Conductive piezoelectric laminate film and manufacturing method
A laminated structure with specific refractive indices for coating layers and a conductive layer in conductive piezoelectric films addresses color change and tint issues, ensuring high transparency and suitability for touch panels.
Patent Information
- Application Number
- JP2023506866
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-19
- Filing Date
- 2022-02-10
- Publication Date
- 2024-09-27
- Estimated Expiration
- 2042-02-10
AI Technical Summary
Conductive piezoelectric laminate films used in touch panels face issues with high heat treatment causing color change in piezoelectric films and amorphous films exhibiting a yellowish tint without heat treatment.
A laminated structure comprising a piezoelectric film with specific refractive indices for a first and second coating layer and a conductive layer, avoiding high-temperature processing to maintain transparency and suitable color.
The laminated structure achieves high transparency and suitable color, suitable for use in touch panels without the yellowish tint and simplifies the film structure.
Smart Images

Figure 0007557614000003 
Figure 0007557614000004 
Figure 0007557614000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive piezoelectric laminate film and a manufacturing method thereof. [Background technology]
[0002] Touch panels are widely used as devices that allow users to input information by directly touching an image display. A typical form of touch panel is the capacitive touch panel, which uses the change in current capacity that occurs between an electrode and a finger. Conductive films used as touch panels are required to have high transparency and to suppress the generation of color tints.
[0003] As such conductive films, for example, conductive films are disclosed in Patent Documents 1 and 2. The conductive films disclosed in Patent Documents 1 and 2 use a polyethylene terephthalate (PET) film as a base film, and an indium-tin composite oxide (ITO) film is formed as a conductive film, and the crystallinity of the ITO is increased by a heat treatment at about 150° C., thereby realizing a conductive film with high transparency and suppressed color generation. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-074792 A [Patent Document 2] JP 2013-25737 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, attention has been focused on technology that simultaneously detects the position where the operation surface is touched by a finger or the like and the pressure applied to the operation surface by the finger or the like, and it has been proposed to realize this by combining a pressure detection sensor made of a piezoelectric sensor. However, the piezoelectric film used in the piezoelectric sensor loses its color when heated at high temperatures, just like PET film. Therefore, there was a problem that it was difficult to use a conductive piezoelectric laminate film with a piezoelectric film in a touch panel. On the other hand, there was a problem that if an amorphous conductive film was used without heat treatment, a yellowish tinge derived from the conductive film would appear in the conductive piezoelectric laminate film.
[0006] An object of one aspect of the present invention is to provide a conductive piezoelectric laminate film having a piezoelectric film, which has high transparency and a suitable color. [Means for solving the problem]
[0007] In order to solve the above problems, the conductive piezoelectric laminate film of the present invention is configured by stacking a first coating layer, a second coating layer, and a conductive layer in this order on at least one surface of a piezoelectric film, wherein the refractive index of the piezoelectric film is 1.30 or more and 1.50 or less, the refractive index of the first coating layer is 1.45 or more and less than 1.60, the refractive index of the second coating layer is 1.60 or more and less than 1.80, and the refractive index of the conductive layer is 1.80 or more and 2.20 or less.
[0008] In order to solve the above problems, the conductive piezoelectric laminate film manufactured by the manufacturing method for a conductive piezoelectric laminate film according to one embodiment of the present invention is a laminate film constituted by stacking a first coating layer, a second coating layer, and a conductive layer in this order on at least one surface of the piezoelectric film, and the manufacturing method includes a first step of manufacturing a piezoelectric film to form a film having a refractive index of 1.30 or more and 1.50 or less, a second step of forming a first coating layer having a refractive index of 1.45 or more and less than 1.60 on at least one surface of the piezoelectric film, a third step of forming a second coating layer having a refractive index of 1.60 or more and less than 1.80 on a surface of the first coating layer, and a fourth step of forming a conductive layer having a refractive index of 1.80 or more and 2.20 or less on a surface of the second coating layer. Effect of the Invention
[0009] The present invention can realize a conductive piezoelectric laminate film having a piezoelectric film, which has high transparency and a suitable color. [Brief description of the drawings]
[0010] [Figure 1] 1 is a cross-sectional view of a conductive piezoelectric laminate film 10 according to one embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view of a modified example 10' of the conductive piezoelectric laminate film 10 according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described in detail.
[0012] [Configuration of conductive piezoelectric laminate film] A conductive piezoelectric laminate film according to one embodiment of the present invention is configured by stacking a first coating layer, a second coating layer, and a conductive layer in this order on at least one surface of a piezoelectric film, wherein the refractive index of the piezoelectric film is 1.30 or more and 1.50 or less, the refractive index of the first coating layer is 1.45 or more and less than 1.60, the refractive index of the second coating layer is 1.60 or more and less than 1.80, and the refractive index of the conductive layer is 1.80 or more and 2.20 or less.
[0013] In this embodiment, "superimposed in this order" means that in a laminate including the above-mentioned films and layers, the films and layers are arranged in the order listed. The above-mentioned films and layers may be superimposed in contact with each other or may be superimposed via another film or layer within a range in which the effects of this embodiment are exhibited.
[0014] In addition to the above configuration, the conductive piezoelectric laminate film according to this embodiment is configured so that the refractive index of the first coating layer is higher than the refractive index of the piezoelectric film.
[0015] In a further preferred embodiment, in addition to the above configuration, the refractive index of the second coating layer is higher than that of the first coating layer by 0.05 or more, which further improves the transmittance and color.
[0016] In this embodiment, the "refractive index" refers to the refractive index at a wavelength of 589 nm.
[0017] The refractive index of the first coating layer and the second coating layer was measured in accordance with JIS K7142. Specifically, each coating layer prepared experimentally was measured three times at 25.0±1.0°C using an Abbe refractometer by irradiating each layer with measuring light having a wavelength of 589 nm, and the average of the measured values was taken as the refractive index.
[0018] The refractive index of the conductive layer was measured by a multi-angle high-speed spectroscopic ellipsometer (JA Woollam: M-2000) to measure psi (Ψ) and delta (Δ), and the refractive index at a wavelength of 589 nm was calculated therefrom.
[0019] The refractive index of the piezoelectric film was measured in accordance with ASTM D542.
[0020] In this embodiment, the conductive piezoelectric laminate film is not particularly limited in the configuration of the other surface as long as the first coating layer, the second coating layer, and the conductive layer are laminated in this order on one surface of the piezoelectric film. For example, as shown in FIG. 1, the first coating layer 2, the second coating layer 3, and the conductive layer 4 may be laminated only on one surface of the piezoelectric film 1 to form a conductive piezoelectric laminate film 10. Also, as shown in FIG. 2, the first coating layers 2 and 2' may be formed on both surfaces of the piezoelectric film 1, and the second coating layer 3 and the conductive layer 4 may be laminated in this order on one surface of the first coating layer 2 to form a conductive piezoelectric laminate film 10'. Also, the first coating layer 2, the second coating layer 3, and the conductive layer 4 may be laminated in this order on one surface of the piezoelectric film 1, and the first coating layer 2, the second coating layer 3, and the conductive layer 4 may be laminated in this order on the other surface of the piezoelectric film 1.
