SUBSTRATE PROCESSING METHOD, SUBSTRATE PROCESSING APPARATUS, AND SUBSTRATE PROCESSING SYSTEM
By irradiating metal-containing resist patterns with vacuum ultraviolet light in a low-oxygen atmosphere and subsequent heat treatment, the substrate processing apparatus enhances etching resistance and reduces surface roughness, enabling precise pattern formation on lower layer films.
Patent Information
- Application Number
- JP2020135982
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-11
- Publication Date
- 2024-09-26
- Estimated Expiration
- 2040-08-11
AI Technical Summary
Existing methods fail to effectively increase the etching resistance and reduce surface roughness of metal-containing resist patterns on substrates during semiconductor manufacturing.
A substrate processing apparatus that irradiates metal-containing resist patterns with vacuum ultraviolet light in a low-oxygen atmosphere, promoting the oxidation of metal components within the resist patterns, followed by heat treatment to enhance etching resistance and reduce surface roughness.
The method increases etching resistance and reduces surface roughness of metal-containing resist patterns, ensuring precise pattern formation on lower layer films.
Smart Images

Figure 0007556230000008 
Figure 0007556230000003 
Figure 0007556230000009
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a substrate processing method, a substrate processing apparatus, and a substrate processing system. [Background technology]
[0002] In the manufacturing process of semiconductor devices, a resist pattern is formed on a semiconductor wafer (hereinafter, referred to as a wafer) as a substrate by photolithography. Patent Document 1 discloses that the resist pattern is irradiated with vacuum ultraviolet light from a deuterium lamp to reduce surface roughness of the pattern.
[0003] Patent Document 2 also describes that a wafer on which a resist pattern made of a metal-containing resist is formed is irradiated with UV light having a peak wavelength of 172 nm in an oxygen atmosphere. This process crosslinks the resist and breaks the bond between the metal component remaining at the bottom of the recess formed by the pattern and the underlying film that forms the bottom, and then the metal component is sublimated by heating the wafer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] WO2019 / 131144 [Patent Document 2] WO2019 / 082851 Summary of the Invention [Problem to be solved by the invention]
[0005] The present disclosure provides a technique that can increase the etching resistance and reduce surface roughness of a metal-containing resist pattern formed on the surface of a substrate. [Means for solving the problem]
[0006] The substrate processing apparatus according to the present disclosure includes a step of irradiating a substrate having a metal-containing resist pattern formed on a surface thereof with vacuum ultraviolet light in a low-oxygen atmosphere in a processing vessel that stores the substrate, the resist pattern being formed on a surface of the substrate; The resist used for the resist pattern containing the metal contains the metal as a constituent component of the resist, and the metal contained in the resist before the irradiation with vacuum ultraviolet light includes a metal having a ligand and a hydroxyl group bonded thereto. Effect of the Invention
[0007] According to the present disclosure, it is possible to increase the etching resistance and reduce surface roughness of a metal-containing resist pattern formed on the surface of a substrate. [Brief description of the drawings]
[0008] [Figure 1] 1 is a plan view of a substrate processing system according to an embodiment of the present disclosure; [Diagram 2] 2 is a vertical sectional side view of a light irradiation module provided in the substrate processing system. FIG. [Diagram 3] 4 is a schematic diagram showing a reaction caused by the light irradiation module. FIG. [Figure 4] FIG. 13 is a plan view of a substrate processing system according to another embodiment. [Diagram 5] FIG. 2 is a side view of the substrate processing system. [Figure 6] FIG. 1 is a schematic diagram showing a longitudinal sectional side view of a wafer obtained in an evaluation test. [Figure 7A] FIG. 1 is a schematic diagram showing a longitudinal sectional side view of a wafer obtained in an evaluation test. [Figure 7B] FIG. 1 is a schematic diagram showing a longitudinal sectional side view of a wafer obtained in an evaluation test. [Figure 7C] FIG. 1 is a schematic diagram showing a longitudinal sectional side view of a wafer obtained in an evaluation test. [Figure 7D] FIG. 1 is a schematic diagram showing a longitudinal sectional side view of a wafer obtained in an evaluation test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] FIG. 1 shows a plan view of a substrate processing system 1 including a light irradiation module 3 which is an embodiment of a substrate processing apparatus according to the present disclosure. The substrate processing system 1 performs a vacuum ultraviolet light (VUV light) irradiation process and a heating process on a wafer W on whose surface a resist pattern, which is a metal-containing resist, is formed. By performing these processes, the etching resistance of the resist pattern is increased and roughness (surface roughness) is reduced. Note that the above-mentioned metal-containing resist contains a metal as a constituent component of the resist, and does not mean a resist containing a metal only as an impurity. An example of the metal that is a constituent component of this resist is tin.
