Method for manufacturing silicon carbide semiconductor device

By forming defects in the excess epitaxial film to reduce its hardness, the method efficiently removes surplus film, addressing the prolonged processing time issue and enhancing manufacturing efficiency in silicon carbide semiconductor devices.

JP7560324B2Active Publication Date: 2024-10-02DENSO CORP +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020185690
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-06
Publication Date
2024-10-02
Estimated Expiration
2040-11-06

AI Technical Summary

Technical Problem

The processing time for removing excess p-type epitaxial film deposited on the surface of an n-type semiconductor layer in silicon carbide semiconductor devices is prolonged due to the high hardness of silicon carbide, which complicates the manufacturing process.

Method used

A method involving defect formation in the excess portion of the epitaxial film, such as through ion implantation or laser irradiation, reduces the hardness of the surplus film, allowing for efficient removal using grinding or polishing techniques.

Benefits of technology

The method significantly shortens the time required to remove the excess epitaxial film, thereby reducing manufacturing time and costs while maintaining the integrity of the semiconductor device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560324000001
    Figure 0007560324000001
  • Figure 0007560324000002
    Figure 0007560324000002
  • Figure 0007560324000003
    Figure 0007560324000003
Patent Text Reader

Abstract

To provide an art of removing the excess part of an epitaxial film in a short time in a manufacturing method of a silicon carbide semiconductor device including a process of filling an epitaxial film in a trench.SOLUTION: The manufacturing method of a silicon carbide semiconductor device 1 includes: a trench forming step of forming a trench TR in a silicon carbide semiconductor layer 140; an epitaxial film forming step of forming epitaxial films 14b, 42, 44 of silicon carbide to fill inside the trench; a defect formation step of forming defects in surplus portions 42, 44 of the epitaxial film deposited on the surface of the semiconductor layer; and a removal step of shaving and removing the surplus portion of the epitaxial film.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technology disclosed in this specification relates to a method for manufacturing a silicon carbide semiconductor device. [Background technology]

[0002] A superjunction structure (hereinafter referred to as an "SJ structure") has been proposed as a structure that achieves both low on-resistance and high breakdown voltage. Patent Document 1 discloses an example of a silicon carbide semiconductor device having such an SJ structure. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-140258 A Summary of the Invention [Problem to be solved by the invention]

[0004] To form such an SJ structure, a plurality of trenches are formed in an n-type semiconductor layer to form a plurality of n-type mesas remaining between the trenches, and a p-type epitaxial film is filled into each of the plurality of trenches to form a plurality of p-type epitaxial films. In this way, the SJ structure is formed by the plurality of n-type mesas and the plurality of p-type epitaxial films.

[0005] When filling the trench with the p-type epitaxial film, the p-type epitaxial film is also deposited on the surface of the n-type semiconductor layer. The p-type epitaxial film deposited on the surface of the n-type semiconductor layer is not a part that constitutes the semiconductor device, but is an excess part. Therefore, the excess part of the p-type epitaxial film is removed in a later process using grinding or polishing technology.

[0006] However, since silicon carbide has a high hardness, there is a problem that the processing time required to remove the excess portion of the epitaxial film becomes long.

[0007] The above-mentioned problems do not occur only when forming an SJ structure. The above-mentioned problems can occur widely when forming a trench in a silicon carbide semiconductor layer and forming a silicon carbide epitaxial film in the trench. This specification provides a technology for removing an excess portion of an epitaxial film in a short time in a manufacturing method for a silicon carbide semiconductor device including a step of filling an epitaxial film in a trench. [Means for solving the problem]

[0008] The manufacturing method of the silicon carbide semiconductor device (1) disclosed in this specification can include a trench forming step of forming a trench (TR) in a silicon carbide semiconductor layer (140), an epitaxial film forming step of forming an epitaxial film (14b, 42, 44) of silicon carbide so as to fill the trench, a defect forming step of forming defects in an excess portion (42, 44) of the epitaxial film deposited on the surface of the semiconductor layer, and a removal step of scraping and removing the excess portion of the epitaxial film. In this manufacturing method, before performing the removal step, defects are formed in the excess portion of the epitaxial film to reduce the substantial hardness of the excess portion of the epitaxial film. As a result, in the removal step, the excess portion of the epitaxial film can be removed in a short time. [Brief description of the drawings]

