Laser processing method, semiconductor component manufacturing method, and laser processing device
The laser processing method forms first and second modification spots with varying densities to control crack extension, addressing precision issues in semiconductor member separation and producing high-quality semiconductor components.
Patent Information
- Application Number
- JP2020561496
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-12-21
- Filing Date
- 2019-12-18
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2039-12-18
AI Technical Summary
The formation of modified regions in semiconductor processing methods influences the state of obtained semiconductor members, leading to inconsistent crack formation and precision issues during member separation.
A laser processing method involving the formation of first and second modification spots along a virtual plane with varying densities to control crack extension, ensuring precise alignment and connection of cracks across the virtual plane.
This method enables the production of high-precision semiconductor members by accurately forming cracks along the virtual plane, enhancing the quality and consistency of semiconductor components.
Smart Images

Figure 0007560056000001 
Figure 0007560056000002 
Figure 0007560056000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a laser processing method, a semiconductor component manufacturing method, and a laser processing apparatus. [Background technology]
[0002] There is known a processing method in which a semiconductor object such as a semiconductor ingot is irradiated with laser light to form a modified region inside the semiconductor object, and a crack extending from the modified region is propagated, thereby cutting out a semiconductor component such as a semiconductor wafer from the semiconductor object (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-183600 A [Patent Document 2] JP 2017-057103 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the above-mentioned processing method, the manner in which the modified region is formed significantly affects the state of the resulting semiconductor article.
[0005] An object of the present disclosure is to provide a laser processing method, a semiconductor component manufacturing method, and a laser processing apparatus that enable the production of suitable semiconductor components. [Means for solving the problem]
[0006] A laser processing method according to one aspect of the present disclosure is a laser processing method for cutting a semiconductor object along a virtual plane inside the semiconductor object that faces a surface of the semiconductor object, and includes a first step of forming a plurality of first modified spots along the virtual plane at a first formation density by directing laser light into the interior of the semiconductor object from the surface, and a second step of forming a plurality of second modified spots along the virtual plane after the first step at a second formation density higher than the first formation density by directing laser light into the interior of the semiconductor object from the surface.
[0007] In this laser processing method, a plurality of first modified spots are formed along an imaginary surface to have a first formation density, and then a plurality of second modified spots are formed along the imaginary surface to have a second formation density higher than the first formation density. This makes it possible to suppress the extension width of a plurality of cracks extending from the plurality of second modified spots in a direction perpendicular to the imaginary surface, and as a result, it becomes possible to form a crack across the imaginary surface with high accuracy. Therefore, according to this laser processing method, a semiconductor component is obtained from a semiconductor object with the crack across the imaginary surface as a boundary, thereby making it possible to obtain a suitable semiconductor component.
[0008] In the laser processing method according to one aspect of the present disclosure, in the first step, a plurality of first modified spots may be formed so that a plurality of cracks extending from the plurality of first modified spots are not connected to each other. This makes it possible to suppress the extension width of the plurality of cracks extending from the plurality of first modified spots in a direction perpendicular to the imaginary surface, and as a result, it becomes possible to form the cracks spanning the imaginary surface along the imaginary surface with higher accuracy.
[0009] In the laser processing method according to one aspect of the present disclosure, in the second step, a plurality of second modification spots may be formed so that a plurality of cracks extending from the plurality of second modification spots are connected to each other. This makes it possible to reliably suppress the extension width of the plurality of cracks extending from the plurality of second modification spots in a direction perpendicular to the imaginary surface, and as a result, it becomes possible to more accurately form cracks spanning the imaginary surface along the imaginary surface.
[0010] In the laser processing method according to one aspect of the present disclosure, in the second step, a plurality of second modification spots may be formed so that the plurality of second modification spots are connected to each other. This makes it possible to reliably suppress the extension width of a plurality of cracks extending from the plurality of second modification spots in a direction perpendicular to the imaginary surface, and as a result, it becomes possible to more accurately form a crack spanning the imaginary surface along the imaginary surface.
[0011] In the laser processing method according to one aspect of the present disclosure, in the first step, a focus point of the pulsed laser light is moved along the imaginary surface at a first pulse pitch to form a plurality of first modified spots, and in the second step, a focus point of the pulsed laser light is moved along the imaginary surface at a second pulse pitch smaller than the first pulse pitch to form a plurality of second modified spots. This makes it possible to reliably suppress the extension width in the direction perpendicular to the imaginary surface of the plurality of cracks extending from the plurality of second modified spots, respectively, and as a result, it becomes possible to more accurately form cracks spanning the imaginary surface along the imaginary surface.
[0012] In the laser processing method according to one aspect of the present disclosure, the material of the semiconductor object may contain gallium. In this case, when gallium is precipitated in the cracks extending from the first modified spots by irradiation with the laser light, the gallium is likely to absorb the laser light. Therefore, adjusting the formation of the first modified spots and the formation of the second modified spots is effective in forming the cracks across the virtual surface along the virtual surface with high accuracy.
[0013] In the laser processing method according to one aspect of the present disclosure, the material of the semiconductor object may include gallium nitride. In this case, when the gallium nitride is decomposed by the irradiation of the laser light, gallium is precipitated in a plurality of cracks extending from the plurality of first modified spots, and the gallium is in a state in which the laser light is easily absorbed. Therefore, adjusting the formation of the plurality of first modified spots and the formation of the plurality of second modified spots is effective in forming the cracks across the virtual surface along the virtual surface with high accuracy. Furthermore, when the gallium nitride is decomposed by the irradiation of the laser light, nitrogen gas is generated in the plurality of cracks. Therefore, it is possible to easily form the cracks across the virtual surface by utilizing the pressure (internal pressure) of the nitrogen gas.
[0014] A semiconductor component manufacturing method according to one aspect of the present disclosure comprises the first and second steps of the laser processing method described above, and a third step of obtaining a semiconductor component from a semiconductor object using a crack spanning an imaginary surface as a boundary.
[0015] According to this semiconductor article manufacturing method, the first and second steps make it possible to form a crack spanning the imaginary surface along the imaginary surface with high precision, thereby making it possible to obtain a suitable semiconductor article.
[0016] In the semiconductor article manufacturing method according to one aspect of the present disclosure, a plurality of imaginary surfaces may be set so as to be aligned in a direction facing the front surface, which makes it possible to obtain a plurality of semiconductor articles from one semiconductor object.
[0017] In the semiconductor article manufacturing method according to one aspect of the present disclosure, the semiconductor object may be a semiconductor ingot and the semiconductor article may be a semiconductor wafer, thereby making it possible to obtain a plurality of suitable semiconductor wafers.
