Molded body, method for manufacturing positive electrode active material for non-aqueous electrolyte secondary battery, and method for manufacturing non-aqueous electrolyte secondary battery

By molding lithium mixture powder into shaped bodies for direct gas exchange during firing, the method addresses low productivity and high costs in producing lithium-nickel composite oxide, achieving efficient and cost-effective production.

JP7558633B2Active Publication Date: 2024-10-01SUMITOMO METAL MINING CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2018062857
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-03-28
Publication Date
2024-10-01
Estimated Expiration
2038-03-28

AI Technical Summary

Technical Problem

Existing methods for producing lithium-nickel composite oxide for non-aqueous electrolyte secondary batteries face challenges such as long firing times, poor gas exchange during sintering, and the use of containers like crucibles or saggers that deteriorate, leading to low productivity and high costs.

Method used

The method involves molding a lithium mixture powder into shaped bodies that allow direct gas exchange during firing, eliminating the need for containers and spacers, thereby enhancing productivity and reducing costs.

Benefits of technology

This approach enables efficient and cost-effective production of lithium-nickel composite oxide with improved productivity by shortening firing times and optimizing gas exchange, allowing for higher volumes of active material to be produced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007558633000001
    Figure 0007558633000001
  • Figure 0007558633000002
    Figure 0007558633000002
  • Figure 0007558633000003
    Figure 0007558633000003
Patent Text Reader

Abstract

To provide a molded body that can be calcined efficiently and at low cost without using a container such as a crucible or a sagger, or a member such as a spacer during calcination, thereby improving productivity.SOLUTION: Provided is one or a plurality of molded bodies obtained by molding a lithium mixture powder containing a powder of a compound containing nickel and a powder of a lithium compound, having a shape that forms a space that can come into contact with the gas supplied from the calcination furnace and discharge the gas generated by sintering of the molded bodies when the molded bodies are calcined.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a molded body, a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, and a method for producing a non-aqueous electrolyte secondary battery. [Background technology]

[0002] In recent years, with the widespread use of portable electronic devices such as mobile phones and notebook computers, there has been a strong demand for the development of small, lightweight secondary batteries with high energy density and durability, as well as high-output secondary batteries for use in power tools and electric vehicles, including hybrid cars.

[0003] As a secondary battery that meets such requirements, there are non-aqueous electrolyte secondary batteries such as lithium ion secondary batteries. Non-aqueous electrolyte secondary batteries are composed of a negative electrode, a positive electrode, an electrolyte solution, etc., and materials capable of desorbing and inserting lithium are used as the active materials of the negative electrode and the positive electrode.

[0004] Research and development of non-aqueous electrolyte secondary batteries is currently being actively conducted. In particular, non-aqueous electrolyte secondary batteries that use layered or spinel-type lithium composite oxides as the positive electrode material can achieve a high voltage of about 4 V, and are therefore being put into practical use as batteries with high energy density.

[0005] Currently, the positive electrode active materials for non-aqueous electrolyte secondary batteries include lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), which uses nickel, which is less expensive than cobalt, and lithium nickel cobalt manganese composite oxide (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), lithium manganese composite oxide (LiMn2O4), lithium nickel manganese composite oxide (LiNi 0.5 Mn 0.5 Lithium composite oxides such as CrO2 have been proposed.

[0006] Among these, lithium nickel composite oxide has attracted attention because of its high capacity and high output, and because it meets the characteristics required for the positive electrode active material of the secondary batteries of future environmentally friendly automobiles, and demand for it is rapidly expanding.

[0007] Furthermore, as the demand for eco-friendly vehicles increases, there is a demand for lower prices, which in turn increases the demand for lower costs of secondary batteries, which are one of the factors that make eco-friendly vehicles expensive.

[0008] The lithium nickel composite oxide can be obtained by mixing a nickel-containing compound with a lithium compound to prepare a lithium mixture (raw material mixture), and then calcining the lithium mixture. The lithium mixture is calcined, for example, at a temperature of about 650°C to 950°C for 3 hours or more. During this calcination process, the lithium compound reacts (sinters) with the nickel-containing compound to obtain a lithium nickel composite oxide having high crystallinity.

[0009] In general, the lithium mixture is fired in a firing furnace by putting the lithium mixture powder in a container such as a sagger. However, when the powder is fired in a container, the thermal conductivity is poor and the exchangeability between the generated gas and the reaction gas is also poor, so that in order to sufficiently react the lithium compound with the nickel-containing compound, a long heating and reaction time are required, and the total firing time including these may be long.

[0010] Several proposals have been made so far regarding the sintering conditions for efficiently sintering the lithium mixture powder.

[0011] For example, Patent Document 1 discloses a method for firing a mixture (powder) obtained by mixing a nickel composite compound and a lithium compound in a firing vessel, filling the resulting mixture (powder) into the firing vessel and firing the mixture as efficiently as possible by specifying a minimum holding time for which the mixture is held in a specific temperature range relative to the pile amount of the mixture (the thickness of the mixture when placed in the firing vessel) and a range of oxygen concentration, in order to sufficiently diffuse oxygen into the mixture.

[0012] Also disclosed are several methods in which a lithium mixture is granulated to obtain a granulated product or molded to obtain a compact, and then calcined to obtain a lithium nickel composite oxide.

[0013] For example, Patent Document 2 describes a method for producing a LiNiO2-based layered composite oxide, which is characterized in that at least a nickel salt and a lithium salt are mixed in a predetermined amount to prepare a raw material mixture, and the raw material mixture is fired to synthesize LiNiO2, the raw material mixture is granulated, and the resulting granulated material is fired. In addition, an example of Patent Document 2 describes that the granulated material in an alumina container is charged into a firing furnace, and then heated to 700°C while introducing an oxidizing gas, and held for 24 hours to obtain a fired composite material. Patent Document 2 describes that the above production method can produce a composite material having a desired crystal structure with good productivity, including in terms of workability.

[0014] Patent Document 3 also describes that a raw material mixture containing a lithium raw material is granulated and formed into a compact, which is then sintered at a temperature of 700°C to 1000°C for 2 to 15 hours in an oxidizing atmosphere to synthesize a lithium composite oxide. 2 It is described that the mixture was molded under a pressure of 1000 MPa to form pellets, and the pellets were fired in a pure oxygen atmosphere at 800°C for 10 hours.

[0015] In addition, in the examples of Patent Document 4, the mixed powder of the raw materials is pressed into a compact with a diameter of 50 mm and a thickness of 5 mm under a pressure of 500 kg / cm. 2It is described in Patent Document 4 that the press molding is performed at 740° C., pieces of an alumina spacer having a thickness of 1 mm are sandwiched between appropriate positions of the pressed compact, and the compact is fired at 740° C. for 10 hours, and then the compact is fired by holding it as it is for 20 hours at 820° C. According to Patent Document 4, press molding is extremely useful in that it shortens the distance of intermolecular movement and promotes crystal growth during firing.

[0016] Patent Document 5 also describes a method of forming a slurry from a raw material containing a lithium compound, spray-drying or freeze-drying the slurry, and then pressing the resulting dried product into a molded product, which is then fired. In the examples of Patent Document 5, a dry gel is compressed to 2 t / cm using a static compressor. 2 It is described that the mixture was pressed into pellets measuring φ14 and 2 mm in thickness, which were then placed in an alumina boat and fired in a tubular furnace in an oxygen atmosphere at 750° C. for 48 hours. [Prior art documents] [Patent documents]

[0017] [Patent Document 1] JP 2011-146309 A [Patent Document 2] JP 2000-072446 A [Patent Document 3] Japanese Patent Application Publication No. 11-135123 [Patent Document 4] Japanese Patent Application Publication No. 06-290780 [Patent Document 5] International Publication No. 98 / 06670 Summary of the Invention [Problem to be solved by the invention]

[0018] However, in the manufacturing method of Patent Document 1, if the amount of mixture is increased to increase productivity, the time required to heat the mixture is extended, and the replacement of the evolved gas with the reactive gas is deteriorated, so that the firing time is extended and productivity is impaired. Also, in the manufacturing methods of Patent Documents 2 to 5, the firing time is 10 hours or more, and the time required to produce the lithium nickel composite oxide is long, resulting in poor productivity.