[0021] Hereinafter, a conductive piezoelectric laminate film 10 shown in FIG. 1 will be mainly described as one embodiment of the present invention.
[0022] [Piezoelectric film 1] The piezoelectric film 1 included in the conductive piezoelectric laminate film 10 according to one embodiment of the present invention means a film having piezoelectricity. For example, the piezoelectric film 1 may be a resin film.
[0023] The refractive index of the piezoelectric film 1 is 1.30 or more and 1.50 or less. Preferably, the refractive index of the piezoelectric film 1 is 1.35 or more and 1.47 or less, and more preferably, 1.38 or more and 1.45 or less. The piezoelectric film 1 that satisfies these conditions may be manufactured by a known method, and the raw material and manufacturing method thereof are not particularly limited.
[0024] For example, a resin film that satisfies the above conditions may be a fluororesin film. In this embodiment, "made of fluororesin" means that the composition constituting the piezoelectric film 1 is mainly composed of fluororesin. Furthermore, "mainly composed of fluororesin" means that the fluororesin is the most abundant component among the resin components in the composition. The content of fluororesin in the composition may be 51% by mass or more, 80% by mass or more, or 100% by mass.
[0025] The resin in this embodiment may be any resin, and may be one or more resins, that can be used in the piezoelectric film 1 of the present invention. For example, fluororesins that can be used in the piezoelectric film 1 include vinylidene fluoride resin, tetrafluoroethylene resin, and mixtures thereof.
[0026] Examples of vinylidene fluoride resins include homopolymers of vinylidene fluoride and copolymers thereof. The content of constituent units derived from monomers other than vinylidene fluoride in the copolymers of vinylidene fluoride may be appropriately determined within a range that allows the piezoelectric film 1 to exhibit characteristics according to its intended use.
[0027] Examples of the monomer other than vinylidene fluoride in the copolymer of vinylidene fluoride include hydrocarbon monomers and fluorine compounds. Examples of the hydrocarbon monomer include ethylene and propylene. The fluorine compound is a fluorine compound other than vinylidene fluoride and has a polymerizable structure. Examples of the fluorine compound include vinyl fluoride, trifluoroethylene, trifluorochloroethylene, tetrafluoroethylene, hexafluoropropylene, and fluoroalkyl vinyl ether.
[0028] For example, the vinylidene fluoride copolymer may be a vinylidene fluoride copolymer (VDF / TFE) in which vinylidene fluoride and trifluoroethylene are copolymerized in a mixing ratio of 80:20, or a vinylidene fluoride copolymer (VDF / TFE / HFP) in which vinylidene fluoride, trifluoroethylene, and hexafluoropropene are copolymerized in a mixing ratio of 40:40:20.
[0029] Examples of tetrafluoroethylene resins include homopolymers of tetrafluoroethylene and copolymers thereof. Examples of monomers other than tetrafluoroethylene that constitute the structural units of the copolymers include ethylene, fluoropropylene, fluoroalkylvinylether, perfluoroalkylvinylether, and perfluorodioxysol.
[0030] A copolymer of vinylidene fluoride and tetratrifluoroethylene can also be suitably used as the fluororesin.
[0031] The piezoelectric film 1 in this embodiment may contain various additives within the range in which the effects of this embodiment can be obtained. The additives may be one or more kinds, and examples thereof include a plasticizer, a lubricant, a crosslinking agent, an ultraviolet absorbing agent, a pH adjusting agent, a stabilizer, an antioxidant, a surfactant, and a pigment.
[0032] The thickness of the piezoelectric film 1 in this embodiment can be appropriately determined within a range in which the effects of this embodiment can be obtained, depending on the application of the conductive piezoelectric laminate film 10. If the thickness of the piezoelectric film 1 is too thin, the mechanical strength may be insufficient, whereas if the thickness is too thick, the effect may plateau or the transparency may become insufficient, making it difficult to use for optical applications. The thickness of the piezoelectric film 1 can be appropriately determined, for example, within a range of 10 to 200 μm.
[0033] More specifically, from the viewpoint of mechanical strength, the thickness of the piezoelectric film 1 is preferably 10 μm or more, more preferably 20 μm or more, and even more preferably 30 μm or more. From the viewpoint of both mechanical strength and economic efficiency, the thickness of the piezoelectric film 1 is preferably 200 μm or less, more preferably 150 μm or less, and even more preferably 100 μm or less. A conductive piezoelectric laminate film 10 including a piezoelectric film 1 having a thickness within the above range can be suitably used for a touch panel.
[0034] [First coating layer 2] In this embodiment, the first coating layer 2 is a layer located between the piezoelectric film 1 and the second coating layer 3.
[0035] The first coating layer 2 may be disposed on only one surface of the piezoelectric film 1 as shown in Fig. 1, or may be disposed on both surfaces as shown in Fig. 2 from the viewpoint of imparting suitable optical properties to the piezoelectric film 1. The first coating layer 2 is preferably disposed adjacent to the piezoelectric film 1 in the thickness direction of the conductive piezoelectric laminate film 10 from the viewpoint of increasing the transparency of the conductive piezoelectric laminate film 10 and from the viewpoint of preventing color development of the piezoelectric film 1 due to the environment.
[0036] The refractive index of the first coating layer 2 is 1.45 or more and less than 1.60, preferably 1.47 or more and 1.57 or less, more preferably 1.49 or more and 1.55 or less.
[0037] The material of the first coating layer 2 may be appropriately selected from any usable material as long as it satisfies such a refractive index. The material may be an inorganic material or an organic material, and may be one or more kinds. The material of the coating layer may also be the material of the hard coat layer. Examples of the material include melamine resin, urethane resin, (meth)acrylic acid ester resin, silane compound, and metal oxide. Note that "(meth)acrylic acid" is a general term for acrylic acid and methacrylic acid, and means one or both of them. In particular, (meth)acrylic acid ester resin is preferable from the viewpoints of sufficient transparency, a wide variety of materials, and low raw material prices.
