Controlled Porous Yttrium Oxide for Etching Applications

JP7560478B2Active Publication Date: 2024-10-02HERAEUS CONAMIC NORTH AMERICA LLC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021560433
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-01
Filing Date
2020-04-04
Publication Date
2024-10-02
Estimated Expiration
2040-04-04

AI Technical Summary

Technical Problem

Yttrium oxide materials used in plasma etching processes suffer from low sintering strength, high porosity, and poor adhesion, leading to erosion and contamination issues in semiconductor manufacturing, limiting their use in large-scale components.

Method used

A high-purity, high-density yttrium oxide sintered body with controlled pore size and impurity levels is produced through spark plasma sintering, ensuring minimal porosity and improved mechanical strength, suitable for large-scale components in plasma etching chambers.

Benefits of technology

The resulting yttrium oxide sintered body exhibits enhanced corrosion and erosion resistance, reduced particle generation, and improved etch resistance, extending component life and maintaining process integrity in harsh plasma environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560478000015
    Figure 0007560478000015
  • Figure 0007560478000016
    Figure 0007560478000016
  • Figure 0007560478000017
    Figure 0007560478000017
Patent Text Reader

Abstract

A yttrium oxide sintered body having a total impurity content of 40 ppm or less and a density of 4.93 g / cm or more, the yttrium oxide sintered body having at least one surface containing at least one pore, and no pores having a diameter greater than 5 μm. A method for producing the yttrium oxide sintered body is also disclosed.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to high purity and high density yttrium oxide sintered bodies, characteristics which translate into exceptional etching resistance when used as components in plasma etching chambers. Additionally, the present disclosure provides methods for producing the yttrium oxide sintered bodies. [Background technology]

[0002] In the field of semiconductor material processing, vacuum process chambers are used for etching and chemical vapor deposition (CVD) of materials on substrates. A process gas is introduced into the process chamber and simultaneously a radio frequency (RF) field is applied to the process gas, generating a plasma of the process gas.

[0003] During semiconductor substrate processing, the substrate is typically supported within a vacuum chamber by a substrate holder, as disclosed, for example, in US 5,262,029 and US 5,838,529. Process gases can be supplied to the chamber by a variety of gas delivery systems. Other equipment used in the processing of semiconductor substrates includes windows, nozzles, showerheads, (etch) chamber liners, mixing manifolds, wafer supports, electronic wafer chucks, and various rings (such as focus rings and guard rings), among other components.

[0004] In such processes, plasma is typically used to remove material on the chamber walls and substrate. Plasma etching conditions result in significant ion bombardment of the process chamber surfaces exposed to the plasma. This ion bombardment, combined with plasma species and / or etch by-products, can result in significant surface roughening, erosion, corrosion, and corrosion-erosion of the plasma-exposed surfaces of the process chamber. As a result, surface material is removed by physical and / or chemical attack. This attack causes problems such as reduced part life resulting in extended tool downtime, increased consumable costs, particulate contamination, transition metal contamination on the wafer, and process fluctuations.

[0005] Additionally, plasma processing chambers have been designed to include parts such as disks, rings, and cylinders that trap the plasma on the wafer being processed. However, these parts used in plasma processing chambers are continually attacked by the plasma, resulting in erosion and the accumulation of contaminants and polymer deposits.

[0006] Due to the erosive and corrosive nature of the plasma environment in such reactors, it is desirable to minimize particle and / or metallic contamination. Therefore, it is desirable for the components of such equipment, including consumables and other parts, to have a suitably high resistance to erosion and corrosion. Such parts are made of materials that provide resistance to corrosion and erosion in the plasma environment, as described, for example, in US 5,798,016, US 5,911,852, US 6,123,791, and US 6,352,611.

[0007] Yttrium oxide is known to exhibit significantly higher resistance to halogen-based corrosive gases and the plasmas of such gases than other common ceramic materials such as alumina, silicon carbide, silicon nitride, and zirconia, and is therefore widely used as a layer for corrosion-resistant components in semiconductor manufacturing equipment involving plasma processing.

[0008] However, there are drawbacks to the use of yttrium oxide. Yttrium oxide has persistent problems, such as low sintering strength, which prevents its development as a structural material in these plasma-resistant applications. Low sintering strength can also be a limiting factor in the manufacture of large parts due to breakage as the component size increases. Thus, yttrium oxide can be used as a corrosion-resistant component coating in some cases where components are manufactured by spraying yttrium oxide onto a base material made of a metallic material or a ceramic material made of other materials that are cheaper and stronger than yttrium oxide, such as alumina.

[0009] However, yttrium oxide materials still suffer from many drawbacks in plasma etching processes, such as high porosity in the yttria coating and low adhesion strength between the yttria and the base layer. The presence of voids in the coating will adversely affect the corrosion and erosion resistance of the components. In addition, yttrium oxide is difficult to sinter using conventional methods. Therefore, there is a need for yttrium oxide materials for use in plasma etching chambers that do not have such drawbacks.

[0010] Summary of the Invention These and other needs are addressed by the various embodiments, aspects, and configurations disclosed herein.

[0011] / 1 / Total impurities below 40 ppm and 4.93 g / cm 34. An yttrium oxide sintered body having a density of 1000 nm or more, said yttrium oxide sintered body having at least one surface containing at least one pore, and having no pores with a diameter exceeding 5 μm.

[0012] / 2 / The density is 4.96g / cm 3 The yttrium oxide sintered body according to claim 1, wherein:

[0013] / 3 / The density is 4.98 g / cm 3 The yttrium oxide sintered body according to claim 1 or 2.

[0014] / 4 / The density is 5.01 g / cm 3 The yttrium oxide sintered body according to any one of claims 1, 2, and 3.

[0015] / 5 / A yttrium oxide sintered body according to any one of the preceding claims, having no pores with a diameter exceeding 4 μm.

[0016] / 6 / A yttrium oxide sintered body according to any one of the preceding claims, having no pores with a diameter exceeding 3 μm.

[0017] / 7 / A yttrium oxide sintered body according to any one of the preceding claims, having no pores with a diameter exceeding 2 μm.

[0018] / 8 / A yttrium oxide sintered body according to any one of the preceding claims, having no pores with a diameter exceeding 1 μm.

[0019] / 9 / The yttrium oxide sintered body according to any one of the preceding claims, wherein the total amount of impurities is 35 ppm or less.

[0020] / 10 / The yttrium oxide sintered body according to any one of the preceding claims, wherein the total amount of impurities is 30 ppm or less.

[0021] / 11 / The yttrium oxide sintered body according to any one of the preceding claims, wherein the total amount of impurities is 25 ppm or less.

[0022] / 12 / The yttrium oxide sintered body according to any one of the preceding claims, wherein the total amount of impurities is 20 ppm or less.

[0023] / 13 / The yttrium oxide sintered body according to any one of the preceding claims, wherein the total amount of impurities is 15 ppm or less.

[0024] / 14 / The yttrium oxide sintered body according to any one of the preceding claims, wherein the total amount of impurities is 10 ppm or less.

[0025] / 15 / The yttrium oxide sintered body according to any one of the preceding claims, wherein the total amount of impurities is 6 ppm or less.

[0026] / 16 / In a process where a 10 mm x 5 mm area of ​​the at least one surface is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power, a 375,000 μm 3 5. The yttrium oxide sintered body according to claim 1, wherein the yttrium oxide sintered body exhibits an etching amount of less than 1000 nm, the process comprising a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 1500 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, the first and second steps being repeated successively until the exposure time to CF4 in the first step is 24 hours.

[0027] / 17 / Approx. 325,000μm 3 13. The yttrium oxide sintered body according to any one of the preceding claims, exhibiting an etching amount of less than 1000 nm.

[0028] / 18 / Approx. 275,000μm 313. The yttrium oxide sintered body according to any one of the preceding claims, exhibiting an etching amount of less than 1000 nm.

[0029] / 19 / The yttrium oxide sintered body according to any one of the preceding claims, having a pore size distribution with a maximum pore size of 1.50 μm for more than 95% of all pores on said at least one surface.

[0030] / 20 / The yttrium oxide sintered body according to any one of the preceding claims, having a pore size distribution with a maximum pore size of 1.75 μm for more than 97% of all pores on said at least one surface.

[0031] / 21 / The yttrium oxide sintered body according to any one of the preceding claims, having a pore size distribution with a maximum pore size of 2.00 μm for more than 99% of all pores on said at least one surface.

[0032] 22. The yttrium oxide sintered body of any one of the preceding claims, wherein a 10 mm x 5 mm area of ​​at least one surface exhibits an etch rate of less than 1.0 nm / min in a process subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 1500 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, the first step and the second step being repeated successively until the exposure time to CF4 in the first step is 24 hours.

[0033] / 23 / The yttrium oxide sintered body according to any one of the preceding claims, wherein the etching rate is 0.9 nm / min.

[0034] / 24 / The yttrium oxide sintered body according to any one of the preceding claims, wherein the etching rate is 0.8 nm / min.

[0035] / 25 / In the unetched area, 250 × 10 as determined by ISO standard 25178-2-2012, section 4.3.2 -5 13. The yttrium oxide sintered body according to claim 1, exhibiting a developed area Sdr of less than 130 mm.

[0036] / 26 / The developed area in the unetched area is 225×10 -5 13. The yttrium oxide sintered body according to any one of the preceding claims, wherein the yttrium oxide sintered body has a molecular weight of less than 1.0.

[0037] / 27 / The developed area in the unetched area is 200×10 -5 13. The yttrium oxide sintered body according to any one of the preceding claims, wherein the yttrium oxide sintered body has a molecular weight of less than 1.0.

[0038] / 28 / In a process in which a 6 mm x 6 mm x 2 mm area of ​​said at least one surface is subjected to etching conditions of 10 mTorr pressure with a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm, and an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts, the etched area is 200 x 10 -5 13. The yttrium oxide sintered body according to any one of the preceding claims, exhibiting a developed area of ​​less than 100 mm.

[0039] / 29 / The developed area of ​​the etched area is 175×10 -5 13. The yttrium oxide sintered body according to any one of the preceding claims, wherein the yttrium oxide sintered body has a molecular weight of less than 1.0.

[0040] / 30 / The developed area of ​​the etched area is 150×10 -5 13. The yttrium oxide sintered body according to any one of the preceding claims, wherein the yttrium oxide sintered body has a molecular weight of less than 1.0.

[0041] 31. The yttrium oxide sintered body of any one of the preceding claims, wherein a 10 mm by 5 mm area of ​​at least one surface exhibits an arithmetic mean roughness Sa of less than 30 nm as determined by ISO standard 25178-2-2012, section 4.1.7, in a process subjected to etching conditions of a pressure of 10 mTorr, an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 300 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and the first step and the second step being repeated consecutively for a total etching time of 6 hours.

[0042] / 32 / The yttrium oxide sintered body according to any one of the preceding claims, wherein Sa is less than 20 nm.

[0043] / 33 / The yttrium oxide sintered body according to any one of the preceding claims, wherein Sa is less than 15 nm.

[0044] / 34 / The yttrium oxide sintered body according to any one of the preceding claims, wherein the at least one surface has an area of ​​which less than 0.15% is occupied by pores.

[0045] / 35 / The yttrium oxide sintered body according to any one of the preceding claims, wherein the at least one surface has an area of ​​which less than 0.10% is occupied by pores.

[0046] / 36 / The yttrium oxide sintered body according to any one of the preceding claims, exhibiting a step change of 0.27-0.28 μm after an SF6 etching process.

[0047] / 37 / The yttrium oxide sintered body according to any one of the preceding claims, having a grain size d50 of 0.1 µm to 25 µm.

[0048] / 38 / The yttrium oxide sintered body according to any one of the preceding claims, having a grain size d50 of 0.5 μm to 15 μm.

[0049] / 39 / The yttrium oxide sintered body according to any one of the preceding claims, having a grain size d50 of 0.5 μm to 10 μm.

[0050] 40. The yttrium oxide sintered body according to any one of the preceding claims, having at least one dimension between 100 mm and 600 mm.

[0051] / 41 / The yttrium oxide sintered body according to any one of the preceding claims, having at least one dimension between 100 mm and 406 mm.

[0052] / 42 / The yttrium oxide sintered body according to any one of the preceding claims, having at least one dimension between 200 mm and 600 mm.

[0053] / 43 / The yttrium oxide sintered body according to any one of the preceding claims, having at least one dimension between 350 mm and 600 mm.

[0054] / 44 / The yttrium oxide sintered body according to any one of the preceding claims, having at least one dimension between 500 mm and 600 mm.

[0055] 10. The yttrium oxide sintered body according to any one of the preceding claims, having at least one dimension between 450 mm and 550 mm and 600 mm.

[0056] / 46 / A yttrium oxide sintered body according to any one of the preceding claims, wherein the density does not vary by more than 3% along at least one dimension.

[0057] / 47 / A yttrium oxide sintered body according to any one of the preceding claims, wherein the density does not vary by more than 2% along at least one dimension.

[0058] / 48 / A yttrium oxide sintered body according to any one of the preceding claims, wherein the density does not vary by more than 1% along at least one dimension.

[0059] A method for producing an yttrium oxide sintered body, comprising the steps of: placing yttrium oxide powder in a volume defined by a tool set of a sintering apparatus; forming a vacuum condition or an inert environment in the volume; applying a pressure of 10 MPa to 60 MPa to the yttrium oxide powder while heating to a sintering temperature of 1200 to 1600°C to form an yttrium oxide sintered body by sintering; and lowering the temperature of the yttrium oxide sintered body, 2 / g or less, and the yttrium oxide sintered body has a total impurity content of 40 ppm or less and a surface area of ​​4.93 g / cm 3 and at least one surface comprising at least one pore, wherein no pores have a diameter greater than 5 μm.

[0060] 50. The method of claim 49, further comprising: annealing the yttrium oxide sintered body by applying heat to raise the temperature of the yttrium oxide sintered body to an annealing temperature; reducing the temperature of the annealed yttrium oxide sintered body to ambient temperature by removing the heat source applied to the yttrium oxide sintered body; and, optionally, machining the annealed yttrium oxide sintered body to form a yttrium oxide sintered body component, the component being selected from the group consisting of a dielectric or RF window, a focus ring, a nozzle or gas injector, a showerhead, a gas distribution plate, an etching chamber liner, a plasma source adapter, a gas inlet adapter, a diffuser, an electronic wafer chuck, a chuck, a puck, a mixing manifold, an ion suppressor element, a faceplate, an isolator, a spacer, and a guard ring.

[0061] / 51 / The method according to any one of claims 49 to 50, wherein the yttrium oxide powder is calcined prior to step a).

[0062] / 52 / The method according to any one of claims 49 to 51, wherein the pressure applied to the yttrium oxide during heating is 10 MPa to 40 MPa.

[0063] / 53 / The method according to any one of claims 49 to 52, wherein the pressure applied to the yttrium oxide during heating is 20 MPa to 40 MPa.

[0064] / 54 / The yttrium oxide powder is 1.5 to 7.0 m 2 The method according to any one of claims 49 to 53, having a surface area of ​​ / g.

[0065] / 55 / The yttrium oxide powder is 2.0 to 4.0 m 2 The method according to any one of claims 49 to 54, having a surface area of ​​ / g.

[0066] / 56 / The method according to any one of claims 49 to 55, wherein the purity of the yttrium oxide powder is greater than 99.998%.

[0067] / 57 / The method according to any one of claims 49 to 56, wherein the purity of the yttrium oxide powder is greater than 99.999%.

[0068] / 58 / The method according to any one of claims 49 to 57, wherein the yttrium oxide sintered body has a purity of 99.99 to 99.999%.

[0069] / 59 / The method according to any one of claims 49 to 58, wherein the yttrium oxide sintered body has a purity of 99.999 to 99.9996%.

[0070] / 60 / A method according to any one of claims 49 to 59, wherein the sintering is carried out for a time period between 1 minute and 120 minutes.

[0071] / 61 / A method according to any one of claims 49 to 60, wherein the sintering is carried out for a time period between 2 minutes and 60 minutes.

[0072] / 62 / The yttrium oxide sintered body is 4.96 g / cm 3 The method according to any one of claims 49 to 61, having a density equal to or greater than 60%.

[0073] / 63 / The yttrium oxide sintered body is 4.98 g / cm 3 The method according to any one of claims 49 to 62, having a density equal to or greater than 60%.

[0074] / 64 / The yttrium oxide sintered body is 5.01 g / cm 3 The method according to any one of claims 49 to 63, having a density equal to or greater than 60%.

