Fastness improver composition and method for producing dyed polyester fiber products
A polyester copolymer-based fastness improver composition enhances the fastness of dyed polyester textiles by incorporating specific dicarboxylic acid and diol units, addressing the fastness issues in one-bath two-step methods and achieving performance comparable to two-bath methods while reducing water consumption.
Patent Information
- Application Number
- JP2023571981
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-06
- Filing Date
- 2023-11-15
- Publication Date
- 2024-10-02
- Estimated Expiration
- 2043-11-15
AI Technical Summary
Polyester dyed textile products produced by conventional methods suffer from inadequate fastness, particularly when the soaping treatment is performed in a one-bath two-step method, leading to a reduction in fastness compared to the two-bath two-step method.
A fastness improver composition comprising a polyester copolymer with specific dicarboxylic acid and diol units, including units derived from dicarboxylic acids with sulfonic acid groups and tricarboxylic acids, is used in the soaping treatment, either in the same bath as dyeing or in a separate bath, along with a method that includes hot water washing and water washing processes.
The composition and method significantly improve the fastness of polyester dyed textile products, achieving results comparable to or better than the two-bath two-step method while reducing water usage and processing costs.
Smart Images

Figure 0007560682000001 
Figure 0007560682000002 
Figure 0007560682000003
Abstract
Description
[Technical field]
[0001] The present application discloses a fastness improver composition and a method for producing a dyed polyester textile product. [Background technology]
[0002] Generally, polyester fibers are dyed by a method called a two-bath, two-stage method, in which a dyeing process is carried out at about 120 to 135° C. using a dyeing solution containing a dye, the dyeing solution is then drained, and a soaping process is carried out in a bath separate from the dyeing solution using a soaping solution containing a soaping agent at about 60 to 100° C. For example, Patent Document 1 discloses a two-bath, two-stage method in which polyester fibers are dyed, removed, and then soaped at 85° C. using a reducing washing bath to which a liquid reducing agent consisting of a reducing sugar such as glucose has been added. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2020 / 196902 Summary of the Invention [Problem to be solved by the invention]
[0004] There is room for improvement in fastness of the polyester dyed fiber products produced by the method disclosed in Patent Document 1. A new technique for improving the fastness of polyester dyed fiber products is needed. [Means for solving the problem]
[0005] The present application discloses the following aspects as means for solving the above problems. (Aspect 1) A fastness improver composition comprising a polyester copolymer, The polyester copolymer contains dicarboxylic acid units and diol units, the dicarboxylic acid unit contains at least one of a unit derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, and a unit derived from a tricarboxylic acid, in an amount of 5 mol % to 30 mol %; The diol unit is derived from a diol having a molecular weight of 48 or more and less than 900, and The intramolecular content ratio of the dicarboxylic acid unit in the polyester copolymer is 50% by mass or more and 75% by mass or less. Fastness improver composition. (Aspect 2) A method for producing a polyester dyed fiber product, comprising the steps of: Dyeing polyester fibers; The polyester-based fiber after the dyeing treatment is subjected to a soaping treatment in the same bath as the dyeing solution or in a separate bath; and subjecting the polyester-based fiber after the soaping treatment to one or both of a hot water washing treatment and a water washing treatment; Including, One or both of the soaping liquid used in the soaping treatment and the cleaning liquid used in the cleaning treatment contain a polyester copolymer; The polyester copolymer contains dicarboxylic acid units and diol units, the dicarboxylic acid unit contains at least one of a unit derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, and a unit derived from a tricarboxylic acid, in an amount of 5 mol % to 30 mol %; The diol unit is derived from a diol having a molecular weight of 48 or more and less than 900, and The intramolecular content ratio of the dicarboxylic acid unit in the polyester copolymer is 50% by mass or more and 75% by mass or less. Manufacturing method. (Aspect 3) The method for producing aspect 2, The polyester-based fiber after the dyeing treatment is subjected to the soaping treatment in the same bath as the dyeing solution, The dyeing solution used in the dyeing treatment contains the polyester copolymer, and At least a part of the polyester copolymer contained in the dyeing solution is used as at least a part of the polyester copolymer contained in the soaping solution. Manufacturing method. (Aspect 4) The method for producing aspect 2 or 3, The method includes performing the soaping treatment on the polyester fiber after the dyeing treatment in the same bath as the dyeing solution, and The soaping solution used in the soaping treatment is prepared by adding at least the polyester copolymer to the dyeing solution after the dyeing treatment. Manufacturing method. (Aspect 5) In the production method according to any one of aspects 2 to 4, The amount of the polyester copolymer contained in the soaping liquid is 0.005 g / L or more and 5.0 g / L or less. Manufacturing method. (Aspect 6) In any one of the production methods of the second to fifth aspects, The amount of the polyester copolymer contained in the cleaning solution is 0.005 g / L or more and 5.0 g / L or less. Manufacturing method. Effect of the Invention
[0006] According to the composition and production method of the present disclosure, for example, by using a soaping solution containing a specified polyester copolymer in a soaping treatment, it is possible to improve the fastness of a polyester-based dyed fiber product to a level equal to or greater than that achieved by performing a conventional dyeing treatment and soaping treatment.
[0007] In recent years, dyeing and soaping treatments have been increasingly performed in the same bath (one bath, two-stage method) to reduce processing costs by streamlining the process, as well as to take environmental measures such as saving water and reducing CO2. However, in the case of the one-bath, two-stage method, the drop in fastness is particularly noticeable when using conventional soaping agents compared to the two-bath, two-stage method. According to the composition and production method of the present disclosure, good fastness can be obtained even when soaping is performed in one bath, two stages.
