Ultraviolet light emitting device
The ultraviolet light emitting device with a specific semiconductor layer structure and Al-containing region enhances power conversion efficiency and emission intensity, addressing the need for improved performance in illumination and sterilization applications.
Patent Information
- Application Number
- JP2020147118
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-01
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2040-09-01
AI Technical Summary
Ultraviolet light emitting elements require further improvement in power conversion efficiency to enhance their performance in applications such as illumination and sterilization.
The ultraviolet light emitting device incorporates a substrate, a first conductivity type nitride semiconductor layer containing Al and Ga, a light-emitting layer with Al and Ga, a second conductivity type nitride semiconductor layer with a different conductivity type, and an Al-containing region between the second conductivity type nitride semiconductor layer and a contact electrode, which reduces contact resistance and improves emission intensity.
The device achieves high power conversion efficiency and improved emission intensity by reducing contact resistance and optimizing the semiconductor layer structures, leading to enhanced performance in various applications.
Smart Images

Figure 0007560296000002 
Figure 0007560296000003 
Figure 0007560296000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to ultraviolet light emitting devices. [Background technology]
[0002] UV light emitting devices can control the emission wavelength by controlling the band gap energy of the light emitting layer, and have a long life and high reliability. Therefore, UV light emitting devices are used for various purposes such as lighting, light sources for measuring instruments, and light sources for sterilization. A typical UV light emitting device has a PIN structure on a substrate, with an emission layer sandwiched between a p-type nitride semiconductor and an n-type nitride semiconductor.
[0003] In order to improve the power conversion efficiency (WPE: Wall Plug Efficiency) of ultraviolet light emitting elements, it is necessary to improve the emission intensity (emission output) of the ultraviolet light emitting elements and reduce the series resistance. For this reason, a method has been studied in which a low-resistance p-type AlGaN layer is obtained as a nitride semiconductor layer constituting an ultraviolet light emitting element by alternately irradiating a group V gas and a group III gas containing C and Mg (for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5940355 [Patent Document 2] International Publication No. 2011-104969 Summary of the Invention [Problem to be solved by the invention]
[0005] However, there is a demand for further improvement in the power conversion efficiency of the ultraviolet light emitting elements as described above.
[0006] An object of the present disclosure is to provide an ultraviolet light emitting element with high power conversion efficiency. [Means for solving the problem]
[0007] In order to solve the above-mentioned problems, an ultraviolet light-emitting element according to one embodiment of the present disclosure is characterized by comprising a substrate, a first conductivity-type nitride semiconductor layer disposed on the substrate and containing Al and Ga, a light-emitting layer disposed on the first conductivity-type nitride semiconductor layer and containing a nitride semiconductor containing Al and Ga, a second conductivity-type nitride semiconductor layer disposed on the light-emitting layer and having a conductivity type different from that of the first conductivity-type nitride semiconductor layer, a contact electrode disposed on the second conductivity-type nitride semiconductor layer and containing at least Au, and an Al-containing region provided between the second conductivity-type nitride semiconductor layer and the contact electrode. Effect of the Invention
[0008] According to the present disclosure, it is possible to provide an ultraviolet light emitting element with high power conversion efficiency. [Brief description of the drawings]
[0009] [Figure 1] 1 is a cross-sectional view showing a configuration example of an ultraviolet light emitting element according to a first embodiment of the present disclosure. [Diagram 2] FIG. 4 is a cross-sectional view showing another configuration example of the ultraviolet light emitting device according to the first embodiment of the present disclosure. [Diagram 3] FIG. 4 is a cross-sectional view showing a configuration example of an ultraviolet light emitting element according to a second embodiment of the present disclosure. [Figure 4] FIG. 4 is a cross-sectional view showing a configuration example of an ultraviolet light emitting element according to a third embodiment of the present disclosure. [Diagram 5] FIG. 11 is a cross-sectional view showing a configuration example of an ultraviolet light emitting device according to a fourth embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The ultraviolet light emitting device according to the present embodiment will be described below through the embodiments, but the following embodiments do not limit the invention according to the claims. In addition, not all of the combinations of features described in the embodiments are necessarily essential to the solution of the invention.
[0011] 1. First embodiment Hereinafter, an ultraviolet light emitting element 1 according to the first embodiment will be described with reference to FIG. The ultraviolet light emitting element 1 is a semiconductor element capable of emitting ultraviolet light.
[0012] (1.1) Structure of ultraviolet light emitting element An ultraviolet light emitting element 1 according to the first embodiment will be described with reference to Fig. 1. The ultraviolet light emitting element 1 includes a substrate 11, a first conductivity type nitride semiconductor layer 12 that is disposed on the substrate and contains Al and Ga, a light emitting layer 13 that is disposed on the first conductivity type nitride semiconductor layer 11 and contains a nitride semiconductor that contains Al and Ga, and a second conductivity type nitride semiconductor layer 14 that is disposed on the light emitting layer 13 and has a conductivity type different from that of the first conductivity type nitride semiconductor layer 12. The ultraviolet light emitting element 1 also includes a second contact electrode 16B (an example of a contact electrode) that is disposed on the second conductivity type nitride semiconductor layer 14 and contains at least Au, and an Al-containing region 15 that is provided between the second conductivity type nitride semiconductor layer 14 and the second contact electrode 16B.
[0013] 1, the ultraviolet light emitting element 1 is configured by sequentially stacking a substrate 11, a first conductivity type nitride semiconductor layer 12, a light emitting layer 13, a second conductivity type nitride semiconductor layer 14, and an Al-containing region 15. The ultraviolet light emitting element 1 also includes a first contact electrode 16A connected to the first conductivity type nitride semiconductor layer 12, and a second contact electrode 16B connected to the Al-containing region 15. Each layer will be described in detail below.
[0014] (substrate) The substrate 11 may be made of any material that can be used as a semiconductor substrate, but may be a nitride semiconductor substrate containing a nitride semiconductor, such as an AlN single crystal substrate or an AlGaN substrate, or a sapphire substrate. Alternatively, the substrate 11 may be a laminate substrate in which an AlN layer (not shown) is disposed on an AlN single crystal substrate or a sapphire substrate. When the substrate 11 is a nitride semiconductor single crystal substrate such as AlN or AlGaN, the difference in lattice constant with the nitride semiconductor layer formed on the upper side of the substrate 11 becomes small, and threading dislocations can be reduced by growing the nitride semiconductor layer in a lattice-matched system.
[0015] Here, the wording "contains" in the expression "substrate 11 contains a nitride semiconductor..." means that the layer mainly contains a nitride semiconductor, but this expression also includes cases where other elements are contained. Specifically, this expression also includes cases where the composition of this layer is slightly changed by adding a small amount of other elements (for example, elements such as Ga (when Ga is not the main element), In, As, P, or Sb, at a few percent or less). In expressions of the compositions of other layers, the wording "contains" has a similar meaning. Also, the small amount of elements contained is not limited to the above.
[0016] The AlN layer is an example of an underlayer, and is formed on the entire surface of an AlN single crystal substrate, a sapphire substrate, etc. That is, the AlN layer is provided on the substrate 11 side of the first conductivity type nitride semiconductor layer 12. The AlN layer can recover pits and polishing marks formed on the surface of the AlN single crystal substrate or sapphire substrate. In addition, the difference in lattice constant and thermal expansion coefficient between the AlN layer and the first conductive type nitride semiconductor layer 12 is small, and a nitride semiconductor layer with few defects can be grown on the AlN layer. In addition, the AlN layer can grow the first conductive type nitride semiconductor layer 12 under compressive stress, and can suppress the occurrence of cracks in the first conductive type nitride semiconductor layer 12. Therefore, even if the substrate 11 is formed of a nitride semiconductor such as AlN or AlGaN, a nitride semiconductor layer with few defects can be grown above the substrate 11 via the AlN layer.
[0017] The AlN layer may contain impurities such as C, B, O, H, Si, Fe, and Mg. When AlN is used as the material for forming the substrate 11, the AlN layer and the substrate 11 are made of the same material, and therefore the boundary between the AlN layer and the substrate 11 becomes unclear. When the substrate 11 is made of AlN, the substrate 11 may be regarded as constituting the substrate 11 and the AlN layer.
[0018] The AlN layer has a thickness of, for example, several μm. Specifically, the thickness of the AlN layer is preferably greater than 10 nm and less than 3 μm. When the thickness of the AlN layer is greater than 10 nm, the recovery of the substrate surface advances and the crystallinity of AlN becomes high. In addition, from the viewpoint of raw material costs, the thickness of the AlN layer is preferably less than 3 μm.
[0019] The substrate 11 may be doped with a donor impurity or an acceptor impurity to be n-type or p-type. The substrate 11 may be a mixed crystal of a nitride semiconductor such as AlN and sapphire (Al2O3), Si, SiC, MgO, Ga2O3, ZnO, GaN, or InN.
[0020] The substrate 11 preferably has a layer thickness of, for example, 100 μm or more and 600 μm or less. The plane orientation may be c-plane (0001), a-plane (11-20), m-plane (10-10), etc., with the c-plane substrate 11 being more preferable.
[0021] (First conductivity type nitride semiconductor layer) The first-conductivity-type nitride semiconductor layer 12 is a layer of a nitride semiconductor containing Al and Ga. In the present disclosure, the first-conductivity-type nitride semiconductor layer 12 is electrically connected to the n-type first contact electrode 16A (details will be described later) and forms an n-type nitride semiconductor layer. The first-conductivity-type nitride semiconductor layer 12 is formed on the substrate 11. Here, for example, in the expression "the first-conductivity-type nitride semiconductor layer 12 is formed on the substrate 11", the word "on" means that the first-conductivity-type nitride semiconductor layer 12 is formed on the substrate 11. Also, the above expression includes the case where another layer further exists between the substrate 11 and the first-conductivity-type nitride semiconductor layer 12. In the relationship between other layers, the word "above" has the same meaning. For example, when the second-conductivity-type nitride semiconductor layer 14 is formed on the light-emitting layer 13 via an electron blocking layer (which will be described in detail in a modified example), it is also included in the expression "the second-conductivity-type nitride semiconductor layer 14 is formed on the light-emitting layer 13".
[0022] The first-conductivity-type nitride semiconductor layer 12 is, for example, A z Ga (1-z) N (0 < z < 1). Thus, when a material corresponding to the bandgap energy in the deep ultraviolet region is formed as the light-emitting layer 13, it is possible to enhance the crystallinity of the light-emitting layer 13 and improve the light-emitting efficiency. From the viewpoint of realizing high light-emitting efficiency, the nitride semiconductor constituting the first-conductivity-type nitride semiconductor layer 12 is preferably a mixed crystal of AlN and GaN. Also, from the viewpoint of the transmittance of the light emitted from the light-emitting layer 13, the first-conductivity-type nitride semiconductor layer 12 is more preferably formed by A z Ga (1-z) N (0.6 ≤ z ≤ 0.9).
[0023] The first-conductivity-type nitride semiconductor layer 12 may contain impurities such as group V elements other than N, such as P, As, and Sb, and impurities such as C, H, F, O, Mg, and Si, but the types of impurity elements are not limited to this. Moreover, the first conductivity type nitride semiconductor layer 12 and the second conductivity type nitride semiconductor layer 14 are layers of nitride semiconductors having mutually different conductivity types. In general, an n-type semiconductor has better crystallinity than a p-type semiconductor, and has less effect on the light emitting layer 13. For this reason, it is preferable that the first conductivity type nitride semiconductor layer 12 is an n-type, and the second conductivity type nitride semiconductor layer 14 is a p-type different from the first conductivity type nitride semiconductor layer 12.
