Method for producing hollow spherical alumina particles

A two-step process for producing hollow spherical alumina particles addresses productivity and efficiency issues, resulting in high-quality alumina with desirable properties for various applications.

JP7560195B1Active Publication Date: 2024-10-02ASADA KAGAKU IND

Patent Information

Application Number
JP2024104097
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-02
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

Existing methods for producing hollow spherical alumina particles face challenges such as low productivity, complex processes, and poor thermal efficiency due to the need for large equipment and multi-step processes, which hinder the production of high-quality alumina particles.

Method used

A two-step method involving the granulation of a basic aluminum lactate aqueous solution at controlled temperatures and pressures followed by calcination at specific temperatures to produce hollow spherical alumina particles with desired properties.

Benefits of technology

The method yields alumina particles with excellent heat resistance, thermal shock resistance, and chemical resistance, suitable for high-performance compounding materials, heat dissipation fillers, and cosmetic ingredients.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560195000001_ABST
    Figure 0007560195000001_ABST
Patent Text Reader

Abstract

To provide a method for easily producing hollow, spherical alumina particles using an aqueous basic aluminum lactate solution in two steps: granulation and calcination. The present invention relates to a method for producing a granulated product by drying and granulating an aqueous solution of basic aluminum lactate at a temperature of 210 to 280°C under a gas pressure of 0.01 to 1 MPa in the atmosphere or inert gas, and reducing the volatile content of the granulated product to 0 to 10% and the bulk density to 0.2 to 0.7 g / cm. 3 A first step of forming a hollow dry granule having a controlled diameter; A second step of calcining the dried granules obtained in the first step at a calcination temperature within a range of 1050°C or more and less than 1200°C for 2 to 8 hours to obtain hollow spherical alumina particles; The basic aluminum lactate aqueous solution is a specific one having a small amount of impurities, and the obtained hollow spherical alumina particles have a D50 of 5 to 50 μm and a D90 of 200 μm or less in particle size distribution measurement, and the crystalline phase is the α-phase.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing hollow spherical alumina particles. [Background technology]

[0002] Hollow alumina particles are produced by various methods. For example, Japanese Patent No. 4271045 (Patent Document 1) and Japanese Patent No. 4043805 (Patent Document 2) disclose a method for producing hollow alumina particles, which is characterized by irradiating an aqueous solution of raw material containing aluminum nitrate or aluminum acetate and an organic acid selected from citric acid, amino acid, and malic acid with ultrasonic waves, and then feeding minute droplets from a droplet selection section to a firing furnace and firing them in air at 1200 to 1300°C. To obtain hollow alumina particles by this method, it is necessary to limit the amount of droplets to be fed, and in order to synthesize α-alumina from an aqueous solution, a series of steps from drying to firing must be carried out in the furnace, which increases the size of the device and reduces productivity.

[0003] Patent Document 3 (Patent No. 6316153) describes a method for producing hollow alumina particles, which is characterized by spraying an aluminum salt aqueous solution with a spray nozzle, passing the solution through both a drying zone at 300 to 600 ° C and a pyrolysis zone at 600 to 1600 ° C to obtain hollow particles mainly composed of γ-alumina, and heating the obtained hollow particles mainly composed of γ-alumina to 1000 to 1150 ° C. In order to obtain γ-alumina by spray pyrolysis in a furnace having two types of zones, a drying zone at 300 to 600 ° C and a pyrolysis zone at 600 to 1600 ° C, the apparatus becomes large, which deteriorates productivity. In addition, a process is required to further heat γ-alumina to 1000 to 1150 ° C to produce hollow alumina having an α phase, which requires two steps, resulting in poor production efficiency, and the firing process is two steps, which results in poor thermal efficiency.

[0004] Patent Document 4 (Patent No. 6730045) describes a method for producing α-alumina particles for friction materials, which are at least one of spherical and irregular shapes, characterized by heating at least one of agglomerates of boehmite and agglomerates of pseudo-boehmite for 1 to 20 hours at a temperature range of 1200 to 1500° C. In this production method, agglomerates of plate-like boehmite and pseudo-boehmite are granulated and fired at a temperature of 1200 to 1500° C., so that even if the agglomerates are spherical, hollow bodies cannot be produced.

[0005] Patent Document 5 (Patent No. 5568399) describes a method for producing a ferroelectric material with a specific surface area of ​​10 to 20 m 2 This publication discloses a method for producing spherical alumina particles, characterized in that an alcohol slurry of fine alumina powder with a particle size of 100 / g is sprayed into a flame having a flame temperature of 1300 to 1650° C. In this production method, since an alcohol slurry of ultrafine alumina powder is sprayed into a flame, hollow particles cannot be obtained, and since ultrafine alumina powder is used as a raw material, a high sintering temperature of 1300 to 1650° C. is required to sinter the α-alumina powder particles together, resulting in poor productivity.

[0006] Patent Document 6 (JP Patent No. 7406444) describes a method for producing a spherical particulate material, which includes a first pickling step in which a raw material particle material mainly composed of alumina is immersed in an acid solution to produce a raw material particle material, a melting and spheroidizing step in which the raw material particle material is melted and rapidly cooled to produce a coarse spherical particle material, and a second pickling step in which the coarse spherical particle material is immersed in an acid solution to produce a spherical particle material. In this production method, at least one of the first and second pickling steps must be performed in a high-temperature environment, and the raw material particle material must be immersed in nitric acid, sulfuric acid, hydrofluoric acid, etc., which makes the process complicated and requires the use of a large amount of acid, and may make it impossible to produce hollow alumina. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 4271045 [Patent Document 2] Patent No. 4043805 [Patent Document 3] Patent No. 6316153 [Patent Document 4] Patent No. 6730045 [Patent Document 5] Patent No. 5568399 [Patent Document 6] Patent No. 7406444 Summary of the Invention [Problem to be solved by the invention]

[0008] We have discovered a method for easily producing hollow, spherical alumina particles using an aqueous solution of basic aluminum lactate in two steps: granulation and calcination. [Means for solving the problem]

[0009] That is, the present invention includes the following aspects: [1] The basic aluminum lactate aqueous solution is dried and granulated at a temperature of 210 to 280°C under a gas pressure of 0.01 to 1 MPa in air or inert gas, and the volatile content of the granulated product is adjusted to 0 to 10% and the bulk density to 0.2 to 0.7 g / cm. 3 A first step of forming a hollow dry granule having a controlled diameter; A second step of calcining the dried granules obtained in the first step at a calcination temperature within a range of 1050°C or more and less than 1200°C for 2 to 8 hours to obtain hollow spherical alumina particles; The basic aluminum lactate aqueous solution contains iron (Fe) in an amount of 0 to 0.01 mass%, calcium (Ca) in an amount of 0 to 0.01 mass%, magnesium (Mg) in an amount of 0 to 0.01 mass%, silicon (Si) in an amount of 0.005 to 1.2 mass%, an alkali metal element ion in an amount of 0.005 to 1.2 mass%, a basicity of 60 to 80%, and aluminum is Al 2 O 3 It contains 8 to 13 mass% in terms of The obtained hollow spherical alumina particles have a D50 of 5 to 50 μm and a D90 of 200 μm or less in particle size distribution measurement, are hollow inside and have through holes on the outside, and have a specific surface area of ​​1 to 20 m. 2 / g, and the crystal phase is an α phase. [2] The hollow spherical alumina particles have a loss on drying of 4% or less, a loss on ignition of 6% or less, and a bulk density of 0.4 to 0.7 g / cm3, as determined by aluminum oxide analysis in accordance with the 2021 Standards for Pharmaceutical and Medical Devices. 3 The method for producing hollow spherical alumina particles according to [1], [3] The method for producing hollow spherical alumina particles according to [1] or [2], characterized in that the basic aqueous aluminum lactate solution is obtained by mixing an aluminum chloride solution with either or both of sodium aluminate and potassium aluminate, and water to form an aluminum hydroxide gel, washing the resulting gel with water, adding water to obtain an aluminum hydroxide slurry, and then adding lactic acid to cause a reaction. [4] The method for producing hollow spherical alumina particles according to [1] or [2], wherein the drying and granulation in the first step is a spray drying method. [5] The method for producing hollow spherical alumina particles according to [1] or [2], wherein the firing in the second step is carried out in air, nitrogen or an inert gas, or in vacuum. Effect of the Invention