[0008] Furthermore, according to the composition and production method of the present disclosure, for example, by using a cleaning solution containing a specific polyester copolymer in a cleaning treatment (hot water washing treatment and / or water washing treatment) after a soaping treatment, it is possible to improve the fastness of a polyester-based dyed fiber product. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] 1. Manufacturing method for polyester dyed textile products Hereinafter, a method for producing a polyester-based dyed fiber product according to one embodiment will be described. The method for producing a polyester-based dyed fiber product according to one embodiment includes dyeing a polyester-based fiber, soaping the polyester-based fiber after the dyeing treatment in the same bath (1 bath) as the dyeing solution or in a different bath (2 baths), and washing the polyester-based fiber after the soaping treatment with one or both of hot water washing and water washing. Here, one or both of the soaping solution used in the soaping treatment and the washing solution used in the washing treatment contain a polyester copolymer (polymer A). The polyester copolymer contains a dicarboxylic acid unit and a diol unit. The dicarboxylic acid unit contains at least one of a unit derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, and a unit derived from a tricarboxylic acid, in an amount of 5 mol% to 30 mol%. The diol unit is derived from a diol having a molecular weight of 48 to less than 900. The intramolecular content ratio of the dicarboxylic acid unit in the polyester copolymer is 50 mass% to 75 mass%.
[0010] 1.1 Dyeing process The manufacturing method of the present disclosure includes performing a dyeing treatment on the polyester-based fiber. A dye solution is used for the dyeing treatment.
[0011] 1.1.1 Polyester fibres The polyester fiber to be dyed may be any fiber containing polyester. The polyester fiber may be, for example, one or both of polyester fibers made of at least one homopolymer selected from ethylene terephthalate, propylene terephthalate, trimethylene terephthalate, and butylene terephthalate, or a copolymer thereof; and at least one composite fiber selected from blends, interwovens, and interknits of polyester fibers and other synthetic fibers or natural fibers. The form of the polyester fiber may be, for example, at least one form selected from yarn, knitted fabric, woven fabric, and nonwoven fabric. It is preferable that the polyester fiber is scoured.
[0012] 1.1.2 Components of staining solution The components of the dyeing solution include water, an organic solvent, and a surfactant. The dyeing solution may also contain an acid for adjusting the pH, a chelating agent, and the like. As described below, the dyeing solution may also contain a predetermined polyester copolymer (polymer A). Alternatively, as described below, a predetermined polyester copolymer (polymer A) may be added to the dyeing solution after the dyeing process.
[0013] The organic solvent may be, for example, an alcohol having a carbon number of 1 to 10. Specifically, it may be at least one selected from methanol, ethanol, isopropyl alcohol, ethylene glycol monobutyl ether, and diethylene glycol monobutyl ether.
[0014] The surfactant is not particularly limited and may be a known surfactant, for example, at least one selected from an anionic surfactant, a nonionic surfactant, and a cationic surfactant.
[0015] The anionic surfactant is, for example, Sulfate esters, phosphate esters, or salts thereof of alkylene oxide adducts of aliphatic alcohols (aliphatic alcohols having 1 to 22 carbon atoms); A sulfate ester or a phosphate ester of a polyalkylene glycol obtained from an alkylene oxide having 2 to 4 carbon atoms, or a salt thereof; Sulfate esters, phosphate esters, or salts thereof of alkylene oxide adducts of mono- or polystyrenated phenols; Sulfate esters, phosphate esters, or salts thereof of alkylene oxide adducts of mono- or polystyrenated alkyl (alkyl group having 1 to 22 carbon atoms)phenols; Alkyl (alkyl group having 8 to 22 carbon atoms) benzenesulfonic acid or its salt; Alkyl (alkyl group having 8 to 22 carbon atoms) sulfonic acid or a salt thereof; α-olefin sulfonic acid having 8 to 22 carbon atoms or a salt thereof; and α-sulfofatty acid alkyl ester (α-sulfofatty acid having 8 to 22 carbon atoms, alkyl group having 1 to 12 carbon atoms) or a salt thereof; The salt may be, for example, at least one selected from an alkali metal salt, an alkaline earth metal salt, an ammonium salt, and an alkanolamine salt.
[0016] Nonionic surfactants include, for example, Alkylene oxide adducts of aliphatic alcohols (fatty alcohols having 1 to 22 carbon atoms) or their fatty acid esters (fatty acid having 8 to 24 carbon atoms); Polyalkylene glycol obtained from an alkylene oxide having 2 to 4 carbon atoms, or its fatty acid ester (fatty acid having 8 to 24 carbon atoms); Alkylene oxide adducts of mono- or polystyrenated phenols, or their fatty acid esters (fatty acid having 8 to 24 carbon atoms); and Fatty acid (fatty acid having 8 to 24 carbon atoms) esters of alkylene oxide adducts of mono- or polystyrenated alkyl (alkyl group having 1 to 22 carbon atoms) phenols; It may be at least one selected from the following.
[0017] The cationic surfactant may be at least one quaternary ammonium surfactant selected from, for example, benzalkonium chloride; a reaction product of a trialkylamine having one or two long-chain alkyl groups and a quaternizing agent; a reaction product of an alkylene oxide adduct of a mono- or dialkylamine and a quaternizing agent; and an alkylpyridinium salt. The carbon number of the long-chain alkyl group of the trialkylamine may be, for example, 6 to 24, and the carbon number of the remaining alkyl group of the trialkylamine may be, for example, 1 to 5. The carbon number of the alkyl group of the mono- or dialkylamine may be, for example, 6 to 24. The alkylene oxide may be, for example, an alkylene oxide having 2 to 4 carbon atoms, and the number of moles added thereto may be, for example, 2 to 50. The quaternizing agent may be, for example, at least one selected from an alkyl halide having an alkyl group having 1 to 5 carbon atoms, and a dialkyl sulfate having an alkyl group having 1 to 5 carbon atoms. The carbon number of the alkyl group of the alkylpyridinium salt may be, for example, 3 to 24.
