Silicon-carbon negative electrode material and preparation method and application thereof

By introducing carbon nanotubes and nitrogen heterocyclic conductive polymer layers into silicon carbon anode materials, the problems of poor conductivity and strength of silicon-based anode materials are solved, significantly improving the magnification and cycling performance of lithium-ion batteries, and extending the battery's Service life.

CN118978160APending Publication Date: 2024-11-19四川长虹杰创锂电科技有限公司

Patent Information

Application Number
CN202411040637.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing silicon-based negative electrode materials have poor conductivity and poor material strength, and their performance gradually deteriorates during repeated charging and discharging.

Method used

Copolymer acrylonitrile hydrogel is used as the carbon source, and the high-strength carbon nanotubes are introduced to pre-oxidize, pre-carbonize, and activated pores to form a porous carbon framework, and silane and acetylene are deposited under an inert atmosphere, and finally coated. A nitrogen heterocyclic conductive polymer layer was used to prepare a silicon carbon negative electrode material.

Benefits of technology

It improves the conductivity and cycling performance of silicon-carbon anode materials, extends the service life of lithium-ion batteries, and improves the magnification and conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978160A_ABST
    Figure CN118978160A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion battery negative electrode materials, and particularly relates to a silicon-carbon negative electrode material and a preparation method and application thereof. In order to solve the technical problems that an existing silicon-based negative electrode is poor in conductivity, poor in material strength and gradually deteriorated in performance in the repeated charging and discharging process, the invention provides a preparation method of a silicon-carbon negative electrode material. Carrying out pre-oxidation, pre-carbonization, activated pore-forming and high-temperature purification to obtain a porous carbon skeleton; and then silane deposition is carried out, and after nano silicon is deposited, hard carbon and a nitrogen heterocyclic conductive polymer layer are sequentially coated, so that the conductivity of the silicon-carbon negative electrode material and the capacity and rate capability of the silicon-carbon negative electrode material in a lithium battery negative electrode are improved. The silicon-carbon negative electrode material prepared by the method is used for preparing a lithium ion battery, the rate, the conductivity and the cycle performance of the battery can be improved, and the service life of the battery is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of negative electrode materials for lithium-ion batteries, and in particular relates to silicon-carbon negative electrode materials and preparation methods and applications thereof. Background Art

[0002] Porous carbon is an important raw material for manufacturing new silicon-carbon negative electrode materials. Silicon materials undergo large volume changes during the lithiation / delithiation process, and the huge internal stress can easily cause the material to break and pulverize, causing the active material to fall off the electrode, lose electrical contact and become inactive, thus affecting the battery's service life due to the high expansion rate problem. Porous carbon materials not only ensure the effective penetration of the electrolyte, but also accommodate the effective expansion of silicon during the cycle process, which can extend the battery's service life, inhibit the formation and growth of lithium dendrites during charging and discharging, and improve the safety of the battery. However, the porous carbon materials prepared by existing methods have low skeleton strength, and the strength and conductivity after silicon-carbon compounding are poor, making it difficult to meet the technical requirements of supercapacitors and new silicon-carbon negative electrodes.

[0003] Therefore, in the art, it is desired to develop a silicon-carbon negative electrode material with excellent electrochemical performance, simple preparation process and low cost. Summary of the invention

[0004] The purpose of this application is to provide a silicon-carbon negative electrode material and a preparation method and application thereof, aiming to solve the technical problems of poor conductivity, poor material strength, and gradual deterioration of performance of existing silicon-based negative electrodes during repeated charging and discharging.

[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:

[0006] In a first aspect, the present invention provides a method for preparing a silicon-carbon negative electrode material, comprising the following steps:

[0007] S1, after drying the copolymerized polyacrylonitrile hydrogel, dispersing the dry gel and the carbon nanotubes with a solvent respectively and then mixing them, removing the solvent and drying to obtain a carbon nanotube-doped three-dimensional stacked porous carbon precursor;

[0008] S2, pre-oxidizing and pre-carbonizing the precursor, and then activating and purifying it to obtain a porous carbon skeleton;

[0009] S3, introducing silane into the porous carbon skeleton under an inert atmosphere for deposition, and then introducing acetylene for further deposition, thereby obtaining a porous carbon material deposited with silane;

[0010] S4. Dissolve the nitrogen heterocyclic conductive polymer monomer in an organic solvent, then mix it with the porous carbon material, and perform heat treatment under the protection of an inert atmosphere to obtain a silicon-carbon negative electrode material coated with the nitrogen heterocyclic conductive polymer.