[0010] The hollow spherical alumina particles of the present invention have the heat resistance, thermal shock resistance, chemical resistance, and high-temperature strength properties derived from alpha alumina, and the hollow and spherical properties give them excellent light weight, insulation, fluidity, etc., so they are expected to be used as high-performance compounding materials for resins, rubbers, etc., heat dissipation fillers for electronic materials, polishing fillers for electronic components, etc. In addition, by designing them in accordance with the 2021 Standards for Pharmaceutical and Medical Devices, they can be used as cosmetic compounding agents, scrubs, etc. [Brief description of the drawings]

[0011] [Figure 1] 1 is a graph showing the particle size distribution of the alumina particles obtained in Example 1, measured in a dry state using a laser diffraction particle size distribution analyzer (Mastersizer 3000, manufactured by Malvern Panalytical). [Diagram 2] FIG. 2 is a diagram showing the results of measurement of the alumina particles obtained in Example 1 using an X-ray diffractometer (MiniFlex manufactured by Rigaku Corporation) with a Cu target by the θ / 2θ method. [Diagram 3] FIG. 13 is a diagram showing the results of measurement of the alumina particles obtained in Comparative Example 4 using an X-ray diffractometer (MiniFlex manufactured by Rigaku Corporation) with a Cu target by the θ / 2θ method. [Figure 4] 1 is a 100,000-times magnified SEM image of the alumina particles of Example 1 measured using a field emission scanning electron microscope (FE-SEM: JSM-7001F manufactured by JEOL Ltd.). [Diagram 5] 1 is a 10,000-times magnification SEM image of the alumina particles of Example 1 measured using a field emission scanning electron microscope (FE-SEM: JSM-7001F manufactured by JEOL Ltd.). [Figure 6] 1 is a 25,000-times magnification SEM image of the alumina particles of Example 1 measured using a field emission scanning electron microscope (FE-SEM: JSM-7001F manufactured by JEOL Ltd.). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] (Definition of terms) In this specification, "hollow" means that there is a gap inside the particle, and does not mean that there is a perfectly spherical space. Therefore, there is a gap or space in a part of the inside of the alumina particle. In addition, "there is a through hole" means that not all particles have a through hole, but the gap inside the particle continues to the particle surface. In this specification, "spherical" does not mean a perfect sphere, but means that the surface is uneven, but looks spherical overall.

[0013] In the present invention, a basic aluminum lactate aqueous solution is dried and granulated at a temperature of 210 to 280°C under a gas pressure of 0.01 to 1 MPa in air or an inert gas, and the volatile content of the granulated product is adjusted to 0 to 10% and the bulk density to 0.2 to 0.7 g / cm. 3 and a second step of calcining the dried granules obtained in the first step at a calcination temperature within a temperature range of 1050°C or more and less than 1200°C for 2 to 8 hours to obtain alumina particles. The aqueous basic aluminum lactate solution contains 0 to 0.01 mass% iron (Fe), 0 to 0.01 mass% calcium (Ca), 0 to 0.01 mass% magnesium (Mg) and 0 to 0.01 mass% silicon (Si), and also contains alkali metal element ions in an amount of 0.005 to 1.2 mass%, has a basicity of 60 to 80%, and contains aluminum in an amount of Al. 2 O 3 The alumina particles obtained have a particle size distribution measurement in which D50 is 5 to 50 μm, D90 is 200 μm or less, the inside is hollow and has through holes to the outside, and the specific surface area is 1 to 20 m 2 / g, and in the aluminum oxide analysis according to the Pharmaceutical and Medical Devices Raw Materials Standards 2021, the loss on drying is 4% or less, the loss on ignition is 6% or less, and the bulk density is 0.4 to 0.7 g / cm 3 The present invention is characterized in that it can provide a method for producing hollow spherical alumina particles having an α-phase crystal phase.

[0014] (raw materials) The raw materials used for synthesizing the hollow spherical alumina particles of the present invention should be selected as follows: (I) The basic aluminum lactate aqueous solution is controlled to have iron (Fe) of 0 to 0.01 mass%, calcium (Ca) of 0 to 0.01 mass%, magnesium (Mg) of 0 to 0.01 mass%, and silicon (Si) of 0 to 0.01 mass%. (II) The basic aluminum lactate aqueous solution contains alkali metal ions in an amount of 0.005 to 1.2 mass % and has a basicity of 60 to 80%, and Al is 2 O 3 It must have a converted mass of 8 to 13% by mass. (III) The basic aqueous aluminum lactate solution is obtained by mixing, as necessary, an aluminum chloride solution, a sodium aluminate or potassium aluminate solution or a combination of both with water to form an aluminum hydroxide gel, washing the gel with water, adding water to obtain an aluminum hydroxide slurry, and then adding lactic acid to cause a reaction.

[0015] In the present invention, the aqueous basic aluminum lactate solution used as the main raw material contains 0-0.01% by mass of iron (Fe), 0-0.01% by mass of calcium (Ca), 0-0.01% by mass of magnesium (Mg), and 0-0.01% by mass of silicon (Si), and the amount of alkali metals is controlled to control the basicity and aluminum content within predetermined ranges. The solution is spray-dried and calcined at a temperature of 1050°C or higher and lower than 1200°C for 2-8 hours, thereby providing hollow, spherical, and through-hole hollow spherical alumina particles which meet the specified particle size, specific surface area, loss on drying, and loss on ignition specifications and have a specified bulk density.

[0016] The present invention is produced by using the materials described in (I), (II), and (III) above and by the production method described below.

[0017] (Manufacturing method) (Step 1) A basic aluminum lactate aqueous solution satisfying the above requirements (I) and (II) is dried and granulated at a temperature of 210 to 280°C in air or an inert gas at a gas pressure of 0.01 to 1 MPa to reduce the volatile content of the granulated product to 0 to 10% and the bulk density to 0.2 to 0.7 g / cm. 3 and forming a controlled dry granulation. (Step 2) The dried granulated material obtained in step 1 is placed in an alumina crucible or sagger and fired in a firing furnace at a firing temperature within the range of 1050°C or higher and lower than 1200°C for 2 to 8 hours to obtain hollow spherical alumina particles exhibiting the α phase.

[0018] The raw materials and production method used to produce the hollow spherical alumina particles will be described in detail below.

[0019] (Basic aluminum lactate aqueous solution) The basic aluminum lactate aqueous solution used in the present invention has the following characteristics (I) to (III): (I) The basic aluminum lactate aqueous solution is controlled to have iron (Fe) of 0 to 0.01 mass%, calcium (Ca) of 0 to 0.01 mass%, magnesium (Mg) of 0 to 0.01 mass%, and silicon (Si) of 0 to 0.01 mass%. (II) The basic aluminum lactate aqueous solution contains alkali metal ions in an amount of 0.005 to 1.2 mass % and has a basicity of 60 to 80%, and Al is 2 O 3 It contains 8 to 13 mass% in converted mass.

[0020] As described in (I) above, the basic aluminum lactate aqueous solution used in the present invention is controlled to have iron (Fe) of 0-0.01 mass%, calcium (Ca) of 0-0.01 mass%, magnesium (Mg) of 0-0.01 mass%, and silicon (Si) of 0-0.01 mass%. If the Fe content, Ca content, Mg content, or Si content contained in the basic aluminum lactate aqueous solution exceeds 0.01 mass%, it may cause formation of a different crystal phase other than alumina during firing or cause defects such as coloring. The contents of Fe, Ca, Mg, and Si are preferably 0.007 mass% or less, more preferably 0.006 mass% or less, respectively.

[0021] As described in (II) above, the basic aluminum lactate aqueous solution used in the present invention must contain 0.005-1.2% by mass of alkali metal element ions. More preferably, it contains 0.01-0.5% by mass of alkali metal element ions. If the amount of alkali metal element ions is less than 0.005% by mass, the amount of alkali metal element ions is too small, and the phase transition temperature to α-alumina becomes high, and α-alumina is not produced at temperatures below 1200°C. On the other hand, if the amount of alkali metal element ions exceeds 1.2% by mass, the amount of alkali metal element ions is too large, and β-alumina and the like other than α-alumina are produced, making it impossible to obtain the desired α-alumina.