[0075] / 65 / A method according to any one of claims 49 to 64, wherein there are no pores on said at least one surface with a diameter greater than 4 µm.

[0076] / 66 / A method according to any one of claims 49 to 65, wherein there are no pores on said at least one surface with a diameter greater than 3 µm.

[0077] / 67 / A method according to any one of claims 49 to 66, wherein there are no pores on said at least one surface with a diameter greater than 2 µm.

[0078] / 68 / A method according to any one of claims 49 to 67, wherein there are no pores on said at least one surface with a diameter greater than 1 µm.

[0079] / 69 / The method according to any one of claims 49 to 68, wherein the total impurity content of the yttrium oxide sintered body is 35 ppm or less.

[0080] / 70 / The method according to any one of claims 49 to 69, wherein the total impurity content of the yttrium oxide sintered body is 30 ppm or less.

[0081] / 71 / The method according to any one of claims 49 to 70, wherein the total impurity content of the yttrium oxide sintered body is 25 ppm or less.

[0082] / 72 / The method according to any one of claims 49 to 71, wherein the total impurity content of the yttrium oxide sintered body is 20 ppm or less.

[0083] / 73 / The method according to any one of claims 49 to 72, wherein the total impurity content of the yttrium oxide sintered body is 15 ppm or less.

[0084] / 74 / The method according to any one of claims 49 to 73, wherein the total impurity content of the yttrium oxide sintered body is 10 ppm or less.

[0085] / 75 / The method according to any one of claims 49 to 74, wherein the total impurity content of the yttrium oxide sintered body is 6 ppm or less.

[0086] In a process in which a 10 mm x 5 mm area of ​​the at least one surface is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power, the yttrium oxide body is etched to a thickness of about 375,000 μm. 3 76. The method of claim 49, wherein the etching amount of the silicon dioxide gas is less than 100 nm, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 1500 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and the first step and the second step being repeated successively until the exposure time to CF4 in the first step is 24 hours.

[0087] / 77 / The yttrium oxide sintered body has a thickness of about 325,000 μm 3 77. The method according to claim 49, wherein the etching amount is less than 100 nm.

[0088] / 78 / The yttrium oxide sintered body has a thickness of about 275,000 μm 3 78. The method according to claim 49, wherein the etching amount is less than 100 nm.

[0089] / 79 / The method according to any one of claims 49 to 78, wherein the yttrium oxide sintered body has a pore size distribution having a maximum pore size of 1.50 μm for at least 95% of all pores on the at least one surface.

[0090] 80. The method according to any one of claims 49 to 79, wherein the yttrium oxide sintered body has a pore size distribution having a maximum pore size of 1.75 μm for 97% or more of all pores on the at least one surface.

[0091] / 81 / The method according to any one of claims 49 to 80, wherein the yttrium oxide sintered body has a pore size distribution having a maximum pore size of 2.00 μm for at least 99% of all pores on the at least one surface.

[0092] 82. The method of claim 49, wherein the yttrium oxide body exhibits an etch rate of less than 1.0 nm / min in a process where a 10 mm x 5 mm area of ​​at least one surface is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 1500 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and the first step and the second step are repeated successively until the exposure time to CF4 in the first step is 24 hours.

[0093] / 83 / A method according to any one of claims 49 to 82, wherein the etching rate is less than 0.9 nm / min.

[0094] / 84 / A method according to any one of claims 49 to 83, wherein the etching rate is less than 0.8 nm / min.

[0095] In the unetched areas, the yttrium oxide sintered body has a thickness of 250×10 as determined by ISO standard 25178-2-2012, section 4.3.2. -5 The method according to any one of claims 49 to 84, wherein the method exhibits a development area Sdr of less than 100 mm.

[0096] / 86 / The developed area in the unetched area is 225×10 -5 The method according to any one of claims 49 to 85, wherein the amount of

[0097] / 87 / The developed area in the unetched area is 200×10 -5 The method according to any one of claims 49 to 86, wherein the amount is less than 100%.

[0098] / 88 / In a process where a 6 mm x 6 mm x 2 mm area of ​​the at least one surface is subjected to etching conditions of 10 mTorr with a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm, and an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts, the yttrium oxide sintered body is etched to a thickness of 200 x 100 nm as determined by ISO standard 25178-2-2012, section 4.3.2. -5 The method according to any one of claims 49 to 87, wherein the method exhibits a development area of ​​less than 100 mm.

[0099] / 89 / The developed area of ​​the etched area is 175×10 -5 The method according to any one of claims 49 to 88, wherein the amount is less than 100%.

[0100] / 90 / The developed area of ​​the etched area is 150×10 -5 The method according to any one of claims 49 to 89, wherein the amount of

[0101] 91. The method of claim 49, wherein a 10 mm by 5 mm area of ​​at least one surface is subjected to etching conditions of a pressure of 10 mTorr, an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 300 seconds, and the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, a total etching time of 6 hours, and steps 1 and 2 being repeated consecutively, wherein the yttrium oxide sintered body exhibits an arithmetic mean roughness Sa of less than 30 nm as determined by ISO standard 25178-2-2012, section 4.1.7.

[0102] / 92 / The method according to any one of claims 49 to 91, wherein Sa is less than 20.

[0103] / 93 / The method according to any one of claims 49 to 92, wherein Sa is less than 15.

[0104] / 94 / A method according to any one of claims 49 to 93, wherein the at least one surface has an area of ​​which less than 0.15% is occupied by pores.

[0105] / 95 / A method according to any one of claims 49 to 94, wherein the at least one surface has an area of ​​which less than 0.10% is occupied by pores.

[0106] / 96 / The method according to any one of claims 49 to 95, wherein the yttrium oxide sintered body has a grain size d50 of 0.1 µm to 25 µm.

[0107] / 97 / The method according to any one of claims 49 to 96, wherein the yttrium oxide sintered body has a grain size d50 of 0.5 µm to 15 µm.

[0108] / 98 / The method according to any one of claims 49 to 97, wherein the yttrium oxide sintered body has a grain size d50 of 0.5 µm to 10 µm.

[0109] / 99 / The method according to any one of claims 49 to 98, wherein the yttrium oxide sintered body has at least one dimension between 100 mm and 600 mm.

[0110] / 100 / The method according to any one of claims 49 to 99, wherein the yttrium oxide sintered body has at least one dimension between 100 mm and 406 mm.

[0111] / 101 / The method according to any one of claims 49 to 100, wherein the yttrium oxide sintered body has at least one dimension between 200 mm and 600 mm.

[0112] / 102 / The method according to any one of claims 49 to 101, wherein the yttrium oxide sintered body has at least one dimension between 350 mm and 600 mm.

[0113] / 103 / The method according to any one of claims 49 to 102, wherein the yttrium oxide sintered body has at least one dimension between 500 mm and 600 mm.

[0114] / 104 / The method according to any one of claims 49 to 103, wherein the yttrium oxide sintered body has at least one dimension between 550 mm and 600 mm.

[0115] / 105 / A method according to any one of claims 49 to 104, wherein the density does not vary by more than 3% along at least one dimension.

[0116] / 106 / A method according to any one of claims 49 to 105, wherein the density does not vary by more than 2% along at least one dimension.

[0117] / 107 / A method according to any one of claims 49 to 106, wherein the density does not vary by more than 1% along at least one dimension.

[0118] / 108 / The method according to any one of claims 49 to 107, wherein the yttrium oxide sintered body exhibits a step change of 0.27 to 0.28 µm after an SF6 etching process.

[0119] A method for producing an yttrium oxide sintered body, comprising the steps of: placing yttrium oxide powder in a volume defined by a tool set of a sintering apparatus; forming a vacuum condition or an inert environment in the volume; applying a pressure of 10 MPa to 60 MPa to the yttrium oxide powder while heating to a sintering temperature of 1200 to 1600°C to form an yttrium oxide sintered body by sintering; and lowering the temperature of the yttrium oxide sintered body, 2 / g or less, and the yttrium oxide sintered body has a total impurity content of 40 ppm or less and a surface area of ​​4.93 g / cm 3 and at least one surface comprising at least one pore, and wherein the pores do not have a diameter greater than 5 μm.

[0120] 110 / The yttrium oxide sintered body of claim 109, wherein the method further comprises the steps of annealing the yttrium oxide sintered body by applying heat to raise the temperature of the yttrium oxide sintered body to an annealing temperature, lowering the temperature of the annealed yttrium oxide sintered body, and machining the annealed yttrium oxide sintered body to form an yttrium oxide sintered body component, the component being selected from the group consisting of a dielectric or RF window, a focus ring, a nozzle or gas injector, a showerhead, a gas distribution plate, an etching chamber liner, a plasma source adapter, a gas inlet adapter, a diffuser, an electronic wafer chuck, a chuck, a puck, a mixing manifold, an ion suppressor element, a faceplate, an isolator, a spacer, and a guard ring.

[0121] / 111 / The density is 4.96g / cm 3 111. The yttrium oxide sintered body according to claim 109, wherein the yttrium oxide sintered body is a sintered body having an yttrium oxide content of 100 to 115.

[0122] / 112 / The density is 4.98g / cm 3 112. The yttrium oxide sintered body according to claim 109, wherein the yttrium oxide sintered body is a sintered body having an yttrium oxide content of 100% or more.

[0123] / 113 / The density is 5.01 g / cm 3 113. The yttrium oxide sintered body according to any one of claims 109 to 112.

[0124] / 114 / The yttrium oxide sintered body according to any one of claims 109 to 113, having no pores with a diameter exceeding 4 µm.

[0125] / 115 / The yttrium oxide sintered body according to any one of claims 109 to 114, having no pores with a diameter exceeding 3 µm.

[0126] / 116 / The yttrium oxide sintered body according to any one of claims 109 to 115, having no pores with a diameter exceeding 2 µm.

[0127] / 117 / The yttrium oxide sintered body according to any one of claims 109 to 116, having no pores with a diameter exceeding 1 µm.

[0128] / 118 / The yttrium oxide sintered body according to any one of claims 109 to 117, wherein the amount of impurities is 35 ppm or less.

[0129] / 119 / The yttrium oxide sintered body according to any one of claims 109 to 118, wherein the amount of impurities is 30 ppm or less.

[0130] / 120 / The yttrium oxide sintered body according to any one of claims 109 to 119, wherein the amount of impurities is 25 ppm or less.

[0131] / 121 / The yttrium oxide sintered body according to any one of claims 109 to 120, wherein the amount of the impurities is 20 ppm or less.

[0132] / 122 / The yttrium oxide sintered body according to any one of claims 109 to 121, wherein the amount of impurities is 15 ppm or less.

[0133] / 123 / The yttrium oxide sintered body according to any one of claims 109 to 122, wherein the amount of impurities is 10 ppm or less.

[0134] / 124 / The yttrium oxide sintered body according to any one of claims 109 to 123, wherein the amount of impurities is 6 ppm or less.

[0135] In a process where a 10 mm by 5 mm area of ​​the at least one surface is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power, a 375,000 μm 3125. The yttrium oxide sintered body according to claim 109, wherein the yttrium oxide sintered body exhibits an etching amount of less than 1000 nm, the process has a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 1500 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and the first step and the second step are continuously repeated until the exposure time to CF4 in the first step is 24 hours.

[0136] / 126 / Approx. 325,000μm 3 126. The yttrium oxide sintered body according to claim 109, which exhibits an etching amount of less than 100%.

[0137] / 127 / Approx. 275,000μm 3 127. The yttrium oxide sintered body according to any one of claims 109 to 126, which exhibits an etching amount of less than 100%.

[0138] / 128 / The yttrium oxide sintered body according to any one of claims 109 to 127, having a pore size distribution in which 95% or more of all pores on the at least one surface have a maximum pore size of 1.50 µm.

[0139] / 129 / The yttrium oxide sintered body according to any one of claims 109 to 128, having a pore size distribution in which 97% or more of all pores on the at least one surface have a maximum pore size of 1.75 µm.

[0140] / 130 / The yttrium oxide sintered body according to any one of claims 109 to 129, having a pore size distribution in which 99% or more of all pores on the at least one surface have a maximum pore size of 2.00 µm.

[0141] / 131 / The yttrium oxide sintered body according to any one of claims 109 to 130, wherein a 10 mm x 5 mm area of ​​the at least one surface exhibits an etch rate of less than 1.0 nm / min in a process subjected to etching conditions of a pressure of 10 mTorr, an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 1500 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and the first step and the second step being repeated continuously until the exposure time to CF4 in the first step is 24 hours.

[0142] / 132 / The yttrium oxide sintered body according to any one of claims 109 to 131, wherein the etching rate is 0.9 nm / min.

[0143] / 133 / The yttrium oxide sintered body according to any one of claims 109 to 132, wherein the etching rate is 0.8 nm / min.

[0144] / 134 / In the unetched area, 250 × 10 as determined by ISO standard 25178-2-2012, section 4.3.2 -5 134. The yttrium oxide sintered body according to any one of claims 109 to 133, having a developed area Sdr of less than 100 μm.

[0145] / 135 / The developed area in the unetched area is 225×10 -5 135. The yttrium oxide sintered body according to any one of claims 109 to 134, wherein the yttrium oxide sintered body is less than 100%.

[0146] / 136 / The developed area in the unetched area is 200×10 -5 136. The yttrium oxide sintered body according to any one of claims 109 to 135, wherein the yttrium oxide sintered body is less than 100%.

[0147] / 137 / In a process in which a 6 mm x 6 mm x 2 mm area of ​​said at least one surface is subjected to etching conditions of 10 mTorr pressure with a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm, and an argon flow rate of 20 sccm, and a bias of 600 volts and an ICP power of 2000 watts, the etched area is 200 x 10 -5 137. The yttrium oxide sintered body according to any one of claims 109 to 136, having a developed area of ​​less than 100 mm.

[0148] / 138 / The developed area of ​​the etched region is 175×10 -5 The yttrium oxide sintered body according to any one of claims 109 to 137, wherein the yttrium oxide sintered body is less than 100%.

[0149] / 139 / The developed area of ​​the etched region is 150×10 -5 The yttrium oxide sintered body according to any one of claims 109 to 138, wherein the yttrium oxide sintered body is less than 100%.

[0150] / 140 / The yttrium oxide sintered body according to any one of claims 109 to 139, wherein a 10 mm x 5 mm area of ​​the at least one surface exhibits an arithmetic mean roughness Sa of less than 30 nm as determined by ISO standard 25178-2-2012, section 4.1.7, in a process subjected to etching conditions of a pressure of 10 mTorr, an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 300 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and the first step and the second step being repeated consecutively for a total etching time of 6 hours.

[0151] / 141 / The yttrium oxide sintered body according to any one of claims 109 to 140, wherein Sa is less than 20 nm.

[0152] / 142 / The yttrium oxide sintered body according to any one of claims 109 to 141, wherein Sa is less than 15 nm.

[0153] / 143 / The yttrium oxide sintered body according to any one of claims 109 to 142, wherein the at least one surface has an area in which less than 0.15% is occupied by pores.

[0154] / 144 / The yttrium oxide sintered body according to any one of claims 109 to 143, wherein the at least one surface has a region where less than 0.10% of the surface is occupied by pores.

[0155] / 145 / The yttrium oxide sintered body according to any one of claims 109 to 144, which exhibits a step change of 0.27 to 0.28 µm after an SF6 etching process.

[0156] / 146 / The yttrium oxide sintered body according to any one of claims 109 to 145, having a grain size d50 of 0.1 µm to 25 µm.

[0157] / 147 / The yttrium oxide sintered body according to any one of claims 109 to 146, having a grain size d50 of 0.5 µm to 15 µm.

[0158] / 148 / The yttrium oxide sintered body according to any one of claims 109 to 147, having a grain size d50 of 0.5 µm to 10 µm.

[0159] / 149 / The yttrium oxide sintered body according to any one of claims 109 to 148, having at least one dimension of 100 mm to 600 mm.

[0160] The yttrium oxide sintered body according to any one of claims 109 to 149, having at least one dimension of 100 mm to 406 mm.

[0161] / 151 / The yttrium oxide sintered body according to any one of claims 109 to 150, having at least one dimension of 200 mm to 600 mm.

[0162] / 152 / The yttrium oxide sintered body according to any one of claims 109 to 151, having at least one dimension of 350 mm to 600 mm.

[0163] / 153 / The yttrium oxide sintered body according to any one of claims 109 to 152, having at least one dimension of 500 mm to 600 mm.