[0011] Wherein, in step S1, the copolymerized polyacrylonitrile hydrogel is prepared by a photo-initiated one-step in-situ polymerization method.

[0012] Furthermore, the preparation method of the hydrogel comprises the following steps: in the presence of a ZnCl2 aqueous solution, acrylonitrile, a monomer copolymerizable with acrylonitrile, and a crosslinking agent are mixed evenly, a photoinitiator is added, and polymerization is carried out under ultraviolet light to obtain a copolymerized acrylonitrile hydrogel.

[0013] Preferably, the monomer copolymerized with acrylonitrile is selected from at least one of acrylamide, aniline, 2-acrylamide-2-methylpropanesulfonic acid or sulfobetaine methacrylate.

[0014] Preferably, in the hydrogel preparation method, at least one of the following is satisfied:

[0015] The mass ratio of the acrylonitrile to the monomer copolymerized with acrylonitrile is 7:3 to 5:5.

[0016] The amount of the ZnCl2 aqueous solution added is 9 to 10 times that of the monomer raw material, and the concentration of the ZnCl2 aqueous solution is 50 to 60 wt%.

[0017] The cross-linking agent is N,N'-methylenebisacrylamide, and the amount of the cross-linking agent added is 0.3-0.4wt% of the monomer raw material.

[0018] The amount of the initiator added is 1-2 wt % of the monomer raw material.

[0019] The initiation polymerization time is 3.5 to 5.0 hours.

[0020] Furthermore, the copolymerized polyacrylonitrile xerogel is obtained by immersing the prepared hydrogel in water for solvent exchange and then freeze-drying.

[0021] Wherein, in step S1, the mass ratio of dry gel to carbon nanotubes is 1:0.001-0.1.

[0022] The dry gel and the carbon nanotubes are dispersed in ethanol respectively, and the dispersion concentration is 5-50wt%.

[0023] Wherein, in step S2, at least one of the following is satisfied:

[0024] The pre-oxidation temperature is 100-400°C, and the pre-oxidation time is 3-8h.

[0025] The pre-carbonization temperature is 500-600°C, and the pre-carbonization time is 1-2h.

[0026] The activation temperature is 700-900°C, and the activation time is 1-5h.

[0027] The purification temperature is 700-900°C, and the purification time is 1-4h.

[0028] Wherein, in step S2, an alkaline substance is used to perform pre-oxidation, pre-carbonization and activation treatment on the precursor, and after activation, the precursor is washed and dried to remove residual alkali. Preferably, the alkaline substance is selected from at least one of KOH and NaOH. In the present invention, the role of the alkaline substance is to activate the precursor to form pores.

[0029] Wherein, in step S3, the volume ratio of silane to nitrogen is 1:5-10, the flow rate is 30 mL / min, and the deposition is 8 h.

[0030] Wherein, in step S3, the volume ratio of acetylene to nitrogen is 1:10, the flow rate is 100 mL / min, and the deposition time is 2 h.

[0031] Wherein, in step S4, the mass ratio of the nitrogen heterocyclic polymer monomer to the porous carbon material is 1:1-9.

[0032] Wherein, in step S4, the nitrogen heterocyclic conductive polymer is selected from at least one of polyacrylonitrile, polypyrrole, polyaniline, polycarbazole or polythiophene.

[0033] Wherein, in step S4, the organic solvent is N-methylpyrrolidone.

[0034] Wherein, in step S4, the heat treatment temperature is 500-800° C., and the heat treatment time is 6-8 hours.

[0035] In a second aspect, the present invention provides a silicon-carbon negative electrode material prepared by the above preparation method.

[0036] In a third aspect, the present invention provides application of the above silicon-carbon negative electrode material in lithium-ion batteries.

[0037] Among them, the application is to mix the silicon-carbon negative electrode material with graphite, a conductive agent, a binder and a solvent to obtain a negative electrode slurry, which is then coated on a negative electrode collector, and then dried, rolled, cut and sliced ​​to serve as the negative electrode of a lithium-ion battery.