[0010] The substrate processing system 1 is provided under an atmospheric atmosphere and is composed of a carrier block D1 and a processing block D2. In the following, unless otherwise specified, the atmospheric pressure means the atmospheric pressure of the environment in which the substrate processing system is provided. The carrier block D1 and the processing block D2 are arranged on the left and right and connected to each other. The wafer W having the resist pattern described above is transported to the carrier block D1 while being stored in a carrier C, which is a substrate transport container. The carrier block D1 is provided with a stage 11 for the transport container (for the carrier C). The carrier block D1 is also provided with an opening / closing section 12 formed on a side wall of the block, and a transport arm 13 that transports the wafer W to the carrier C placed on the stage 11 via the opening / closing section 12.
[0011] The processing block D2 includes a transfer path 21 for the wafer W extending in the left-right direction and a transfer arm 22 provided on the transfer path 21. The transfer arm 22 and the transfer arm 13 are a transfer mechanism for transferring the wafer W between the carrier C and each processing module provided in the processing block D2. A plurality of processing modules are provided on the front and rear sides of the transfer path 21, lined up in the left-right direction. For example, each processing module on the front side is a light irradiation module 3, and each processing module on the rear side is a heating module 23. A transfer module TRS on which the wafer W is temporarily placed is provided at a position on the transfer path 21 near the carrier block D1, and the wafer W is transferred between the carrier block D1 and the processing block D2 via the transfer module TRS.
[0012] The configuration of each processing module will be described below. Fig. 2 shows a side view of the light irradiation module 3. The light irradiation module 3 includes a processing vessel 31, the interior of which is kept in a vacuum atmosphere. The processing vessel 31 includes a transfer port for the wafer W that opens to the transfer path 21, and is closed by a gate valve 32 except when the wafer W is loaded or unloaded. A stage 33 on which the wafer W is placed is provided within the processing vessel 31. The stage 33 includes lift pins (not shown) and is configured to be able to transfer the wafer W between the stage 33 and the transfer arm 22.
[0013] A housing 34 is provided on the upper part of the processing vessel 31. A plurality of light irradiation units 35 are provided inside the housing 34, which irradiate the wafer W placed on the stage 33 with the above-mentioned VUV light, i.e., light having a wavelength of 10 to 200 nm, and light (shown by a dashed line in the figure) is supplied to the entire surface of the wafer W. As will be described in detail later in the evaluation test, the VUV light irradiated onto the wafer W by the light irradiation units 35 preferably includes light having a wavelength of less than 160 nm, and more specifically, for example, preferably includes light having a wavelength of 120 nm or more.
[0014] Therefore, for example, a light source that irradiates light having a peak wavelength in the range of 120 nm to less than 160 nm can be preferably used as the light irradiation unit 35. As a specific example, a deuterium lamp can be configured to have a peak wavelength of about 150 nm, and therefore can be preferably used as the light irradiation unit 35. In addition, an Ar (argon) excimer lamp with a peak wavelength of 126 nm and a Kr (krypton) excimer lamp with a peak wavelength of 146 nm can be preferably used as the light irradiation unit 35.
[0015] As described above, the light irradiation module 3 is configured to irradiate the wafer W with light having a spectrum with high relative energy at a relatively short wavelength. The reason for this will be described with reference to FIG. 3, which is a schematic diagram of the reaction occurring in the resist. As described above, a resist pattern that is a metal-containing resist film is formed on the surface of the wafer W, and the resist that is the material of this resist film originally contains a ligand (shown as L in the figure) and a metal (shown as M in the figure) to which a hydroxyl group is bonded, as shown on the left side of FIG. 3. Then, by exposure and PEB (Post Exposure Bake) until the resist pattern is formed, the bond between the metal M and the ligand L is cut (i.e., detachment of the ligand L), followed by bonding between the metal M and the oxygen atoms constituting the hydroxyl group (rebonding of the metal M) and dehydration condensation between the hydroxyl groups. By the progression of such a series of reactions, each metal M is present in the resist pattern as an oxide, as shown on the right side of FIG. 3. The metals M that have become oxides are bonded to each other through oxygen atoms, so that they exist in the resist pattern as a stronger compound than before they became oxides.