[0018] In the semiconductor article manufacturing method according to one aspect of the present disclosure, a plurality of imaginary surfaces may be set so as to be aligned in a direction in which the surface extends, which makes it possible to obtain a plurality of semiconductor articles from one semiconductor object.
[0019] In the semiconductor article manufacturing method according to one aspect of the present disclosure, the semiconductor object may be a semiconductor wafer and the semiconductor article may be a semiconductor device. This makes it possible to obtain a plurality of suitable semiconductor devices.
[0020] A laser processing apparatus according to one aspect of the present disclosure is a laser processing apparatus for cutting a semiconductor object along a virtual plane inside the semiconductor object that faces a surface of the semiconductor object, and includes a stage for supporting the semiconductor object, and a laser irradiation unit for forming a plurality of first modified spots and a plurality of second modified spots along the virtual surface by directing laser light into the interior of the semiconductor object from the surface, and forms the plurality of first modified spots along the virtual surface to have a first formation density, and after forming the plurality of first modified spots, forms a plurality of second modified spots along the imaginary surface to have a second formation density higher than the first formation density.
[0021] According to this laser processing device, it is possible to form a crack that spans the imaginary surface along the imaginary surface with high accuracy, so that a suitable semiconductor component can be obtained. Effect of the Invention
[0022] According to the present disclosure, it is possible to provide a laser processing method, a semiconductor component manufacturing method, and a laser processing apparatus that enable the production of suitable semiconductor components. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a configuration diagram of a laser processing device according to one embodiment. [Diagram 2] FIG. 2 is a side view of a GaN ingot that is a target of the laser processing method and the semiconductor product manufacturing method of the first embodiment. [Diagram 3] FIG. 3 is a plan view of the GaN ingot shown in FIG. [Figure 4] FIG. 4 is a vertical cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method according to the first embodiment. [Diagram 5]FIG. 5 is a cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method according to the first embodiment. [Figure 6] FIG. 6 is a vertical cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method according to the first embodiment. [Figure 7] FIG. 7 is a cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method according to the first embodiment. [Figure 8] FIG. 8 is a vertical cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method according to the first embodiment. [Figure 9] FIG. 9 is a cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method of the first embodiment. [Figure 10] FIG. 10 is a vertical cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method of the first embodiment. [Figure 11] FIG. 11 is a cross-sectional view of a portion of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method of the first embodiment. [Figure 12] FIG. 12 is a side view of a GaN ingot in a step of the laser processing method and the semiconductor product manufacturing method of the first embodiment. [Figure 13] FIG. 13 is a side view of a GaN wafer in a step of the laser processing method and the semiconductor article manufacturing method of the first embodiment. [Figure 14] FIG. 14 shows images of modified spots and cracks formed by the laser processing method and the semiconductor component manufacturing method of the embodiment. [Figure 15] FIG. 15 is a schematic diagram of modified spots and cracks formed in the second step of the laser processing method and the semiconductor article manufacturing method of the first embodiment. [Figure 16] FIG. 16 is a plan view of a GaN wafer which is an object of the laser processing method and the semiconductor article manufacturing method according to the second embodiment. [Figure 17]FIG. 17 is a side view of a part of a GaN wafer in a step of the laser processing method and semiconductor article manufacturing method of the second embodiment. [Figure 18] FIG. 18 is a side view of a part of a GaN wafer in a step of the laser processing method and semiconductor article manufacturing method of the second embodiment. [Figure 19] FIG. 19 is a side view of a semiconductor device in a step of the laser processing method and the semiconductor article manufacturing method of the second embodiment. [Figure 20] FIG. 20 is a plan view of a GaN ingot in a step of a laser processing method and a semiconductor product manufacturing method according to a modified example. [Figure 21] FIG. 21 is a plan view of a GaN ingot in a step of a laser processing method and a semiconductor product manufacturing method according to a modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings. In each drawing, the same or corresponding parts are denoted by the same reference numerals, and duplicated explanations will be omitted. [Laser processing equipment configuration]
[0025] 1, the laser processing apparatus 1 includes a stage 2, a light source 3, a spatial light modulator 4, a condenser lens 5, and a control unit 6. The laser processing apparatus 1 is an apparatus that forms a modified region 12 in an object 11 by irradiating the object 11 with laser light L. Hereinafter, the first horizontal direction is referred to as the X direction, and the second horizontal direction perpendicular to the first horizontal direction is referred to as the Y direction. In addition, the vertical direction is referred to as the Z direction.
[0026] The stage 2 supports the object 11, for example, by adsorbing a film attached to the object 11. In this embodiment, the stage 2 is movable along both the X direction and the Y direction. In addition, the stage 2 is rotatable about an axis parallel to the Z direction.
[0027] The light source 3 outputs laser light L having transparency to the object 11, for example, by a pulse oscillation method. The spatial light modulator 4 modulates the laser light L output from the light source 3. The spatial light modulator 4 is, for example, a reflective liquid crystal (LCOS: Liquid Crystal on Silicon) spatial light modulator (SLM: Spatial Light Modulator). The condenser lens 5 condenses the laser light L modulated by the spatial light modulator 4. In this embodiment, the spatial light modulator 4 and the condenser lens 5 are movable along the Z direction as a laser irradiation unit.
[0028] When the laser light L is focused inside the object 11 supported by the stage 2, the laser light L is particularly absorbed in a portion corresponding to the focusing point C of the laser light L, and a modified region 12 is formed inside the object 11. The modified region 12 is a region whose density, refractive index, mechanical strength, and other physical properties are different from those of the surrounding non-modified region. Examples of the modified region 12 include a melting treatment region, a crack region, a dielectric breakdown region, a refractive index change region, and the like.
[0029] As an example, when the stage 2 is moved along the X direction and the focal point C is moved along the X direction relative to the object 11, multiple modified spots 13 are formed in a row along the X direction. One modified spot 13 is formed by irradiating one pulse of laser light L. One row of modified regions 12 is a collection of multiple modified spots 13 lined up in a row. Adjacent modified spots 13 may be connected to each other or separated from each other depending on the relative moving speed of the focal point C with respect to the object 11 and the repetition frequency of the laser light L.