[0038] Wherein, in the application, the preparation method of the lithium ion battery comprises the following steps:

[0039] (a) mixing the silicon-carbon negative electrode material prepared above with graphite, a conductive agent, a binder and a solvent to obtain a negative electrode slurry, and then coating it on a negative electrode current collector, drying, rolling, slitting and sheeting to obtain a negative electrode;

[0040] (b) mixing the ternary material, the conductive agent, the binder, the additive and the solvent to obtain a positive electrode slurry, which is then coated on a positive electrode current collector, and then dried, rolled, cut and sliced ​​to obtain a positive electrode;

[0041] (c) The positive electrode in step (a), the negative electrode in step (b) and the single-sided coated ceramic diaphragm are wound, shelled, injected, sealed, pre-charged, formed, aged and capacity divided to obtain a lithium ion battery.

[0042] In a fourth aspect, the present invention provides a lithium-ion battery, the negative electrode of which contains the above-mentioned silicon-carbon negative electrode material.

[0043] Beneficial effects: The present invention selects copolymerized polyacrylonitrile hydrogel as a carbon source, introduces high-strength carbon nanotubes therein, performs pre-oxidation, pre-carbonization, activation pore formation and high-temperature purification, and obtains a porous carbon skeleton; then performs silane deposition, and after depositing nano-silicon, sequentially coats hard carbon and nitrogen heterocyclic conductive polymer layers, thereby improving the conductivity of the silicon-carbon negative electrode material and the capacity and rate performance in the lithium battery negative electrode. The silicon-carbon negative electrode material prepared by the present invention is used to prepare lithium-ion batteries, which can improve the rate, conductivity and cycle performance of the battery and extend the service life of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 is a SEM image of the silicon-carbon negative electrode material prepared in Example 1;

[0045] Figure 2 The cycle retention rate diagram of the lithium ion battery prepared in Examples 1 to 3 at 4A / 30A;

[0046] Figure 3 This is a rate performance diagram of the lithium ion battery prepared in Example 1. DETAILED DESCRIPTION

[0047] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clear, the present application is further described in detail below in combination with the implementation methods. Unless otherwise defined, all scientific and technological terms used herein have the same meanings as understood by ordinary technicians in the field.

[0048] In order to solve the technical problems that the existing silicon-based negative electrode has poor conductivity, poor material strength, and gradually deteriorates in performance during repeated charging and discharging, the present invention specifically provides a method for preparing a silicon-carbon negative electrode material, comprising the following steps:

[0049] S1, after drying the copolymerized polyacrylonitrile hydrogel, dispersing the dry gel and the carbon nanotubes with a solvent respectively and then mixing them, removing the solvent and drying to obtain a carbon nanotube-doped three-dimensional stacked porous carbon precursor;

[0050] S2, pre-oxidizing and pre-carbonizing the precursor, and then activating and purifying it to obtain a porous carbon skeleton;

[0051] S3, introducing silane into the porous carbon skeleton under an inert atmosphere for deposition, and then introducing acetylene for further deposition, thereby obtaining a porous carbon material deposited with silane;

[0052] S4. Dissolve the nitrogen heterocyclic conductive polymer monomer in an organic solvent, then mix it with the porous carbon material, and perform heat treatment under the protection of an inert atmosphere to obtain a silicon-carbon negative electrode material coated with the nitrogen heterocyclic conductive polymer.

[0053] In the present invention, hydrogel is used as the carbon source for the synthesis of silicon-carbon negative electrode material because hydrogel has the advantages of easy synthesis, high conductivity, good stability, environmental non-toxicity and reversible redox characteristics. The polymer network of the hydrogel is a precursor of the carbon material. The freeze-dried hydrogel can be carbonized to form a porous carbon material. By adjusting the composition of the polymer network, the expansion degree of the hydrogel and the carbonization procedure can regulate the porous structure. Moreover, the copolymerized double network gel has better stability than the traditional single system gel, and its high specific surface area and good conductivity can provide a larger capacity and improve battery performance.