[0019] Furthermore, when attempting to sinter a positive electrode active material, a method is widely used in which a mixed powder of raw materials, a pellet-shaped granulated product, or a molded product is placed in a container such as a crucible or a sagger and then sintered, as described in Patent Documents 1, 2, and 5. When a container such as a crucible or a sagger is used during sintering, there is a problem that the crucible or the sagger deteriorates and breaks due to repeated use because the crucible or the sagger has low thermal shock resistance. These problems have limited the reduction in the cost of manufacturing a positive electrode active material.

[0020] On the other hand, the manufacturing method described in Patent Document 4 involves pressing and molding the raw material powder (lithium mixture) into a specific shape, and therefore does not require a container such as a crucible or a sagger during firing. This solves the problem of damage to the container, but it requires 10 hours or more for firing, resulting in poor productivity.

[0021] In addition, in Patent Document 4, a spacer of 1 mm or more is sandwiched between the compacts obtained by pressing the raw material powder (lithium mixture) and sintered. However, when sintering using a spacer, a process of placing a spacer between the compacts is required. When sintering a compact in a sintering furnace, the compact is placed on a base plate called a setter. If the setter and the compact are in close contact with each other, the exchange of the reaction gas and the generated gas becomes poor, so a process of placing a spacer between the setter and the compact is also required. Furthermore, when sintering using a spacer, a process of removing the spacer after sintering is also required, which causes a problem of worsening productivity.

[0022] In view of the above problems, the present invention provides a molded body that can efficiently sinter a lithium mixture at low cost and improve productivity without using a container such as a crucible or a sagger, or a member such as a spacer during sintering. Also, the present invention provides a method for producing a large amount of a positive electrode active material for a non-aqueous electrolyte secondary battery at low cost and with high productivity using the molded body. [Means for solving the problem]

[0023] According to a first aspect of the present invention, there is provided one or more molded bodies obtained by molding a lithium mixture powder containing a powder of a compound containing nickel and a powder of a lithium compound, the molded body having a shape that can contact a gas supplied from a firing furnace when the molded body is fired and that forms a space through which a gas generated by sintering the molded body can be discharged.

[0024] The molded body may be used as a positive electrode active material for a non-aqueous electrolyte secondary battery after firing. The molded body may have one or more protrusions, and may form a space using the protrusions. A plurality of molded bodies are stacked to form a space. Among the plurality of molded bodies, another molded body that contacts the molded body having the protrusions may have a fixing part that can fix the position of the protrusions, and the protrusions and the fixing part may be combined to form a space.

[0025] The molded body may have at least one surface that is curved, and the curved shape may form a space. The molded body may have a hole that opens toward the inside, and the hole may form a space. The molded body may have a rod-like or plate-like shape, and a space may be formed by combining a plurality of the molded bodies.

[0026] According to a second aspect of the present invention, there is provided a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, comprising: molding a lithium mixture powder containing a powder of a nickel-containing compound and a powder of a lithium compound to obtain one or more molded bodies; sintering the molded body to obtain a sintered body; and crushing the sintered body to obtain a lithium nickel composite oxide powder, wherein the molded body has a shape that allows it to come into contact with a gas supplied from a firing furnace during sintering and that forms a space through which gas generated by sintering the molded body can be discharged.

[0027] According to a third aspect of the present invention, there is provided a method for producing a nonaqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a nonaqueous electrolyte solution, the method comprising producing a positive electrode using the above-mentioned positive electrode active material for nonaqueous electrolyte secondary batteries.

[0028] According to a fourth aspect of the present invention, there is provided a molded body obtained by molding a lithium mixture powder containing a powder of a compound containing nickel and a powder of a lithium compound, the molded body having one or more protrusions and being used as a positive electrode active material for a non-aqueous electrolyte secondary battery after being fired.

[0029] According to a fifth aspect of the present invention, there is provided a molded body obtained by molding a lithium mixture powder containing a powder of a compound containing nickel and a powder of a lithium compound, the molded body having pores and being used as a positive electrode active material for a non-aqueous electrolyte secondary battery after sintering. Effect of the Invention

[0030] According to the molded body of the present invention, the molded body can be efficiently fired at low cost without using containers such as crucibles and saggers, or members such as spacers during firing, and productivity can be improved. Also, according to the manufacturing method of the positive electrode active material for non-aqueous electrolyte secondary batteries of the present invention, a large amount of the positive electrode active material can be manufactured at low cost and with high productivity. Also, the time required for installing the spacer before firing and removing the spacer after firing can be saved. [Brief description of the drawings]

[0031] [Figure 1] FIG. 1(A) is a perspective view showing an example of a molded article according to this embodiment, and FIG. 1(B) is a cross-sectional view thereof. [Diagram 2] FIG. 2(A) is a perspective view showing an example of a molded body according to this embodiment, and FIG. 2(B) is a cross-sectional view thereof. [Diagram 3] FIG. 3(A) is a perspective view showing an example of a molded body according to this embodiment, and FIG. 3(B) is a cross-sectional view thereof. [Figure 4] FIG. 4(A) is a perspective view showing an example of a molded body according to this embodiment, and FIG. 4(B) is a cross-sectional view thereof. [Diagram 5] 5(A) and 5(B) are perspective views showing an example of a molded body according to this embodiment. [Figure 6] FIG. 6(A) is a perspective view showing an example of a molded body according to this embodiment, and FIG. 6(B) is a cross-sectional view thereof. [Figure 7] FIG. 7 is a diagram showing an example of a method for manufacturing a nonaqueous electrolyte secondary battery according to this embodiment. [Figure 8] 8(A) to 8(C) are diagrams showing an example of an apparatus for producing a molded body. [Figure 9] FIG. 9 is a diagram showing an example of an apparatus for firing a molded body. [Figure 10] FIG. 10 is a schematic diagram of a coin-type secondary battery used in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] The present invention will be described below with reference to the drawings. However, the present invention is not limited thereto. In addition, in the drawings, in order to explain the embodiment, some parts are enlarged or emphasized, and the scale is appropriately changed. In addition, in each of the following drawings, the directions in the drawings are described using an XYZ coordinate system. In this XYZ coordinate system, the vertical direction is the Z direction, and the horizontal directions are the X direction and the Y direction. In addition, for each of the X direction, Y direction, and Z direction, the side at the tip of the arrow is appropriately referred to as the + side (e.g., +X side), and the opposite side is appropriately referred to as the - side (e.g., -X side).

[0033] In this specification, the molded body may be singular or plural. In addition, a molded body (plural) formed by combining a plurality of single molded bodies (e.g., FIG. 1(A) etc.) is also called an assembly (e.g., FIG. 2(A) etc.) to distinguish it from a single molded body.

[0034] [Molded body] (First embodiment) FIG. 1(A) is a perspective view showing an example of a molded product of the present embodiment, and FIG. 1(B) is a cross-sectional view taken along line AA in FIG. 1(A) as viewed from the -Y side.

[0035] 1(A) and 1(B), the molded body 10 includes a protrusion 1 and a main body 2. The molded body 10 has a shape that allows contact with a gas (reactive gas) supplied from a firing furnace during firing and forms a space SP (space portion) through which gas generated by sintering the molded body 10 can be discharged.

[0036] The compact 10 is obtained by molding a lithium mixture powder containing a nickel-containing compound powder and a lithium compound powder. The compact 10 can be obtained by pressing the lithium mixture powder using, for example, a press device. The manufacturing method of the compact will be described later in detail. After firing, the compact 10 is used, for example, as a positive electrode active material for a non-aqueous electrolyte secondary battery. A lithium nickel composite oxide is formed by firing the compact 10.

[0037] 1(B), the space SP is formed between the main body 2 and the mounting part 20 on which the molded body 10 is placed, by using the protrusions 1. Since the molded body 10 has a shape that allows the space SP to be formed, when the molded body 10 is fired to form a lithium nickel composite oxide, the molded body 10 can be fired efficiently without using a spacer as in the conventional technology described in Patent Document 4, and as a result, productivity is improved.

[0038] For example, when firing the molded body 10 alone (one piece), the molded body 10 is placed on a setter (shelf). In this case, the placement part 20 in Fig. 1(B) is the setter. In this case, the molded body 10 forms a space SP between the molded body 10 and the placement part 20 (setter) by the protrusion part 1.

[0039] During firing, reactive gases and heat are directly supplied to the surface of the molded body 10 that contacts the outside (including the space SP), and gas generated by sintering the molded body 10 can be directly discharged to the outside. The molded body 10 in which the space SP is formed comes into contact with gas supplied from the firing furnace and can discharge gas generated by sintering the molded body 10, and the surface area increases, improving firing efficiency.