[0038] The material of the first coating layer 2 may contain other materials necessary to form a coating layer. In the case of a material for a (meth)acrylic acid ester resin coating layer, a composition in which an initiator, an oligomer, a monomer and other components are mixed can generally be used. In this case, the physical properties of the first coating layer 2 are mainly determined by the oligomer and the monomer. Examples of the oligomer include monofunctional or polyfunctional (meth)acrylate. Examples of the monomer include urethane (meth)acrylate, epoxy (meth)acrylate, and polyester (meth)acrylate. Furthermore, inorganic particles and polymer beads, etc. may be added to the material of the first coating layer 2 from the viewpoint of preventing blocking between films and improving adhesion. Examples of the inorganic particles that can be used include synthetic silica, talc, diatomaceous earth, calcium carbonate, feldspar, quartz, etc., and synthetic silica is particularly preferable from the viewpoint of improving the quality of the plastic film. Examples of the synthetic silica include SiO 2 Examples include:
[0039] The first coating layer 2 may further include a material for exhibiting an arbitrary function. For example, the first coating layer 2 may include an antistatic agent. Examples of the antistatic agent include a surfactant, antimony pentoxide, indium-tin oxide (ITO), and a conductive polymer.
[0040] The thickness of the first coating layer 2 is not particularly limited, but the thickness of the first coating layer 2 may be 0.3 μm or more and 3.0 μm or less, and more preferably 0.5 μm or more and 2.0 μm or less.
[0041] 2, by coating the first coating layers 2 and 2' on each side of the piezoelectric film 1, respectively, it is possible to prevent scratches and unevenness on both sides of the piezoelectric film 1. As a result, it is possible to further improve the haze value of the conductive piezoelectric laminate film 10'.
[0042] The first coating layer 2 may be a transparent surface protection layer for preventing scratches, also called a hard coat layer.
[0043] Furthermore, when the refractive index and thickness of the first coating layer 2 are within the ranges specified above, the haze value of the conductive piezoelectric laminate film 10 can be improved.
[0044] [Second coating layer 3] The second coating layer 3 in this embodiment is a layer located between the first coating layer 2 and the conductive layer 4 .
[0045] The refractive index of the second coating layer 3 is 1.60 or more and less than 1.80. The refractive index of the second coating layer 3 is preferably 1.63 or more and less than 1.78, more preferably 1.65 or more and 1.75 or less. The refractive index of the second coating layer 3 is further preferably 0.05 or more higher than that of the first coating layer 2.
[0046] The material of the second coating layer 3 may be appropriately selected from all available materials as long as it satisfies the above refractive index. For example, a resin whose refractive index is adjusted by adding metal oxide fine particles to the materials exemplified as the material of the first coating layer 2 may be used. The metal oxide fine particles are preferably a refractive index material having a refractive index of 1.50 or more. Examples of the metal oxide fine particles include aluminum oxide, titanium oxide, zirconium oxide, zinc oxide, and tin oxide, and among them, titanium oxide and zirconium oxide are preferred.
[0047] The material of the second coating layer 3, like the material of the first coating layer 2, may contain other materials necessary to constitute a coating layer.
[0048] The thickness of the second coating layer 3 may be, for example, 50 nm or more and 500 nm or less. As one example, the film thickness of the second coating layer 3 may be 90 nm or more and 180 nm or less. As another example, the film thickness of the second coating layer 3 may be 240 nm or more and 310 nm or less. As yet another example, the film thickness of the second coating layer 3 may be 380 nm or more and 420 nm or less. When the thickness of the second coating layer 3 is within the above range, the transmittance and color of the conductive piezoelectric laminate film 10 can be improved.
[0049] The second coating layer 3 serves to suitably adjust the transmittance and color of the conductive piezoelectric laminate film 10. In particular, by adjusting the refractive index and thickness of the second coating layer 3, the conductive piezoelectric laminate film 10 can have suitable optical properties.
[0050] As will be described later, when the conductive layer 4 of this embodiment is amorphous, coloring is likely to occur in the conductive piezoelectric laminate film 10. In order to suppress the occurrence of such coloring, the refractive indexes of the first coating layer 2 and the second coating layer 3 are particularly important.
[0051] [Conductive layer 4] In this embodiment, the conductive layer 4 is laminated on the second coating layer 3 .
[0052] The conductive layer 4 in this embodiment has a planar extension and is conductive, and can be called an electrode. When the planar extension is assumed to be one layer, the conductive layer 4 only needs to exhibit sufficient transparency, and the conductive layer 4 itself does not need to have transparency if it has such a structure. For example, the conductive layer 4 may be composed of a conductive member or composition having high transparency, or may be composed of a material that does not have transparency but has an extremely thin or extremely fine structure that can exhibit sufficient transparency.
[0053] The conductive layer 4 may be formed on a transparent substrate and bonded to the transparent coating layer together with the substrate. The conductive layer 4 may be disposed on at least one side of the piezoelectric film 1. In the case where the first coating layer 2 is formed on both sides of the piezoelectric film 1, the conductive layer 4 may be disposed on at least one of the second coating layers 3. The form of the conductive layer 4 is not limited, and may be a nanowire, a mesh, or a thin film. The thin film may be a single layer or a laminated structure of multiple layers.
[0054] The material constituting the conductive layer 4 is not limited, and a metal oxide of at least one metal selected from the group consisting of In, Sn, Zn, Ga, Sb, Ti, Si, Zr, Mg, Al, Au, Ag, Cu, Pd, and W is preferably used. The metal oxide may further contain a metal atom shown in the above group as necessary. As the metal oxide, ITO, antimony-tin composite oxide (ATO), etc. are preferably used, and ITO is particularly preferably used. Other representative examples of materials for the conductive layer 4 include silver nanowires, silver mesh, copper mesh, graphene, and carbon nanotubes.
[0055] The thickness of the conductive layer 4 is not limited, but the surface resistance is preferably 1×10 3From the viewpoint of obtaining a continuous coating having good electrical conductivity of Ω / sq or less, the thickness is preferably 10 nm or more. If the thickness is too thick, the transparency may decrease, and if the thickness is too thin, the electrical resistance may increase and discontinuous parts may be formed in the film structure. From the viewpoint of further increasing the electrical conductivity, the thickness is preferably 15 nm or more, and more preferably 20 nm or more. From the viewpoint of further increasing the transparency of the conductive layer 4, the thickness of the conductive layer 4 is preferably less than 55 nm, and more preferably less than 45 nm. The thickness of the conductive layer 4 can be obtained by a known method of obtaining the thickness from observation of a cross section of such a laminate.
[0056] The amorphousness of the conductive layer 4 can be determined by using an X-ray diffraction method. The amorphousness can be adjusted by the presence or absence of a process for promoting crystallization in the preparation of the conductive layer 4, such as annealing after the formation of the conductive layer 4, and the extent of the process.
[0057] In the conductive piezoelectric laminate film 10 of this embodiment, in order to prevent discoloration of the piezoelectric film 1, it is necessary to avoid heating at high temperatures during processing. For this reason, the material of the conductive layer 4 may become amorphous. Here, amorphous refers to a state of matter in which atoms are irregularly arranged without a crystal structure. It is possible to confirm that the conductive layer 4 is made of an amorphous material by, for example, not detecting a crystal peak of the material of the conductive layer 4 by X-ray diffraction, as described above.