[0054] In a specific embodiment of the present invention, polyacrylonitrile hydrogel is used because polyacrylonitrile is a hard, relatively insoluble, high-melting-point polymer with a high melting point and a high carbon yield. It is an excellent precursor for producing high-performance carbon materials. The carbonized copolymer hydrogel has the advantages of large specific surface area, high porosity, low mass density, good conductivity, and high temperature resistance. Therefore, copolymer polyacrylonitrile hydrogel is selected.

[0055] In a specific embodiment of the present invention, in step S1, the amount of ethanol used when dispersing carbon nanotubes and dry gel powder will affect the dispersion effect. Too little ethanol will lead to a large adsorption force between the powders, making it difficult to fully disperse them, and then the two will be difficult to mix evenly. Through exploration, it was found that the dispersion concentration of carbon nanotubes and dry gel powder in ethanol is 5-50wt% and the dispersion effect is better. When the dispersion concentration is 20wt%, the dispersion is most uniform.

[0056] In a specific embodiment of the present invention, in step S1, the carbonized copolymerized polyacrylonitrile hydrogel is a carbon skeleton of a silicon-carbon material, and the porous structure inside reserves space for the volume expansion of silicon; and the addition of carbon nanotubes can improve the electronic conductivity and structural stability of the material. Moreover, the mass ratio of the dry gel to the carbon nanotubes should be 1:0.001-0.1. If it is higher than this range, it will increase the difficulty of dispersing the carbon nanotubes. If it is lower than this range, the carbon nanotubes will have almost no effect on improving the electronic conductivity and structural stability of the material.

[0057] In a specific embodiment of the present invention, in step S2, the pre-oxidation, pre-carbonization, activation and high-temperature purification of the present invention are mainly used to form a porous carbon matrix for depositing silicon during the production process of silicon-carbon negative electrode materials. Pre-oxidation can stabilize the polymer skeleton before carbonization; the purpose of pre-carbonization is to prevent melting during carbonization, and to allow the molecules to contain hydroxyl and carbonyl groups through oxidation reactions. In this way, hydrogen bonds can be formed between and within molecules, thereby improving the thermal stability of the fiber; activation can activate the pores of the carbon material and significantly increase the specific surface area of ​​the carbon material; high-temperature purification is to graphitize the carbon material while removing impurities. The role of alkaline substances such as KOH or NaOH is to activate the precursor to form pores.

[0058] The temperature and time of pre-oxidation, pre-carbonization, activation and high-temperature purification are controlled as follows in order to better form a stable porous carbon skeleton: the pre-oxidation temperature is 100-400°C, and the pre-oxidation time is 3-8h; the pre-carbonization temperature is 500-600°C, and the pre-carbonization time is 1-2h; the activation temperature is 700-900°C, and the activation time is 1-5h; the purification temperature is 700-900°C, and the purification time is 1-4h.

[0059] In a specific embodiment of the present invention, in step S3, nitrogen is used as a protective gas, silane gas is passed in order to deposit silane, and acetylene gas is passed in order to make a hard carbon coating. The hard carbon coating can effectively avoid direct contact between silicon and the electrolyte and maintain a stable SEI film. The amount of silane deposition will affect the silicon content of the silicon-carbon negative electrode material, the resistivity and gram capacity of the material itself, etc. A high silicon content will increase the gram capacity of the material itself but will increase the risk of excessive expansion of the material during lithium insertion and extraction, and the cycle and safety performance will deteriorate. A low silicon content will reduce the gram capacity of the material. Therefore, in the present invention, the amount of silane deposition is controlled at 1.3 to 2.4 L, that is, the volume ratio of silane to nitrogen is 1:5 to 10, the flow rate is 30 mL / min, and the deposition is 8 hours.

[0060] In a specific embodiment of the present invention, in step S4, the nitrogen heterocyclic conductive polymer is a new generation of polymer materials. Different from traditional covalent polymer materials, it has a large conjugated π electron system in its molecule and high carrier mobility, and can become a precursor of graphite negative electrode coating materials. The nitrogen heterocyclic conductive polymer coating can provide additional lithium ion adsorption active sites for carbon materials, thereby improving the capacity and rate performance of the material in the lithium battery negative electrode.