[0016] Therefore, when the resist pattern contains a large amount of the above-mentioned non-oxidized metal M, the hardness of the pattern is low, and in that case, when the resist pattern is used to dry etch the underlayer film formed below the resist film, the resist pattern does not have sufficient etching resistance. In other words, the resist pattern is also etched to a large extent, and the CD (Critical Dimension), which is the line width of the resist pattern, becomes smaller during etching, which is called pattern thinning.
[0017] In addition, since the non-oxidized metal M on the surface of the resist pattern is not bonded to other metals M via oxygen, it is easily detached from the surface after the pattern is formed. In other words, if there is a large amount of non-oxidized metal M, the surface roughness of the resist pattern becomes large. The thinning and surface roughness of the resist pattern affect the shape of the pattern formed in the above-mentioned underlayer film by dry etching, so there is a risk that the pattern of the underlayer film cannot be formed into the desired shape.
[0018] In order to prevent such a problem, the light irradiation module 3 irradiates the wafer W with the above-mentioned light to promote the oxidation of the metal M. In detail, since a light component with a small wavelength has high energy, in a resist pattern that receives such high energy, the bond between the metal M with the ligand L still bonded thereto and the ligand L is broken. Furthermore, by receiving such high energy, the metal M whose bond has been broken recombines with the oxygen atom of the hydroxyl group and the above-mentioned dehydration condensation occurs. In other words, the reaction of the metal M shown in FIG. 3 to become an oxide is promoted by the light irradiation. This increases the hardness of the resist pattern, reducing the above-mentioned pattern thinning and surface roughness.
[0019] Incidentally, as described in the Background Art section, in Patent Document 1, the resist pattern is irradiated with light including VUV light from a deuterium lamp. The reason for irradiating light from a deuterium lamp in this manner is that the wavelength range of the spectrum of the deuterium lamp is relatively wide, and various reactions are caused in the resist pattern to increase fluidity, thereby obtaining an effect of improving the roughness of the surface of the pattern. However, Patent Document 1 does not state that the resist pattern is made of a metal-containing resist, and therefore does not focus on the fact that the reaction of the metal-containing resist described in Figure 3 is promoted by using light with a relatively short wavelength.
[0020] That is, this technology, which improves the etching resistance of a pattern in a metal-containing resist and reduces surface roughness by focusing on the reaction mechanism described in Fig. 3, is a technology different from Patent Document 1. Also, in Patent Document 2, as described above, the wafer W is surrounded by an oxygen atmosphere and light including VUV light is irradiated onto the resist pattern, but the VUV light is absorbed by oxygen. Therefore, the technology disclosed in Patent Document 2 does not cause the reaction described in Fig. 3 to proceed by VUV light, and is different from this technology.
[0021] Returning to the description of the configuration of the light irradiation module 3, the upstream end of the exhaust pipe 41 is open in the processing vessel 31 of the light irradiation module 3. The downstream side of the exhaust pipe 41 is connected to an exhaust mechanism 42, which is composed of a vacuum pump capable of adjusting the amount of exhaust in the processing vessel 31. As described above, in the light irradiation module 3, the resist pattern is processed by irradiating VUV light, so that atmospheric components (nitrogen and oxygen) that absorb VUV light are exhausted and removed from the processing vessel 31 by the exhaust mechanism 42, and a vacuum atmosphere is formed in the processing vessel 31 as a low-oxygen atmosphere.
[0022] The downstream end of the gas supply pipe 43 is open to the processing vessel 31. The upstream side of the gas supply pipe 43 branches and is connected to a N2 (nitrogen) gas supply source 44 and an Ar (argon) gas supply source 45, respectively. The Ar gas is supplied into the processing vessel 31 during exhaust by the exhaust mechanism 42, and serves to more reliably remove the atmosphere by purging it from the processing vessel 31. The N2 gas is supplied into the processing vessel 31 immediately before the gate valve 32 is opened, and serves to restore the pressure inside the processing vessel 31 after the vacuum atmosphere is formed to the same pressure as the atmospheric pressure, thereby enabling the gate valve 32 to be opened. The exhaust mechanism 42 and the Ar gas supply source 45 constitute a low-oxygen atmosphere forming mechanism.
[0023] Returning to Fig. 1, the heating module 23 will be described. The wafer W that has been processed in the light irradiation module 3 is transported to this heating module 23. As described in Fig. 3, the generation of an oxide of the metal M is contributed to by dehydration condensation between hydroxyl groups after the ligand L is released from the metal M. The heat treatment in this heating module 23 causes the dehydration condensation, accelerating the generation of the oxide of the metal M.