[0058] The refractive index of the conductive layer 4 in this embodiment is 1.80 or more and 2.20 or less. Preferably, the refractive index of the conductive layer 4 is 1.83 or more and 2.00 or less, and more preferably, 1.85 or more and 1.95 or less. When the refractive index of the conductive layer 4 is within the above range, problems such as interference fringes can be prevented from occurring, and the visibility can be prevented from decreasing.
[0059] In one aspect of the conductive piezoelectric laminate film 10 of this embodiment, the conductive layer 4 is made of an indium-tin composite oxide. In yet another aspect, the conductive layer 4 is made of an indium-tin composite oxide, and no peak of the indium-tin composite oxide is detected in X-ray diffraction. This configuration allows the conductive layer 4 to be amorphous and have a refractive index within a suitable range.
[0060] [Other layer configurations] Although not shown, the conductive piezoelectric laminate film 10 of the present invention may be formed by stacking the piezoelectric film 1, the first coating layer 2, the second coating layer 3, and the conductive layer 4 in this order, and other layer configurations may be appropriately added to form the conductive piezoelectric laminate film of the present invention. The other layer configurations may be one or more types.
[0061] For example, one or more additional coating layers different from the first coating layer 2 and the second coating layer 3 may be included.
[0062] When the conductive piezoelectric laminate film 10 has coating layers other than the first coating layer 2 and the second coating layer 3, the total thickness of the coating layers is 0.3 to 4.5 μm. In this embodiment, the "total thickness" of the coating layers is the sum of the thicknesses of the individual coating layers of the conductive piezoelectric laminate film 10. When a coating layer is present only on one main surface of the piezoelectric film 1, the total thickness is the thickness of the coating layer on that one main surface. When coating layers are present on both the one and the other main surfaces of the piezoelectric film 1, the total thickness is the sum of the thickness of the coating layer on one main surface and the thickness of the coating layer on the other main surface.
[0063] The conductive piezoelectric laminated film 10 may be used in combination with an existing electrode layer. The existing electrode layer, for example, serves as a sensor for detecting a position. The existing electrode layer may be, for example, a film containing one or more of polyethylene terephthalate (PET), cycloolefin polymer (COP), and polycarbonate (PC) as materials, to which a conductive layer is laminated. The conductive layer included in the existing electrode layer may contain the same material as the conductive layer 4 according to the present invention described above.
[0064] Other layer configurations include a pressure-sensitive adhesive layer and a release layer that is in contact with the pressure-sensitive adhesive layer and can be peeled off.
[0065] The adhesive layer is a transparent layer having adhesiveness capable of adhering any layer constituting the conductive piezoelectric laminate film 10 or a touch panel described later to other layers. The adhesive layer may be an adhesive having transparency. Such an adhesive may contain a base polymer that exhibits transparency and adhesiveness. Examples of the base polymer include acrylic polymers, silicone polymers, polyesters, polyurethanes, polyamides, polyvinyl ethers, vinyl acetate / vinyl chloride copolymers, modified polyolefins, epoxy polymers, fluorine polymers, and rubber polymers. Examples of rubber polymers include natural rubber and synthetic rubber. The base polymer may be appropriately selected from the above examples. As the adhesive, an acrylic adhesive is preferably used from the viewpoints that it has excellent optical transparency, exhibits adhesive properties such as moderate wettability, cohesiveness, and adhesiveness, and is also excellent in weather resistance and heat resistance.
[0066] Furthermore, other layer configurations may include additional layers that improve the optical properties of the conductive piezoelectric laminate film 10. For example, an anti-glare layer and an anti-reflection layer may be included.
[0067] The anti-glare layer is a layer that contains fine particles and plays a role in preventing reflections. For example, it can be formed by putting fine particles into the resin that is the material of the coating layer. The anti-reflection layer is a layer that improves optical characteristics by adjusting the refractive index. The anti-reflection layer can be formed using the resin that is the material of the coating layer.
[0068] In addition, the optical film may further include a layer having a protective function, such as a known anti-smudge (anti-fingerprint) layer and a protective film layer.
[0069] The thickness of each layer constituting the conductive piezoelectric laminate film 10 can be measured by embedding the conductive piezoelectric laminate film 10 in epoxy resin, cutting the epoxy resin so as to expose a cross section of the conductive piezoelectric laminate film 10, and observing the cross section with a scanning electron microscope. The thickness of the layer may be a representative value of the thickness of the layer, and may be the average value of any multiple measured values, the maximum value of the measured values, or the minimum value of the measured values.
[0070] [Function and effect of conductive piezoelectric laminate film 10] As described above, the conductive piezoelectric laminate film 10 according to the embodiment of the present invention is configured by stacking the first coating layer 2, the second coating layer 3, and the conductive layer 4 in this order on at least one surface of the piezoelectric film 1, and the refractive index of the piezoelectric film 1 is 1.30 or more and 1.50 or less, the refractive index of the first coating layer 2 is 1.45 or more and less than 1.60, the refractive index of the second coating layer 3 is 1.60 or more and less than 1.80, and the refractive index of the conductive layer 4 is 1.80 or more and 2.20 or less. With this configuration, the conductive piezoelectric laminate film 10 has high transparency and a suitable color in addition to having sufficient piezoelectricity due to the piezoelectric film 1. In one embodiment, the conductive piezoelectric laminate film 10 is configured such that the layer shown on the upper side in FIG. 1 has a lower refractive index, and the layer shown on the lower side has a higher refractive index. With such a configuration, the above-mentioned effects are more excellent.
[0071] The conductive piezoelectric laminate film 10 exhibits high transparency as described above and can be suitably used as a pressure detection sensor for devices such as touch panels, etc. By using the conductive piezoelectric laminate film 10, it is possible to simplify the layer structure of devices such as touch panels, or to reduce the overall layer thickness, and it is also possible to increase the degree of freedom in the number and locations of conductive piezoelectric laminate films 10 arranged in devices such as touch panels.
[0072] [Physical Properties of Conductive Piezoelectric Laminated Film 10] The conductive piezoelectric laminate film 10 of this embodiment is preferably sufficiently transparent from the viewpoint of realizing sufficient light transmittance. In this embodiment, the term "transparent" may be appropriately determined depending on the application of the conductive piezoelectric laminate film 10, but it means optical properties such as transmitting a desired proportion or more of visible light, suppressing color, and having sufficiently low turbidity.
[0073] The visible light transmittance of the conductive piezoelectric laminate film 10 can be appropriately determined depending on the application of the conductive piezoelectric laminate film 10. As an example of the visible light transmittance, the transmittance of light having a wavelength of 550 nm may be measured. The wavelength of 550 nm is a wavelength that is called the maximum luminosity in bright light, and is generally used as a guide for measuring the transmittance of visible light. The 550 nm transmittance can be measured, for example, using a haze meter ("NDH7700SP II", manufactured by Nippon Denshoku Industries Co., Ltd.) based on the method described in JIS K7361-1.