[0040] The density of the molded body 10 is, for example, 1.3 g / cm 3 or more, preferably 1.4 g / cm 3 More than 2.4g / cm 3 When the density is in the above range, sufficient strength can be obtained and productivity is excellent. 3 When the density is 2.4 g / cm or more, chipping at the corners and ridges of the molded body 10 can be suppressed, and the productivity is further improved. 3 When it is equal to or less than this, the crushability of the molded body 10 after firing is good, and the productivity is further improved.

[0041] The molded body 10 has one or more protrusions 1. When there is at least one protrusion 1, a space SP can be formed. When there are three or more, preferably four or more, protrusions 1, the molded body 10 can be stably placed on the placement part 20.

[0042] The distance between the main body 2 (molded body 10) and the mounting portion 20 can be adjusted as appropriate, but is, for example, 1 mm or more, and preferably 5 mm or more, on average. The distance between the main body 2 and the mounting portion 20 can be set within the above range, for example, by adjusting the height of the protrusion 1. For example, as shown in FIG. 1(A), when multiple protrusions 1 of the same shape are provided perpendicular to the surface direction of the main body 2, the height of the protrusions 1 is, for example, 1 mm or more, and preferably 5 mm or more.

[0043] In addition, the greater the distance between the main body 2 and the mounting part 20, the more efficient the movement of the reaction gas and the gas and heat generated from the molded body 10 becomes, but the amount of molded body 10 that can be fired at one time decreases. Therefore, the upper limit of the average distance between the main body 2 and the mounting part 20 is, for example, 20 mm or less, and preferably 15 mm or less.

[0044] In addition, when the molded body 10 has a plurality of protrusions 1, the protrusions 1 are preferably provided on the main body 2 so as to protrude in the same direction from the main body 2. The protrusions 1 are preferably provided so that the main body 1 is arranged in a horizontal direction when the molded body 10 is placed on the placement part 20, as shown in FIG. 1(B). In this case, the molded body 10 has three or more protrusions 1 of similar shapes provided on the main body 2 so as to protrude in the same direction, improving stability when placed. In this embodiment, four protrusions 1 of similar shapes are provided at the four corners of the main body 2 so as to protrude in the same direction toward the -Z direction.

[0045] As shown in Fig. 1(A), the main body 2 has, for example, a plate-like shape. In Fig. 1(A), the cross-sectional shape of the main body 2 in the XY plane is a rectangle, but it does not have to be a rectangle. The cross-sectional shape of the main body 2 in the XY plane is not particularly limited, and may be, for example, a polygon having three or more sides, or may be a circle or an ellipse. When the cross-sectional shape of the main body 2 in the XY plane is a rectangle, it is easy to efficiently arrange it in a firing furnace.

[0046] The thickness of the main body 2 (e.g., height in the Z direction) is, for example, 5 mm or more and 200 mm or less, and preferably 10 mm or more and 100 mm or less. When the thickness of the main body 2 is in the above range, the amount of the lithium mixture to be fired per one molded body 10 can be made sufficient, resulting in excellent productivity.

[0047] The maximum distance L between any two points in the plane (e.g., XY plane) of the main body 2 is, for example, 50 mm or more, and preferably 100 mm or more and 300 mm or less. When the maximum value L is in the above range, the amount of the lithium mixture to be fired per one molded body 10 can be made sufficient, resulting in excellent productivity.

[0048] The ratio (L / t) of the maximum distance L between any two points within the plane of the main body 2 to the thickness t of the main body 2 is, for example, 0.3 to 30.0, and preferably 0.5 to 10.0.

[0049] The shape of the main body 2 is arbitrary and may be a shape other than a plate shape. The main body 2 may be, for example, a rectangular parallelepiped (including a cube) or a truncated quadrangular pyramid.

[0050] When the main body 2 is a rectangular parallelepiped or a truncated pyramid, the dimensions of the rectangular parallelepiped or truncated pyramid are preferably 50 mm to 300 mm in height, 50 mm to 300 mm in width, and 50 mm to 500 mm in depth, more preferably 200 mm in height, 200 mm in width, and 300 mm in depth. If the height, width, and depth of the main body 2 are less than 50 mm, the labor required for stacking or arranging the molded bodies may increase, which may result in poor productivity. If the height, width, and depth of the main body 2 are more than 300 mm, the weight of the molded body 10 may increase, which may result in poor handling and poor productivity.

[0051] During firing, the molded body 10 may be placed on a setter or on another molded body. When the molded body 10 is placed on another molded body, a space SP is formed between the main body 2 and the other molded body, for example, by using the protrusion 1 (see FIG. 2(B)). The other molded body may or may not have a shape that forms the space SP. When multiple molded bodies are combined to form an assembly 30 (see FIG. 2(A)) and fired, one or more molded bodies 10 having a shape that forms the space SP may be used.

[0052] Second embodiment A second embodiment will be described below. In this embodiment, the same components as those in the above-described embodiment are denoted by the same reference numerals, and the description thereof will be omitted or simplified.

[0053] A plurality of the molded bodies 10 of the first embodiment can be combined to form an assembly 30. Fig. 2(A) is a perspective view showing an example of the assembly 30 of this embodiment, and Fig. 2(B) is a cross-sectional view taken along line BB in Fig. 2(A) as viewed from the -Y side. Fig. 2(B) shows an example of the assembly 30 placed in a firing furnace.

[0054] 2(A) and 2(B), the assembly 30 is formed by combining a plurality of the molded bodies 10. The assembly 30 has a shape that allows contact with the gas supplied from the firing furnace during firing and forms a space SP through which the gas generated by sintering the molded bodies 10 can be discharged.

[0055] In the case of the assembly 30 in Fig. 2(A), each molded body 10 is placed on a mounting portion 20 or on another molded body 10. In the assembly 30, a space SP is formed between the molded body 10 and the mounting portion 20 or between the molded bodies 10 by the protrusions 1 of each molded body 10, as shown in Fig. 2(B), for example. Each molded body 10 forms a space SP by using its protrusions 1.

[0056] In this way, because the assembly 30 has a shape that can form a space SP, the molded body can be fired efficiently without using a spacer as in the conventional technology described in Patent Document 4, thereby improving productivity.

[0057] In the assembly 30, the distance between each of the main body parts 2 (molded bodies 10) can be appropriately adjusted in the same manner as the above-mentioned distance between the main body part 2 (molded body 10) and the mounting part 20, and is, for example, 1 mm or more, and preferably 5 mm or more, on average, between each of the main body parts 2. The distance between each of the molded bodies 10 can be set within the above range, for example, by setting the height of the protrusion part 1 to a corresponding height.

[0058] In addition, the greater the distance between the main bodies 2, the more efficient the transfer of the reaction gas and the gas generated from the molded body 10 and the heat becomes, but the amount of the molded body 10 that can be fired at one time decreases. Therefore, the upper limit of the distance between the main bodies 2 is, for example, 20 mm or less, and preferably 15 mm or less.

[0059] The multiple molded bodies 10 constituting the assembly 30 may have the same shape or may be different from each other. Any of the above-mentioned molded bodies 10 may be used as the multiple molded bodies 10 constituting the assembly 30. When the multiple molded bodies 10 constituting the assembly 30 have the same shape, they can be manufactured efficiently, resulting in improved productivity.

[0060] Third embodiment A third embodiment will be described below. In this embodiment, the same components as those in the above-described embodiments are given the same reference numerals, and the description thereof will be omitted or simplified.

[0061] FIG. 3(A) is an oblique view showing another example of the molded body 10 and assembly 30 of this embodiment, and FIG. 3(B) is a cross-sectional view taken along line CC shown in FIG. 3(A) as viewed from the -Y side.

[0062] 3(A) is different from the molded body 10 of the second embodiment in that it is provided with a fixing portion 3 that supports the protrusions 1 of the molded bodies 10 other than itself. The assembly 30 of this embodiment is formed by stacking a plurality of molded bodies 10, and among the plurality of molded bodies 10, the molded body 10 that comes into contact with the molded body 10 having the protrusions 1 has a fixing portion 3 that can fix the position of the protrusions 1, and the protrusions 1 and the fixing portions 3 are combined to form a space SP.

[0063] When firing is performed using a firing furnace in which the assembly 30 moves within the firing furnace, there is a risk that the stacked molded bodies 10 may collapse within the firing furnace due to vibrations caused when the assembly 30 is moved. In this embodiment, each molded body 10 is provided with a fixing part 3, so that the molded bodies 10 can be prevented from collapsing within the firing furnace.

