values are replaced with values in the examples described below.
[0060] This disclosure includes the following contents [1] to
[11] . [1] A ceramic plate, a metal plate, and a bonding layer that bonds the ceramic plate and the metal plate, When viewed in a cross section perpendicular to the main surface of the ceramic plate on which the bonding layer is provided and passing through the center of the metal plate, the bonding layer, and the ceramic plate, the thickness D of the bonding layer between the end of the metal plate and the ceramic plate E is smaller than the thickness D of the bonding layer between the center of the metal plate and the ceramic plate. C It is larger than The bonding layer is formed continuously from between the end portion of the metal plate and the ceramic plate to between the center portion of the metal plate and the ceramic plate. [2] Thickness D C The thickness D E The circuit board according to [1], wherein the ratio is 5 or more. [3] When viewed in the cross section, the maximum area of the gap of the bonding layer between the ceramic plate and the metal plate is 1000 μm 2 The circuit board according to [1] or [2], [4] When viewed in the cross section, the bonding layer has a protruding portion formed so as to protrude outward from the lower end of the side surface of the metal plate, and the thickness D of the bonding layer E The circuit board according to any one of [1] to [3], wherein a ratio of a length L of the protruding portion to a length L of the protruding portion is 0.1 or more. [5] The circuit board according to any one of [1] to [4], wherein, when viewed in cross section, the bonding layer has a gradient portion in which the thickness increases from the center toward the end. [6] The circuit board according to any one of [1] to [5], wherein when viewed in cross section, the metal plate has a convex shape, and the convex surface of the metal plate is joined to the ceramic plate by the joining layer. [7] The circuit board according to [6], wherein the height of the convex portions on the convex surface is 10 to 100 μm. [8] A step of applying a brazing material to a main surface of the ceramic plate to provide a brazing material layer; a step of stacking the ceramic plate and the metal plate with the brazing material layer therebetween to produce a laminate; and heating the laminate to obtain a bonded body in which the ceramic plate and the metal plate are bonded together with a bonding layer. A method for manufacturing a circuit board, wherein, when providing the brazing material layer, a thickness of a second portion of the brazing material layer that contacts an end portion of the metal plate is made greater than a thickness of a first portion of the brazing material layer that contacts a center portion of the metal plate. [9] The method for manufacturing a circuit board according to [8], wherein the second portion is formed by applying the brazing material more times than the first portion.
[10] The method for manufacturing a circuit board described in [8] or [9], wherein the brazing material is applied to the first portion a number of times, n1, and the brazing material is applied to the second portion a number of times, n2-n1≧2, to provide the brazing material layer.
[11] When viewed in a cross section perpendicular to the main surface of the ceramic plate and passing through the center of the metal plate, the bonding layer, and the ceramic plate, the thickness D of the bonding layer between the end of the metal plate and the ceramic plate E is smaller than the thickness D of the bonding layer between the center of the metal plate and the ceramic plate. C It is larger than The method for manufacturing a circuit board according to any one of [8] to
[10] , wherein the bonding layer is formed continuously from between the end of the metal plate and the ceramic plate to between the center of the metal plate and the ceramic plate. EXAMPLES
[0061] The present disclosure will be described in more detail with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.
[0062] Example 1 [Creating a circuit board] A silicon nitride ceramic plate with a thickness of 0.32 mm, multiple copper metal plates (length x width x thickness = 35 mm x 35 mm x 0.8 mm), and brazing material were prepared. The metal plates were obtained by punching, and were prepared with one main surface warped to be convex and the other main surface concave. The brazing material contained Ag, Cu, Sn, and TiH2. The mass ratio of Ag to Cu was 9:1. The brazing material contained 3 parts by mass of Sn and 3.5 parts by mass of TiH2 per 100 mass of Ag and Cu combined.
[0063] The brazing filler metal was applied by screen printing to predetermined locations on both main surfaces of the ceramic plate. At this time, as shown in Figure 4, the brazing filler metal was applied three times to the area where the edge of the metal plate would come into contact, forming a second part with a three-layer structure. Meanwhile, the area where the center of the metal plate would come into contact formed a first part with a one-layer structure. After forming the brazing filler metal layer, the metal plate was bonded to the main surface of the ceramic plate with the brazing filler metal layer interposed between them. At this time, they were bonded so that the convex main surface of the metal plate and the main surface of the ceramic plate faced each other.
[0064] The metal plate on the main surface of the ceramic plate was pressed toward the ceramic plate at 0.015 MPa to obtain a laminate. A total of 24 metal plates were attached to the main surface of the ceramic plate. The laminate was then heated at 790°C for 1 hour in a vacuum. In this way, a bonded body was obtained in which the metal plate was bonded to the main surface of the ceramic plate via a bonding layer. Then, electroless plating was performed using a Ni-P plating solution (phosphorus concentration: 8 to 12 mass%) to form a circuit board having a plating film on the metal plate.