[0018] From the viewpoint of achieving better level dyeing ability and dyeing ability, the dye solution preferably contains at least one surfactant selected from the group consisting of anionic surfactants and nonionic surfactants.
[0019] The amount of the surfactant contained in the dyeing solution is not particularly limited. From the viewpoint of obtaining superior dyeing uniformity and dyeing ability, the amount of the surfactant contained in the dyeing solution is preferably 0 g / L or more and 25 g / L or less, and more preferably 0.015 g / L or more and 6.0 g / L or less.
[0020] 1.1.3 Other conditions for dyeing process Other conditions in the dyeing treatment are not particularly limited, and conditions that allow the polyester fiber to be dyed with the dye solution are adopted. For example, the following conditions can be mentioned.
[0021] 1.1.3.1 Liquor ratio in dyeing process The liquor ratio of polyester fiber to dye solution varies depending on the desired performance, but may be, for example, 1:3 to 1:30, preferably 1:5 to 1:25, and more preferably 1:5 to 1:20.
[0022] 1.1.3.2 Dyes The dye may be any dye capable of dyeing polyester fibers. For example, a disperse dye is suitable. The amount of the dye used may be appropriately selected. For example, the amount may be 0.001% owf or more and 20% owf or less.
[0023] 1.1.3.3 Dyeing machinery The dyeing machine used in the dyeing process is not particularly limited, and a conventional one can be used, for example, a jet dyeing machine, a winch dyeing machine, a jigger dyeing machine, a beam dyeing machine, a cheese dyeing machine, an Obermeyer dyeing machine, a high-pressure jet dyeing machine, etc.
[0024] 1.1.3.4 Dyeing temperature and dyeing time The dyeing process is carried out by contacting the polyester fiber with the dyeing solution using the dyeing machine. The dyeing temperature and dyeing time can be the same as those of the conventional dyeing process. For example, the dyeing solution is heated to about 40 to 60°C, and the temperature is gradually increased over about 50 to 80 minutes, or about 30 to 50 minutes if it is desired to complete the dyeing quickly, and high-temperature treatment is carried out at 120 to 140°C (preferably 125 to 135°C) for about 0 to 90 minutes, preferably 30 to 60 minutes.
[0025] 1.2 Soaping process The manufacturing method of the present disclosure includes performing a soaping treatment on the polyester-based fiber after the dyeing treatment in the same bath as the dyeing solution or in a separate bath. Here, the soaping solution used in the soaping treatment may contain a polyester copolymer (polymer A) described later.
[0026] 1.2.1 Soaping solution The soaping liquid may contain polymer A. The soaping liquid may contain components other than polymer A in addition to polymer A. When the cleaning liquid in the cleaning treatment described below contains polymer A, the soaping liquid may or may not contain polymer A. When the cleaning liquid described below does not contain polymer A, the soaping liquid contains polymer A.
[0027] 1.2.1.1 Polymer A The polymer A contains a dicarboxylic acid unit and a diol unit, and can be obtained by, for example, a transesterification method or a direct polymerization method.
[0028] (dicarboxylic acid unit) The dicarboxylic acid unit constituting the polymer A contains at least one of a unit (unit X) derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, and a unit (unit Y) derived from a tricarboxylic acid, in an amount of 5 mol% to 30 mol%. In other words, the dicarboxylic acid unit constituting the polymer A contains one or both of the units X and the units Y in total in an amount of 5 mol% to 30 mol%, and the remainder is composed of dicarboxylic acid units other than the units X and the units Y. The dicarboxylic acid unit constituting the polymer A contains preferably 5 mol% to 15 mol%, more preferably 5 mol% to 12 mol%, of the unit X derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group. Alternatively, the dicarboxylic acid unit constituting the polymer A contains preferably 8 mol% to 20 mol%, more preferably 10 mol% to 20 mol%, of the unit Y derived from a tricarboxylic acid. When the dicarboxylic acid unit constituting the polymer A has a unit X derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, if the unit X is too small, the solubility in water is deteriorated, and there is a concern that the dye may not be dispersed well in the dyeing process or soaping process. On the other hand, if the unit X is too large, it is difficult to obtain sufficient fastness. The same applies to the case where the dicarboxylic acid unit constituting the polymer A has a unit Y derived from a tricarboxylic acid.
[0029] Incidentally, a "unit derived from a tricarboxylic acid" can be expressed as a "unit derived from a dicarboxylic acid having one additional carboxylic acid group or carboxylate group". In other words, in the present application, exceptionally, a "unit derived from a tricarboxylic acid" is considered to be a type of "dicarboxylic acid unit". On the other hand, in the present application, a "unit derived from a polyvalent carboxylic acid having 4 or more valences" is not considered to be a "dicarboxylic acid unit".
[0030] The dicarboxylic acid unit constituting the polymer A may be derived from an aliphatic dicarboxylic acid or an aromatic dicarboxylic acid, but is preferably derived from an aromatic dicarboxylic acid. The aromatic dicarboxylic acid may be, for example, at least one selected from terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, diphenyldicarboxylic acid, diphenoxyethanedicarboxylic acid, β-hydroxyethoxybenzoic acid, and p-hydroxybenzoic acid. In particular, when the dicarboxylic acid unit constituting the polymer A contains one or both of terephthalic acid and isophthalic acid, more excellent performance is likely to be obtained. The aliphatic dicarboxylic acid may be, for example, at least one selected from adipic acid, sebacic acid, dodecanedioic acid, maleic acid, and succinic acid. These dicarboxylic acids may be acid anhydrides or ester derivatives with lower alcohols or glycols.