[0022] The alkali metal element ion species contained in the basic aqueous aluminum lactate solution used in the present invention must be at least one selected from sodium and potassium.

[0023] The aqueous solution of basic aluminum lactate used in the present invention has a basicity of 60 to 80%, and contains Al. 2 O 3 It is necessary that the content is 8 to 13 mass% converted into Al. If the basicity is less than 60%, there is a problem that the lactic acid content is too high and the solubility in water is deteriorated. On the other hand, if it exceeds 80%, there is a problem that insoluble aluminum hydroxide precipitates, the liquid becomes cloudy, and hollow dried granules cannot be obtained when spray-dried. 2 O 3 If the content is less than 8% by mass in terms of converted mass, there is a problem that hollow dried granules cannot be obtained when dried by spray drying. On the other hand, if it exceeds 13% by mass, the amount of Al is too large, the storage stability is poor, and precipitates are generated in the basic aluminum lactate aqueous solution, which is not suitable for spray drying. The basicity of the basic aluminum lactate aqueous solution is preferably 62 to 78%, more preferably 64 to 76%. "Basicity" is a value indicating what percentage of valences that can be replaced by bases are filled, and since aluminum is trivalent, if 2 / 3 (divalent of the trivalent) is used, it means that it will be 66.66% (i.e., about 67%), and is measured in accordance with the measurement method for basicity of liquid polyaluminum chloride for water supply in JIS K1475. The Al of aluminum (Al) in the basic aluminum lactate aqueous solution 2 O 3 The converted mass is preferably 8.5 to 12.5 mass%, more preferably 9 to 12 mass%. 2 O 3 The equivalent mass is that commonly used when using aluminum salts, Al 2 O 3 The amount of aluminum is determined by converting it into mass.

[0024] The basic aluminum lactate aqueous solution used in the present invention is preferably obtained by the method described in (III) above. Specifically, the basic aluminum lactate aqueous solution is obtained by mixing an aluminum chloride solution with a sodium aluminate or potassium aluminate solution or a combination of both with water to form an aluminum hydroxide gel, washing the gel with water, adding water to obtain an aluminum hydroxide slurry, and then adding lactic acid to react with the mixture. Of course, the basic aluminum lactate aqueous solution may be obtained by any method as long as it satisfies the above (I) and (II), but the basic aluminum lactate aqueous solution obtained by the above (III) is more preferable.

[0025] (Method for producing hollow spherical alumina particles) The hollow spherical alumina particles of the present invention are produced by the following steps 1 and 2: (Step 1) The aqueous solutions of basic aluminum lactate (I) and (II) (and, if necessary, (III)) are dried and granulated at a temperature of 210 to 280°C in air or an inert gas at a gas pressure of 0.01 to 1 MPa to reduce the volatile content of the granulated product to 0 to 10% and the bulk density to 0.2 to 0.7 g / cm. 3 and forming a controlled dry granulation. (Step 2) The dried granulated material obtained in step 1 is placed in an alumina crucible or sagger and fired in a firing furnace at a firing temperature within the range of 1050°C or higher and lower than 1200°C for 2 to 8 hours to obtain hollow spherical alumina particles exhibiting the α phase.

[0026] In step 1, the basic aluminum lactate aqueous solution is dry-granulated at a temperature of 210 to 280°C under a gas pressure of 0.01 to 1 MPa in air or an inert gas, and the volatile content of the granulated product is reduced to 0 to 10% and the bulk density to 0.20 to 0.7 g / cm. 3Dry granulation is performed in the atmosphere or in an inert gas, and the inert gas may be a rare gas (e.g., helium, neon, or argon) or nitrogen gas. Usually, the drying is performed in the atmosphere. The drying temperature is 210 to 280°C, preferably 230 to 270°C. If the drying granulation is performed at a temperature lower than 210°C, the moisture content of the dried material is high, so that aggregates are likely to be generated in the dried state, and independent hollow spherical alumina cannot be obtained after firing. If the drying granulation is performed at a temperature higher than 280°C, a part of the organic component of basic aluminum lactate is oxidized, the dried material turns brown, the physical properties deteriorate, and the spherical shape is destroyed during firing. If the gas pressure is less than 0.01 MPa, the pressure is insufficient, and a spherical dried product cannot be obtained, resulting in a problem that hollow spherical alumina cannot be obtained even after firing, while if the gas pressure is more than 1 MPa, the pressure is too high, the through holes become too large, the dried product cannot maintain its spherical shape, and hollow spherical alumina cannot be obtained even after firing. The gas pressure is preferably 0.1 to 0.8 MPa, and more preferably 0.2 to 0.7 MPa.

[0027] The drying and granulation in step 1 is generally performed by spray drying, but it is not limited to spray drying. Usable drying and granulation methods include spray drying, fluidized bed, and spray freeze drying.

[0028] The dried granules obtained in step 1 have a volatile content of 0 to 10% and a bulk density of 0.2 to 0.7 g / cm 3 If the volatile content exceeds 10%, the drying is insufficient and the moisture content of the dried product is high, which makes it easy for agglomerates to form in the dry state, and there is a drawback in that independent hollow spherical alumina particles are not obtained after firing. It is preferable that the volatile content is 0. The dried granules have a bulk density of 0.20 to 0.7 g / cm. 3 , preferably 0.25 to 0.65 g / cm 3 , more preferably 0.3 to 0.6 g / cm 3 The bulk density is 0.2 g / cm 3 If it is smaller than this, the hollowness becomes large and the thickness of the outer shell becomes thin, which is disadvantageous in that the strength of the hollow spherical alumina particles decreases. 3If it is larger, the hollowness during granulation decreases and the thickness of the outer shell increases, which makes it easier to deform and makes it difficult to form a spherical shape. The volatile content is measured using an A&D heated and dried moisture meter MX50 at 105°C for 30 minutes. The bulk density is the value obtained by dividing the mass by the volume. In the embodiment of the present invention, about 40 g of sample (M) obtained by weighing powder passed through a 1 mm mesh sieve with an accuracy of 0.1 mass% is placed in a 100 ml measuring cylinder (minimum unit of measurement is 1 ml), the surface is lightly smoothed, and the loose bulk volume (V 0 ) and bulk density: M / V 0 (g / cm 3 The volatile content can be adjusted by the temperature and liquid delivery speed during granulation, and the bulk density can be controlled by the air pressure during spray granulation.

[0029] In step 2 of the method for producing hollow spherical alumina particles of the present invention, the dried granulated material obtained in step 1 is placed in an alumina crucible or sagger, and fired in a firing furnace at a firing temperature within a range of 1050°C to 1200°C for 2 to 8 hours to obtain hollow spherical alumina particles exhibiting the α phase. The dried granulated material in step 1 is fired at a temperature of 1050°C to 1200°C for 2 to 8 hours. If the firing temperature is less than 1050°C, firing is insufficient and crystal phases other than α-alumina remain. On the other hand, if the firing temperature exceeds 1200°C, a firing furnace with heat resistance measures is required, and productivity is deteriorated. If the firing time is less than 2 hours, firing is insufficient and crystal phases other than α-alumina remain. On the other hand, if the firing time exceeds 8 hours, productivity is deteriorated.

[0030] In the firing step 2, the firing furnace in which the material is placed in a crucible or sagger is preferably a batch furnace, lift furnace, pusher furnace, or conveyor furnace. If firing is performed in a rotary kiln or drop-type rapid firing furnace, there is a problem that the shape may be distorted due to collisions during firing, or agglomerates may be generated, making it impossible to obtain hollow spherical alumina particles.

[0031] The atmosphere in the firing in step 2 may be any of air, nitrogen, vacuum, inert gas, etc., as long as the organic matter disappears and the desired alumina crystal system is properly formed when firing is performed at a predetermined firing temperature and time. If the atmosphere is inappropriate, the organic matter will not vaporize sufficiently during firing and will remain in the particles as residual carbon, resulting in defects, or the crystal phase will not be formed as desired, resulting in defects.