[0030] The control unit 6 controls the stage 2, the light source 3, the spatial light modulator 4, and the condenser lens 5. The control unit 6 is configured as a computer device including a processor, a memory, a storage, a communication device, etc. In the control unit 6, software (programs) loaded into the memory, etc. are executed by the processor, and the reading and writing of data in the memory and storage, as well as communication by the communication device, are controlled by the processor. In this way, the control unit 6 realizes various functions. [First embodiment of laser processing method and semiconductor member manufacturing method]
[0031] The object 11 in the laser processing method and the semiconductor member manufacturing method of the first embodiment is a GaN ingot (semiconductor ingot, semiconductor object) 20 shown in FIG. 2 and FIG. 3. The GaN ingot 20 is made of gallium nitride (GaN) and has, for example, a disk shape. As an example, the diameter of the GaN ingot 20 is 2 in, and the thickness of the GaN ingot 20 is 2 mm. A plurality of imaginary planes 15 are set in the GaN ingot 20. Each of the plurality of imaginary planes 15 is a surface facing the surface 20a of the GaN ingot 20 inside the GaN ingot 20, and is set to be aligned in a direction facing the surface 20a. As an example, each of the plurality of imaginary planes 15 is a surface parallel to the surface 20a, and has a circular shape. A plurality of peripheral regions 16 are set in the GaN ingot 20 so as to surround each of the plurality of imaginary planes 15. That is, each of the plurality of imaginary planes 15 does not reach the side surface 20b of the GaN ingot 20. As an example, the distance between adjacent imaginary faces 15 is 100 μm, and the width of peripheral region 16 (the distance between the outer edge of imaginary face 15 and side face 20b in the first embodiment) is 30 μm or more.
[0032] In the laser processing method and the semiconductor member manufacturing method of the first embodiment, the above-mentioned laser processing apparatus 1 is used to form a plurality of modified spots 13 along each of the plurality of imaginary planes 15. Specifically, the stage 2 supports the GaN ingot 20, and the laser irradiation unit composed of the spatial light modulator 4 and the condenser lens 5 irradiates the laser light L from the surface 20a into the inside of the GaN ingot 20 to form a plurality of modified spots 13 along each of the plurality of imaginary planes 15. In the semiconductor member manufacturing method of the first embodiment, the GaN ingot 20 is cut along each of the plurality of imaginary planes 15 to obtain a plurality of GaN wafers (semiconductor members) 30 from the GaN ingot 20. The GaN wafer 30 is made of GaN and has, for example, a disk shape. As an example, the diameter of the GaN wafer 30 is 2 in, and the thickness of the GaN wafer 30 is 100 μm.
[0033] The laser processing method and the semiconductor member manufacturing method of the first embodiment will be described in detail below. In the laser processing method and the semiconductor member manufacturing method of the first embodiment, the formation of the multiple modified spots 13 is performed sequentially for each imaginary surface 15 from the opposite side to the surface 20a by irradiation with laser light L having a wavelength of, for example, 532 nm. Since the formation of the multiple modified spots 13 is similar for each of the multiple imaginary surfaces 15, the formation of the multiple modified spots 13 along the imaginary surface 15 closest to the surface 20a will be described in detail below with reference to Figs. 4 to 11. Note that in Figs. 5, 7, 9 and 11, the arrows indicate the trajectory of the focal point C of the laser light L. In addition, the modified spots 13a, 13b, 13c, and 13d described later may be collectively referred to as the modified spots 13, and the cracks 14a, 14b, 14c, and 14d described later may be collectively referred to as the cracks 14.
[0034] First, as shown in Fig. 4 and Fig. 5, a laser beam L is incident on the inside of the GaN ingot 20 from the surface 20a to form a plurality of modified spots (first modified spots) 13a along the imaginary plane 15 (for example, arranged two-dimensionally along the entire imaginary plane 15) (first step). At this time, the modified spots 13a are formed so that the plurality of cracks 14a extending from the plurality of modified spots 13a are not connected to each other. In addition, the focal point C of the pulsed laser beam L is moved along the imaginary plane 15 to form a plurality of rows of modified spots 13a. In Fig. 4 and Fig. 5, the modified spots 13a are shown in white (without hatching), and the ranges to which the cracks 14a extend are shown by dashed lines (similar to Figs. 6 to 11).
[0035] In the first embodiment, in order to form a plurality of modified spots 13a, the pulsed laser light L is modulated by the spatial light modulator 4 so as to be focused on a plurality of (for example, six) focusing points C arranged in the Y direction. Then, the plurality of focusing points C are moved relatively on the virtual plane 15 along the X direction. As an example of forming a plurality of modified spots 13a, the distance between adjacent focusing points C in the Y direction is 8 μm, the pulse pitch of the laser light L (i.e., the value obtained by dividing the relative moving speed of the plurality of focusing points C by the repetition frequency of the laser light L) is 10 μm, and the pulse energy of the laser light L per focusing point C (hereinafter simply referred to as "pulse energy of the laser light L") is 0.33 μJ. In this case, the center-to-center distance between adjacent modified spots 13a in the Y direction is 8 μm, and the center-to-center distance between adjacent modified spots 13a in the X direction is 10 μm.
[0036] 6 and 7, a laser beam L is incident on the inside of the GaN ingot 20 from the surface 20a to form a plurality of modified spots (first modified spots) 13b along the imaginary plane 15 (for example, arranged two-dimensionally along the entire imaginary plane 15) (first step). At this time, the modified spots 13b are formed so as not to overlap the modified spots 13a and the cracks 14a, and so that the cracks 14b extending from the modified spots 13b are not connected to each other. In addition, the focal point C of the pulsed laser beam L is moved along the imaginary plane 15 between the rows of the modified spots 13a to form a plurality of rows of modified spots 13b. In addition, in FIG. 6 and FIG. 7, the modified spots 13b are indicated by dot hatching, and the ranges to which the cracks 14b extend are indicated by dashed lines (similar to FIG. 8 to FIG. 11).
[0037] In the first embodiment, in order to form a plurality of modified spots 13b, the pulsed laser light L is modulated by the spatial light modulator 4 so as to be focused on a plurality of (for example, six) focusing points C arranged in the Y direction. Then, the plurality of focusing points C are relatively moved on the virtual plane 15 along the X direction at the center between the rows of the plurality of rows of modified spots 13a. As an example of forming a plurality of modified spots 13b, the distance between adjacent focusing points C in the Y direction is 8 μm, the pulse pitch of the laser light L is 10 μm, and the pulse energy of the laser light L is 0.33 μJ. In this case, the center-to-center distance between adjacent modified spots 13b in the Y direction is 8 μm, and the center-to-center distance between adjacent modified spots 13b in the X direction is 10 μm.