[0031] The dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group may be a dicarboxylic acid having a sulfonic acid group and / or a sulfonate group bonded to the above-mentioned various dicarboxylic acids. The sulfonate group may be a metal salt group such as Li salt, Na salt, K salt, Mg salt, or an amine salt group such as ammonia or triethanolamine. In particular, an alkali metal salt group, particularly a Na salt group, is preferred. The dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group may be at least one selected from, for example, sulfoterephthalic acid, 5-sulfoisophthalic acid, 4-sulfophthalic acid, salts thereof, and ester derivatives thereof such as dimethyl ester, diethyl ester, diphenyl ester, etc.
[0032] The tricarboxylic acid (dicarboxylic acid having one or both of a carboxylic acid group and a carboxylate group) may be a dicarboxylic acid having a carboxylic acid group and / or a carboxylate group bonded to the above-mentioned dicarboxylic acid. The carboxylate group may be a metal salt group such as Li salt, Na salt, K salt, or Mg salt, or an amine salt group such as ammonia or triethanolamine. In particular, an alkali metal salt group, and among these, a Na salt group, is preferred. The tricarboxylic acid (dicarboxylic acid containing a carboxylic acid group) may be at least one selected from trimellitic acid, trimesic acid, 1,2,3-benzenetricarboxylic acid, salts thereof, and ester derivatives thereof such as dimethyl ester, diethyl ester, and diphenyl ester.
[0033] The dicarboxylic acid unit constituting the polymer A may, for example, include a unit derived from a dicarboxylic acid a1 that does not have a sulfonic acid group or a sulfonate group and does not fall under the category of a tricarboxylic acid, and a unit derived from a dicarboxylic acid a2 that has one or both of a sulfonic acid group and a sulfonate group and does not fall under the category of a tricarboxylic acid. Alternatively, the dicarboxylic acid unit constituting the polymer A may, for example, include a unit derived from a dicarboxylic acid a1 that does not have a sulfonic acid group or a sulfonate group and does not fall under the category of a tricarboxylic acid, and a unit derived from a tricarboxylic acid (a dicarboxylic acid having one or both of a carboxylic acid group and a carboxylic acid group) a3. The carbon skeleton of the dicarboxylic acid a1, the carbon skeleton of the dicarboxylic acid a2, and the carbon skeleton of the tricarboxylic acid a3 may be the same or different from each other. The dicarboxylic acid unit constituting the polymer A may, for example, contain a unit derived from one or both of terephthalic acid and isophthalic acid as a dicarboxylic acid a1 that does not have a sulfonic acid group or a sulfonate group and does not fall under the category of a tricarboxylic acid, and may contain a unit derived from sulfoisophthalic acid as a dicarboxylic acid a2 that has a sulfonic acid group or a sulfonate group and does not fall under the category of a tricarboxylic acid. Specific examples of the tricarboxylic acid a3 are as described above.
[0034] The dicarboxylic acid unit constituting the polymer A may be, for example, a unit derived from a dicarboxylic acid having a molecular weight of 100 or more and 300 or less. The dicarboxylic acid unit constituting the polymer A may be the same type as or different from the polybasic acid unit constituting the polyester fiber described above.
[0035] (Polycarboxylic acid units other than dicarboxylic acid units) In addition to the dicarboxylic acid, the polymer A may contain, as a structural unit, a unit derived from a tetracarboxylic to hexacarboxylic polycarboxylic acid such as tetracarboxylic acid, pentacarboxylic acid, or hexacarboxylic acid. In the polymer A, the ratio of the dicarboxylic acid units to the total polycarboxylic acid units may be, for example, more than 50 mol%, 60 mol% or more, 70 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more. In addition, the ratio of the polycarboxylic acid units other than the dicarboxylic acid units to the total polycarboxylic acid units may be, for example, less than 50 mol%, 40 mol% or less, 30 mol% or less, 20 mol% or less, 10 mol% or less, 5 mol% or less, or 1 mol% or less.
[0036] (diol unit) The diol unit constituting the polymer A is derived from a diol having a molecular weight of 48 or more and less than 900. The molecular weight of the diol is preferably 60 or more and 600 or less, more preferably 60 or more and 300 or less, and even more preferably 60 or more and 200 or less. If the molecular weight of the diol is too low, there is a concern that sufficient water solubility is not obtained and stability in the bath is poor. On the other hand, if the molecular weight is too high, there is a concern that the water solubility is excessively high, which may adversely affect fastness improvement performance.
[0037] The diol unit constituting the polymer A may be derived from an aliphatic diol or an aromatic diol, but is preferably derived from an aliphatic diol. Examples of such diols include alkylene glycol and polyalkylene glycol. The diol may be at least one selected from polyethylene glycol, ethylene glycol, alkylene glycols having 3 or more carbon atoms, neopentyl glycol, polypropylene glycol, Pluronic (registered trademark) type surfactants, and ethylene oxide adducts of bisphenol A. Among them, ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycols having a molecular weight of 200 to 600, 1,4-butanediol, and neopentyl glycol are preferred. The diol unit constituting the polymer A may be the same type as or different from the polyhydric alcohol unit constituting the polyester-based fiber described above.
[0038] (Polyhydroxy compound units other than diol units) In addition to the diols, the polymer A may contain, as a constituent unit, a unit derived from a trivalent to hexavalent polyhydric hydroxy compound such as a triol, a tetraol, a pentaol, or a hexaol. In the polymer A, the ratio of the diol units to the total polyhydric hydroxy compound units may be, for example, more than 50 mol%, 60 mol% or more, 70 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more. In addition, the ratio of the polyhydric hydroxy compound units other than the diol units to the total polyhydric hydroxy compound units may be, for example, less than 50 mol%, 40 mol% or less, 30 mol% or less, 20 mol% or less, 10 mol% or less, 5 mol% or less, or 1 mol% or less.
