Method for surface modification of silicon wafers after etching treatment
Laser heat treatment with CW, femtosecond, and nanosecond pulse lasers addresses surface unevenness on silicon wafers post-etching, enhancing surface flatness and device performance in integrated circuits.
Patent Information
- Application Number
- JP2020034796
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-02
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-03-02
AI Technical Summary
Conventional methods like etching and chemical mechanical polishing (CMP) create unevenness and recesses on silicon wafer surfaces, leading to particle generation and reduced productivity, and affect device performance and quality control, especially in highly integrated MOS devices.
Applying laser heat treatment using CW, femtosecond, and nanosecond pulse lasers to modify the silicon wafer surface after etching, with specific wavelengths and irradiation conditions to flatten and improve surface quality.
The laser treatment effectively flattens the silicon wafer surface, ensuring consistent device performance even in highly integrated devices, reducing particle generation and improving yield.
Smart Images

Figure 0007558666000001 
Figure 0007558666000002 
Figure 0007558666000003
Abstract
Description
[Technical field]
[0001] The present invention relates to repairing surface defects, which are process-degraded layers on the surface of a silicon wafer, and more particularly to a method for modifying the surface of a silicon wafer by using laser heat treatment to modify and flatten the surface. [Background technology]
[0002] Semiconductor wafers such as silicon wafers used in the manufacture of semiconductor devices are surface-treated by mechanical processes such as cutting, grinding, lapping, and polishing. However, the surface and interior of the wafer are damaged by the process, and some of the damaged layers contain microcracks. These internal cracks are mainly removed by chemical and mechanical methods such as etching and chemical mechanical polishing (CMP).
[0003] For example, Patent Document 1 describes a method for improving the polishing quality of the outer periphery of a semiconductor wafer as a workpiece by applying a uniform pressing force to the edge face at each point on the surface of a polishing tool, thereby polishing the edge face to a high quality.
[0004] Furthermore, Patent Document 2 describes that the use of laser irradiation makes it possible to remove oxygen from silicon wafers and improve their crystallinity, and describes that a method for repairing surface defects, which are layers affected by processing on the surface of a single crystal wafer, involves irradiating a pulsed laser onto the single crystal surface. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2009-297842 A [Patent Document 2] JP 2008-147639 A Summary of the Invention [Problem to be solved by the invention]
[0006] In the above-mentioned conventional techniques described in Patent Documents 1 and 2, in particular, etching and chemical mechanical polishing (CMP) cause recesses (facets) on the silicon wafer surface, and unevenness remains on the wafer surface after etching. Large unevenness on the wafer surface (large surface roughness) causes particle generation in the device manufacturing process, leading to reduced productivity.
[0007] In addition, as MOS devices become smaller and more highly integrated, the surface condition of the wafer has a significant impact on the performance of the final device. In particular, device characteristics such as switching characteristics and voltage resistance are strongly affected by atomic-order unevenness at the interface.
[0008] Furthermore, chemical mechanical polishing (CMP) after etching involves changes from the original shape (design value), making quality control difficult, and there is a possibility that the flatness of the wafer surface, which was improved in the previous process, will be reduced.In addition, chemical mechanical polishing (CMP) uses consumable materials such as abrasive grains, polishing thread, and cleaning liquid, which is costly and has a large environmental impact.
[0009] The object of the present invention is to solve the above-mentioned problems of the conventional technology, to perform a suitable heat treatment using a laser on the surface of a silicon wafer after etching, to flatten the surface, and to improve the performance of the device as well as the yield in the subsequent processes. [Means for solving the problem]
[0010] In order to achieve the above-mentioned object, the present invention provides a method for modifying the surface of a silicon wafer using laser heat treatment, in which after etching the silicon wafer, the surface of the silicon wafer is irradiated with a CW laser (continuous wave laser) or a femtosecond laser, and then irradiated with a nanosecond pulsed laser.
