Method for manufacturing nitride semiconductor device
By controlling ion-implantation conditions to meet specific dislocation and depth criteria, the activation rate of n-type impurities in nitride semiconductor devices is enhanced, addressing low activation rates and defects, thus improving device performance.
Patent Information
- Application Number
- JP2020045614
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-16
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-03-16
AI Technical Summary
The activation rate of n-type impurities in nitride semiconductor devices is low due to low annealing rates, leading to implantation defects and device deterioration, particularly in vertical GaN semiconductor devices.
A method for manufacturing nitride semiconductor devices that involves controlling the donor concentration by ion-implanting n-type impurities into a gallium nitride-based semiconductor layer, setting ion-implantation conditions to form an n-type region where the relationship between dislocation density, implantation depth, and tail length satisfies specific formulae, ensuring an activation rate of 20% or more.
Improves the activation rate of n-type impurities, reduces crystal defects, and maintains device characteristics by suppressing charge traps, thereby enhancing the performance of nitride semiconductor devices.
Smart Images

Figure 0007559334000002 
Figure 0007559334000003 
Figure 0007559334000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a nitride semiconductor device and a nitride semiconductor device. [Background technology]
[0002] 2. Description of the Related Art Nitride semiconductor devices having a MOS (Metal Oxide Semiconductor) structure are known. For example, Patent Document 1 discloses a vertical GaN semiconductor device. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-96744 A Summary of the Invention [Problem to be solved by the invention]
[0004] Ion implantation is a method for controlling the donor concentration in an n-type GaN layer. For example, a vertical GaN semiconductor device has an n-type GaN layer and a JFET region between a pair of source regions that are spaced apart from each other. The donor concentration in the JFET region can be controlled by ion implantation, and can be, for example, 1E+17 / cm 3 It is desirable to control it at the same time. However, the activation rate of n-type impurities in the GaN layer by annealing tends to be low. For this reason, when the activation rate is less than 20%, the ion implantation of n-type impurities is performed at a rate of 1E+18 / cm 3 It is necessary to implant n-type impurities at a high concentration of at least 2.5 times the concentration of n-type impurities. If n-type impurity ions are implanted at a high concentration, there is a possibility that many implantation defects will occur in the GaN layer. The implantation defects may cause charge traps and other problems that may degrade the characteristics of the semiconductor device. The present invention has been made in view of the above circumstances, and has an object to provide a manufacturing method for a nitride semiconductor device and a nitride semiconductor device that are capable of improving the activation rate of n-type impurities. [Means for solving the problem]
[0005] In order to solve the above problems, a method for manufacturing a nitride semiconductor device according to one aspect of the present invention includes the steps of: preparing a gallium nitride semiconductor layer having a first surface and a second surface opposite to the first surface; and ion-implanting an n-type impurity into the gallium nitride semiconductor layer from the first surface side to adjust a donor concentration in an n-type region. A relationship is determined in advance between the dislocation density of the gallium nitride semiconductor layer, the depth from the first surface to the implantation peak position of the n-type impurity in the n-type region, and the tail length from the implantation peak position of the n-type impurity to the second surface side, when the activity rate of the n-type impurity in the n-type region reaches a preset value. In the step of ion-implanting the n-type impurity, processing conditions for ion implantation are set so that an n-type region that satisfies this relationship is formed.