[0039] (Weight average molecular weight of polymer A) The weight average molecular weight of the polymer A is not particularly limited. When the dicarboxylic acid unit constituting the polymer A includes a unit derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, the weight average molecular weight of the polymer A may be, for example, 2000 to 80000, or 5000 to 70000. When the dicarboxylic acid unit constituting the polymer A includes a unit derived from a tricarboxylic acid, the weight average molecular weight of the polymer A may be, for example, 2000 to 80000, or 2000 to 20000. When the weight average molecular weight of the polymer A is within such a range, the fastness of the polyester-based dyed fiber product can be further improved. In the present application, the "weight average molecular weight" is measured by size exclusion chromatography using an instrument: HLC-8120 (manufactured by Tosoh Corporation), a column: TSK-GEL Super AWM-H (manufactured by Tosoh Corporation), 10 mM LiBr-DMF as the mobile phase, and polystyrene as the standard substance.
[0040] (Intramolecular content ratio of dicarboxylic acid units in polymer A) The intramolecular content of dicarboxylic acid units in polymer A is 50% by mass or more and 75% by mass or less, preferably 55% by mass or more and 75% by mass or less, and more preferably 60% by mass or more and 75% by mass or less. If this ratio is too low or too high, sufficient fastness is difficult to obtain.
[0041] (Amount of Polymer A in soaping solution) The amount of polymer A contained in the soaping liquid is not particularly limited. The amount of polymer A contained in the soaping liquid is preferably 0.005 g / L or more and 5.0 g / L or less, more preferably 0.010 g / L or more and 3.0 g / L or less, and even more preferably 0.1 g / L or more and 2.5 g / L or less.
[0042] 1.2.1.2 Components other than polymer A The soaping liquid may contain components other than the polymer A. Examples of the components other than the polymer A include known components (alkali, reducing agent, etc.) used in soaping treatment. The soaping liquid may also contain water, an organic solvent, a surfactant, etc. These may be derived from the dyeing liquid. Details of the organic solvent, surfactant, etc. are as described above. The soaping liquid may also contain an acid for adjusting the pH, a chelating agent, etc.
[0043] The reducing agent may be, for example, at least one selected from hydrosulfite, sodium hydrosulfite, thiourea dioxide, and reducing sugars (D-glucose, D-xylose, etc.). In this case, the pH adjuster may be any alkaline substance such as caustic soda or soda ash. When at least one selected from hydrosulfite, sodium hydrosulfite, thiourea dioxide, and reducing sugars is used as the reducing agent, the pH adjuster is preferably caustic soda from the viewpoint of soaping effect. Alternatively, when at least one selected from hydrosulfite, sodium hydrosulfite, and thiourea dioxide is used as the reducing agent, the pH adjuster may be soda ash from the same viewpoint.
[0044] The reducing agent may be, for example, at least one sulfinic acid selected from sodium hydroxymethanesulfinate or a salt thereof, and in this case, the pH adjuster may be any acidic substance such as acetic acid or formic acid.
[0045] The reducing agent is preferably at least one selected from hydrosulfite, sodium hydrosulfite, thiourea dioxide, and sodium hydroxymethanesulfinate, and more preferably at least one selected from hydrosulfite, sodium hydrosulfite, and thiourea dioxide. When such a reducing agent is combined with the polymer A, fastness is likely to be improved more significantly.
[0046] 1.2.2 Other conditions in soaping process Other conditions for the soaping treatment are not particularly limited, and any conditions that allow the above-mentioned polyester-based fiber to be soaped with the above-mentioned soaping liquid are adopted. For example, the following conditions can be mentioned.
[0047] 1.2.2.1 Liquor ratio in soaping process The liquor ratio of polyester fibers to soaping liquid varies depending on the desired performance, but may be, for example, 1:3 to 1:30, preferably 1:5 to 1:25, more preferably 1:5 to 1:20, and even more preferably 1:5 to 1:15.
[0048] 1.2.2.2 Soaping temperature and soaping time The soaping temperature may be the same as that used in general dyeing processes, that is, in the range of 60 to 140° C., but considering deterioration of the various physical properties and texture of the textile product, it is preferably in the range of 70 to 100° C., more preferably in the range of 70 to 90° C. The soaping time may be, for example, 5 to 60 minutes. From the viewpoint of sufficient soaping and suppressing deterioration of the various physical properties of the textile product, 10 to 30 minutes is preferred.
[0049] 1.3. Separate bath treatment (two-bath, two-stage method) As an example of a method in which the dyeing process and the soaping process are carried out in separate baths (two baths) (two-bath, two-stage method), the following first example can be mentioned.
[0050] First type: After the dyeing process, the dyeing solution is discharged and new soaping solution (soaping bath) is prepared and then soaping process is carried out.
[0051] 1.4.Same-bath treatment (one-bath, two-stage method) A specific example of the form in which the dyeing process and soaping process are performed in the same bath (one bath), that is, the form in which the dyeing process and soaping process are performed in a one-bath two-step method, is a form in which, after the dyeing process, the entire amount of the dyeing solution is not drained, but a part or all of the dyeing solution is left and a component required for soaping is added to perform the soaping process. In this way, by performing the dyeing process and soaping process in the same bath (one bath), it is possible to save water and reduce energy.
[0052] When soaping is performed in a state where components (dyes, etc.) derived from the dyeing solution remain in the soaping solution, as in the one-bath, two-stage method, there is a problem that the fastness of the polyester-based dyed fiber product is more likely to decrease. In contrast, in the manufacturing method of the present disclosure, as described above, the soaping solution contains a polyester copolymer (polymer A), so that even when soaping is performed by the one-bath, two-stage method, fastness equal to or higher than that when dyeing and soaping are performed by the conventional two-bath, two-stage method can be ensured.