[0024] From the viewpoints of relaxation and film resistance, first conductivity type nitride semiconductor layer 12 preferably has a layer thickness of 200 nm or more and 800 nm or less, more preferably 300 nm or more and 750 nm or less, and further preferably 300 nm or more and 500 nm or less.
[0025] (Light Emitting Layer) The light emitting layer 13 is a layer of a nitride semiconductor containing Al and Ga. The light emitting layer 13 is formed on the first conductive type nitride semiconductor layer 12. The nitride semiconductor contained in the light emitting layer 13 is preferably a mixed crystal of, for example, AlN or GaN, from the viewpoint of realizing high light emission efficiency. In addition to N, the light emitting layer 13 may contain impurities such as V group elements other than N, such as P, As, and Sb, and impurities such as C, H, F, O, Mg, and Si, but the types of impurity elements are not limited to these. The light emitting layer 13 may have a quantum well structure or a single layer structure. From the viewpoint of realizing high light emission efficiency, the light emitting layer 13 preferably has at least one well structure.
[0026] Furthermore, when it is desired to set the emission wavelength of the ultraviolet light-emitting element 1 to a wavelength in the deep ultraviolet region (380 nm or less), the nitride semiconductor constituting the light-emitting layer 13 preferably contains Al, Ga, and N. Furthermore, from the viewpoint of improving the light-emitting efficiency, the light-emitting layer 13 preferably has a multiple quantum well structure (MQW) having a quantum well layer containing Al, Ga, and N, and an electron barrier layer containing AlN (neither of which are shown).
[0027] (Second conductive type nitride semiconductor layer) As described above, the second conductivity type nitride semiconductor layer 14 is a layer of a nitride semiconductor having a conductivity type different from that of the first conductivity type nitride semiconductor layer 12. In the present disclosure, the second conductivity type nitride semiconductor layer 14 is electrically connected to a p-type second contact electrode 16B containing at least Au (details will be described later), forming a p-type nitride semiconductor layer. The second conductivity type nitride semiconductor layer 14 is formed on the light emitting layer 13. The nitride semiconductor constituting the second conductivity type nitride semiconductor layer 14 is formed of, for example, GaN, AlN or InN, or a mixed crystal containing these.
[0028] The second conductivity type nitride semiconductor layer 14 contains dopant atoms. The dopant atoms are preferably at least one of Mg, Zn, and Be, and in view of the versatility of the source gas, it is more preferable that the impurity contained in the second conductivity type nitride semiconductor layer 14 is Mg. The second conductivity type nitride semiconductor layer 14 may also contain impurities such as Group V elements other than N, such as P, As, and Sb, and C, H, F, O, and Si. However, as described above, it is preferable that the conductivity type of the first conductivity type nitride semiconductor layer 12 is n-type and the conductivity type of the second conductivity type nitride semiconductor layer 14 is p-type.
[0029] In the second conductivity type nitride semiconductor layer 14, the concentration of dopant atoms (hereinafter referred to as dopant atom concentration) has a concentration distribution in the thickness direction of the second nitride semiconductor layer 14. The dopant atom concentration in a central region 14A in the thickness direction of the second conductivity type nitride semiconductor layer 14 is preferably lower than the dopant atom concentration in an end region 14B in the thickness direction of the second conductivity type nitride semiconductor layer 14. Here, the end region 14B refers to the regions at both ends in the thickness direction of the second conductivity type nitride semiconductor layer 14. This is for the purpose of improving the contact between the second conductivity type nitride semiconductor layer 14 and an electrode (second contact electrode 16B) or a semiconductor layer (light emitting layer 13) arranged on the substrate 11 side of the second conductivity type nitride semiconductor layer 14.
[0030] For example, if the dopant atom concentration is increased in a state where the dopant atoms are uniformly distributed in the second conductivity type nitride semiconductor layer 14, electrons are generated from dislocations caused by lattice disorder, resulting in a decrease in the hole concentration. On the other hand, if the dopant atom concentration in both end regions 14B of the second conductivity type nitride semiconductor layer 14 is increased more than that in the central region 14A, a pseudo tunnel junction is formed between the second conductivity type nitride semiconductor layer 14 and a layer in contact with the second conductivity type nitride semiconductor layer 14. This reduces the contact resistance between the second conductivity type nitride semiconductor layer 14 and a layer in contact with the second conductivity type nitride semiconductor layer 14.
[0031] From the viewpoint of contact resistance, the Mg concentration in the end region 14B of the second conductive type nitride semiconductor layer 14 is 8×10 19 cm -3 More than 1×10 21 cm -3 Preferably, 5×10 20 cm -3 More than 1×10 21 cm -3 Similarly, the Mg concentration in the central region 14A of the second conductive type nitride semiconductor layer 14 is preferably 1×10 18 cm -3 More than 4×10 19 cm -3 Preferably, 5×10 18 cm -3 More than 4×10 19 cm -3 The same applies to the concentrations of dopant atoms other than Mg.
[0032] There is also a suitable range for the concentration distribution of dopant atoms in second conductivity type nitride semiconductor layer 14. The thickness of the region with high dopant atom concentration is preferably 5% to 50% of the entire film thickness of second conductivity type nitride semiconductor layer 14. Here, the "region with a high dopant atom concentration (hereinafter sometimes referred to as a high dopant concentration region)" refers to a region in the thickness direction of second conductivity type nitride semiconductor layer 14 from the point where the peak dopant atom concentration is obtained to the point where the dopant atom concentration is 50%. Furthermore, when both end regions 14B of the second conductivity type nitride semiconductor layer 14 are "regions with a high dopant atom concentration," the "film thickness of the regions with a high dopant atom concentration" refers to the total thickness of the film thicknesses of both end regions 14B.
[0033] The thickness of the second conductive type nitride semiconductor layer 14 is preferably 2 nm or more and 200 nm or less, and more preferably 3 nm or more and 200 nm or less from the viewpoint of contact resistance and light absorption. The thinner the thickness of the second conductive type nitride semiconductor layer 14, the higher the emission intensity of the ultraviolet light emitting element 1, and the thicker the layer thickness, the lower the emission intensity of the ultraviolet light emitting element 1. On the other hand, the thinner the layer thickness of the second conductive type nitride semiconductor layer 14, the higher the threshold voltage of the ultraviolet light emitting element 1, and the thicker the layer thickness, the lower the threshold voltage of the ultraviolet light emitting element 1. Therefore, when the thickness of the second conductive type nitride semiconductor layer 14 is 2 nm or more and 200 nm or less, the threshold voltage does not become too high while maintaining a high emission intensity, and the device characteristics of the ultraviolet light emitting element 1 are improved overall.
[0034] From the viewpoint of improving the IV characteristics (electrical characteristics) of the ultraviolet light emitting device 1, the coverage of the second conductivity type nitride semiconductor layer 14 with respect to the layer immediately below is preferably 80% or more and 100% or less, and more preferably 90% or more and 100% or less. From the viewpoint of increasing the carrier injection efficiency of the ultraviolet light emitting device 1 as a p-type semiconductor, the second conductivity type nitride semiconductor layer 14 is preferably made of AlGaN (0≦x≦0.2). From the viewpoint of increasing the carrier injection efficiency, it is preferable that the second conductivity type nitride semiconductor layer 14 is epitaxially grown coherently from the layer immediately below and is lattice-matched with the layer immediately below. More specifically, it is preferable that the lattice constant in the in-plane a-axis direction parallel to the upper surface of the substrate 11 matches the lattice constant in the same direction of the layer immediately below, that is, it is matched with the layer immediately below. At the same time, it is preferable that atoms (e.g., Mg) contained as impurities are substituted for the lattices of Ga or Al and N. This makes it possible to obtain the second conductivity type nitride semiconductor layer 14 having high carrier injection efficiency and excellent IV characteristics.
[0035] (Al-containing area) The Al-containing region 15 is a layer containing at least Al atoms, and is provided between the second conductive type nitride semiconductor layer 14 and the second contact electrode 16B. Here, for example, the wording "between" in the expression "between the second conductive type nitride semiconductor layer 14 and the second contact electrode 16B" means that the Al-containing region 15 is formed in a region sandwiched between the second conductive type nitride semiconductor layer 14 and the second contact electrode 16B. In this case, a layer other than the Al-containing region 15 may be further provided between the second conductive type nitride semiconductor layer 14 and the second contact electrode 16B. For example, a layer formed of another metal or nitride semiconductor may be included between the second conductive type nitride semiconductor layer 14 and the second contact electrode 16B. In addition, among the layers constituting the ultraviolet light-emitting device 1, there may be other layers containing Al atoms, but here, the layer containing Al atoms located between the second conductivity-type nitride semiconductor layer 14 and the second contact electrode 16B is defined as the Al-containing region 15. In this case, the film thickness of the Al-containing region 15 is defined as the total film thickness of all the layers containing Al atoms.
[0036] Examples of the Al-containing region 15 include an elemental Al region made of elemental Al, an Al alloy region made of an Al alloy, and a nitride semiconductor region containing Al. The Al-containing region 15 is not limited to these layers and may contain other elements. Furthermore, the Al-containing region 15 may have a structure in which two or more of these layers are stacked.
[0037] The provision of the Al-containing region 15 reduces the contact resistance between the second conductivity type nitride semiconductor layer 14 and the second contact electrode 16B. Both ends of the second conductivity type nitride semiconductor layer 14 are doped with a high concentration of impurities, so a pinning effect is observed. Therefore, the Schottky barrier height is not determined by the work function of the metal. Various studies have shown that the presence of the Al-containing region 15, which contains Al, at the interface between the second conductivity type nitride semiconductor layer 14 and the second contact electrode 16B reduces the contact resistance between the second conductivity type nitride semiconductor layer 14 and the second contact electrode 16B.
[0038] Furthermore, when a nitride semiconductor region such as an AlGaN layer exists as the Al-containing region 15, piezoelectric polarization occurs according to the lattice constant difference. This, combined with the spontaneous polarization of the nitride semiconductor layer, generates two-dimensional electron gas at the interface. Due to the band structure, these electrons form a tunnel junction and contribute to hole injection. These effects reduce the contact resistance. Furthermore, when a simple Al region and an Al alloy region formed of an Al alloy are present as the Al-containing region 15, light emitted from the light-emitting layer 13 and traveling in the opposite direction to the substrate 11 travels toward the substrate 11 due to reflection by Al. This improves the emission intensity of the ultraviolet light-emitting element 1. Therefore, when the Al-containing region 15 includes a simple Al region and an Al alloy region formed of an Al alloy, the power conversion efficiency (WPE) is improved due to the reduced contact resistance and the increased emission intensity.
[0039] From the viewpoint of such a mechanism, it is preferable that the thickness of the Al-containing region 15 is 0.5 nm or more and 5 nm or less. When the thickness of the Al-containing region 15 is within the above range, it is possible to obtain high emission intensity and a low threshold voltage while maintaining a high power conversion efficiency (WPE).
[0040] (Contact electrode) The ultraviolet light-emitting element 1 further includes a second contact electrode 16B disposed on the second conductive type nitride semiconductor layer 14 and containing at least Au. The ultraviolet light-emitting element 1 also includes a first contact electrode 16A connected to the first conductive type nitride semiconductor layer 12. The first contact electrode 16A and the second contact electrode 16B may be at least one of an n-type electrode and a p-type electrode. In the ultraviolet light-emitting element 1 of the present disclosure, the first contact electrode 16A is an n-type electrode, and the second contact electrode 16B is a p-type electrode containing at least Au.