[0064] The fixing part 3 supports the protrusion 1 of the molded body 10 other than itself when the molded body 10 other than itself is combined with the fixing part 3. The fixing part 3 is configured according to the position, shape, etc. of the protrusion 1 of the molded body 10 other than itself. In this embodiment, the four fixing parts 3 are provided in a concave shape on the upper surface of the main body 2 so that when the molded body 10 other than itself is combined with the fixing part 3, each of the four protrusions 1 of the molded body 10 other than itself fits into the fixing part 3 to fix (hold) the position of the molded body 10 other than itself. Each fixing part 3 in FIG. 3(A) fixes the horizontal position (XY direction) of the protrusion 1 when the molded body 10 other than itself is combined with the fixing part 3, and fixes the horizontal position (XY direction) of the molded body 10 other than itself. In addition, each fixing part 3 in FIG. 3(A) detachably supports the protrusion 1 of the molded body 10 other than itself, and for example, after the protrusion 1 is supported by the fixing part 3, the supported protrusion 1 can be removed from the fixing part 3 to easily separate the molded body 10 other than itself from the fixing part 3. The fixing portion 3 may have a shape other than a concave shape, and may be a protrusion formed so as to fix the position of the protruding portion 1.

[0065] The assembly 30 in Fig. 3(A) is configured by combining a plurality of molded bodies 10 each having the fixing portion 3 described above. When each molded body 10 is combined with another molded body 10, the support portion 1 of the other molded body 10 is fixed to the fixing portion 3 of the other molded body 10, so that the other molded body 10 can be combined with the other molded body 10 simply and reliably. This provides the assembly 30 with a stable structure. The assembly 30 can also be formed from the molded bodies 10 simply and reliably.

[0066] (Fourth embodiment) A fourth embodiment will be described below. In this embodiment, the same components as those in the above-described embodiments are given the same reference numerals, and the description thereof will be omitted or simplified.

[0067] FIG. 4(A) is a perspective view showing another example of the molded body 10 and assembly 30 of this embodiment, and FIG. 4(B) is a cross-sectional view taken along line DD shown in FIG. 4(A) as viewed from the -Y side.

[0068] The molded body 10 in Fig. 4(A) is different from the molded body 10 in the first embodiment in that it does not include a protrusion 1 and at least one surface of the main body 2 has a curved shape. The molded body 10 or assembly 30 in Fig. 4 is also different from the molded body 10 in the first embodiment or the assembly 30 in the second embodiment in that a space SP is formed between the main body 2 and the mounting part 20 on which the molded body 10 is mounted, or between the molded bodies 10, by one surface (e.g., the -Z side) of the main body 2 being curved, as shown in Fig. 4(B), for example.

[0069] In the assembly 30 of this embodiment, the distance between each of the molded bodies 10 can be appropriately adjusted, and the average height (e.g., Z direction) of the space SP formed between each of the molded bodies 10 is, for example, 1 mm or more, and preferably 5 mm or more. The average height of the space SP can be set to the above range, for example, by adjusting the shape of the curved surface.

[0070] In addition, the larger the average height of the space SP formed between each of the molded bodies 10, the more efficient the movement of the reaction gas and the gas and heat generated from the molded body 10 becomes, but the amount of the molded body 10 that can be fired at one time decreases. Therefore, the upper limit of the average height of the space SP is, for example, 20 mm or less, and preferably 15 mm or less.

[0071] Fifth embodiment A fifth embodiment will be described below. In this embodiment, the same components as those in the above-mentioned embodiments are given the same reference numerals, and the description thereof will be omitted or simplified.

[0072] 5(A) and 5(B) are perspective views showing other examples of the assembly 30. The molded bodies 10 in FIG. 5(A) and FIG. 5(B) have a rod-like or plate-like shape, and are different from the assembly 30 of the second embodiment in that a space SP is formed by combining a plurality of the rod-like or plate-like molded bodies 10. The molded bodies 10 constituting the assembly 30 may have at least one of a rod-like and a plate-like shape, and the assembly 30 may be formed by combining both the rod-like molded body 10 and the plate-like molded body 10. The shape and size of the rod-like or plate-like molded body 10 may be within the same range as the main body 2 described above.

[0073] In the assembly 30 of this embodiment, the distance between each of the molded bodies 10 can be appropriately adjusted, and is, for example, 1 mm or more, preferably 5 mm or more, as the average distance between adjacent molded bodies 10 that are spaced apart but not in contact with each other. The distance between each of the molded bodies 10 can be set within the above range, for example, by adjusting the arrangement of the rod- or plate-shaped molded bodies 10.

[0074] In addition, the larger the average distance between each of the molded bodies 10, the more efficient the transfer of the reaction gas and the gas generated from the molded body 10 and the heat becomes possible, but the amount of the molded body 10 that can be fired at one time decreases. Therefore, the upper limit of the average distance between each of the molded bodies 10 is, for example, 20 mm or less, and preferably 15 mm or less.

[0075] Sixth embodiment A sixth embodiment will be described below. In this embodiment, the same components as those in the above-mentioned embodiments are given the same reference numerals, and the description thereof will be omitted or simplified.

[0076] Figures 6(A) and 6(B) are diagrams showing another example of a molded body. Figure 6(A) is a perspective view. Figure 6(B) is a diagram showing a cross section taken along line EE shown in Figure 6(A) as viewed from the -Y direction.

[0077] The molded body 10 in FIG. 6(A) has a hole 4 that opens toward the inside of the molded body 10, and differs from the molded body 10 in the first embodiment in that the hole 4 forms a space SP. The hole 4 may be a through hole 4a or a non-through hole 4b as shown in FIGS. 6(A) and 6(B). The diameter of the rear portion 4 may be, for example, 5 mm or more. Furthermore, the shape of the hole 4 in FIG. 6(A) is cylindrical, but it may be another shape, for example, a slit shape.

[0078] The molded body 10 having the holes 4 may be fired alone, or a plurality of molded bodies may be stacked to form an assembly 30, which may then be fired.

[0079] [Method of manufacturing positive electrode active material for non-aqueous electrolyte secondary battery] 7 is a diagram showing an example of a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to this embodiment (hereinafter also referred to as a "method for producing a positive electrode active material"). In the method for producing a positive electrode active material according to this embodiment, the above-mentioned molded body 10 is used, so that the lithium mixture can be efficiently fired and the productivity can be improved.

[0080] 7, the method for producing the positive electrode active material includes the steps of mixing a powder of a compound containing nickel with a powder of a lithium compound to obtain a lithium mixture powder (step S10), molding the lithium mixture powder to obtain one or more molded bodies 10 (step S20), sintering the molded bodies 10 to obtain a sintered body (step S30), and crushing the sintered body to obtain a lithium nickel composite oxide powder (step S40). Each step will be described below.

[0081] (Mixing process: step S10) First, a lithium mixture containing a nickel-containing compound and a lithium compound is obtained (step S10). Note that the lithium mixture may contain a binder that binds particles together in order to form a compact having sufficient strength, as described later.

[0082] (Nickel-containing compounds) The nickel-containing compound used in the present embodiment is not particularly limited, and any known compound can be used. For example, at least one of nickel-containing hydroxide and nickel-containing oxide can be used as the nickel-containing compound.

[0083] (Nickel hydroxide) The nickel-containing hydroxide includes nickel hydroxide and hydroxides containing nickel and a metal other than nickel (nickel composite hydroxide). The nickel composite hydroxide may contain at least one of cobalt, aluminum, and manganese in addition to nickel. As the nickel composite hydroxide, for example, nickel-cobalt composite hydroxide, nickel-cobalt aluminum composite hydroxide, nickel-cobalt manganese composite hydroxide, etc. are used. In addition, the nickel composite hydroxide may contain elements such as molybdenum, tungsten, silicon, boron, niobium, vanadium, and titanium.

[0084] The method for producing the nickel-containing hydroxide is not particularly limited, but for example, a crystallization method can be used. The nickel-containing hydroxide obtained by the crystallization method has a uniform composition throughout the particles, and the composition of the finally obtained positive electrode active material is also uniform.