[0164] / 154 / The yttrium oxide sintered body according to any one of claims 109 to 153, having at least one dimension of 550 mm to 600 mm.

[0165] / 155 / The yttrium oxide sintered body according to any one of claims 109 to 154, wherein the density does not vary by more than 3% along at least one dimension.

[0166] / 156 / The yttrium oxide sintered body according to any one of claims 109 to 155, wherein the density does not vary by more than 2% along at least one dimension.

[0167] / 157 / The yttrium oxide sintered body according to any one of claims 109 to 156, wherein the density does not vary by more than 1% along at least one dimension.

[0168] The above-described embodiments of the yttrium oxide sintered body and the method for producing the yttrium oxide sintered body can be combined in any manner and the embodiments can be combined. Thus, as outlined in the following description, the above-described features can be combined to describe the yttrium oxide body and / or the method, and vice versa.

[0169] The development is described by way of example only with reference to the accompanying drawings, in which: Features disclosed in relation to the yttrium oxide sintered body also apply to the method and vice versa. [Brief description of the drawings]

[0170] [Figure 1] 1 is a semiconductor processing system in accordance with an embodiment of the present technique. [Diagram 2] 1 is another embodiment of a semiconductor processing system in accordance with embodiments of the present technique. [Diagram 3] CF etch amount for prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure. [Figure 4] CF4+O2 average etch amount for prior art TSC 03 (quartz) and sintered yttrium oxide samples 118 and 107 compared to various sintered yttrium oxide samples produced according to embodiments of the present disclosure. [Diagram 5] CF4+O2 average step height for prior art TSC 03 (quartz) and sintered yttrium oxide samples 118 and 107 compared to various sintered yttrium oxide samples produced according to embodiments of the present disclosure. [Figure 6] CF4+O2 average etch rate of prior art TSC 03 (quartz) and sintered yttrium oxide samples 118 and 107 compared to various samples manufactured according to embodiments of the present disclosure. [Figure 7] 5A-5C are SEM micrographs at 50x of the surfaces of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 before and after a CF4 etching process. [Figure 8] 5A-5C are SEM micrographs at 50x of the surfaces of sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 produced in accordance with the present disclosure before and after a CF4 etching process. [Figure 9]1A-1C are SEM micrographs at 1000x of the surfaces of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 before and after a CF4 etching process. [Figure 10] 1000X SEM micrographs of the surfaces of sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 produced in accordance with the present disclosure before and after a CF4 etching process. [Figure 11] 5A-5C are SEM micrographs at 5000x of the surfaces of prior art sintered yttrium oxide samples 107 and 118 before and after a CF4+O2 etching process. [Figure 12] 5A-5C are SEM micrographs at 5000X of the surfaces of sintered yttrium oxide samples 152 and 189-1 produced in accordance with the present disclosure before and after a CF4+O2 etching process. [Figure 13] 1A-1C are SEM micrographs at 1000X and 5000X of the edge surface of a sintered yttrium oxide sample and the center surface of the same sintered yttrium oxide sample 457 produced in accordance with the present disclosure. [Figure 14] This shows that the yttrium oxide body (H1 / 66 to H4 / 152) according to one embodiment of the present disclosure does not have pores with a pore size exceeding 2.00 μm. [Figure 15] 1 is a graph showing the developed area ratio Sdr at 50x optical magnification of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure before and after a CF4 etching process. [Figure 16] 1 is a graph showing the arithmetic mean height Sa (nm) measured at 50x optical magnification of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure before and after a CF4 etching process. [Figure 17]1 is a graph showing the developed area ratio Sdr measured at 50x optical magnification of the prior art sintered yttrium oxide sample CM1 / 107 from the examples and various sintered yttrium oxide samples before and after the CF4+O2 etching process. [Figure 18] 1 is a graph showing the arithmetic mean height Sa (nm) measured at an optical magnification of 50x of the prior art sintered yttrium oxide sample CM1 / 107 from the examples and various sintered yttrium oxide samples before and after the CF4+O2 etching process. [Figure 19] 1 is a graph showing the percent area porosity of various sintered yttrium oxide samples from the examples compared to prior art sintered yttrium oxide samples. [Figure 20] 1 is a graph showing cumulative area % versus pore size (pore size distribution) for various samples from the examples compared to a prior art sintered yttrium oxide sample. [Figure 21] 1 is a graph showing porosity distribution versus log pore size for various samples from the examples compared to prior art sintered yttrium oxide samples. [Figure 22] 1 is a graph showing sintering pressure and temperature conditions required for obtaining an yttrium oxide sintered body having a density 98% or more higher than the theoretical density of yttrium oxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0171] Yttrium oxide sintered bodies are proposed as materials for parts used in plasma etch process chambers manufactured by the sintering process disclosed herein, including windows, nozzles, showerheads, (etch) chamber liners, mixing manifolds, wafer supports, electronic wafer chucks, and various rings (such as focus rings and guard rings), among other components.

[0172] Reference will now be made in detail to specific embodiments. Examples of specific embodiments are illustrated in the accompanying drawings. Although the present disclosure will be described in conjunction with these specific implementations, it will be understood that it is not intended to limit the present disclosure to such specific embodiments. Rather, it is intended to cover alternatives, modifications, and equivalents that may be included within the spirit and scope defined by the appended claims. In the following description, numerous specific details are set forth in order to provide a thorough understanding of the disclosed embodiments. This disclosure can be practiced without some or all of these specific details.

[0173] definition As used herein, the terms "semiconductor wafer," "wafer," "substrate," and "wafer substrate" are used interchangeably. Wafers or substrates used in the semiconductor device industry typically have a diameter of, for example, 200 mm, or 300 mm, or 450 mm.

[0174] As used herein, the term "yttrium oxide sintered body" is synonymous with "sinter," "body," or "sintered body" or "ceramic sintered body," and refers to a solid article that includes yttrium oxide and is formed when exposed to a pressure and heat treatment process that forms a monolithic yttrium oxide sintered body from the yttrium oxide powder disclosed herein.

[0175] The term "purity" as used herein refers to the presence of various contaminants that are typically considered detrimental in application to the starting materials capable of forming the yttrium oxide sintered bodies disclosed herein.

[0176] As used herein, the term "tool set" can include a die and two punches, and can optionally also include additional spacer elements.

[0177] As used herein, the terms "stiffness" and "rigidity" are synonymous and are consistent with the definition of Young's modulus known to those of skill in the art.

[0178] The terms "calcination" or "calcining" when used in reference to a heat treatment process are understood herein to mean a heat treatment step that may be performed on a powder in air at a temperature below the sintering temperature to remove moisture and / or impurities, to increase crystallinity, and in some cases to modify the surface area of ​​the powder mixture.

[0179] The term "annealing" as applied to ceramic heat treatment is understood herein to mean a heat treatment performed on the yttrium oxide sintered body of the present disclosure in air to a temperature and allowed to cool slowly to relieve stresses and / or normalize stoichiometry.

[0180] The term "Sa" as known in the art relates to the arithmetic mean height of a surface and represents the absolute value of the arithmetic mean over the entire surface. The definition according to ISO 25178-2-2012 section 4.1.7 is the arithmetic mean of the absolute values ​​of the ordinate values ​​within a defined area (A).

[0181] The term "Sdr" as known in the art refers to a calculated number defined as the "Developed Area Ratio" and is a proportional expression of the increase in actual surface area over that of a perfectly flat surface. The definition according to ISO 25178-2-2012 section 4.3.2 is the ratio of the increase in interfacial area of ​​a scale-limited surface within a defined area (A) to the defined area.

[0182] As used herein, the term "about" in connection with numbers allows for a variation of plus or minus 10%.

[0183] In the following description, the indicated ranges include the lower and upper thresholds. Thus, a definition of a parameter A in the sense of "within the range of X and Y" or "within the range between X and Y" means that A may be any value of X and Y and any value between X and Y. A definition of a parameter A in the sense of "up to Y" or "at least X" means that A may be any value less than Y and Y, or A may be any value greater than X and X, respectively.

[0184] Yttrium oxide sintered body The following detailed description assumes that the invention is practiced in an apparatus such as an etching or deposition chamber necessary as part of the manufacture of semiconductor wafer substrates. However, the invention is not so limited. The workpieces may be of various shapes, sizes, and materials. In addition to semiconductor wafer processing, other workpieces that may utilize the invention include various articles such as inorganic circuit boards with fine feature sizes, magnetic recording media, magnetic recording sensors, mirrors, optical elements, micromechanical devices, and the like.

[0185] Semiconductor processing reactors associated with etching or deposition processes require chamber components fabricated from materials that are highly resistant to chemical corrosion by the reactive plasmas required for semiconductor processing. These plasmas or process gases may be composed of various halogen, oxygen, and nitrogen based chemicals such as O2, F, Cl2, HBr, BCl3, CCl4, N2, NF3, NO, N2O, C2H4, CF4, SF6, C4F8, CHF3, CH2F2, etc. Use of the corrosion resistant materials disclosed herein reduces chemical corrosion during use.

[0186] 1 and 2 show an etching / deposition chamber in which the yttrium oxide sintered body disclosed herein is useful. As shown in FIG. 1, an embodiment of the present technology may include a semiconductor processing system 9500, also referred to as a processing system. The processing system 9500 may include a remote plasma region. The remote plasma region may include a plasma source 9502, also referred to as a remote plasma source ("RPS").

[0187] The processing system 9500, which may represent a capacitively coupled plasma (CCP) processing apparatus, includes a vacuum chamber 9550, a vacuum source, and a chuck 9508 on which a wafer 50, also denoted as a semiconductor substrate, is supported. A window 9507 forms the upper wall of the vacuum chamber 9550. The window 9507 may be made of yttrium oxide sintered body according to one of the previously described embodiments. In some embodiments, the window 9507 may be partially made of yttrium oxide sintered body according to one of the previously described embodiments. 9506 may be a gas inlet, and the gas inlet assembly gas supply system injector or nozzle may be made of yttrium oxide sintered body. The gas injector 9506 may include a separate member of the same or different material as the window.

[0188] The plasma source 9502 is provided outside a window 9507 of the vacuum chamber 9550 to accommodate the wafer 50 to be processed. In the vacuum chamber 9550, a capacitively coupled plasma can be generated by supplying a process gas to the vacuum chamber 9550 and supplying a high frequency power to the plasma source 9502. A predetermined plasma process is performed on the wafer 50 using the capacitively coupled plasma thus generated. A planar antenna having a predetermined pattern is widely used as the high frequency antenna of the capacitively coupled processing system 9500.

[0189] The processing system 9500 may further include an electrostatic chuck 9508 designed to carry the wafer 50. The chuck 9508 may include a puck 9509 for supporting the wafer 50. The puck 9509 may have a chuck electrode disposed in the puck near a support surface of the puck 9509 and electrostatically holding the wafer 50 when disposed on the puck 9509. The chuck 9508 may include a base 9511 extending in a ring shape to support the puck 9509, and a shaft 9510 disposed between the base and the puck and supporting the puck on the base such that a gap is formed between the puck 9509 and the base 9510, the shaft 9510 supporting the puck close to the periphery of the puck 9509. The puck 9509 may be manufactured from a yttrium oxide sintered body according to one of the previous embodiments to minimize generated particles that may contaminate the wafer.

[0190] In a physical vapor deposition (PVD) process, a substrate ring including a cover ring 9514 is provided around the substrate. The cover ring 9514 typically has a lip or ledge that surrounds the wafer and rests on the wafer support surface of the puck 9509. The cover ring 9514 protects the sidewall surfaces and periphery of the puck 9509, which would otherwise be exposed to energized gases in the chamber, from the deposition of process residues. Thus, the cover ring 9514 reduces the buildup of process residues on the puck 9509. Such buildup of process residues would eventually flake off and contaminate the wafer. The cover ring 9514 can be fabricated from a sintered yttrium oxide body according to one of the embodiments described above.

[0191] The cover ring 9514 may also reduce erosion of the puck 9509 by energized gases. The provision of the cover ring 9514 also reduces the frequency with which the chuck and / or puck 9509 require cleaning, since the cover ring itself may be periodically removed from the chamber and cleaned, for example with HF or HNO3, to remove process residues that build up on the ring during substrate processing cycles. The placement of the cover ring 9514 can be seen in FIG. 1 where it covers a portion of the support surface of the puck 9509. However, another portion of the surface of the puck 9509 may be covered by the upper shield ring 9512 and / or the shield ring 9513. To obtain a suitably high resistance to erosion and corrosion, the upper shield ring 9512 and / or the shield ring 9513 may be manufactured from a sintered yttrium oxide body according to one of the previously described embodiments.

[0192] As shown in FIG. 2, another embodiment of the present technology may include a semiconductor processing system 9600. The processing system 9600, which may represent an inductively coupled plasma (ICP) processing apparatus, includes a vacuum chamber 9650, a vacuum source, and a chuck 9608 on which a wafer 50, also shown as a semiconductor substrate, is supported. A showerhead 9700 forms an upper wall of the vacuum chamber 9650 or is attached below the upper wall of the vacuum chamber 9650. The ceramic showerhead 9700 includes a gas plenum in fluid communication with a plurality of showerhead gas outlets for supplying process gases to the interior of the vacuum chamber 9650. Additionally, the showerhead 9700 may include a central opening configured to receive a central gas injector. An RF energy source excites the process gases into a plasma state to process the semiconductor substrate. The flow rate of the process gases provided by the central gas injector and the flow rate of the process gases provided by the ceramic showerhead 9700 may be independently controlled. The processing system 9600 may include a showerhead 9700, which may be fabricated from yttrium oxide sintered body according to one of the embodiments described above. The showerhead 9700 may be in fluid communication with a gas supply system 9606. The gas supply system 9606 may be fabricated from yttrium oxide sintered body and may have an injector or nozzle 9714 made from yttrium oxide sintered body.

[0193] The system 9600 may further include a chuck 9608 designed to carry the wafer 50. The chuck 9608 may include a puck 9609 for supporting the wafer 50. The puck 9609 may be formed from a dielectric material and may have a chuck electrode disposed within the puck near a support surface of the puck 9609 for electrostatically holding the wafer 50 when placed on the puck 9609. The chuck 9608 may include a base 9611 extending in a ring shape to support the puck 9609, and a shaft 9610 disposed between the base and the puck to support the puck on the base such that a gap is formed between the puck 9609 and the base 9610, the shaft 9610 supporting the puck close to the periphery of the puck 9609. The puck 9609 may be manufactured from a yttrium oxide sintered body according to one of the embodiments described above to minimize generated particles that may contaminate the wafer.

[0194] A portion of the surface of the showerhead 9700 may be covered with a shield ring 9712. A portion of the surface of the showerhead 9700, in particular a radial side of the surface of the showerhead 9700, may be covered with an upper shield ring 9710. A portion of the support surface of the puck 9609 may be covered with a cover ring 9614. Another portion of the surface of the puck 9609 may be covered with an upper shield ring 9612 and / or an insulating ring 9613. To obtain a suitably high erosion and corrosion resistance, the cover ring 9614 and / or the upper shield ring 9612 and / or the insulating ring 9613 may be manufactured from an yttrium oxide sintered body according to one of the previously described embodiments.

[0195] The showerhead 9700 can include two parallel plates, both of which can include or can consist of yttrium oxide sintered bodies according to one of the embodiments disclosed herein. The two plates can be bonded together to define a volume between the plates. The bonding of the plates can provide a fluid flow path through the upper plate and the lower plate. The showerhead can distribute process gases through the fluid flow paths, including plasma effluent upon excitation by plasma in the chamber plasma region or from the plasma source. An ion suppressor (not shown) can be disposed near a surface of the second plate and can be bonded to the surface of the second plate. The ion suppressor can include or can consist of yttrium oxide sintered bodies according to one of the embodiments disclosed herein. The ion suppressor can be configured to reduce ion migration to a processing region of the process chamber housing the wafer. The ion suppressor can define a plurality of openings through the structure.

[0196] Providing chamber construction materials such as sintered ceramic bodies with very high purity results in a uniform corrosion-resistant body with few impurities that can act as initiation sites for corrosion. Materials used as chamber components also require high resistance to erosion and spalling. However, erosion can result from ion bombardment of the component surfaces from the use of inert plasma gases such as Ar, as discussed above. Additionally, components made from dense materials with minimal voids distributed on a fine scale may provide greater resistance to corrosion and erosion during etching and deposition processes. As a result, preferred chamber components may be made from materials that have high resistance to erosion and corrosion during plasma etching, deposition, and chamber cleaning processes. This resistance to corrosion and erosion prevents the release of particles from the component surfaces into the etching or deposition chamber during semiconductor processing. The release or shedding of such particles into the process chamber contributes to wafer contamination, semiconductor process fluctuations, and semiconductor device level yield loss.