[0024] The heating module 23 includes a hot plate 24 on which the wafer W is placed, and a cooling plate 25. The cooling plate 25 is movable between a position near the transfer path 21 (the front side of the module) and a position above the hot plate 24 at the rear side of the module, and the wafer W is delivered to the cooling plate 25 by the lifting and lowering operation of the transfer arm 22 at the front side of the module. The hot plate 24 includes a heater and lifting pins that support the wafer W, and is configured to heat the placed wafer W to a desired temperature and to transfer the wafer W between the hot plate 24 and the cooling plate 25 that has moved to the rear side of the module. In order to cause the dehydration condensation, the hot plate 24 is set to, for example, 170°C to 200°C. The cooling plate 25 includes a flow path for a refrigerant, and the wafer W heated by the hot plate 24 is placed on the cooling plate 25 and cooled before being delivered to the transfer arm 22.
[0025] Next, the control unit 10 shown in Fig. 1 will be described. The control unit 10 is a computer, and a program stored in a storage medium such as a compact disc, a hard disk, a memory card, or a DVD is installed in the control unit 10. The installed program incorporates instructions (each step) so that a control signal is output to each part of the substrate processing system 1 by the installed program. Then, the wafer W is transported by each transport arm, and the wafer W is processed by each processing module in accordance with the control signal.
[0026] Next, the transfer path and processing of the wafer W in the substrate processing system 1 will be described. The wafer W is transferred in the order of the carrier C → transfer arm 13 → transfer module TRS → transfer arm 22. The wafer W is then transferred into the processing vessel 31 of the light irradiation module 3, which is supplied with N2 gas to have a pressure equivalent to atmospheric pressure, and placed on the stage 33. The processing vessel 31 storing the wafer W is evacuated in this manner, and Ar gas is supplied into the processing vessel 31 at, for example, 10 L / min to 30 L / min. When the inside of the processing vessel 31 becomes a vacuum atmosphere of, for example, 8000 Pa to 12000 Pa, the light irradiation unit 35 irradiates the wafer W with VUV light, and the generation of oxide of the metal M is promoted as described in FIG. 3.
[0027] After that, the irradiation of the VUV light and the evacuation of the inside of the processing vessel 31 are stopped, and N2 gas is supplied into the processing vessel 31 instead of Ar gas, so that the pressure inside the processing vessel 31 becomes equal to atmospheric pressure. After that, the wafer W is carried out from the light irradiation module 3 by the transfer arm 22, and is transferred to the hot plate 24 via the cooling plate 25 of the heating module 23, and the wafer W is placed on the hot plate 24 for, for example, 60 seconds, and heated to the temperature described above. After that, the wafer W is separated from the hot plate 24 by the lifting pins being raised, and then transferred to the transfer arm 22 via the cooling plate 25, and is transferred in the order of the transfer module TRS → the transfer arm 13, and returned to the carrier C. The carrier C to which the wafer W has been returned is transferred to an etching device, where an etching gas is supplied to the wafer W, and the underlying film is etched using the resist pattern as a mask.
[0028] As described above, the light irradiation module 3 irradiates the wafer W, on whose surface a resist pattern made of a metal-containing resist is formed, with VUV light, thereby promoting the oxidation of the metal M, thereby increasing the etching resistance of the resist pattern and reducing surface roughness. Therefore, the shape of the pattern formed in the underlayer film can be made into a desired shape. In the substrate processing system 1, the wafer W is heated in the heating module 23 after irradiation with VUV light. The heating ensures that the metal M is oxidized, so that the etching resistance can be increased and the surface roughness can be reduced.
[0029] Incidentally, the substrate processing system may be configured to form a resist film and form a resist pattern by development. Figures 4 and 5 show a substrate processing system 5 capable of forming the resist pattern and the above-mentioned underlayer film, and the following mainly describes the differences from the substrate processing system 1. The substrate processing system 5 is configured by connecting a carrier block D1, a processing block D5, and an interface block D3 in this order in the left-right direction. An exposure machine D4 that exposes a wafer W along a pattern, for example by EUV (Extreme ultraviolet), is connected to the interface block D3.
[0030] Regarding the processing block D5, it has a configuration in which stories E1 to E6 are stacked. A tower T1 spanning the stories E1 to E6 is provided at a position close to the carrier block D1 of the transfer path 21, and the tower T1 includes transfer modules TRS stacked in multiple stages. In addition, a transfer arm 50 is provided to transfer wafers W between the transfer modules TRS of the tower T1.