[0074] In this embodiment, the transmittance of the conductive piezoelectric laminate film 10 at a wavelength of 550 nm (hereinafter referred to as "550 nm transmittance") is preferably 83% or more, and more preferably 85% or more. If the 550 nm transmittance of the conductive piezoelectric laminate film 10 is within this range, the transmittance is sufficiently high for a film used in devices such as touch panels.
[0075] The degree of color suppression can be appropriately determined depending on the application of the conductive piezoelectric laminate film 10. * a * b * L in color space * Value, a * value, and b * You may also evaluate it by value. * a * b * Each value in the color system can be measured by a known method described in JIS Z8722, for example, using a spectrophotometer.
[0076] From the viewpoint of realizing stable light transmittance, it is preferable that the conductive piezoelectric laminate film 10 of this embodiment does not have a color. In particular, it is preferable that the yellow color derived from the conductive layer 4 is suitably suppressed, so that the yellow chromaticity b * It may also be evaluated by the value of the lightness L * Value and red and green chromaticity a * The value is not particularly limited as long as it does not cause any problems when the conductive piezoelectric laminate film 10 is used as a touch panel.
[0077] The conductive piezoelectric laminate film 10 of this embodiment is b * b may be ≦4; * It is more preferable that the ratio is ≦3. The conductive piezoelectric laminate film 10 within this range has a suppressed yellowish color and has high transparency, and therefore can be suitably used for a touch panel. * The L value of the conductive piezoelectric laminate film 10 is preferably −4 or more. * The value is 85 or more, * The value may be less than or equal to 3. * Value, a * value, and b * If the conductive piezoelectric laminate film 10 has each of these values within the range, the color is sufficiently suppressed and the film has high transparency as a film for use in devices such as touch panels.
[0078] The degree of turbidity can be appropriately determined depending on the application of the conductive piezoelectric laminate film 10. The turbidity may be evaluated by a haze value. The haze value can be measured, for example, using a haze meter based on the method described in JIS K7136.
[0079] The conductive piezoelectric laminate film 10 of this embodiment preferably has a haze value of 2% or less, more preferably 1.5% or less, and even more preferably 1.0% or less. The conductive piezoelectric laminate film 10 having a haze value within this range has sufficiently suppressed turbidity and can be suitably used in devices such as touch panels.
[0080] The conductive piezoelectric laminate film 10 of this embodiment has a surface resistance and a piezoelectric constant d 33 is not particularly limited as long as it is within a range that does not cause practical problems in the application of devices such as touch panels.
[0081] The surface resistance of the conductive piezoelectric laminate film 10 can be measured, for example, using a resistivity meter based on a known method described in JIS K 7194. The surface resistance is, for example, 1×10 3 It is preferably Ω / sq or less, more preferably 400Ω / sq or less, more preferably 300Ω / sq or less, and even more preferably 200Ω / sq or less. In order to obtain better conductivity in the use of devices such as touch panels, the surface resistance is preferably lower, and the lower limit is, for example, 10Ω / sq or more, 20Ω / sq or more.
[0082] Piezoelectric constant d of conductive piezoelectric laminate film 10 33 The piezoelectric constant d can be measured using a piezoelectric constant measuring device. For example, the sample is clipped with 0.2 N, and the generated charge is read when a force of 0.15 N and 110 Hz is applied, and the absolute value is measured. 33The value is, for example, preferably 6 pC / N or more, more preferably 10 pC / N or more, and even more preferably 12 pC / N or more. There is no upper limit to the piezoelectric characteristic, but in the above case, from the viewpoint of sufficiently obtaining the desired effect regarding the piezoelectric performance of the piezoelectric film 1, the piezoelectric constant d 33 It is sufficient that the resistivity is 45 pC / N or less, more preferably 35 pC / N or less, and even more preferably 30 pC / N or less.
[0083] 〔device〕 A device according to an embodiment of the present invention includes the conductive piezoelectric laminate film 10 of the present embodiment described above. The device may be any type as long as it includes the conductive piezoelectric laminate film 10 of the present embodiment. For example, the position and number of the conductive piezoelectric laminate films 10 can be appropriately determined depending on the application or intended function of the device. The conductive piezoelectric laminate film 10 may be used in the device as a pressure detection sensor, such as a touch panel.
[0084] When used as a pressure detection sensor for a touch panel, the conductive piezoelectric laminate film 10 of the present embodiment may be appropriately added to the laminate structure of a conventional touch panel such as a GFF type or GF2 type. In this case, an electrode layer for detecting pressure and a position sensor for detecting position may be directly laminated on the conductive piezoelectric laminate film 10 of the present embodiment, or may be bonded via an adhesive layer. A touch panel having such a configuration can further exhibit functions attributable to the conductive piezoelectric laminate film 10 in addition to the functions of conventional touch panels, and it is possible to configure a touch panel including both a position sensor and a pressure sensor in a transparent laminate structure.
[0085] When the film is used as a touch panel, the adhesive layer may be formed not only on the coating layer but also on another layer that adheres to the coating layer via the adhesive layer during the production of the touch panel. In this case, the adhesive layer may or may not be present on the coating layer side.
[0086] When the conductive piezoelectric laminate film 10 is included in a device, the conductive piezoelectric laminate film 10 serves as an electrode, making it possible to eliminate an electrode layer made of, for example, PET / ITO, which is included in the layered structure of the pressure sensor of a conventional device. This makes it possible to simplify the layered structure of the pressure detection sensor compared to conventional devices.
[0087] [Method for manufacturing conductive piezoelectric laminate film 10] Hereinafter, a method for manufacturing the conductive piezoelectric laminated film 10 of this embodiment will be described. The manufacturing method according to this embodiment is a method for manufacturing a laminated film configured by stacking a first coating layer 2, a second coating layer 3, and a conductive layer 4 in this order on at least one surface of a piezoelectric film 1, and includes a first step of manufacturing the piezoelectric film 1 forming a film having a refractive index of 1.30 or more and 1.50 or less, a second step of forming a first coating layer 2 having a refractive index of 1.45 or more and less than 1.60 on at least one surface of the piezoelectric film 1, a third step of forming a second coating layer 3 having a refractive index of 1.60 or more and less than 1.80 on the surface of the first coating layer 2, and a fourth step of forming a conductive layer 4 having a refractive index of 1.80 or more and 2.20 or less on the surface of the second coating layer 3.
[0088] The first step may be any step for producing the piezoelectric film 1, and steps may be changed or added as appropriate depending on the type of piezoelectric film 1 to be produced. For example, the piezoelectric film 1 can be produced by successively carrying out a step of producing a resin film by a conventionally known method such as a casting method, a heat pressing method, or a melt extrusion method, a step of stretching the resin film, and a step of polarizing a non-polarized resin film.