[0032] (Hollow spherical alumina particles) The hollow spherical alumina particles of the present invention are produced by the above-mentioned steps 1 and 2. The hollow spherical alumina particles obtained by this method have, in particle size distribution measurement, a D50 of 5 to 50 μm and a D90 of 200 μm or less, are hollow inside and have through holes connecting to the outside, and have a specific surface area of ​​1 to 20 m 2 / g, and the crystal system (also called the crystalline phase) exhibits the α phase.

[0033] The particle size distribution is obtained by dry measurement using a laser diffraction particle size distribution analyzer (Malvern Panalytical's Mastersizer 3000). FIG. 1 shows the particle size distribution results of the alumina particles of Example 1. In the particle size distribution, D50 means the diameter below which half of the population is, and D90 means that 90% of the population is below this value. As shown in FIG. 1, the particle size distribution of the alumina particles of Example 1 has been confirmed to have a D50 of 6 μm and a D90 of less than 100 μm. If the D50 is less than 5 μm, the powder flowability will be poor and handling will be difficult, and if the D50 is 50 μm or more, the use applications will be narrowed. Furthermore, if the D90 exceeds 200 μm, the use applications will be narrowed. In terms of particle size distribution, the alumina particles of the present invention preferably have a D50 of 5.5 to 45 μm, more preferably 6 to 35 μm. D90 is preferably from 60 to 120 μm, and more preferably from 70 to 90 μm.

[0034] The alumina particles obtained by the manufacturing method of the present invention are hollow inside and often have through holes between the inside and the outside. As described in the definition of the term, "hollow" and "through holes" do not mean a completely spherical hollow, but may have a fairly spherical cavity, as shown in the electron microscope photographs of the alumina particles of Example 1 in Figures 5 and 6, but may also have one or more voids of various shapes. Through holes are not necessarily present, and may simply be connected between the inside and the outside by some kind of cavity. As described in the definition of the term "spherical," the alumina particles of the present invention are not completely spherical, but merely appear to be spherical.

[0035] The hollow spherical alumina particles obtained by the production method of the present invention have a specific surface area of ​​1 to 20 m 2 / g, and the crystal system shows the α phase. The specific surface area is the surface area per unit mass or the surface area per unit volume of a certain object. In the present invention, the specific surface area is measured by an automatic specific surface area measuring device (Shimadzu Corporation Gemini7 2390) using N 2 The specific surface area of ​​the alumina particles of the present invention is 1 m 2 If the specific surface area is less than 20 m / g, the specific surface area is too small, and there are few adsorption sites when performing surface treatment using a dispersant, etc., which makes surface treatment difficult. 2 / g, N is deposited on the alumina surface. 2 The hollow spherical alumina particles of the present invention have a specific surface area of ​​preferably 3 to 15 m. 2 / g, more preferably 5 to 13m 2 / g. The crystal system of the hollow spherical alumina particles of the present invention is α type. In the present invention, it is not assumed that other crystal systems of alumina particles such as γ type are mixed in. The crystal system is mainly measured by the θ / 2θ method using an X-ray diffraction device (specifically, MiniFlex manufactured by Rigaku Corporation) with a Cu target.

[0036] The hollow spherical alumina particles of the present invention preferably have a loss on drying of 4% or less, a loss on ignition of 6% or less, and a bulk density of 0.4 to 0.7 g / cm, as determined by aluminum oxide analysis in accordance with the Standards for Pharmaceutical and Medical Devices 2021. 3 It is.

[0037] Loss on drying in the Pharmaceutical and Medical Devices Standards 2021 is defined as: weighing approximately 1 g of the raw material on a precision balance into a glass dish (A), drying it in a hot air circulation dryer set to 105°C for 2 hours, allowing it to cool naturally to room temperature in a desiccator, and then measuring the weight again on the precision balance (B). The loss on drying is calculated using the following formula (i). If it is 4.0% or less, it is considered to have passed the test. (B – A) / A × 100 (i) In the hollow spherical alumina particles of the present invention, the loss on drying is preferably 3.0% or less, and more preferably 2.0% or less.

[0038] The loss on ignition in the Pharmaceutical and Medical Devices Standards 2021 is determined by weighing out approximately 1 g of the raw material using a precision balance into an alumina crucible (C), placing it in an electric furnace set to 850°C, heating for 30 minutes, allowing it to cool naturally to room temperature, and then weighing it again using the precision balance (D). The weight is calculated using the following formula (ii). If the loss is 6.0% or less, it is considered to have passed the test. (C - D) / C × 100 (ii) In the hollow spherical alumina particles of the present invention, the loss on drying is preferably 4.0% or less, and more preferably 3.0% or less.

[0039] The hollow spherical alumina particles in the present application have a bulk density of 0.4 to 0.7 g / cm 3 More preferably, it is 0.5 to 0.65 g / cm 3 If the bulk density is less than 0.4, the shell becomes too thin and the hollow spherical alumina particles cannot retain their shape. 3If the thickness exceeds this value, the outer shell becomes too thick and the hollow spherical alumina particles will no longer function. The bulk density is calculated by dividing the mass by the volume. Specifically, the powder is sieved through a 1 mm mesh and weighed to an accuracy of 0.1 mass%, and approximately 40 g of sample (M) is placed in a 100 ml measuring cylinder (minimum unit: 1 ml). The surface is lightly smoothed and the loose bulk volume (V 0 ) and bulk density: M / V 0 (g / cm 3 ) is calculated.

[0040] (Example) The present invention will be described in more detail with reference to examples. The present invention should not be construed as being limited to these examples. In the examples, % and parts are based on mass unless otherwise specified.

[0041] Example 1 Using a 10 L jacketed GL (with glass-lined inner wall) stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 1429.8 g of tap water to the kettle and add aluminum chloride aqueous solution (Al 2 O 3 1909.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content: 23.0% by weight, Na 2 At the same time, 1660.8 g (18.0% Na equivalent in terms of O) was added to obtain 5000 g of an aluminum hydroxide gel solution.

[0042] Next, the obtained aluminum hydroxide gel solution was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated seven times. The obtained washed gel weighed 2190 g. Next, 103.2 g of the obtained washed gel was added to a 1 L glass separable flask placed on a mantle heater, followed by 157.1 g of tap water, and stirred for 30 minutes to obtain 260.3 g of slurry. Next, 39.7 g of lactic acid (90% lactic acid) was added to the obtained slurry, which was heated and stirred at 100°C for 3 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate aqueous solution (Al 2 O 3The resulting mixture had an Al content of 8.8% by mass, a basicity of 70.2%, sodium ions of 0.01% by weight, Si: 0.005% by mass, Ca: 0.0048% by mass, Mg: 0.0007% by mass, and Fe: 0.0015% by mass.

[0043] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 250°C, an outlet temperature of 110°C, and a gas pressure of 0.45 MPa using a nozzle. The collected dried granules (volatile content of the granules: 4.3% and bulk density: 0.35 g / cm 3 ) was placed in an alumina crucible and fired at 1100°C for 5 hours under peak firing conditions to obtain alumina particles.

[0044] The particle size distribution of the obtained alumina particles was measured, and D50 and D90 were determined and listed in Table 1. The particle size distribution was measured in a dry state using a laser diffraction particle size distribution analyzer (Malvern Panalytical Mastersizer 3000). Figure 1 shows the particle size distribution results of Example 1. D50 means the diameter below which half of the population is located, and D90 means that 90% of the population is located below this value. As shown in Figure 1, it was confirmed that the particle size distribution of the alumina particles of Example 1 had a D50 of 6 μm and a D90 of less than 100 μm.