[0006] A nitride semiconductor device according to one aspect of the present invention includes a gallium nitride semiconductor layer having a first surface and a second surface opposite to the first surface, and an n-type region provided on the first surface side of the gallium nitride semiconductor layer. The following formula (1) is satisfied, where β is the common logarithm of the dislocation density of the gallium nitride semiconductor layer, T is the depth from the first surface to the injection peak position of the n-type impurity in the n-type region, and ΔT is the tail length from the injection peak position of the n-type impurity to the second surface side. ΔT / T≧0.25β-0.73…(1) Effect of the Invention
[0007] According to the present invention, it is possible to provide a manufacturing method for a nitride semiconductor device and a nitride semiconductor device that are capable of improving the activation rate of n-type impurities. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the configuration of a MOS transistor according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing an ion implantation step for forming a JFET region in a manufacturing process of a MOS transistor according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a graph showing an example (first example) of an implantation profile of n-type impurities in the JFET region shown in FIG. [Figure 4] FIG. 4 is a graph showing an example (second example) of an implantation profile of n-type impurities in the JFET region shown in FIG. [Diagram 5] FIG. 5 is a graph showing an example of a suitable range of α and β that satisfies the formula (2). [Figure 6] FIG. 6 is a cross-sectional view showing a configuration example of a MOS transistor (in the case where the tail length parameter α is small) according to an embodiment of the present invention. [Figure 7] FIG. 7 is a cross-sectional view showing a configuration example of a MOS transistor (in the case where the tail length parameter α is large) according to an embodiment of the present invention. [Figure 8] FIG. 8 is a graph showing the relationship between the tail length parameter and the activation rate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] An embodiment of the present invention will be described below. In the following description of the drawings, the same or similar parts are given the same or similar reference numerals. However, it should be noted that the drawings are schematic, and the relationship between thickness and planar dimensions, the thickness ratio of each device and each member, etc., differ from the actual ones. Therefore, the specific thickness and dimensions should be determined by taking into consideration the following description. In addition, it goes without saying that the drawings include parts whose dimensional relationships and ratios differ from each other.
[0010] In the following description, directions may be described using the terms X-axis, Y-axis, and Z-axis. For example, the X-axis or Y-axis direction is a direction parallel to the surface 12a of the GaN layer 12. The X-axis, Y-axis, or both the X-axis and Y-axis directions are also referred to as horizontal directions. The Z-axis direction is a normal direction to the surface 12a. The Z-axis direction is also the thickness direction of the GaN layer 12. The X-axis, Y-axis, and Z-axis directions are orthogonal to each other.
[0011] In the following description, the direction of the arrow on the Z-axis may be referred to as "up", and the opposite direction of the arrow on the Z-axis may be referred to as "down". "Up" and "down" do not necessarily mean the vertical direction with respect to the ground. That is, the directions of "up" and "down" are not limited to the direction of gravity. "Up" and "down" are merely convenient expressions for specifying the relative positional relationship in a region, layer, film, substrate, etc., and do not limit the technical idea of the present invention. For example, if the paper surface is rotated 180 degrees, it goes without saying that "up" becomes "down" and "down" becomes "up".
[0012] In the following description, n or p means that there are a large number of electrons or holes, respectively. Also, + or - attached to p or n means that the semiconductor region has a relatively high or low impurity concentration compared to the semiconductor region to which + and - are not attached. However, even for semiconductor regions with the same p attached, it does not mean that the impurity concentrations of the respective semiconductor regions are exactly the same.
[0013] <Configuration of MOS Transistor> FIG. 1 is a cross-sectional view showing a configuration example of a MOS (Metal Oxide Semiconductor) transistor 100 according to an embodiment of the present invention. The nitride semiconductor device according to the embodiment of the present invention is, for example, a power semiconductor device, and includes a gallium nitride-based semiconductor substrate 1 shown in FIG. 1 and a MOS transistor 100 provided on the gallium nitride-based semiconductor substrate 1. FIG. 1 shows the unit structure of the MOS transistor 100. The unit structure extends in the Y-axis direction and is repeatedly provided in the X-axis direction. A region where a plurality of unit structures are provided is called an active region. Although not shown, an edge termination structure having a function of preventing electric field concentration in the active region is provided around the active region. The edge termination structure may include one or more of a guard ring structure, a field plate structure, and a JTE (Junction Termination ExtenSiOn) structure.
