Laser processing method, semiconductor component manufacturing method, and laser processing device
The laser processing method forms non-overlapping modification spots within semiconductor objects to create precise cracks, addressing the inconsistency in existing methods and enhancing the quality of semiconductor members by reducing surface irregularities and improving production efficiency.
Patent Information
- Application Number
- JP2020561495
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-21
- Filing Date
- 2019-12-18
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-12-18
AI Technical Summary
Existing laser processing methods for semiconductor members fail to form modified regions with precision, leading to inconsistent and inaccurate formation of cracks, which affects the quality of obtained semiconductor members.
A laser processing method that forms a plurality of first and second modification spots along a virtual plane within a semiconductor object, ensuring they do not overlap, and uses precise control of the focal point of the pulsed laser beam to form cracks with high accuracy, utilizing the properties of gallium nitride decomposition and nitrogen gas pressure to enhance precision.
The method enables the formation of cracks with high precision, resulting in the production of suitable semiconductor members such as wafers and devices with reduced surface irregularities, improving material efficiency and production quality.
Smart Images

Figure 0007560055000001 
Figure 0007560055000002 
Figure 0007560055000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a laser processing method, a semiconductor component manufacturing method, and a laser processing apparatus. [Background technology]
[0002] There is known a processing method in which a semiconductor object such as a semiconductor ingot is irradiated with laser light to form a modified region inside the semiconductor object, and a crack extending from the modified region is propagated, thereby cutting out a semiconductor component such as a semiconductor wafer from the semiconductor object (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-183600 A [Patent Document 2] JP 2017-057103 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the above-mentioned processing method, the manner in which the modified region is formed significantly affects the state of the resulting semiconductor article.
[0005] An object of the present disclosure is to provide a laser processing method, a semiconductor component manufacturing method, and a laser processing apparatus that enable the production of suitable semiconductor components. [Means for solving the problem]
[0006] A laser processing method according to one aspect of the present disclosure is a laser processing method for cutting a semiconductor object along a virtual plane inside the semiconductor object that faces a surface of the semiconductor object, and includes a first step of forming a plurality of first modified spots along the virtual plane by directing laser light into the interior of the semiconductor object from the surface, and a second step of forming a plurality of second modified spots along the virtual plane by directing laser light into the interior of the semiconductor object from the surface so as not to overlap the plurality of first modified spots.
[0007] In this laser processing method, a plurality of first modified spots are formed along the imaginary surface, and a plurality of second modified spots are formed along the imaginary surface so as not to overlap the plurality of first modified spots. This allows the plurality of first modified spots and the plurality of second modified spots to be formed along the imaginary surface with high precision, and as a result, it becomes possible to form a crack across the imaginary surface with high precision. Therefore, according to this laser processing method, a semiconductor component is obtained from a semiconductor object with the crack across the imaginary surface as a boundary, thereby making it possible to obtain a suitable semiconductor component.
[0008] In the laser processing method according to one aspect of the present disclosure, in the second step, a plurality of second modified spots may be formed along the imaginary surface so as not to overlap with a plurality of cracks extending from the plurality of first modified spots, respectively. This makes it possible to form the plurality of first modified spots and the plurality of second modified spots along the imaginary surface with higher accuracy, and as a result, it becomes possible to form cracks spanning the imaginary surface along the imaginary surface with higher accuracy.
[0009] In the laser processing method according to one aspect of the present disclosure, in the second step, after forming the second modified spots, a laser beam may be incident on the inside of the semiconductor object from the surface to form a third modified spot along the imaginary surface so as not to overlap the first modified spots and the second modified spots. This makes it possible to more accurately form a crack spanning the imaginary surface along the imaginary surface.
[0010] In the laser processing method according to one aspect of the present disclosure, in the first step, the first modified spots may be formed so that the cracks extending from the first modified spots are not connected to each other. This makes it possible to form the second modified spots along the virtual surface with higher accuracy.
[0011] In the laser processing method according to one aspect of the present disclosure, in the first step, a focus point of the pulsed laser light is moved along a virtual plane to form a plurality of rows of first modified spots as a plurality of first modified spots, and in the second step, a focus point of the pulsed laser light is moved along the virtual plane between the rows of the first modified spots to form a plurality of rows of second modified spots as a plurality of second modified spots. This can reliably prevent the plurality of second modified spots from overlapping with the plurality of first modified spots and the plurality of cracks extending from the plurality of first modified spots, respectively, and can more accurately form the plurality of second modified spots along the virtual plane.
[0012] In the laser processing method according to one aspect of the present disclosure, the material of the semiconductor object may contain gallium. In this case, when gallium is precipitated in the cracks extending from the first modification spots by irradiation with the laser light, the gallium is likely to absorb the laser light. Therefore, forming the second modification spots so as not to overlap the cracks is effective in forming the second modification spots along the virtual surface with high accuracy.
[0013] In the laser processing method according to one aspect of the present disclosure, the material of the semiconductor object may contain gallium nitride. In this case, when the gallium nitride is decomposed by the irradiation of the laser light, gallium is precipitated in a plurality of cracks extending from the plurality of first modified spots, and the gallium is easily capable of absorbing the laser light. Therefore, forming a plurality of second modified spots so as not to overlap the cracks is effective in forming the plurality of second modified spots along the virtual surface with high accuracy. Furthermore, when the gallium nitride is decomposed by the irradiation of the laser light, nitrogen gas is generated in the plurality of cracks. Therefore, it is possible to easily form cracks across the virtual surface by utilizing the pressure (internal pressure) of the nitrogen gas.
[0014] A semiconductor component manufacturing method according to one aspect of the present disclosure comprises the first and second steps of the laser processing method described above, and a third step of obtaining a semiconductor component from a semiconductor object using a crack spanning an imaginary surface as a boundary.
[0015] According to this semiconductor article manufacturing method, the first and second steps make it possible to form a crack spanning the imaginary surface along the imaginary surface with high precision, thereby making it possible to obtain a suitable semiconductor article.
[0016] In the semiconductor article manufacturing method according to one aspect of the present disclosure, a plurality of imaginary surfaces may be set so as to be aligned in a direction facing the front surface, which makes it possible to obtain a plurality of semiconductor articles from one semiconductor object.
[0017] In the semiconductor article manufacturing method according to one aspect of the present disclosure, the semiconductor object may be a semiconductor ingot and the semiconductor article may be a semiconductor wafer, thereby making it possible to obtain a plurality of suitable semiconductor wafers.
[0018] In the semiconductor article manufacturing method according to one aspect of the present disclosure, a plurality of imaginary surfaces may be set so as to be aligned in a direction in which the surface extends, which makes it possible to obtain a plurality of semiconductor articles from one semiconductor object.
[0019] In the semiconductor article manufacturing method according to one aspect of the present disclosure, the semiconductor object may be a semiconductor wafer and the semiconductor article may be a semiconductor device. This makes it possible to obtain a plurality of suitable semiconductor devices.
[0020] A laser processing apparatus according to one aspect of the present disclosure is a laser processing apparatus for cutting a semiconductor object along a virtual plane inside the semiconductor object that faces a surface of the semiconductor object, and includes a stage for supporting the semiconductor object, and a laser irradiation unit for forming a plurality of first modified spots and a plurality of second modified spots along the virtual surface by directing laser light into the interior of the semiconductor object from the surface, wherein the laser irradiation unit forms the plurality of first modified spots along the virtual surface, and after forming the plurality of first modified spots, forms a plurality of second modified spots along the virtual surface so as not to overlap the plurality of first modified spots.