[0053] In the manufacturing method of the present disclosure, for example, 20% by volume to 100% by volume, 50% by volume to 100% by volume, 70% by volume to 100% by volume, or 90% by volume to 100% by volume of the dyeing solution may be used to prepare the soaping solution. If the dyeing solution is not drained after the dyeing process, 100% by volume of the dyeing solution will be used as the soaping solution.
[0054] Specific examples of the dyeing process and the soaping process in the same bath (one bath) include the following second and third forms. In the manufacturing method of the present disclosure, even if the dye solution used in the dyeing process contains a polyester copolymer (polymer A), as in the second form, the dyeing process of the polyester fiber using the dye solution is appropriately performed.
[0055] Second form: A form in which the dyeing solution used in the dyeing process contains a polyester copolymer (polymer A), and at least a part of the polymer A contained in the dyeing solution is used as at least a part of the polymer A contained in the soaping solution. More specifically, for example, after dyeing is performed with a dyeing solution containing polymer A, a pH adjuster, a reducing agent, etc. are added to the dyeing solution (dye bath) to prepare a soaping solution (soaping bath), and then a soaping process is performed.
[0056] Third form: A form in which at least a polyester copolymer (polymer A) is added to the dyeing solution (dye bath) after the dyeing process to prepare a soaping solution, and then a soaping process is performed. More specifically, for example, a form in which a pH adjuster, a reducing agent, and the like are added together with polymer A to the dyeing solution (dye bath) after the dyeing process to prepare a soaping solution (soaping bath), and then a soaping process is performed.
[0057] In both the second and third forms, the timing of adding a pH adjuster and a reducing agent to the dyeing solution after the dyeing process is not particularly limited. In particular, it is preferable to add a pH adjuster and a reducing agent to the dyeing solution when the temperature is lowered after the dyeing process, or after the temperature is lowered to the temperature for performing the soaping process (preferably after the temperature is lowered to the temperature for performing the soaping process). The same applies to the timing when the polyester copolymer (polymer A) is added in the third form. In the second form, after the dyeing process using the dyeing solution containing the polyester copolymer (polymer A), the polyester copolymer (polymer A) may or may not be added to the dyeing solution. In the second form, when the polyester copolymer (polymer A) is further added to the dyeing solution after the dyeing process, the timing may be the same as above.
[0058] 1.5 Cleaning process The manufacturing method of the present disclosure includes performing one or both of hot water washing and water washing on the polyester fiber after the soaping treatment. Here, the washing liquid used in the washing treatment may contain the above-mentioned polymer A. In addition to the polymer A, the washing liquid may contain components other than the polymer A. When the soaping liquid in the above-mentioned soaping treatment contains the polymer A, the washing liquid in the washing treatment may or may not contain the polymer A. When the soaping liquid does not contain the polymer A, the washing liquid contains the polymer A.
[0059] (Amount of Polymer A in the cleaning solution) The amount of polymer A contained in the cleaning solution is not particularly limited, but is preferably 0.005 g / L or more and 5.0 g / L or less, more preferably 0.010 g / L or more and 3.0 g / L or less, and even more preferably 0.1 g / L or more and 2.5 g / L or less.
[0060] (Components other than polymer A) The cleaning liquid may contain components other than the polymer A. Examples of the components other than the polymer A include known components (such as a pH adjuster) used in hot water washing treatment and / or water washing treatment.
[0061] (Other conditions for cleaning process) Other conditions in the washing treatment are not particularly limited, and conditions that allow the polyester fiber to be washed with hot water and / or water by the washing solution are adopted. For example, the following conditions can be mentioned.
[0062] (Liquid ratio in cleaning process) The liquor ratio of polyester fibers to cleaning liquid varies depending on the desired performance, but may be, for example, 1:3 to 1:30, preferably 1:5 to 1:25, more preferably 1:5 to 1:20, and even more preferably 1:5 to 1:15.
[0063] (Cleaning temperature and cleaning time) The temperature of the washing treatment may be a general treatment temperature, for example, in the range of 20 to 100° C., and preferably in the range of 30 to 90° C. The time of the washing treatment may be, for example, 2 to 60 minutes. From the viewpoint of sufficient washing and improvement of the quality of various physical properties of the textile product, the time of 5 to 30 minutes is preferable.
[0064] (Method of adding polymer A) In the manufacturing method of the present disclosure, good performance can be obtained when at least one of the dyeing solution, soaping solution, and washing solution contains the above-mentioned polyester copolymer (polymer A). In particular, it is preferable that at least two or three of the dyeing solution, soaping solution, and washing solution contain the above-mentioned polyester copolymer (polymer A). It is more preferable to add it to the soaping solution and washing solution from the viewpoint of reducing the change in color of polyester-based dyed fiber products.
[0065] 1.6 Other Processing The manufacturing method of the present disclosure may include any method that uses a predetermined polyester copolymer (polymer A), performs dyeing and soaping in the same bath (1 bath) or in separate baths (2 baths), and then performs washing, and may further include various other treatments. For example, in the manufacturing method of the present disclosure, scouring is preferably performed before the above-mentioned dyeing. Scouring is performed, for example, using a scouring agent in a batch system using a wince or liquid flow dyeing machine, or in a continuous system using a continuous scouring device. The scouring agent may be at least one selected from the following: a nonionic surfactant such as polyoxyalkylene alkyl ether or polyoxyalkylene alkyl allyl ether; a blend of a nonionic surfactant and an anionic surfactant such as alkylbenzene sulfonate or fatty alcohol sulfate;
[0066] 2. Fastness improver composition The technology of the present disclosure has an aspect as a fastness improver composition in addition to the above-mentioned aspect as a method for producing a polyester-based dyed fiber product. That is, the fastness improver composition according to one embodiment contains a polyester copolymer (polymer A). Here, the polyester copolymer contains a dicarboxylic acid unit and a diol unit. The dicarboxylic acid unit contains at least one of a unit derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, and a unit derived from a tricarboxylic acid, in an amount of 5 mol% to 30 mol%. The diol unit is derived from a diol having a molecular weight of 48 or more and less than 900. The intramolecular content ratio of the dicarboxylic acid unit in the polyester copolymer is 50 mass% to 75 mass%.