[0065] [Circuit board evaluation] The circuit board was cut along a direction perpendicular to the main surface of the ceramic board, passing through the center of the metal plate, the bonding layer, and the ceramic board. The cross section obtained by cutting was observed by SEM. Figures 5 and 6 are SEM photographs of the cross section of the circuit board of Example 1. From such cross-sectional images, the thickness D of the end of the bonding layer was E , thickness of the center of the bonding layer D C The thickness of the bonding layer was 100 mm, and the length L of the protruding portion was measured. The bonding layer was also checked for the presence or absence of voids. The results are shown in Table 1.
[0066] 5 and 6 are SEM photographs taken at different positions. Fig. 6 shows a cross-sectional image at a higher magnification than Fig. 5. In the circuit board of Example 1, the thickness D of the bonding layer 31 between the end of the metal plate 21 and the ceramic plate 10 is E is the thickness D of the bonding layer 31 between the center of the metal plate 21 and the ceramic plate 10 C The thickness D was larger than E was measured at a position a distance W (=100 μm) inward from the lower end of the side of the metal plate (the boundary between the copper circuit plate and the bonding layer). The specific measurement procedure was as follows.
[0067] Since the side surface of the metal plate 21 was uneven, first, an imaginary line VL0 was drawn that passed through the lower end of the side surface of the metal plate 21 and was perpendicular to the main surface of the ceramic plate 10. Then, an imaginary line VL1 was drawn parallel to the imaginary line VL0 and spaced 100 μm apart from the imaginary line VL0. On this imaginary line VL1, the thickness D of the bonding layer 31 was E was measured.
[0068] The bonding layer 31 of the circuit board of Example 1 had no voids. The protruding portion of the bonding layer 31 had a skirt-like shape that spread toward the main surface of the ceramic plate 10. The length L of this protruding portion was calculated as the distance between an imaginary line VL3 that passes through an end point E1 of the protruding portion 31A on the main surface of the ceramic plate 10 and is perpendicular to the main surface 10A, and an imaginary line VL0 that is parallel to the imaginary line VL3. The height of the protruding portion on the convex surface of the metal plate 21 (the surface in contact with the bonding layer) was calculated using the formula (D E -D C ) was calculated.
[0069] Example 2 A circuit board was formed and evaluated in the same manner as in Example 1, except that the brazing filler metal was applied twice to the portion of the ceramic plate that was to come into contact with the edge of the metal plate to form a two-layered second portion. The results are shown in Table 1.
[0070] 7 is a SEM photograph of a cross section of the circuit board of Example 2. In the circuit board of Example 2, the thickness D of the bonding layer 31 between the end of the metal plate 21 and the ceramic plate 10 is E is the thickness D of the bonding layer 31 between the center of the metal plate 21 and the ceramic plate 10 C The cross section shown in Figure 7 had no voids, but other cross sections had voids. The area S of the void with the largest area was as shown in Table 1. The area S of the void was determined by image processing of the SEM image.
[0071] Comparative Example 1 A circuit board was formed and evaluated in the same manner as in Example 1, except that when applying the brazing filler metal to the ceramic plate, the brazing filler metal was not applied in multiple coats to the portions that would come into contact with the ends of the metal plate, and all brazing filler metal layers were made into a single layer structure. The results are shown in Table 1.
[0072] 8 is an SEM photograph of a cross section of the circuit board of Comparative Example 1. The bonding layer 131 was not formed between the end of the metal plate 121 and the ceramic plate 110. The bonding layer 131 was not continuous from between the end of the metal plate 121 and the ceramic plate 110 to between the center of the metal plate 121 and the ceramic plate 110, but was divided.
[0073] [Table 1]
[0074] [Optical microscope observation results] Fig. 9 is optical electron microscope photographs taken from the side of the circuit boards of Example 1, Example 2, and Comparative Example 1. Photograph (A) of Fig. 9 is the circuit board of Example 1. Photograph (B) of Fig. 9 is the circuit board of Example 2. Photograph (C) of Fig. 9 is the circuit board of Comparative Example 1. Photographs (A), (B), and (C) all show a part of the metal plate on the upper side, a part of the ceramic plate on the lower side, and a bonding layer therebetween.
[0075] In photo (C) of Figure 9, it was confirmed that a void was exposed at the end of the bonding layer (inside the square frame). In photos (A) and (B) of Figure 9, no void was exposed. Comparing photos (A), (B), and (C) of Figure 9, the bonding layer of Example 1 was the thickest, and the bonding layer of Comparative Example 1 was the thinnest.