[0197] In addition, chamber components must have sufficient bending strength and stiffness for handling required during component installation, removal, cleaning, and use within the process chamber. High mechanical strength allows intricate features with fine geometries to be machined into the sintered ceramic body without breaking, cracking, or chipping. Bending strength or stiffness becomes especially important with the large component sizes used in modern process tools. For some component applications, such as chamber windows on the order of 200-600 mm in diameter, corrosion-resistant materials must be selected due to the large stresses placed on the windows during use under vacuum conditions.

[0198] The ceramic sintered bodies and related components disclosed herein provide improved plasma etch resistance and enhanced ability to be cleaned within semiconductor process chambers due to certain material properties and characteristics described below.

[0199] Total impurities below 40 ppm and 4.93 g / cm 3 The yttrium oxide sintered body is disclosed having a density of 0.1 to 1.0 μm, and the yttrium oxide sintered body has at least one surface containing at least one pore, and no pores have a diameter exceeding 5 μm. The yttrium oxide sintered body disclosed herein is provided by applying a specific manufacturing procedure and some specific process parameters in a spark plasma sintering (SPS) process, which will be described in more detail hereinafter.

[0200] The yttrium oxide sintered body produced by the method disclosed herein has a total impurity content of 40 ppm or less. In one embodiment, the yttrium oxide sintered body has a total impurity content of 35 ppm or less. In another embodiment, the yttrium oxide sintered body has a total impurity content of 30 ppm or less. In another embodiment, the yttrium oxide sintered body has a total impurity content of 25 ppm or less. In yet another embodiment, the yttrium oxide sintered body has a total impurity content of 20 ppm or less. In yet another embodiment, the yttrium oxide sintered body has a total impurity content of 15 ppm or less. In yet another embodiment, the yttrium oxide sintered body has a total impurity content of 10 ppm or less. In yet another embodiment, the yttrium oxide sintered body has a total impurity content of 5 ppm or less. In yet another embodiment, the yttrium oxide sintered body has a total impurity content of 0 ppm or less. As used herein, the term "impurities" refers to any element or compound other than yttrium oxide. Exemplary impurities include, but are not limited to, silicon, calcium, sodium, strontium, zirconia, magnesium, potassium, iron, phosphorus, boron, and low melting point elements (zinc, tin, indium, etc.). Thus, in some embodiments, the yttrium oxide sintered body is substantially free or free of at least one or all of these impurities.

[0201] The yttrium oxide sintered body disclosed in this specification has a density of 4.93 g / cm3, which is 98% of the theoretical density. 3DRLide, CRC Handbook of Chemistry and Physics 84 th According to the CRC Handbook, Edition, 2012, the theoretical density of yttrium oxide is 5.03 g / cm 3 The yttrium oxide sintered body produced according to the present disclosure has a theoretical density of 98% or more, preferably 98.5% or more, more preferably 99% or more, even more preferably 99.5% or more, and even more preferably 100% or more of the theoretical density of yttrium oxide described in the CRC Handbook. In other words, the yttrium oxide sintered body disclosed in the present specification has a theoretical density of 4.93 g / cm 3 In some embodiments, the yttrium oxide sintered body disclosed herein has a density of 4.96 g / cm or more (98% or more of the theoretical value). 3 In another embodiment, the yttrium oxide sintered body disclosed herein has a density of 4.98 g / cm or more (98.5% or more of the theoretical value). 3 In yet another embodiment, the yttrium oxide sintered body disclosed herein has a density of 5.01 g / cm or more (99% or more of the theoretical value). 3 The density is 99.5% or more of the theoretical value. The deviation of the density measurement is less than 0.002 g / cm 3The density measurements were performed using the Archimedes method known to those skilled in the art. As such, the yttrium oxide sintered body disclosed herein does not include a mixture of yttrium oxide with other oxides, such as zirconium oxide or aluminum oxide, but rather, the yttrium oxide sintered body disclosed herein consists essentially of yttrium oxide consistent with the potential impurity amounts described above, or consists of yttrium oxide consistent with the potential impurity amounts described above. Prior art solutions require combining yttrium oxide with other materials to increase the bending strength required for application in large-scale semiconductor processing systems. The combination of methods and materials disclosed herein provides high purity sintered bodies with greater than 98% theoretical density. Successful production of yttrium oxide sintered bodies across the longest dimension (greater than about 200-600 mm) can also be enabled by controlling the variation in density across at least one of the longest dimensions. Densities less than 98% can also result in greater density variation and reduced strength and handling. Thus, a density of at least 98% is desirable with less than 3% variation in density across at least one dimension, which may be the longest dimension. The solid yttrium oxide bodies of the present disclosure were tested using a four-point bend method according to ASTM C1161-13 and measured to have an average bend strength of 224 MPa with a standard deviation of 14 MPa.

[0202] Mechanical strength properties are known to improve with decreasing grain size. To evaluate grain size, linear intercept grain size measurements were performed according to the Heyn linear intercept method described in ASTM standard E112-2010 "Standard Test Method for Determining Average Grain Size". Grain size measurements were also performed using electron backscatter diffraction (EBSD) techniques known in the art. To meet the high bending strength and stiffness requirements for use in reactor chambers as large components of 100-600 mm, the ceramic sintered body may have fine grain sizes, such as grain sizes d50 of 0.1 μm to 25 μm, in some embodiments 1 μm to 20 μm, in other embodiments 0.5 μm to 20 μm, in other embodiments 0.5 μm to 15 μm, in yet other embodiments 0.5 μm to 10 μm, in other embodiments 0.75 μm to 5 μm, in other embodiments 2 μm or less, in other embodiments 1.5 μm or less, and in yet other embodiments 1.0 μm or less. These grain sizes may result in yttrium oxide sintered bodies having a four-point bending strength according to ASTM C1161-13 of 250 MPa or less, 300 MPa or less, preferably 350 MPa or less, preferably at least 400 MPa or less. Too large grain sizes, on the order of more than 25 μm in diameter, may result in sintered bodies with low bending strength values, which may make them unsuitable for use as components of etching chambers, particularly of large dimensions. For this reason, it is preferred that the yttrium oxide sintered bodies have an average grain size of preferably less than 13 μm (i.e., 0.01 μm to 13 μm).

[0203] The yttrium oxide sintered body disclosed herein has very small pores both on the surface and throughout the body. Preferably, the yttrium oxide sintered body is made only of yttrium oxide produced according to the process disclosed herein, and is therefore a monolithic body with pores throughout the body. In other words, the porous structure measured on the surface can represent the porosity level inside the bulk yttrium oxide body, as described in more detail below.

[0204] The yttrium oxide sintered body disclosed herein has at least one surface containing at least one pore, and has no pores with a diameter greater than 5 μm. In one embodiment, no pores with a diameter greater than 4.0 μm. In one embodiment, no pores with a diameter greater than 3 μm. In another embodiment, no pores with a diameter greater than 2 μm. In yet another embodiment, no pores with a diameter greater than 1.5 μm. In yet another embodiment, no pores with a diameter greater than 1 μm. The pore size can be measured, for example, by scanning electron microscopy (SEM).

[0205] The yttrium oxide body is further characterized by having a pore size distribution in which 95% or more of the total pores on at least one surface of the yttrium oxide body have a maximum pore size of 1.50 μm, preferably 97% or more of the total pores on at least one surface of the yttrium oxide body have a maximum pore size of 1.75 μm, more preferably 99% or more have a maximum pore size of 2.00 μm. The pore size distribution and overall porosity were determined by porosity measurements over a 5 mm x 5 mm area of ​​the polished sample using SEM images obtained from a Phenom XL scanning electron microscope. Representative SEM images were taken from the left, right, top, and bottom areas of the sample to gather information regarding the uniformity of the material over the entire sample area. Four images at 1000 times the image dimensions of 269 um x 269 um and four images at 5000 times the image dimensions of 53.7 um x 53.7 um were analyzed to determine the number of pores, percent porous area, and pore size over the entire image measurement area. The total image measurement area over which porosity was measured was 0.301 mm 2 The images were imported into ImageJ software for porosity analysis using contrast techniques. ImageJ, developed at the National Institutes of Health (NIH), is a Java-based public domain image processing and analysis program for the image processing of scientific multidimensional images.

[0206] Preferably, the at least one pore occupies less than 0.2%, more preferably less than 0.15%, and most preferably less than 0.1% of the surface area of ​​at least one surface of the yttrium oxide sintered body, as determined by the methods disclosed herein.

[0207] The yttrium oxide sintered body produced according to the present development preferably exhibits a step height of 0.2-0.98 μm for the CF4 / O2 etching process disclosed herein, 0.27-0.28 μm for the SF6 etching process disclosed herein, and 0.1-0.13 μm for the O2 etching process disclosed herein. The step height as a result of the etching process can be measured directly by using a Keyence 3D laser scanning confocal digital microscope model VK-X250X at 20x magnification. Selected areas of the etched and unetched areas of the sample are used to form separate reference planes. The difference in average height of the three measurements between these reference planes is considered the step height.

[0208] The yttrium oxide sintered body disclosed herein has a diameter of about 375,000 μm 3 Less than about 325,000 μm 3 less than about 275,000 μm 3 less than about 175,000 μm, more preferably 3The etching volume shows a calculated CF4 / O2 etch volume of less than 100 nm. The etching volume is measured in an etching process in which at least one surface area of ​​10 mm×5 mm is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power. The etching process has a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 1500 seconds, and the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds. The first and second steps are repeated consecutively until the exposure time to CF4 in the first step is 24 hours. The etching volume as a result of the etching process can be measured using a Keyence 3D laser scanning confocal digital microscope model VK-X250X at 20x magnification. The defined selected area of ​​the etched region of the sample is compared to the reference plane height, and the volume defined by the selected area between the reference plane height and the etched surface is the calculated etch volume, which thereby correlates to the volume of the yttrium oxide body removed during the etching process.

[0209] The yttrium oxide sintered body disclosed herein exhibits a calculated etch rate of less than about 1.0 nm / min, preferably less than about 0.90 nm / min, more preferably less than about 0.8 nm / min, more preferably less than about 0.7 nm / min, more preferably less than about 0.6 nm / min, more preferably less than about 0.5 nm / min, more preferably less than about 0.4 nm / min, more preferably less than about 0.3 nm / min. The etch rate is measured in an etching process in which a 10 mm×5 mm area of ​​at least one surface is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power. The etching process has a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 1500 seconds, and the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds. The first and second steps are then successively repeated until the exposure time to CF4 in the first step is 24 hours. The etch rate is calculated from the measured step height and etch time, thereby correlating with the reduction in thickness of the yttrium oxide body removed during the indicated etching process.

[0210] The yttrium oxide sintered body disclosed herein has a 250×10 -5 Less than 225×10 -5 Less than 200×10 -5 The surface is further characterized by having a developed area ratio Sdr in the unetched area of ​​less than 0.05 mm. Typically, the surface is polished prior to determining the developed area ratio in the unetched area.

[0211] The yttrium oxide sintered body disclosed herein has a sintering rate of 1500×10 according to ISO standard 25178-2-2012, section 4.3.2. -5 Less than 1300×10 -5 Less than 1000×10 -5 less than 800×10-5 Less than 600×10 -5 The surface area is further characterized by having a developed area ratio Sdr in the etched area of ​​less than 100 μm. The developed area ratio is determined by an etching process in which at least one surface area of ​​10 mm×5 mm is subjected to etching conditions of a pressure of 10 mTorr, an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts. The process includes a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 300 seconds, and the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, with a total etching time of 6 hours, and steps 1 and 2 are repeated consecutively.

[0212] The yttrium oxide sintered body disclosed herein has a 250×10 -5 Less than 225×10 -5 Less than 200×10 -5 and has a developed area ratio Sdr in the unetched area of ​​less than 1500 × 10 according to ISO standard 25178-2-2012, section 4.3.2. -5 Less than 1300×10 -5 Less than 1000×10 -5 less than 800×10 -5 Less than 600×10 -5The latter area ratio is further characterized by having a developed area ratio Sdr in the etched area of ​​less than 100 μm. This latter developed area ratio is determined by an etching process in which at least one surface area of ​​10 mm×5 mm is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power. The process includes a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 300 seconds, and the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, with a total etching time of 6 hours, and steps 1 and 2 being repeated consecutively.

[0213] The yttrium oxide sintered body disclosed herein is further characterized by having an arithmetic mean height Sa in the unetched area of ​​less than 10 nm, more preferably less than 8 nm, and most preferably less than 5 nm, according to ISO standard 25178-2-2012, section 4.1.7. Typically, the surface is polished before determining the arithmetic mean height of the unetched area.

[0214] The yttrium oxide sintered body disclosed herein is further characterized by exhibiting an arithmetic mean height Sa of less than 20 nm, more preferably less than 16 nm, and most preferably less than 12 nm according to ISO standard 25178-2-2012, section 4.1.7. The arithmetic mean height Sa is measured after an etching process in which at least one surface area of ​​10 mm x 5 mm is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power. The process includes a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 300 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and steps 1 and 2 are repeated consecutively for a total etching time of 6 hours.

[0215] In another embodiment, the yttrium oxide sintered body exhibits an arithmetic mean height Sa according to ISO standard 25178-2-2012, section 4.1.7 of less than 10 nm, more preferably less than 8 nm, most preferably less than 5 nm, and has an arithmetic mean height Sa according to ISO standard 25178-2-2012, section 4.1.7 of less than 20 nm, more preferably less than 16 nm, most preferably less than 12 nm. The latter arithmetic mean height Sa was achieved when a sample of yttrium oxide sintered body having an area of ​​10 mm x 5 mm on at least one surface was subjected to etching conditions of a pressure of 10 mTorr, an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 300 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and steps 1 and 2 being repeated consecutively for a total etching time of 6 hours.

[0216] The above-mentioned yttrium oxide sintered bodies show improved behavior in etching processes and can be easily used as materials for the manufacture of etching chamber components. The yttrium oxide materials used to date for etching chamber components, typically coatings made of yttrium oxide, suffer from the main problem of generating particles under harsh etching conditions, which contaminate the products being processed, as already mentioned above. The prior art's emphasis on the bulk (percentage) porosity properties of the yttrium oxide materials used to avoid such contamination and, consequently, the generation of particles under etching conditions. The challenge of sintering solid yttrium oxide to a sufficiently high density results in a material with low strength that is unsuitable for semiconductor process chambers requiring large components with dimensions on the order of more than 100 mm.

[0217] According to the above features, the resulting microstructure and surface of the yttrium oxide sintered body after etching is uniform, and the amount of material etched is small while maintaining a small development area, thus increasing the product life cycle and low particle generation characteristics in etching applications.

[0218] The yttrium oxide sintered body disclosed herein is the result of a specific manufacturing method. Whether the yttrium oxide sintered body exhibits the above characteristics can be easily determined by a person skilled in the art by applying the measurement methods disclosed herein, which at least in part correspond to standard procedures (ISO standards). Thus, a person skilled in the art can directly and reliably confirm whether the yttrium oxide material meets the claimed characteristics by tests or procedures appropriately specified in the present specification or known to a person skilled in the art. The implementation of these measurements does not require a person skilled in the art to carry out undue experimentation. The methods are disclosed in detail hereinafter.

[0219] Method for producing yttrium oxide sintered body The production of sintered yttrium oxide bodies can be accomplished by using pressure assisted sintering in combination with DC sintering and related techniques, which use direct current to heat a conductive die arrangement or tool set, which in turn heats the material to be sintered. This form of heating allows for the utilization of very high heating and cooling rates, which enhances densification mechanisms over grain growth driven diffusion mechanisms, thereby facilitating the production of very fine grained sintered yttrium oxide bodies, which transfer the inherent properties of the original powder to their nearly or completely dense products.

[0220] The above-mentioned properties of the corrosion-resistant yttrium oxide sintered body and components formed therefrom are achieved by adjusting, inter alia, the purity of the yttrium oxide powder, the surface area of ​​the yttrium oxide powder, the heating and cooling rates of the yttrium oxide powder and the sintered body, the pressure applied to the yttrium oxide powder, the temperature of the yttrium oxide powder, the sintering time of the powder, the temperature during the optional annealing step of the yttrium oxide sintered body or the component, and the time of the annealing step.