[0011] In the above, it is preferable that the nanosecond pulse laser has a wavelength that is highly absorbed by c-Si (silicon carbide).
[0012] Furthermore, in the above, it is preferable that the nanosecond pulse laser has a wavelength selected from one of 355, 532, and 785 nm.
[0013] Furthermore, in the above, it is preferable that the surface of the silicon wafer is irradiated with the CW laser (continuous wave laser), and that the wavelength of the CW laser (continuous wave laser) is 1080 nm.
[0014] Furthermore, in the above, it is preferable that the surface of the silicon wafer is irradiated with a femtosecond laser, and the surface of the silicon wafer is converted into a-Si (amorphous silicon).
[0015] Furthermore, in the above, it is desirable that the femtosecond laser has a wavelength λ=800 nm.
[0016] Furthermore, in the above, the femtosecond laser is a single shot laser. It is desirable.
[0017] Furthermore, in the above, it is desirable that the femtosecond laser has a low intensity equal to or lower than the processing threshold of a c-Si (silicon carbide) layer.
[0018] Furthermore, in the above, it is desirable that the femtosecond laser has a low intensity equal to or lower than the processing threshold of a c-Si (silicon carbide) layer.
[0019] Furthermore, in the above, it is desirable that the fluence (energy per unit area) of the femtosecond laser is set lower than the fluence at which ablation occurs on the surface of the silicon wafer.
[0020] Furthermore, in the above, it is preferable that the nanosecond pulse laser is a scanning optical system and is irradiated so that the angle of incidence is approximately perpendicular to the surface of the silicon wafer in accordance with the shape of the surface.
[0021] Furthermore, in the above, it is desirable to irradiate the CW laser (continuous wave laser), nanosecond pulse laser, or femtosecond laser by changing at least one of the incident angle, energy density, scan pitch, and scan speed in response to the shape of the silicon wafer surface. Effect of the Invention
[0022] According to the present invention, after etching of a silicon wafer, the surface of the silicon wafer is irradiated with a CW laser (continuous wave laser) or a femtosecond laser, and then irradiated with a nanosecond pulsed laser, so that the surface of the silicon wafer after etching can be flattened by performing a suitable heat treatment using a laser. Therefore, even if the miniaturization and high integration of devices progresses, the performance of the final product is not impaired. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is an explanatory diagram showing a laser irradiation method according to a first embodiment of the present invention. [Diagram 2] FIG. 1 is a block diagram showing an apparatus configuration according to a first embodiment of the present invention. [Diagram 3] Graph showing timing of CW laser and nanosecond pulse laser irradiation in the first embodiment [Figure 4] FIG. 10 is an explanatory diagram showing a laser irradiation method according to a second embodiment of the present invention. [Diagram 5] FIG. 11 is a block diagram showing the configuration of an apparatus according to a second embodiment of the present invention. [Figure 6] Graph showing timing of femtosecond laser and nanosecond pulse laser irradiation in the second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Usually, the etching process of a silicon wafer removes the fractured layer closest to the surface among the surface alteration layers. The etching process ends when the groove width of the microcracks remaining on the silicon wafer surface falls within a predetermined range. As a result, the etching process cannot remove the residual stress layer, and it is difficult to say that the etching process is sufficient to improve the quality of the semiconductor wafer.
[0025] In addition, the surface that has been etched is composed of SiO2 (a silicon oxide film) near the surface, and although this process-affected layer is extremely thin, it has a significant effect on mechanical, electrical, and optical performance. For example, the miniaturization and high integration of MOS devices progresses by thinning the gate oxide film, and the film thickness has reached 2 nm or less.
[0026] Therefore, the surface condition of the silicon wafer has a large effect on the performance of the final device. In particular, the unevenness of the silicon wafer surface has a large effect on the switching characteristics and voltage resistance of the device. To solve these problems, it is essential to create a flatter silicon wafer surface.