[0009] [Figure 1] 1 is a schematic cross-sectional view of a main portion of a silicon carbide semiconductor device disclosed in this specification. [Diagram 2] 1A to 1C are schematic cross-sectional views of essential parts of a process for manufacturing a silicon carbide semiconductor device disclosed in this specification. [Diagram 3] 1A to 1C are schematic cross-sectional views of essential parts of a process for manufacturing a silicon carbide semiconductor device disclosed in this specification. [Figure 4] 1A to 1C are schematic cross-sectional views of essential parts of a process for manufacturing a silicon carbide semiconductor device disclosed in this specification. [Diagram 5] 1A to 1C are schematic cross-sectional views of essential parts of a process for manufacturing a silicon carbide semiconductor device disclosed in this specification. [Figure 6] 1A to 1C are schematic cross-sectional views of essential parts of a process for manufacturing a silicon carbide semiconductor device disclosed in this specification. [Figure 7] 1A to 1C are schematic cross-sectional views of essential parts of a process for manufacturing a silicon carbide semiconductor device disclosed in this specification. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The technical elements disclosed in this specification are listed below. Note that each of the technical elements below is useful independently.

[0011] The method for manufacturing a silicon carbide semiconductor device disclosed in the present specification may include a trench forming step of forming a trench in a silicon carbide semiconductor layer, an epitaxial film forming step of forming an epitaxial film of silicon carbide so as to fill the trench, a defect forming step of forming defects in an excess portion of the epitaxial film deposited on the surface of the semiconductor layer, and a removal step of scraping and removing the excess portion of the epitaxial film. This manufacturing method can be used in various steps for manufacturing a silicon carbide semiconductor device, and can also be used in steps other than the step of forming a superjunction structure. In the defect forming step, it is sufficient to form defects in at least a part of the excess portion of the epitaxial film. In this manufacturing method, before performing the removal step, defects are formed in the excess portion of the epitaxial film to reduce the substantial hardness of the excess portion of the epitaxial film. As a result, in the removal step, the excess portion of the epitaxial film can be removed in a short time.

[0012] In the above manufacturing method, the semiconductor layer may be of a first conductivity type, and the epitaxial film may be of a second conductivity type. In this case, the trench forming step may include forming a plurality of the trenches in the semiconductor layer to form a plurality of mesa portions of the first conductivity type remaining between the trenches. As a result, a superjunction structure is formed by the plurality of mesa portions of the first conductivity type and the plurality of epitaxial films of the second conductivity type filled in the plurality of trenches. According to this manufacturing method, the superjunction structure can be formed in a short time.

[0013] In the above manufacturing method, the excess portion of the epitaxial film may have a covering portion covering the entire surface of the semiconductor layer and a plurality of columnar portions protruding from the covering portion. In this case, the defect forming step may form defects in at least the covering portion. Since the substantial hardness of the covering portion, which is continuously expanded in the surface direction, is reduced, the excess portion of the epitaxial film can be removed in a short time.

[0014] In the defect forming step of the above-mentioned manufacturing method, defects may be formed by implanting ions into the excess portion of the epitaxial film. In this case, the ions may be non-metallic. It is possible to form defects in the excess portion of the epitaxial film while preventing metal contamination.

[0015] In the defect forming step of the above-mentioned manufacturing method, the ions may be implanted into the excess portion of the epitaxial film from a direction oblique to the surface of the semiconductor layer. Since channeling can be suppressed, defects can be formed at a predetermined depth in the excess portion based on implantation energy.

[0016] In the defect forming step of the above-described manufacturing method, the ions may be implanted in multiple stages into the excess portion of the epitaxial film. Since defects can be formed over a wide range in the thickness direction of the excess portion, the excess portion of the epitaxial film can be removed in a shorter time.

[0017] In the defect forming step of the above manufacturing method, a laser may be irradiated to the excess portion of the epitaxial film to form defects. In this case, in the defect forming step, the laser may be focused and irradiated to the excess portion of the epitaxial film. Defects can be efficiently formed in the excess portion of the epitaxial film. Note that the defect forming may be performed by only laser irradiation, or may be performed by combining ion implantation and laser irradiation.

[0018] In the defect forming step of the above-described manufacturing method, the excess portion of the epitaxial film may be irradiated with the laser in multiple stages. Since defects can be formed over a wide range in the thickness direction of the excess portion, the excess portion of the epitaxial film can be removed in a shorter time.

[0019] In the defect forming step of the above manufacturing method, the defect density of the excess portion of the epitaxial film may be adjusted so that the hardness of the excess portion of the epitaxial film in which defects are formed is smaller than the hardness of the abrasive material used in the removing step, so that the excess portion of the epitaxial film can be efficiently removed while suppressing damage to the semiconductor layer and the epitaxial film filled in the trench. EXAMPLES

[0020] 1 is a schematic cross-sectional view of a main portion of a silicon carbide semiconductor device 1. The silicon carbide semiconductor device 1 is a power semiconductor element known as a MOSFET, and includes a silicon carbide layer 10, a drain electrode 22 covering the back surface of the silicon carbide layer 10, a source electrode 24 covering the front surface of the silicon carbide layer 10, and a plurality of insulating trench gates 30 provided in trenches extending from the front surface of the silicon carbide layer 10 toward the depth thereof.