[0014] As shown in FIG. 1, the MOS transistor 100 has a gate insulating film 5 provided on a gallium nitride semiconductor substrate 1, a gate electrode 6 provided on the gate insulating film 5, and a source electrode 7 and a drain electrode 8 provided on the gallium nitride semiconductor substrate 1. Gallium nitride semiconductor substrate 1 has, for example, a GaN substrate 11 and a GaN layer 12 (an example of a "gallium nitride semiconductor layer" of the present invention) provided on GaN substrate 11. As shown in Fig. 1, front surface 12a (an example of a "first surface" of the present invention) of GaN layer 12 is also front surface 1a of gallium nitride semiconductor substrate 1. A back surface 12b (an example of a "second surface" of the present invention) located opposite front surface 12a of GaN layer 12 is in contact with GaN substrate 11. Back surface 11b of GaN substrate 11 is also back surface 1b of gallium nitride semiconductor substrate 1.
[0015] The GaN substrate 11 is a GaN single crystal substrate. The conductivity type of the GaN substrate 11 is, for example, n+ type. The n-type impurity (dopant) contained in the GaN substrate 11 is one or more elements selected from the group consisting of Si (silicon), O (oxygen), and Ge (germanium), and an example of this is O. The impurity concentration of O in the GaN substrate 11 is 2E+18 / cm 3 That's it. Note that E+ is an exponential notation. For example, 2E+18 is 2×10 18 means... The GaN substrate 11 has a dislocation density of 1E+7 / cm 2 The GaN substrate 11 may be a low dislocation freestanding substrate having a dislocation density of less than 100 nm. When the GaN substrate 11 is a low dislocation freestanding substrate, the dislocation density of the GaN layer 12 formed on the GaN substrate 11 is also low. Furthermore, by using a low dislocation freestanding substrate for the GaN substrate 11, it is possible to reduce leakage current in the power device even when a large-area power device is formed on the GaN substrate 11. This allows the manufacturing equipment to manufacture power devices with a high yield rate. Furthermore, it is possible to prevent ion-implanted impurities from diffusing deeply along the dislocations during heat treatment.
[0016] The GaN layer 12 is provided on the GaN substrate 11. The GaN layer 12 is an n -GaN layer 12 is an n-type GaN single crystal layer, which is formed by epitaxial growth on GaN substrate 11. GaN layer 12 contains n-type impurities of one or more elements selected from the group consisting of Si (silicon), O (oxygen), and Ge (germanium), and one example of such an element is O.
[0017] On the surface 12a side of the GaN layer 12, a p-type well region 13 (an example of the "p-type region" of the present invention), an n+-type source region 14, and an n-type JFET region 15 (an example of the "n-type region" of the present invention) are provided. In the GaN layer 12, a region in which the well region 13 and the source region 14 are not provided may be called a drift region. The drift region functions as a current path between the GaN substrate 11 and the well region 13. The JFET region 15 is a part of the drift region. The JFET region 15 has a higher concentration of n-type impurities and a lower electrical resistance than the other drift regions. The provision of the JFET region 15 reduces the on-resistance of the MOS transistor 100.
[0018] Well region 13 is formed by ion-implanting p-type impurities from the surface 12a side of GaN layer 12 and activating the p-type impurities by heat treatment. The p-type impurities are, for example, magnesium. Well region 13 faces surface 12a of GaN layer 12. Well region 13 also has a first end located on the source region 14 side and a second end located on the JFET region 15 side. In well region 13, a channel of MOS transistor 100 is formed between the first end and the second end, at the contact interface with gate insulating film 5 and in the vicinity thereof.
[0019] The source region 14 is formed by ion-implanting n-type impurities from the surface 12a side of the GaN layer 12 and activating the n-type impurities by heat treatment. The n-type impurities are, for example, one or more elements selected from the group consisting of Si, O, and Ge. The source region 14 faces the surface 12a of the GaN layer 12 and is located inside the well region 13. The sides and bottom of the source region 14 are in contact with the well region 13. The source region 14 and the well region 13 are in contact with each other in the X-axis direction, the Y-axis direction, and the Z-axis direction.
[0020] The JFET region 15 has a higher concentration of n-type impurities than the n-type GaN layer 12. The JFET region 15 is formed by ion-implanting n-type impurities from the surface 12a side of the GaN layer 12 and activating the n-type impurities by heat treatment. The n-type impurities are, for example, one or more elements among Si, O, and Ge, and in one example, it is O. The JFET region 15 faces the surface 12a of the GaN layer 12 and is in contact with the gate insulating film 5. Further, the JFET region 15 is sandwiched from both sides in the horizontal direction (for example, the X-axis direction) by the well region 13. The JFET region 15 faces the source region 14 with the well region 13 in between.