[0027] Since the surface vicinity is composed of SiO2 (silicon oxide film), the first embodiment of the present invention irradiates a CW laser (continuous wave laser) of 1080 nm, which is a wavelength with high absorption rate for SiO2, as a laser heat treatment. Then, in the first embodiment, the irradiated portion is heated and the heat is transferred to the c-Si (silicon carbide) portion of the lower layer. After that, one of the nanosecond pulse lasers of 355, 532, and 785 nm, which are wavelengths with high absorption rate for c-Si (silicon carbide), is selected and irradiated according to the surface shape (roughness) after etching.
[0028] In the second embodiment, the surface of the silicon wafer is irradiated with a femtosecond laser once as a laser heat treatment to turn it into a-Si (amorphous silicon). A femtosecond laser is an optical laser that measures time in "femto" (one quadrillionth) units and emits light for only a few to a few hundred femtoseconds. Then, a pulsed laser of 355, 532, or 785 nm, which has a high absorption rate for a-Si (amorphous silicon), is selected and irradiated onto the a-Si (amorphous silicon) portion, melting it and causing epitaxial growth to turn it into a single crystal with a uniform crystal orientation.
[0029] The first and second embodiments are common in that after etching, the silicon wafer surface is irradiated with a CW laser (continuous wave laser) or a femtosecond laser, and then irradiated with a nanosecond pulsed laser. In particular, the nanosecond pulsed laser is characterized by being irradiated with a wavelength of 355, 532, or 785 nm.
[0030] Fig. 1 is an explanatory diagram showing a method of irradiating a silicon wafer surface with a laser according to the first embodiment, and Fig. 2 is a block diagram showing the configuration of the apparatus. As shown in Fig. 1(1), the surface that has been subjected to the etching process is composed of SiO2 (silicon oxide film) near the surface and c-Si (silicon carbide) below that.
[0031] Therefore, the laser irradiation is performed as (1) with a CW laser (continuous wave laser) that performs continuous excitation, with a wavelength of λ = 1080 nm. This heats up the SiO2 (silicon oxide film) on the surface, and the c-Si (silicon carbide) is also heated by heat transfer.
[0032] Next, as shown in Fig. 1(2), the laser is irradiated by selecting one of the nanosecond pulse lasers with wavelengths λ=355, 532, and 785 nm depending on the thickness, surface roughness, and surface shape of the SiO2 (silicon oxide film). The wavelengths λ=355, 532, and 785 nm have high absorption rates for c-Si (silicon carbide).
[0033] The pulse laser conditions are preferably a wavelength of 532 nm, a pulse irradiation time within the range of 3 nanoseconds to 4 nanoseconds, a pulse width of 0.5 μJ to 30 μJ per pulse, and an energy density of 0.125 J / cm. 2 to 7.5 J / cm 2 It is considered good to be.
[0034] Irradiation with a nanosecond pulsed laser melts and solidifies the c-Si (silicon carbide) as shown in Figure 1 (3), promoting flattening.
[0035] 2, the silicon wafer is rotating clockwise. The CW laser oscillator 1 has a wavelength λ=1080 nm and heats a point a on the surface of the silicon wafer via a prism system 10 and a focusing optical system 11. The pulse laser oscillator 2 has a wavelength λ=355, 532, or 785 nm, for example, a wavelength λ=532 nm.
[0036] The pulsed laser oscillator 2 irradiates point b with a nanosecond pulsed laser via a prism system 20 and a focusing optical system 21. If the rotation direction of the silicon wafer is clockwise, the outer peripheral surface of the silicon wafer is heated at point a, and then c-Si (silicon carbide) melts and solidifies at point b.
[0037] Figure 3 is a graph showing the timing of CW laser and nanosecond pulse laser irradiation. The horizontal axis is time t. The outer peripheral surface of the silicon wafer is first irradiated with a CW laser (continuous laser) with a wavelength λ = 1080 nm from CW laser oscillator 1, and after a time determined by the distance between points a and b and the rotation speed of the silicon wafer, one shot of nanosecond pulse laser is emitted.