[0045] Table 1 shows the volatile content and bulk density of the dried granules of the aqueous solution of basic aluminum lactate. The volatile content was measured at 105°C for 30 minutes using an MX50 heat and dry moisture meter manufactured by A&D. The bulk density was measured in the same manner as the method for measuring the bulk density of alumina particles described below. Table 1 also shows the specific surface area (m 2 / g), bulk density (g / cm 3 ), crystal system, loss on drying (mass%), loss on ignition (mass%), and the contents of impurities such as sodium (Na), potassium (K), calcium (Ca), magnesium (Mg), silicon (Si), and iron (Fe) are also listed. The specific surface area was measured using an automatic specific surface area measuring device (Shimadzu Corporation Gemini7 2390) using the N 2The data shown here was obtained by measuring the bulk density and analyzing it using the BET method. The bulk density is calculated by dividing the mass by the volume. Specifically, the powder was sieved through a 1 mm mesh screen, and approximately 40 g of sample (M) was weighed to an accuracy of 0.1 mass%, placed in a 100 ml measuring cylinder (minimum unit: 1 ml), the surface was lightly smoothed, and the loose bulk volume (V 0 ) and bulk density: M / V 0 (g / cm 3 ) was calculated. The crystal system (crystal phase) is shown in Table 1 based on the results of measurement using an X-ray diffractometer (MiniFlex, manufactured by Rigaku Corporation) with a Cu target by the θ / 2θ method. FIG. 2 shows the measurement results of the crystal system of the alumina particles obtained in Example 1. The loss on drying and loss on ignition were measured in accordance with the measurement method for aluminum oxide in the Pharmaceutical and Medical Devices Raw Materials Standards 2021, and the results are shown in Table 1. The contents of Na, K, Ca, Si, Mg, and Fe were measured using energy dispersive X-ray fluorescence analysis (EDX) with a tabletop scanning electron microscope (SEM: JCM-7000, manufactured by JEOL Ltd.).

[0046] From the X-ray diffraction result of the alumina particles of Example 1 shown in FIG. 2, it was confirmed that the alumina particles of Example 1 were made of α-alumina.

[0047] 4, 5 and 6 are SEM images of the alumina particles of Example 1 measured using a field emission scanning electron microscope (FE-SEM: JSM-7001F manufactured by JEOL Ltd.). FIG. 4 is a 100,000x SEM image, and it is confirmed that the microcrystals of α-alumina are aggregated to form the outer skin of hollow spherical alumina. From the 10,000x SEM image of the alumina particles of Example 1 in FIG. 5, it is confirmed that the hollow spherical alumina particles have through holes. From the 25,000x SEM photograph of the alumina particles of Example 1 shown in FIG. 6, it is confirmed that the hollow spherical alumina is hollow. Therefore, it was confirmed that the alumina particles obtained in Example 1 are hollow spherical alumina particles.

[0048] Example 2 Using a 10 L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 1429.8 g of tap water to the kettle and add an aqueous aluminum chloride solution (Al 2 O 3 1909.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content: 23.0% by weight, Na 2 At the same time, 1660.8 g (18.0% Na equivalent in O) was added to obtain 5000 g of aluminum hydroxide gel solution.

[0049] Next, the obtained aluminum hydroxide gel solution was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated seven times. The obtained washed gel weighed 2190 g. Next, 103.2 g of the obtained washed gel was added to a 1 L glass separable flask placed on a mantle heater, and then 157.1 g of tap water was added and stirred for 30 minutes to obtain 260.3 g of slurry. Next, 39.7 g of lactic acid (lactic acid 90%) was added to the obtained slurry, and the mixture was heated and stirred at 100°C for 3 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution (Al 2 O 3 The resulting mixture had an Al content of 8.8% by mass, a basicity of 70.2%, sodium ions of 0.01% by mass, Si: 0.005% by mass, Ca: 0.0048% by mass, Mg: 0.0007% by mass, and Fe: 0.0015% by mass.

[0050] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 250°C, an outlet temperature of 110°C, and a gas pressure of 0.45 MPa using a nozzle. The collected dried granules (volatile content 5.2% and bulk density 0.39 g / cm 3 ) was placed in an alumina crucible and fired at 1150°C for 5 hours under peak firing conditions to obtain alumina particles.

[0051] The volatile content and bulk density of the dried granules of the basic aluminum lactate aqueous solution were measured in the same manner as in Example 1, and are shown in Table 1. In addition, the D50 and D90 of the particle size distribution, specific surface area, bulk density, crystal system, loss on drying and loss on ignition, and the contents of Na, K, Ca, Si, Mg and Fe of the obtained alumina particles were measured in the same manner as in Example 1, and the results are shown in Table 1. Although FE-SEM images and X-ray diffraction images are not shown, it was confirmed that the alumina particles had an α crystal system and were hollow spherical.

[0052] Example 3 Using a 10 L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 1429.8 g of tap water to the kettle and add an aqueous aluminum chloride solution (Al 2 O 3 1909.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content: 23.0% by weight, Na 2 At the same time, 1660.8 g of Na (calculated as O: 18.0%) was added to obtain 5000 g of an aluminum hydroxide gel solution.

[0053] Next, the gel solution obtained was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated seven times. The washed gel obtained weighed 2190 g. Next, 103.2 g of the washed gel obtained was added to a 1 L glass separable flask placed on a mantle heater, and then 157.1 g of tap water was added and stirred for 30 minutes to obtain 260.3 g of slurry. Next, 39.7 g of lactic acid (90% lactic acid) was added to the resulting slurry, which was heated and stirred at 100°C for 3 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution (Al 2 O 3 The resulting mixture had an Al content of 8.8% by mass, a basicity of 70.2%, sodium ions of 0.01% by weight, Si: 0.005% by mass, Ca: 0.0048% by mass, Mg: 0.0007% by mass, and Fe: 0.0015% by mass.

[0054] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 220°C, an outlet temperature of 95°C, and a gas pressure of 0.45 MPa using a nozzle. The collected dried granules (volatile content 6.0% and bulk density 0.45 g / cm 3 ) was placed in an alumina crucible and fired at 1100°C for 5 hours under peak firing conditions to obtain alumina particles.

[0055] The volatile content and bulk density of the dried granules of the basic aluminum lactate aqueous solution were measured in the same manner as in Example 1, and are shown in Table 1. In addition, the D50 and D90 of the particle size distribution, specific surface area, bulk density, crystal system, loss on drying and loss on ignition, and the contents of Na, K, Ca, Si, Mg and Fe of the obtained alumina particles were measured in the same manner as in Example 1, and the results are shown in Table 1. Although FE-SEM images and X-ray diffraction images are not shown, it was confirmed that the alumina particles had an α crystal system and were hollow spherical.

[0056] Example 4 Using a 10 L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 1531.6 g of tap water to the kettle and add an aqueous solution of aluminum chloride (Al 2 O 3 1909.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content 20.0% by weight, Na 2 At the same time, 1,559.0 g (18.9% Na equivalent in O) was added to obtain 5,000 g of an aluminum hydroxide gel solution.

[0057] Next, the gel solution obtained was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated seven times. The washed gel obtained weighed 1,920 g. Next, using a 1 L glass separable flask installed on a mantle heater, 103.2 g of the washed gel obtained was added, followed by 157.1 g of tap water, and stirred for 30 minutes to obtain 260.3 g of slurry. Next, 39.7 g of lactic acid (90% lactic acid) was added to the resulting slurry, which was heated and stirred at 100°C for 3 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution (Al 2 O 3 The resulting mixture had an Al content of 8.9 mass%, a basicity of 71.5%, sodium ions of 0.05 mass%, Si: 0.0052 mass%, Ca: 0.0040 mass%, Mg: 0.0006 mass%, and Fe: 0.0012 mass%.

[0058] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 250°C, an outlet temperature of 110°C, and a gas pressure of 0.45 MPa using a nozzle. The collected dried granules (volatile content 4.9% and bulk density 0.42 g / cm 3 ) was placed in an alumina crucible and fired at 1100°C for 5 hours under peak firing conditions to obtain alumina particles.

[0059] The volatile content and bulk density of the dried granules of the basic aluminum lactate aqueous solution were measured in the same manner as in Example 1, and are shown in Table 1. In addition, the D50 and D90 of the particle size distribution, specific surface area, bulk density, crystal system, loss on drying and loss on ignition, and the contents of Na, K, Ca, Si, Mg and Fe of the obtained alumina particles were measured in the same manner as in Example 1, and the results are shown in Table 1. Although FE-SEM images and X-ray diffraction images are not shown, it was confirmed that the alumina particles had an α crystal system and were hollow spherical.

[0060] Example 5 Using a 1L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 153.1g of tap water to the kettle and add an aqueous solution of aluminum chloride (Al 2 O 3190.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content 20.0% by weight, Na 2 At the same time, 155.9 g (18.9% Na equivalent in O) was added to obtain 500 g of an aluminum hydroxide gel solution.