[0041] The first contact electrode 16A, which is an n-type electrode, is formed of a metal such as Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zr, or the like, a mixed crystal thereof, or a conductive oxide such as ITO or Ga2O3. The n-type electrode is preferably formed so as to contact the layer having n-type conductivity out of the first conductivity type nitride semiconductor layer 12 and the second conductivity type nitride semiconductor layer 14. In FIG. 1, the first contact electrode 16A connected to the first conductivity type nitride semiconductor layer 12 is an n-type electrode.
[0042] The second contact electrode 16B, which is a p-type electrode, contains at least Au. The second contact electrode 16B is further formed of a metal such as Ni, Pt, Ru, Ag, Rh, Pd, Pt, Cu, Al, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Co, Ir, Zr, etc., preferably any one of Ti, Pt, Rd, Ru, Ni and Rh, a mixed crystal thereof, or a conductive oxide such as ITO or Ga2O3. The p-type electrode is preferably formed so as to contact the layer having p-type conductivity of the first conductive type nitride semiconductor layer 12 and the second conductive type nitride semiconductor layer 14. As described above, in FIG. 1, the second contact electrode 16B connected to the Al-containing region 15 is a p-type electrode.
[0043] (1.2) Modifications of ultraviolet light emitting devices The ultraviolet light emitting device 1A described above may include an electron blocking layer 17 provided between the light emitting layer 13 and the second conductivity type nitride semiconductor layer . The electron blocking layer 17 will be described in detail below with reference to FIG.
[0044] (Electron Block Layer) The electron blocking layer 17 has a function of preventing electrons injected from the first conductive type nitride semiconductor layer 12 from recombining in the light emitting layer 13 and overflowing to the second conductive type nitride semiconductor layer 14. For example, the electron blocking layer 17 is made of GaN, AlN, or InN, or a mixed crystal containing these. However, the electron blocking layer 17 is not limited to being made of these materials as long as it can prevent the overflow of electrons. The electron blocking layer 17 may contain impurities such as V group elements other than N, such as P, As, and Sb, and C, H, F, O, Mg, Si, and Be. From the viewpoints of lattice matching and electron blocking effect, the electron blocking layer 17 is preferably made of AlGaN having a band gap larger than that of the light emitting layer 13.
[0045] (1.3) Manufacturing method of ultraviolet light emitting element The ultraviolet light emitting device 1 of this embodiment is manufactured through the process of forming each layer on a substrate 11. The substrate 11 is formed by a general substrate growth method such as a vapor phase growth method, such as a sublimation method or a hydride vapor phase epitaxy (HVPE) method, or a liquid phase growth method.
[0046] The process of forming each layer on the substrate 11 can be performed by, for example, a molecular beam epitaxy (MBE) method, a hydride vapor phase epitaxy (HVPE) method, a metal organic chemical vapor deposition (MOCVD) method, or the like. Here, among the layers formed on the substrate 11, the nitride semiconductor layer can be formed using an Al source containing, for example, trimethylaluminum (TMAl), a Ga source containing, for example, trimethylgallium (TMGa) or triethylgallium (TEGa), or an N source containing, for example, ammonia (NH3).
[0047] The ultraviolet light emitting element 1 is manufactured through a process of removing unnecessary portions of each layer formed on the substrate 11 by etching (see FIG. 1). This process can be performed by, for example, inductively coupled plasma (ICP) etching or the like. The ultraviolet light emitting element 1 can be manufactured through a process of forming electrodes (first contact electrode 16A, second contact electrode 16B). This process can be performed by various methods, such as evaporating metal by electron beam deposition (EB) method. Here, the ultraviolet light emitting element is manufactured by dividing the substrate 11 on which each layer has been formed through the above-mentioned steps into individual pieces by dicing.
[0048] The electrodes such as the first contact electrode 16A and the second contact electrode 16B are formed by resistance heating deposition, electron gun deposition, sputtering, or the like, but are not limited to these methods. The electrodes may be formed as a single layer or may be formed by laminating multiple layers. In addition, the electrodes may be heat-treated in an oxygen, nitrogen, or air atmosphere after the layers are formed.
[0049] (1.4) Measurement methods for the physical properties of ultraviolet light-emitting devices The physical properties of the above-mentioned ultraviolet light emitting device 1 can be measured as follows.
[0050] (Measurement of impurity concentration, doping atom concentration and distribution film thickness of second conductive type nitride semiconductor layer) The impurity concentration, doping atom concentration, and distribution of impurities and doping atoms contained in the second conductive type nitride semiconductor layer 14 can be obtained by atomic mapping. Atom Probe Tomography (APT) can be used for atomic mapping. In the APT analysis of the second conductive type nitride semiconductor layer 14, a multilayer film portion to be observed is processed into a needle-shaped sample having a tip curvature radius of about 100 nm by a focused ion beam (FIB) processing device (manufactured by Toshiba). If an electrode is formed on the surface of the semiconductor multilayer film, the electrode is left as it is, and if no electrode is formed, a tungsten protective film is formed and processed into a needle-shaped sample by FIB. In processing into a needle-shaped sample, the vertical direction of the film of the semiconductor laminate is processed to be the axial direction of the needle-shaped sample, and the portion to be observed is located near the tip.
[0051] Next, a voltage pulse is applied to the needle-shaped sample, or a voltage pulse is applied and a laser pulse is irradiated to the observation area. The ion species are identified by mass analysis of the ions released from the tip of the needle-shaped sample, and the position within the needle-shaped sample from which the ions were released is identified by a two-dimensional detector, thereby obtaining the three-dimensional distribution of atoms within the needle-shaped sample. As described above, the APT method is used to observe the mapping of atoms in the film in the depth direction. Also, by extracting the line profile in the cross section in the depth direction, the film thickness of the concentration distribution can be obtained.
[0052] The method for measuring the concentration of impurities or doping atoms and the distributed film thickness by the APT method is described below. From the 3D data of the needle-shaped sample thus formed, a region corresponding to 50% of the region of the sample center in the in-plane direction perpendicular to the depth direction is removed, and a line profile in the depth direction is obtained for a plurality of points (for example, any 5 points). Then, the peak values of the atomic concentration in the high dopant concentration region of the second conductive type nitride semiconductor layer 14 are set as the doping atomic concentrations. That is, when the doping atomic concentration in the end regions 14B at both ends of the second conductive type nitride semiconductor layer 14 is higher than the doping concentration in the central region 14A, the peak values of the atomic concentration in the end regions 14B at both ends of the second conductive type nitride semiconductor layer 14 are set as the doping atomic concentrations.
[0053] When there is a difference between the concentration values at each measurement point, the higher concentration is taken as the concentration of impurities or doping atoms in the high dopant concentration region (e.g., edge region 14B) in the thickness direction. In addition, when the rate of change in concentration per 1 nm in the thickness direction of second conductivity type nitride semiconductor layer 14 is obtained, the concentration at the point where the lowest rate of change is obtained is taken as the concentration of impurities or doping atoms in the region other than the high dopant concentration region (e.g., central region 14A). The concentrations in edge region 14B and central region 14A are each taken as the average value at any five points, for example.
[0054] Next, the concentration distribution film thickness will be described. The point from where the peak concentration is obtained in the high dopant concentration region (e.g., end region 14B) to where the concentration is 50% is defined as the region with high concentration, i.e., the high dopant concentration region, and the film thickness of the high dopant concentration region is specified. At this time, when there are multiple high dopant concentration regions (e.g., when there are multiple end regions 14B as shown in FIG. 1), the total film thickness of the multiple high dopant concentration regions is defined as the film thickness of the high dopant concentration region.
[0055] (Measurement of coverage of second conductive type nitride semiconductor layer) The coverage of the second conductivity type nitride semiconductor layer 14 is measured using, for example, a scanning electron microscope (FE-SEM "SU9000" manufactured by Hitachi High-Technologies Corporation) and image processing software (image analysis software "A-zo-kun" (registered trademark) manufactured by Asahi Kasei Engineering Co., Ltd.). More specifically, during SEM measurement, the exposed surface of the second conductivity type nitride semiconductor layer 14 is measured at three arbitrary points within a measurement range of 50 μm×50 μm. At this time, a backscattered electron image is obtained by the lower detector, thereby obtaining an SEM image in which the contrast due to composition differences is clear.
[0056] The obtained SEM image is processed using image processing software. Areas in the SEM image whose brightness is 50% or more lower than the average brightness are determined to be areas that are not covered by second conductivity type nitride semiconductor layer 14 with respect to light emitting layer 13, which is the layer directly below. The coverage is the ratio of the covered area, and the average value of any three points is determined to be the coverage of second conductivity type nitride semiconductor layer 14.
[0057] (Measurement of impurity and doping concentrations) The concentrations of dopants and impurities contained in the substrate 11 and each layer constituting the ultraviolet light emitting device 1 can be measured by secondary ion mass spectrometry (SIMS). When the concentration of dopants and impurities contained in each layer is measured by SIMS after processing into a device, the measurement can be performed in a state where the electrodes are removed by chemical etching or physical polishing. The concentration of dopants and impurities contained in each layer can also be measured by sputtering from the substrate 11 side where no electrodes are formed. Specifically, SIMS measurements are performed under the measurement conditions provided by Evans Analytical Group (EAG), Inc. A cesium (Cs) ion beam with an energy of 14.5 keV is used to sputter the sample during the measurements.
[0058] (Layer thickness measurement method) The thickness of each layer constituting the ultraviolet light emitting element 1 can be measured by cutting out a predetermined cross section perpendicular to the substrate 11, observing this cross section with a transmission electron microscope (TEM), and using the length measurement function of the TEM. As a measurement method, first, a cross section perpendicular to the main surface of the substrate 11 of the ultraviolet light emitting element is observed using a TEM. Specifically, for example, an observation width is set to a range of 2 μm or more in a direction parallel to the main surface of the substrate 11 in a TEM image showing a cross section perpendicular to the main surface of the substrate 11 of the ultraviolet light emitting element 1. Since contrast is observed at the interface between two layers with different compositions within this observation width, the thickness up to this interface is observed in a continuous observation region with a width of 200 nm. The average value of the thickness of each layer included in this 200 nm wide observation region can be calculated from five points arbitrarily extracted from the above-mentioned observation width of 2 μm or more to obtain the layer thickness of each layer.
[0059] (Method of measuring the Al composition of the first conductivity type nitride semiconductor layer) The Al composition of the first conductivity type nitride semiconductor layer 12 can be measured by reciprocal space mapping (RSM) using an X-ray diffraction (XRD) method. Specifically, the lattice relaxation rate and Al composition relative to the underlayer can be obtained by analyzing reciprocal space mapping data in the vicinity of a diffraction peak obtained using an asymmetric plane as a diffraction plane. Examples of the diffraction plane include the (10-15) plane and the (30-24) plane.
[0060] (Method for measuring the Al composition of the light-emitting layer) It can be measured by X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray spectroscopy (EDX), and electron energy-loss spectroscopy (EELS). In EELS, the composition of a sample is analyzed by measuring the energy lost when an electron beam passes through the sample. Specifically, for example, the energy loss spectrum of the intensity of the transmitted electron beam is measured and analyzed for a thin-sectioned sample used in TEM observation. The position of the peak that appears around 20 eV of energy loss changes depending on the composition of each layer, and the composition can be determined from the peak position. In the same manner as in the method for calculating layer thickness by TEM observation described above, the Al composition of each layer is obtained by calculating the average value of the Al composition in an observation width of 200 nm from five points arbitrarily selected from an observation region of 2 μm or more.
[0061] In EDX, characteristic X-rays generated by an electron beam in a thin-sectioned sample used in the above-mentioned TEM observation, etc. are measured and analyzed. In the same manner as the method for calculating layer thickness using TEM observation described above, the Al composition of each layer is obtained by calculating the average value of the Al composition in an observation width of 200 nm from five points arbitrarily selected from an observation region of 2 μm or more.