[0021] The gate insulating film 5 is provided on the well region 13. The gate insulating film 5 is, for example, a silicon oxide film (SiO 2 film) or an aluminum oxide (Al 2 O 3 ) film. The thickness of the gate insulating film 5 is, for example, 50 nm or more and 100 nm or less. The gate electrode 6 is provided on the gate insulating film 5. The gate electrode 6 is a planar electrode provided on the flat gate insulating film 5. The gate electrode 6 is formed of, for example, impurity-doped polysilicon.
[0022] The source electrode 7 is continuously provided from above the source region 14 over the well region 13 and is electrically connected to the source region 14 and the well region 13, respectively. Although not shown, the source electrode 7 may be provided to cover the gate electrode 6 via an interlayer insulating film. The source electrode 7 is made of, for example, Al or an Al-Si alloy. The drain electrode 8 is provided on the back surface 11b side of the GaN substrate 11 and is electrically connected to the GaN substrate 11. The drain electrode 8 is made of, for example, Al or an Al-Si alloy.
[0023] <Ion Implantation Process of n-Type Impurities> Figure 2 is a cross-sectional view showing an ion implantation process for forming the JFET region 15 in the manufacturing process of the MOS transistor 100 according to an embodiment of the present invention. As shown in Figure 2, a resist pattern RP is formed on the surface 12a of the GaN layer 12 during ion implantation. The resist pattern RP has a shape that opens above a planned region (hereinafter, JFET formation region) 15' where the JFET region 15 is to be formed and covers other regions. The ion implantation apparatus uses the resist pattern RP as a mask to ion implant n-type impurities into the GaN layer 12 from the surface 12a side of the GaN layer 12. The implantation angle of the n-type impurities with respect to a straight line CL (virtual line) perpendicular to the surface 12a of the GaN layer 12 is called the tilt angle θ. In the ion implantation process shown in Figure 2, the tilt angle θ is arbitrary, but for example, it is 7°. Also, the tilt angle θ is not limited to 7°, and it may be 0°, for example.
[0024] After the n-type impurities are ion implanted into the JFET formation region 15', the resist pattern RP is removed. Thereafter, the GaN layer 12 is heat treated, so that the n-type impurities ion implanted into the JFET formation region 15' are activated, and the JFET region 15 is formed. In the embodiment of the present invention, the implantation profile of the n-type impurities is defined in association with the transition density of the GaN layer 12 so that the activation rate of the n-type impurities by this heat treatment is 20% or more.
[0025] <Implantation profile of n-type impurities> (1) First example Figure 3 is a graph showing an example (first example) of the implantation profile of n-type impurities in the JFET region 15 shown in Figure 1. Figure 3 shows the concentration profile at a position overlapping the straight line CL shown in Figures 1 and 2. In Figure 3, the vertical axis represents the concentration (oxygen concentration) of oxygen, which is an example of n-type impurities [ / cm 3 . The horizontal axis represents the depth [μm] from the surface 12a of the GaN layer 12 to the back surface 12b side. In the first example shown in Figure 3, the type of n-type impurity (dopant) to be ion implanted is oxygen (O). The tilt angle θ of ion implantation is 0 [°], the implantation energy is 700 [keV], and the dose amount is 2.28E+13 [ / cm2 ].
[0026] In the first example, the dislocation density ρd of the GaN layer 12 is 1E+6 [ / cm 3 ]. For the n-type impurity in the JFET region 15, the depth T from the surface 12a of the GaN layer 12 to the injection peak position P1 (hereinafter, injection depth) is 1000 [nm]. For the n-type impurity in the JFET region 15, the tail length ΔT from the injection peak position P1 of the n-type impurity to the back surface 12b side is 1100 [nm]. The tail length is the length from the injection peak position P1 to a position P2 where the concentration of the n-type impurity is 1 / 10 of the concentration at the injection peak position P1 (i.e., the injection peak concentration). The first example satisfies the following formula (2). α≧0.25β-0.73…(2) Equation (2) is a relational expression showing the relationship between α and β. In equation (2), α is a tail length parameter, and is expressed as α=ΔT / T. In addition, β is the common logarithm of the dislocation density ρd of the GaN layer 12, and is expressed as β=log 10 The common logarithm is a logarithm with the base being 10. When formula (2) is satisfied, the activation rate of the n-type impurity in the GaN layer 12 is 20% or more.