[0076] [Ultrasonic inspection results] FIG. 10 shows images of ultrasonic testing (SAT) of the circuit boards of Example 1, Example 2, and Comparative Example 1. Image (A) of FIG. 10 is the circuit board of Example 1. Image (B) of FIG. 10 is the circuit board of Example 2. Image (C) of FIG. 10 is the circuit board of Comparative Example 1. In image (C) of FIG. 10, the edges of some of the metal plates are white (indicated by circles in the figure). These white areas indicate the presence of voids in the bonding layer. Image (B) of FIG. 10 also confirmed the presence of voids in the bonding layer bonding some of the metal plates. In contrast, no voids were confirmed in image (A) of FIG. 10. [Industrial Applicability]
[0077] According to the present disclosure, a circuit board having excellent bonding reliability and a method for manufacturing the same are provided. [Explanation of symbols]
[0078] 10,110...ceramic plate, 10A,10B,21A,21B,22B...main surface, 31,32,131...joining layer, 21,22,121...metal plate, 21C,22C,31C...center, 21E,22E,31E...end, 21S...side, 41...first brazing material layer, 42...second brazing material layer, 43...third brazing material layer, 31A...protruding portion, 35...sloping portion, 70...lower end, 81...first portion, 82...second portion, 100...circuit board.
Claims
1. A ceramic plate, a metal plate, and a bonding layer that bonds the ceramic plate and the metal plate, When viewed in a cross section perpendicular to the main surface of the ceramic plate on which the bonding layer is provided and passing through the center of the metal plate, the bonding layer, and the ceramic plate, a thickness D E of the bonding layer between the end of the metal plate and the ceramic plate is larger than a thickness D C of the bonding layer between the center of the metal plate and the ceramic plate, C The thickness D E is 5 or more, the bonding layer is formed continuously from between the end portion of the metal plate and the ceramic plate to between the center portion of the metal plate and the ceramic plate, In a plan view, the bonding layer has a protruding portion formed along an outer edge of the metal plate so as to surround the metal plate, The protruding portion spreads out in a skirt shape toward the main surface of the ceramic plate.
2. When viewed in cross section, the maximum area of the gap in the bonding layer between the ceramic plate and the metal plate is 1000 μm 2 2. The circuit board of claim 1, wherein:
3. When viewed in the cross section, the bonding layer has the protruding portion formed so as to protrude outward from the lower end of the side surface of the metal plate, and the thickness D of the bonding layer E 2. The circuit board according to claim 1, wherein a ratio of a length L of the protruding portion to a length L of the protruding portion is 0.1 or more.
4. The circuit board according to claim 1 , wherein the bonding layer has a gradient portion in which the thickness increases from a center portion toward an end portion when viewed in cross section.
5. 2. The circuit board according to claim 1, wherein the metal plate has a convex shape when viewed in cross section, and the convex surface of the metal plate is joined to the ceramic plate by the joining layer.
6. 6. The circuit board according to claim 5, wherein the height of the convex portions on the convex surface is 10 to 100 μm.
7. A step of applying a brazing material to a main surface of the ceramic plate to provide a brazing material layer; a step of stacking the ceramic plate and the metal plate with the brazing material layer therebetween to produce a laminate; and heating the laminate to obtain a bonded body in which the ceramic plate and the metal plate are bonded together with a bonding layer. A method for manufacturing a circuit board, in which, when providing the brazing material layer, the thickness of a second portion of the brazing material layer that contacts an end portion of the metal plate is made greater than the thickness of a first portion of the brazing material layer that contacts the center portion of the metal plate by applying the brazing material to the second portion more times than to the first portion.
8. The number of times the brazing material is applied to the first portion is n 1 times, and the number of times the brazing material is applied to the second portion is n 2 When the number of times is n 2 -n 1 The method for manufacturing a circuit board according to claim 7 , wherein the brazing material layer is provided by applying the brazing material so as to satisfy a ratio of 1:1 or more to 1:
2.
9. A thickness D of the bonding layer between the end of the metal plate and the ceramic plate when viewed in a cross section perpendicular to the main surface of the ceramic plate and passing through the center of the metal plate, the bonding layer, and the ceramic plate. E is smaller than the thickness D of the bonding layer between the center of the metal plate and the ceramic plate. C It is larger than 9. The method for manufacturing a circuit board according to claim 7, wherein the bonding layer is formed continuously from between the end of the metal plate and the ceramic plate to between the center of the metal plate and the ceramic plate.
10. The method for manufacturing a circuit board according to claim 9 , wherein the bonding layer has a protruding portion formed so as to surround the metal plate along an outer edge of the metal plate in a plan view.
Citation Information
Patent Citations
Circuit board
JP1998190176A
Power module, substrate thereof, and manufacturing method thereof
JP2007311527A
Method of manufacturing substrate for power module
JP2008311294A
Insulation circuit board manufacturing method and insulation circuit board manufactured using the method
JP2020107671A
Electrical circuit board and power module
JP2022000871A