[0021] According to this laser processing device, it is possible to form a crack that spans the imaginary surface along the imaginary surface with high accuracy, so that a suitable semiconductor component can be obtained. Effect of the Invention
[0022] According to the present disclosure, it is possible to provide a laser processing method, a semiconductor component manufacturing method, and a laser processing apparatus that enable the production of suitable semiconductor components. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a configuration diagram of a laser processing device according to one embodiment. [Diagram 2] FIG. 2 is a side view of a GaN ingot that is a target of the laser processing method and the semiconductor product manufacturing method of the first embodiment. [Diagram 3] FIG. 3 is a plan view of the GaN ingot shown in FIG. [Figure 4] FIG. 4 is a vertical cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method according to the first embodiment. [Diagram 5]FIG. 5 is a cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method according to the first embodiment. [Figure 6] FIG. 6 is a vertical cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method according to the first embodiment. [Figure 7] FIG. 7 is a cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method according to the first embodiment. [Figure 8] FIG. 8 is a vertical cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method according to the first embodiment. [Figure 9] FIG. 9 is a cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method of the first embodiment. [Figure 10] FIG. 10 is a vertical cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method of the first embodiment. [Figure 11] FIG. 11 is a cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method of the first embodiment. [Figure 12] FIG. 12 is a side view of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method of the first embodiment. [Figure 13] FIG. 13 is a side view of a GaN wafer in a step of the laser processing method and the semiconductor article manufacturing method of the first embodiment. [Figure 14] FIG. 14 is an image of a peeled surface of a GaN wafer formed by an example of the laser processing method and the semiconductor component manufacturing method. [Figure 15] FIG. 15 is a height profile of the peel surface shown in FIG. [Figure 16] FIG. 16 is an image of a peeled surface of a GaN wafer formed by another example of the laser processing method and the semiconductor component manufacturing method. [Figure 17] FIG. 17 is a height profile of the peel surface shown in FIG. [Figure 18] FIG. 18 is a schematic diagram for explaining the principle of forming a peeled surface by an example of the laser processing method and the semiconductor article manufacturing method. [Figure 19] FIG. 19 is a schematic diagram for explaining the principle of formation of a peeled surface by the laser processing method and the semiconductor article manufacturing method according to another example. [Figure 20] FIG. 20 is an image of a crack formed during an example laser processing method and semiconductor component manufacturing method. [Figure 21] FIG. 21 shows an image of a crack formed during another example of the laser processing method and the semiconductor component manufacturing method. [Figure 22] FIG. 22 shows images of modified spots and cracks formed by the laser processing method and the semiconductor component manufacturing method of the comparative example. [Figure 23] FIG. 23 is an image of modified spots and cracks formed by the laser processing method and the semiconductor component manufacturing method of the first embodiment. [Figure 24] FIG. 24 shows images of modified spots and cracks formed by the laser processing methods and semiconductor component manufacturing methods of the second and third embodiments. [Diagram 25] FIG. 25 is a plan view of a GaN wafer which is a target of the laser processing method and the semiconductor article manufacturing method of the second embodiment. [Figure 26] FIG. 26 is a side view of a part of a GaN wafer in a step of the laser processing method and semiconductor article manufacturing method of the second embodiment. [Figure 27] FIG. 27 is a side view of a part of a GaN wafer in a step of the laser processing method and semiconductor article manufacturing method of the second embodiment. [Figure 28] FIG. 28 is a side view of a semiconductor device in a step of the laser processing method and the semiconductor article manufacturing method of the second embodiment. [Figure 29] FIG. 29 is an image of a crack in a SiC wafer formed by the laser processing method and the semiconductor component manufacturing method of the comparative example. [Diagram 30]FIG. 30 is an image of a crack in a SiC wafer formed by the laser processing method and the semiconductor component manufacturing method of the embodiment. [Diagram 31] FIG. 31 is an image of the peeled surface of a SiC wafer formed by the laser processing method and the semiconductor component manufacturing method of the embodiment. [Diagram 32] FIG. 32 is a height profile of the peel surface shown in FIG. [Diagram 33] FIG. 33 is a plan view of a GaN ingot in a step of a laser processing method and a semiconductor product manufacturing method according to a modified example. [Diagram 34] FIG. 34 is a plan view of a GaN ingot in a step of a laser processing method and a semiconductor product manufacturing method according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. In each drawing, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. [Laser processing equipment configuration]
[0025] 1, the laser processing apparatus 1 includes a stage 2, a light source 3, a spatial light modulator 4, a condenser lens 5, and a control unit 6. The laser processing apparatus 1 is an apparatus that forms a modified region 12 in an object 11 by irradiating the object 11 with laser light L. Hereinafter, the first horizontal direction is referred to as the X direction, and the second horizontal direction perpendicular to the first horizontal direction is referred to as the Y direction. In addition, the vertical direction is referred to as the Z direction.
[0026] The stage 2 supports the object 11, for example, by adsorbing a film attached to the object 11. In this embodiment, the stage 2 is movable along both the X direction and the Y direction. In addition, the stage 2 is rotatable about an axis parallel to the Z direction.
[0027] The light source 3 outputs laser light L having transparency to the object 11, for example, by a pulse oscillation method. The spatial light modulator 4 modulates the laser light L output from the light source 3. The spatial light modulator 4 is, for example, a reflective liquid crystal (LCOS: Liquid Crystal on Silicon) spatial light modulator (SLM: Spatial Light Modulator). The condenser lens 5 condenses the laser light L modulated by the spatial light modulator 4. In this embodiment, the spatial light modulator 4 and the condenser lens 5 are movable along the Z direction as a laser irradiation unit.
[0028] When the laser light L is focused inside the object 11 supported by the stage 2, the laser light L is particularly absorbed in a portion corresponding to the focusing point C of the laser light L, and a modified region 12 is formed inside the object 11. The modified region 12 is a region whose density, refractive index, mechanical strength, and other physical properties are different from those of the surrounding non-modified region. Examples of the modified region 12 include a melting treatment region, a crack region, a dielectric breakdown region, a refractive index change region, and the like.
[0029] As an example, when the stage 2 is moved along the X direction and the focal point C is moved along the X direction relative to the object 11, multiple modified spots 13 are formed in a row along the X direction. One modified spot 13 is formed by irradiating one pulse of laser light L. One row of modified regions 12 is a collection of multiple modified spots 13 lined up in a row. Adjacent modified spots 13 may be connected to each other or separated from each other depending on the relative moving speed of the focal point C with respect to the object 11 and the repetition frequency of the laser light L.
[0030] The control unit 6 controls the stage 2, the light source 3, the spatial light modulator 4, and the condenser lens 5. The control unit 6 is configured as a computer device including a processor, a memory, a storage, a communication device, etc. In the control unit 6, software (programs) loaded into the memory, etc. are executed by the processor, and the reading and writing of data in the memory and storage, as well as communication by the communication device, are controlled by the processor. In this way, the control unit 6 realizes various functions. [First embodiment of laser processing method and semiconductor member manufacturing method]
[0031] An object 11 in the laser processing method and semiconductor member manufacturing method of the first embodiment is a GaN ingot (semiconductor ingot, semiconductor object) 20 formed of gallium nitride (GaN) in, for example, a disk shape, as shown in Figures 2 and 3. As an example, the GaN ingot 20 has a diameter of 2 inches and a thickness of 2 mm. The laser processing method and semiconductor member manufacturing method of the first embodiment are performed to cut out a plurality of GaN wafers (semiconductor wafers, semiconductor members) 30 from the GaN ingot 20. As an example, the GaN wafer 30 has a diameter of 2 inches and a thickness of 100 µm.
[0032] First, the above-mentioned laser processing device 1 forms a plurality of modified spots 13 along each of the plurality of imaginary surfaces 15. Each of the plurality of imaginary surfaces 15 is a surface facing the surface 20a of the GaN ingot 20 inside the GaN ingot 20, and is set to be aligned in a direction facing the surface 20a. In this embodiment, each of the plurality of imaginary surfaces 15 is a surface parallel to the surface 20a, and has, for example, a circular shape. Each of the plurality of imaginary surfaces 15 is set to overlap each other when viewed from the surface 20a side. In the GaN ingot 20, a plurality of peripheral regions 16 are set to surround each of the plurality of imaginary surfaces 15. That is, each of the plurality of imaginary surfaces 15 does not reach the side surface 20b of the GaN ingot 20. As an example, the distance between adjacent imaginary surfaces 15 is 100 μm, and the width of the peripheral region 16 (in this embodiment, the distance between the outer edge of the imaginary surface 15 and the side surface 20b) is 30 μm or more.