[0027] In the first example, since formula (2) is satisfied, the activation rate of the n-type impurity in GaN layer 12 is 20% or more. The method of deriving formula (2) will be described later with reference to FIG. (2) Second Example Fig. 4 is a graph showing an example (second example) of an implantation profile of an n-type impurity in the JFET region 15 shown in Fig. 1. Fig. 4 shows a concentration profile at a position overlapping with the straight line CL shown in Fig. 1 and Fig. 2. In Fig. 4, the vertical axis represents the concentration of oxygen (oxygen concentration) [ / cm 34 ]. The horizontal axis represents the depth [μm] from the front surface 12a of the GaN layer 12 to the rear surface 12b side. In the second example shown in FIG. 4 , the type of n-type impurity (dopant) ion-implanted is oxygen (O). The tilt angle θ of the ion implantation is 7 [°], the implantation energy is 700 [keV], and the dose is 6.03E+13 [ / cm 2 ].
[0028] In the second example, the dislocation density ρd of the GaN layer 12 is 1E+4 [ / cm 3 ]. The implantation depth T of the n-type impurity in the JFET region 15 is 650 [nm]. The tail length ΔT of the n-type impurity in the JFET region 15 is 310 [nm]. As in the first example, the second example also satisfies the above formula (2), and therefore the activation rate of the n-type impurity in the GaN layer 12 is 20% or more.
[0029] (3) Suitable ranges for α and β Fig. 5 is a graph showing an example of suitable ranges of α and β that satisfy formula (2). In Fig. 5, the vertical axis indicates the tail length parameter α. The horizontal axis indicates β, which is the common logarithm of the dislocation density ρd of GaN layer 12. In Fig. 5, the range above the line indicating α=0.25β-0.73 is the range that satisfies the above formula (2), and for example, ranges A to H shown in Fig. 5 are suitable ranges of α and β, respectively.
[0030] For example, range A is a range where α is 0.1 or more and less than 0.2, and β is 3.32 or more and less than 3.72. Range B is a range where α is 0.2 or more and less than 0.3, and β is 3.72 or more and less than 4.12. Range C is a range where α is 0.3 or more and less than 0.4, and β is 4.12 or more and less than 4.52. Range D is a range where α is 0.4 or more and less than 0.5, and β is 4.52 or more and less than 4.92. Range E is a range where α is 0.5 or more and less than 0.6, and β is 4.92 or more and less than 5.32. Range F is a range where α is 0.6 or more and less than 0.7, and β is 5.32 or more and less than 5.72. Range G is a range where α is 0.7 or more and less than 0.8, and β is 5.72 or more and less than 6.12. Range H is a range in which α is equal to or greater than 0.8 and less than 0.9, and β is equal to or greater than 6.12 and less than 6.52.
[0031] Also, the smaller the tail length parameter α, the more preferable. That is, the smaller the tail length ΔT relative to the implantation depth T, the more preferable. In FIG. 5, the range A with the smallest tail length parameter α is the most preferable, the range B is the next most preferable, and the range C is the next most preferable. Similarly, the range C is followed by the range D, the range D is followed by the range E, the range E is followed by the range F, the range F is followed by the range G, and the range G is followed by the range H. The smaller the tail length parameter α, the less the depletion layer is prevented from extending from the p-type well region 13 to the back surface 12b side of the GaN layer 12. This makes it possible to suppress the decrease in the off-state breakdown voltage of the MOS transistor 100. This effect will be described with reference to FIG. 6 and FIG. 7.