[0221] a. placing yttrium oxide powder within a volume defined by a sintering apparatus tool set and creating a vacuum condition or an inert environment within the volume; b. A process of applying a pressure of 10 MPa to 60 MPa to the yttrium oxide powder while heating it to a sintering temperature of 1200 to 1600 ° C., and sintering it to form an yttrium oxide sintered body; c. A step of lowering the temperature of the yttrium oxide sintered body; A method for producing an yttrium oxide sintered body comprising: The yttrium oxide powder of step a) is 10 m 2 / g or less, and the yttrium oxide sintered body has a total impurity content of 40 ppm or less and a surface area of ​​4.93 g / cm 3 or greater density and at least one surface comprising at least one pore, the pore having a diameter not exceeding 5 μm.

[0222] The following additional steps: d. Optionally, annealing the yttrium oxide sintered body by applying heat to raise the temperature of the yttrium oxide sintered body to an annealing temperature; e. Reducing the temperature of the annealed yttrium oxide sintered body to ambient temperature by removing the heat source applied to the yttrium oxide sintered body; and f. optional machining the annealed yttrium oxide sintered body to form a yttrium oxide sintered body component; is optional, and the component is selected from the group consisting of a dielectric or RF window, a focus ring, a nozzle or gas injector, a showerhead, a gas distribution plate, an etch chamber liner, a plasma source adapter, a gas inlet adapter, a diffuser, an electronic wafer chuck, a chuck, a puck, a mixing manifold, an ion suppressor element, a faceplate, an isolator, a spacer, and a guard ring.

[0223] The sintering equipment can be, for example, a pressure-assisted sintering equipment such as a spark plasma sintering (SPS) equipment. SPS is also called field-assisted sintering technology (FAST) or direct current sintering (DCS). DC and related techniques use direct current to heat an electrically conductive die configuration, which in turn heats the material to be sintered. This heating method allows for the utilization of very high heating and cooling rates, which favors densification mechanisms over grain growth driven diffusion mechanisms, and transfers the inherent properties of the original powders to their nearly or completely dense products.

[0224] Process step (a) - Placing yttrium oxide powder in a volume defined by the toolset of a spark plasma sintering machine and creating a vacuum condition or an inert environment within the volume. The disclosed method utilizes commercially available yttrium oxide powder or that prepared from chemical synthesis techniques without the need for sintering aids, cold pressing, shaping or machining of green bodies prior to sintering.

[0225] The yttrium oxide powder is filled, for example, in a die of an SPS sintering apparatus. The plasma sintering apparatus used in the method according to one embodiment of the present development may, for example, comprise a cylindrical or disk-shaped graphite die. The yttrium oxide powder is placed in the graphite die, and the die filled with the powder is placed between two graphite punches. Vacuum conditions known to those skilled in the art are set up within the powder between the punches enclosed in the die. Typical vacuum conditions include a vacuum of 10 -2 ~10 -3The vacuum is primarily used to remove air to protect the graphite from combustion and to remove most of the air from the powder.

[0226] The yttrium oxide starting material for carrying out the sintering process is a commercially available yttrium oxide powder with high purity. However, other yttrium oxide powders, such as those produced from chemical synthesis processes and related methods, can also be used. The purity of the yttrium oxide starting powder is preferably greater than 99.99%, more preferably greater than 99.998%, and most preferably greater than 99.999%. In some embodiments, the purity of the yttrium oxide starting powder is greater than 99.99999%. In other words, the total impurity content of the yttrium oxide powder can be less than 50 ppm, preferably less than 40 ppm, more preferably less than 30 ppm, more preferably less than 25 ppm, more preferably less than 20 ppm, more preferably less than 15 ppm, even more preferably less than 10 ppm, and even more preferably less than 6 ppm (including 0 ppm) in terms of total impurities. For optimal etching performance of the finished yttrium oxide sintered body / component, a high purity starting powder is desirable.

[0227] In contrast to other sintering techniques in the prior art, the yttrium oxide powder used in the process of the present disclosure does not contain sintering aids and polymer binders.

[0228] The average particle size of the yttrium oxide powder used as a starting material in the SPS process according to one embodiment of the present invention is usually 0.5-20 μm, preferably 1-15 μm, more preferably 2-10 μm.

[0229] The yttrium oxide powder is preferably 10 2 In some embodiments, the yttrium oxide powder has a surface area of ​​1.0 to 10.0 m 2 / g, preferably 1.5 to 8.0 m 2 / g, preferably 2 to 7, more preferably 2 to 5m 2 / g surface area.

[0230] Preferably, the yttrium oxide powder starting material is not ball milled prior to use in the methods of the present development, as ball milling is a potential source of contaminants / impurities.

[0231] In some embodiments, the yttrium oxide powder can be treated in a manner to remove undesirable moisture, organic matter, or agglomerates, which can include tumbling, jet milling, and / or sieving prior to use in step a) of the methods disclosed herein.

[0232] In embodiments, the yttrium oxide powder can be calcined prior to use in the methods of the present development. Exemplary calcination temperatures include temperatures of about 600° C. to about 1000° C. for 4 hours to 12 hours in an oxygen-containing environment. Before and / or after calcination, the yttrium oxide powder can be sieved and / or tumbled without the use of grinding media according to known methods.

[0233] Process step (b) - applying a pressure of 10 MPa to 60 MPa to the yttrium oxide powder while heating to a sintering temperature of 1200 to 1600°C to form a yttrium oxide sintered body, and process step (c) - reducing the temperature of the yttrium oxide sintered body by removing the heat source to the sintering device in which the yttrium oxide sintered body is contained.

[0234] After the yttrium oxide mass is placed into the die and most of the air is removed from the die / powder, pressure is applied to the yttrium oxide mass positioned between the graphite punches, the pressure is increased to a pressure of preferably 10 MPa to 60 MPa, preferably 10 MPa to 40 MPa, more preferably 15 MPa to 40 MPa, even more preferably 20 to 40 MPa, even more preferably 20 to 30 MPa.

[0235] Pressure is preferably applied axially to the material being fed into the die.

[0236] In a preferred embodiment, the yttrium oxide powder is heated directly by the punch and die of the SPS apparatus. The die can be constructed of a conductive material such as graphite to facilitate resistive / joule heating. SPS apparatus and procedures are disclosed, for example, in US2010 / 0156008A1, which is incorporated herein by reference.

[0237] The heating of the yttrium oxide powder fed to the die promotes a sintering temperature of about 1000-1700° C., preferably about 1200-1600° C., preferably about 1300-1550° C., preferably about 1350-1500° C., more preferably about 1400-1500° C. In one embodiment, sintering is accomplished for a time of 0-1440 minutes, in one embodiment, sintering is accomplished for a time of 0-720 minutes, in another embodiment, sintering is accomplished for a time of 0-360 minutes, in another embodiment, sintering is accomplished for a time of 0-240 minutes, in another embodiment, sintering is accomplished for a time of 0-120 minutes, in another embodiment, sintering is accomplished for a time of 0-60 minutes, in another embodiment, sintering is accomplished for a time of 0-30 minutes, in another embodiment, sintering is accomplished for a time of 0-20 minutes, in another embodiment, sintering is accomplished for a time of 0-10 minutes, and in another embodiment, sintering is accomplished for a time of 0-5 minutes.

[0238] The temperatures of the sintering apparatus according to the present disclosure are typically measured in the graphite die of the apparatus, and therefore it is preferred that the temperatures are measured as close as possible to the yttrium oxide to be sintered, so that the temperatures indicated are actually realized in the yttrium oxide.

[0239] The order of application of pressure and temperature in one embodiment may vary according to the present disclosure. This means that it is possible to apply the indicated pressure first and then heat to achieve the target temperature. Furthermore, in another embodiment, it is also possible to apply the indicated heat first to achieve the target temperature and then apply the indicated pressure. In a third embodiment according to the present disclosure, temperature and pressure can be applied simultaneously to the yttrium oxide to sinter and increase until the indicated value is reached.

[0240] Induction or radiation heating methods can also be used to heat the sintering apparatus and indirectly heat the yttrium oxide powder in the tool set.

[0241] In contrast to other sintering techniques, no sample preparation before sintering, i.e. by cold pressing or forming a green body before sintering, is necessary and the powder is directly filled into the mould, which allows for a high purity of the final yttrium oxide sintered body.

[0242] In further contrast to other sintering techniques, no sintering aids are required. In addition, high purity starting powders are desirable. The use of high purity starting materials, from 99.99% to over 99.9999%, without sintering aids, allows for the production of high purity yttrium oxide sintered bodies with improved etch resistance for use in semiconductor etching chambers.

[0243] In some embodiments, the sintering during the isothermal residence time can be performed for a period of 0 to 1440 minutes, in other embodiments, the sintering during the isothermal residence time can be performed for a period of 0 to 720 minutes, in other embodiments, the sintering during the isothermal residence time can be performed for a period of 0 to 360 minutes, in other embodiments, the sintering during the isothermal residence time can be performed for a period of 0 to 240 minutes, in other embodiments, the sintering during the isothermal residence time can be performed for a period of 0 to 120 minutes, in other embodiments, the sintering during the isothermal residence time can be performed for a period of 0 to 60 minutes, in other embodiments, the sintering during the isothermal residence time can be performed for a period of 0 to 30 minutes, in other embodiments, the sintering during the isothermal residence time can be performed for a period of 0 to 20 minutes, in other embodiments, the sintering during the isothermal residence time can be performed for a period of 0 to 10 minutes, and in other embodiments, the sintering during the isothermal residence time can be performed for a period of 0 to 5 minutes.

[0244] In one embodiment of the present invention, the SPS treatment process comprises a pre-sintering step which is carried out at a specific heating ramp of 0.1°C / min-100°C / min, 0.25°C / min-50°C / min, preferably 0.5°C / min-50°C / min, preferably 0.75°C / min-50°C / min, preferably 1°C / min-50°C / min, more preferably 2-25°C / min, more preferably 3-20°C / min, preferably 4-15°C / min, preferably 5-10°C / min until a specific pre-sintering time is reached.

[0245] In a further embodiment of the present invention, the SPS treatment step comprises a pre-sintering step carried out with a specific pressure ramp of 0.10 MPa / min - 30 MPa / min, 0.2 - 25, preferably 0.25 - 20, 0.25 MPa / min - 15 MPa / min, preferably 0.5 - 10 MPa / min, preferably 1 - 10 MPa / min until a specific pre-sintering time is reached.

[0246] In another embodiment of the invention, the SPS process includes a pre-sintering step in which the specific heating ramp described above and the specific pressure ramp described above are used.

[0247] In process step (c), the sintered yttrium oxide can be passively cooled by removal of the heat source, and natural convection occurs until a temperature is reached that can facilitate the optional annealing process. In a further embodiment, the yttrium oxide sintered body can be cooled under convection of an inert gas, for example argon or nitrogen at 1 bar. Other gas pressures above or below 1 bar can also be used. To start the cooling step, the power applied to the SPS device can be removed. The pressure applied to the sintered sample is removed at the end of the SPS process before (natural) cooling takes place.

[0248] During sintering, a volume reduction typically occurs, such that the yttrium oxide sintered body may contain a volume that is approximately one-third the volume of the starting yttrium oxide powder when placed in the toolset of the sintering apparatus.

[0249] Process step (d) - in an optional step, annealing the yttrium oxide sintered body by applying heat to raise the temperature of the yttrium oxide sintered body to an annealing temperature, and process step (e) reducing the temperature of the annealed yttrium oxide sintered body to ambient temperature by removing the heat source applied to the yttrium oxide sintered body. In optional step (d), the yttrium oxide sintered body obtained in step c) is subjected to an annealing process. The annealing can be performed in a furnace outside the sintering device or inside the sintering device itself without removing the yttrium oxide sintered body from the sintering device. For example, in one embodiment, the sintered yttrium oxide can be removed from the sintering device after cooling according to process step (c), and the annealing step can be performed in another device, such as a furnace. In another embodiment, for the purposes of the annealing treatment according to the present disclosure, the yttrium oxide sintered in step (b) can then be annealed in sintering device without the need to remove it from the sintering device between the sintering step (b) and the optional annealing step (d).

[0250] The annealing improves the chemical and physical properties of the yttrium oxide sintered body, and the annealing process can be carried out in a conventional manner used for annealing glasses, ceramics, and metals, and the degree of improvement can be selected by selecting the annealing temperature and the duration of the annealing process.

[0251] The optional annealing step (d) can be carried out at temperatures between 1200 and 1800° C., preferably between 1250 and 1700° C., more preferably between 1300 and 1650° C. At such temperatures, residual carbon can be removed and oxygen vacancies in the crystal structure can be corrected back to stoichiometric proportions.

[0252] The step of annealing the sintered yttrium oxide can be completed in 5 minutes to 24 hours, preferably 20 minutes to 20 hours, and more preferably 60 minutes to 16 hours.

[0253] The optional annealing step (d) is preferably carried out in an oxidizing atmosphere in air.

[0254] After the optional process step (d) of annealing the sintered yttrium oxide has been performed, the temperature of the annealed yttrium oxide sintered body is reduced to ambient temperature as per process step (c) above. The sintered and annealed yttrium oxide body is dense and typically has an average grain size of 0.25 μm to 25 μm, preferably 0.5 to 20 μm, preferably 0.75 to 15 μm, preferably 1 to 10 μm, more preferably 1 to 5 μm.

[0255] The SPS process described above according to one embodiment is suitable for use in the manufacture of large yttrium oxide sintered bodies. The method disclosed herein provides rapid powder solidification and densification, maintains small (on the order of less than 13 um) d50 grain size in the sintered body transferred from the starting powder material, and achieves high uniform density of more than 98% of theoretical with minimal (<3%) density variation across the longest dimension. This combination of fine grain size, uniformity, and high density provides high strength large dimension yttrium oxide sintered bodies suitable for machining, handling, and use as components of semiconductor process chambers. For example, in one embodiment, the yttrium oxide sintered body can be formed into a disk shape having dimensions ranging from 40 mm to 600 mm in size over a thickness range of 40 mm to 100 mm. In another embodiment, the yttrium oxide sintered body can be formed into a disk shape having a diameter ranging from 100 mm to 600 mm in diameter. In another embodiment, the yttrium oxide sintered body can be formed having dimensions ranging from 100 mm to 406 mm in diameter. In another embodiment, the yttrium oxide sintered body has a size of 200 mm to 600 mm, preferably 300 to 600 mm, preferably 350 to 600 mm, preferably 400 to 600 mm, more preferably 450 to 600 mm, more preferably 500 to 600 mm, more preferably 550 to 600 mm, each of which relates to at least one dimension which may be the longest dimension of the sintered body.

[0256] Finally, the sintered (or sintered and annealed) yttrium oxide body can then be optionally machined into final components for use in plasma etch chambers, such as, for example, dielectric or RF windows, focus rings, nozzles or gas injectors, showerheads, gas distribution plates, etch chamber liners, plasma source adapters, gas inlet adapters, diffusers, electronic wafer chucks, chucks, pucks, mixing manifolds, ion suppressor elements, faceplates, isolators, spacers, and guard rings. Machining of the sintered (or sintered and annealed) yttrium oxide body to form sintered components can be performed according to methods known to those skilled in the art.

[0257] The methods disclosed herein provide improved control over maximum pore size, high density, density variation, high purity, improved mechanical strength, and thereby handleability of yttrium oxide sintered bodies / components, particularly for objects with dimensions greater than 200-600 mm in the maximum dimension, for example.

[0258] Thus, in one embodiment disclosed herein, the total impurities content is 40 ppm or less and the total impurities content is 4.93 g / cm 3 The present invention discloses an yttrium oxide sintered body having a density of 0.1 to 1.0 μm, and having at least one surface containing at least one pore, the pore having a diameter not exceeding 5 μm, the yttrium oxide sintered body being produced by the following method. a. placing yttrium oxide powder within a volume defined by a toolset of a spark plasma sintering apparatus and creating a vacuum condition or an inert environment within the volume; b. A process of applying a pressure of 10 MPa to 60 MPa to the yttrium oxide powder while heating it to a sintering temperature of 1200 to 1600 ° C., and sintering it to form an yttrium oxide sintered body; c. A step of lowering the temperature of the yttrium oxide sintered body; wherein the yttrium oxide powder in step a) is 10 ml 2 / g or less, and the yttrium oxide sintered body has a total impurity content of 40 ppm or less and a surface area of ​​4.93 g / cm 3 and at least one surface containing at least one pore, wherein no pores exceed 5 μm in diameter.