[0038] 8 and 9, a laser beam L is incident on the inside of the GaN ingot 20 from the surface 20a to form a plurality of modified spots (second modified spots) 13c along the imaginary surface 15 (for example, arranged two-dimensionally along the entire imaginary surface 15) (second step). At this time, a plurality of modified spots 13c are formed so that the plurality of modified spots 13c are connected to each other. Furthermore, as shown in FIG. 10 and FIG. 11, a laser beam L is incident on the inside of the GaN ingot 20 from the surface 20a to form a plurality of modified spots (second modified spots) 13d along the imaginary surface 15 (for example, arranged two-dimensionally along the entire imaginary surface 15) (second step). At this time, a plurality of modified spots 13d are formed so that the plurality of modified spots 13d are connected to each other. When forming a plurality of modified spots 13c, 13d, the plurality of modified spots 13c, 13d are formed so as not to overlap with a plurality of modified spots 13a, 13b. In addition, the focal point C of the pulsed laser light L is moved along the virtual plane 15 between the rows of the modified spots 13a and 13b to form the rows of modified spots 13c and 13d. At this time, the cracks 14c and 14d extending from the modified spots 13c and 13d may be connected to the cracks 14a and 14b. In addition, in Fig. 8 and Fig. 9, the modified spot 13c is shown by solid hatching, and the range into which the crack 14c extends is shown by dashed lines (similar to Fig. 10 and Fig. 11). In addition, in Fig. 10 and Fig. 11, the modified spot 13d is shown by solid hatching (solid hatching inclined opposite to the solid hatching of the modified spot 13c), and the range into which the crack 14d extends is shown by dashed lines.
[0039] In the first embodiment, the pulsed laser light L is modulated by the spatial light modulator 4 so as to be focused on a plurality of (for example, six) focusing points C arranged in the Y direction. Then, the plurality of focusing points C are relatively moved on the virtual plane 15 along the X direction at the center between the rows of the modified spots 13a, 13b. As an example of forming a plurality of modified spots 13c, 13d, the distance between adjacent focusing points C in the Y direction is 8 μm, the pulse pitch of the laser light L is 1 μm, and the pulse energy of the laser light L is 0.33 μJ. In this case, the center-to-center distance between adjacent modified spots 13c in the Y direction is 8 μm, and the center-to-center distance between adjacent modified spots 13c in the X direction is 1 μm. In addition, the center-to-center distance between adjacent modified spots 13d in the Y direction is 8 μm, and the center-to-center distance between adjacent modified spots 13d in the X direction is 1 μm.
[0040] As described above, in the first step of forming the multiple modified spots 13a, 13b along each of the multiple imaginary surfaces 15, the multiple modified spots 13a, 13bd are formed along each of the multiple imaginary surfaces 15 to have a first formation density. The first formation density corresponds to the "number of modified spots 13a, 13b per unit area" when focusing on one imaginary surface 15. Then, in the second step of forming the multiple modified spots 13c, 13d along each of the multiple imaginary surfaces 15, the multiple modified spots 13c, 13d are formed along each of the multiple imaginary surfaces 15 to have a second formation density higher than the first formation density. The second formation density corresponds to the "number of modified spots 13c, 13d per unit area" when focusing on one imaginary surface 15. In the first embodiment, in a first step of forming a plurality of modified spots 13a, 13b along each of the plurality of imaginary surfaces 15, the focal point C of the pulsed laser light L is moved along each of the plurality of imaginary surfaces 15 at a first pulse pitch (e.g., 10 μm). Then, in a second step of forming a plurality of modified spots 13c, 13d along each of the plurality of imaginary surfaces 15, the focal point C of the pulsed laser light L is moved along each of the plurality of imaginary surfaces 15 at a second pulse pitch (e.g., 1 μm) smaller than the first pulse pitch.
[0041] Next, the GaN ingot 20 is heated using a heating device equipped with a heater or the like, and the cracks 14 extending from the modified spots 13 are connected to each other on each of the imaginary planes 15, thereby forming a crack 17 (hereinafter simply referred to as "crack 17") across the imaginary planes 15 on each of the imaginary planes 15 as shown in FIG. 12. In FIG. 12, the modified spots 13 and the cracks 14, as well as the range in which the cracks 17 are formed, are shown by dashed lines. Note that the cracks 17 may be formed by connecting the cracks 14 to each other by applying some force to the GaN ingot 20 by a method other than heating. Also, the cracks 17 may be formed by connecting the cracks 14 to each other by forming the modified spots 13 along the imaginary planes 15.
[0042] Here, in the GaN ingot 20, nitrogen gas is generated in the multiple cracks 14 extending from the multiple modified spots 13. Therefore, by heating the GaN ingot 20 to expand the nitrogen gas, the pressure (internal pressure) of the nitrogen gas can be used to form the cracks 17. Moreover, the peripheral region 16 prevents the multiple cracks 14 from progressing to the outside of the virtual surface 15 surrounded by the peripheral region 16 (for example, the side surface 20b of the GaN ingot 20), so that the nitrogen gas generated in the multiple cracks 14 can be prevented from escaping to the outside of the virtual surface 15. In other words, the peripheral region 16 is a non-modified region that does not include the modified spots 13, and is a region that prevents the multiple cracks 14 from progressing to the outside of the virtual surface 15 surrounded by the peripheral region 16 when the cracks 17 are formed on the virtual surface 15 surrounded by the peripheral region 16. For this reason, it is preferable to set the width of the peripheral region 16 to 30 μm or more.
[0043] Next, a grinding device is used to grind (polish) the portions of GaN ingot 20 corresponding to each of the peripheral regions 16 and each of the imaginary planes 15, thereby obtaining a plurality of GaN wafers 30 from GaN ingot 20 with each of the cracks 17 as boundaries, as shown in Fig. 13 (third step). In this manner, GaN ingot 20 is cut along each of the imaginary planes 15. Note that the portions of GaN ingot 20 corresponding to each of the peripheral regions 16 may be removed by mechanical processing, laser processing, or the like other than grinding.
[0044] Of the above steps, the laser processing method of the first embodiment includes the steps up to the step of forming the multiple modified spots 13 along each of the multiple imaginary planes 15. Also, of the above steps, the semiconductor component manufacturing method of the first embodiment includes the steps up to the step of obtaining the multiple GaN wafers 30 from the GaN ingot 20 with each of the multiple cracks 17 as boundaries.