[0032] FIG. 6 is a cross-sectional view showing a configuration example of a MOS transistor 100A (when the tail length parameter α is small) according to an embodiment of the present invention. FIG. 7 is a cross-sectional view showing a configuration example of a MOS transistor 100B (when the tail length parameter α is large) according to an embodiment of the present invention. In FIG. 6 and FIG. 7, the implantation depth T of the n-type impurity in the JFET region 15 is the same. In FIG. 6 and FIG. 7, the tail length ΔT of the JFET region 15 is different from each other.
[0033] For example, if the tail length of the MOS transistor 100A shown in Fig. 6 is ΔT1 and the tail length of the MOS transistor 100B shown in Fig. 7 is ΔT2, then ΔT1 is smaller than ΔT2 (ΔT1<ΔT2). As a result, the tail length parameter α of the MOS transistor 100A shown in Fig. 6 is smaller than the tail length parameter α of the MOS transistor 100B shown in Fig. 7. Note that in Figs. 6 and 7, the bottom of the JFET region 15 is illustrated as the position P2 of the tail end.
[0034] 6 and 7, DL and DH show examples of the extension of the depletion layer from the p-type well region 13 to the n-type drift region. DL shows an example of the extension of the depletion layer when no electric field is applied between the drain electrode 8 and the source electrode 7. DH shows an example of the extension of the depletion layer when a high electric field is applied between the drain electrode 8 and the source electrode 7. When a high electric field is applied between the drain electrode 8 and the source electrode 7, a reverse bias state is created between the p-type region and the drift region, and the extension of the depletion layer becomes large as shown by DH.
[0035] As shown in Fig. 6, in a MOS transistor 100A having a short tail length ΔT1, when a high electric field is applied, the depletion layer extends so as to wrap around to below the bottom of the JFET region 15. On the other hand, as shown in Fig. 7, in a MOS transistor 100B having a long tail length ΔT1, when a high electric field is applied, the depletion layer does not easily wrap around to below the bottom of the JFET region 15. The bottom corners 15E of the JFET region 15 and their vicinity are locations where the electric field is likely to concentrate, but if the wraparound of the depletion layer is small, insulation breakdown is likely to occur at these locations. In this way, it is easier to maintain the off-state breakdown voltage of the MOS transistor 100A compared to the MOS transistor 100B, and it is easier to reduce the on-state resistance while maintaining the off-state breakdown voltage. This is why it is preferable that the tail length ΔT is short and the tail length parameter α is small.
[0036] <How to derive the relational equation> Next, a method for deriving the above formula (2) showing the relationship between α and β will be described. FIG. 8 is a graph showing the relationship between the tail length parameter α and the activation rate. In FIG. 8, the vertical axis indicates the activation rate [%], and the vertical axis indicates the tail length parameter. As shown in FIG. 8, the present inventor investigated the relationship between the activation rate of n-type impurities in the n-type region and the tail length parameter α for each dislocation density ρd of the GaN layer, and found that there is a correlation between the activation rate and the tail length parameter α. The combination of tail length parameter α and dislocation density ρd that results in an activation rate of 20% or more is extracted. The extracted data is then plotted on a graph with the tail length parameter α on the vertical axis and the common logarithm β of the dislocation density on the horizontal axis. The obtained plot is approximated, for example, by the least squares method to obtain equation (2). Table 1 shows some of the data obtained in the process of deriving equation (2).
[0037] [Table 1]
[0038] <Effects of the embodiment> As described above, the nitride semiconductor device according to the embodiment of the present invention includes the GaN layer 12 and the JFET region 15 provided on the front surface 12a side of the GaN layer 12. When the common logarithm of the dislocation density ρd of the GaN layer 12 is β, the depth (implantation peak depth) from the front surface 12a to the implantation peak position P1 of the n-type impurity (e.g., oxygen (O)) in the JFET region 15 is T, and the tail length from the implantation peak position P1 of the n-type impurity to the back surface 12b side is ΔT, the above formula (2) is established.