[0031] Each of the stories E5 and E6 is configured substantially similarly to the processing block D2 in the substrate processing system 1, and includes a transfer arm 22. However, both the light irradiation module 3 and the heating module 23 are provided on the rear side of the transfer path 21, and a plurality of developing modules 51 that supply a developer to the surface of the wafer W to perform development are provided along the front side of the transfer path 21. Some of the many provided heating modules 23 are used as heating modules for performing PEB.
[0032] The levels E3 and E4 are similar in configuration to the levels E5 and E6, except that the light irradiation module 3 and the heating module 23 are not provided, and a resist film forming module that supplies a metal-containing resist as a chemical solution to the surface of the wafer W to form a resist film is provided instead of the developing module 51. The levels E1 and E2 are provided with a first film forming module that supplies a chemical solution to form a carbon-based film called an SOC film, and a second film forming module that forms an anti-reflective film containing silicon called an SiARC, instead of the resist film forming module. Except for such differences, the levels E1 and E2 are configured similarly to the levels E3 and E4. The above-mentioned anti-reflective film is a lower layer film that is etched using the resist film as a mask. The heating module 23 provided in the levels E1 to E4 is used to remove the solvent that is a component of each chemical solution and remains in the film.
[0033] The interface block D3 includes towers T2, T3, and T4, which are configured by stacking a plurality of modules on top of each other. Detailed description of the modules included in the towers T2 to T4 will be omitted, but the modules of the tower T2 include a transfer module TRS that is stacked in multiple stages. Reference numerals 61, 62, and 63 in the figure are transfer arms that transfer the wafer W between the towers T2 and T3, between the towers T3 and T4, and between the tower T2 and the exposure machine D4, respectively. The transfer arms 13, 22, 50, and 61 to 63 are transfer mechanisms that transfer the wafer W between the carrier C, each processing module provided in the processing block D2, and the exposure machine D4.
[0034] In the substrate processing system 5, the wafer W is transferred from the carrier C to the tower T1 via the transfer arm 22, and then transferred to the story E1 or E2 via the transfer arm 50. The wafer W is then transferred by the transfer arm 22 in the order of the first film forming module, the heating module 23, the second film forming module, and the heating module 23, where an SOC film and an underlying SiARC film are formed in that order. The wafer W is then transferred between the TRSs of the tower T1 by the transfer arm 50, and transferred to the story E3 or E4, and then transferred by the transfer arm 22 in the order of the resist film forming module, the heating module 23, and the tower T2, where a resist film is formed. Thereafter, the wafer W is transferred between the towers T2 and T4 by the transfer arms 61 to 63, and transferred to the exposure machine D4 for exposure.
[0035] The exposed wafer W is transferred between towers T2 to T4 by transfer arms 61 to 63, loaded into floor E5 or E6, and transferred by transfer arm 22 to heating module 23, developing module 51, light irradiation module 3, and heating module 23 in that order. This sequentially performs PEB, resist pattern formation by development processing, VUV light irradiation on the resist pattern, and heating after VUV light irradiation. The wafer W is then returned to carrier C via tower T1 and transfer arms 50 and 13.
[0036] In addition, the heating process after the VUV light irradiation may be performed on the resist pattern in a state in which the ligand L is desorbed from the metal M by the irradiation of VUV light, so for example, a heater may be provided on the stage 33 of the light irradiation module 3 to perform heating during the irradiation of VUV light. In other words, the timing of the VUV light irradiation and the timing of the heating may overlap each other. In addition, the irradiation of VUV light and the heating process after the VUV light irradiation may be performed in separate substrate processing systems. In other words, after the VUV light is irradiated in the light irradiation module 3 of the substrate processing system 1, the wafer W may be stored in the carrier C, and the carrier C may be transported to another substrate processing system, where the processing may be performed in the heating module 23 included in the substrate processing system. In other words, the heating process after the VUV light irradiation may be performed before the start of dry etching of the lower layer film, and may be performed by heating the wafer W before etching using a heater built in a module that performs dry etching of the lower layer film, for example.
[0037] In the light irradiation module 3, the VUV light reaches the wafer W, and a vacuum atmosphere in the pressure range described above is formed in the processing vessel 31 as a low-oxygen atmosphere in order to advance the reaction described above, but this low-oxygen atmosphere is not limited to a vacuum atmosphere. For example, the processing vessel 31 can be processed in an inert gas atmosphere other than N2 gas, such as Ar gas or He (helium) gas, in which case, it is not necessary to form a vacuum in the processing vessel 31, and the wafer W can be processed at a pressure equivalent to atmospheric pressure. In the example described above, when the processing vessel 31 is evacuated to form a vacuum atmosphere, Ar gas is supplied to more reliably remove the air, but such a gas supply is not necessary.