[0259] The yttrium oxide sintered body thus produced (including the annealed yttrium oxide sintered body) can be used in an apparatus for plasma etching. Most integrated circuit (IC) manufacturing processes typically include a number of manufacturing steps that can sequentially form, shape, or modify various layers. One way to form a layer can be to deposit a layer and then etch it. Typically, etching can include forming an etch mask over the underlying layer. The etch mask can have a specific pattern that can mask certain parts of the underlying layer while exposing other parts. Etching can then remove the parts of the underlying layer exposed by the etch mask. In this way, the pattern of the etch mask can be introduced into the underlying layer.

[0260] Plasma etching is currently used in semiconductor material processing for use in the manufacture of electronic devices. When used in electronic devices, small features can be etched into the surface of the semiconductor material to make it more efficient or to enhance certain properties. For example, plasma etching can be used to form deep trenches in silicon surfaces for use in microelectromechanical systems. This application suggests that plasma etching may also have a large role to play in the manufacture of microelectronics. Similarly, research is currently being conducted into how the process can be tuned to the nanometer scale.

[0261] Plasma etching is usually performed in a plasma etch chamber, which is commonly used to etch one or more layers formed on a semiconductor substrate, which is typically supported on a substrate support within the chamber.

[0262] During plasma etching, a plasma is formed above the surface of the substrate by supplying radio frequency (RF) electromagnetic radiation to a low pressure gas (or gas mixture). By adjusting the potential of the substrate, charged species in the plasma can be directed to impinge on the surface of the substrate, thereby removing material (e.g., atoms) therefrom.

[0263] Plasma etching can be made more effective by using gases that are chemically reactive with the material being etched. So-called "reactive ion etching" combines the energetic bombardment effect of a plasma with the chemical etching effect of reactive gases.

[0264] The sintered yttrium oxide according to one embodiment of the present disclosure can be used to manufacture plasma chamber components. Such components can be produced with high density and purity by sintering using the SPS process described above, which may have advantages such as long life under aggressive etching conditions. Yttrium oxide sintered bodies have many advantages in the context of plasma processing, such as resistance to particle generation, improved plasma etching resistance, and increased component life. In addition, cleaning of yttrium oxide parts can be made easier, as aggressive cleaning methods, such as highly corrosive or reactive chemicals, may be used.

[0265] Examples of chamber components that can be formed from the yttrium oxide sintered bodies disclosed herein include electrostatic chucks (ESCs), rings (e.g., process kit rings or single rings), chamber wall liners, bases, gas distribution plates, showerheads, liners, liner kits, shields, plasma screens, flow balancers, cooling bases, chamber viewports, chamber lids, and the like.

[0266] In one embodiment, a process chamber according to an embodiment of the present disclosure includes a chamber body and a showerhead that enclose an internal volume. Alternatively, the showerhead may be replaced by a lid and a nozzle, which may be fabricated from yttrium oxide as described above, either as a complete material or as a coating. The chamber body may be fabricated from aluminum, stainless steel, or other suitable materials. The chamber body typically includes a sidewall, a focus or edge ring that surrounds the wafer, and a bottom. One or more of the showerhead (or lid and / or nozzle), sidewall, and / or bottom include sintered yttrium oxide according to an embodiment of the present disclosure.

[0267] The features and advantages are more fully illustrated by the exemplary embodiments described hereinafter. EXAMPLES

[0268] The following yttrium oxide samples, H1 / 66-H4 / 152, were produced according to embodiments of the present invention and compared with yttrium oxide samples CM1 / 107, CM2 / 108, and 118, which were not produced according to the present disclosure.

[0269] H1 / 66: 2.89m 2An 80mm yttrium oxide compact was produced from powder with a surface area of ​​1.2g / g, a d50 particle size of 5.4um, <10ppm TREO (total rare earth oxides) and 48ppm total impurities for a powder purity of 99.9952%. The compact was formed at 30MPa for 60 minutes at a sintering temperature of 1500°C. Annealing was performed in air with a temperature ramp of 5°C / min to 1450°C for 1 hour, then at 1400°C for 8 hours. The yttrium oxide compact had a mass of 4.948g / cm 3 and maximum pore size of 1.1 μm. The d10, d50, and d90 particle sizes were measured to be 0.5, 0.8, and 1.4 um, respectively.

[0270] H2 / 65: 6.84m 2 Yttrium oxide samples of 40 mm were formed at 30 MPa at a sintering temperature of 1550°C for 10 minutes from the powder having a surface area of ​​0.1 μm / g. Annealing was performed in a furnace at a temperature of 1300°C for 4 hours in air. The total purity of the starting yttrium oxide powder was 99.999%, which corresponds to 10 ppm. The median grain size was measured to be 5.82 μm. The yttrium oxide sintered body had a total impurity content of 11 ppm. The purity of the starting powder was maintained in the yttrium oxide sintered body, suggesting that little or no contaminants were introduced during processing. The d10, d50, and d90 grain sizes were measured to be 4.0, 13.0, and 27.1 um, respectively, with an average grain size of 14 um.

[0271] H3 / 79: 3.33m 2A 40 mm yttrium oxide body was formed from powder having a surface area of ​​1 / g and a median particle size (d50) of 5.17 μm. The total impurities of the starting powder were 2-4 ppm. Sintering of the yttrium oxide body was carried out at 30 MPa pressure for 10 minutes using a sintering temperature of 1500°C. The temperature was ramped at 50°C / min while simultaneously applying a pressure of 5 MPa / min. Annealing was carried out by ramping the temperature to 1300°C at 5°C / min and holding in air for 4 hours. The yttrium oxide body had a total impurity level of 9-10 ppm. This indicates that the introduction of contaminants as a result of the process was minimal. The maximum pore size was measured to be 0.6 um and the density was measured to be 5.03 g / cc. The d10, d50, and d90 grain sizes were measured to be 0.8, 1.4, and 2.4 um, respectively. An average grain size of 1.47 um was also measured.

[0272] H4 / 152: 6.95m 2 A 100 mm yttrium oxide sintered body was formed from powder with a surface area of ​​0.01 g / g, 99.999% purity of TREO (<10 ppm), and an average total impurity of 18 ppm. The median grain size (d50) was 4.65 μm. Sintering was performed at 1400 °C for 30 minutes at 30 MPa. Subsequent annealing was performed in air at 1400 °C for 8 hours. The mass of the yttrium oxide sintered body was 5.024 g / cm. 3 After the two-step CF4 / O2 etching process disclosed herein, the average step height was 0.98 um, the average etch rate was 0.68 nm / min, and the average pore size was 340,000 um. 3 An etch volume of 1000 μm was obtained. Before and after the two-step CF4 / O2 etching process disclosed herein, an arithmetic mean height Sa of 10 and 14 nm, respectively, was measured. After the oxygen etching process disclosed herein, an average step height of 0.1 μm, an average etch rate of 0.07 nm / min, and an average step height of 30,000 μm were measured. 3 After the SF6 etching process disclosed herein, an average step height of 0.28 um, an average etch rate of 0.19 nm / min, and an etch depth of 90,000 um were obtained. 3 The etching amount was obtained.

[0273] Single-step, CF4 etching procedure To evaluate the etching performance, polished ceramic samples with dimensions of 6 mm × 6 mm × 2 mm were mounted on a c-plane sapphire wafer using a silicone-based heat sink compound. Areas of each part were blocked from exposure to the etching process by gluing a 5 mm × 5 mm square piece of sapphire ceramic to the sample surface.

[0274] The dry etching process was performed using an industry standard Plasma-Therm Versaline DESC PDC Deep Silicon Etch. The etch was completed for a total duration of 24 hours with 4 hour etch segments. The process was performed at a pressure of 10 millitorr with a CF4 flow rate of 90 standard cubic centimeters per minute (sccm), an oxygen flow rate of 30 sccm, and an argon flow rate of 20 sccm. The bias was 600 volts and the ICP power was 2000 watts. This etch recipe has a silicon etch rate of 512 nm / min. This etch recipe etches fused silica (quartz glass) at a rate of 72 nm / min. The etch conditions used herein to evaluate sample performance were selected to subject the materials of the present disclosure to extreme etch conditions in order to identify performance.

[0275] After the etching procedure was completed, the surface roughness was measured.

[0276] Single step, CF4 etch volume procedure: In one embodiment, the yttrium oxide sintered body has a diameter of about 12000 μm. 3 Less than about 9000 μm, preferably 3 less than about 7000 μm, more preferably 3The etching amounts are characterized by an etching amount of less than 1000 nm. This etching amount is achieved when a reference etching process is performed in which a sample with dimensions of 6 mm x 6 mm x 2 mm is subjected to etching conditions of 10 millitorr with a CF4 flow rate of 90 standard cubic centimeters per minute (sccm), an oxygen flow rate of 30 standard cubic centimeters per minute (sccm), and an argon flow rate of 20 standard cubic centimeters per minute (sccm), and an etching condition of 24 hours at a bias of 600 volts and an ICP power of 2000 watts. Each etching process is described in more detail in the experimental section below. The etching amount is then related to the volume of the yttrium oxide body removed during the indicated etching process.

[0277] Single-step, CF4 etch rate procedure: In some embodiments, the yttrium oxide body is characterized by exhibiting an etch rate of less than about 0.08 nm / min, preferably less than about 0.06 nm / min, more preferably less than about 0.05 nm / min. This etch rate is achieved when a single step CF4 etch process is performed as a reference process, where a sample with dimensions of 6 mm x 6 mm x 2 mm is subjected to etch conditions of 10 mTorr with a CF4 flow rate of 90 standard cubic centimeters per minute (sccm), an oxygen flow rate of 30 standard cubic centimeters per minute (sccm), and an argon flow rate of 20 standard cubic centimeters per minute (sccm), and an ICP power of 600 volts and 2000 watts for 24 hours. As a result, the etch rate is related to the reduction in the thickness of the yttrium oxide body removed during the indicated etch process.

[0278] Single-step, CF4Sdr procedure (without and with etch) In some embodiments, the yttrium oxide sintered body has a molecular weight of 100×10 -5 Less than 75×10 -5 Less than 50×10 -5and has a developed area ratio in the unetched area of ​​less than 600 × 10 according to ISO standard 25178-2-2012, section 4.3.2. -5 Less than 500×10 -5 Less than 400×10 -5 less than 300×10 -5 Less than 200×10 -5 The latter expansion area ratio is achieved when a sample of a yttrium oxide body with dimensions of 6 mm x 6 mm x 2 mm is subjected to conditions of 10 millitorr pressure with a CF4 flow rate of 90 standard cubic centimeters per minute (sccm), an oxygen flow rate of 30 standard cubic centimeters per minute (sccm), and an argon flow rate of 20 standard cubic centimeters per minute (sccm), and a CF4 etch time of 24 hours at a bias of 600 volts and an ICP power of 2000 watts. Each etching process is described in more detail below.

[0279] Single process, CF4Sa (without etching, with etching) In some embodiments, the yttrium oxide sintered body is further characterized by having an arithmetic mean height Sa of less than 30 nm, more preferably less than 28 nm, and most preferably less than 25 nm, according to ISO standard 25178-2-2012, section 4.1.7, and an arithmetic mean height Sa of less than 40 nm, more preferably less than 35 nm, and most preferably less than 30 nm, according to ISO standard 25178-2-2012, section 4.1.7. The latter arithmetic mean height Sa is achieved when a sample of the yttrium oxide body with dimensions of 6 mm x 6 mm x 2 mm is subjected to etching conditions of 10 mTorr with a CF4 flow rate of 90 standard cubic centimeters per minute (sccm), an oxygen flow rate of 30 standard cubic centimeters per minute (sccm), and an argon flow rate of 20 standard cubic centimeters per minute (sccm), and an ICP power of 600 volts and 2000 watts for 24 hours. Each etching process is described in more detail below.

[0280] Surface roughness measurement Surface roughness measurements were performed using a Keyence 3D laser scanning confocal digital microscope model VK-X250X under ambient conditions in a Class 1 cleanroom. The microscope is placed on a TMC tabletop CSP benchtop passive isolator with a natural frequency of 2.8 Hz.

[0281] This non-contact system uses a laser beam of light and an optical sensor to analyze a surface by reflected light intensity. The microscope acquires 1,024 data points in the x-direction and 786 data points in the y-direction for a total of 786,432 data points. Once a given scan is completed, the objective lens moves a set pitch in the z-direction and intensity is compared between scans to determine focus. ISO 25178 Surface Characterization (Area Roughness Measurement) is a collection of international standards related to the analysis of surface roughness to which this microscope adheres.

[0282] To capture detailed images of the samples, the surfaces of the samples were laser scanned at 10x magnification using a confocal microscope. Line roughness was obtained on the profiles of the seven divided blocks. Lambda chi (λ), which represents the measurement sampling length, was adjusted to restrict the line reading to measurements from the central five blocks out of seven, according to ISO specification 4288: Geometrical Property Specification (GPS) - Surface Quality: Profile Curve Method - Rules and Procedures for the Evaluation of Surface Quality.

[0283] Areas within the etched and masked regions of the sample were selected for measurement, which were most representative of a typical sample surface, and were used to calculate Sa and Sdr.

[0284] Surface roughness Sa and Sdr are parameters well known in the field of infrastructure technology and are described, for example, in sections 4.1.7 (surface roughness Sa) and 4.3.2 (surface roughness Sdr) of ISO standard 25178-2-2012.

[0285] Measuring step height The step height as a result of the etching process was measured directly by using a Keyence 3D laser scanning confocal digital microscope model VK-X250X at 20x magnification. Selected areas of the etched and unetched areas of the sample were used to form separate reference planes. The average height difference over three measurements between these reference planes can be considered as the step height.

[0286] Etch rate calculation The average etch rate in nanometers / hour can be calculated from the average step height by dividing the step height by the total etch time to arrive at an etch rate in nanometers / minute.

[0287] Volume measurement Etch volumes were calculated from measurements at 50x on a Keyence 3D laser scanning confocal digital microscope model VK-X250X. A 7x7 image template is formed from which a 7x1 region is selected for measurement. A reference plane is first defined in a representative area of ​​the sample that was masked and therefore not etched. An area within the masked region is selected to define the reference plane. A software tilt correction is completed over that area to account for sample thickness and mounting variations. A total area of ​​600um x 200um is then selected in the etched region of the image at the maximum distance from the masked surface. The height of the etched surface compared to the reference plane formed on the masked surface is measured and the volume of material removed by etching relative to the reference plane is calculated over the entire selected region.

[0288] Difference between Ra and Sa measurements: Sa is the arithmetic mean height of the surface and is described in ISO 25178: Geometric Property Specifications (GPS) - Surface Texture:, which is a collection of International Organization for Standardization international standards related to the analysis of 3D areal surface texture. It is based on non-contact laser microscopy.

[0289] Ra is the arithmetic mean roughness of a 2D profile according to ISO 4287:1997 Geometrical Characteristics Specification (GPS)-Surface Texture: Profile Method. It is based on a mechanical stylus contacting the surface to produce a linear profile.

[0290] Sa represents the height difference across the 3D measurement surface, while Ra represents the height difference across the 2D linear profile scan.

[0291] Ra is limited by the geometry of the stylus tip, which can result in loss of fine feature detail and distorted peaks and valleys, which is problematic when measuring fine sub-micron features and is a limitation in the use of Ra values ​​for comparison with Sa values.

[0292] Additional samples were prepared according to the method of the present invention and are summarized in the table below, where applicable, they are compared to a commercial quartz (TSC 03) and comparative yttrium oxide samples (107, 108, and 118).

[0293] As an example, sample 188-1 was prepared as follows: 2 Yttrium oxide powder with a molecular weight of 1.01 g / g and a total impurity of 13 ppm corresponding to a powder purity of 99.9987% was used to form a 100 mm yttrium oxide sintered body. Pressure preapplication was performed in a multi-step process where a pressure of 20 MPa was preapplication under vacuum. Then, 5 MPa was applied while heating from room temperature to 600 °C at a rate of 10 °C / min. The pressure was increased to 30 MPa between 600 °C and the sintering temperature at a rate of 10 °C / min. Sintering was performed at a temperature of 1400 °C and a pressure of 30 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was turned off and the body was allowed to cool naturally. Annealing was performed at a temperature of 1400 °C for 8 hours in an oxygen-containing environment. The density was 5.002 g / cm 3 It was.