[0045] As described above, in the laser processing method of the first embodiment, in each of the multiple imaginary surfaces 15, the multiple modified spots 13a, 13b are formed along the virtual surface 15 so as to have a first formation density, and then the multiple modified spots 13c, 13d are formed along the virtual surface 15 so as to have a second formation density higher than the first formation density. As a result, for the multiple cracks 14c, 14d extending from the multiple modified spots 13c, 13d, respectively, in each of the multiple imaginary surfaces 15, the extension width (hereinafter simply referred to as "extension width") in the direction perpendicular to the virtual surface 15 can be suppressed, and as a result, the crack 17 can be formed accurately along the virtual surface 15. It is presumed that the extension width of the multiple cracks 14c, 14d is suppressed because the multiple cracks 14a, 14b already formed function as guides. Therefore, according to the laser processing method of the first embodiment, by obtaining a plurality of GaN wafers 30 from the GaN ingot 20 using each of the plurality of cracks 17 as a boundary, a plurality of preferable GaN wafers 30 can be obtained.
[0046] Similarly, according to the laser processing apparatus 1 that performs the laser processing method of the first embodiment, it is possible to precisely form the cracks 17 along the virtual surfaces 15 on each of the multiple virtual surfaces 15, thereby making it possible to obtain multiple suitable GaN wafers 30.
[0047] Moreover, in the laser processing method of the first embodiment, the multiple modified spots 13a, 13b are formed so that the multiple cracks 14a, 14b extending from the multiple modified spots 13a, 13b, respectively, are not connected to each other on each of the multiple imaginary surfaces 15. This makes it possible to suppress the extension width of the multiple cracks 14a, 14b extending from the multiple modified spots 13a, 13b, respectively, on each of the multiple imaginary surfaces 15, and as a result, it becomes possible to form the crack 17 along the imaginary surface 15 with higher accuracy.
[0048] Moreover, in the laser processing method of the first embodiment, the modified spots 13c, 13d are formed so that the modified spots 13c, 13d are connected to each other on each of the virtual surfaces 15. This makes it possible to reliably suppress the extension width of the cracks 14c, 14d extending from the modified spots 13c, 13d on each of the virtual surfaces 15, and as a result, it becomes possible to more accurately form the cracks 17 along the virtual surfaces 15.
[0049] In addition, in the laser processing method of the first embodiment, the focal point C of the pulsed laser light L is moved along the virtual surface 15 at a first pulse pitch on each of the multiple imaginary surfaces 15 to form multiple modified spots 13a, 13b, and then the focal point C of the pulsed laser light L is moved along the virtual surface 15 at a second pulse pitch smaller than the first pulse pitch to form multiple modified spots 13c, 13d. This makes it possible to reliably suppress the extension width of the multiple cracks 14c, 14d extending from the multiple modified spots 13c, 13d on each of the multiple imaginary surfaces 15, and as a result, it becomes possible to form the crack 17 along the virtual surface 15 with higher accuracy.
[0050] In the laser processing method of the first embodiment, when gallium nitride contained in the material of the GaN ingot 20 is decomposed by irradiation with the laser light L, gallium is precipitated in the cracks 14 extending from the modified spots 13, and the laser light L is easily absorbed by the gallium. Therefore, adjusting the formation of the modified spots 13a, 13b and the formation of the modified spots 13c, 13d is effective in forming the cracks 17 accurately along the imaginary plane 15. Furthermore, when gallium nitride contained in the material of the GaN ingot 20 is decomposed by irradiation with the laser light L, nitrogen gas is generated in the cracks 14. Therefore, it is possible to easily form the cracks 17 by utilizing the pressure (internal pressure) of the nitrogen gas.
[0051] Furthermore, according to the semiconductor component manufacturing method of the first embodiment, the steps included in the laser processing method of the first embodiment make it possible to form cracks 17 accurately along each of the multiple imaginary surfaces 15, thereby making it possible to obtain multiple preferable GaN wafers 30.
[0052] Moreover, in the semiconductor component manufacturing method of the first embodiment, the multiple imaginary planes 15 are set to be aligned in a direction facing the front surface 20a of the GaN ingot 20. This makes it possible to obtain multiple GaN wafers 30 from one GaN ingot 20.
[0053] Fig. 14 is an image of modified spots and cracks formed by the laser processing method and the semiconductor member manufacturing method of the embodiment. In Example 1 shown in Fig. 14, a plurality of modified spots 13 were formed along the imaginary surface 15 under the same conditions as the laser processing method of the first embodiment described above, except that the pulse pitch of the laser light L was set to 5 μm when forming the plurality of modified spots 13c, 13d along the imaginary surface 15. In Example 1, the extension width in the direction perpendicular to the imaginary surface 15 of the plurality of cracks 14 extending from each of the plurality of modified spots 13 was about 100 μm.
[0054] In Example 2 shown in FIG. 14, a plurality of modified spots 13 were formed along the imaginary surface 15 under the same conditions as the laser processing method of the first embodiment described above, except that the pulse pitch of the laser light L was set to 2.5 μm when forming a plurality of modified spots 13c, 13d along the imaginary surface 15. Example 2 corresponds to a case where a plurality of modified spots 13c, 13d were formed so that the plurality of modified spots 13c, 13d were not connected to each other, and so that a plurality of cracks 14c, 14d extending from the plurality of modified spots 13c, 13d were connected to each other. In Example 2, the extension width in the direction perpendicular to the imaginary surface 15 of the plurality of cracks 14 extending from the plurality of modified spots 13 was about 100 μm.
[0055] In Example 3 shown in Fig. 14, a plurality of modified spots 13 were formed along the imaginary surface 15 under the same conditions as those of the laser processing method of the first embodiment described above, including the fact that the pulse pitch of the laser light L was 1 µm when forming the plurality of modified spots 13c, 13d along the imaginary surface 15. Example 3 corresponds to the case where a plurality of modified spots 13c, 13d were formed so that the plurality of modified spots 13c, 13d were connected to each other. In Example 3, the extension width of the plurality of cracks 14 extending from each of the plurality of modified spots 13 in the direction perpendicular to the imaginary surface 15 was about 25 µm.