[0062] In XPS, the evaluation in the depth direction can be performed by performing XPS measurement while performing sputter etching using an ion beam. Although Ar+ is generally used as the ion beam, other ion species such as Ar cluster ions may be used as long as they can be irradiated by an etching ion gun mounted on the XPS device. The XPS peak intensities of Al, Ga, and N are measured and analyzed to obtain the depth direction distribution of the Al composition of each layer. Instead of sputter etching, the ultraviolet light emitting element may be obliquely polished so that a cross section perpendicular to the main surface of the substrate 11 is enlarged and exposed, and the exposed cross section may be measured by XPS. The composition of each layer can be measured not only by XPS but also by Auger Electron Spectroscopy (AES). In this case, the composition can be measured by Auger Electron Spectroscopy on a cross section exposed by sputter etching or oblique polishing. The composition of each layer can also be measured by SEM-EDX measurement of a cross section exposed by oblique polishing.
[0063] (Method of identifying film thickness and elements in Al-containing region) The Al-containing region 15 can be identified by using the above-mentioned transmission electron microscope (TEM) and energy dispersive X-ray analysis (EDX) in combination. Specifically, a predetermined cross section perpendicular to the substrate 11 is cut out and the cross section is subjected to EDX measurement, whereby the range of the region containing Al atoms (i.e., the thickness of the Al-containing region 15) can be identified. In this case, EDX allows identification based on an element-specific energy peak, so it is possible to identify whether the Al-containing region 15 is a simple Al region, an Al alloy region, or an Al-containing nitride semiconductor region.
[0064] Next, the film thickness of the Al-containing region 15 can be measured by observing it with a TEM and using the length measuring function of the TEM. As a measuring method, first, a cross section perpendicular to the main surface of the substrate 11 of the ultraviolet light emitting element 1 is observed using a TEM. Specifically, for example, a range of 2 μm or more in a direction parallel to the main surface of the substrate 11 in a TEM image showing a cross section perpendicular to the main surface of the substrate 11 is set as the observation width. Within this observation width, the region containing Al atoms previously identified by EDX is observed in a continuous observation region with a width of 200 nm. The average value of the thickness of the region containing Al atoms contained in this 200 nm wide observation region is calculated from five points arbitrarily extracted from the above-mentioned observation width of 2 μm or more, thereby obtaining the film thickness of the Al-containing region 15. Similar results can also be obtained by the APT method described above. When the APT method is used, the Al concentration can be obtained with high resolution, so that it is more effective than EDX measurement when the Al-containing region 15 is thin.
[0065] (Measurement of atomic arrangement in nitride semiconductor layers) The atomic arrangement of each layer constituting the ultraviolet light emitting device 1 can be measured by high-resolution TEM measurement. The sample that was exfoliated to 50 nm during the above-mentioned TEM measurement is subjected to high-resolution TEM measurement using an atomic resolution analytical electron microscope (manufactured by JEOL Ltd., "JEM-ARM200F" (accelerating voltage: 200 kV). The atomic arrangement is a state in which group III atoms and nitrogen atoms are alternately stacked, and if it is observed that the group III atoms are vertically arranged (i.e., there is no misalignment), it can be determined that there is lattice matching. Furthermore, it can be observed that Mg is substituted into the lattice as an impurity because there are no dangling atoms between the atoms.
[0066] (1.5) Application fields of ultraviolet light emitting devices The ultraviolet light emitting element according to this embodiment can be applied to devices in, for example, the medical and life science fields, the environmental field, the industrial and manufacturing fields, the lifestyle and home appliances fields, the agricultural field, and other fields. The ultraviolet light emitting element can be applied to a drug or chemical substance synthesis and decomposition device, a liquid / gas / solid (container, food, medical equipment, etc.) sterilization device, a semiconductor cleaning device, etc., a surface modification device for film, glass, metal, etc., an exposure device for manufacturing semiconductors, FPD, PCB, and other electronic products, a printing and coating device, an adhesive and sealing device, a transfer and molding device for film, pattern, mockup, etc., and a measurement and inspection device for banknotes, wounds, blood, chemical substances, etc.
[0067] Examples of liquid sterilization equipment include, but are not limited to, automatic ice makers, ice trays and ice storage containers in refrigerators, water tanks for ice makers, freezers, ice makers, humidifiers, dehumidifiers, cold water tanks, hot water tanks and flow piping for water servers, freezer-type water purifiers, portable water purifiers, water supply units, hot water heaters, wastewater treatment equipment, garbage disposers, toilet drain traps, washing machines, water sterilization modules for dialysis, connector sterilizers for peritoneal dialysis, and disaster water storage systems.
[0068] Examples of gas sterilization devices include, but are not limited to, air purifiers, air conditioners, ceiling fans, floor or bedding vacuum cleaners, futon dryers, shoe dryers, washing machines, clothes dryers, indoor germicidal lamps, storage ventilation systems, shoe boxes, chests of drawers, etc.
[0069] Examples of solid sterilization equipment (including surface sterilization equipment) include, but are not limited to, vacuum packing machines, belt conveyors, hand tool sterilization equipment for medical, dental, barber, and beauty salon use, toothbrushes, toothbrush holders, chopstick cases, cosmetic pouches, drain covers, toilet spot cleaners, and toilet lids.
[0070] (1.6) Effects of the First Embodiment The ultraviolet light emitting element according to the first embodiment has the following effects. (1) The ultraviolet light-emitting element 1 is disposed on a second conductivity-type nitride semiconductor layer 14 and has a contact electrode containing at least Au, and also has an Al-containing region provided between the second conductivity-type nitride semiconductor layer 14 and the contact electrode. This allows the ultraviolet light emitting element 1 to have a reduced contact resistance between the second conductivity type nitride semiconductor layer 14 and the second contact electrode 16B, thereby achieving high power conversion efficiency.
[0071] (2) It is preferable that the contact electrode of the ultraviolet light emitting element 1 contains any one of Ti, Pt, Rd, Ru, Ni, and Rh. This allows the ultraviolet light emitting element 1 to obtain a higher reflectance in the ultraviolet range, and therefore a higher power conversion efficiency.
[0072] (3) The ultraviolet light emitting element 1 preferably has an Al-containing region, which is a nitride semiconductor region containing Al. This allows the ultraviolet light emitting element 1 to have a reduced contact resistance between the second conductivity type nitride semiconductor layer 14 and the second contact electrode 16B, thereby achieving high power conversion efficiency.
[0073] (4) The ultraviolet light emitting device 1 preferably has, as the Al-containing region, a simple Al region made of simple Al. As a result, in the ultraviolet light-emitting element 1, light emitted from the light-emitting layer 13 and traveling in the opposite direction to the substrate 11 is reflected by the substrate 11, thereby improving the luminous intensity of the ultraviolet light-emitting element 1 and further improving the power conversion efficiency (WPE).
[0074] (5) The ultraviolet light emitting device 1 preferably has, as the Al-containing region, an Al alloy region made of an Al alloy. As a result, in the ultraviolet light-emitting element 1, light emitted from the light-emitting layer 13 and traveling in the opposite direction to the substrate 11 is reflected by the substrate 11, thereby improving the luminous intensity of the ultraviolet light-emitting element 1 and further improving the power conversion efficiency (WPE).
[0075] (6) In the ultraviolet light emitting device 1, the thickness of the Al-containing region is preferably 0.5 nm or more and 5 nm or less. This reduces the contact resistance between the second conductive type nitride semiconductor layer 14 and the second contact electrode 16B in the ultraviolet light emitting element 1, improving the emission intensity of the ultraviolet light emitting element 1 and further improving the power conversion efficiency (WPE).
[0076] (7) In the ultraviolet light emitting device 1, the dopant atom concentration in the central region in the thickness direction of the second conductive type nitride semiconductor layer is 1×10 17 cm -3 More than 4×10 19 cm -3 and the dopant atom concentration in the edge region is 8×10 19 cm -3 More than 1×10 21 cm -3 It is preferable that: As a result, the power conversion efficiency (WPE) of the ultraviolet light emitting element 1 is significantly improved, and the threshold voltage of the ultraviolet light emitting element 1 is lowered, thereby improving the emission intensity.
[0077] (8) In the ultraviolet light-emitting device 1, the thickness of the end region is preferably 5% to 50% of the thickness of the second conductivity type nitride semiconductor layer. As a result, the power conversion efficiency of the ultraviolet light emitting element 1 is significantly improved, and the threshold voltage of the ultraviolet light emitting element 1 can be reduced.
[0078] (9) In the ultraviolet light-emitting device 1, the thickness of the second conductivity type nitride semiconductor layer 14 is preferably not less than 3 nm and not more than 200 nm. As a result, the contact resistance and light absorption of the ultraviolet light emitting element 1 are reduced, and the power conversion efficiency and light emission intensity of the ultraviolet light emitting element 1 are significantly improved.
[0079] (10) In the ultraviolet light-emitting device 1, the coverage of the second conductivity type nitride semiconductor layer 14 with respect to the layer immediately below is preferably 80% or more and 100% or less. In this case, the contact area between the layer immediately below and the second conductive type nitride semiconductor layer 14 is increased, and the area where the electrode (second contact electrode 16B) is in direct contact with the layer immediately below is reduced, thereby suppressing leakage current and discontinuous changes, and improving IV characteristics.
[0080] (11) The ultraviolet light emitting device 1 has a second conductive type nitride semiconductor layer made of Al x Ga (1-x) It is preferable that the insulating layer is formed of N (0≦x≦0.2). This improves the carrier injection efficiency of the p-type semiconductor, leading to a further increase in emission intensity, improved IV characteristics, and a lower threshold voltage.
[0081] (12) The ultraviolet light emitting element 1 includes a substrate 11 which is a laminated substrate in which an AlN layer is disposed on an AlN single crystal substrate or a sapphire substrate. This reduces the difference in lattice constant with the nitride semiconductor layer formed on the upper side of the substrate 11, making it possible to grow a nitride semiconductor layer with fewer defects on the substrate 11, thereby improving the emission intensity and other device characteristics.
[0082] (13) The ultraviolet light emitting element 1 includes a first conductivity type nitride semiconductor layer 12 having a thickness of 300 nm or more and 750 nm or less. This causes the first conductivity type nitride semiconductor layer 12 to be lattice relaxed relative to the underlayer, reducing the film resistance, improving the emission intensity, and also improving other device characteristics.
[0083] (14) The lattice constant of the second conductivity type nitride semiconductor layer in the in-plane a-axis direction is matched with that of the layer immediately below, and dopant atoms are substituted into the lattice. This makes it possible to obtain the second conductivity type nitride semiconductor layer 14 having high carrier injection efficiency and excellent IV characteristics.
[0084] (15) The ultraviolet light emitting element 1 is Al z Ga (1-z) The semiconductor device includes a first conductivity type nitride semiconductor layer 12 made of N (0.6≦z≦0.9). This improves the transmittance of the first conductivity type nitride semiconductor layer 12 for the light emitted from the light emitting layer 13, improving the emission intensity and also improving other device characteristics.
[0085] 2. Second embodiment An ultraviolet light emitting device 2 according to the second embodiment will be described with reference to Fig. 3. As shown in Fig. 3, the ultraviolet light emitting device 2 includes a substrate 11, a first conductive type nitride semiconductor layer 12, a light emitting layer 13, a second conductive type nitride semiconductor layer 14, and an Al-containing region 15. The ultraviolet light emitting device 2 also includes a first contact electrode 16A connected to the first conductive type nitride semiconductor layer 12, a second contact electrode 16B connected to the Al-containing region 15, and a reflective electrode 26C provided on the Al-containing region 15. That is, the ultraviolet light emitting device 2 differs from the ultraviolet light emitting device 1 according to the first embodiment in that the ultraviolet light emitting device 2 includes a reflective electrode 26C on the Al-containing region 15.