[0089] In the second step, the material of the first coating layer 2 may be applied to at least one surface of the piezoelectric film 1 produced in the first step. The application method may be a conventionally known method and is not particularly limited, but a wet coating method is particularly preferred in terms of productivity and production costs. The wet coating method may be a known method, and representative methods include roll coating, spin coating, dip coating, and gravure coating. Among these, methods that can form layers continuously, such as roll coating and gravure coating, are preferred in terms of productivity.
[0090] The material for the first coating layer 2 may be applied using, for example, a bar coater or a gravure coater. After application of the material, the material may be dried at 50°C to 180°C for 0.5 to 60 minutes. Furthermore, the dried coating film of the first coating layer 2 may be solidified by UV irradiation. The solidification by UV irradiation may be performed, for example, using a UV irradiation device with 50 to 1200 mJ / cm. 2 The conditions such as the device, material concentration, and temperature used in the second step may be appropriately changed depending on the material and film thickness of the first coating layer 2.
[0091] In the third step, the material of the second coating layer 3 may be applied to the first coating layer 2 prepared in the second step by a known method. For example, it may be applied by a wet coating method like the first coating layer 2. It is also possible to apply it together with the conductive layer 4 by a dry coating method. The conditions of the apparatus, material concentration, temperature, etc. in the third step may be the same as those in the second step. The film thickness of the second coating layer 3 can be adjusted by adjusting the concentration of the material.
[0092] In the fourth step, the conductive layer 4 may be formed on the second coating layer 3 produced in the third step by a known method. The conductive layer 4 may be formed by depositing the material of the conductive layer 4 by, for example, a sputtering method, a vacuum deposition method, an ion plating method, or the like. These methods may be appropriately adopted depending on the required film thickness.
[0093] When the sputtering method is employed, examples of the target material include the above-mentioned inorganic substances constituting the conductive layer 4, and preferably ITO. The tin oxide concentration of ITO is, for example, 0.5 mass% or more, preferably 2 mass% or more, and for example, 15 mass% or less, preferably 13 mass% or less.
[0094] The sputtering gas may be, for example, an inert gas such as Ar. If necessary, a reactive gas such as oxygen gas may be used in combination. When a reactive gas is used in combination, the flow rate of the reactive gas is not particularly limited, but is, for example, 0.1% to 5% of the total flow rate of the sputtering gas and the reactive gas.
[0095] The air pressure during sputtering is, for example, 1 Pa or less, and preferably 0.7 Pa or less, from the viewpoints of suppressing a decrease in the sputtering rate, discharging stability, and the like.
[0096] The power source used in the sputtering method may be, for example, any of a DC power source, an AC power source, an MF power source, and an RF power source, or a combination of these.
[0097] The manufacturing method of this embodiment may further include other steps as long as it includes the first to fourth steps. For example, a step of adding another layer configuration to the conductive piezoelectric laminate film 10 may be added. Also, a step of corona treating the piezoelectric film 1 to enhance adhesion with the first coating layer 2 may be added.
[0098] According to the manufacturing method of this embodiment, a conductive piezoelectric laminate film 10 having high transparency and a suitable color can be manufactured.
[0099] In the manufacturing method of this embodiment, it is not necessary to perform an annealing treatment of the conductive layer 4 after the fourth step. By not performing the annealing treatment, the color of the piezoelectric film 1 is not impaired, so that a conductive piezoelectric laminate film 10 that can be suitably used in devices such as touch panels can be produced.
[0100] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0101] (summary) The present invention can also be expressed as follows.
[0102] The conductive piezoelectric laminate film according to the first embodiment is configured by stacking a first coating layer, a second coating layer, and a conductive layer in this order on at least one surface of a piezoelectric film, the refractive index of the piezoelectric film being 1.30 or more and 1.50 or less, the refractive index of the first coating layer being 1.45 or more and less than 1.60, the refractive index of the second coating layer being 1.60 or more and less than 1.80, and the refractive index of the conductive layer being 1.80 or more and 2.20 or less. This configuration can impart high transparency and a suitable color to the conductive piezoelectric laminate film.
[0103] The conductive piezoelectric laminated film according to the present embodiment is the same as that according to the embodiment 1, except that b * ≦4. The conductive piezoelectric laminate film having this configuration has a suitable color tone and can be suitably used in devices such as touch panels.
[0104] The conductive piezoelectric laminate film according to the present embodiment 3 has a transmittance of 83% or more at a wavelength of 550 nm in the above-mentioned embodiment 1 or 2. The conductive piezoelectric laminate film having this configuration has high transparency and is therefore suitable for use in devices such as touch panels.
[0105] The conductive piezoelectric laminate film according to Aspect 4 has a haze value of 2.0% or less in any one of Aspects 1 to 3. The conductive piezoelectric laminate film having this configuration has a sufficiently low haze and is therefore suitable for use in devices such as touch panels.
[0106] In the conductive piezoelectric laminate film according to aspect 5, in any one of aspects 1 to 4, the conductive layer is made of an indium-tin composite oxide, and no peak of the indium-tin composite oxide is detected in X-ray diffraction. This configuration allows the conductive layer to be amorphous and have a refractive index within a suitable range.
[0107] A device according to the present embodiment 6 includes the conductive piezoelectric laminate film according to any one of the present embodiments 1 to 5. According to this configuration, the film structure of a touch panel or the like in the device can be simplified compared to conventional ones.
[0108] The manufacturing method according to the seventh aspect is a method for manufacturing a conductive piezoelectric laminate film, the conductive piezoelectric laminate film being a laminate film constituted by stacking a first coating layer, a second coating layer, and a conductive layer in this order on at least one surface of the piezoelectric film, and includes the steps of: a first step of manufacturing a piezoelectric film forming a film having a refractive index of 1.30 or more and 1.50 or less, a second step of forming a first coating layer having a refractive index of 1.45 or more and less than 1.60 on at least one surface of the piezoelectric film, a third step of forming a second coating layer having a refractive index of 1.60 or more and less than 1.80 on the surface of the first coating layer, and a fourth step of forming a conductive layer having a refractive index of 1.80 or more and 2.20 or less on the surface of the second coating layer. With this configuration, a conductive piezoelectric laminate film having high transparency and a suitable color can be manufactured.