[0039] This makes it possible to improve the activation rate of the n-type impurities in the JFET region 15, and to make the activation rate 20% or more. This makes it possible to keep the concentration of the n-type impurities contained in the JFET region 15 low. For example, when the activation rate of the n-type impurities in the JFET region 15 is less than 20%, the concentration of the n-type impurities is set to 1E+18 / cm 3However, if the activation rate is 20% or more, the n-type impurity concentration should be 1E+17 / cm 3 In this way, in the step of forming the JFET region 15, the dose of n-type impurities to be ion-implanted can be kept low, and the generation of crystal defects in the JFET region 15 due to ion implantation can be suppressed. In the JFE region 15, the generation of charge traps due to crystal defects can be suppressed, and therefore the deterioration of the characteristics of the MOS transistor 100 can be suppressed.
[0040] The method for manufacturing a nitride semiconductor device according to the embodiment of the present invention includes a step of ion-implanting an n-type impurity into the GaN layer 12 from the surface 12a side of the GaN layer 12 to adjust the donor concentration of the JFET region 15. The relationship between the dislocation density ρd of the GaN layer 12, the depth (implantation peak depth) T of the n-type impurity in the JFET region 15 from the surface 12a to the implantation peak position P1, and the tail length ΔT from the implantation peak position P1 of the n-type impurity to the back surface 12b side is obtained in advance when the activity rate of the n-type impurity in the JFET region 15 becomes a preset value (for example, 20% or more). This relationship is shown, for example, in the above formula (2). In the step of ion-implanting the n-type impurity, the process conditions of the ion implantation are set so that the JFET region 15 that satisfies the above formula (2) is formed. The process conditions of the ion implantation include parameters (for example, tilt angle θ and implantation energy) that control the implantation peak depth T and the tail length ΔT. The process conditions of the ion implantation may also include the selection of the dislocation density ρd of the substrate (for example, the GaN layer 12) to be implanted with ions.
[0041] According to this, the activation rate of the n-type impurity in the JFET region 15 can be increased to 20% or more, and the dose of the n-type impurity to be ion-implanted can be kept low. This makes it possible to prevent crystal defects from occurring in the JFET region 15 due to ion implantation. Since it is possible to prevent the occurrence of charge traps due to crystal defects in the JFET region 15, it is possible to prevent deterioration of the characteristics of the MOS transistor 100. In the embodiment of the present invention, the tail length ΔT may be limited to 100 nm or more. In addition to ion implantation, a method of in-situ doping during epitaxial growth may be considered as a method of doping the JFET region 15 with n-type impurities. When doping the n-type impurities in-situ, switching between doped and undoped is performed in a short time by operating a valve in a pipe connected to the chamber, so the tail length ΔT is short, usually less than 100 nm. Therefore, by limiting the tail length ΔT to 100 nm or more, the method of doping the n-type impurities can be substantially limited to ion implantation.
[0042] <Other embodiments> As described above, the present invention has been described by the embodiments and modifications, but the descriptions and drawings forming a part of this disclosure should not be understood as limiting the present invention. Various alternative embodiments and modifications will become apparent to those skilled in the art from this disclosure. For example, in the above embodiment, oxygen (O) is ion-implanted as an n-type impurity when forming the JFET region 15, but the n-type impurity is not limited to oxygen. In the embodiment of the present invention, the n-type impurity to be ion-implanted may include one or more elements of oxygen, silicon (Si), and germanium (Ge). Even in such a case, the relationship between the dislocation density ρd of the GaN layer 12, the implantation peak depth T of the n-type impurity, and the tail length ΔT of the n-type impurity when the activation rate of the n-type impurity is a preset value (for example, 20%) or more is obtained in advance, and the processing conditions of the ion implantation are set so that the JFET region 15 that satisfies this relationship is formed. This makes it possible to achieve an activation rate of 20% or more while keeping the dose of ion implantation low and suppressing the occurrence of crystal defects.