[0086] The reflective electrode 26C will be described in detail below. Note that the substrate 11, the first conductive type nitride semiconductor layer 12, the light emitting layer 13, the second conductive type nitride semiconductor layer 14, the first contact electrode 16A, and the second contact electrode 16B have the same configuration as those of the ultraviolet light emitting device 1, and therefore descriptions thereof will be omitted.
[0087] (2.1) Structure of ultraviolet light emitting element (Reflecting electrode) The reflective electrode 26C has a function of reflecting light emitted from the light emitting layer 13 toward the second conductive type nitride semiconductor layer 14 toward the light emitting layer 13, thereby improving the emission intensity of the ultraviolet light emitting element 2. From the viewpoint of improving the emission intensity, the reflective electrode 26C preferably has an ultraviolet light reflectance of 90% or more. More specifically, the ultraviolet light reflectance of the reflective electrode 26C at a peak wavelength of 265 nm measured by a reflection / transmission measuring device is preferably 90% or more.
[0088] The reflective electrode 26C is formed of, for example, Al, Ti, Pt, Rd, Ru, Ni, or Rh, but is not limited thereto as long as the reflectance is satisfied. The reflective electrode 26C may be used as the second contact electrode 16B, which is a p-type electrode, or may be provided on the second contact electrode 16B. Furthermore, the reflective electrode 26C may be provided at a location on the Al-containing region 15 other than the second contact electrode 16B. The reflecting electrode 26C may be a semiconductor multilayer distributed Bragg reflector in which oxides such as HfO2 and SiO2 are laminated. The reflective electrode 26C may be a single layer, or may be a laminate of multiple layers.
[0089] (2.2) Manufacturing method of ultraviolet light emitting element The reflective electrode 26C is preferably formed by resistance heating evaporation, electron gun evaporation, sputtering, or the like, but is not limited to these methods.
[0090] (2.3) Effects of the Second Embodiment The ultraviolet light emitting device 2 according to the second embodiment has the following effects in addition to the effects described in the first embodiment. (16) The ultraviolet light emitting element 2 includes a reflective electrode 26C provided on the Al-containing region 15. This allows the ultraviolet light emitting element 2 to reflect light emitted from the light emitting layer 13 toward the second conductivity type nitride semiconductor layer 14 toward the light emitting layer 13, thereby improving the emission intensity of the ultraviolet light emitting element 2.
[0091] 3. Third embodiment With reference to Fig. 4, an ultraviolet light emitting device 3 according to the third embodiment will be described. As shown in Fig. 4, the ultraviolet light emitting device 3 includes a substrate 11, a first conductive type nitride semiconductor layer 12, a light emitting layer 13, a compositionally graded layer 38, and a second conductive type nitride semiconductor layer 14. The ultraviolet light emitting device 3 also includes a first contact electrode 16A connected to the first conductive type nitride semiconductor layer 12, and a second contact electrode 16B connected to the Al-containing region 15. That is, the ultraviolet light emitting device 3 differs from the ultraviolet light emitting device 1 according to the first embodiment in that a compositionally graded layer 38 in which the Al composition decreases in a direction away from the substrate 11 is provided between the light emitting layer 13 and the second conductive type nitride semiconductor layer 14.
[0092] The following describes in detail the composition gradient layer 38. Note that the substrate 11, the first conductivity type nitride semiconductor layer 12, the light emitting layer 13, the second conductivity type nitride semiconductor layer 14, the first contact electrode 16A, and the second contact electrode 16B have the same configuration as those of the ultraviolet light emitting device 1, and therefore descriptions thereof will be omitted.
[0093] (3.1) Structure of ultraviolet light emitting element (composition gradient layer) The composition gradient layer 38 is provided between the light emitting layer 13 and the second conductivity type nitride semiconductor layer 14. The composition gradient layer 38 is composed of Al y Ga (1-y) N (0.1≦y≦1.0), with the Al composition y decreasing in the direction away from the substrate 11. The Al composition y of the composition gradient layer 38 decreases in the direction away from the substrate 11. The profile (gradient) of the Al composition y in the composition gradient layer 38 may decrease continuously or may decrease intermittently. Here, "intermittently decreasing" means that the composition gradient layer 38 includes a portion in which the Al composition y is constant. In other words, the composition gradient layer 38 may include a portion in which the Al composition y does not decrease in the direction away from the substrate 11, but does not include a portion in which it increases.
[0094] The composition gradient layer 38 has the effect of generating holes by a polarization doping effect and efficiently injecting the holes into the active layer in the light emitting layer 13. Therefore, by providing the composition gradient layer 38 between the light emitting layer 13 and the second conductivity type nitride semiconductor layer 14, the luminous efficiency of the ultraviolet light emitting element 3 can be improved. From the viewpoint of increasing the light emission efficiency, the thickness of the compositionally graded layer 38 is preferably 15 nm or more and 60 nm or less, and more preferably 20 nm or more and 50 nm or less.
[0095] The compositionally graded layer 38 may be in contact with the light emitting layer 13, or another layer may be present between the compositionally graded layer 38 and the light emitting layer 13. The compositionally graded layer 38 may be in contact with the second conductive type nitride semiconductor layer 14, or another layer may be present between the compositionally graded layer 38 and the second conductive type nitride semiconductor layer 14. Specifically, the electron blocking layer 17 may be present between the light emitting layer 13 and the compositionally graded layer .
[0096] Here, in the ultraviolet light emitting device 3 according to this embodiment, the coverage of the second conductivity type nitride semiconductor layer 14 indicates the coverage of the composition gradient layer 38 .
[0097] (3.2) Manufacturing method of ultraviolet light emitting element The compositionally graded layer 38, like the other layers, can be formed by any one of molecular beam epitaxy (MBE), hydride vapor phase epitaxy (HVPE), metalorganic chemical vapor deposition (MOCVD), etc. The waveguide layer 49, like the other layers, can be formed using an Al source containing, for example, trimethylaluminum (TMAl), a Ga source containing, for example, trimethylgallium (TMGa) or triethylgallium (TEGa), or an N source containing, for example, ammonia (NH3).
[0098] (3.3) Measurement methods for the physical properties of ultraviolet light-emitting devices (Method of measuring the Al composition of the compositionally graded layer) The Al composition of the compositionally graded layer 38, like the light emitting layer 13 and the electron blocking layer 17, can be measured by X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray spectroscopy (EDX), electron energy loss spectroscopy (EELS), or the like.
[0099] (3.4) Modifications of ultraviolet light emitting devices The ultraviolet light emitting element 3 according to this embodiment may have a configuration including the reflective electrode 26C (not shown) described in the second embodiment.
[0100] (3.5) Effects of the Third Embodiment The ultraviolet light emitting device according to the third embodiment has the following effects in addition to the effects described in the first or second embodiment. (17) The ultraviolet light emitting device 3 includes a compositionally graded layer 38 provided between the light emitting layer 13 and the second conductivity type nitride semiconductor layer 14. This allows the ultraviolet light emitting element 3 to efficiently inject holes into the active layer in the light emitting layer 13, thereby improving the light emitting efficiency of the ultraviolet light emitting element 3.
[0101] 4. Fourth embodiment With reference to Fig. 5, an ultraviolet light emitting device 4 according to the fourth embodiment will be described. As shown in Fig. 5, the ultraviolet light emitting device 4 includes a substrate 11, a first conductive type nitride semiconductor layer 12, a first waveguide layer 49A, a light emitting layer 13, a second waveguide layer 49B, and a second conductive type nitride semiconductor layer 14. The ultraviolet light emitting device 4 also includes a first contact electrode 16A connected to the first conductive type nitride semiconductor layer 12, and a second contact electrode 16B connected to the Al-containing region 15. That is, the ultraviolet light emitting device 4 differs from the ultraviolet light emitting device 1 according to the first embodiment in that it includes waveguide layers 49 (the first waveguide layer 49A and the second waveguide layer 49B) above and below the light emitting layer 13.
[0102] The following describes in detail the waveguide layer 49. Note that the substrate 11, the first conductive type nitride semiconductor layer 12, the light emitting layer 13, the second conductive type nitride semiconductor layer 14, the first contact electrode 16A, and the second contact electrode 16B have the same configuration as those of the ultraviolet light emitting device 1, and therefore descriptions thereof will be omitted.
[0103] (4.1) Structure of UV light emitting element (Waveguide layer) The waveguide layer 49 has a function of confining light from the light emitting layer 13. In order to confine light more efficiently, the waveguide layer 49 is preferably disposed above and below the light emitting layer 13 as a first waveguide layer 49A and a second waveguide layer 49B, as shown in FIG. The waveguide layer 49 is, for example, Al p Ga (1-p) It is preferable that the waveguide layer 49 is formed of N (0.5≦p≦z). From the viewpoint of optical confinement, the Al composition p of the waveguide layer 49 is preferably lower than the Al composition z of the first conductivity type nitride semiconductor layer 12. The waveguide layer 49 may contain impurities such as P, As, Sb, and other group V elements other than N, as well as C, H, F, O, Mg, Si, and Be.
[0104] (4.2) Manufacturing method of ultraviolet light emitting element The waveguide layer 49, like the other layers, can be formed by any one of molecular beam epitaxy (MBE), hydride vapor phase epitaxy (HVPE), metalorganic chemical vapor deposition (MOCVD), etc. Also, the waveguide layer 49, like the other layers, can be formed using an Al source containing, for example, trimethylaluminum (TMAl), a Ga source containing, for example, trimethylgallium (TMGa) or triethylgallium (TEGa), or an N source containing, for example, ammonia (NH3).
[0105] (4.3) Measurement methods for the physical properties of ultraviolet light-emitting devices (Method of measuring the Al composition of the waveguide layer) The Al composition of the waveguide layer 49, like the light emitting layer 13 and the electron blocking layer 17, can be measured by X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray spectroscopy (EDX), electron energy loss spectroscopy (EELS), or the like.
[0106] (4.4) Modifications of ultraviolet light emitting devices The ultraviolet light emitting device 4 according to this embodiment may include at least one of the reflective electrode 26C described in the second embodiment and the compositionally graded layer 38 described in the third embodiment, in addition to the waveguide layers 49 provided above and below the light emitting layer 13. In this case, the compositionally graded layer 38 may be provided between the second waveguide layer 49B provided above the light emitting layer 13 and the second conductivity type nitride semiconductor layer 14.
[0107] Furthermore, the ultraviolet light emitting device 4 according to this embodiment may include a compositionally graded layer 38 similar to the ultraviolet light emitting device 2 according to the fourth embodiment, in addition to the waveguide layers 49 (first waveguide layer 49A and second waveguide layer 49B) provided above and below the light emitting layer 13. In this case, the compositionally graded layer 38 may be provided between the second waveguide layer 49B provided above the light emitting layer 13 and the second conductivity type nitride semiconductor layer 14.