[0038] Fig. 4 is an explanatory diagram showing a method of irradiating a laser onto a surface according to the second embodiment, and Fig. 5 is a block diagram showing the configuration of the device. The c-Si (silicon carbide) layer on the surface that has been etched is converted into a-Si (amorphous silicon) by a femtosecond laser. A femtosecond laser is an optical laser that measures time in "femto" (one quadrillionth) units and emits light for only a few femtoseconds to a few hundred femtoseconds.
[0039] As shown in Fig. 4(1), the femtosecond laser is irradiated as a single shot with a wavelength of λ = 800 nm, with a low intensity below the processing threshold of the c-Si (silicon carbide) layer. The fluence (energy per unit area) of the femtosecond laser is set lower than the fluence at which ablation occurs on the surface of the silicon wafer.
[0040] The c-Si (silicon carbide) layer has a unique processing threshold, and if the pulse width is sufficiently short, such as femtoseconds, special absorption that differs from normal absorption characteristics occurs, and the outer surface of the silicon wafer is converted into a-Si (amorphous silicon).
[0041] In addition, femtosecond laser irradiation with a laser fluence that usually causes ablation forms a nano-periodic structure in a self-organized manner in the direction perpendicular to the polarization of the laser light. The period of the nano-periodic structure varies depending on the fluence, wavelength, and number of incident pulses of the incident laser. On the other hand, femtosecond laser irradiation with a fluence lower than the ablation threshold is known to form a striped nano-structure through a mechanism different from the above.
[0042] Next, as shown in Fig. 4(2), the a-Si (amorphous silicon) portion is irradiated with a pulsed laser of 355, 532, or 785 nm, which are wavelengths with high absorption rates for a-Si (amorphous silicon). At this time, one of the nanosecond pulsed lasers with wavelengths λ=355, 532, or 785 nm is selected according to the thickness, surface roughness, and surface shape of the SiO2 (silicon oxide film).
[0043] Nanosecond pulsed laser irradiation melts and solidifies the c-Si (silicon carbide) that has been converted into a-Si (amorphous silicon) as shown in Fig. 1 (3), promoting flattening. The pulsed laser conditions are the same as those in the first embodiment, with a wavelength of 532 nm and a pulsed irradiation time in the range of 3 to 4 nanoseconds.
[0044] 5, a femtosecond laser oscillator 3 has a wavelength λ=800 nm, and is irradiated to point a on the surface of a silicon wafer via a prism system 30 and a focusing optical system 31. The femtosecond laser is irradiated as a single shot with a low intensity below the processing threshold of a c-Si (silicon carbide) layer.
[0045] In addition, a polarizer such as a λ / 2 wave plate is also used in the prism system 30 so that the polarization is parallel to the scanning direction. At point a on the surface of the silicon wafer, special absorption different from normal absorption characteristics occurs, and the surface becomes a-Si (amorphous silicon).
[0046] The pulsed laser oscillator 4 irradiates point b with a nanosecond pulsed laser via a prism system 40 and a focusing optical system 41. The nanosecond pulsed laser has a wavelength λ of 355, 532, or 785 nm, for example, a wavelength λ of 532 nm. If the rotation direction of the silicon wafer is clockwise, the outer peripheral surface of the silicon wafer is turned into a-Si (amorphous silicon) at point a, and melted, epitaxially grown, and solidified at point b.
[0047] Figure 6 is a graph showing the timing of femtosecond laser and nanosecond pulsed laser irradiation. The horizontal axis is time t. The outer peripheral surface of the silicon wafer is first irradiated with a femtosecond laser oscillator 3 for a few femtoseconds to a few hundred femtoseconds, and after a time determined by the distance between points a and b and the rotation speed of the silicon wafer, one shot of nanosecond pulsed laser is emitted.