[0033] The formation of the multiple modified spots 13 is performed sequentially for each imaginary surface 15 from the opposite side to the surface 20a by irradiation with laser light L having a wavelength of, for example, 532 nm. Since the formation of the multiple modified spots 13 is similar for each of the multiple imaginary surfaces 15, the formation of the multiple modified spots 13 along the imaginary surface 15 closest to the surface 20a will be described in detail below with reference to Figures 4 to 11. In addition, in Figures 5, 7, 9, and 11, the arrows indicate the trajectory of the focal point C of the laser light L. In addition, the modified spots 13a, 13b, 13c, and 13d described later are collectively referred to as the modified spots 13, and the cracks 14a, 14b, 14c, and 14d described later are collectively referred to as the cracks 14.
[0034] First, as shown in Fig. 4 and Fig. 5, the laser processing apparatus 1 forms a plurality of modified spots (first modified spots) 13a along the imaginary plane 15 (for example, arranged two-dimensionally along the entire imaginary plane 15) by irradiating the laser light L into the inside of the GaN ingot 20 from the surface 20a (first step). At this time, the laser processing apparatus 1 forms a plurality of modified spots 13a so that a plurality of cracks 14a extending from each of the modified spots 13a are not connected to each other. In addition, the laser processing apparatus 1 forms a plurality of rows of modified spots 13a by moving the focal point C of the pulsed laser light L along the imaginary plane 15. Note that in Fig. 4 and Fig. 5, the modified spots 13a are shown in white (without hatching), and the ranges to which the cracks 14a extend are shown by dashed lines (similar to Figs. 6 to 11).
[0035] In this embodiment, the pulsed laser light L is modulated by the spatial light modulator 4 so as to be focused on a plurality of (for example, six) focusing points C arranged in the Y direction. Then, the plurality of focusing points C are moved relatively on the virtual plane 15 along the X direction. As an example, the distance between adjacent focusing points C in the Y direction is 8 μm, and the pulse pitch of the laser light L (i.e., the value obtained by dividing the relative moving speed of the plurality of focusing points C by the repetition frequency of the laser light L) is 10 μm. In addition, the pulse energy of the laser light L per one focusing point C (hereinafter simply referred to as the "pulse energy of the laser light L") is 0.33 μJ. In this case, the center-to-center distance between the adjacent modified spots 13a in the Y direction is 8 μm, and the center-to-center distance between the adjacent modified spots 13a in the X direction is 10 μm. In addition, the plurality of cracks 14a extending from the plurality of modified spots 13a are not connected to each other.
[0036] Next, as shown in Fig. 6 and Fig. 7, the laser processing apparatus 1 applies laser light L to the inside of the GaN ingot 20 from the surface 20a to form a plurality of modified spots (second modified spots) 13b along the imaginary plane 15 (for example, arranged two-dimensionally along the entire imaginary plane 15) (second step). At this time, the laser processing apparatus 1 forms a plurality of modified spots 13b so as not to overlap with the plurality of modified spots 13a and the plurality of cracks 14a. In addition, the laser processing apparatus 1 moves the focal point C of the pulsed laser light L along the imaginary plane 15 between the plurality of rows of modified spots 13a to form a plurality of rows of modified spots 13b. In this step, the plurality of cracks 14b extending from the plurality of modified spots 13b may be connected to the plurality of cracks 14a. In addition, in Figs. 6 and 7, the modified spots 13b are indicated by dot hatching, and the ranges into which the cracks 14b extend are indicated by dashed lines (the same applies to Figs. 8 to 11).
[0037] In this embodiment, the pulsed laser light L is modulated by the spatial light modulator 4 so as to be focused on a plurality of (for example, six) focusing points C arranged in the Y direction. Then, the plurality of focusing points C are relatively moved on the virtual plane 15 along the X direction at the center between the rows of the modified spots 13a. As an example, the distance between adjacent focusing points C in the Y direction is 8 μm, and the pulse pitch of the laser light L is 10 μm. In addition, the pulse energy of the laser light L is 0.33 μJ. In this case, the center-to-center distance between adjacent modified spots 13b in the Y direction is 8 μm, and the center-to-center distance between adjacent modified spots 13b in the X direction is 10 μm.
[0038] Next, as shown in Figures 8 and 9, the laser processing device 1 causes the laser light L to be incident on the inside of the GaN ingot 20 from the surface 20a, thereby forming a plurality of modified spots (third modified spots) 13c along the imaginary surface 15 (for example, arranged two-dimensionally along the entire imaginary surface 15) (second step). Furthermore, as shown in Figures 10 and 11, the laser processing device 1 causes the laser light L to be incident on the inside of the GaN ingot 20 from the surface 20a, thereby forming a plurality of modified spots (third modified spots) 13d along the imaginary surface 15 (for example, arranged two-dimensionally along the entire imaginary surface 15) (second step). At this time, the laser processing device 1 forms a plurality of modified spots 13c and 13d so as not to overlap with the plurality of modified spots 13a and 13b. In addition, the laser processing apparatus 1 forms a plurality of rows of modified spots 13c, 13d by moving the focal point C of the pulsed laser light L between the rows of the modified spots 13a, 13b along the imaginary plane 15. In this process, a plurality of cracks 14c, 14d extending from the modified spots 13c, 13d may be connected to a plurality of cracks 14a, 14b. In addition, in Fig. 8 and Fig. 9, the modified spot 13c is shown by solid hatching, and the range into which the crack 14c extends is shown by dashed lines (similar to Fig. 10 and Fig. 11). In addition, in Fig. 10 and Fig. 11, the modified spot 13d is shown by solid hatching (solid hatching inclined opposite to the solid hatching of the modified spot 13c), and the range into which the crack 14d extends is shown by dashed lines.
[0039] In this embodiment, the pulsed laser light L is modulated by the spatial light modulator 4 so as to be focused on a plurality of (for example, six) focusing points C arranged in the Y direction. The plurality of focusing points C are relatively moved on the virtual plane 15 along the X direction at the center between the rows of the modified spots 13a and 13b. As an example, the distance between adjacent focusing points C in the Y direction is 8 μm, and the pulse pitch of the laser light L is 5 μm. The pulse energy of the laser light L is 0.33 μJ. In this case, the center-to-center distance between the modified spots 13c adjacent in the Y direction is 8 μm, and the center-to-center distance between the modified spots 13c adjacent in the X direction is 5 μm. The center-to-center distance between the modified spots 13d adjacent in the Y direction is 8 μm, and the center-to-center distance between the modified spots 13d adjacent in the X direction is 5 μm.
[0040] Next, a heating device including a heater or the like heats the GaN ingot 20, and the cracks 14 extending from the modified spots 13 are connected to each other on each of the imaginary planes 15, thereby forming a crack 17 (hereinafter simply referred to as "crack 17") across the imaginary planes 15 on each of the imaginary planes 15 as shown in FIG. 12. In FIG. 12, the modified spots 13 and the cracks 14, as well as the range in which the cracks 17 are formed, are shown by dashed lines. Note that the cracks 17 may be formed by connecting the cracks 14 to each other by applying some force to the GaN ingot 20 by a method other than heating. Also, the cracks 17 may be formed by connecting the cracks 14 to each other by forming the modified spots 13 along the imaginary planes 15.
[0041] Here, in the GaN ingot 20, nitrogen gas is generated in the multiple cracks 14 extending from the multiple modified spots 13. Therefore, by heating the GaN ingot 20 to expand the nitrogen gas, the pressure (internal pressure) of the nitrogen gas can be used to form the cracks 17. Moreover, the peripheral region 16 prevents the multiple cracks 14 from progressing to the outside of the virtual surface 15 surrounded by the peripheral region 16 (for example, the side surface 20b of the GaN ingot 20), so that the nitrogen gas generated in the multiple cracks 14 can be prevented from escaping to the outside of the virtual surface 15. In other words, the peripheral region 16 is a non-modified region that does not include the modified spots 13, and is a region that prevents the multiple cracks 14 from progressing to the outside of the virtual surface 15 surrounded by the peripheral region 16 when the cracks 17 are formed on the virtual surface 15 surrounded by the peripheral region 16. For this reason, it is preferable to set the width of the peripheral region 16 to 30 μm or more.