[0294] In another example, sample 116 was manufactured as follows: 2Yttrium oxide samples of 40 mm were formed at 30 MPa at a sintering temperature of 1550°C for 10 minutes from powders with a surface area of ​​0.1 μm / g. Annealing was performed in a furnace at a temperature of 1400°C-1450°C for 9 hours in air. The total purity of the starting yttrium oxide powder was 99.999%, which corresponds to 10 ppm. The median particle size was measured to be 5.82 μm. The yttrium oxide sintered body had a total impurity content of 11 ppm. The purity of the starting powder was maintained in the yttrium oxide sintered body. This suggests that little or no contaminants were introduced during processing. The d10, d50, and d90 particle sizes were measured to be 0.7, 6.7, and 25.4 um, respectively.

[0295] In another example, sample 224 was prepared as follows: 2 Yttrium oxide powder with an average of 8 ppm total impurities at 0.015 g / g, corresponding to a powder purity of 99.9992%, was used to form a 100 mm yttrium oxide sintered body. A pressure of 20 MPa was pre-applied for approximately 5 minutes, followed by a vacuum of 50 mTorr. The pressure was then reduced to 5 MPa and heating to 600°C was performed at a rate of 10°C / min. Heat and pressure were applied simultaneously to reach a pressure of 20 MPa and heating to 1400°C at a rate of 10°C / min. Sintering was performed at a temperature of 1400°C and a pressure of 20 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was turned off and the body was allowed to cool naturally. The d10, d50, and d90 grain sizes of the yttrium oxide sintered body were 0.4, 0.7, and 1.2 um, respectively.

[0296] In another example, sample 189-1 was prepared as follows: 2A 100 mm yttrium oxide sintered body was formed using yttrium oxide powder with a total impurity of 24.8 ppm, corresponding to a powder purity of 99.9975. The pre-application of pressure was performed in a multi-step process in which a pressure of 20 MPa was pre-application under vacuum. Then, 5 MPa was applied while heating from room temperature to 600°C at a rate of 10°C / min. The pressure was increased to 30 MPa between 600°C and the sintering temperature at a rate of 10°C / min. Sintering was performed at a temperature of 1400°C and a pressure of 30 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was turned off and the body was allowed to cool naturally. Annealing was performed at a temperature of 1400°C for 8 hours in an oxygen-containing environment. The yttrium oxide sintered body had 36 ppm impurities and a purity of 99.996%. The density of the annealed yttrium oxide sintered body was 5.006 g / cm 3 After the two-step CF4 / O2 etching process disclosed herein, the average step height was 0.82 um, the average etch rate was 0.57 nm / min, and the maximum pore size was 0.7 microns. 3 The etching amount was obtained.

[0297] In another example, sample 045 was prepared as follows: 2 A 100 mm yttrium oxide sintered body was formed using yttrium oxide powder with a total impurity of 26 ppm, corresponding to a powder purity of 99.9974%, and a pre-application of pressure of 20 MPa under vacuum in a multi-step process as disclosed herein. Then, heating was performed from room temperature to 600°C at a rate of 10°C / min while simultaneously applying 5 MPa. The pressure was increased to 30 MPa between 600°C and the sintering temperature at a rate of 10°C / min. Sintering was performed at a temperature of 1400°C and a pressure of 30 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was turned off and the body was allowed to cool naturally. The average density using Archimedes' method was 5.021 g / cm 3 The annealing was performed at a temperature of 1400 °C for 8 hours in an oxygen-containing environment. The average density after annealing was measured to be 5.010 g / cm using the Archimedes method. 3 It was measured to be.

[0298] In another example, sample 200-1 was prepared as follows: 2 A 150 mm yttrium oxide sintered body was formed using yttrium oxide powder with a total impurity of 9.5 ppm, corresponding to a powder purity of 99.9991%, at 20 MPa. Pressure was pre-applied for about 5 minutes. The pressure was then reduced to 5 MPa and heating was performed to 600 °C at a rate of 25 °C / min. Simultaneous application of heat and pressure was performed at a heating rate of 25 °C / min and a pressurization rate of 5 MPa / min up to 1000 °C and 20 MPa. Heating was performed from 1000 °C to the sintering temperature at a rate of 10 °C / min. Sintering was performed at a temperature of 1400 °C and a pressure of 20 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was turned off and the body was allowed to cool naturally. Annealing was performed at a temperature of 1400 °C for 8 hours in an oxygen-containing environment. The density of the annealed yttrium oxide sintered body was 4.945 g / cm 3 with a maximum pore size of 1.4 microns. After the two-step CF4 / O2 etching process disclosed herein, an average step height of 0.2 um, an average etch rate of 0.14 nm / min, and an etch volume of 60,000 um3 were obtained. After the oxygen etching process disclosed herein, an average step height of 0.1 μm, an average etch rate of 0.07 nm / min, and an etch volume of 30,000 um3 were obtained. 3 After the SF6 etching process disclosed herein, an average step height of 0.27 μm, an average etch rate of 0.19 nm / min, and an etch depth of 80,000 μm were obtained. 3 The etching amount was obtained.

[0299] In another example, sample 212-1 was prepared as follows: 2A 100 mm yttrium oxide sintered body was formed using yttrium oxide powder with a total impurity of 8.1 ppm / g, corresponding to a powder purity of 99.9992%. Pressure was pre-applied at 20 MPa for about 5 minutes and a vacuum of 50 mTorr was applied. The pressure was then reduced to 5 MPa and heated to 600°C at a rate of 50°C / min. Simultaneous application of heat and pressure was performed at a pressure rate of 10 MPa / min and a heating rate of 25°C / min up to 30 MPa and 1450°C. Sintering was performed at a temperature of 1450°C and a pressure of 30 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was turned off and the body was allowed to cool naturally. Annealing was performed at a temperature of 1400°C for 8 hours in an oxygen-containing environment. The density of the annealed yttrium oxide sintered body was 5.022 g / cm 3 The maximum pore size was 1.0 microns. The yttrium oxide sintered body had a total average impurity of 6 ppm, corresponding to a purity of 99.9994%. After the two-step CF4 / O2 etching process disclosed herein, the average step height was 1.1 um, the average etch rate was 0.77 nm / min, and the maximum pore size was 358,000 um. 3 The etching amount was obtained.

[0300] In another example, sample 314 was prepared as follows: 2 Yttrium oxide powder with a total impurity of 24.8 ppm, corresponding to a powder purity of 99.9975%, was used to form yttrium oxide sintered bodies with a longest dimension of 406 mm. Pressure was pre-applied at 5 MPa and the temperature was increased from room temperature to 800 °C at 10 °C / min. Simultaneous application of heat and pressure was performed from 800 °C to 1000 °C with a heating rate of 10 °C / min and a pressurizing rate of 20 MPa / min. Pressure was maintained at 20 MPa from 1000 °C to the sintering temperature and the heating rate was 10 °C / min. Sintering was performed at a temperature of 1450 °C and a pressure of 20 MPa for a sintering time of 60 minutes. After the sintering time, heating and pressurizing were stopped and natural cooling was performed. The yttrium oxide sintered bodies were annealed at a temperature of 1400 °C in an oxygen-containing environment for 8 hours using heating and cooling rates of 0.8 °C / min. The average density of the annealed yttrium oxide sintered bodies was 4.935 g / cm 3and the density range across the longest dimension is 4.898-4.970 g / cm 3 It was.

[0301] In another example, sample 457 was prepared as follows: 2 Yttrium oxide powder having 17 ppm total impurities, corresponding to a powder purity of 99.9983%, was used to form a sintered yttrium oxide body having a longest dimension of 406 mm. Calcination of the powder was performed at 600 °C for 8 hours, 5-6 mm. 2 Sintering was performed at a surface area of ​​100 / g. Pressure was pre-applied at 5 MPa and the temperature was ramped from room temperature to 600°C at 10°C / min. Simultaneous application of heat and pressure was performed from 600°C to 1000°C with a heating rate of 5°C / min and a pressure ramp to 30 MPa. Pressure was maintained at 30 MPa from 1000°C to the sintering temperature and the heating rate was 5°C / min. Sintering was performed at a temperature of 1475°C and a pressure of 30 MPa for a sintering time of 60 minutes. After the sintering time, the pressure was removed. Cooling was performed using forced convection at 50% blower power for approximately 4 hours. Cooling by varying the blower power level from approximately 25% to 100% allows forced convection cooling rates of 2.5°C / min to 5°C / min. Sintering was performed at a temperature of 1475°C and a pressure of 30 MPa for 60 minutes. The yttrium oxide sintered body was annealed at a temperature of 1400°C for 4 hours in an oxygen-containing environment using a heating rate of 0.8°C / min and a cooling rate of 2°C / min. The average density of the annealed and sintered yttrium oxide was 4.985 g / cm 3 and the density range across the longest dimension is 4.980-4.989 g / cm 3 The maximum pore diameter was measured to be 1.4 um, with a Sa value of 18 nm and a pore size of 1178×10 after the disclosed CF4 / O2 etching process. -5 An Sdr value of 0.65um was measured for this sample using the line intercept method.

[0302] In another example, sample 353 was prepared as follows: 2Yttrium oxide powder having an average of 11 ppm total impurities per gram, corresponding to a powder purity of 99.9989%, was used to form a sintered yttrium oxide body having a longest dimension of 406 mm. Calcination of the powder was performed at 1000 °C for 24 hours at 1.5-2.5 mm. 2 The sintering was carried out at a surface area of ​​100 / g. Pressure was applied at 5 MPa beforehand, and the temperature was increased from room temperature to 800°C at 10°C / min. Simultaneous application of heat and pressure was carried out from 800°C to 1000°C with a heating rate of 10°C / min and a pressure increase to 30 MPa. The pressure was maintained at 30 MPa from 1000°C to the sintering temperature, and the heating rate was 10°C / min. Sintering was carried out at a temperature of 1475°C and a pressure of 30 MPa for a sintering time of 60 minutes. After the sintering time was over, the heating and pressure were stopped and natural cooling was carried out. The yttrium oxide sintered body was annealed at 1400°C for 0 minutes (no isothermal annealing time) in an oxygen-containing environment with a heating rate of 0.8°C / min and a passive cooling rate of 0.8°C / min. The density of the annealed yttrium oxide sintered body was 4.981 g / cm 3 It was.

[0303] In another example, sample 414 was prepared as follows: 2 Yttrium oxide powder having an average of 11 ppm total impurities per gram, corresponding to a powder purity of 99.9989%, was used to form a sintered yttrium oxide body having a longest dimension of 406 mm. Calcination of the powder was performed at 500 °C for 48 hours, with a temperature of 6.5-7.5 mm. 2 The sintering was carried out at a surface area of ​​1 / g. Pressure was pre-applied at 5 MPa and the temperature was increased from room temperature to 800 °C at 10 °C / min. Simultaneous application of heat and pressure was carried out from 800 °C to 1000 °C with a heating rate of 10 °C / min and pressurization up to 30 MPa. Pressure was maintained at 30 MPa from 1000 °C to the sintering temperature and the heating rate was 10 °C / min. Sintering was carried out at a temperature of 1400 °C and a pressure of 30 MPa for a sintering time of 60 minutes. After the sintering time, heating and pressurization were stopped and natural / passive cooling was carried out. The density of the annealed yttrium oxide sintered body was 4.985 g / cm 3 It was.

[0304] In yet another example, sample 476 was prepared as follows: 2 Yttrium oxide powder with 0.01 g / g and 5-6 ppm total impurities corresponding to a powder purity of 99.9995% was used to form yttrium oxide sintered bodies with a longest dimension of 406 mm. The powder was tumbled for 24 hours and then sintered without the use of grinding media. Pressure was pre-applied at 5 MPa and the temperature was ramped from room temperature to 600 °C at 10 °C / min. Simultaneous application of heat and pressure was performed from 600 °C to 1000 °C with a heating rate of 5 °C / min and a pressure ramp to 30 MPa. Pressure was maintained at 30 MPa from 1000 °C to the sintering temperature and the heating rate was 5 °C / min. Sintering was performed at a temperature of 1475 °C and a pressure of 30 MPa with a sintering time of 60 minutes. After the sintering time, the pressure was removed. Cooling was performed using forced convection with a blower power of 50%. Cooling using varying blower power levels allows forced convection cooling rates of 2.5 °C / min to 5 °C / min. The yttrium oxide sintered bodies were annealed at a temperature of 1400°C for 4 hours in an oxygen-containing environment using a heating rate of 1°C / min and a cooling rate of 2°C / min. The average density of the annealed yttrium oxide sintered bodies was 4.953 g / cm 3 and the density range across the longest dimension is 4.891 to 5.014 g / cm 3 It was.

[0305] In a series of examples, samples 084 and 084-1, 085 and 085-1, 086 and 086-1, 087 and 087-1, 095, and 096 were prepared as follows. 100 mm yttrium oxide sintered bodies corresponding to samples 084 and 084-1, 085 and 085-1, 086 and 086-1, 087 and 087-1, 095, and 096 were cut into 6.5 to 7.5 mm pieces. 2 The powder was prepared from a powder having a surface area of ​​5–6.5 m / g and an average of 11 ppm total impurities giving a powder purity of 99.9989%. The powder was calcined at 800 °C for 8 h before sintering to give a surface area of ​​5–6.5 m. 2 / g. Samples 084-1, 085-1, 086-1, 087-1, 095, and 096 were annealed at 1400°C at a ramp rate of 5°C / min for 8 hours in an oxygen environment. The density and processing conditions are as disclosed in the corresponding density and sintering / annealing tables herein.

[0306] Comparative Sample 107: The purity of the comparative yttrium oxide body was determined by ICPMS to be 99.9958% with 42 ppm contaminants. Porosity measurements were performed as disclosed herein to determine a maximum pore size of 38 um. Particle size measurements were performed to determine a large average particle size of 27 um. Using the Archimedes method, the material was determined to have a mass of 4.987 g / cm 3 The material was measured to have an average density of 0.038 with a standard deviation of 0.038. Although the exact sintering conditions are unknown, it is speculated that high sintering temperatures in excess of 1600° C. were used for extended periods of time, such as several days, to sinter the yttrium oxide powder to form this material. These parameters contribute to the large grain size measured. The sample exhibited a significant proportion of porous regions, with large pore sizes, poor etching performance, and extensive surface roughness compared to the sintered yttrium oxide of the present disclosure.

[0307] Comparative Sample 108: The material properties of the comparative yttrium oxide body were analyzed. The purity of the comparative yttrium oxide body was determined to be 99.8356% by ICPMS and had 1644 ppm of contaminants, including 1291 ppm of zirconia as a sintering aid to promote densification. Porosity measurements were performed as disclosed herein and a maximum pore size of 12 um was measured. Using the Archimedes method, the material was determined to have an average density of 4.997 g / cc with a standard deviation of 0.011. While the exact sintering conditions are unknown, it is speculated that zirconia was added to the powder to sinter the yttrium oxide to form this material to promote densification, which may have reduced the etching performance. The sample exhibited a significant proportion of porous regions and had a large pore size and surface roughness compared to the sintered yttrium oxide of the present disclosure.

[0308] Comparative Sample 118: The purity of the comparative yttrium oxide body was determined by ICPMS to be 99.9967% with 33 ppm contaminants. Porosity measurements were performed as disclosed herein and a maximum pore size of 7 um was measured. The material was determined to have an average density of 5.003 g / cc using the Archimedes method. The sample exhibited a significant proportion of porous regions, with larger pore sizes and poorer etching performance compared to the sintered yttrium oxide of the present disclosure.

[0309] Tables 1-4 summarize the processing conditions and resulting densities of samples produced according to the methods of the present disclosure. [Table 1-1] [Table 1-2] [Table 1-3] [Table 2] [Table 3] [Table 4] [Table 5]

[0310] Tables 6 and 7 summarize the purities measured for the starting powder and sintered yttrium oxide samples produced according to the methods disclosed herein. [Table 6-1] [Table 6-2]

[0311] Table 7 shows the maintenance of purity during the process disclosed herein from powder to yttrium oxide sintered body. [Table 7]

[0312] Tables 8-10 show the etching results on quartz (TSC 03), commercial yttrium oxide parts (107, 108, 118), and sintered yttrium oxide samples produced according to the present disclosure for different process gases along with their processing conditions. The CF4 / O2 etch was performed in a two-step process. Step 1 was performed at 10 mtorr pressure, 90 sccm CF4 flow rate, 30 sccm O2 flow rate, 20 sccm argon flow rate, 600 V bias voltage, 2000 W power for 1500 seconds. Step 2 was performed at 10 mtorr pressure, 0 sccm CF4 flow rate, 100 sccm O2 flow rate, 20 sccm argon flow rate, 600 V bias voltage, 2000 W power for 300 seconds. The first and second steps were repeated consecutively until the CF4 exposure time in the first step was 24 hours. The O2 etch conditions are as follows: pressure of 25 mtorr, CF4 / SF6 flow rate of 0 sccm, O2 flow rate of 100 sccm, Ar flow rate of 20 sccm, bias voltage of 600 V, power of 2000 W for a total of 6 hours. The SF6 etch conditions are as follows: pressure of 25 mtorr, SF6 flow rate of 100 sccm, O2 flow rate of 0 sccm, Ar flow rate of 50 sccm, bias voltage of 300 V, power of 2000 W for a total of 24 hours. The results show the excellent corrosion resistance of the yttrium oxide sintered body produced according to the present disclosure.