[0061] Next, the gel solution obtained was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated five times. The washed gel obtained was 195 g. Next, using a 1 L glass separable flask installed on a mantle heater, 103.7 g of the washed gel obtained was added, followed by 156.6 g of tap water, and stirred for 30 minutes to obtain 260.3 g of slurry. Next, 39.7 g of lactic acid (90% lactic acid) was added to the obtained slurry, which was heated and stirred at 100°C for 1.5 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution (Al 2 O 3 The resulting mixture had an Al content of 8.6% by mass, a basicity of 72.4%, sodium ions of 0.02% by weight, Si: 0.0041% by mass, Ca: 0.0043% by mass, Mg: 0.0008% by mass, and Fe: 0.0017% by mass.

[0062] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 250°C, an outlet temperature of 110°C, and a gas pressure of 0.45 MPa using a nozzle. The collected dried granules (volatile content 5.7% and bulk density 0.37 g / cm 3 ) was placed in an alumina crucible and fired at 1100°C for 5 hours under peak firing conditions to obtain alumina particles exhibiting the α phase.

[0063] The volatile content and bulk density of the dried granules of the basic aluminum lactate aqueous solution were measured in the same manner as in Example 1 and are shown in Table 1. In addition, the D50 and D90 of the particle size distribution, specific surface area, bulk density, crystal system, loss on drying and loss on ignition, and the contents of Na, K, Ca, Si, Mg and Fe of the obtained alumina particles were measured in the same manner as in Example 1 and the results are shown in Table 2. Although FE-SEM images and X-ray diffraction images are not shown, it was confirmed that the alumina particles had an α crystal system and were hollow spherical.

[0064] Example 6 Using a 1L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 153.1g of tap water to the kettle and add an aqueous solution of aluminum chloride (Al 2 O 3 190.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content 20.0% by weight, Na 2 153.9g of 18.9% Na (O equivalent) and 2g of potassium aluminate powder were added at the same time to obtain 500g of aluminum hydroxide gel solution. Next, the obtained gel solution was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated five times. The obtained washed gel weighed 195g.

[0065] Next, 103.7 g of the obtained washing gel was added to a 1 L glass separable flask placed on a mantle heater, followed by 156.6 g of tap water, and the mixture was stirred for 30 minutes to obtain 260.3 g of slurry. Next, 39.7 g of lactic acid (90% lactic acid) was added to the obtained slurry, which was then heated and stirred at 100°C for 5 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution (Al 2 O 3 The resulting mixture had an Al content of 8.8% by mass, a basicity of 72.4%, sodium ions of 0.02% by weight, potassium ions of 0.01% by weight, Si: 0.0047% by mass, Ca: 0.0050% by mass, Mg: 0.0006% by mass, and Fe: 0.0011% by mass.

[0066] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 250°C, an outlet temperature of 110°C, and a gas pressure of 0.45 MPa using a nozzle. The collected dried granules (volatile content 5.8% and bulk density 0.44 g / cm 3 ) was placed in an alumina crucible and fired at 1100°C for 5 hours under peak firing conditions to obtain alumina particles.

[0067] The volatile content and bulk density of the dried granules of the basic aluminum lactate aqueous solution were measured in the same manner as in Example 1 and are shown in Table 1. In addition, the D50 and D90 of the particle size distribution, specific surface area, bulk density, crystal system, loss on drying and loss on ignition, and the contents of Na, K, Ca, Si, Mg and Fe of the obtained alumina particles were measured in the same manner as in Example 1 and the results are shown in Table 2. Although FE-SEM images and X-ray diffraction images are not shown, it was confirmed that the alumina particles had an α crystal system and were hollow spherical.

[0068] Example 7 Using a 10 L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 1429.8 g of tap water to the kettle and add an aqueous aluminum chloride solution (Al 2 O 3 1909.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content: 23.0% by weight, Na 2 At the same time, 1660.8 g of Na (calculated as O: 18.0%) was added to obtain 5000 g of an aluminum hydroxide gel solution.

[0069] Next, the gel solution obtained was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated seven times. The washed gel obtained weighed 2190 g. Next, 103.2 g of the washed gel obtained was added to a 1 L glass separable flask installed on a mantle heater, and then 157.1 g of tap water was added and stirred for 30 minutes to obtain 260.3 g of slurry. Next, 39.7 g of lactic acid (90% lactic acid) was added to the resulting slurry, and the mixture was heated and stirred at 100°C for 3 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution of the present invention (Al 2 O 3 The resulting mixture had an Al content of 8.8% by mass, a basicity of 70.2%, sodium ions of 0.01% by weight, Si: 0.0050% by mass, Ca: 0.0048% by mass, Mg: 0.0007% by mass, and Fe: 0.0015% by mass.

[0070] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 250°C, an outlet temperature of 110°C, and an atomizer at 18,000 rpm. The collected dried granules (volatile content 7.4% and bulk density 0.51 g / cm 3 ) was placed in an alumina crucible and fired at 1100°C for 5 hours under peak firing conditions to obtain hollow spherical alumina particles.

[0071] The volatile content and bulk density of the dried granules of the basic aluminum lactate aqueous solution were measured in the same manner as in Example 1 and are shown in Table 1. In addition, the D50 and D90 of the particle size distribution, specific surface area, bulk density, crystal system, loss on drying and loss on ignition, and the contents of Na, K, Ca, Si, Mg and Fe of the obtained alumina particles were measured in the same manner as in Example 1 and the results are shown in Table 2. Although FE-SEM images and X-ray diffraction images are not shown, it was confirmed that the alumina particles had an α crystal system and were hollow spherical.

[0072] Comparative Example 1 Using a 10 L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 1429.8 g of tap water to the kettle and add an aqueous aluminum chloride solution (Al 2 O 31909.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content: 23.0% by weight, Na 2 At the same time, 1660.8 g (18.0% Na equivalent in O) was added to obtain 5000 g of aluminum hydroxide gel solution.

[0073] Next, the gel solution obtained was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated seven times. The washed gel obtained weighed 2190 g. Next, using a 1 L glass separable flask installed on a mantle heater, 103.2 g of the washed gel obtained was added, followed by 157.1 g of tap water, and stirred for 30 minutes to obtain 260.3 g of slurry. Next, 39.7 g of lactic acid (90% lactic acid) was added to the resulting slurry, which was heated and stirred at 100°C for 3 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution (Al 2 O 3 The resulting mixture had an Al content of 8.8% by mass, a basicity of 70.2%, sodium ions of 0.01% by weight, Si: 0.0050% by mass, Ca: 0.0048% by mass, Mg: 0.0007% by mass, and Fe: 0.0015% by mass.

[0074] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 150°C, an outlet temperature of 65°C, and a gas pressure of 0.45 MPa using a nozzle. The collected dried granules (volatile content 12.5% ​​and bulk density 0.90 g / cm 3 ) was placed in an alumina crucible and fired at 1100°C for 5 hours under peak firing conditions to obtain alumina particles.

[0075] The volatile content and bulk density of the dried granules of the aqueous basic aluminum lactate solution were measured in the same manner as in Example 1 and are listed in Table 1. The D50 and D90 of the particle size distribution, the specific surface area, bulk density, crystal system, loss on drying and loss on ignition, and the contents of Na, K, Ca, Si, Mg, and Fe of the obtained alumina particles were measured in the same manner as in Example 1 and the results are listed in Table 3. Although no X-ray diffraction image is shown, it was confirmed that the alumina particles have an α crystal system. However, in Comparative Example 1, drying during spray drying was insufficient, so aggregates were generated during firing, and the particle size distribution D50 showed a large value of 530 μm.

[0076] Comparative Example 2 Using a 10 L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 1429.8 g of tap water to the kettle and add an aqueous aluminum chloride solution (Al 2 O 3 1909.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content: 23.0% by weight, Na 2 At the same time, 1660.8 g of Na (calculated as O: 18.0%) was added to obtain 5000 g of an aluminum hydroxide gel solution.