[0085] Hereinafter, a method for producing a nickel-cobalt composite hydroxide will be described as an example of a method for producing a hydroxide containing nickel. The nickel-cobalt composite hydroxide can be produced, for example, by neutralizing an aqueous solution containing nickel (Ni), cobalt (Co), and any metal M with an alkaline aqueous solution in the presence of a complexing agent such as an ammonium ion donor while stirring, and then carrying out a crystallization reaction. The nickel-cobalt composite hydroxide obtained by the crystallization method is composed of secondary particles formed by agglomeration of a plurality of primary particles, and the positive electrode active material obtained by using the particles of this nickel-cobalt composite hydroxide as a precursor is also composed of secondary particles formed by agglomeration of a plurality of primary particles.

[0086] As the metal salt used in preparing the aqueous solution containing nickel (Ni), cobalt (Co), or any metal M, for example, sulfates, nitrates, chlorides, etc. can be used.

[0087] When the nickel composite hydroxide is a nickel-cobalt-aluminum composite hydroxide, for example, it can be produced by carrying out a crystallization reaction in which an aqueous solution containing nickel (Ni), cobalt (Co), and aluminum (Al) is neutralized with an aqueous alkali solution in the presence of a complexing agent such as an ammonium ion donor while being stirred.

[0088] Furthermore, when the nickel composite hydroxide contains a metal M, for example, it may be crystallized together with Ni and Co in a crystallization reaction and uniformly dispersed in the nickel composite hydroxide, or after the nickel composite hydroxide is formed by crystallization, it may be coated on the surfaces of the obtained nickel composite oxide particles, or it may be added and mixed simultaneously with the addition of the lithium compound.

[0089] The nickel composite hydroxide preferably contains, for example, nickel (Ni), cobalt (Co), and optionally other metals (M), and from the viewpoint of obtaining a high battery capacity, the molar ratio of each element is more preferably expressed as Ni:Co:M=(1-xy):x:y (0.03≦x≦0.10, 0.03≦y≦0.10), and it is even more preferable that M contains aluminum (Al). The ratio of each element contained in the nickel composite hydroxide is inherited by the molded body 10 and the lithium nickel composite oxide. Therefore, the composition of the entire nickel composite hydroxide can be made similar to the composition of metals other than lithium in the lithium nickel composite oxide to be obtained.

[0090] (Oxides containing nickel) The oxide containing nickel includes nickel oxide and an oxide containing nickel and a metal other than nickel (nickel composite oxide). The nickel composite oxide may contain at least one of cobalt, aluminum, and manganese in addition to nickel. For example, nickel-cobalt composite oxide, nickel-cobalt aluminum composite oxide, nickel-cobalt manganese composite oxide, etc. are used as the nickel composite oxide. In addition, the nickel composite oxide may contain elements such as molybdenum, tungsten, silicon, boron, niobium, vanadium, and titanium.

[0091] The nickel-containing oxide can be obtained, for example, by oxidizing the nickel-containing hydroxide described above. By converting the nickel-containing hydroxide into an oxide, the amount of water vapor generated during firing of the compact made of the lithium mixture is reduced, the sintering reaction is further promoted, and the firing time can be significantly shortened.

[0092] The oxidation of nickel-containing hydroxide can be carried out, for example, by oxidizing roasting (heat treatment). The temperature of the oxidizing roasting is preferably, for example, 600°C or more and 800°C or less. If the temperature of the oxidizing roasting is less than 600°C, moisture may remain in the nickel-containing oxide, and the oxidation may not proceed sufficiently. On the other hand, if the temperature of the oxidizing roasting is more than 800°C, the nickel-containing oxide may bond to each other to form coarse particles, and a large amount of energy is used, which is not industrially appropriate from the viewpoint of cost.

[0093] The time for the oxidizing roasting is preferably, for example, 0.5 to 3.0 hours. If the time for the oxidizing roasting is less than 0.5 hours, the oxidation of the nickel-containing hydroxide may not proceed sufficiently. On the other hand, if the time for the oxidizing roasting is more than 3.0 hours, the energy cost becomes high, which is not industrially appropriate.

[0094] (Lithium compounds) The lithium compound refers to a compound containing lithium. The lithium compound is not particularly limited, and any known lithium compound can be used, such as lithium hydroxide, lithium nitrate, lithium carbonate, lithium acetate, or a mixture thereof. Among these, lithium hydroxide and lithium carbonate are preferably used.

[0095] When lithium hydroxide is used as the lithium compound, a molded body having sufficient strength can be obtained without using a binder, as described later, and therefore the inclusion of impurities in the positive electrode active material can be suppressed. In addition, because lithium hydroxide is highly reactive, the molded body using this can be fired in a shorter time.

[0096] The lithium hydroxide may be a lithium hydroxide hydrate such as lithium hydroxide monohydrate (LiOH·H2O) or anhydrous lithium hydroxide (LiOH). Anhydrous lithium hydroxide can be obtained by heat treating lithium hydroxide hydrate. When anhydrous lithium hydroxide is used, the generation of moisture during the firing step can be further suppressed, the synthesis reaction of the lithium nickel composite oxide can be further promoted, and the firing time can be shortened.

[0097] (Lithium mixture) The nickel-containing compound and the lithium compound are mixed so that the ratio (Li / Me ratio) of the total number of atoms (Me) of metal elements (including nickel) in the nickel-containing compound to the number of lithium atoms (Li) in the lithium compound is, for example, in the range of 0.95 to 1.10, preferably 1.00 to 1.05, more preferably more than 1.01 to 1.03. If the Li / Me ratio is 1 or less, some of the nickel composite oxide may remain unreacted and sufficient battery performance may not be obtained. In addition, if the Li / Me ratio is more than 1.05, sintering may be promoted, the fired product may become hard and difficult to crush, or the particle size or crystallite size of the positive electrode active material may become large, and sufficient battery performance may not be obtained.

[0098] The Li / Me ratio remains almost unchanged before and after the firing step (step S30) described later, so the Li / Me ratio in the lithium mixture is almost maintained in the lithium nickel composite oxide. Therefore, the nickel-containing compound and the lithium compound can be mixed so that the Li / Me ratio becomes the same as the Li / Me ratio in the lithium nickel composite oxide to be obtained. The Li / Me ratio can be appropriately selected as appropriate depending on the battery characteristics required for the secondary battery, the configuration of the secondary battery, and the like.

[0099] A general mixer can be used for mixing, such as a shaker mixer, a Loedige mixer, a Julia mixer, or a V blender. This mixing should be sufficient so long as the nickel-containing compound is not destroyed. If the mixing is insufficient, the Li / Me ratio will vary between individual particles, which may result in problems such as insufficient battery characteristics.

[0100] (binder) The lithium mixture may contain a binder. When the lithium mixture contains a binder, the moldability of the lithium mixture is improved, and molded bodies of various shapes can be easily formed. When lithium carbonate is used as the lithium compound, a molded body having sufficient strength can be easily obtained by containing a binder. As the binder, a known binder can be used, for example, polyvinyl alcohol, polyacrylamide, carboxymethyl cellulose, etc. can be used. Among these, it is preferable to use polyvinyl alcohol.

[0101] The content of the binder in the lithium mixture can be, for example, 0.05% by mass or more and 0.2% by mass or less, preferably 0.08% by mass or more and 0.12% by mass or less, based on the total amount of the lithium mixture. When the content of the binder is within the above range, a molded body having an appropriate strength can be produced. When the content of the binder is too high, the adhesive strength of each particle constituting the molded body becomes too strong, and the efficiency of discharging the generated gas generated by the reaction between lithium and nickel composite oxide decreases, or the amount of carbon dioxide gas generated by the decomposition of the binder increases, and the generated gas cannot be discharged inside the molded body, so that the internal pressure of the molded body increases, and the molded body may be crushed.

[0102] The lithium mixture may not contain a binder. When lithium hydroxide is used as the lithium compound, a molded body can be formed only from the nickel composite oxide and lithium hydroxide without using a binder. When no binder is used, the content of impurities (e.g., carbon, etc.) in the obtained lithium nickel composite oxide can be reduced.

[0103] (Pre-firing) Furthermore, the lithium mixture powder may be calcined in an oxidizing atmosphere prior to calcination (step S30) at a temperature of 350° C. to 800° C., which is lower than the calcination temperature described below. Calcination is preferably carried out at a temperature of, for example, 350° C. to 800° C., preferably 450° C. to 780° C., for about 1 hour to 10 hours, preferably 2 hours to 6 hours. When calcination is performed prior to calcination, lithium is sufficiently diffused, and a more uniform lithium nickel composite oxide can be obtained.