[0108] (4.5) Effects of the Fourth Embodiment The ultraviolet light emitting device according to the fourth embodiment has the following effect in addition to any of the effects described in the first to third embodiments. (18) The ultraviolet light emitting element 4 includes waveguide layers 49 (a first waveguide layer 49A and a second waveguide layer 49B) provided above and below the light emitting layer 13, respectively. This allows the ultraviolet light emitting element 4 to efficiently guide light from the light emitting layer 13 to the outside, thereby improving the luminous efficiency of the ultraviolet light emitting element 4. EXAMPLES
[0109] [Example 1] A c-plane AlN single crystal substrate with a thickness of 550 μm was annealed using a metal-organic chemical vapor deposition (MOCVD) apparatus. The annealing process was carried out in two sets, one for 5 minutes in an NH3 atmosphere and the other for 5 minutes in an H2 atmosphere at 1300°C. Next, an AlN layer, which is a homoepitaxial layer, was formed at 1200°C to a thickness of 500 nm. At this time, the ratio (V / III ratio) of the supply rate of the group III element source gas to the supply rate of the nitrogen source gas was set to 50. The degree of vacuum was set to 50 mbar. The growth rate of the AlN layer was 0.5 μm / hr. Trimethylaluminum (TMAl) was used as the Al source, and ammonia (NH3) was used as the N source.
[0110] On the AlN layer formed as described above, a first conductive type nitride semiconductor layer, which is an n-type AlGaN layer, was formed. The first conductive type nitride semiconductor layer was an n-type AlGaN layer (Al: 70%, i.e., Al 0.70 Ga 0.30 N layer). The first conductive type nitride semiconductor layer was formed to a thickness of 500 nm under the conditions of a temperature of 1080°C, a degree of vacuum of 50 mbar, and a V / III ratio of 4000. The growth rate of the first conductive type nitride semiconductor layer was 0.5 μm / hr. Trimethylaluminum (TMAl) was used as the Al raw material. Triethylgallium (TEGa) was used as the Ga raw material. Ammonia (NH3) was used as the N raw material. Monosilane (SiH4) was used as the Si raw material.
[0111] Next, a light emitting layer was formed on the first conductive type nitride semiconductor layer. The light emitting layer was formed to have a multiple quantum well structure in which quantum well layers and barrier layers were stacked five times. Here, the quantum well layer was an AlGaN layer (Al: 52%, i.e., Al 0.52 Ga 0.48 The barrier layer having a thickness of 6.0 nm was an AlGaN layer (Al: 75%, i.e., Al 0.75 Ga0.25 N layer). The light-emitting layer was formed under conditions of a vacuum degree of 50 mbar and a V / III ratio of 4000. The growth rate of the quantum well layer was 0.18 μm / hr, and the growth rate of the barrier layer was 0.15 μm / hr.
[0112] Next, an electron blocking layer was formed on the light emitting layer. Here, the electron blocking layer was an AlGaN layer (Al: 85%, i.e., Al 0.85 Ga 0.15 N layer). The electron blocking layer was formed under conditions where the degree of vacuum was set to 50 mbar and the V / III ratio was set to 4000. The growth rate of the electron blocking layer at this time was 0.12 μm / hr.
[0113] Next, a compositionally graded layer was formed on the electron blocking layer. The compositionally graded layer was an AlGaN layer having a thickness of 35 nm and a uniform Al composition gradient from 75% to 30% (Al: 70→30%, i.e., Al 0.75 Ga 0.25 N → Al 0.3 Ga 0.7 N layer). The composition gradient layer was formed under conditions of a degree of vacuum of 50 mbar and a V / III ratio of 4,000.
[0114] Next, a second conductivity type nitride semiconductor layer was formed on the compositionally graded layer. Here, the second conductivity type nitride semiconductor layer was a p-type GaN layer (i.e., Al: 0%) having a thickness of 10 nm and using Mg as a dopant impurity. The second conductive type nitride semiconductor layer was formed under the conditions of a temperature of 920° C., a degree of vacuum of 150 mbar, and a V / III ratio of 3650. The growth rate of the second conductive type nitride semiconductor layer at this time was 0.2 μm / hr. The second conductive type nitride semiconductor layer was formed so that a Mg concentration distribution was generated. Specifically, the Mg concentration was 1×10 20 cm -3 The first layer was deposited to a thickness of 2 nm, and then a layer with a Mg concentration of 1×1019 cm -3 The second layer was deposited to a thickness of 6 nm, and the final Mg concentration was 1×10 20 cm -3 The third layer was formed to a thickness of 2 nm. That is, the edge concentration of the second conductive type nitride semiconductor layer was 1×10 20 cm -3 , central concentration is 1×10 19 cm -3 It was decided. In this way, a second conductivity type nitride semiconductor layer having a total thickness of 10 nm and a Mg concentration distribution was formed. The Mg concentration was adjusted by adjusting the Mg flow rate, and the film thickness was adjusted by adjusting the film formation time.
[0115] Subsequently, an Al-containing region was formed on the second conductive type nitride semiconductor layer. The Al-containing region was an AlGaN layer (Al: 70%, i.e., Al 0.7 Ga 0.3 N). The region containing Al was formed under conditions of a vacuum degree of 50 mbar and a V / III ratio of 4000. The growth rate of the quantum well layer at this time was 0.14 μm / hr. In this manner, a nitride semiconductor laminate was formed on the AlN substrate.
[0116] When the nitride semiconductor laminate formed as described above was observed using a SEM, the surface coverage of the second conductivity type nitride semiconductor layer with respect to the composition gradient layer immediately below was 85%. Finally, when a cross-sectional TEM measurement was performed using a high-resolution TEM, it was found that the composition gradient layer and the second conductivity type nitride semiconductor layer were lattice-matched, and the film thickness of the region containing Al was the desired film thickness. Furthermore, when a part of the obtained second conductivity type nitride semiconductor layer was measured by APT, it was found that the Al composition of the region containing Al was the desired composition, and the Mg concentration and film thickness of the second conductivity type nitride semiconductor layer were the desired Mg concentration and film thickness.
[0117] The obtained nitride semiconductor laminate was dry etched from the second conductivity type nitride semiconductor layer side to expose a part of the first conductivity type nitride semiconductor layer, which is an n-type AlGaN layer. An alloy electrode (corresponding to an n-type contact electrode) containing Ti, Al, Ni and Au was formed on the exposed first conductivity type nitride semiconductor layer. Also, an alloy electrode (corresponding to a p-type contact electrode) containing Ni and Au was formed on the second conductivity type nitride semiconductor layer, which is a p-type GaN layer. The AlN substrate was ground from the back side to a thickness of 100 μm, and then the nitride semiconductor laminate was divided into individual pieces of ultraviolet light emitting elements by dicing. The obtained ultraviolet light emitting device was evaluated by driving it at a current of 500 mA, and the driving voltage was 6.5 V, and the emission intensity at a peak wavelength of 265 nm was 54 mW. The WPE at this time was 1.66%.
[0118] [Example 2] The Mg concentration (edge concentration) of the first layer in the second conductive type nitride semiconductor layer is 3×10 20 cm -3 The ultraviolet light emitting device was fabricated in the same manner as in Example 1, except that the second conductive type nitride semiconductor layer was formed so that the surface coverage of the second conductive type nitride semiconductor layer was 90%. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.3 V, and the emission intensity at a peak wavelength of 265 nm was 55 mW. The WPE at this time was 1.75%.
[0119] [Example 3] The Mg concentration of the first layer in the second conductive type nitride semiconductor layer is 7×10 20 cm -3 The ultraviolet light emitting device was fabricated in the same manner as in Example 1, except that the second conductive type nitride semiconductor layer was formed so that the surface coverage of the second conductive type nitride semiconductor layer was 100%. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 5.9 V, and the emission intensity at a peak wavelength of 265 nm was 62 mW. The WPE at this time was 2.10%.
[0120] [Example 4] The Mg concentration of the first layer in the second conductive type nitride semiconductor layer is 9×10 20 cm -3 The ultraviolet light emitting device was fabricated in the same manner as in Example 1, except that the second conductive type nitride semiconductor layer was formed so that the surface coverage of the second conductive type nitride semiconductor layer was 100%. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.0 V, and the emission intensity at a peak wavelength of 265 nm was 59 mW. The WPE at this time was 1.97%.
[0121] [Example 5] The Mg concentration of the first layer in the second conductive type nitride semiconductor layer is 6×10 19 cm -3 The ultraviolet light emitting device was fabricated in the same manner as in Example 1, except that the second conductive type nitride semiconductor layer was formed so that the surface coverage of the second conductive type nitride semiconductor layer was 75%. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.8 V, and the emission intensity at a peak wavelength of 265 nm was 49 mW. The WPE at this time was 1.44%.
[0122] [Example 6] The Mg concentration of the first layer in the second conductive type nitride semiconductor layer is 3×10 21 cm -3 The ultraviolet light emitting device was fabricated in the same manner as in Example 1, except that the second conductive type nitride semiconductor layer was formed so that the surface coverage of the second conductive type nitride semiconductor layer was 100%. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.9 V, and the emission intensity at a peak wavelength of 265 nm was 51 mW. The WPE at this time was 1.48%.
[0123] [Example 7] The Mg concentration (center concentration) of the second layer in the second conductive type nitride semiconductor layer is 3×10 19 cm -3An ultraviolet light emitting device was manufactured in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the ultraviolet light emitting device was formed as follows. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 5.8 V, and the emission intensity at a peak wavelength of 265 nm was 60 mW. The WPE at this time was 2.07%.
[0124] [Example 8] The Mg concentration of the second layer in the second conductive type nitride semiconductor layer is 7×10 18 cm -3 An ultraviolet light emitting device was manufactured in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the ultraviolet light emitting device was formed as follows. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.2 V, and the emission intensity at a peak wavelength of 265 nm was 55 mW. The WPE at this time was 1.77%.
[0125] [Example 9] The Mg concentration of the second layer in the second conductive type nitride semiconductor layer is 3×10 18 cm -3 An ultraviolet light emitting device was manufactured in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the ultraviolet light emitting device was formed as follows. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.5 V, and the emission intensity at a peak wavelength of 265 nm was 53 mW. The WPE at this time was 1.63%.
[0126] [Example 10] The Mg concentration of the second layer in the second conductive type nitride semiconductor layer is 6×10 19 cm -3 An ultraviolet light emitting device was manufactured in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the ultraviolet light emitting device was formed as follows. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 7.1 V, and the emission intensity at a peak wavelength of 265 nm was 54 mW. The WPE at this time was 1.52%.
[0127] [Example 11] The Mg concentration of the second layer in the second conductive type nitride semiconductor layer is 7×10 17cm -3 An ultraviolet light emitting device was manufactured in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the ultraviolet light emitting device was formed as follows. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.8 V, and the emission intensity at a peak wavelength of 265 nm was 50 mW. The WPE at this time was 1.47%.
[0128] [Example 12] An ultraviolet light emitting device was formed in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the first and third layers in the second conductive type nitride semiconductor layer had thicknesses of 1.0 nm each. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 5.9 V and the emission intensity at a peak wavelength of 265 nm was 60 mW. The WPE at this time was 2.03%.
[0129] [Example 13] An ultraviolet light emitting device was formed in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the first and third layers in the second conductive type nitride semiconductor layer had thicknesses of 3.5 nm each. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.8 V and the emission intensity at a peak wavelength of 265 nm was 51 mW. The WPE at this time was 1.50%.
[0130] [Example 14] An ultraviolet light emitting device was formed in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the first and third layers in the second conductive type nitride semiconductor layer had thicknesses of 0.5 nm and the second layer had a thickness of 1 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.4 V and the emission intensity at a peak wavelength of 265 nm was 70 mW. The WPE at this time was 2.19%.
[0131] [Example 15] An ultraviolet light emitting device was formed in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the first and third layers in the second conductive type nitride semiconductor layer had thicknesses of 3.0 nm and the second layer had a thickness of 14 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 5.7 V and the emission intensity at a peak wavelength of 265 nm was 53 mW. The WPE at this time was 1.86%.