[0077] Next, the gel solution obtained was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated seven times. The washed gel obtained weighed 2190 g. Next, using a 1 L glass separable flask installed on a mantle heater, 103.2 g of the washed gel obtained was added, followed by 157.1 g of tap water, and stirred for 30 minutes to obtain 260.3 g of slurry. Next, 39.7 g of lactic acid (90% lactic acid) was added to the resulting slurry, which was heated and stirred at 100°C for 3 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution (Al 2 O 3 The resulting mixture had an Al content of 8.8% by mass, a basicity of 70.2%, sodium ions of 0.01% by weight, Si: 0.0050% by mass, Ca: 0.0048% by mass, Mg: 0.0007% by mass, and Fe: 0.0015% by mass.

[0078] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 250°C, an outlet temperature of 110°C, and a gas pressure of 0.45 MPa using a nozzle. The collected dried granules (volatile content 4.4% and bulk density 0.45 g / cm 3 ) was placed in an alumina crucible and fired at a peak firing condition of 800°C for 5 hours to obtain alumina particles.

[0079] The volatile content and bulk density of the dried granules of the basic aluminum lactate aqueous solution were measured in the same manner as in Example 1, and are shown in Table 1. Furthermore, the D50 and D90 of the particle size distribution, specific surface area, bulk density, crystal system, loss on drying and loss on ignition, and the contents of Na, K, Ca, Si, Mg and Fe of the obtained alumina particles were measured in the same manner as in Example 1, and the results are shown in Table 3. In Comparative Example 2, the final firing conditions were 800°C for 5 hours, and the crystal system was γ-alumina, not a single phase of α-alumina.

[0080] Comparative Example 3 Using a 10 L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 1429.8 g of tap water to the kettle and add an aqueous aluminum chloride solution (Al 2 O 3 1909.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content: 23.0% by weight, Na 2 At the same time, 1660.8 g (18.0% Na equivalent in O) was added to obtain 5000 g of aluminum hydroxide gel solution.

[0081] Next, the gel solution obtained was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated seven times. The washed gel obtained weighed 2190 g. Next, using a 1 L glass separable flask installed on a mantle heater, 103.2 g of the washed gel obtained was added, followed by 157.1 g of tap water, and stirred for 30 minutes to obtain 260.3 g of slurry. Next, 39.7 g of lactic acid (90% lactic acid) was added to the resulting slurry, which was heated and stirred at 100°C for 3 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution (Al 2 O 3 The resulting mixture had an Al content of 8.8% by mass, a basicity of 70.2%, sodium ions of 0.01% by weight, Si: 0.0050% by mass, Ca: 0.0048% by mass, Mg: 0.0007% by mass, and Fe: 0.0015% by mass.

[0082] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 250°C, an outlet temperature of 110°C, and a gas pressure of 0.45 MPa using a nozzle. The collected dried granules (volatile content 4.3% and bulk density 0.47 g / cm 3 ) was placed in an alumina crucible and fired at 1050°C for 1 hour under peak firing conditions.

[0083] The volatile content and bulk density of the dried granules of the basic aluminum lactate aqueous solution were measured in the same manner as in Example 1 and are shown in Table 1. Furthermore, the D50 and D90 of the particle size distribution, specific surface area, bulk density, crystal system, loss on drying and loss on ignition, and the contents of Na, K, Ca, Si, Mg and Fe of the obtained alumina particles were measured in the same manner as in Example 1 and the results are shown in Table 3. In Comparative Example 3, the final firing conditions were 1050°C for 1 hour, and the firing time was insufficient, and although an X-ray diffraction image is not shown, the alumina became a mixed alumina of α-alumina and γ-alumina, and not a single phase of α-alumina.

[0084] Comparative Example 4 Using a 10 L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 1429.8 g of tap water to the kettle and add an aqueous aluminum chloride solution (Al2 O 3 1909.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content: 23.0% by weight, Na 2 At the same time, 1660.8 g of Na (calculated as O: 18.0%) was added to obtain 5000 g of an aluminum hydroxide gel solution.

[0085] Next, the obtained gel solution was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated seven times. The obtained washed gel weighed 2190 g. Next, 103.2 g of the obtained washed gel was added to a 1 L glass separable flask installed on a mantle heater, followed by 152.1 g of tap water, and stirred for 30 minutes to obtain 255.3 g of slurry. Next, 34.7 g of lactic acid (90% lactic acid) and 10.0 g of calcium chloride were added to the obtained slurry, which was then heated and stirred at 100°C for 3 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution (Al 2 O 3 The resulting mixture had an Al content of 8.2% by mass, a basicity of 70.5%, sodium ions of 0.01% by weight, Si: 0.0050% by mass, Ca: 1.2% by mass, Mg: 0.0007% by mass, and Fe: 0.0015% by mass.

[0086] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 250°C, an outlet temperature of 110°C, and a gas pressure of 0.45 MPa using a nozzle. The collected dried granules (volatile content 4.6% and bulk density 0.50 g / cm 3 ) was placed in an alumina crucible and fired for 5 hours at 1100°C under peak firing conditions.

[0087] The volatile content and bulk density of the dried granules of the basic aluminum lactate aqueous solution were measured in the same manner as in Example 1, and are shown in Table 1. The D50 and D90 of the particle size distribution, the specific surface area, bulk density, crystal system, loss on drying and loss on ignition, and the contents of Na, K, Ca, Si, Mg, and Fe of the obtained alumina particles were measured in the same manner as in Example 1, and the results are shown in Table 3. Figure 3 shows the X-ray diffraction result of Comparative Example 4. The peak pattern is different from that in Figure 1, and it was confirmed that a composite oxide of aluminum and calcium was formed. Furthermore, the Ca value is high in the energy dispersive X-ray fluorescence evaluation results in Table 3.

[0088] Comparative Example 5 Using a 10 L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 1429.8 g of tap water to the kettle and add an aqueous aluminum chloride solution (Al 2 O 3 1909.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content: 23.0% by weight, Na 2 At the same time, 1660.8 g of Na (calculated as O: 18.0%) was added to obtain 5000 g of an aluminum hydroxide gel solution.

[0089] Next, the gel solution obtained was dehydrated using a centrifugal dehydrator, and the washed gel obtained was 2430 g. Water was added to the washed gel, and without additional washing, 103.2 g of the washed gel obtained was added to a 1 L glass separable flask placed on a mantle heater, followed by 157.1 g of tap water, and stirred for 30 minutes to obtain 260.3 g of slurry. Next, 39.7 g of lactic acid (90% lactic acid) was added to the obtained slurry, and the mixture was heated and stirred at 100°C for 3 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution (Al 2 O 3 A solution with a calculated Al content of 8.8% by mass, a basicity of 70.2%, sodium ion content of 1.7% by weight, Si: 0.0050% by mass, Ca: 0.0048% by mass, Mg: 0.0007% by mass, and Fe: 0.0015% by mass was prepared.

[0090] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) at an inlet temperature of 250°C, an outlet temperature of 110°C, and a gas pressure of 0.45 MPa using a nozzle. The collected dried granules (volatile content 7.5% and bulk density 0.54 g / cm 3 ) was placed in an alumina crucible and fired under peak firing conditions of 1100°C for 5 hours.

[0091] The volatile content and bulk density of the dried granules of the aqueous basic aluminum lactate solution were measured in the same manner as in Example 1, and are shown in Table 1. The D50 and D90 of the particle size distribution, specific surface area, bulk density, crystal system, loss on drying and loss on ignition, and the contents of Na, K, Ca, Si, Mg and Fe of the obtained alumina particles were measured in the same manner as in Example 1, and the results are shown in Table 4. In Comparative Example 5, it was confirmed that the alumina particles were not composed of α-alumina alone, since the amount of Na in the basic aluminum lactate solution was too high.

[0092] Comparative Example 6 Using a 10 L jacketed GL stirring kettle, first circulate 5°C cooling water through the jacket. Next, add 1429.8 g of tap water to the kettle and add an aqueous aluminum chloride solution (Al 2 O 3 1909.4 g of sodium aluminate solution (Al 2 O 3 Converted Al content: 23.0% by weight, Na 2 At the same time, 1660.8 g of Na (calculated as O: 18.0%) was added to obtain 5000 g of an aluminum hydroxide gel solution.