[0056] From the above results, it was found that it is more preferable to form the multiple modified spots 13c, 13d along the virtual surface 15 so that the density (second formation density) is higher than the formation density (first formation density) of the multiple modified spots 13a, 13b, and to form the multiple modified spots 13c, 13d so that the multiple cracks 14c, 14d are connected to each other, or the multiple modified spots 13c, 13d are connected to each other. When forming the multiple modified spots 13c, 13d along the virtual surface 15, the multiple modified spots 13c, 13d may be formed so that the multiple stress change regions 18 shown in FIG. 15 are connected to each other, or the multiple light collection regions Cr shown in FIG. 15 are connected to each other (FIG. 15 illustrates the modified spot 13c of the modified spots 13c, 13d). The stress change region 18 is a region around each modified spot 13, and is a region in which internal stress is generated in the object 11 by the formation of each modified spot 13. The light-concentration region Cr is a region including the focal point C of the laser light L, and is a region where the laser light L is concentrated to form each modified spot 13. [Laser processing method and semiconductor member manufacturing method according to the second embodiment]
[0057] The object 11 in the laser processing method and the semiconductor member manufacturing method of the second embodiment is a GaN wafer (semiconductor wafer, semiconductor object) 30 shown in FIG. 16. The GaN wafer 30 is made of GaN and has, for example, a disk shape. As an example, the diameter of the GaN wafer 30 is 2 in, and the thickness of the GaN wafer 30 is 100 μm. A plurality of imaginary surfaces 15 are set on the GaN wafer 30. Each of the plurality of imaginary surfaces 15 is a surface facing the surface 30a of the GaN wafer 30 inside the GaN wafer 30, and is set to be aligned in the direction in which the surface 30a extends. As an example, each of the plurality of imaginary surfaces 15 is a surface parallel to the surface 30a, and has, for example, a rectangular shape. As an example, each of the plurality of imaginary surfaces 15 is set to be aligned two-dimensionally in a direction parallel to and perpendicular to the orientation flat 31 of the GaN wafer 30. A plurality of peripheral regions 16 are set on the GaN wafer 30 so as to surround each of the plurality of imaginary surfaces 15. That is, each of the multiple imaginary surfaces 15 does not reach the side surface 30b of the GaN wafer 30. As an example, the width of the peripheral region 16 corresponding to each of the multiple imaginary surfaces 15 (half the distance between adjacent imaginary surfaces 15 in the second embodiment) is 30 μm or more.
[0058] In the object 11 of the laser processing method and the semiconductor member manufacturing method of the second embodiment, the above-mentioned laser processing device 1 is used to form a plurality of modified spots 13 along each of the plurality of imaginary surfaces 15. Specifically, the stage 2 supports the GaN wafer 30, and the laser irradiation unit composed of the spatial light modulator 4 and the condenser lens 5 causes the laser light L to be incident from the surface 30a into the inside of the GaN wafer 30, thereby forming a plurality of modified spots 13 along each of the plurality of imaginary surfaces 15. Then, in the semiconductor member manufacturing method of the second embodiment, the GaN wafer 30 is cut along each of the plurality of imaginary surfaces 15 to obtain a plurality of semiconductor devices (semiconductor members) 40 from the GaN wafer 30. The substrate portion of the semiconductor device 40 is made of GaN and has, for example, a rectangular shape. As an example, the outer shape of the substrate portion of the semiconductor device 40 is 1 mm×1 mm, and the thickness of the substrate portion of the semiconductor device 40 is several tens of μm.
[0059] Hereinafter, the laser processing method and the semiconductor member manufacturing method of the second embodiment will be described in detail. First, the above-mentioned laser processing device 1 is used to form a plurality of modified spots 13 along each of the plurality of imaginary surfaces 15. The formation of the plurality of modified spots 13 along each of the plurality of imaginary surfaces 15 is performed in the same manner as the first and second steps of the laser processing method and the semiconductor member manufacturing method of the first embodiment. As a result, in the GaN wafer 30, as shown in FIG. 17, a plurality of modified spots 13 (i.e., modified spots 13a, 13b, 13c, 13d) and a plurality of cracks 14 (i.e., cracks 14a, 14b, 14c, 14d) are formed along each of the plurality of imaginary surfaces 15. In FIG. 17, the ranges in which the plurality of modified spots 13 and the plurality of cracks 14 are formed are indicated by dashed lines.
[0060] Next, using a semiconductor manufacturing apparatus, a plurality of functional elements 32 are formed on the surface 30a of the GaN wafer 30, as shown in Fig. 18. Each of the plurality of functional elements 32 is formed so that one functional element 32 is included in one imaginary plane 15 when viewed from the thickness direction of the GaN wafer 30. The functional elements 32 are, for example, light receiving elements such as photodiodes, light emitting elements such as laser diodes, circuit elements such as memories, etc.
[0061] In the second embodiment, when forming a plurality of functional elements 32 on the surface 30a of the GaN wafer 30, the semiconductor manufacturing apparatus functions as a heating apparatus. That is, when forming a plurality of functional elements 32 on the surface 30a of the GaN wafer 30 using the semiconductor manufacturing apparatus, the GaN wafer 30 is heated, and a plurality of cracks 14 extending from a plurality of modified spots 13 are connected to each other on each of the plurality of imaginary surfaces 15, thereby forming a crack 17 (i.e., a crack 17 across the imaginary surface 15) on each of the plurality of imaginary surfaces 15. In FIG. 18, the plurality of modified spots 13 and the plurality of cracks 14, as well as the range in which the crack 17 is formed, are shown by dashed lines. Note that a heating apparatus other than the semiconductor manufacturing apparatus may be used. Also, the plurality of cracks 14 may be connected to each other to form the crack 17 by applying some force to the GaN wafer 30 by a method other than heating. Also, the plurality of modified spots 13 may be formed along the imaginary surface 15, thereby forming the crack 17 by connecting the plurality of cracks 14 to each other.
[0062] Here, in the GaN wafer 30, nitrogen gas is generated in the multiple cracks 14 extending from the multiple modified spots 13. Therefore, by heating the GaN ingot 20 to expand the nitrogen gas, the cracks 17 can be formed by utilizing the pressure of the nitrogen gas. Moreover, the peripheral region 16 prevents the multiple cracks 14 from progressing to the outside of the virtual surface 15 surrounded by the peripheral region 16 (for example, the adjacent virtual surface 15, the side surface 30b of the GaN wafer 30), so that the nitrogen gas generated in the multiple cracks 14 can be prevented from escaping to the outside of the virtual surface 15. In other words, the peripheral region 16 is a non-modified region that does not include the modified spots 13, and is a region that prevents the multiple cracks 14 from progressing to the outside of the virtual surface 15 surrounded by the peripheral region 16 when the cracks 17 are formed in the virtual surface 15 surrounded by the peripheral region 16. For this reason, it is preferable to set the width of the peripheral region 16 to 30 μm or more.
[0063] Next, the GaN wafer 30 is cut into individual functional elements 32 using a laser processing device, and the portions corresponding to the respective imaginary planes 15 are ground using a grinding device, thereby obtaining a plurality of semiconductor devices 40 from the GaN wafer 30 with the respective cracks 17 as boundaries, as shown in Fig. 19 (third step). In this manner, the GaN wafer 30 is cut along each of the respective imaginary planes 15. The GaN wafer 30 may be cut into individual functional elements 32 by mechanical processing other than laser processing (e.g., blade dicing) or the like.