[0042] Next, a grinding device grinds (polishes) the portions of the GaN ingot 20 corresponding to each of the peripheral regions 16 and each of the imaginary planes 15, thereby obtaining a plurality of GaN wafers 30 from the GaN ingot 20 with each of the cracks 17 as boundaries, as shown in Fig. 13 (third step). In this manner, the GaN ingot 20 is cut along each of the imaginary planes 15. Note that in this step, the portions of the GaN ingot 20 corresponding to each of the peripheral regions 16 may be removed by mechanical processing, laser processing, or the like other than grinding.
[0043] Of the above steps, the laser processing method of the first embodiment includes the steps up to the step of forming the multiple modified spots 13 along each of the multiple imaginary planes 15. Also, of the above steps, the semiconductor component manufacturing method of the first embodiment includes the steps up to the step of obtaining the multiple GaN wafers 30 from the GaN ingot 20 with each of the multiple cracks 17 as boundaries.
[0044] As described above, in the laser processing method of the first embodiment, a plurality of modified spots 13a are formed along each of the plurality of imaginary surfaces 15, and a plurality of modified spots 13b are formed along each of the plurality of imaginary surfaces 15 so as not to overlap the plurality of modified spots 13a and the plurality of cracks 14a. Furthermore, in the laser processing method of the first embodiment, a plurality of modified spots 13c, 13d are formed along each of the plurality of imaginary surfaces 15 so as not to overlap the plurality of modified spots 13a, 13b. This makes it possible to form a plurality of modified spots 13 accurately along each of the plurality of imaginary surfaces 15, and as a result, it becomes possible to form a plurality of cracks 17 accurately along each of the plurality of imaginary surfaces 15. Therefore, according to the laser processing method of the first embodiment, a plurality of GaN wafers 30 are obtained from the GaN ingot 20 with each of the plurality of cracks 17 as a boundary, thereby making it possible to obtain a plurality of suitable GaN wafers 30.
[0045] Similarly, according to the laser processing apparatus 1 that performs the laser processing method of the first embodiment, it is possible to form the cracks 17 accurately along each of the multiple imaginary surfaces 15, making it possible to obtain multiple suitable GaN wafers 30.
[0046] In the laser processing method of the first embodiment, the modified spots 13a are formed so that the cracks 14a extending from the modified spots 13a are not connected to each other. This makes it possible to form the modified spots 13b along the imaginary plane 15 with higher accuracy.
[0047] Moreover, in the laser processing method of the first embodiment, a plurality of rows of modified spots 13a are formed by moving the focal point C of the pulsed laser light L along the imaginary plane 15, and a plurality of rows of modified spots 13b are formed by moving the focal point C of the pulsed laser light L between the plurality of rows of modified spots 13a along the imaginary plane 15. This reliably prevents the plurality of modified spots 13b from overlapping with the plurality of modified spots 13a and the plurality of cracks 14a, and allows the plurality of modified spots 13b to be formed along the imaginary plane 15 with higher accuracy.
[0048] In particular, in the laser processing method of the first embodiment, when gallium nitride contained in the material of the GaN ingot 20 is decomposed by irradiation with the laser light L, gallium precipitates in the multiple cracks 14a extending from the multiple modified spots 13a, and the gallium becomes prone to absorb the laser light L. Therefore, forming the multiple modified spots 13b so as not to overlap the cracks 14a is effective in forming the multiple modified spots 13b along the imaginary plane 15 with high accuracy.
[0049] Moreover, in the laser processing method of the first embodiment, when gallium nitride contained in the material of the GaN ingot 20 is decomposed by irradiation with the laser light L, nitrogen gas is generated in the multiple cracks 14. Therefore, it is possible to easily form the cracks 17 by utilizing the pressure of the nitrogen gas.
[0050] Furthermore, according to the semiconductor component manufacturing method of the first embodiment, the steps included in the laser processing method of the first embodiment make it possible to form cracks 17 accurately along each of the multiple imaginary surfaces 15, thereby making it possible to obtain multiple preferable GaN wafers 30.
[0051] Moreover, in the semiconductor component manufacturing method of the first embodiment, the multiple imaginary planes 15 are set to be aligned in a direction facing the front surface 20a of the GaN ingot 20. This makes it possible to obtain multiple GaN wafers 30 from one GaN ingot 20.
[0052] Here, experimental results showing that in the GaN wafer 30 formed by the laser processing method and semiconductor article manufacturing method of the first embodiment, irregularities appearing on the peeled surface of the GaN wafer 30 are reduced will be described.
[0053] FIG. 14 is an image of the peeled surface of a GaN wafer formed by an example of the laser processing method and the semiconductor member manufacturing method, and (a) and (b) of FIG. 15 are height profiles of the peeled surface shown in FIG. 14. In this example, a laser beam L having a wavelength of 532 nm is incident on the inside of the GaN ingot 20 from the surface 20a of the GaN ingot 20, and one focal point C is relatively moved on the virtual surface 15 along the X direction to form a plurality of modified spots 13 along the virtual surface 15. At this time, the distance between adjacent focal points C in the Y direction is 10 μm, the pulse pitch of the laser beam L is 1 μm, and the pulse energy of the laser beam L is 1 μJ. In this case, as shown in (a) and (b) of FIG. 15, irregularities of about 25 μm appeared on the peeled surface (surface formed by the cracks 17) of the GaN wafer 30.
[0054] FIG. 16 is an image of the peeled surface of a GaN wafer formed by another example of the laser processing method and the semiconductor member manufacturing method, and (a) and (b) of FIG. 17 are height profiles of the peeled surface shown in FIG. 16. In this example, a laser beam L having a wavelength of 532 nm is incident on the inside of the GaN ingot 20 from the surface 20a of the GaN ingot 20, and a plurality of modified spots 13 are formed along the imaginary plane 15, similar to the first and second steps of the laser processing method and the semiconductor member manufacturing method of the first embodiment. When forming a plurality of modified spots 13a, the distance between adjacent focusing points C in the Y direction was set to 6 μm, the pulse pitch of the laser beam L was set to 10 μm, and the pulse energy of the laser beam L was set to 0.33 μJ. When forming a plurality of modified spots 13b, the distance between adjacent focusing points C in the Y direction was set to 6 μm, the pulse pitch of the laser beam L was set to 10 μm, and the pulse energy of the laser beam L was set to 0.33 μJ. When forming the multiple modified spots 13c, the distance between adjacent focusing points C in the Y direction was 6 μm, the pulse pitch of the laser light L was 5 μm, and the pulse energy of the laser light L was 0.33 μJ. When forming the multiple modified spots 13d, the distance between adjacent focusing points C in the Y direction was 6 μm, the pulse pitch of the laser light L was 5 μm, and the pulse energy of the laser light L was 0.33 μJ. In this case, as shown in (a) and (b) of FIG. 17, irregularities of about 5 μm appeared on the peeled surface of the GaN wafer 30.
[0055] From the above experimental results, it was found that in the GaN wafer formed by the laser processing method and the semiconductor component manufacturing method of the first embodiment, the unevenness appearing on the peeled surface of the GaN wafer 30 is reduced, that is, the cracks 17 are formed accurately along the imaginary plane 15. When the unevenness appearing on the peeled surface of the GaN wafer 30 is reduced, the amount of grinding required to flatten the peeled surface is reduced. Therefore, reducing the unevenness appearing on the peeled surface of the GaN wafer 30 is advantageous in terms of both material utilization efficiency and production efficiency.
[0056] Next, the principle behind the appearance of irregularities on the peeled surface of the GaN wafer 30 will be described.