[0061] The nitrogen heterocyclic conductive polymer monomer is in solid powder form, and the solid phase coating uniformity is insufficient. Therefore, an organic solvent such as N-methylpyrrolidone is used as a solvent to dissolve it and then perform liquid phase coating to achieve a more uniform coating. The amount of N-methylpyrrolidone is determined by the solubility of the nitrogen heterocyclic conductive polymer, and it is sufficient to completely dissolve the monomer.

[0062] Specific examples will be listed below to explain the scheme of the present invention. It will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. Where specific techniques or conditions are not indicated in the examples, the techniques or conditions described in the literature in this area or the product instructions are used. Reagents or instruments used that do not indicate manufacturers are all conventional products that can be obtained commercially.

[0063] Example 1

[0064] (1) Weigh 5g ZnCl2 and add it to 4g deionized water, and stir at room temperature to obtain a ZnCl2 aqueous solution. Dissolve 0.7g acrylonitrile, 0.3g 2-acrylamide-2-methylpropanesulfonic acid and 0.004g N,N'-methylenebisacrylamide in the ZnCl2 aqueous solution, then add 0.01g photoinitiator 1173, stir for 2min, transfer the above solution to a glass mold, and polymerize it under 365nm ultraviolet light for 4h. The obtained hydrogel is soaked in deionized water for 3 days, and the water is changed every 4h to remove ZnCl2 to obtain a copolymerized polyacrylonitrile hydrogel. Freeze-dry for 2 days to obtain a xerogel. The xerogel and carbon nanotubes are dispersed in ethanol respectively, with a dispersion concentration of 20wt%, and a mass ratio of xerogel to carbon nanotubes of 1:0.001. Then the two dispersions are mixed in a stirring tank to obtain a mixed slurry, and the mixed slurry is dried while stirring to obtain a CNTs-doped three-dimensional stacked porous carbon precursor.

[0065] (2) The precursor obtained in step (1) is mixed with KOH in a mass ratio of 1:1, pre-oxidized at 240°C at a heating rate of 2°C / min for 5h, pre-carbonized at 550°C for 1h, and then activated at 800°C for 1h, washed with water to remove residual alkali, dried, and then purified at 800°C to obtain a porous carbon skeleton; placed in a CVD deposition furnace, heated to 500°C with nitrogen, and then introduced a mixed gas of silane and nitrogen, maintained for 1h, and the proportion of infiltrated silane is adjusted, the silane flow rate is 30mL / min, the volume ratio of the mixed gas of silane and nitrogen is 1:5, and the deposition is carried out for 8h, and then a mixed gas of acetylene and nitrogen is introduced, the volume ratio is 1:10, the flow rate is 100mL / min, and the deposition is continued for 2h to obtain a porous carbon material deposited with silane.

[0066] (3) Dissolve 10 g of polyacrylonitrile monomer in 100 g of N-methylpyrrolidone, and mix evenly with the porous carbon material prepared in step (2) in a mass ratio of 1:1 (polyacrylonitrile monomer: porous carbon material). Stir the mixed solution at room temperature for 1 h and then heat treat it under nitrogen protection at 700° C. for 8 h to obtain a silicon-carbon negative electrode material coated with a nitrogen heterocyclic conductive polymer.

[0067] Lithium-ion battery preparation:

[0068] In the positive electrode of the lithium-ion battery, the positive electrode collector is aluminum foil, the conductive agent is Super P (SP) and carbon nanotubes (CNT), and the binder is polyvinylidene fluoride (PVDF); among them, the mass ratio of the positive electrode active material, the conductive agent and the binder is 96.4:2:1.6; the positive electrode active material used in the lithium-ion battery is a ternary material (NCM: nickel (NI), cobalt (CO), manganese (Mn) or NCA: nickel (NI), cobalt (CO), aluminum (Al)).

[0069] In the negative electrode of the lithium-ion battery, the negative electrode collector is copper foil, the conductive agent is Super P (SP) and CNT, the binder is sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR), and the mass ratio of the negative electrode active material, the conductive agent and the binder is 94.7:1.5:3.8; the negative electrode active material in the lithium-ion battery is a mixture of graphite and silicon-carbon negative electrode materials, and its mass ratio is 91.7:8.3.