[0313] The yttrium oxide sintered body produced according to the present development preferably exhibits a step height of 0.2-0.98 μm for the CF4 / O2 etching process disclosed herein, 0.27-0.44 μm for the SF6 etching process disclosed herein, and 0.1-0.13 μm for the O2 etching process disclosed herein.

[0314] The yttrium oxide sintered body produced according to the present development preferably has a melting point of 0.6×10 for the disclosed CF4 / O2 etching process. 5 ~3.4×10 5 μm 3 etch amount for the SF6 etching process disclosed herein is 0.8×10 5 ~1.4×10 5 μm 3 etch amount of 0.28-0.39 μm for the O2 etching process disclosed herein 3 The etching amount is shown.

[0315] The yttrium oxide sintered body produced according to the present development preferably exhibits an etch rate of 0.14-0.68 nm / min for the disclosed CF4 / O2 etching process, 0.19-0.310 nm / min for the disclosed SF6 etching process, and 0.07-0.09 nm / min for the disclosed O2 etching process. [Table 8] [Table 9] [Table 10] [Table 11]

[0316] With reference to the figures, selected results are summarized as follows:

[0317] 3 shows the single step CF etch amount of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure. The sintered yttrium oxide samples according to the present disclosure are much more etch resistant than the prior art.

[0318] 4 shows the average CF4+O2 etch amount for prior art TSC 03 (quartz) and sintered yttrium oxide samples 118 and 107 compared to various sintered yttrium oxide samples produced according to embodiments of the present disclosure. The sintered yttrium oxide samples according to the present disclosure are much more etch resistant than the prior art.

[0319] 5 shows the CF4+O2 average step height for prior art TSC 03 (quartz) and sintered yttrium oxide samples 118 and 107 compared to various sintered yttrium oxide samples produced according to embodiments of the present disclosure. The sintered yttrium oxide samples according to the present disclosure are much more etch resistant than the prior art.

[0320] 6 shows the CF4+O2 average etch rates of prior art TSC 03 (quartz) and sintered yttrium oxide samples 118 and 107 compared to various samples made according to embodiments of the present disclosure. The sintered yttrium oxide samples according to the present disclosure are much more etch resistant than the prior art.

[0321] 7 shows SEM micrographs at 50x of the surfaces of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 before and after the single step CF4 etching process. Significant etching is observed.

[0322] 8 shows SEM micrographs at 1000X of the surfaces of sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 made in accordance with the present disclosure before and after a single step CF4 etching process. The samples made in accordance with the present disclosure are resistant to etching.

[0323] 9 shows SEM micrographs at 1000x of the surfaces of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 before and after the single step CF4 etching process. Significant etching is observed.

[0324] 10 shows SEM micrographs at 1000X of the surfaces of sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 made in accordance with the present disclosure before and after a single step CF4 etching process. The samples made in accordance with the present disclosure are resistant to etching.

[0325] 11 shows SEM micrographs at 5000x of the surfaces of prior art sintered yttrium oxide samples 107 and 118 before and after the CF4+O2 etching process. Significant etching is observed.

[0326] 12 shows SEM micrographs at 5000X of the surfaces of sintered yttrium oxide samples 152 and 189-1 made in accordance with the present disclosure before and after a CF4+O2 etching process. The samples made in accordance with the present disclosure are resistant to etching.

[0327] 13 shows SEM micrographs at 1000X and 5000X of the edge and center of a sintered yttrium oxide sample 457 made in accordance with the present disclosure. It shows uniform density across the surface and little to no porosity. The sample made in accordance with the present disclosure is dense and resistant to etching.

[0328] FIG. 14 shows that the yttrium oxide bodies (H1 / 66 to H4 / 152) according to one embodiment of the present disclosure have no pores with a pore size greater than 2.00 μm.

[0329] 15 is a graph showing the developed area ratio Sdr at 50x optical magnification for prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure before and after a single step CF4 etching process. Samples made according to the present disclosure are resistant to etching.

[0330] 16 is a graph showing the arithmetic mean height Sa (nm) measured at 50x optical magnification of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure before and after a single step CF4 etching process. Figures 15 and 16 show that the yttrium oxide materials according to embodiments of the present disclosure (H1 / 66-H3 / 79) have much lower developed area ratios Sdr and arithmetic mean heights Sa compared to the comparative materials (CM1 / 107 and CM2 / 108).

[0331] 17 is a graph showing the developed area ratio Sdr of various sintered yttrium oxide samples from the examples before and after the CF4+O2 etching process. Samples made according to the present disclosure are resistant to etching.

[0332] 18 is a graph showing the arithmetic mean height Sa (nm) of various samples from the examples before and after the CF4+O2 etching process. Samples manufactured according to the present disclosure are resistant to etching.

[0333] 19 is a graph showing the percent areal porosity of various sintered yttrium oxide samples from the Examples compared to the prior art sintered yttrium oxide samples, with the yttrium oxide materials according to one embodiment of the invention (H1 / 66-H4 / 152) having a much smaller percent pore area compared to the comparative materials (CM1 / 107 and CM2 / 108).

[0334] 20 is a graph showing cumulative area % versus pore size (pore size distribution) for various samples from the Examples compared to prior art sintered yttrium oxide samples. In particular, for pore sizes less than 1 μm, the cumulative percent area that is porous is 96-100% for yttrium oxide materials H1 / 66-H3 / 79 according to an embodiment of the invention, while the cumulative percent area is about 10% or less for comparative materials CM1 / 107-CM3 and H5 / 62.

[0335] Figure 21 is a graph showing the porosity distribution versus log pore size for various samples from the examples compared to prior art sintered yttrium oxide samples. Prior art materials 107, 108, and 118 show larger pore sizes on the order of 7 um or greater and a higher percentage of the surface and therefore volume of the yttrium oxide sintered body that contains porosity.

[0336] FIG. 22 is a graph showing sintering pressure and temperature conditions required for obtaining an yttrium oxide sintered body having a density 98% or more higher than the theoretical density of yttrium oxide.

[0337] As disclosed herein, a number of embodiments have been described. However, it will be understood that various modifications can be made without departing from the spirit and scope of the embodiments disclosed herein. Accordingly, other embodiments are within the scope of the following claims.

Claims

1. Total impurities of 40 ppm or less and 4.93 g / cm 3 A yttrium oxide sintered body having a density of 1000 or more, having at least one surface containing at least one pore; The yttrium oxide sintered body has no pores having a diameter exceeding 5 μm.

2. A 10 mm by 5 mm area of ​​the at least one surface is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power to remove 375,000 μm 3 indicates an etching amount of less than The process includes a first step and a second step, the first step being 90 sccm CF for 1500 seconds. 4 and an oxygen flow rate of 30 sccm for 300 seconds, and the second step is a CF4 flow rate of 0 sccm for 300 seconds. 4 flow rate of 100 sccm and an oxygen flow rate of 100 sccm; The first step and the second step are 4 This is repeated successively until the exposure time is 24 hours. The yttrium oxide sintered body according to claim 1.

3. 2. The yttrium oxide sintered body according to claim 1, having a pore size distribution with a maximum pore size of 1.50 μm for 95% or more of all pores on said at least one surface.

4. a 10 mm x 5 mm area of ​​said at least one surface exhibits an etch rate of less than 1.0 nm / min in a process subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power; The process includes a first step and a second step, the first step being 90 sccm CF for 1500 seconds. 4 and an oxygen flow rate of 30 sccm for 300 seconds, and the second step is a CF4 flow rate of 0 sccm for 300 seconds. 4flow rate of 100 sccm and an oxygen flow rate of 100 sccm; The first step and the second step are 4 This is repeated successively until the exposure time is 24 hours. The yttrium oxide sintered body according to claim 1.

5. In the unetched area, 250×10 as determined by ISO standard 25178-2-2012, section 4.3.2 -5 The yttrium oxide sintered body according to claim 4, which has a development area Sdr of less than 100 nm.

6. A 6 mm x 6 mm x 2 mm area of ​​the at least one surface is treated with 90 sccm CF 4 In a process subjected to etching conditions of 10 mTorr with an oxygen flow rate of 30 sccm, an argon flow rate of 20 sccm, and an etching bias of 600 volts and an ICP power of 2000 watts for 24 hours, the etched area was 200×10 Å as determined by ISO standard 25178-2-2012, section 4.3.

2. -5 The yttrium oxide sintered body according to claim 1, wherein the yttrium oxide sintered body exhibits a developed area of ​​less than 100 mm.

7. a 10 mm by 5 mm area of ​​the at least one surface exhibits an arithmetic mean height Sa of less than 30 nm as determined by ISO standard 25178-2-2012, section 4.1.7, in a process subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volts bias, and 2000 watts ICP power; The process includes a first step and a second step, the first step being 90 sccm of CF for 300 seconds. 4 and an oxygen flow rate of 30 sccm for 300 seconds, and the second step is a CF4 flow rate of 0 sccm for 300 seconds. 4 flow rate of 100 sccm and an oxygen flow rate of 100 sccm; 2. The yttrium oxide sintered body according to claim 1, wherein the first step and the second step are continuously repeated for a total etching time of 6 hours.

8. The yttrium oxide sintered body according to any one of claims 1 to 7, wherein the at least one surface has an area in which less than 0.15% is occupied by pores.

9. Science fiction 6 The yttrium oxide sintered body according to claim 7, which exhibits a step change of 0.27 to 0.28 μm after an etching process.

10. The yttrium oxide sintered body according to any one of claims 1 to 9, having a grain size d50 of 0.1 µm to 25 µm.

11. The yttrium oxide sintered body according to any one of claims 1 to 10, having at least one dimension between 100 mm and 600 mm, preferably between 350 mm and 600 mm.

12. A yttrium oxide sintered body according to any one of the preceding claims, wherein the density does not vary by more than 3% along at least one dimension.

13. a. placing yttrium oxide powder within a volume defined by a toolset of a sintering apparatus; b. creating a vacuum condition or an inert environment within said volume; c. applying a pressure of 10 MPa to 60 MPa to the yttrium oxide powder while heating it to a sintering temperature of 1200 to 1600°C to form a yttrium oxide sintered body; d. A step of lowering the temperature of the yttrium oxide sintered body; A method for producing an yttrium oxide sintered body comprising: The yttrium oxide powder of step a) is 10 m 2 / g or less, The yttrium oxide sintered body has a total impurity content of 40 ppm or less and a total impurity content of 4.93 g / cm 3 and at least one surface comprising at least one pore; The process, wherein the porous membrane has no pores having a diameter greater than 5 μm.

14. e. Annealing the yttrium oxide sintered body by applying heat to raise the temperature of the yttrium oxide sintered body to an annealing temperature; f. Reducing the temperature of the annealed yttrium oxide sintered body to ambient temperature by removing the heat source applied to the yttrium oxide sintered body; g. Optionally, machining the annealed yttrium oxide sintered body to form a yttrium oxide sintered body component; Further comprising:

14. The method of claim 13, wherein the component is selected from the group consisting of a dielectric or RF window, a focus ring, a nozzle or gas injector, a showerhead, a gas distribution plate, an etch chamber liner, a plasma source adapter, a gas inlet adapter, a diffuser, an electronic wafer chuck, a chuck, a puck, a mixing manifold, an ion suppressor element, a faceplate, an isolator, a spacer, and a guard ring.

15. 15. The method according to claim 13 or 14, wherein the yttrium oxide powder is calcined prior to step a).

16. The method according to any one of claims 13 to 15, wherein the purity of the yttrium oxide powder is greater than 99.998%.

17. The method according to any one of claims 13 to 16, wherein the yttrium oxide sintered body has a purity of 99.99 to 99.999%.

18. The method according to any one of claims 13 to 17, wherein the sintering is carried out for a time period between 1 minute and 120 minutes.

19. In a process where a 10 mm x 5 mm area of ​​the at least one surface is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power, the yttrium oxide body is etched to a thickness of 375,000 μm. 3 indicates an etching amount of less than The process includes a first step and a second step, the first step being 90 sccm CF for 1500 seconds. 4 and an oxygen flow rate of 30 sccm for 300 seconds, and the second step is a CF4 flow rate of 0 sccm for 300 seconds. 4 flow rate of 100 sccm and an oxygen flow rate of 100 sccm; The first step and the second step are 4 This is repeated successively until the exposure time is 24 hours. The method according to any one of claims 13 to 18.

20. The method according to any one of claims 13 to 19, wherein the yttrium oxide sintered body has a pore size distribution with a maximum pore size of 1.50 μm for 95% or more of all pores on the at least one surface.

21. In a process where a 10 mm x 5 mm area of ​​the at least one surface is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power, the yttrium oxide body exhibits an etch rate of less than 1.0 nm / min; The process includes a first step and a second step, the first step being 90 sccm CF for 1500 seconds. 4 and an oxygen flow rate of 30 sccm for 300 seconds, and the second step is a CF4 flow rate of 0 sccm for 300 seconds. 4 flow rate of 100 sccm and an oxygen flow rate of 100 sccm; The first step and the second step are 4 This is repeated successively until the exposure time is 24 hours. The method according to any one of claims 13 to 20.

22. In the unetched areas, the yttrium oxide sintered body has a thickness of 250×10 as determined by ISO standard 25178-2-2012, section 4.3.

2. -5The method according to any one of claims 13 to 21, exhibiting a development area Sdr of less than

23. A 6 mm x 6 mm x 2 mm area of ​​the at least one surface is treated with 90 sccm CF 4 In a process subjected to etching conditions of 10 mTorr with an oxygen flow rate of 30 sccm, an argon flow rate of 20 sccm, and a bias of 600 volts and an ICP power of 2000 watts, the etched area of ​​the yttrium oxide sintered body is 200×10 as determined by ISO standard 25178-2-2012, section 4.3.

2. -5 The method of any one of claims 13 to 22, wherein the method exhibits a deployment area of ​​less than

24. A process in which a 10 mm by 5 mm area of ​​the at least one surface is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow, 600 volt bias, and 2000 watts ICP power, the process having a first step and a second step, the first step being 300 seconds with 90 sccm CF 4 and an oxygen flow rate of 30 sccm for 300 seconds, and the second step is a CF4 flow rate of 0 sccm for 300 seconds. 4 24. The method according to any one of claims 13 to 23, wherein in the process having an oxygen flow rate of 100 sccm and an oxygen flow rate of 100 sccm, a total etching time of 6 hours, and in which steps 1 and 2 are repeated successively, the yttrium oxide sintered body exhibits an arithmetic mean height Sa of less than 30 nm as determined by ISO standard 25178-2-2012, section 4.1.

7.

25. A method according to any one of claims 13 to 24, wherein the at least one surface has an area of ​​which less than 0.15% is occupied by pores.

26. The method according to any one of claims 13 to 25, wherein the yttrium oxide sintered body has a grain size d50 of 0.1 μm to 25 μm.

27. The method according to any one of claims 13 to 26, wherein the yttrium oxide sintered body has at least one dimension between 100 mm and 600 mm.

28. A method according to any one of claims 13 to 27, wherein the density does not vary by more than 3% along at least one dimension.

29. The yttrium oxide sintered body is SF 6 The method of any one of claims 13 to 28, exhibiting a step change of 0.27 to 0.28 μm after the etching process.

Citation Information

Patent Citations

  • Electrode built-in ceramics and its manufacturing method

    JP2002047067A

  • Y2o3-based sintered compact

    JP2008260651A

  • Yttria insulator ring for use inside plasma chambers

    JP2008511175A

  • Yttria sintered compact and member for plasma processing device

    JP2009263187A