[0132] [Example 16] An ultraviolet light emitting device was formed in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the first and third layers in the second conductive type nitride semiconductor layer had thicknesses of 5.0 nm and the second layer had a thickness of 140 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 5.6 V and the emission intensity at a peak wavelength of 265 nm was 50 mW. The WPE at this time was 1.79%.
[0133] [Example 17] An ultraviolet light emitting device was formed in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the first and third layers in the second conductive type nitride semiconductor layer had thicknesses of 7.5 nm and the second layer had a thickness of 235 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.1 V and the emission intensity at a peak wavelength of 265 nm was 42 mW. The WPE at this time was 1.38%.
[0134] [Example 18] The second conductive type nitride semiconductor layer is an AlGaN layer (Al: 10%, i.e., Al 0.1 Ga 0.9 An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the second conductive type nitride semiconductor layer had a wavelength of 1.2 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.3 V and the emission intensity at a peak wavelength of 265 nm was 58 mW. The WPE at this time was 1.84%.
[0135] [Example 19] The second conductive type nitride semiconductor layer is an AlGaN layer (Al: 18%, i.e., Al 0.18 Ga 0.82 An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the second conductive type nitride semiconductor layer had a wavelength of 1.2 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.7 V and the emission intensity at a peak wavelength of 265 nm was 50 mW. The WPE at this time was 1.49%.
[0136] [Example 20] The second conductive type nitride semiconductor layer is an AlGaN layer (Al: 25%, i.e., Al 0.25 Ga 0.75 An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the second conductive type nitride semiconductor layer had a wavelength of 1.2 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 7.0 V, and the emission intensity at a peak wavelength of 265 nm was 48 mW. The WPE at this time was 1.37%.
[0137] [Example 21] An ultraviolet light emitting device was produced in the same manner as in Example 3, except that no composition gradient layer was formed. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 7.2 V, and the emission intensity at a peak wavelength of 265 nm was 49 mW. The WPE at this time was 1.36%.
[0138] [Example 22] An ultraviolet light emitting device was produced in the same manner as in Example 3, except that the composition gradient layer was formed so that the film thickness of the composition gradient layer was 10 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.8 V, and the emission intensity at a peak wavelength of 265 nm was 47 mW. The WPE at this time was 1.38%.
[0139] [Example 23] An ultraviolet light emitting device was produced in the same manner as in Example 3, except that the composition gradient layer was formed so that the film thickness of the composition gradient layer was 20 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.1 V, and the emission intensity at a peak wavelength of 265 nm was 55 mW. The WPE at this time was 1.80%.
[0140] [Example 24] An ultraviolet light emitting device was produced in the same manner as in Example 3, except that the composition gradient layer was formed so that the film thickness of the composition gradient layer was 50 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 5.8 V, and the emission intensity at a peak wavelength of 265 nm was 53 mW. The WPE at this time was 1.83%.
[0141] [Example 25] An ultraviolet light emitting device was produced in the same manner as in Example 3, except that the composition gradient layer was formed so that the film thickness of the composition gradient layer was 70 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.0 V, and the emission intensity at a peak wavelength of 265 nm was 49 mW. The WPE at this time was 1.63%.
[0142] [Example 26] An ultraviolet light emitting device was produced in the same manner as in Example 3, except that the first conductive type nitride semiconductor layer was formed so that the film thickness of the first conductive type nitride semiconductor layer was 200 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 7.1 V, and the emission intensity at a peak wavelength of 265 nm was 60 mW. The WPE at this time was 1.69%.
[0143] [Example 27] An ultraviolet light emitting device was produced in the same manner as in Example 3, except that the first conductive type nitride semiconductor layer was formed so that the film thickness of the first conductive type nitride semiconductor layer was 300 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.6 V, and the emission intensity at a peak wavelength of 265 nm was 60 mW. The WPE at this time was 1.82%.
[0144] [Example 28] An ultraviolet light emitting device was produced in the same manner as in Example 3, except that the first conductive type nitride semiconductor layer was formed so that the film thickness of the first conductive type nitride semiconductor layer was 800 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 5.6 V, and the emission intensity at a peak wavelength of 265 nm was 48 mW. The WPE at this time was 1.71%.
[0145] [Example 29] An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the Al-containing region was formed so that the film thickness of the Al-containing region was 3 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 5.9 V, and the emission intensity at a peak wavelength of 265 nm was 65 mW. The WPE at this time was 2.20%.
[0146] [Example 30] An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the Al-containing region was formed so that the film thickness of the Al-containing region was 5 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.2 V, and the emission intensity at a peak wavelength of 265 nm was 60 mW. The WPE at this time was 1.94%.
[0147] [Example 31] An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the Al-containing region was formed so that the film thickness of the Al-containing region was 7 nm. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.8 V, and the emission intensity at a peak wavelength of 265 nm was 52 mW. The WPE at this time was 1.53%.
[0148] [Example 32] An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the region containing Al was formed to a thickness of 0.5 nm by using Al metal deposited by EB deposition. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 6.0 V, and the emission intensity at a peak wavelength of 265 nm was 66 mW. The WPE at this time was 2.20%.
[0149] [Example 33] An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the region containing Al was formed to a thickness of 3 nm by depositing Al metal by EB deposition. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 5.9 V, and the emission intensity at a peak wavelength of 265 nm was 70 mW. The WPE at this time was 2.37%.
[0150] [Example 34] An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the region containing Al was formed to a thickness of 5 nm by depositing Al metal by EB deposition. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 5.8 V, and the emission intensity at a peak wavelength of 265 nm was 65 mW. The WPE at this time was 2.24%.
[0151] [Example 35] The ultraviolet light emitting device was formed in the same manner as in Example 3, except that the region containing Al was formed by depositing 0.5 nm of Al by EB deposition, depositing 0.5 nm of Ni, and then annealing with lamp heating at 900°C for 1 minute to alloy the p-electrode containing Ni and Al. When a part of the obtained nitride semiconductor laminate was measured using APT, the total thickness of the region containing Al was 1 nm, and the Mg concentration and thickness of the second conductive type nitride semiconductor layer were the desired Mg concentration and thickness. When the obtained ultraviolet light emitting device was driven with a current of 500 mA, the driving voltage was 5.9 V, and the emission intensity at a peak wavelength of 265 nm was 63 mW. The WPE at this time was 2.14%.
[0152] [Example 36] The ultraviolet emitting device was formed in the same manner as in Example 35, except that the region containing Al was formed by depositing 2.5 nm of Al by EB deposition, depositing 0.5 nm of Ni, and then annealing at 900°C for 1 minute by lamp heating to alloy the p-electrode containing Ni with Al. When a part of the obtained nitride semiconductor laminate was measured using APT, the total thickness of the region containing Al was 3 nm, and the Mg concentration and thickness of the second conductive type nitride semiconductor layer were the desired Mg concentration and thickness. When the obtained ultraviolet emitting device was driven with a current of 500 mA, the driving voltage was 6.0 V, and the emission intensity at a peak wavelength of 265 nm was 66 mW. The WPE at this time was 2.20%.
[0153] [Example 37] The ultraviolet light emitting device was formed in the same manner as in Example 3, except that the region containing Al was formed by depositing 4.5 nm of Al and 0.5 nm of Ni by EB deposition, followed by annealing at 900°C for 1 minute by lamp heating, and alloying the p-electrode containing Ni with Al. When a part of the obtained nitride semiconductor laminate was measured using APT, the total thickness of the region containing Al was 5 nm, and the Mg concentration and thickness of the second conductive type nitride semiconductor layer were the desired Mg concentration and thickness. When the obtained ultraviolet light emitting device was driven with a current of 500 mA, the driving voltage was 6.2 V, and the emission intensity at a peak wavelength of 265 nm was 61 mW. The WPE at this time was 1.97%.
[0154] [Example 38] The region containing Al was treated as a 0.5 nm thick AlGaN layer (Al: 70%, i.e., Al 0.7 Ga 0.3On the p-type nitride semiconductor layer (N layer), 0.5 nm of Al was deposited by EB deposition, and 0.5 nm of Ni was deposited, and then annealing was performed for 1 minute at 900°C by lamp heating, and the p-electrode containing Ni and Al were alloyed to form the p-electrode. Except for this, an ultraviolet light emitting device was formed in the same manner as in Example 3. When a part of the obtained nitride semiconductor laminate was measured using APT, the total film thickness of the region containing Al was 1.5 nm, and the Mg concentration and film thickness of the second conductive type nitride semiconductor layer were the desired Mg concentration and film thickness. When the obtained ultraviolet light emitting device was driven with a current of 500 mA, the driving voltage was 5.9 V, and the emission intensity at a peak wavelength of 265 nm was 70 mW. The WPE at this time was 2.37%.
[0155] [Example 39] The region containing Al was treated as a 1.5 nm-thick AlGaN layer (Al: 70%, i.e., Al 0.7 Ga 0.3 On the p-type nitride semiconductor layer (N layer), 1.0 nm of Al was deposited by EB deposition, and 0.5 nm of Ni was deposited, and then annealed at 900°C for 1 minute by lamp heating to alloy the p-electrode containing Ni with Al. Except for this, an ultraviolet light emitting device was formed in the same manner as in Example 3. When a part of the obtained nitride semiconductor laminate was measured using APT, the total film thickness of the region containing Al was 3 nm, and the Mg concentration and film thickness of the second conductive type nitride semiconductor layer were the desired Mg concentration and film thickness. When the obtained ultraviolet light emitting device was driven with a current of 500 mA, the driving voltage was 5.8 V, and the emission intensity at a peak wavelength of 265 nm was 73 mW. The WPE at this time was 2.52%.
[0156] [Example 40] The region containing Al was treated as a 0.5 nm thick AlGaN layer (Al: 70%, i.e., Al 0.7 Ga 0.3An ultraviolet light emitting device was formed in the same manner as in Example 3, except that an Al-containing region was formed on the nitride semiconductor layer (N layer) so as to have 0.5 nm of Al deposited by EB deposition. When a part of the obtained nitride semiconductor laminate was measured using APT, the total thickness of the Al-containing region was 1 nm, and the Mg concentration and thickness of the second conductivity type nitride semiconductor layer were the desired Mg concentration and thickness. When the obtained ultraviolet light emitting device was driven with a current of 500 mA, the driving voltage was 5.9 V, and the emission intensity at a peak wavelength of 265 nm was 76 mW. The WPE at this time was 2.58%.
[0157] [Example 41] The region containing Al was treated as a 1.0 nm-thick AlGaN layer (Al: 70%, i.e., Al 0.7 Ga 0.3 An ultraviolet light emitting device was formed in the same manner as in Example 3, except that an Al-containing region was formed on the nitride semiconductor layer (N layer) so as to have 2.0 nm of Al deposited by EB deposition. When a part of the obtained nitride semiconductor laminate was measured using APT, the total thickness of the Al-containing region was 3 nm, and the Mg concentration and thickness of the second conductivity type nitride semiconductor layer were the desired Mg concentration and thickness. When the obtained ultraviolet light emitting device was driven with a current of 500 mA, the driving voltage was 5.8 V, and the emission intensity at a peak wavelength of 265 nm was 83 mW. The WPE at this time was 2.86%.
[0158] [Example 42] A laminated substrate in which an AlN layer was formed on a (0001) sapphire substrate tilted 0.2° toward the m-plane was used as the substrate, and an ultraviolet light emitting device was formed in the same manner as in Example 3, except that the second conductive type nitride semiconductor layer was formed so that the surface coverage of the second conductive type nitride semiconductor layer was 65%. When the obtained ultraviolet light emitting device was driven with a current of 500 mA, the driving voltage was 6.5 V and the emission intensity at a peak wavelength of 265 nm was 32 mW. The WPE at this time was 0.98%.