[0021] The silicon carbide layer 10 is, but is not limited to, for example, 4H silicon carbide, and the crystal plane of the surface is inclined by an off angle with respect to the (0001) Si plane. The off angle is, but is not limited to, for example, 4°. The silicon carbide layer 10 is n + a p-type drain region 12, a drift region 14, a p-type body region 16, + A source region 18 of the p + The semiconductor device has a body contact region 19 of the same type.

[0022] The drain region 12 is disposed in a lower portion of the silicon carbide layer 10 and is exposed on the back surface of the silicon carbide layer 10. The drain region 12 is in ohmic contact with a drain electrode 22 that covers the back surface of the silicon carbide layer 10.

[0023] The drift region 14 is provided between the drain region 12 and the body region 16, and has a plurality of n-type partial regions 14a and a plurality of p-type partial regions 14b. The n-type partial regions 14a and the p-type partial regions 14b are arranged alternately and repeatedly along at least one direction in the cross section of the silicon carbide layer 10, forming an SJ structure. Although not particularly limited, the plurality of n-type partial regions 14a and the plurality of p-type partial regions 14b are arranged in a stripe pattern in plan view.

[0024] The body region 16 is provided on the drift region 14 and arranged in an upper layer portion of the silicon carbide layer 10. The body region 16 is provided between the n-type partial region 14a of the drift region 14 and the source region 18, and is in contact with both the n-type partial region 14a and the source region 18, separating the n-type partial region 14a from the source region 18. The dopant concentration of the body region 16 is adjusted according to a desired gate threshold voltage.

[0025] The source region 18 is provided on the body region 16, is disposed in an upper portion of the silicon carbide layer 10, and is exposed on the surface of the silicon carbide layer 10. The source region 18 contacts a side surface of the insulating trench gate 30. The source region 18 is in ohmic contact with a source electrode 24 that covers the surface of the silicon carbide layer 10.

[0026] The body contact region 19 is provided on the body region 16, is disposed in an upper portion of the silicon carbide layer 10, and is exposed on the surface of the silicon carbide layer 10. The body contact region 19 is in ohmic contact with a source electrode 24 that covers the surface of the silicon carbide layer 10.

[0027] The insulating trench gate 30 is filled in a trench formed in an upper layer portion of the silicon carbide layer 10, and penetrates the source region 18 and the body region 16 to reach the n-type partial region 14a of the drift region 14. The insulating trench gate 30 has a gate electrode 32 and a gate insulating film 34. The gate electrode 32 is made of polysilicon containing impurities, and faces the silicon carbide layer 10 via the gate insulating film 34. In particular, the gate electrode 32 faces a part of the body region 16 that separates the n-type partial region 14a of the drift region 14 and the source region 18 via the gate insulating film 34. The gate insulating film 34 is made of silicon oxide, and covers the inner wall of the trench.

[0028] Next, the operation of the silicon carbide semiconductor device 1 will be described with reference to FIG. 1. When the potential of the gate electrode 32 of the insulating trench gate 30 is controlled to be more positive than the source electrode 24 and higher than the threshold value in a state in which the potential of the drain electrode 22 is more positive than the potential of the source electrode 24, the silicon carbide semiconductor device 1 turns on. At this time, an inversion layer is formed in the body region 16 in a portion separating the source region 18 and the n-type partial region 14a of the drift region 14. Electrons supplied from the source region 18 reach the n-type partial region 14a of the drift region 14 via the channel of the inversion layer. Electrons that reach the n-type partial region 14a flow to the drain region 12 via the n-type partial region 14a. The dopant concentration of the multiple n-type partial regions 14a that constitute the SJ structure is relatively high. For this reason, the silicon carbide semiconductor device 1 can have a characteristic of low on-resistance.

[0029] When the potential of the gate electrode 32 of the insulating trench gate 30 is controlled to be the same as the potential of the source electrode 24, the channel of the inversion layer disappears and the silicon carbide semiconductor device 1 is turned off. The multiple n-type partial regions 14a and the multiple p-type partial regions 14b constituting the SJ structure are fully depleted, and a wide range of the drift region 14 is depleted. In addition, since the drift region 14 has the SJ structure, the electric field distribution of the drift region 14 is leveled in the thickness direction. Therefore, the drift region 14 can bear a large potential difference, and the silicon carbide semiconductor device 1 can have a high breakdown voltage characteristic.