[0038] The substrate is not limited to the wafer W, and may be, for example, a glass substrate for manufacturing a flat panel display. The embodiments disclosed herein are illustrative in all respects and should not be considered as limiting. The above embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims.
[0039] [Evaluation test] Next, evaluation tests carried out in relation to the present technology will be described. Evaluation test 1 In the evaluation test 1, a resist film consisting of an SOC film, an anti-reflection film consisting of a SiARC, and a metal-containing resist was formed in this order on a silicon wafer W, and the resist film was exposed and developed to form a resist pattern. The wafer W was then divided vertically and horizontally in a plan view to form a number of chips. Light was irradiated onto the surfaces of a number of chips using a test device having a configuration roughly similar to that of the light irradiation module 3. A deuterium lamp capable of emitting light with a wavelength of 120 nm to 400 nm was used as the light irradiation unit 35, but the material of the window constituting the light irradiation unit 35 was changed for each process. Of the light directed toward the wafer W, some wavelengths of light are blocked depending on the material of the window. In other words, depending on the chip, only light of a part of the wavelength range described above is irradiated.
[0040] The material of the window is MgF2 (magnesium fluoride), synthetic quartz glass, or borosilicate glass. When the MgF2 window is used, light with a wavelength of 120 nm to 400 nm is irradiated onto the chip, when the synthetic quartz glass window is used, light with a wavelength of 160 nm to 400 nm is irradiated onto the chip, and when the borosilicate glass window is used, light with a wavelength of 270 nm to 400 nm is irradiated onto the chip. Images of the longitudinal sections of the samples irradiated with light using the MgF2 window, the synthetic quartz glass window, and the borosilicate glass window (hereinafter referred to as the MgF2 sample, the synthetic quartz sample, and the borosilicate sample) were obtained by SEM (scanning electron microscope). Images of the longitudinal sections of the chips not irradiated with light (hereinafter referred to as the comparative sample) were also obtained by SEM. The obtained images were compared.
[0041] Furthermore, the comparative sample, MgF2 sample, synthetic quartz sample, and borosilicate sample were each immersed in an aqueous solution of TMAH (tetramethylammonium hydroxide) for 60 seconds to wet etch the resist pattern. Each sample that had been wet etched in this way was then washed for 10 seconds, and images of the longitudinal sections were taken by SEM and compared with each other.
[0042] When the images of each sample before etching were compared, no significant difference was found in the shape of the resist pattern 71. More specifically, the height of the resist pattern 71 of each sample was approximately the same and was generally rectangular. A schematic diagram obtained from an image of a comparative sample representative of the images of each sample before etching is shown in Figure 6. In the figure, the resist pattern is shown as 71, the anti-reflective film (SiARC film) as 72, and the SOC film as 73.
[0043] As a result of comparing the images of each sample after etching and cleaning, a relatively large difference was observed in the shape of the resist pattern 71. Schematic diagrams obtained from the images of each sample after cleaning are shown in Figures 7A to 7D, and Figures 7A, 7B, 7C, and 7D respectively show the comparative sample, the MgF2 sample, the synthetic quartz sample, and the borosilicate sample. In addition, in Figures 7A to 7D, in order to show the difference in height of each resist pattern 71, the bottom height and the top height of the resist pattern 71 of the comparative sample before etching shown in Figure 6 are shown by dotted lines and dashed lines, respectively.
[0044] The resist pattern 71 of the borosilicate sample lost its rectangular shape and its height was reduced due to the etching of the surface layer. The resist pattern 71 of the synthetic quartz sample was also etched on the surface, and although the rectangular shape was relatively high, the height and CD were reduced. The resist pattern 71 of the comparative sample was also etched on the surface, and the height and CD were reduced. The resist pattern 71 of the MgF2 sample was more inhibited from etching than the other samples, and had a shape similar to that before etching.
[0045] It is considered that the etched portion of the resist pattern 71 of each sample is insufficient in the oxidation of the metal M described in FIG. 3. As described above, the MgF2 sample irradiated with light having a wavelength of 120 nm to 400 nm has sufficient oxidation of the metal M, but the synthetic quartz sample irradiated with light having a wavelength of 160 nm to 400 nm and the borosilicate sample irradiated with light having a wavelength of 270 nm to 400 nm have a small degree of oxidation. This is considered to be because, even if light having a wavelength of 160 nm to 400 nm can break the bond between the metal M and the ligand L, the energy of the metal M is insufficient to recombine with oxygen. And, it was confirmed from this evaluation test 1 that the contribution of light having a wavelength of less than 120 nm to 160 nm is large in promoting the oxidation of the metal M, and it is preferable to irradiate the wafer W with light having a wavelength in this range.