[0159] [Example 43] An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the contact electrode was formed from a metal containing only Au. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 8.0 V, and the emission intensity at a peak wavelength of 265 nm was 44 mW. The WPE at this time was 1.10%. [Example 44] An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the contact electrodes were formed from an alloy containing Au and V. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 7.6 V, and the emission intensity at a peak wavelength of 265 nm was 42 mW. The WPE at this time was 1.11%.
[0160] [Comparative Example 1] An ultraviolet light emitting device was formed in the same manner as in Example 3, except that no region containing Al was provided. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 7.2 V, and the emission intensity at a peak wavelength of 265 nm was 48 mW. The WPE at this time was 1.33%.
[0161] [Comparative Example 2] A sapphire substrate with a (0001) plane tilted 0.2° toward the m-plane was used as the substrate, a second conductive type nitride semiconductor layer was formed so that the surface coverage of the second conductive type nitride semiconductor layer was 65%, and an ultraviolet light emitting device was formed in the same manner as in Example 3, except that no region containing Al was provided. When the obtained ultraviolet light emitting device was driven with a current of 500 mA, the driving voltage was 7.2 V and the emission intensity at a peak wavelength of 265 nm was 25 mW. The WPE at this time was 0.69%.
[0162] [Comparative Example 3] An ultraviolet light emitting device was fabricated in the same manner as in Example 3, except that the contact electrode was formed to contain only Ni. When the obtained ultraviolet light emitting device was driven at a current of 500 mA, the driving voltage was 8.5 V, and the emission intensity at a peak wavelength of 265 nm was 38 mW. The WPE at this time was 0.89%.
[0163] Table 1 below shows the configuration and evaluation of each of the examples and comparative examples.
[0164] [Table 1]
[0165] As shown in Table 1, it was found that the ultraviolet light emitting devices of the examples, which include a contact electrode containing at least Au and an Al-containing region provided between the second conductivity type nitride semiconductor layer and the contact electrode, have a higher power conversion efficiency (WPE) than Comparative Examples 1 and 2, which do not include an Al-containing region, and Comparative Example 3, in which the contact electrode does not contain Au. It was also found that the ultraviolet light emitting devices of the examples further provide at least one of the effects of improving the emission intensity or lowering the threshold voltage, compared to the ultraviolet light emitting devices of the comparative examples.
[0166] From Examples 3, 43 and 44, it was found that ultraviolet light-emitting elements in which the contact electrodes are formed of an alloy of Au and other metals such as Ni have a power conversion efficiency (WPE) equal to or greater than that in the case where the contact electrodes are formed containing only Au. From each example, it was found that the power conversion efficiency (WPE) is improved when the Al-containing region has at least one region selected from the group consisting of a nitride semiconductor region containing Al, an elemental Al region formed of elemental Al, and an Al alloy region formed of an Al alloy.
[0167] From Examples 1 to 11, the dopant atom concentration in the central region in the thickness direction of the second conductive type nitride semiconductor layer is 1×10 17 cm -3 More than 4×10 19 cm -3 and the dopant atom concentration in the edge region is 8×10 19 cm -3 More than 1×10 21 cm -3 or less, it has been found that the threshold voltage is reduced as compared to when the dopant atom concentrations in the center and edge regions are outside the ranges stated above.
[0168] From Example 3 and Examples 12 to 17, it was found that the threshold voltage decreases when the thickness of the end region, which is the high dopant concentration region in the second conductivity type nitride semiconductor layer, is 5% or more and 50% or less of the thickness of the second conductivity type nitride semiconductor layer. Moreover, from Examples 3 and 14 to 17, it was found that the thinner the second conductivity type nitride semiconductor layer, the higher the power conversion efficiency (WPE) and the emission intensity, and it was particularly preferable that the thickness of the second conductivity type nitride semiconductor layer be 200 nm or less. Furthermore, when the thickness of the second conductivity type nitride semiconductor layer was 3 nm or more and 200 nm or less, it was possible to achieve both an improvement in the power conversion efficiency (WPE) and the emission intensity and a decrease in the threshold voltage.
[0169] From Examples 1 to 3, it was found that by setting the coverage of the second nitride semiconductor layer with respect to the layer immediately below to 80% or more, the power conversion efficiency (WPE) was significantly improved, the luminous efficiency was improved, and the threshold voltage was also reduced. From Example 3 and Example 21, it was confirmed that when a compositionally graded layer is provided between the light emitting layer and the second conductivity type nitride semiconductor layer, the power conversion efficiency (WPE) and light emission intensity are significantly improved and the threshold voltage is reduced, compared to when no compositionally graded layer is provided. From Example 3, Example 25 to Example 27, and Example 28, when the thickness of the composition gradient layer is 15 nm or more and 60 nm or less, the power conversion efficiency (WPE) is significantly improved compared to when the thickness of the composition gradient layer is not within the above range. In this case, the emission intensity also tends to improve and the threshold voltage also tends to decrease.
[0170] Moreover, from Example 3 and Examples 42 to 44 and Comparative Examples 1 and 2, it was found that if an Al-containing region and a contact electrode containing Au were provided, the power conversion efficiency (WPE) and luminous efficiency improved and the threshold voltage decreased regardless of whether the substrate was an AlN single crystal substrate or a sapphire substrate. It was also found that these effects were high when the substrate was an AlN single crystal substrate, and that when the substrate included a sapphire substrate, these effects could be obtained even more when the substrate was a laminate substrate in which an AlN layer was disposed on a sapphire substrate. From Example 3 and Examples 26 to 28, when the thickness of the first conductivity type nitride semiconductor layer was 300 nm or more and 750 nm or less, the power conversion efficiency (WPE) was significantly improved compared to when the thickness of the first conductivity type nitride semiconductor layer was not within the above range.
[0171] From Examples 3 and 9, it was confirmed that when a composition gradient layer is provided between the light emitting layer and the second conductivity type nitride semiconductor layer, the light emission intensity is improved and the threshold voltage is reduced compared to when no composition gradient layer is provided. Moreover, from Example 3, Example 24 to Example 26, and Example 27, it was confirmed that when the layer thickness of the composition gradient layer was 15 nm or more and 60 nm or less, the emission intensity was improved and the threshold voltage was reduced.
[0172] The scope of the present disclosure is not limited to the exemplary embodiments shown and described, but includes all embodiments that achieve equivalent effects to those contemplated by the present disclosure. Furthermore, the scope of the present disclosure is not limited to the combination of inventive features defined by the claims, but may be defined by any desired combination of specific features among all the respective disclosed features. [Explanation of symbols]
[0173] 1,2,3,4 UV light emitting element 11 Substrate 12 First conductive type nitride semiconductor layer 13 Emitting layer 14 Second conductive type nitride semiconductor layer 15 Al-containing region 16A 1st electrode 16B 2nd electrode 17 Electron Block Layer 26C reflective electrode 38 Compositionally graded layer 49 Waveguide Layer 49A 1st waveguide layer 49B 2nd waveguide layer
Claims
1. A substrate; a first conductivity type nitride semiconductor layer disposed on the substrate and containing Al and Ga; a light emitting layer disposed on the first conductivity type nitride semiconductor layer and including a nitride semiconductor including Al and Ga; a second conductivity type nitride semiconductor layer disposed on the light emitting layer and having a conductivity type different from that of the first conductivity type nitride semiconductor layer; a contact electrode disposed on the second conductivity type nitride semiconductor layer and including an alloy including at least Au and Ni; an Al-containing region including an elemental Al region formed of elemental Al, the elemental Al region being provided between the second conductive type nitride semiconductor layer and the contact electrode and in direct contact with the second conductive type nitride semiconductor layer; Equipped with the Al-containing region is formed of the elemental Al region, or the elemental Al region and at least one region selected from an Al alloy region formed of an Al alloy and a nitride semiconductor region containing Al; The thickness of the Al-containing region is 0.5 nm or more and 5 nm or less. Ultraviolet light emitting element.
2. A substrate; a first conductivity type nitride semiconductor layer disposed on the substrate and containing Al and Ga; a light emitting layer disposed on the first conductivity type nitride semiconductor layer and including a nitride semiconductor including Al and Ga; a second conductivity type nitride semiconductor layer disposed on the light emitting layer and having a conductivity type different from that of the first conductivity type nitride semiconductor layer; a contact electrode disposed on the second conductivity type nitride semiconductor layer and including an alloy including at least Au and Ni; an Al-containing region including an Al alloy region made of an Al alloy, the Al-containing region being provided between the second conductivity type nitride semiconductor layer and the contact electrode and in direct contact with the second conductivity type nitride semiconductor layer; Equipped with the Al-containing region is formed of the Al alloy region, or the Al alloy region and a nitride semiconductor region containing Al; The thickness of the Al-containing region is 0.5 nm or more and 5 nm or less. Ultraviolet light emitting element.
3. The contact electrode includes an alloy including any one of Ti, Pt, Rd, Ru, and Rh. The ultraviolet light emitting element according to claim 1 .
4. the second conductive type nitride semiconductor layer contains dopant atoms, The concentration of the dopant atoms in the central region in the thickness direction of the second conductive type nitride semiconductor layer is 1×10 18 cm -3 Above 4 x 10 19 cm -3 is as follows: The concentration of the dopant atoms in the end region in the thickness direction of the second conductive type nitride semiconductor layer is 8×10 19 cm -3 Above 1 x 10 21 cm -3 is as follows:
4. The ultraviolet light emitting element according to claim 1, wherein a thickness of the end region is 5% to 50% of a thickness of the second conductivity type nitride semiconductor layer.
5. The second conductive type nitride semiconductor layer has a thickness of 3 nm or more and 200 nm or less. The ultraviolet light emitting element according to claim 1 .
6. The coverage of the second conductive type nitride semiconductor layer with respect to the layer immediately below is 80% or more and 100% or less. The ultraviolet light emitting element according to claim 1 .
7. The second conductive type nitride semiconductor layer is made of Al x G (1-x) N (0≦x≦0.2) The ultraviolet light emitting element according to claim 1 .
8. a composition gradient layer provided between the light emitting layer and the second conductivity type nitride semiconductor layer, The composition gradient layer is Al y G (1-y) N (0.1≦y≦1.0), where the Al composition y decreases in the direction away from the substrate. The ultraviolet light emitting element according to claim 1 .
9. The thickness of the composition gradient layer is 15 nm or more and 60 nm or less. The ultraviolet light emitting element according to claim 8 .
10. the substrate is an AlN single crystal substrate or a laminate substrate in which an AlN layer is disposed on a sapphire substrate, The first conductive type nitride semiconductor layer is an AlN layer having a thickness of 300 nm to 750 nm. z G (1-z) N (0.6≦z≦0.9) The ultraviolet light emitting element according to claim 1 .
11. the second conductive type nitride semiconductor layer contains dopant atoms, The lattice constant of the second conductive type nitride semiconductor layer in the in-plane a-axis direction is matched with that of the layer immediately below, and the dopant atoms are substituted into the lattice. The ultraviolet light emitting element according to claim 1 .
12. The first conductive type nitride semiconductor layer is made of Al z G (1-z) N (0.6≦z≦0.9), Above and below the light-emitting layer, p G (1-p) N (0.5≦p≦z), The ultraviolet light emitting element according to claim 1 .
Citation Information
Patent Citations
Drop-out compensating circuit of disk reproducer
JP1984040355A
Nitride semiconductor light emitting element
JP2006080469A
Nitride semiconductor element, and manufacturing method thereof
JP2009152448A
Semiconductor light-emitting element
JP2012119515A
Ultraviolet light-emitting element, and light-emitting structure
JP2014096539A