[0093] Next, the obtained gel solution was dehydrated using a centrifugal dehydrator, and the process of adding water and stirring was repeated seven times. The obtained washed gel weighed 2190 g. Next, using a 1 L glass separable flask installed on a mantle heater, 103.2 g of the obtained washed gel was added, followed by 157.1 g of tap water, and the mixture was stirred for 30 minutes to obtain 260.3 g of slurry. Next, 70 g of lactic acid (90% lactic acid) was added to the obtained slurry, which was heated and stirred at 100°C for 3 hours, and then slowly cooled to obtain 300 g of basic aluminum lactate solution (Al 2 O 3 The resulting mixture had an Al content of 8.8% by mass, a basicity of 45%, sodium ions of 0.01% by weight, Si: 0.0050% by mass, Ca: 0.0048% by mass, Mg: 0.0007% by mass, and Fe: 0.0015% by mass.

[0094] The obtained aqueous solution of basic aluminum lactate was granulated and dried using a spray dryer (TR-160 manufactured by PRIS Co., Ltd.) with an inlet temperature of 250°C, an outlet temperature of 110°C, and a gas pressure of 0.45 MPa using a nozzle, and the collected dried granules were placed in an alumina crucible and sintered under peak sintering conditions of 1100°C for 5 hours.

[0095] In Comparative Example 6, the basicity of the basic aluminum lactate was lower than the lower limit of 60% to 80%, so that the storage stability was poor, crystal precipitation occurred in the liquid during spray drying, causing clogging of the nozzle, and it was confirmed that spray drying could not be performed properly. This is shown in Table 4. In Tables 1 to 4, "nd" means that it was not possible to measure.

[0096] [Table 1]

[0097] [Table 2]

[0098] [Table 3]

[0099] [Table 4]

[0100] As shown in Tables 1 and 2, the hollow spherical alumina particles shown in Examples 1 to 7 all exhibit α-alumina, and it was confirmed by particle size distribution measurement that D50 was 5 to 50 μm and D90 was 200 μm or less. In addition, the loss on drying was 4 mass % or less, the loss on ignition was 6 mass % or less, and the bulk density was 0.4 to 0.7 g / cm. 3 In addition, when these hollow spherical alumina particles were subjected to elemental analysis using energy dispersive X-ray fluorescence, it was confirmed that they contained alkali metal element ions (Na and K) in the range of 0.005 to 1.2 mass %, and that the concentrations of Ca, Mg, Si, and Fe were not detected.

[0101] As shown in Table 3, in Comparative Example 1, drying during spray drying was insufficient (high volatile content), so aggregates were generated during firing, and it was confirmed that the particle size distribution D50 showed a large value of 530 μm. In Comparative Examples 2 and 3, the firing conditions were not appropriate, so the crystal systems were γ-alumina and α-alumina + γ-alumina, respectively, and it was confirmed that the α-alumina single phase was not formed. In Comparative Example 4, the Ca content was too high, so a composite oxide of aluminum and calcium was formed, and it was confirmed that the α-alumina single phase was not formed. As shown in Table 4, in Comparative Example 5, the Na content was too high, so β-alumina was formed together with α-alumina when fired, and it was confirmed that the α-alumina single phase was not formed.

[0102] The present invention also proposes the following aspects. [1] The basic aluminum lactate aqueous solution is dried and granulated at a temperature of 210 to 280°C under a gas pressure of 0.01 to 1 MPa in air or inert gas, and the volatile content of the granulated product is adjusted to 0 to 10% and the bulk density to 0.2 to 0.7 g / cm. 3 A first step of forming a hollow dry granule having a controlled diameter; A second step of calcining the dried granules obtained in the first step at a calcination temperature within a range of 1050°C or more and less than 1200°C for 2 to 8 hours to obtain hollow spherical alumina particles; The basic aluminum lactate aqueous solution contains iron (Fe) in an amount of 0 to 0.01 mass%, calcium (Ca) in an amount of 0 to 0.01 mass%, magnesium (Mg) in an amount of 0 to 0.01 mass%, silicon (Si) in an amount of 0.005 to 1.2 mass%, an alkali metal element ion in an amount of 0.005 to 1.2 mass%, a basicity of 60 to 80%, and aluminum is Al 2 O 3 It contains 8 to 13 mass% in terms of The obtained hollow spherical alumina particles have a D50 of 5 to 50 μm and a D90 of 200 μm or less in particle size distribution measurement, are hollow inside and have through holes on the outside, and have a specific surface area of ​​1 to 20 m. 2 / g, and the crystal phase is an α phase. [2] The hollow spherical alumina particles have a loss on drying of 4% or less, a loss on ignition of 6% or less, and a bulk density of 0.4 to 0.7 g / cm3, as determined by aluminum oxide analysis in accordance with the 2021 Standards for Pharmaceutical and Medical Devices. 3 The method for producing hollow spherical alumina particles according to [1], [3] The method for producing hollow spherical alumina particles according to [1] or [2], characterized in that the basic aqueous aluminum lactate solution is obtained by mixing an aluminum chloride solution with either or both of sodium aluminate and potassium aluminate, and water to form an aluminum hydroxide gel, washing the resulting gel with water, adding water to obtain an aluminum hydroxide slurry, and then adding lactic acid to cause a reaction. [4] The method for producing hollow spherical alumina particles according to any one of [1] to [3], wherein the drying and granulation in the first step is a spray drying method. [5] The method for producing hollow spherical alumina particles according to any one of [1] to [4], wherein the firing in the second step is carried out in air, nitrogen or an inert gas, or in vacuum.

Claims

1. The aqueous solution of basic aluminum lactate is dried and granulated at a temperature of 210 to 280°C under a gas pressure of 0.01 to 1 MPa in air or inert gas, and the volatile content of the granulated product is reduced to 0 to 10% and the bulk density to 0.2 to 0.7 g / cm. 3 A first step of forming a hollow dry granule having a controlled diameter; A second step of calcining the dried granules obtained in the first step at a calcination temperature within a range of 1050° C. or more and less than 1200° C. for 2 to 8 hours to obtain hollow spherical alumina particles; The basic aluminum lactate aqueous solution contains iron (Fe) in an amount of 0 to 0.01 mass %, calcium (Ca) in an amount of 0 to 0.01 mass %, magnesium (Mg) in an amount of 0 to 0.01 mass %, silicon (Si) in an amount of 0.005 to 1.2 mass %, an alkali metal element ion in an amount of 0.005 to 1.2 mass %, a basicity of 60 to 80%, and aluminum in an amount of Al 2 O 3 It contains 8 to 13 mass% in terms of The obtained hollow spherical alumina particles have a particle size distribution of D50 of 5 to 50 μm and D90 of 200 μm or less, are hollow inside and have through holes connecting to the outside, and have a specific surface area of ​​1 to 20 m. 2 / g, and the crystal phase is an α phase.

2. The hollow spherical alumina particles have a drying loss of 4% or less, an ignition loss of 6% or less, and a bulk density of 0.4 to 0.7 g / cm3, as determined by aluminum oxide analysis in accordance with the Pharmaceutical and Medical Devices Raw Materials Standards 2021. 3 2. The method for producing hollow spherical alumina particles according to claim 1,

3. 3. The method for producing hollow spherical alumina particles according to claim 1, wherein the basic aqueous aluminum lactate solution is obtained by mixing an aluminum chloride solution with either or both of sodium aluminate and potassium aluminate and water to form an aluminum hydroxide gel, washing the resulting gel with water, adding water to obtain an aluminum hydroxide slurry, and then adding lactic acid to cause a reaction.

4. 3. The method for producing hollow spherical alumina particles according to claim 1, wherein the drying and granulation in the first step is a spray drying method.

5. 3. The method for producing hollow spherical alumina particles according to claim 1, wherein the firing in the second step is carried out in air, nitrogen or an inert gas, or in vacuum.

Citation Information

Patent Citations

  • Washing machine with dryer

    JP1980068399A

  • Engine control device

    JP1988016153A

  • Basic aluminum lactate solution for forming ceramic, and production method of the same

    JP2023068864A

  • Method for producing hollow porous alumina particle

    JP2023129187A

  • Method and apparatus for producing alumina hollow particles

    JP4043805B2

Cited By

  • Spherical alumina detection method based on data analysis

    CN120063930A

  • Method for producing hollow spherical alumina particles

    JP2026168993A

  • Method for producing hollow spherical alumina particles

    JP7696670B1