[0070] The ternary material lithium nickel cobalt manganese oxide, the conductive agent SP and CNT (mass ratio 3:2), and the binder PVDF are mixed in a mass ratio of 96.4:2:1.6, and the solvent is N-methylpyrrolidone (NMP). The amount is calculated based on the solid content of the slurry of 67%, and stirred to obtain a positive electrode slurry, which is then coated on the positive electrode current collector aluminum foil, and dried, rolled, cut, and sliced ​​to obtain a positive electrode;

[0071] The graphite prepared above and the silicon-carbon negative electrode material (mass ratio 91.7:8.3) are mixed as negative electrode active materials, conductive agents SP and CNT (mass ratio 25:4), binders CMC and SBR (mass ratio 9:10) and deionized water, wherein the mass ratio of the negative electrode active material, the conductive agent and the binder is 94.7:1.5:3.8, and the amount of water is calculated based on the solid content of the slurry of 45% to obtain a negative electrode slurry, which is then coated on a negative electrode current collector copper foil, and dried, rolled, cut, and sliced ​​to obtain a negative electrode;

[0072] The positive electrode, negative electrode and single-sided coated ceramic diaphragm are wound, shelled, injected, sealed, pre-charged, formed, aged and capacity divided to obtain a lithium ion battery.

[0073] Example 2

[0074] The difference between this embodiment and embodiment 1 is that the polymer copolymerized with acrylonitrile is replaced by acrylamide instead of 2-acrylamide-2-methylpropanesulfonic acid, and the other conditions are exactly the same as those in embodiment 1.

[0075] Example 3

[0076] The difference between this embodiment and embodiment 1 is that the nitrogen heterocyclic conductive polymer monomer is replaced by polypyrrole from polyacrylonitrile monomer, and other conditions are exactly the same as those in embodiment 1.

[0077] Example 4

[0078] The difference between this embodiment and embodiment 1 is that the polymer copolymerized with acrylonitrile is replaced by aniline instead of 2-acrylamide-2-methylpropanesulfonic acid, and the other conditions are exactly the same as those in embodiment 1.

[0079] Example 5

[0080] The difference between this embodiment and embodiment 1 is that the polymer copolymerized with acrylonitrile is replaced by sulfobetaine methacrylate instead of 2-acrylamide-2-methylpropanesulfonic acid, and the other conditions are exactly the same as those in embodiment 1.

[0081] Example 6

[0082] The difference between this embodiment and embodiment 1 is that the nitrogen heterocyclic conductive polymer monomer is replaced by polyaniline from polyacrylonitrile monomer, and the other conditions are exactly the same as those in embodiment 1.

[0083] Performance Test:

[0084] The capacity and rate performance of the lithium ion batteries prepared in Examples 1 to 6 were tested by constant current charging and discharging, with a charging current of 4A and a discharging current of 0.2C / 0.5C / 1C / 10A / 20A / 30A. The test results are shown in Table 1. Figure 2 This is a graph of the cycle retention rate of the lithium-ion battery prepared in Examples 1 to 3 at 4A / 30A. From the graph, it can be seen that the energy retention rate of this type of battery after 200 cycles is ≥80%. Figure 3 It can be seen that the capacity of the lithium-ion battery prepared in Example 1 at different discharge rates has little difference, which indirectly reflects the excellent rate performance of the silicon-carbon material used in Example 1.

[0085] It can be seen that the present invention uses polyacrylonitrile as a carbon source, and forms a conjugated structure on the graphite surface during the coating process, which is beneficial to improving the conductivity and providing a lithium ion transmission channel. On the other hand, since the conjugated structure of polyacrylonitrile contains heteroatom N, it can not only be used to optimize the electronic structure of the carbon layer and improve the conductivity, but also can be used as an adsorption site for lithium ions, thereby improving the capacity and rate performance of the negative electrode material to a certain extent.