[0104] (Molding: Step S20) Next, the lithium mixture powder is molded to obtain the molded body 10 (step S20). The molded body 10 used in this embodiment has a shape that forms a space SP that can contact the gas supplied from a firing furnace during firing and can discharge the gas generated by sintering the molded body 10. The shape of the molded body 10 is as described above. By firing the molded body 10 with the space SP formed therein, a lithium nickel composite oxide can be obtained with high productivity by firing for a short period of time.

[0105] The apparatus for producing the compact is not particularly limited, and may be any apparatus capable of compressing the lithium mixture powder, such as a press apparatus, etc. For example, when producing a plate-shaped compact 10 having long and short sides of 10 mm to 100 mm and a thickness of 5 mm to 200 mm, it is preferable to use a hydraulic press machine.

[0106] 8(A) to 8(C) are diagrams showing an example of a press device for manufacturing a compact 10 using the floating die method. This press device includes at least a die 50, an upper punch 70, and a lower punch 60. For example, after supplying a lithium mixture powder 40 to the die 50 (see FIG. 8(A)), the upper punch 70 is lowered to pressurize the lithium mixture powder 40 and form a compact 10 (see FIGS. 8(B) and (C)). Thereafter, the die 50 is lowered together with the lowering of the upper punch 70 to punch out the compact 10 (see FIG. 8(C)). This makes it possible to easily and efficiently manufacture a compact 10 of a predetermined shape having a predetermined density with high uniformity.

[0107] (Baking: Step S30) Next, the obtained molded body 10 is fired to obtain a sintered body of the lithium nickel composite oxide (step S30). By firing the molded body 10, the nickel composite oxide reacts with the lithium compound to produce a sintered body of the lithium nickel composite oxide.

[0108] For example, the calcination is preferably performed in an oxygen atmosphere at 650°C or more and 850°C or less. If the calcination temperature is less than 650°C, lithium diffusion may not be sufficient, unreacted lithium compound particles may remain, or the crystal structure of the lithium nickel composite oxide may not be fully aligned, so that a secondary battery using the obtained positive electrode active material may not have sufficient battery characteristics. On the other hand, if the calcination temperature is more than 850°C, intense sintering may occur between the particles of the lithium nickel composite oxide, and abnormal grain growth may occur, resulting in a decrease in the specific surface area. The decrease in the specific surface area of ​​the positive electrode active material may increase the resistance of the positive electrode and decrease the battery capacity.

[0109] The firing temperature can be adjusted as appropriate depending on the composition of the molded body. For example, the firing temperature is preferably gradually increased from room temperature and maintained at a temperature range of 650° C. to 850° C. for 3 hours or less.

[0110] When firing is performed at a temperature range of 650° C. to 850° C., the firing time is, for example, 3 hours or less, and preferably 2 hours or more and less than 2.5 hours. The temperature rise rate of the molded body is, for example, 4° C. / min or more, preferably 6° C. / min or more, and more preferably 8° C. / min or more.

[0111] In the method for producing a positive electrode active material of the present embodiment, by firing the above-mentioned molded body 10, a lithium nickel composite oxide having high crystallinity equivalent to or higher than that of the conventional method can be obtained in 60 to 80% of the firing time required in the conventional method.

[0112] The atmosphere during firing is an oxidizing atmosphere, for example, an atmosphere with an oxygen concentration of 80 to 100% by volume, and firing is preferably performed in an oxygen stream. If the oxygen concentration is less than 80% by volume, the amount of oxygen required for the reaction between the nickel composite oxide and the lithium compound cannot be supplied, and the lithium nickel composite oxide may not be sufficiently formed.

[0113] The firing furnace is not particularly limited, and may be any furnace capable of heating in an oxygen stream, such as a vertical furnace, a rotary hearth furnace, or a roller hearth kiln. Among these, it is preferable to use a roller hearth kiln from the viewpoint of capital investment and running costs. In the firing furnace, the compact 10 is arranged so as to have a shape that forms a space SP that can contact the gas supplied from the firing furnace and can discharge the gas generated by sintering the compact 10.

[0114] Fig. 9 is a diagram showing an example of the inside of a firing furnace when a roller hearth kiln is used. As shown in Fig. 9, in the firing furnace 100, for example, while the assembly 30 placed on the placement section 20 (setter) is transported by a roll R (roller), heat is supplied by a battery heater h (heater) and the firing process proceeds. In addition, the reactive gas and heat from the firing furnace are supplied to the space SP formed in the assembly 30. This allows the solid-gas reaction by the reactive gas to be carried out more efficiently through the space SP, and efficient firing can be achieved.

[0115] Conventionally, when sintering a lithium mixture powder or granulated material, the powder or granulated material is placed in a container such as a sagger and sintered. However, in the manufacturing method of this embodiment, it is preferable not to use a container such as a sagger from the viewpoint of increasing the contact area between the molded body and the atmospheric gas to promote the sintering reaction, and from the viewpoint of the amount of raw material to be put in.

[0116] (Crushing process: step S40) Next, the fired lithium nickel composite oxide obtained by the firing step is crushed to obtain a lithium nickel composite oxide powder (Step S40). By crushing, the average particle size and particle size distribution of the resulting positive electrode active material can be adjusted to a suitable range.

[0117] As a method of crushing, known means can be used, for example, a pin mill, a hammer mill, a crusher with a classification function, etc. In this case, it is preferable to adjust the crushing force within an appropriate range so as not to destroy the secondary particles.

[0118] (Water washing filtration) The powder of lithium nickel composite oxide obtained after calcination may be washed with water. When the lithium nickel composite oxide is washed with water, excess lithium on the surface of the lithium nickel composite oxide particles is removed, and a positive electrode active material for a non-aqueous electrolyte secondary battery having a higher capacity and higher thermal stability can be obtained. Here, a known technique is used as the washing method.

[0119] For example, the slurry concentration during washing is preferably 0.5 to 2 parts by mass of lithium nickel composite oxide per 1 part by mass of water, and the mixture is stirred until the excess lithium on the surface of the lithium nickel composite oxide particles is sufficiently removed, followed by solid-liquid separation and drying. If the slurry concentration exceeds 2 by mass, the viscosity is very high, making stirring difficult, and the alkali in the liquid is high, so that the dissolution rate of the deposits slows down due to the equilibrium relationship, and even if peeling occurs, separation from the powder may be difficult. On the other hand, if the slurry concentration is less than 0.5 by mass, the slurry is too dilute, so the amount of lithium elution is large, and lithium is also released from the crystal lattice of the positive electrode active material, making the crystals more likely to collapse, and the high pH aqueous solution absorbs carbon dioxide gas in the air to re-precipitate lithium carbonate.

[0120] The water used for the washing is not particularly limited, but is preferably water having an electrical conductivity of less than 10 μS / cm, more preferably 1 μS / cm or less. In other words, by using water having an electrical conductivity of less than 10 μS / cm, it is possible to prevent a decrease in battery performance due to the adhesion of impurities to the positive electrode active material.

[0121] It is preferable that the amount of adhering water remaining on the particle surface during solid-liquid separation of the above slurry is small. If there is a lot of adhering water, lithium dissolved in the liquid is reprecipitated, and the amount of lithium present on the surface of the lithium nickel composite oxide powder after drying increases. For solid-liquid separation, a commonly used centrifuge, filter press, etc. are used.

[0122] (drying process) The lithium nickel composite oxide after washing may be dried. The drying temperature is not particularly limited, but is preferably 80°C or more and 550°C or less, more preferably 120°C or more and 350°C or less. When the drying temperature is 80°C or more, the positive electrode active material after washing can be quickly dried, and the lithium concentration gradient between the particle surface and the inside of the particle can be prevented. On the other hand, since it is expected that the positive electrode active material is in a state close to the stoichiometric ratio or in a state close to the charged state with some lithium removed near the surface, if the drying temperature exceeds 550°C, the crystal structure of the powder close to the charged state may collapse, which may lead to a deterioration in electrical characteristics. Furthermore, in consideration of productivity and thermal energy costs, the drying temperature is more preferably 120°C or more and 350°C or less. At this time, as a drying method, it is preferable to dry the filtered powder at a predetermined temperature using a dryer that can control the powder to be in a gas atmosphere not containing compound components containing carbon and sulfur, or in a vacuum atmosphere.