[0067] Details of the polyester copolymer (polymer A) contained in the fastness improver composition are as described above. The fastness improver composition of the present disclosure may contain, for example, in addition to polymer A, other components other than polymer A. The other components other than polymer A are also as described above. The fastness improver composition of the present disclosure may be, for example, one used during dyeing of polyester-based fibers, one used during soaping treatment of polyester-based dyed fibers, or one used after soaping treatment.
[0068] 3. Supplementary Information In the above description, the "dicarboxylic acid unit" constituting the polyester copolymer (polymer A) exceptionally includes a "unit derived from tricarboxylic acid (a unit derived from a dicarboxylic acid having one additional carboxylic acid group or one additional carboxylic acid group or both)". On the other hand, if the "dicarboxylic acid unit" and the "unit derived from tricarboxylic acid" are distinguished, the polyester copolymer (polymer A) of the present disclosure can also be expressed as one or both of the following polyester copolymer A1 and polyester copolymer A2. That is, the technology of the present disclosure also has an aspect as a fastness improver composition containing one or both of the following polyester copolymer A1 and polyester copolymer A2, and an aspect as a manufacturing method for a polyester-based dyed fiber product using one or both of the following polyester copolymer A1 and polyester copolymer A2.
[0069] (Polyester Copolymer A1) The polyester copolymer A1 contains a dicarboxylic acid unit A1-1 and a diol unit A1-2, the dicarboxylic acid unit A1-1 contains 5 mol % or more and 30 mol % or less of units derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate salt group; The diol unit A1-2 is derived from a diol having a molecular weight of 48 or more and less than 900, and The intramolecular content of the dicarboxylic acid unit A1-1 in the polyester copolymer A1 is 50% by mass or more and 75% by mass or less.
[0070] (Polyester Copolymer A2) The polyester copolymer A2 contains dicarboxylic acid units A2-1, diol units A2-2, and tricarboxylic acid units A2-3, the proportion of the tricarboxylic acid units A2-3 in the total of the dicarboxylic acid units A2-1 and the tricarboxylic acid units A2-3 is 5 mol % or more and 30 mol % or less; the diol unit A2-2 is derived from a diol having a molecular weight of 48 or more and less than 900; The total intramolecular content of the dicarboxylic acid unit A2-1 and the tricarboxylic acid unit A2-3 in the polyester copolymer A2 is 50% by mass or more and 75% by mass or less.
[0071] In the polyester copolymer A2, the dicarboxylic acid unit A2-1 may or may not contain a unit X derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group. The total proportion of the unit X and the unit Y derived from a tricarboxylic acid in the dicarboxylic acid unit A2-1 may be 5 mol % or more and 30 mol % or less. EXAMPLES
[0072] The manufacturing method of the present disclosure will be further described below with reference to examples, but the manufacturing method of the present disclosure is not limited to the following examples. In the manufacturing method of the present disclosure, various conditions can be adopted as long as the object is achieved without departing from the gist of the method.
[0073] 1. Preparation of polyester copolymer (polymer A) 1.1 Synthesis Example 1 In a reaction vessel, 155.4g (0.8 mol) of dimethyl terephthalate, 59.2g (0.2 mol) of dimethyl 5-sulfoisophthalate sodium salt, 62g of ethylene glycol, 12g of polyethylene glycol with a molecular weight of 600, and 0.1g of zinc acetate were charged, and the temperature was raised from 150°C to 230°C over about 3 hours while stirring under a nitrogen gas atmosphere to carry out an ester exchange reaction, and volatiles were distilled out of the system. Next, 0.1g of tetrabutyl titanate was added and the pressure was gradually reduced to about 10kPa, and the reaction was carried out at 250°C for 2 hours to obtain about 224g of polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was about 72% by mass, and the weight average molecular weight was 19,000.
[0074] 1.2 Synthesis Example 2 The reaction was carried out in the same manner as in Synthesis Example 1, except that 165.1 g (0.85 mol) of dimethyl terephthalate, 44.4 g (0.15 mol) of dimethyl 5-sulfoisophthalate sodium salt, 62 g of ethylene glycol, 12 g of polyethylene glycol having a molecular weight of 600, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain approximately 219 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was approximately 71 mass%, and the weight average molecular weight was 6,500.
[0075] 1.3 Synthesis Example 3 The reaction was carried out in the same manner as in Synthesis Example 1, except that 174.8 g (0.9 mol) of dimethyl terephthalate, 29.6 g (0.1 mol) of dimethyl 5-sulfoisophthalate sodium salt, 31 g of ethylene glycol, 52 g of neopentyl glycol, 12 g of polyethylene glycol having a molecular weight of 600, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain approximately 235 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was approximately 65 mass%, and the weight average molecular weight was 65,000.
[0076] 1.4 Synthesis Example 4 The reaction was carried out in the same manner as in Synthesis Example 1, except that 174.8 g (0.9 mol) of dimethyl terephthalate, 29.6 g (0.1 mol) of dimethyl 5-sulfoisophthalate sodium salt, 106 g of diethylene glycol, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain approximately 244 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was approximately 62 mass%, and the weight average molecular weight was 9,000.
[0077] 1.5 Synthesis Example 5 The reaction was carried out in the same manner as in Synthesis Example 1, except that 116.5 g (0.6 mol) of dimethyl terephthalate, 49.8 g (0.3 mol) of isophthalic acid, 29.6 g (0.1 mol) of dimethyl 5-sulfoisophthalate sodium salt, 62 g of ethylene glycol, 12 g of polyethylene glycol having a molecular weight of 600, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain about 214 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was about 70 mass%, and the weight average molecular weight was 16,000.