[0064] Of the above steps, the laser processing method of the second embodiment includes the steps up to the step of forming a plurality of modified spots 13 along each of the plurality of imaginary planes 15. Also, of the above steps, the semiconductor component manufacturing method of the second embodiment includes the steps up to the step of obtaining a plurality of semiconductor devices 40 from the GaN wafer 30 with each of the plurality of cracks 17 as boundaries.
[0065] As described above, according to the laser processing method of the second embodiment, similarly to the laser processing method of the first embodiment, the extension width of the multiple cracks 14c, 14d extending from the multiple modified spots 13c, 13d, respectively, can be suppressed on each of the multiple imaginary planes 15, and as a result, it becomes possible to form the crack 17 with high precision along the imaginary plane 15. Therefore, according to the laser processing method of the second embodiment, by obtaining multiple semiconductor devices 40 from the GaN wafer 30 with each of the multiple cracks 17 as boundaries, it becomes possible to obtain multiple preferable semiconductor devices 40.
[0066] Similarly, according to the laser processing apparatus 1 that performs the laser processing method of the second embodiment, it is possible to precisely form the cracks 17 along the virtual surfaces 15 on each of the multiple virtual surfaces 15, thereby making it possible to obtain multiple preferable semiconductor devices 40.
[0067] In addition, in the laser processing method of the second embodiment, the multiple modified spots 13a, 13b are formed so that the multiple cracks 14a, 14b extending from the multiple modified spots 13a, 13b are not connected to each other on each of the multiple imaginary surfaces 15. This makes it possible to suppress the extension width of the multiple cracks 14a, 14b extending from the multiple modified spots 13a, 13b on each of the multiple imaginary surfaces 15, and as a result, it becomes possible to form the crack 17 along the imaginary surface 15 with higher accuracy.
[0068] Moreover, in the laser processing method of the second embodiment, the modified spots 13c, 13d are formed so that the modified spots 13c, 13d are connected to each other on each of the virtual surfaces 15. This makes it possible to reliably suppress the extension width of the cracks 14c, 14d extending from the modified spots 13c, 13d on each of the virtual surfaces 15, and as a result, it becomes possible to form the cracks 17 along the virtual surfaces 15 with higher accuracy.
[0069] In addition, in the laser processing method of the second embodiment, the focal point C of the pulsed laser light L is moved along the virtual surface 15 at a first pulse pitch on each of the multiple imaginary surfaces 15 to form multiple modified spots 13a, 13b, and then the focal point C of the pulsed laser light L is moved along the virtual surface 15 at a second pulse pitch smaller than the first pulse pitch to form multiple modified spots 13c, 13d. This makes it possible to reliably suppress the extension width of the multiple cracks 14c, 14d extending from the multiple modified spots 13c, 13d on each of the multiple imaginary surfaces 15, and as a result, it becomes possible to form the crack 17 along the virtual surface 15 with higher accuracy.
[0070] In addition, in the laser processing method of the second embodiment, when gallium nitride contained in the material of the GaN wafer 30 is decomposed by irradiation with the laser light L, gallium is precipitated in the multiple cracks 14 extending from the multiple modified spots 13, and the laser light L is easily absorbed by the gallium. Therefore, adjusting the formation of the multiple modified spots 13a, 13b and the formation of the multiple modified spots 13c, 13d is effective in forming the cracks 17 accurately along the virtual plane 15. Furthermore, when gallium nitride contained in the material of the GaN wafer 30 is decomposed by irradiation with the laser light L, nitrogen gas is generated in the multiple cracks 14. Therefore, it is possible to easily form the cracks 17 by utilizing the pressure of the nitrogen gas.
[0071] Furthermore, according to the semiconductor component manufacturing method of the second embodiment, the steps included in the laser processing method of the second embodiment make it possible to accurately form cracks 17 along each of the multiple imaginary surfaces 15, thereby making it possible to obtain multiple preferable semiconductor devices 40.
[0072] In the semiconductor article manufacturing method of the second embodiment, the multiple imaginary planes 15 are set to be aligned in the direction in which the front surface 30a of the GaN wafer 30 extends. This makes it possible to obtain multiple semiconductor devices 40 from one GaN wafer 30. [Variations]
[0073] The present disclosure is not limited to the above-mentioned embodiment. For example, various values related to the laser light L are not limited to those described above. However, in order to suppress the crack 14 from extending from the modified spot 13 to the incident side of the laser light L and the opposite side, it is preferable that the pulse energy of the laser light L is 0.1 μJ to 1 μJ and the pulse width of the laser light L is 200 fs to 1 ns.
[0074] Moreover, the semiconductor object processed by the laser processing method and the semiconductor member manufacturing method according to one aspect of the present disclosure is not limited to the GaN ingot 20 of the first embodiment and the GaN wafer 30 of the second embodiment. Moreover, the semiconductor member manufactured by the semiconductor member manufacturing method according to one aspect of the present disclosure is not limited to the GaN wafer 30 of the first embodiment and the semiconductor device 40 of the second embodiment. As an example, the material of the semiconductor object may be SiC. Even in that case, according to the laser processing method and the semiconductor member manufacturing method according to one aspect of the present disclosure, it is possible to form a crack spanning the imaginary surface along the imaginary surface with high accuracy. Moreover, one imaginary surface may be set for one semiconductor object.
[0075] Furthermore, the method of forming the multiple modified spots 13a, 13b, 13c, and 13d is not limited to the above, and may be any method as long as the multiple modified spots 13a, 13b are formed along the imaginary surface 15 to have a first formation density, and then the multiple modified spots 13c, 13d are formed along the imaginary surface 15 to have a second formation density higher than the first formation density. For example, the multiple modified spots 13a, 13b may be formed so that the multiple cracks 14a, 14b extending from the multiple modified spots 13a, 13b, respectively, are connected to each other. Furthermore, as shown in Figure 20, for example, by rotating the GaN ingot 20, multiple radially arranged focal points can be rotated relatively (dotted arrow) to form multiple rows of modified spots 13, and further, as shown in Figure 21, multiple radially arranged focal points can be rotated relatively (dotted arrow) while each of the multiple focal points is positioned between the multiple rows of modified spots 13 to form multiple rows of modified spots 13.