[0109] The manufacturing method according to the present embodiment 8 does not perform the annealing treatment of the conductive layer after the fourth step in the present embodiment 7. According to this configuration, the color of the piezoelectric film is not impaired, so that a conductive piezoelectric laminate film suitable for use in devices such as touch panels can be produced. EXAMPLES
[0110] Example 1 A resin film (thickness, 120 μm) made of polyvinylidene fluoride (manufactured by Kureha Corporation) with an inherent viscosity of 1.3 dl / g was stretched to a stretch ratio of 4.2 times. After stretching, the film was passed through a polarizing roll to perform a polarization treatment, and a piezoelectric film was obtained. At that time, the polarization treatment was performed by applying a DC voltage that was increased from 0 kV to 12.0 kV. The film after the polarization treatment was further heat-treated at 130°C for 1 minute to obtain a piezoelectric film with a refractive index of 1.42 and a thickness of 40 μm.
[0111] An amorphous silica-containing ultraviolet-curable resin composition made of acrylic resin was applied to the upper surface (A surface) of the piezoelectric film, dried at 80°C, and then irradiated with ultraviolet light to form a first coating layer (thickness 0.4 μm, refractive index 1.52). Next, a first coating layer (thickness 0.4 μm, refractive index 1.52) was formed on the lower surface (B surface) of the piezoelectric film in the same manner. Next, a zirconium oxide particle-containing ultraviolet-curable resin composition was applied to the upper surface of the first coating layer (A surface), dried at 80°C, and then irradiated with ultraviolet light to form a second coating layer (thickness 114 nm, refractive index 1.65). This resulted in a laminate including a piezoelectric film, a first coating layer, and a second coating layer.
[0112] Next, a conductive layer, an ITO film with a refractive index of 1.88 and a thickness of 30 nm, was formed on the second coating layer by reactive sputtering under the following conditions using a sintered material containing 97% by mass of indium oxide and 3% by mass of tin oxide as a target. Thus, a conductive piezoelectric laminate film was obtained.
[0113] Example 2 A conductive piezoelectric laminated film was obtained in the same manner as in Example 1, except that the thickness of the second coating layer was changed to 102 nm.
[0114] Example 3 A conductive piezoelectric laminate film was obtained in the same manner as in Example 1, except that the thicknesses of the first coating layer A, the first coating layer B, the second coating layer, and the conductive layer were changed to 1.0 μm, 0.9 μm, 110 nm, and 35 nm.
[0115] Example 4 A conductive piezoelectric laminated film was obtained in the same manner as in Example 1, except that the thickness of the second coating layer was changed to 84 nm.
[0116] Example 5 A conductive piezoelectric laminate film was obtained in the same manner as in Example 1, except that the refractive index of the second coating layer was changed to 1.75, and the thicknesses of the first coating layer A, the first coating layer B, the second coating layer, and the conductive layer were changed to 1.0 μm, 0.9 μm, 164 nm, and 35 nm, respectively. Example 6 A conductive piezoelectric laminate film was obtained in the same manner as in Example 1, except that the refractive index of the second coating layer was changed to 1.70, and the thicknesses of the first coating layer A, the first coating layer B, the second coating layer, and the conductive layer were changed to 1.0 μm, 1.0 μm, 105 nm, and 28 nm, respectively. Example 7 A conductive piezoelectric laminate film was obtained in the same manner as in Example 1, except that the refractive index of the first coating layer was changed to 1.49, and the thicknesses of the first coating layer B, the second coating layer, and the conductive layer were changed to 1.0 μm, 100 nm, and 28 nm, respectively.
[0117] Comparative Example 1 A conductive piezoelectric laminated film was obtained in the same manner as in Example 1, except that the first coating layer and the second coating layer were not formed.
[0118] Comparative Example 2 A conductive piezoelectric laminated film was obtained in the same manner as in Example 3, except that the second coating layer was not formed.
[0119] Comparative Example 3 A conductive piezoelectric laminated film was obtained in the same manner as in Example 3, except that the refractive index of the second coating layer was changed to 1.52 and the thickness of the second coating layer was changed to 133 nm.
[0120] Comparative Example 4 A conductive piezoelectric laminated film was obtained in the same manner as in Example 3, except that the refractive index of the second coating layer was changed to 1.52 and the thickness of the second coating layer was changed to 212 nm.
[0121] Comparative Example 5 A hollow silica-containing ultraviolet-curable resin composition having a refractive index of 1.35 was applied onto the second coating layer, dried at 80°C, and then irradiated with ultraviolet light to form a third coating layer with a thickness of 80 nm. A conductive piezoelectric laminate film was obtained in the same manner as in Example 3, except that the third coating layer was formed with a thickness of 80 nm.
[0122] Comparative Example 6 A conductive piezoelectric laminated film was obtained in the same manner as in Example 6, except that the refractive index of the first coating layer was changed to 1.65 and the first coating layer B was not provided.
[0123] Comparative Example 7 A conductive piezoelectric laminated film was obtained in the same manner as in Example 6, except that the refractive index of the first coating layer was changed to 1.39, first coating layer B was not provided, and the thickness of the second coating layer was 96.
[0124] The configurations of the conductive piezoelectric laminated films of Examples 1 to 7 and Comparative Examples 1 to 7 are shown in Table 1.
[0125] [Table 1]
[0126] 〔evaluation〕 For the films of Examples 1 to 7 and Comparative Examples 1 to 7, the surface resistivity and the piezoelectric constant d 33 value, 550nm transmittance, haze value, L * , a * , and b * The physical and optical properties of each film were evaluated.
[0127] [Physical property evaluation]
[0128] (Coating layer thickness) Each of the conductive piezoelectric laminate films of Examples 1 to 7 and Comparative Examples 1 to 7 was embedded in epoxy resin, and the epoxy resin was cut so that the cross section of the conductive piezoelectric laminate film was exposed. The exposed cross section of the conductive piezoelectric laminate film was observed using a scanning electron microscope ("SU3800", Hitachi High-Tech Corporation) at an accelerating voltage of 3.0 kV and a magnification of 50,000 times, and the thickness of the coating layer in the conductive piezoelectric laminate film was measured.
[0129] In measuring the thickness of each coating layer, the thickness was measured at two points of each coating layer, and the average value was taken as the thickness of each coating layer. In addition, under the above observation conditions, the interface of each coating layer was observed as a substantially smooth line, and in measuring the thickness of each coating layer, the distance between the lines was measured.
[0130] (Thickness of conductive layer) The cross section of each of the conductive piezoelectric laminated films of Examples 1 to 7 and Comparative Examples 1 to 7 was observed using the above-mentioned scanning electron microscope under conditions of an acceleration voltage of 3.0 kV and a magnification of 50,000 times, and the thickness was measured at two points of each ITO film. The average value of the obtained measurements was calculated and defined as the thickness of the conductive layer. (Surface resistance value) The surface resistance (Ω / sq, hereinafter simply referred to as "resistance") of each of the conductive piezoelectric laminate films of Examples 1 to 7 and Comparative Examples 1 to 7 was measured in accordance with JIS K 7194 using a resistivity meter (LorestaGP MCP-T610, manufactured by Mitsubishi Chemical Analytech Co., Ltd.). The resistance was measured three times, and the average of the three measurements was determined as a representative value. If the resistance is 400Ω / sq or less, it can be determined that there is no practical problem in the use of the film in devices such as touch panels.