[0123] 2.Non-aqueous electrolyte secondary battery The non-aqueous electrolyte secondary battery (hereinafter also referred to as "secondary battery") according to this embodiment includes a positive electrode, a negative electrode, and a non-aqueous electrolyte solution. The secondary battery may be composed of the same components as a general non-aqueous electrolyte secondary battery. Each component of the secondary battery according to this embodiment will be described below.

[0124] The embodiments described below are merely illustrative, and the nonaqueous electrolyte secondary battery of the present invention can be embodied in various forms that are modified and improved based on the embodiments described in this specification and the knowledge of those skilled in the art. In addition, the nonaqueous electrolyte secondary battery of the present invention is not particularly limited in its application.

[0125] (positive electrode) The positive electrode contains the positive electrode active material according to the present embodiment. The positive electrode can be produced, for example, as follows.

[0126] First, the above-mentioned positive electrode active material, conductive material, and binder are mixed, and activated carbon and a solvent for the purpose of viscosity adjustment, etc. are added as necessary, and the mixture is kneaded to prepare a positive electrode mixture paste.

[0127] The mixing ratio of each material in the positive electrode composite paste is not particularly limited and can be adjusted appropriately according to the required performance of the secondary battery. The mixing ratio of the materials can be in the same range as that of the positive electrode of a known non-aqueous electrolyte secondary battery, and for example, when the total mass of the solid content of the positive electrode composite excluding the solvent is 100 parts by mass, the content of the positive electrode active material can be 60 parts by mass or more and 95 parts by mass or less, the content of the conductive material can be 1 part by mass or more and 20 parts by mass or less, and the content of the binder can be 1 part by mass or more and 20 parts by mass or less.

[0128] The obtained positive electrode composite paste is applied to the surface of an aluminum foil current collector, for example, and dried to evaporate the solvent, thereby producing a sheet-shaped positive electrode. If necessary, pressure may be applied by a roll press or the like to increase the electrode density.

[0129] The sheet-like positive electrode thus produced can be cut to an appropriate size according to the intended battery and used to produce the battery. However, the method for producing the positive electrode is not limited to the above-mentioned example, and other methods may be used.

[0130] As the conductive agent, for example, graphite (natural graphite, artificial graphite, expanded graphite, etc.), acetylene black, Ketjen black, and other carbon black-based materials can be used.

[0131] The binder serves to bind the active material particles together, and examples of the binder that can be used include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene propylene diene rubber, styrene butadiene, cellulose-based resin, and polyacrylic acid.

[0132] If necessary, a solvent for dispersing the positive electrode active material, conductive material, and activated carbon and dissolving the binder may be added to the positive electrode mixture. Specifically, an organic solvent such as N-methyl-2-pyrrolidone may be used as the solvent. Activated carbon may be added to the positive electrode mixture to increase the electric double layer capacity.

[0133] (Negative electrode) The negative electrode can be made of metallic lithium, a lithium alloy, etc. The negative electrode can be made by mixing a binder with a negative electrode active material capable of absorbing and desorbing lithium ions, adding an appropriate solvent to make a paste-like negative electrode mixture, applying the mixture to the surface of a metal foil collector such as copper, drying it, and compressing it to increase the electrode density as necessary.

[0134] As the negative electrode active material, for example, natural graphite, artificial graphite, baked organic compounds such as phenolic resin, and powdered carbon materials such as coke can be used.

[0135] As with the positive electrode, a fluorine-containing resin such as PVDF can be used as the negative electrode binder, and an organic solvent such as N-methyl-2-pyrrolidone can be used as the solvent for dispersing these active materials and binder.

[0136] (Separator) A separator is sandwiched between the positive electrode and the negative electrode. The separator separates the positive electrode and the negative electrode and retains the electrolyte. A thin membrane containing a resin such as polyethylene or polypropylene and having many minute pores can be used as the separator.

[0137] (Non-aqueous electrolyte) The non-aqueous electrolyte solution is prepared by dissolving a lithium salt as a supporting electrolyte in an organic solvent.

[0138] The organic solvent may be one selected from the group consisting of cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and trifluoropropylene carbonate; chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate, and dipropyl carbonate; ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran, and dimethoxyethane; sulfur compounds such as ethyl methyl sulfone and butane sultone; and phosphorus compounds such as triethyl phosphate and trioctyl phosphate. The organic solvent may be one selected from the group consisting of cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, and trifluoropropylene ...

[0139] As the supporting salt, LiPF6, LiBF4, LiClO4, LiAsF6, LiN(CF3SO2)2, etc., and composite salts thereof can be used.

[0140] Furthermore, the non-aqueous electrolyte may contain a radical scavenger, a surfactant, a flame retardant, etc. The non-aqueous electrolyte secondary battery may use a known solid electrolyte instead of the non-aqueous electrolyte.

[0141] (Shape and structure of non-aqueous electrolyte secondary batteries) The nonaqueous electrolyte secondary battery of the present invention, which is constituted by the positive electrode, negative electrode, separator and nonaqueous electrolyte as described above, may have various shapes such as a cylindrical type or a laminated type.

[0142] Regardless of the shape adopted, a positive electrode and a negative electrode are laminated with a separator interposed therebetween to form an electrode body, the resulting electrode body is impregnated with a nonaqueous electrolyte solution, the positive electrode current collector and a positive electrode terminal connected to the outside, and the negative electrode current collector and a negative electrode terminal connected to the outside are connected using a current collecting lead or the like, and the battery is sealed in a battery case to complete a nonaqueous electrolyte secondary battery. EXAMPLES

[0143] The positive electrode interface resistance of a non-aqueous electrolyte secondary battery having a positive electrode using the positive electrode active material obtained according to the present invention was confirmed.

[0144] The present invention will be specifically described below using examples, but the present invention is not limited to these examples. The method for evaluating the obtained positive electrode active material will be described below.

[0145] (Production and evaluation of evaluation batteries) A coin-type secondary battery CBA (see FIG. 10) for evaluation was prepared by the following method, and the positive electrode interface resistance was measured and a charge-discharge cycle test was performed.

[0146] (Preparation of coin-type secondary battery CBA) 52.5 mg of the positive electrode active material, 15 mg of acetylene black, and 7.5 mg of polytetrafluoroethylene resin (PTFE) were mixed and pressed at a pressure of 100 MPa to a diameter of 11 mm and a thickness of 100 μm to prepare a positive electrode (electrode for evaluation) PE. The prepared positive electrode PE was then dried in a vacuum dryer at 120°C for 12 hours. As shown in Figure 3, a coin-type secondary battery CBA was prepared using the dried positive electrode (electrode for evaluation) PE, negative electrode NE, separator SE, and electrolyte in a glove box in an Ar atmosphere with a dew point controlled at -80°C.

[0147] The negative electrode NE was a negative electrode sheet in which graphite powder with an average particle size of about 20 μm and polyvinylidene fluoride were applied to copper foil, which was punched into a disk shape with a diameter of 14 mm. The electrolyte was an equal mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) (manufactured by Ube Industries, Ltd.) with 1M LiPF6 as the supporting electrolyte. A polyethylene porous film with a thickness of 25 μm was used for the separator SE. The coin-type secondary battery CBA had a gasket GA and a wave washer WW, and was assembled into a coin-type battery with a positive electrode can PC and a negative electrode can NC.

[0148] (Battery evaluation) The initial charge / discharge capacity, which indicates the performance of the produced coin-type secondary battery CBA, was evaluated as follows. (Initial discharge capacity) The initial discharge capacity was measured by leaving the coin-type secondary battery CBA for about 24 hours after production, and after the open circuit voltage OCV (Open Circuit Voltage) had stabilized, applying a current density of 0.1 mA / cm to the positive electrode. 2 The battery was charged to a cut-off voltage of 4.3 V, and after one hour of rest, the capacity at which the battery was discharged to a cut-off voltage of 3.0 V was defined as the initial discharge capacity.

[0149] [Example 1] (mixture) The raw material powders used were a nickel composite oxide powder with a composition ratio of Ni:Co:Al = 88:9:3 and a lithium hydroxide powder with a moisture content of 1.5% or less and a total carbon content of 1.0% or less. The nickel composite oxide powder and the lithium hydroxide powder were mixed so that the Li / Me ratio was 1.03 to prepare a lithium mixture powder.

[0150] (molding) 12 kg of the obtained lithium mixture powder was put into a hydraulic press to produce 10 compacts. The manufacturing conditions for the compacts are described in detail below.