[0057] For example, as shown in FIG. 18, a plurality of modified spots 13a are formed along the imaginary surface 15, and a plurality of modified spots 13b are formed along the imaginary surface 15 so that the modified spots 13b overlap the cracks 14a extending from the modified spots 13a on one side. In this case, since the laser light L is easily absorbed by the gallium precipitated in the plurality of cracks 14a, even if the focal point C is located on the imaginary surface 15, the modified spots 13b are easily formed on the incident side of the laser light L with respect to the modified spots 13a. Next, a plurality of modified spots 13c are formed along the imaginary surface 15 so that the modified spots 13c overlap the cracks 14b extending from the modified spots 13b on one side. In this case, since the laser light L is easily absorbed by the gallium precipitated in the plurality of cracks 14b, even if the focal point C is located on the imaginary surface 15, the modified spots 13c are easily formed on the incident side of the laser light L with respect to the modified spots 13b. Thus, in this example, multiple modified spots 13b are formed on the incident side of the laser light L relative to the multiple modified spots 13a, and further, multiple modified spots 13c are easily formed on the incident side of the laser light L relative to the multiple modified spots 13b.
[0058] In contrast, for example, as shown in FIG. 19, a plurality of modified spots 13a are formed along the imaginary surface 15, and a plurality of modified spots 13b are formed along the imaginary surface 15 so that the modified spots 13b do not overlap the cracks 14a extending from the modified spots 13a on both sides. In this case, although the laser light L is easily absorbed by the gallium precipitated in the plurality of cracks 14a, the modified spots 13b do not overlap the cracks 14a, so that the modified spots 13b are also formed on the imaginary surface 15 in the same manner as the modified spots 13a. Next, a plurality of modified spots 13c are formed along the imaginary surface 15 so that the modified spot 13c overlaps the cracks 14a, 14b extending from the modified spots 13a, 13b on both sides. Furthermore, a plurality of modified spots 13d are formed along the imaginary surface 15 so that the modified spot 13d overlaps the cracks 14a, 14b extending from the modified spots 13a, 13b on both sides. In these cases, the laser light L is easily absorbed by the gallium precipitated in the cracks 14a, 14b, so that the modified spots 13c, 13d are easily formed on the incident side of the laser light L relative to the modified spots 13a, 13b even if the focal point C is located on the imaginary plane 15. Thus, in this example, the modified spots 13c, 13d are simply easily formed on the incident side of the laser light L relative to the modified spots 13a, 13b.
[0059] From the above principles, it can be seen that in the laser processing method and semiconductor component manufacturing method of the first embodiment, it is extremely important to form the multiple modified spots 13b so as not to overlap with the multiple modified spots 13a and the multiple cracks 14a extending from the multiple modified spots 13a, respectively, in order to reduce the unevenness that appears on the peeled surface of the GaN wafer 30.
[0060] Next, experimental results showing that in the laser processing method and semiconductor product manufacturing method of the first embodiment, the crack 17 advances along the imaginary plane 15 with good precision will be described.
[0061] (a) and (b) of FIG. 20 are images of a crack formed during an example of a laser processing method and a semiconductor member manufacturing method, and (b) of FIG. 20 is an enlarged image of a rectangular frame in (a) of FIG. 20. In this example, a laser beam L having a wavelength of 532 nm is incident on the inside of the GaN ingot 20 from the surface 20a of the GaN ingot 20, and six focal points C arranged in the Y direction are relatively moved on the virtual surface 15 along the X direction to form a plurality of modified spots 13 along the virtual surface 15. At this time, the distance between adjacent focal points C in the Y direction is 6 μm, the pulse pitch of the laser beam L is 1 μm, and the pulse energy of the laser beam L is 1.33 μJ. Then, the laser processing is stopped halfway along the virtual surface 15. In this case, as shown in (a) and (b) of FIG. 20, the crack that has progressed from the processed region to the unprocessed region is largely deviated from the virtual surface 15 in the unprocessed region.
[0062] 21(a) and (b) are images of cracks formed during another example of the laser processing method and the semiconductor member manufacturing method, and FIG. 21(b) is an enlarged image of the rectangular frame in FIG. 21(a). In this example, a laser beam L having a wavelength of 532 nm is incident on the inside of the GaN ingot 20 from the surface 20a of the GaN ingot 20, and six focal points C arranged in the Y direction are relatively moved on the virtual plane 15 along the X direction to form a plurality of modified spots 13 along the virtual plane 15. Specifically, first, a distance between adjacent focal points C in the Y direction is set to 6 μm, the pulse pitch of the laser beam L is set to 10 μm, and the pulse energy of the laser beam L is set to 0.33 μJ, and a plurality of rows of modified spots 13 are formed in the processing region 1 and the processing region 2. Next, the distance between adjacent focus points C in the Y direction was set to 6 μm, the pulse pitch of the laser light L was set to 10 μm, and the pulse energy of the laser light L was set to 0.33 μJ, and multiple rows of modified spots 13 were formed in the processed area 1 and the processed area 2 so that each row was located at the center between the multiple rows of modified spots 13 already formed. Next, the distance between adjacent focus points C in the Y direction was set to 6 μm, the pulse pitch of the laser light L was set to 5 μm, and the pulse energy of the laser light L was set to 0.33 μJ, and multiple rows of modified spots 13 were formed only in the processed area 1 so that each row was located at the center between the multiple rows of modified spots 13 already formed. In this case, as shown in (a) and (b) of FIG. 21, the crack that progressed from the processed area 1 to the processed area 2 did not deviate significantly from the virtual plane 15 in the processed area 2.
[0063] From the above experimental results, it was found that in the laser processing method and the semiconductor component manufacturing method of the first embodiment, the crack 17 grows accurately along the virtual surface 15. This is presumably because the multiple modified spots 13 previously formed in the processing region 2 acted as a guide when the crack grew.
[0064] Next, experimental results showing that in the laser processing method and semiconductor product manufacturing method of the first embodiment, the extension amount of the crack 14 extending from the modified spot 13 to the incident side of the laser light L and the opposite side are suppressed will be described.
[0065] 22 is an image (side view image) of a modified spot and a crack formed by a laser processing method and a semiconductor member manufacturing method of a comparative example. In this comparative example, a laser beam L having a wavelength of 532 nm is incident on the inside of the GaN ingot 20 from the surface 20a of the GaN ingot 20, and one focal point C is relatively moved on the virtual surface 15 along the X direction to form a plurality of modified spots 13 along the virtual surface 15. Specifically, the distance between adjacent focal points C in the Y direction is 2 μm, the pulse pitch of the laser beam L is 5 μm, and the pulse energy of the laser beam L is 0.3 μJ, and a plurality of modified spots 13 are formed along the virtual surface 15. In this case, as shown in FIG. 22, the extension amount of the crack 14 extending from the modified spot 13 to the incident side of the laser beam L and the opposite side is about 100 μm.
[0066] 23 is an image of the modified spots and cracks formed by the laser processing method and the semiconductor member manufacturing method of the first embodiment, where (a) of FIG. 23 is an image in plan view, and (b) of FIG. 23 is an image in side view. In this first embodiment, a laser beam L having a wavelength of 532 nm is incident on the inside of the GaN ingot 20 from the surface 20a of the GaN ingot 20, and six focal points C arranged in the Y direction are relatively moved on the virtual surface 15 along the X direction to form a plurality of modified spots 13 along the virtual surface 15. Specifically, first, a distance between adjacent focal points C in the Y direction is set to 8 μm, the pulse pitch of the laser beam L is set to 10 μm, and the pulse energy of the laser beam L is set to 0.3 μJ, and a plurality of modified spots 13a is formed along the virtual surface 15. Next, in a state where the six focal points C arranged in the Y direction were shifted by +4 μm in the Y direction from the previous state, the distance between adjacent focal points C in the Y direction was 8 μm, the pulse pitch of the laser light L was 10 μm, and the pulse energy of the laser light L was 0.3 μJ, and multiple modified spots 13b were formed along the virtual surface 15. Next, in a state where the six focal points C arranged in the Y direction were shifted by -4 μm in the Y direction from the previous state, the distance between adjacent focal points C in the Y direction was 8 μm, the pulse pitch of the laser light L was 5 μm, and the pulse energy of the laser light L was 0.3 μJ, and multiple modified spots 13 were formed along the virtual surface 15. Next, in a state where the six focal points C arranged in the Y direction were shifted in the Y direction by +4 μm from the previous state, the distance between adjacent focal points C in the Y direction was 8 μm, the pulse pitch of the laser light L was 5 μm, and the pulse energy of the laser light L was 0.3 μJ, and multiple modified spots 13 were formed along the imaginary plane 15. As a result, it is assumed that the modified spot 13a formed in the first time and the modified spot 13 formed in the third time overlap each other, and the modified spot 13b formed in the second time and the modified spot 13 formed in the fourth time overlap each other. In this case, as shown in (b) of FIG. 23, the extension amount of the crack 14 extending from the modified spot 13 to the incident side of the laser light L and the opposite side was about 70 μm.