[0086] Table 1 Capacity and rate performance test results of lithium-ion batteries prepared in different embodiments

[0087] Example Capacity, mAh / g, 0.2C Rating, 30A Example 1 2553 5.45wh, 200 cycles retention rate ≥ 80% Example 2 2547 4.80wh, 200 cycles retention rate ≥ 80% Example 3 2540 4.80wh, 200 cycles retention rate ≥ 80%

Claims

1. A method for preparing a silicon-carbon negative electrode material, characterized in that: The following steps are involved: S1, after drying the copolymerized polyacrylonitrile hydrogel, dispersing the dry gel and the carbon nanotubes with a solvent respectively and then mixing them, removing the solvent and drying to obtain a carbon nanotube-doped three-dimensional stacked porous carbon precursor; S2, pre-oxidizing and pre-carbonizing the precursor, and then activating and purifying it to obtain a porous carbon skeleton; S3, introducing silane into the porous carbon skeleton under an inert atmosphere for deposition, and then introducing acetylene for further deposition, thereby obtaining a porous carbon material deposited with silane; S4. Dissolve the nitrogen heterocyclic conductive polymer monomer in an organic solvent, then mix it with the porous carbon material, and perform heat treatment under the protection of an inert atmosphere to obtain a silicon-carbon negative electrode material coated with the nitrogen heterocyclic conductive polymer.

2. The preparation method according to claim 1, characterized in that: In step S1, the copolymerized polyacrylonitrile hydrogel is prepared by a photo-initiated one-step in-situ polymerization method.

3. The preparation method according to claim 2, characterized in that: The preparation method of the hydrogel comprises the following steps: in the presence of a ZnCl2 aqueous solution, acrylonitrile, a monomer copolymerizable with acrylonitrile, and a crosslinking agent are mixed evenly, a photoinitiator is added, and polymerization is carried out under ultraviolet light to obtain a copolymerized acrylonitrile hydrogel; the monomer copolymerizable with acrylonitrile is selected from at least one of acrylamide, aniline, 2-acrylamide-2-methylpropanesulfonic acid, or sulfonic acid betaine methacrylate.

4. The preparation method according to claim 1, characterized in that: In step S1, the mass ratio of the dry gel to the carbon nanotubes is 1:0.001-0.1; the dry gel and the carbon nanotubes are dispersed in ethanol respectively, and the dispersion concentration is 5-50wt%.

5. The preparation method according to any one of claims 1 to 4, characterized in that: In step S2, at least one of the following is satisfied: The pre-oxidation temperature is 100-400°C and the pre-oxidation time is 3-8h; The pre-carbonization temperature is 500-600°C and the pre-carbonization time is 1-2h; The activation temperature is 700-900°C and the activation time is 1-5h; The purification temperature is 700-900°C, and the purification time is 1-4h.

6. The preparation method according to claim 5, characterized in that: In step S2, alkaline substances are used to perform pre-oxidation, pre-carbonization and activation treatment on the precursor, and after activation, the precursor is washed and dried to remove residual alkali.

7. The preparation method according to claim 1, characterized in that: In step S3, the volume ratio of silane to nitrogen is 1:5-10, the flow rate is 30 mL / min, and the deposition time is 8 h; the volume ratio of acetylene to nitrogen is 1:10, the flow rate is 100 mL / min, and the deposition time is 2 h.

8. The preparation method according to claim 1, characterized in that: In step S4, at least one of the following is satisfied: The mass ratio of the nitrogen heterocyclic polymer monomer to the porous carbon material is 1:1 to 9; The nitrogen heterocyclic conductive polymer is selected from at least one of polyacrylonitrile, polypyrrole, polyaniline, polycarbazole or polythiophene; The organic solvent is N-methylpyrrolidone; The heat treatment temperature is 500-800°C, and the heat treatment time is 6-8h.

9. The silicon-carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the silicon-carbon negative electrode material according to claim 9 in lithium-ion batteries.

Citation Information

Patent Citations

  • Composite graphite material, secondary battery, device, and preparation method

    CN113207315A

  • Multifunctional phase-change energy-storage composite material and preparation method thereof

    CN113403039A

  • Porous carbon-silicon composite negative electrode material and preparation method thereof

    CN117638045A

  • Porous carbon few-walled carbon nanotube silicon nano composite material and preparation and application methods thereof

    CN118352507A

Cited By

  • Preparation method of current collector, current collector, pole piece, secondary battery and electric equipment

    CN119480879A

  • Porous long-circulation silicon-carbon negative electrode material and preparation method thereof

    CN120221631A

  • A porous long-cycle silicon-carbon negative electrode material and its preparation method

    CN120221631B

  • Copolymer and preparation method thereof, battery negative electrode material and preparation method and application thereof

    CN121064380A

  • Silicon-carbon negative electrode material and preparation method thereof, negative electrode plate and battery