[0048] In both the first and second embodiments, when the silicon wafer surface has a complex shape such as a notch, it is preferable to change at least one of the incident angle, energy density, scan pitch, and scan speed of the CW laser (continuous laser), nanosecond pulse laser, or femtosecond laser in accordance with the shape of the silicon wafer surface. This prevents the performance of the final product from being impaired even if the miniaturization and high integration of devices progresses.
[0049] CW lasers (continuous wave lasers) and nanosecond pulsed lasers can be easily configured as scanning optical systems that can change the irradiation direction. Therefore, it is preferable to configure CW lasers (continuous wave lasers) and nanosecond pulsed lasers as scanning optical systems and irradiate them so that the incident angle is approximately perpendicular to the surface shape, in order to effectively supply energy to the material.
[0050] However, when the incident angle is 10 to 15° or less, the substantial difference is small, and it is sufficient that the incident angle is 10 to 15° or less. Therefore, from the viewpoint of ease of configuration, it is preferable to use a nanosecond pulse laser as a scanning optical system and irradiate the surface substantially perpendicularly in accordance with the surface shape, specifically at an incident angle of 10 to 15° or less.
[0051] In addition, in the case of femtosecond laser irradiation, a polarizer is used for the purpose of amorphization, so the irradiation direction may be kept constant and the s-polarized and p-polarized components may be adjusted by the polarizer in accordance with changes in the incident angle corresponding to the surface shape. [Explanation of symbols]
[0052] 1...CW laser oscillator (CW laser) 2, 4...Pulse laser oscillator (nanosecond pulse laser) 3...Femtosecond laser oscillator (femtosecond laser) 10, 20, 30, 40...Prism series 11, 21, 31, 41...Light collecting optical system
Claims
1. A method for modifying a surface of a silicon wafer using laser heat treatment, comprising the steps of: After etching the silicon wafer, the SiO 2 The heated SiO 2 The heat of the SiO 2 Heat is transferred to the lower layers, Then, a nanosecond pulse laser is irradiated, The irradiation of the nanosecond pulsed laser is performed to remove the SiO 2 a wavelength selected from 355, 532, and 785 nm depending on the thickness and surface roughness of the film, and at least one of the incident angle, energy density, scan pitch, and scan speed is changed in response to the shape of the silicon wafer surface.
2. A method for modifying a surface of a silicon wafer using laser heat treatment, comprising the steps of: After etching the silicon wafer, the SiO 2 The heated SiO 2 The heat of the SiO 2 Heat is transferred to the lower layers, Then, a nanosecond pulse laser is irradiated, The nanosecond pulse laser has a wavelength of 532 nm, a pulse irradiation time in the range of 3 nanoseconds to 4 nanoseconds, a pulse width of 0.5 μJ to 30 μJ per pulse, and an energy density of 0.125 J / cm 2 to 7.5 J / cm 2 and changing at least one of the incident angle, energy density, scan pitch, and scan speed in response to the shape of the silicon wafer surface.
3. 3. The method for modifying a surface of a silicon wafer according to claim 1, wherein the wavelength of the CW laser (continuous wave laser) is 1080 nm.
4. 3. The method for modifying a silicon wafer surface according to claim 1, wherein the nanosecond pulse laser is a scanning optical system and is irradiated so that the angle of incidence is 15° or less in accordance with the shape of the silicon wafer surface.
5. The wavelength of the CW laser (continuous wave laser) is 1080 nm, 3. The method for modifying a silicon wafer surface according to claim 1, wherein the nanosecond pulse laser is a scanning optical system and is irradiated so that the angle of incidence is 15° or less in accordance with the shape of the silicon wafer surface.
Citation Information
Patent Citations
Method of reforming surface of solid sample, impurity activating method and manufacturing method of semiconductor device
JP2005317767A
Repairing method and device for surface defect of single crystal wafer
JP2008147639A
Method for manufacturing SOI substrate, and method for manufacturing semiconductor device
JP2009260315A
Polishing apparatus and polishing method for workpiece peripheral portion
JP2009297842A
Crystal material quality improving apparatus, and crystal material quality improving method