[0067] 24(a) and (b) are images of modified spots and cracks formed by the laser processing method and semiconductor member manufacturing method of the second embodiment, where FIG. 24(a) is an image in plan view and FIG. 24(b) is an image in side view. In this second embodiment, a laser beam L having a wavelength of 532 nm is incident on the inside of the GaN ingot 20 from the surface 20a of the GaN ingot 20, and multiple modified spots 13 are formed along the imaginary plane 15 in the same manner as in the first and second steps of the laser processing method and semiconductor member manufacturing method of the first embodiment. When multiple modified spots 13a are formed, the distance between adjacent focusing points C in the Y direction is 8 μm, the pulse pitch of the laser beam L is 10 μm, and the pulse energy of the laser beam L is 0.3 μJ. When multiple modified spots 13b are formed, the distance between adjacent focusing points C in the Y direction is 8 μm, the pulse pitch of the laser beam L is 10 μm, and the pulse energy of the laser beam L is 0.3 μJ. When forming the multiple modified spots 13c, the distance between adjacent focusing points C in the Y direction was 8 μm, the pulse pitch of the laser light L was 5 μm, and the pulse energy of the laser light L was 0.3 μJ. When forming the multiple modified spots 13d, the distance between adjacent focusing points C in the Y direction was 8 μm, the pulse pitch of the laser light L was 5 μm, and the pulse energy of the laser light L was 0.3 μJ. In this case, as shown in (b) of FIG. 24, the extension amount of the crack 14 extending from the modified spot 13 to the incident side of the laser light L and the opposite side was about 50 μm.
[0068] (c) and (d) of FIG. 24 are images of modified spots and cracks formed by the laser processing method and the semiconductor member manufacturing method of the third embodiment, where (c) of FIG. 24 is an image in plan view, and (d) of FIG. 24 is an image in side view. In this third embodiment, a plurality of modified spots 13 were further formed along the imaginary surface 15 (i.e., the imaginary surface 15 on which a plurality of rows of modified spots 13 have already been formed) in the state shown in (a) and (b) of FIG. 24. Specifically, first, the distance between adjacent focusing points C in the Y direction was 8 μm, the pulse pitch of the laser light L was 5 μm, and the pulse energy of the laser light L was 0.1 μJ, and a plurality of rows of modified spots 13 were formed so that each row was located at the center between the rows of the already formed rows of modified spots 13. In this case, as shown in (d) of FIG. 24, the extension amount of the crack 14 extending from the modified spot 13 to the incident side of the laser light L and the opposite side was about 60 μm.
[0069] From the above experimental results, it was found that if multiple modified spots 13b are formed along the imaginary surface 15 so as not to overlap with multiple modified spots 13a and multiple cracks 14a already formed along the imaginary surface 15 (first, second and third examples), the extension amount of the crack 14 extending from the modified spot 13 to the incident side of the laser light L and the opposite side can be suppressed. Note that when multiple modified spots 13 are further formed along the imaginary surface 15, if multiple modified spots 13 are formed along the imaginary surface 15 so as not to overlap with multiple modified spots 13a, 13b already formed along the imaginary surface 15 (second and third examples), it becomes easier to form a crack across the imaginary surface 15. [Laser processing method and semiconductor member manufacturing method according to the second embodiment]
[0070] The object 11 in the laser processing method and semiconductor product manufacturing method of the second embodiment is a GaN wafer (semiconductor wafer, semiconductor object) 30 formed of GaN, for example, in a disk shape, as shown in FIG. 25. As an example, the diameter of the GaN wafer 30 is 2 in, and the thickness of the GaN wafer 30 is 100 μm. The laser processing method and semiconductor product manufacturing method of the second embodiment are performed to cut out a plurality of semiconductor devices (semiconductor products) 40 from the GaN wafer 30. As an example, the outer shape of the GaN substrate portion of the semiconductor device 40 is 1 mm×1 mm, and the thickness of the GaN substrate portion of the semiconductor device 40 is several tens of μm.
[0071] First, the above-mentioned laser processing device 1 forms a plurality of modified spots 13 along each of the plurality of imaginary surfaces 15. Each of the plurality of imaginary surfaces 15 is a surface facing the surface 30a of the GaN wafer 30 inside the GaN wafer 30, and is set to be aligned in the direction in which the surface 30a extends. In this embodiment, each of the plurality of imaginary surfaces 15 is a surface parallel to the surface 30a, and has, for example, a rectangular shape. Each of the plurality of imaginary surfaces 15 is set to be aligned two-dimensionally in a direction parallel to and perpendicular to the orientation flat 31 of the GaN wafer 30. A plurality of peripheral regions 16 are set in the GaN wafer 30 so as to surround each of the plurality of imaginary surfaces 15. That is, each of the plurality of imaginary surfaces 15 does not reach the side surface 30b of the GaN wafer 30. As an example, the width of the peripheral region 16 corresponding to each of the plurality of imaginary surfaces 15 (in this embodiment, half the distance between adjacent imaginary surfaces 15) is 30 μm or more.
[0072] The formation of the multiple modified spots 13 along each of the multiple imaginary surfaces 15 is performed in the same manner as the first and second steps of the laser processing method and the semiconductor component manufacturing method of the first embodiment. As a result, in the GaN wafer 30, multiple modified spots 13 (i.e., modified spots 13a, 13b, 13c, and 13d) and multiple cracks 14 (i.e., cracks 14a, 14b, 14c, and 14d) are formed along each of the multiple imaginary surfaces 15, as shown in Fig. 26. In Fig. 26, the ranges in which the multiple modified spots 13 and multiple cracks 14 are formed are indicated by dashed lines.
[0073] Next, the semiconductor manufacturing equipment forms a plurality of functional elements 32 on the surface 30a of the GaN wafer 30, as shown in Fig. 27. Each of the plurality of functional elements 32 is formed so that one functional element 32 is included in one imaginary plane 15 when viewed from the thickness direction of the GaN wafer 30. The functional elements 32 are, for example, light receiving elements such as photodiodes, light emitting elements such as laser diodes, circuit elements such as memories, etc.
[0074] In this embodiment, when forming a plurality of functional elements 32 on the surface 30a, the semiconductor manufacturing apparatus functions as a heating apparatus. That is, when forming a plurality of functional elements 32 on the surface 30a, the semiconductor manufacturing apparatus heats the GaN wafer 30, and connects a plurality of cracks 14 extending from a plurality of modified spots 13 on each of the plurality of imaginary surfaces 15 to each other, thereby forming a crack 17 (i.e., a crack 17 across the imaginary surface 15) on each of the plurality of imaginary surfaces 15. In FIG. 27, the plurality of modified spots 13 and the plurality of cracks 14, and the range in which the crack 17 is formed, are shown by dashed lines. Note that a heating apparatus other than the semiconductor manufacturing apparatus may be used. Also, the plurality of cracks 14 may be connected to each other to form the crack 17 by applying some force to the GaN wafer 30 by a method other than heating. Also, the plurality of cracks 14 may be connected to each other to form the crack 17 by forming a plurality of modified spots 13 along the imaginary surface 15.