[0046] Evaluation test 2 In evaluation test 2, the same films as those in evaluation test 1 were formed on each of a plurality of wafers W, and the resist film was exposed and developed to form a resist pattern 71. The plurality of wafers W on which the resist pattern 71 was formed were irradiated with light having a wavelength of 120 nm to 400 nm from a deuterium lamp under different processing conditions. More specifically, the combination of the flow rate of Ar gas supplied into the processing vessel 31 during light irradiation and the pressure inside the processing vessel 31 was changed for each wafer W to perform the processing.
[0047] Then, the resist patterns 71 of the wafer W that was irradiated with light and the wafer W that was not irradiated with light were imaged, and the CD and LWR (Line Width Roughness), which is an index of unevenness of the groove width of the pattern, were measured. After that, etching gas was supplied to each wafer W, and a pattern was formed by etching the anti-reflection film 72 using the resist pattern 71 as a mask. The pattern of this anti-reflection film 72 was imaged, and the CD and LWR were measured. Hereinafter, the CD and LWR of the resist pattern 71 obtained after development and before etching are collectively referred to as ADI (After Development Inspection), and the CD and LWR of the anti-reflection film 72 obtained after etching are collectively referred to as AEI (After Etching Inspection). Furthermore, the CD difference (ΔCD=CD of ADI-CD of AEI) was calculated for these ADIs and AEIs.
[0048] There are five combinations of the Ar gas flow rate and the pressure in the processing vessel 31 during the light irradiation, and the above ADI, AEI, and ΔCD were obtained under these five processing conditions in the evaluation tests 2-1 to 2-5. Specifically, the processing conditions were: evaluation test 2-1: Ar gas flow rate 20 L / min, processing vessel 31 pressure 10000 Pa; evaluation test 2-2: Ar gas flow rate 15 L / min, processing vessel 31 pressure 10000 Pa; evaluation test 2-3: Ar gas flow rate 30 L / min, processing vessel 31 pressure 10000 Pa; evaluation test 2-4: Ar gas flow rate 20 L / min, processing vessel 31 pressure 8000 Pa; evaluation test 2-5: Ar gas flow rate 20 L / min, processing vessel 31 pressure 12000 Pa. The light irradiation to the wafer W was performed at 50 mJ / cm 2 In addition, the ADI, AEI, and ΔCD of the wafer W that was not irradiated with light were obtained as Comparative Test 2.
[0049] Table 1 below summarizes the results of Evaluation Tests 2-1 to 2-5 and Comparative Test 2, and the units of each value in the table are nm. As shown in Table 1, the AEI of Evaluation Tests 2-1 to 2-5 is larger than the AEI of Comparative Test 2, and the ΔCD of Evaluation Tests 2-1 to 2-5 is smaller than the ΔCD of Comparative Test 2. Therefore, compared to Comparative Test 2, Evaluation Tests 2-1 to 2-5 suppress the pattern thinning (reduction in CD) of the resist pattern during etching, which shows that the CD of the anti-reflection film 72 can be made larger than that of Comparative Test 2. From the results of Evaluation Test 1 and Evaluation Test 2, it can be seen that the etching resistance of the resist pattern can be increased by irradiating VUV light of 120 nm to less than 160 nm. [Table 1]
[0050] Evaluation Test 3 As in evaluation test 2, a resist pattern 71 was formed on each of a plurality of wafers W, and then a different process was performed on each wafer W, and the upper surface of the wafer W was imaged and the ADI was measured. In evaluation test 3-1, the ADI was measured after heating by the heating module 23. Therefore, in evaluation test 3-1, unlike the process described in the embodiment, VUV light was not irradiated. In evaluation test 3-2, the ADI was measured after irradiation with light having a wavelength of 120 nm to 400 nm. In evaluation test 3-3, the ADI was measured after irradiation with light having a wavelength of 120 nm to 400 nm and heating by the heating module 23. In comparison test 3, the ADI was measured for a wafer W that was not irradiated with light and heated after the formation of the resist pattern 71. In evaluation tests 3-2 and 3-3, the light irradiation to the wafer W was 50 mJ / cm 2 In the evaluation tests 3-1 and 3-3, the wafer W was placed on a hot plate heated to 160° C. for 60 seconds. In the evaluation test 3-3, the time from the end of the light irradiation of the wafer W until the wafer W was placed on the hot plate was 3 minutes.