[0043] In the above embodiment, the activation rate of the n-type impurity is described as 20% or more, but the target value of the activation rate is not limited to 20% or more. The target value of the activation rate may be, for example, 25% or more. Even in such a case, as shown in FIG. 8, the relationship between the activation rate of the n-type impurity and the tail length parameter α is investigated for each dislocation density ρd of the GaN layer 12, and a combination of the tail length parameter α and the dislocation density ρd when the activation rate is 25% or more is extracted to obtain a relational expression such as Equation (2). Then, the processing conditions of the ion implantation are set so that the JFET region 15 that satisfies this relational expression is formed. This makes it possible to achieve an activation rate of 25% or more while suppressing the occurrence of crystal defects while keeping the dose of the ion implantation low.
[0044] In addition, in the above embodiment, the JFET region 15 is exemplified as the "n-type region" of the present invention, but the "n-type region" is not limited to the JFET region 15 and may be another region. In the above embodiment, the GaN layer 12 is exemplified as the "gallium nitride semiconductor layer" of the present invention, but the "gallium nitride semiconductor layer" is not limited to the GaN layer. For example, the "gallium nitride semiconductor layer" may be a bulk GaN substrate. The "gallium nitride semiconductor layer" may contain GaN as a main component, and may further contain one or more elements selected from the group consisting of aluminum (Al) and indium (In).
[0045] Thus, the present invention naturally includes various embodiments not described here. At least one of various omissions, substitutions, and modifications of components can be made without departing from the spirit of the above-mentioned embodiments and modifications. Furthermore, the effects described in this specification are merely examples and are not limited to the present invention, and other effects may also be present. The technical scope of the present invention is defined only by the invention-specific matters related to the scope of the claims that are appropriate from the above description. [Explanation of symbols]
[0046] 1. Gallium nitride semiconductor substrate 1a, 12a surface 1b, 11b, 12b back side 5 Gate insulating film 6 Gate electrode 7. Source Electrode 8 Drain electrode 11 GaN substrate 12 GaN layers 13 Well Area 14 Source Area 15 JFET area 15' JFET formation area 15E Bottom corner 100, 100A, 100B MOS transistors A, B, C, D, E, F, G, H range P1 Injection peak position P2 position RP resist pattern α tail length parameter ΔT, ΔT1, ΔT2 tail length θ Tilt angle ρd Dislocation density
Claims
1. preparing a gallium nitride based semiconductor layer having a first surface and a second surface located opposite to the first surface, and ion-implanting an n-type impurity into the gallium nitride based semiconductor layer from the first surface side to adjust a donor concentration in an n-type region, determining in advance a relationship between a dislocation density of the gallium nitride based semiconductor layer, a depth from the first surface to an implantation peak position of the n-type impurity in the n-type region, and a tail length from the implantation peak position of the n-type impurity toward the second surface when an activity rate of the n-type impurity in the n-type region reaches a preset value; In the step of ion-implanting the n-type impurity, a process condition for ion implantation is set so as to form the n-type region that satisfies the above relationship.
2. The method for manufacturing a nitride semiconductor device according to claim 1 , wherein said preset value is 20% or more.
3. The relationship is expressed by the following formula (1): ΔT / T≧0.25β−0.73…(1) 3. The method for manufacturing a nitride semiconductor device according to claim 1, wherein in said formula (1), ΔT is a tail length, T is an implantation peak depth, and β is a common logarithm of dislocation density.
4. The method for manufacturing a nitride semiconductor device according to claim 3 , wherein in said formula (1), ΔT is 100 nm or more.
5. 5. The method for manufacturing a nitride semiconductor device according to claim 1, wherein the tail length is a length from the implantation peak position to a position where a concentration of the n-type impurity becomes 1 / 10 of a concentration at the implantation peak position.
6. The method for manufacturing a nitride semiconductor device according to claim 1 , wherein the n-type impurity includes at least one element selected from the group consisting of oxygen, silicon, and germanium.
Citation Information
Patent Citations
Method of manufacturing iii nitride film
JP2003347234A
Manufacturing method of gallium nitride semiconductor device
JP2017054852A
Semiconductor device manufacturing method and semiconductor device
JP2017174990A
VERTICAL GaN-BASED SEMICONDUCTOR DEVICE MANUFACTURING METHOD AND VERTICAL GaN-BASED SEMICONDUCTOR DEVICE