[0075] Here, in the GaN wafer 30, nitrogen gas is generated in the multiple cracks 14 extending from the multiple modified spots 13. Therefore, by heating the GaN ingot 20 to expand the nitrogen gas, the cracks 17 can be formed by utilizing the pressure of the nitrogen gas. Moreover, the peripheral region 16 prevents the multiple cracks 14 from progressing to the outside of the virtual surface 15 surrounded by the peripheral region 16 (for example, the adjacent virtual surface 15, the side surface 30b of the GaN wafer 30), so that the nitrogen gas generated in the multiple cracks 14 can be prevented from escaping to the outside of the virtual surface 15. In other words, the peripheral region 16 is a non-modified region that does not include the modified spots 13, and is a region that prevents the multiple cracks 14 from progressing to the outside of the virtual surface 15 surrounded by the peripheral region 16 when the cracks 17 are formed in the virtual surface 15 surrounded by the peripheral region 16. For this reason, it is preferable to set the width of the peripheral region 16 to 30 μm or more.
[0076] Next, the laser processing device cuts the GaN wafer 30 into individual functional elements 32, and the grinding device grinds the portions corresponding to the multiple imaginary planes 15, thereby obtaining multiple semiconductor devices 40 from the GaN wafer 30 with the multiple cracks 17 as boundaries, as shown in Fig. 28 (third step). In this manner, the GaN wafer 30 is cut along the multiple imaginary planes 15. Note that in this step, the GaN wafer 30 may be cut into individual functional elements 32 by mechanical processing other than laser processing (e.g., blade dicing), etc.
[0077] Of the above steps, the laser processing method of the second embodiment includes the steps up to the step of forming a plurality of modified spots 13 along each of the plurality of imaginary planes 15. Also, of the above steps, the semiconductor component manufacturing method of the second embodiment includes the steps up to the step of obtaining a plurality of semiconductor devices 40 from the GaN wafer 30 with each of the plurality of cracks 17 as boundaries.
[0078] As described above, according to the laser processing method of the second embodiment, similarly to the laser processing method of the first embodiment, a plurality of modified spots 13 can be formed along each of the plurality of imaginary planes 15 with high precision, and as a result, it becomes possible to form the cracks 17 along each of the plurality of imaginary planes 15 with high precision. Therefore, according to the laser processing method of the second embodiment, by obtaining a plurality of semiconductor devices 40 from the GaN wafer 30 with each of the plurality of cracks 17 as a boundary, it becomes possible to obtain a plurality of suitable semiconductor devices 40. In addition, it becomes possible to reuse the GaN wafer 30 after the plurality of semiconductor devices 40 have been cut out.
[0079] Similarly, according to the laser processing apparatus 1 that performs the laser processing method of the second embodiment, it is possible to accurately form cracks 17 along each of the multiple virtual surfaces 15, making it possible to obtain multiple preferable semiconductor devices 40.
[0080] In the laser processing method of the second embodiment, the modified spots 13a are formed so that the cracks 14a extending from the modified spots 13a are not connected to each other. This makes it possible to form the modified spots 13b along the imaginary plane 15 with higher accuracy.
[0081] In the laser processing method of the second embodiment, a plurality of rows of modified spots 13a are formed by moving the focal point C of the pulsed laser light L along the imaginary plane 15, and a plurality of rows of modified spots 13b are formed by moving the focal point C of the pulsed laser light L between the plurality of rows of modified spots 13a along the imaginary plane 15. This reliably prevents the plurality of modified spots 13b from overlapping with the plurality of modified spots 13a and the plurality of cracks 14a, and allows the plurality of modified spots 13b to be formed along the imaginary plane 15 with higher accuracy.
[0082] In particular, in the laser processing method of the second embodiment, when gallium nitride contained in the material of the GaN wafer 30 is decomposed by irradiation with the laser light L, gallium precipitates in the multiple cracks 14a extending from the multiple modified spots 13a, and the gallium becomes prone to absorb the laser light L. Therefore, forming the multiple modified spots 13b so as not to overlap the cracks 14a is effective in forming the multiple modified spots 13b along the virtual plane 15 with high accuracy.
[0083] Moreover, in the laser processing method of the second embodiment, when gallium nitride contained in the material of the GaN wafer 30 is decomposed by irradiation with the laser light L, nitrogen gas is generated in the multiple cracks 14. Therefore, it becomes possible to easily form the cracks 17 by utilizing the pressure of the nitrogen gas.
[0084] Furthermore, according to the semiconductor component manufacturing method of the second embodiment, the steps included in the laser processing method of the second embodiment make it possible to accurately form cracks 17 along each of the multiple imaginary surfaces 15, thereby making it possible to obtain multiple preferable semiconductor devices 40.
[0085] In the semiconductor article manufacturing method of the second embodiment, the multiple imaginary planes 15 are set to be aligned in the direction in which the front surface 30a of the GaN wafer 30 extends. This makes it possible to obtain multiple semiconductor devices 40 from one GaN wafer 30. [Variations]
[0086] The present disclosure is not limited to the above-mentioned embodiment. For example, various values related to the laser light L are not limited to those described above. However, in order to suppress the crack 14 from extending from the modified spot 13 to the incident side of the laser light L and the opposite side, it is preferable that the pulse energy of the laser light L is 0.1 μJ to 1 μJ and the pulse width of the laser light L is 200 fs to 1 ns.
[0087] Furthermore, the semiconductor object processed by the laser processing method and the semiconductor product manufacturing method according to one aspect of the present disclosure is not limited to the GaN ingot 20 of the first embodiment and the GaN wafer 30 of the second embodiment. The semiconductor product manufactured by the semiconductor product manufacturing method according to one aspect of the present disclosure is not limited to the GaN wafer 30 of the first embodiment and the semiconductor device 40 of the second embodiment. One virtual plane may be set for one semiconductor object.
[0088] As an example, the material of the semiconductor object may be SiC. In that case, too, according to the laser processing method and the semiconductor member manufacturing method of one aspect of the present disclosure, it is possible to form a crack that spans the virtual surface along the virtual surface with high accuracy, as described below.
[0089] (a) and (b) of FIG. 29 are images (side view images) of cracks in a SiC wafer formed by the laser processing method and the semiconductor member manufacturing method of the comparative example, and (b) of FIG. 29 is an enlarged image of the rectangular frame in (a) of FIG. 29. In this comparative example, a laser beam having a wavelength of 532 nm is incident from the surface of the SiC wafer to the inside of the SiC wafer, and six focusing points arranged in the Y direction are relatively moved on the virtual plane along the X direction to form a plurality of modified spots along the virtual plane. At this time, the distance between adjacent focusing points C in the Y direction is 2 μm, the pulse pitch of the laser beam is 15 μm, and the pulse energy of the laser beam is 4 μJ. In this case, as shown in (a) and (b) of FIG. 29, a crack extending in a direction inclined by 4° to 5° with respect to the virtual plane is generated.
[0090] (a) and (b) of FIG. 30 are images (side view images) of cracks in a SiC wafer formed by the laser processing method and the semiconductor member manufacturing method of the embodiment, and (b) of FIG. 30 is an enlarged image of the rectangular frame in (a) of FIG. 30. In this embodiment, a laser beam having a wavelength of 532 nm is incident from the surface of the SiC wafer into the inside of the SiC wafer, and multiple modified spots are formed along the imaginary plane, similar to the first and second steps of the laser processing method and the semiconductor member manufacturing method of the first embodiment. When multiple modified spots corresponding to each of the multiple modified spots 13a, 13b, 13c, and 13d are formed, the distance between adjacent focusing points C in the Y direction is 8 μm, the pulse pitch of the laser beam L is 15 μm, and the pulse energy of the laser beam L is 4 μJ. In this case, as shown in (a) and (b) of FIG. 30, the occurrence of cracks extending in a direction inclined by 4° to 5° with respect to the imaginary plane is suppressed. Fig. 31 is an image of the peeled surface of a SiC wafer formed by the laser processing method and the semiconductor component manufacturing method of the embodiment, and Fig. 32(a) and (b) are the height profiles of the peeled surface shown in Fig. 31. In this case, the unevenness appearing on the peeled surface of the SiC wafer was suppressed to about 2 µm.