[0030] Next, a description will be given of a step of forming an SJ structure in a method for manufacturing silicon carbide semiconductor device 1. Known manufacturing techniques can be used for the other steps for manufacturing silicon carbide semiconductor device 1.

[0031] First, as shown in Figure 2, + A drain region 12 is prepared as a silicon carbide substrate. Next, an n-type epitaxial layer 140 of silicon carbide is grown on the surface of the drain region 12 by using an epitaxial growth technique such as, but not limited to, a CVD (Chemical Vapor Deposition) method. The n-type epitaxial layer 140 is an example of a semiconductor layer.

[0032] 3, a plurality of trenches TR extending from the surface to the depth of the n-type epilayer 140 are formed by using a dry etching technique such as, but not limited to, RIE (Reactive Ion Etching) (trench formation step). As a result, a plurality of mesa portions are formed by parts of the n-type epilayer 140 remaining between the trenches TR, and the plurality of mesa portions become the n-type partial regions 14a.

[0033] 4, a p-type epitaxial film of silicon carbide is formed so as to fill each of the trenches TR by using an epitaxial growth technique such as, but not limited to, a CVD (Chemical Vapor Deposition) method (epi-film formation step). The p-type epitaxial film filled in each of the trenches TR becomes the p-type partial region 14b. As a result, an SJ structure is formed by the n-type partial regions 14a and the p-type partial regions 14b.

[0034] 4, in the epitaxial film formation step, a p-type epitaxial film is also deposited on the surface of the n-type epilayer 140. The p-type epitaxial film deposited on the surface of the n-type epilayer 140 is not a part that constitutes the silicon carbide semiconductor device, but is an excess portion. This excess portion of the p-type epitaxial film has a covering portion 42 that covers the entire surface of the n-type epilayer 140, and a plurality of columnar portions 44 that protrude from the covering portion 42 above the n-type partial region 14a.

[0035] Next, as shown in FIG. 5, ions are implanted into the excess portion of the p-type epitaxial film using an ion implantation technique to form defects (defect formation process). As the ion species, non-metallic ions are used to prevent metal contamination, and although not particularly limited, argon ions are used, for example. In the defect formation process, ions are implanted into the excess portion of the p-type epitaxial film from an oblique direction relative to the surface of the n-type epitaxial layer 140. By performing such oblique ion implantation, channeling is suppressed and ions can be implanted to a predetermined depth in the excess portion. In addition, in the defect formation process, defects are formed at least in the covering portion 42 of the excess portion. Furthermore, in the defect formation process, ions are implanted in multiple stages to form defects at multiple depths in the excess portion. Instead of this example, in the defect formation process, defects may be formed in at least a part of the excess portion.

[0036] Next, as shown in Fig. 6, although not limited thereto, a grinding or polishing technique such as CMP (Chemical Mechanical Polishing) is used to remove the excess portion of the p-type epitaxial film, i.e., the covering portion 42 and the columnar portion 44 (removal step). As described above, defects are formed in the excess portion of the p-type epitaxial film before this removal step is performed, so that the substantial hardness of the excess portion of the p-type epitaxial film is reduced. Therefore, in the removal step, the excess portion of the p-type epitaxial film can be removed in a short time. Thus, in the manufacturing method of this embodiment, the SJ structure can be formed in a short time, and therefore the manufacturing cost can be reduced.

[0037] As described above, in the defect forming step, defects are formed at least in the covering portion 42 of the excess portion. The covering portion 42 has a shape that is continuously spread in the surface direction. For this reason, when such a covering portion 42 is removed using a grinding or polishing technique, the processing time tends to be long. In the manufacturing method of this embodiment, defects are formed in such a covering portion 42 to reduce the substantial hardness, so that the covering portion 42 can be removed in a short time in the removing step. Also, in the defect forming step, ions are implanted in multiple stages to form defects at multiple depths in the excess portion. Defects may be formed at multiple depths in the covering portion 42, or defects may be formed at multiple depths in the columnar portion 44. In this way, defects are formed over a wide range in the thickness direction of the excess portion of the p-type epitaxial film, so that the excess portion of the p-type epitaxial film can be removed in a short time in the removing step.

[0038] The hardness of the abrasive material used in the removal step is less than the hardness of silicon carbide in which no defects are formed, and greater than the hardness of the excess portion of the p-type epitaxial film in which defects are formed in the defect formation step. In other words, in the defect formation step, the defect density of the excess portion of the p-type epitaxial film is adjusted so that the hardness of the excess portion of the p-type epitaxial film in which defects are formed is less than the hardness of the abrasive material used in the removal step. This makes it possible to efficiently remove the excess portion of the p-type epitaxial film in the removal step while minimizing damage to the SJ structure (area in which no defects are formed).