[0076] Furthermore, in the laser processing method and semiconductor component manufacturing method of the first embodiment, the formation of the multiple modified spots 13 may be performed sequentially for each of the multiple imaginary faces 15 from the side opposite to the surface 20a. Furthermore, in the laser processing method and semiconductor component manufacturing method of the first embodiment, the formation of the multiple modified spots 13 may be performed along one or more imaginary faces 15 on the surface 20a side, and after one or more GaN wafers 30 are cut out, the surface 20a of the GaN ingot 20 may be ground, and the formation of the multiple modified spots 13 may be performed again along one or more imaginary faces 15 on the surface 20a side.
[0077] Furthermore, in the laser processing method and the semiconductor product manufacturing method of the first and second embodiments, the peripheral region 16 may not be formed. When the peripheral region 16 is not formed in the laser processing method and the semiconductor product manufacturing method of the first embodiment, it is also possible to obtain a plurality of GaN wafers 30 by forming a plurality of modified spots 13 along each of the plurality of imaginary planes 15, and then, for example, etching the GaN ingot 20.
[0078] Furthermore, the laser processing apparatus 1 is not limited to the above-mentioned configuration. For example, the laser processing apparatus 1 does not have to include the spatial light modulator 4.
[0079] Furthermore, the respective components in the above-described embodiments are not limited to the materials and shapes described above, and various materials and shapes can be applied. Furthermore, the respective components in one embodiment or modified example described above can be arbitrarily applied to the respective components in other embodiments or modified examples. [Explanation of symbols]
[0080] 1...laser processing apparatus, 2...stage, 4...spatial light modulator (laser irradiation unit), 5...focusing lens (laser irradiation unit), 13...modified spot, 13a, 13b...modified spot (first modified spot), 13c, 13d...modified spot (second modified spot), 14, 14a, 14b, 14c, 14d...crack, 15...virtual surface, 17...crack across virtual surface, 20...GaN ingot (semiconductor ingot, semiconductor object), 20a...surface, 30...GaN wafer (semiconductor wafer, semiconductor member, semiconductor object), 30a...surface, 40...semiconductor device (semiconductor member), C...focusing point, L...laser light.
Claims
1. 1. A laser processing method for cutting a semiconductor object along an imaginary plane inside the semiconductor object facing a surface of the semiconductor object, comprising: a first step of forming a plurality of first modified spots along the imaginary plane at a first formation density by irradiating laser light into the interior of the semiconductor object from the surface, thereby forming a plurality of rows of first modified spots; and a second step of forming a plurality of second modified spots along the imaginary plane so as to have a second formation density higher than the first formation density by irradiating laser light into the interior of the semiconductor object from the surface after the first step, thereby forming a plurality of rows of second modified spots each located between the rows of the first modified spots, A laser processing method in which, in the second step, the plurality of second modified spots are formed so that the plurality of second modified spots are not connected to each other.
2. 2. The laser processing method according to claim 1, wherein in the first step, the plurality of first modified spots are formed so that the plurality of cracks extending from the plurality of first modified spots respectively do not connect to each other.
3. 3. The laser processing method according to claim 1, wherein in the second step, the plurality of second modified spots are formed so that a plurality of cracks extending from the plurality of second modified spots respectively connect to each other.
4. In the first step, a focal point of the pulsed laser light is moved along the virtual plane at a first pulse pitch to form the plurality of first modified spots; The laser processing method according to any one of claims 1 to 3, wherein in the second step, the plurality of second modified spots are formed by moving a focal point of the pulsed laser light along the virtual plane at a second pulse pitch smaller than the first pulse pitch.
5. The laser processing method according to any one of claims 1 to 4, wherein a material of the semiconductor object contains gallium.
6. The laser processing method of claim 5 , wherein the material of the semiconductor object comprises gallium nitride.
7. In the first step, the laser light is focused on a plurality of first focusing points, and the plurality of first focusing points are relatively moved along a direction intersecting a direction in which the plurality of first focusing points are arranged, The laser processing method according to any one of claims 1 to 6, wherein in the second step, the laser light is focused at a plurality of second focal points each located between the rows of the first modification spots, and the plurality of second focal points are moved relatively along a direction intersecting a direction in which the plurality of second focal points are arranged.
8. The first step and the second step of the laser processing method according to any one of claims 1 to 7, A third step of obtaining a semiconductor component from the semiconductor object using a crack that crosses the imaginary surface as a boundary.
9. The method for manufacturing a semiconductor article according to claim 8 , wherein a plurality of the imaginary faces are set so as to be aligned in a direction facing the front surface.
10. the semiconductor object is a semiconductor ingot; The method for producing a semiconductor article according to claim 9 , wherein the semiconductor article is a semiconductor wafer.
11. The method for manufacturing a semiconductor article according to claim 8 , wherein a plurality of the imaginary surfaces are set so as to be aligned in a direction in which the surface extends.
12. the semiconductor object is a semiconductor wafer; The method for producing a semiconductor article according to claim 11, wherein the semiconductor article is a semiconductor device.
13. 1. A laser processing apparatus for cutting a semiconductor object along a virtual plane facing a surface of the semiconductor object within the semiconductor object, comprising: a stage for supporting the semiconductor workpiece; a laser irradiation unit that forms a plurality of first modified spots and a plurality of second modified spots along the virtual plane by irradiating laser light from the surface into the inside of the semiconductor object; The laser irradiation unit includes: forming the plurality of first modified spots along the imaginary surface to have a first formation density, forming a plurality of rows of first modified spots; after forming the plurality of first modified spots, forming the plurality of second modified spots along the imaginary surface to have a second formation density higher than the first formation density, forming a plurality of rows of second modified spots each located between the plurality of rows of first modified spots; A laser processing apparatus that, when forming the plurality of second modified spots, forms the plurality of second modified spots so that the plurality of second modified spots are not connected to each other.
14. The laser irradiation unit comprises: When forming the plurality of first modified spots, the laser light is focused on a plurality of first focusing points, and the plurality of first focusing points are relatively moved along a direction intersecting a direction in which the plurality of first focusing points are arranged, The laser processing apparatus of claim 13, wherein when forming the plurality of second modified spots, the laser light is focused at a plurality of second focal points each located between the plurality of rows of the first modified spots, and the plurality of second focal points are moved relatively along a direction intersecting the direction in which the plurality of second focal points are arranged.
Citation Information
Patent Citations
Separation method for element formed on substrate
JP2004259846A
Substrate processing device and substrate processing method
JP2015123466A
Formation method of gallium nitride substrate
JP2017057103A
Semiconductor element manufacturing method
JP2017069510A
Slice method and slice device
JP2017183600A