[0091] From the above experimental results, it was found that even when the material of the semiconductor object is SiC, according to the laser processing method and the semiconductor component manufacturing method of one aspect of the present disclosure, a crack spanning the virtual surface is formed along the virtual surface with good accuracy. Note that the SiC wafer used in the above-mentioned comparative example and example is a 4H-SiC wafer having an off-angle of 4±0.5°, and the direction in which the focal point of the laser light was moved is the m-axis direction.
[0092] In addition, the method of forming the multiple modified spots 13a, 13b, 13c, and 13d is not limited to the above. The multiple modified spots 13a may be formed so that the multiple cracks 14a extending from the multiple modified spots 13a are connected to each other. In addition, the multiple modified spots 13b may be formed so as not to overlap the multiple modified spots 13a. Even if the multiple modified spots 13b overlap the multiple cracks 14a extending from the multiple modified spots 13a, as long as the multiple modified spots 13b do not overlap the multiple modified spots 13a, the multiple modified spots 13a and 13b are formed with high accuracy along the virtual surface 15. In addition, the method of forming the multiple modified spots 13c and 13d is arbitrary, and the multiple modified spots 13c and 13d may not be formed. Furthermore, as shown in Figure 33, for example, by rotating the GaN ingot 20, multiple radially arranged focal points can be rotated relatively (dotted arrow) to form multiple rows of modified spots 13, and further, as shown in Figure 34, multiple radially arranged focal points can be rotated relatively (dotted arrow) while each of the multiple focal points is positioned between the multiple rows of modified spots 13 to form multiple rows of modified spots 13.
[0093] Furthermore, in the laser processing method and semiconductor component manufacturing method of the first embodiment, the formation of the multiple modified spots 13 may be performed sequentially for each of the multiple imaginary faces 15 from the side opposite to the surface 20a. Furthermore, in the laser processing method and semiconductor component manufacturing method of the first embodiment, the formation of the multiple modified spots 13 may be performed along one or more imaginary faces 15 on the surface 20a side, and after one or more GaN wafers 30 are cut out, the surface 20a of the GaN ingot 20 may be ground, and the formation of the multiple modified spots 13 may be performed again along one or more imaginary faces 15 on the surface 20a side.
[0094] Furthermore, in the laser processing method and the semiconductor product manufacturing method of the first and second embodiments, the peripheral region 16 may not be formed. When the peripheral region 16 is not formed in the laser processing method and the semiconductor product manufacturing method of the first embodiment, it is also possible to obtain a plurality of GaN wafers 30 by forming a plurality of modified spots 13 along each of the plurality of imaginary planes 15, and then, for example, etching the GaN ingot 20.
[0095] Furthermore, the laser processing apparatus 1 is not limited to the above-mentioned configuration. For example, the laser processing apparatus 1 does not have to include the spatial light modulator 4.
[0096] Furthermore, the respective components in the above-described embodiments are not limited to the materials and shapes described above, and various materials and shapes can be applied. Furthermore, the respective components in one embodiment or modified example described above can be arbitrarily applied to the respective components in other embodiments or modified examples. [Explanation of symbols]
[0097] 1...laser processing apparatus, 2...stage, 4...spatial light modulator (laser irradiation unit), 5...focusing lens (laser irradiation unit), 13...modified spot, 13a...modified spot (first modified spot), 13b...modified spot (second modified spot), 13c, 13d...modified spot (third modified spot), 14, 14a, 14b, 14c, 14d...crack, 15...virtual surface, 17...crack across virtual surface, 20...GaN ingot (semiconductor ingot, semiconductor object), 20a...surface, 30...GaN wafer (semiconductor wafer, semiconductor member, semiconductor object), 30a...surface, 40...semiconductor device (semiconductor member), L...laser light.
Claims
1. 1. A laser processing method for cutting a semiconductor object along an imaginary plane inside the semiconductor object facing a surface of the semiconductor object, comprising: A first step of forming a plurality of first modified spots along the imaginary plane by irradiating laser light from the surface into the interior of the semiconductor object to form a plurality of rows of first modified spots; A second step of forming a plurality of second modified spots along the imaginary plane so as not to overlap the plurality of first modified spots by irradiating laser light into the interior of the semiconductor object from the surface, and forming a plurality of rows of second modified spots each located between the plurality of rows of first modified spots, In the first step, the laser beam is focused at a plurality of first focusing points, and the plurality of first focusing points are relatively moved along a direction intersecting a direction in which the plurality of first focusing points are arranged, In the second step, the laser processing method includes focusing the laser light at a plurality of second focal points each located between the rows of the first modification spots, and relatively moving the plurality of second focal points along a direction intersecting the direction in which the plurality of second focal points are arranged.
2. The laser processing method according to claim 1 , wherein in the second step, the second modified spots are formed along the imaginary plane so as not to overlap with a plurality of cracks respectively extending from the plurality of first modified spots.
3. 3. The laser processing method of claim 1 or 2, wherein in the second step, after forming the plurality of second modified spots, laser light is incident from the surface into the interior of the semiconductor object to form a plurality of third modified spots along the virtual plane so as not to overlap the plurality of first modified spots and the plurality of second modified spots.
4. A laser processing method according to any one of claims 1 to 3, wherein in the first step, the plurality of first modified spots are formed so that the plurality of cracks extending from the plurality of first modified spots respectively do not connect to each other.
5. In the first step, a focal point of the pulsed laser light is moved along the virtual plane to form the first modified spots in the plurality of rows, The laser processing method according to any one of claims 1 to 4, wherein in the second step, the plurality of rows of second modified spots are formed by moving a focal point of the pulsed laser light along the virtual plane between the plurality of rows of first modified spots.
6. The laser processing method according to any one of claims 1 to 5, wherein a material of the semiconductor object contains gallium.
7. The laser processing method of claim 6 , wherein the material of the semiconductor object comprises gallium nitride.
8. The first step and the second step of the laser processing method according to any one of claims 1 to 7, A third step of obtaining a semiconductor component from the semiconductor object using a crack that crosses the imaginary surface as a boundary.
9. The method for manufacturing a semiconductor article according to claim 8 , wherein a plurality of the imaginary faces are set so as to be aligned in a direction facing the front surface.
10. the semiconductor object is a semiconductor ingot; The method for producing a semiconductor article according to claim 9 , wherein the semiconductor article is a semiconductor wafer.
11. The method for manufacturing a semiconductor article according to claim 8 , wherein a plurality of the imaginary surfaces are set so as to be aligned in a direction in which the surface extends.
12. the semiconductor object is a semiconductor wafer; The method for producing a semiconductor article according to claim 11, wherein the semiconductor article is a semiconductor device.
13. 1. A laser processing apparatus for cutting a semiconductor object along a virtual plane facing a surface of the semiconductor object within the semiconductor object, comprising: a stage for supporting the semiconductor workpiece; a laser irradiation unit that forms a plurality of first modified spots and a plurality of second modified spots along the virtual plane by irradiating laser light from the surface into the inside of the semiconductor object; The laser irradiation unit includes: forming the plurality of first modified spots along the imaginary surface, forming a plurality of rows of first modified spots; after forming the plurality of first modified spots, forming the plurality of second modified spots along the imaginary surface so as not to overlap the plurality of first modified spots; forming a plurality of rows of second modified spots each located between the plurality of rows of first modified spots; When forming the plurality of first modified spots, the laser light is focused on a plurality of first focusing points, and the plurality of first focusing points are relatively moved along a direction intersecting a direction in which the plurality of first focusing points are arranged, A laser processing apparatus, in which, when forming the plurality of second modified spots, the laser light is focused at a plurality of second focal points each located between the plurality of rows of first modified spots, and the plurality of second focal points are moved relatively along a direction intersecting the direction in which the plurality of second focal points are arranged.
Citation Information
Patent Citations
Separation method for element formed on substrate
JP2004259846A
Substrate processing device and substrate processing method
JP2015123466A
Formation method of gallium nitride substrate
JP2017057103A
Semiconductor element manufacturing method