[0131] (Piezoelectric constant d 33 value) The piezoelectric constants d of the conductive piezoelectric laminated films of Examples 1 to 7 and Comparative Examples 1 to 7 33The sample was clipped with 0.2 N and the generated charge was read when a force of 0.15 N, 110 Hz was applied using a piezoelectric constant measuring device ("Piezometer System PM300", manufactured by PIEZOTEST). 33 The measured value of is a positive or negative value depending on the front and back of the film being measured, but in this specification, the absolute value is described. 33 A value of 6 pC / N or more can be judged to pose no practical problems when used in devices such as touch panels.
[0132] [Diffraction peaks from ITO] For each of the conductive piezoelectric laminate films of Examples 1 to 7 and Comparative Examples 1 to 7, the presence or absence of a diffraction peak derived from ITO in the X-ray diffraction of the conductive layer was measured. The presence or absence of the diffraction peak was measured by an in-plane method on the surface of the conductive layer using an X-ray diffractometer (XRD). In the measurement, the range of diffraction angles (2θ) = 15.0 to 70.0° was scanned at a scanning speed of 1° / min. Details of the measurement conditions are shown below. <Measurement conditions> Equipment: Rigaku SmartLab X-ray source: Cu-Kα (λ=1.5418Å) 40kV 30mA Detector: SC-70 Step width: 0.04° Scan range: 15.0~70.0° Slit: Entrance slit = 0.2 mm Length control slit = 10mm Receiving slit = 20 mm
[0133] In all of the conductive piezoelectric laminated films of Examples 1 to 7 and Comparative Examples 1 to 7, no diffraction peaks derived from ITO were observed.
[0134] [Optical property evaluation] (550nm transmittance) The 550 nm transmittance of each of the conductive piezoelectric laminate films of the examples and comparative examples was measured using a haze meter ("NDH7700SP II", manufactured by Nippon Denshoku Industries Co., Ltd.) based on the method described in JIS K7361-1. It can be determined that a 550 nm transmittance of 83% or more is practically acceptable for use in devices such as touch panels, 84% or more is more preferable, and 85% or more is even more preferable.
[0135] (Haze value) The haze values of the coating films used in the examples and the piezoelectric films used in the comparative examples were measured using a haze meter ("NDH7700SP II", manufactured by Nippon Denshoku Industries Co., Ltd.) according to the method described in JIS K7136. If the haze value is 2.0 or less, it can be determined that there is no practical problem in the use of devices such as touch panels. It can be determined that the haze value is preferably 2.0 or less, more preferably 1.5% or less, and even more preferably 1.0% or less.
[0136] (L * Value, a * Value, b * value) The L of each of the conductive piezoelectric laminated films of the examples and the comparative examples * a * b * L in color space * Value, a * value and b * The L value was measured using a spectrophotometer ("SE7700", manufactured by Nippon Denshoku Industries Co., Ltd.) according to a method conforming to JIS Z8722. * A value of 85 or more can be judged to be satisfactory for practical use in devices such as touch panels. * If the value is 3 or less, it can be determined that there is no practical problem in the use of devices such as touch panels. * If the value is 4 or less, it can be judged that there is no practical problem in the use of devices such as touch panels. *It can be determined that a value of 3 or less is more preferable.
[0137] The results of the above evaluation are shown in Table 2.
[0138] [Table 2]
[0139] As shown in Table 2, the conductive piezoelectric laminate films of Examples 1 to 7 have physical properties that are practically acceptable for use in devices such as touch panels, and further have high transparency and a suitable color. In contrast, the conductive piezoelectric laminate films of Comparative Examples 1 to 7 have * >4 and the film was yellowish. [Industrial Applicability]
[0140] The present invention can be used in devices such as touch panels. [Explanation of symbols]
[0141] 1 Piezoelectric film 2, 2' First coating layer 3 Second Coating Layer 4 Conductive layer 10, 10' Conductive piezoelectric laminate film
Claims
1. A first coating layer, a second coating layer, and a conductive layer are laminated in this order on at least one surface of the piezoelectric film; The refractive index of the piezoelectric film is 1.30 or more and 1.50 or less, The refractive index of the first coating layer is 1.45 or more and less than 1.60; The refractive index of the second coating layer is 1.60 or more and less than 1.80; The conductive layer has a refractive index of 1.80 or more and 2.20 or less, A conductive piezoelectric laminate film, wherein the refractive index of a first coating layer is higher than the refractive index of the piezoelectric film.
2. b * 2. The conductive piezoelectric laminate film according to claim 1, wherein the elastic modulus is ≦4.
3. 3. The conductive piezoelectric laminate film according to claim 1, which has a transmittance of 83% or more at a wavelength of 550 nm.
4. The conductive piezoelectric laminate film according to claim 1 , which has a haze value of 2.0% or less.
5. the conductive layer is made of an indium-tin composite oxide; The conductive piezoelectric laminate film according to any one of claims 1 to 4, wherein no peak of said indium-tin composite oxide is detected in X-ray diffraction.
6. A conductive piezoelectric laminate film described in any one of claims 1 to 5, wherein the thickness of the first coating layer is 0.3 μm or more and 3.0 μm or less.
7. A conductive piezoelectric laminate film described in any one of claims 1 to 6, wherein the refractive index of the second coating layer is 0.05 or more higher than the refractive index of the first coating layer.
8. A device comprising the conductive piezoelectric laminate film according to any one of claims 1 to 7.
9. A method for producing a conductive piezoelectric laminate film, comprising the steps of: the conductive piezoelectric laminate film is a laminate film formed by laminating a first coating layer, a second coating layer, and a conductive layer in this order on at least one surface of a piezoelectric film; A first step of manufacturing a piezoelectric film forming a film having a refractive index of 1.30 or more and 1.50 or less; a second step of forming a first coating layer having a refractive index of 1.45 or more and less than 1.60 on at least one surface of the piezoelectric film; a third step of forming a second coating layer having a refractive index of 1.60 or more and less than 1.80 on the surface of the first coating layer; a fourth step of forming a conductive layer having a refractive index of 1.80 or more and 2.20 or less on the surface of the second coating layer; A method for producing a conductive piezoelectric laminate film, comprising the steps of:
10. The method for producing a conductive piezoelectric laminate film according to claim 9 , wherein the conductive layer is not annealed after the fourth step.
Citation Information
Patent Citations
Tone correction film and transparent conductive film using the same
JP2013025737A
laminate
JP2015186908A
Transparent conductive film and touch panel
JP2017074792A
Piezoelectric sensor and display using piezoelectric sensor
JP2017215319A
Piezoelectric film with transparent electrode, and pressure sensor
JP2017216451A