[0151] Shape of the molded product The molded body was molded into a shape having a plate-like portion (main body) and four protrusions. The dimensions of the plate-like portion (main body) were 165 mm wide x 165 mm deep x 30 mm thick, and the dimensions of the protrusions were 10 mm in diameter x 5 mm high. A total of four protrusions were installed so that the centers of the protrusions were 20 mm inward from each corner of the plate-like portion in the diagonal direction.

[0152] Molding conditions 1.2 kg of lithium mixture (powder) was packed into a mold and pressed (approximately 0.4 t / cm 2 ) and cut out 10 molded bodies (density: 1.5 g / cm3) having the above shape. 3 ) was prepared.

[0153] The obtained green bodies were stacked one on top of the other in a sintering furnace, and two sets of five were arranged side by side. A small hole for measuring the temperature was opened in the center of one side of the third green body, facing the center of the green body, and a thermocouple was inserted and connected to a thermometer to measure the temperature at the center of the green body.

[0154] (Firing) The temperature inside the sintering furnace was rapidly raised in an atmosphere with an oxygen concentration of 90%, and the temperature at the center of the compact was raised from room temperature to 760° C. in 90 minutes and maintained at 760° C. for 2.5 hours. Thereafter, the compact was gradually cooled to room temperature in the sintering furnace over 6 hours and then removed from the sintering furnace.

[0155] The fired body was pulverized to an average particle size of 50 μm using a roll crusher and a pin mill to obtain a lithium nickel composite oxide powder. The obtained powder was used to prepare a coin-type secondary battery CBA, and the initial discharge capacity was measured by the above-mentioned evaluation method. The initial discharge capacity of the obtained coin-type secondary battery CBA was 233 mAh / g.

[0156] [Comparative Example 1] A sagger containing 9.5 kg of the same lithium mixture powder as in Example 1 was placed in the same firing furnace, a thermocouple was inserted into the raw powder and connected to a thermometer, and the temperature was raised in 240 minutes until the temperature inside the raw powder reached 760°C in an atmosphere with an oxygen concentration of 90%, and the temperature was kept at 760°C for 3 hours. Thereafter, the powder was cooled and pulverized in the same manner as in Example 1 to obtain a powder of lithium nickel composite oxide. A coin-type secondary battery CBA was produced using the obtained powder, and the initial discharge capacity was measured. The initial discharge capacity of the obtained coin-type secondary battery CBA was 235mAh / g. The inner dimensions of the sagger were 300mm wide x 300mm deep x 100mm high.

[0157] (evaluation) In the manufacturing method using the molded body of Example 1, the time required for firing was shorter than in the manufacturing method in which the powder was fired using the sagger of Comparative Example 1. Furthermore, in the manufacturing method using the molded body of Example 1, the amount of raw material input per unit volume in the firing furnace was increased, and productivity was greatly improved. [Industrial Applicability]

[0158] According to the manufacturing method of the positive electrode active material for non-aqueous electrolyte secondary batteries of this embodiment, the lithium mixture powder is molded into a compact with higher density, which increases the amount of raw material input per unit volume and shortens the sintering time, thereby greatly improving productivity. In addition, when stacking and sintering compacts, the compacts can be efficiently sintered without placing spacers between them, thereby shortening the time required for arranging and removing the spacers and achieving higher productivity. [Explanation of symbols]

[0159] 1...Protrusion 2…Main body 3…Fixed part 4...Hole 10...Molded body 20...Placement section 30…Aggregation SP…Space 40...Lithium mixture powder 50…Die 60…Lower punch 70…upper punch h…Heater R…Roll PE: Positive electrode (electrode for evaluation) NE: Negative electrode SE…Separator GA…Gasket WW…Wave washer PC…Positive electrode can NC: Negative electrode can CBA: Coin-type secondary battery

Claims

1. A single or multiple molded bodies obtained by molding a lithium mixture powder containing a powder of a compound containing nickel and a powder of a lithium compound, the molded body has a shape that can come into contact with a gas supplied from a firing furnace when the molded body is fired and that forms a space through which a gas generated by sintering the molded body can be discharged; The molded body includes a body portion and one or more protrusions, The molded body can be placed on a placement portion for placing the molded body or on another molded body, The space is formed using the protrusion, The formed space is a space in which, when the molded body is placed on the placement part, the average distance between the main body part and the placement part is 1 mm or more, and, when the molded body is placed on another molded body, the average distance between the respective main body parts is 1 mm or more, The density of the molded body is 1.3 g / cm 3 2.4g / cm or more 3 is as follows: The molded body is used as a powder of a positive electrode active material for a non-aqueous electrolyte secondary battery after being sintered.

2. The molded body according to claim 1 , wherein the maximum distance between any two points in a horizontal cross section of the main body when the molded body is placed is 50 mm or more and 300 mm or less.

3. A plurality of molded bodies formed by stacking the molded bodies according to claim 1 or 2, Among the multiple molded bodies, another molded body that comes into contact with the molded body having the protrusion has a fixing portion that can fix the position of the protrusion, and the protrusion and the fixing portion are combined to form the space.

4. A single or multiple molded bodies obtained by molding a lithium mixture powder containing a powder of a compound containing nickel and a powder of a lithium compound, the molded body has a shape that can come into contact with a gas supplied from a firing furnace when the molded body is fired and that forms a space through which a gas generated by sintering the molded body can be discharged; The molded body has at least one surface having a curved shape, and the curved shape forms the space, The average height of the space formed is 1 mm or more, The density of the molded body is 1.3 g / cm 3 2.4g / cm or more 3 is as follows: The molded body is used as a powder of a positive electrode active material for a non-aqueous electrolyte secondary battery after being sintered.

5. A single or multiple molded bodies obtained by molding a lithium mixture powder containing a powder of a compound containing nickel and a powder of a lithium compound, the molded body has a shape that can come into contact with a gas supplied from a firing furnace when the molded body is fired and that forms a space through which a gas generated by sintering the molded body can be discharged; The molded body has a hole portion that opens toward the inside, and the hole portion forms the space, The diameter of the hole is 5 mm or more, The density of the molded body is 1.3 g / cm 3 2.4g / cm or more 3 is as follows: The molded body is used as a powder of a positive electrode active material for a non-aqueous electrolyte secondary battery after being sintered.

6. A plurality of compacts obtained by compacting a lithium mixture powder containing a powder of a compound containing nickel and a powder of a lithium compound, the molded body has a shape that can come into contact with a gas supplied from a firing furnace when the molded body is fired and that forms a space through which a gas generated by sintering the molded body can be discharged; The molded body has at least one of a rod shape and a plate shape, and the density of the molded body is 1.3 g / cm 3 2.4g / cm or more 3 is as follows: When the molded body is rod-shaped, its length is 50 mm or more, and when the molded body is plate-shaped, the maximum value of the distance between any two points on the plate surface is 50 mm or more; The plurality of molded bodies are arranged in a horizontal direction so that the molded bodies are adjacent to each other at intervals without contacting each other, and are stacked in a vertical direction in a plurality of stages to form the space, A plurality of molded bodies in a lower tier and a plurality of molded bodies in an upper tier adjacent to the lower tier are stacked so as to intersect when viewed from above, The average distance between each of the molded bodies that are adjacent to each other but not in contact with each other in the horizontal direction is 1 mm or more; The molded body is used as a powder of a positive electrode active material for a non-aqueous electrolyte secondary battery after being sintered.

7. A method for producing a compact according to any one of claims 1 to 6, comprising molding a lithium mixture powder containing a powder of a compound containing nickel and a powder of a lithium compound; sintering the molded body to obtain a sintered body; crushing the fired body to obtain a lithium nickel composite oxide powder; Equipped with The molded body has a shape that can contact a gas supplied from a firing furnace during firing and forms a space through which a gas generated by sintering the molded body can be discharged. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery.

8. A method for manufacturing a non-aqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte solution, comprising the steps of: A method for producing a non-aqueous electrolyte secondary battery, comprising producing a positive electrode using the positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 7.

Citation Information

Patent Citations

  • Calcination of oxide superconductor of flat plate

    JP1990302358A

  • Positive electrode material for lithium secondary battery and its synthesis and evaluation, and lithium secondary battery and its manufacture

    JP1994290780A

  • Positive active material for lithium secondary battery and secondary battery using the same

    JP1999135123A

  • Production of linio2-based laminar multiple oxide

    JP2000072446A

  • Manufacture of clay tile

    JP2001009815A