[0039] In the above embodiment, an example of forming defects in the excess portion of the p-type epitaxial film by using ion implantation technology has been described. Instead of this example, or in addition to this example, as shown in FIG. 7, a laser may be irradiated to the excess portion of the p-type epitaxial film to form defects. Furthermore, as shown in FIG. 7, by concentrating the laser to increase the energy density, defects can be efficiently formed even in silicon carbide having high hardness. Note that even when laser irradiation is used, the position where defects are formed and the defect density may be the same as those of the ion implantation technology.

[0040] Although specific examples of the present invention have been described above in detail, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and variations of the specific examples exemplified above. Furthermore, the technical elements described in this specification or drawings exhibit technical utility alone or in various combinations, and are not limited to the combinations described in the claims at the time of filing. Furthermore, the technology exemplified in this specification or drawings can achieve multiple objectives simultaneously, and achieving one of these objectives is itself technically useful. [Explanation of symbols]

[0041] 1: silicon carbide semiconductor device, 10: silicon carbide layer, 12: drain region, 14: drift region, 14a: n-type partial region, 14b: p-type partial region, 16: body region, 18: source region, 19: body contact region, 22: drain electrode, 24: source electrode, 30: insulating trench gate, 32: gate insulating film, 34: gate electrode, 42: covering portion, 44: columnar portion, 140: n-type epitaxial layer

Claims

1. A method for manufacturing a silicon carbide semiconductor device (1), comprising: A trench forming step of forming a trench (TR) in a silicon carbide semiconductor layer (140); an epitaxial film formation step of forming an epitaxial film (14b, 42, 44) of silicon carbide so as to fill the trench; a defect formation step of forming defects in an excess portion (42, 44) of the epitaxial film deposited on the surface of the semiconductor layer; a removing step of scraping away the excess portion of the epitaxial film.

2. the semiconductor layer is of a first conductivity type, the epitaxial film is of a second conductivity type, In the trench forming step, a plurality of trenches are formed in the semiconductor layer to form a plurality of first conductivity type mesa portions (14a) remaining between the trenches; 2. The method for manufacturing a semiconductor device according to claim 1, wherein a superjunction structure is formed by the plurality of mesa portions of the first conductivity type and the plurality of epitaxial films of the second conductivity type filled in the plurality of trenches.

3. The excess portion of the epitaxial film has a covering portion (42) that covers the entire surface of the semiconductor layer, and a plurality of columnar portions (44) that protrude from the covering portion, The method for manufacturing a semiconductor device according to claim 2 , wherein in said defect forming step, defects are formed at least in said covered portion.

4. 4. The method for manufacturing a semiconductor device according to claim 1, wherein in the defect forming step, ions are implanted into the excess portion of the epitaxial film to form defects.

5. The method for manufacturing a semiconductor device according to claim 4 , wherein the ions are non-metallic.

6. 6. The method for manufacturing a semiconductor device according to claim 4, wherein in the defect forming step, the ions are implanted into the excess portion of the epitaxial film from a direction oblique to a surface of the semiconductor layer.

7. 7. The method for manufacturing a semiconductor device according to claim 4, wherein in the defect forming step, the ions are implanted into the excess portion of the epitaxial film in multiple stages.

8. 8. The method for manufacturing a semiconductor device according to claim 1, wherein in the defect forming step, a laser is irradiated to the excess portion of the epitaxial film to form defects.

9. The method for manufacturing a semiconductor device according to claim 8 , wherein in the defect forming step, the laser is focused and irradiated onto the excess portion of the epitaxial film.

10. 10. The method for manufacturing a semiconductor device according to claim 8, wherein in the defect forming step, the laser is irradiated to the excess portion of the epitaxial film in multiple stages.

11. 11. The method for manufacturing a semiconductor device according to claim 1, wherein in the defect formation step, a defect density of the excess portion of the epitaxial film is adjusted so that a hardness of the excess portion of the epitaxial film in which defects are formed is smaller than a hardness of an abrasive material used in the removal step.

Citation Information

Patent Citations

  • SiC WAFER PROCESSING METHOD

    JP2017195244A

  • Grinding device

    JP2017205817A

  • FLATTENING METHOD OF SiC SURFACE

    JP2018203611A

  • Method for manufacturing silicon carbide semiconductor device and method for manufacturing silicon carbide substrate

    JP2019140258A

  • Manufacturing method of silicon carbide substrate and silicon carbide substrate

    JP2020181966A