[0051] Table 2 below summarizes the results of Evaluation Tests 3-1 to 3-3 and Comparative Test 3, and the units of each value in the table are nm. As shown in Table 2, the CDs of Evaluation Tests 3-1 to 3-3 are larger than the CD of Comparative Test 3, and among Evaluation Tests 3-1 to 3-3, Evaluation Test 3-3 has the largest CD, followed by Evaluation Test 3-2. It is believed that such results for CD were due to the fact that the amount of non-oxidized metal M desorbed from the surface layer of resist pattern 71 is smaller in Evaluation Tests 3-3, 3-2, and 3-1, in that order.
[0052] Furthermore, the smaller the LWR, the less the surface roughness of the pattern. As shown in Table 2, the LWR was smaller in Evaluation Tests 3-3 and 3-2 than in Comparative Test 3, with Evaluation Test 3-3 having the smallest LWR. From the results of Evaluation Test 1 and Evaluation Test 3, the hardness of resist pattern 71 is increased and surface roughness is suppressed by irradiating VUV light of 120 nm to less than 160 nm. Furthermore, it can be seen that the hardness of the pattern can be further increased and surface roughness can be reduced by performing a heat treatment after the irradiation of the VUV light. [Table 2] [Explanation of symbols]
[0053] W wafer 31 Processing vessel 71 Resist Pattern
Claims
1. The method includes the step of irradiating the resist pattern with vacuum ultraviolet light in a state in which a processing vessel storing a substrate having a metal-containing resist pattern formed on a surface thereof is set to a low-oxygen atmosphere, A substrate processing method, wherein a resist used for a resist pattern containing the metal contains the metal as a constituent component of the resist, and the metal contained in the resist before the irradiation with vacuum ultraviolet light includes a ligand and a hydroxyl group bonded to the metal.
2. The step of irradiating with vacuum ultraviolet light is a step of breaking the bonds to generate an oxide of the metal, 2. The substrate processing method according to claim 1, wherein the metal oxide is a compound in which the metals are bonded to each other via oxygen.
3. 3. The substrate processing method according to claim 1, further comprising a step of heating the substrate irradiated with the vacuum ultraviolet light in order to generate an oxide of the metal, the oxide of the metal being a compound in which the metals are bonded to each other via oxygen.
4. 4. The substrate processing method according to claim 1, wherein the vacuum ultraviolet light includes light having a wavelength of less than 160 nm.
5. A substrate processing method as described in claim 4, wherein the vacuum ultraviolet light includes light having a wavelength of 120 nm or more and less than 160 nm.
6. 6. The substrate processing method according to claim 1, wherein the low-oxygen atmosphere is a vacuum atmosphere formed by evacuating the inside of the processing vessel, or an inert gas atmosphere other than nitrogen gas.
7. A substrate processing apparatus for carrying out the substrate processing method according to any one of claims 1 to 6, A processing vessel; a stage provided in the processing chamber and configured to support a substrate having a resist pattern containing the metal formed on a surface thereof; a low-oxygen atmosphere forming mechanism for forming a low-oxygen atmosphere in the processing vessel; a light irradiation unit that irradiates the resist pattern with vacuum ultraviolet light; A substrate processing apparatus comprising:
8. A substrate processing system for carrying out the substrate processing method according to any one of claims 1 to 6, a stage for a transfer container on which a transfer container for storing substrates is placed; The substrate processing apparatus according to claim 7 ; a heating module for heating a substrate processed by the substrate processing apparatus in order to generate an oxide of the metal, which is a compound in which the metals are bonded to each other via oxygen; a transfer mechanism for transferring the substrate between the transfer container, the substrate processing apparatus, and the heating module; A substrate processing system comprising:
9. a resist film forming module for forming a resist film containing a metal on the substrate; a developing module for developing the resist film exposed by the exposure machine to form the resist pattern, 9. The substrate processing system according to claim 8, wherein the transport mechanism transports the substrate among the transport container, the resist film forming module, the exposure machine, the substrate processing apparatus, and the heating module.
Citation Information
Patent Citations
Fine patterning method and fabrication process of semiconductor device
JP2005197349A
Method for forming mask pattern, storage medium, and apparatus for processing substrate
WO2019082851A1
Light irradiation device
WO2019131144A1