[0078] 1.6 Synthesis Example 6 The reaction was carried out in the same manner as in Synthesis Example 1, except that 155.4 g (0.8 mol) of dimethyl terephthalate, 14.6 g (0.1 mol) of adipic acid, 29.6 g (0.1 mol) of dimethyl 5-sulfoisophthalate sodium salt, 49.6 g of ethylene glycol, 20.8 g of neopentyl glycol, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain about 206 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was about 71 mass%, and the weight average molecular weight was 22,000.
[0079] 1.7 Synthesis Example 7 A reaction was carried out in the same manner as in Synthesis Example 1, except that 145.7 g (0.75 mol) of dimethyl terephthalate, 31.5 g (0.15 mol) of trimellitic acid, 23.0 g (0.1 mol) of dodecanedioic acid, 23 g of ethylene glycol, 23 g of 1,4-butanediol, 39 g of neopentyl glycol, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain about 228 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was about 68 mass%, and the weight average molecular weight was 2,800.
[0080] 1.8 Synthesis Example 8 A reaction was carried out in the same manner as in Synthesis Example 1, except that 172.8 g (0.89 mol) of dimethyl terephthalate, 23.1 g (0.11 mol) of trimellitic acid, 39 g of ethylene glycol, 39 g of neopentyl glycol, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain about 213 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was about 69 mass%, and the weight average molecular weight was 4,100.
[0081] 1.9 Comparative synthesis example 1 The reaction was carried out in the same manner as in Synthesis Example 1, except that 116.5 g (0.6 mol) of dimethyl terephthalate, 118.4 g (0.4 mol) of dimethyl 5-sulfoisophthalate sodium salt, 62 g of ethylene glycol, 24 g of polyethylene glycol having a molecular weight of 600, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain approximately 256 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was approximately 71 mass%, and the weight average molecular weight was 29,000.
[0082] 1.10 Comparative synthesis example 2 The reaction was carried out in the same manner as in Synthesis Example 1, except that 126.2 g (0.65 mol) of dimethyl terephthalate, 103.6 g (0.35 mol) of dimethyl 5-sulfoisophthalate sodium salt, 62 g of ethylene glycol, 120 g of polyethylene glycol having a molecular weight of 600, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain approximately 347 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was approximately 53 mass%, and the weight average molecular weight was 41,000.
[0083] 1.11 Comparative synthesis example 3 The reaction was carried out in the same manner as in Synthesis Example 1, except that 174.8 g (0.9 mol) of dimethyl terephthalate, 29.6 g (0.1 mol) of dimethyl 5-sulfoisophthalate sodium salt, 62 g of ethylene glycol, 310 g of polyethylene glycol having a molecular weight of 3100, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain approximately 512 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was approximately 32 mass%, and the weight average molecular weight was 85,000.
[0084] 1.12 Comparative Synthesis Example 4 The reaction was carried out in the same manner as in Synthesis Example 1, except that 116.5 g (0.6 mol) of dimethyl terephthalate, 118.4 g (0.4 mol) of dimethyl 5-sulfoisophthalate sodium salt, 57 g of ethylene glycol, 86 g of polyethylene glycol having a molecular weight of 1000, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain approximately 314 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was approximately 59 mass%, and the weight average molecular weight was 31,000.
[0085] 1.13 Comparative Synthesis Example 5 The reaction was carried out in the same manner as in Synthesis Example 1, except that 186.2 g (0.96 mol) of dimethyl terephthalate, 11.8 g (0.04 mol) of dimethyl 5-sulfoisophthalate sodium salt, 31 g of ethylene glycol, 12 g of polyethylene glycol having a molecular weight of 600, 52 g of neopentyl glycol, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain approximately 229 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was approximately 64 mass%, and the weight average molecular weight was 19,000.
[0086] 1.14 Comparative Synthesis Example 6 The reaction was carried out in the same manner as in Synthesis Example 1, except that 135.8 g (0.7 mol) of dimethyl terephthalate, 88.8 g (0.3 mol) of dimethyl 5-sulfoisophthalate sodium salt, 62 g of ethylene glycol, and 0.1 g of zinc acetate were charged into a reaction vessel, to obtain approximately 223 g of a polyester copolymer. The content of dicarboxylic acid component units in the obtained polyester copolymer was approximately 76 mass%, and the weight average molecular weight was 30,000.
[0087] Table 1 below shows, for each of the polyester copolymers according to the above Synthesis Examples and Comparative Synthesis Examples, the amount (mol %) of units derived from a specific dicarboxylic acid (a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group) in the total dicarboxylic acid units, the intramolecular content of the dicarboxylic acid units in the polyester copolymer, and the weight average molecular weight of the polyester copolymer.
[0088] [Table 1]
[0089] 2. Preparation of soaping agent 2.1 Soaping agent A-1 25.0 parts by mass of the polyester copolymer obtained in Synthesis Example 1 and 75.0 parts by mass of water were charged into a mixing kettle and mixed uniformly at 80 to 90° C. to obtain a soaping agent A-1.
[0090] 2.2 Soaping agents A-2 to A-8, B-1 to B-6 Soaping agents A-2 to A-8 and B-1 to B-6 were obtained in the same manner as soaping agent A-1, except that the components shown in Table 2 below were used.
[0091] [Table 2]
[0092] 2.3 Soaping agents C-1 to C-6 (prior art) The components shown in Table 3 below were charged into a mixing kettle and mixed uniformly at 50 to 60° C. to obtain soaping agents C-1 to C-6.
[0093] [Table 3]
[0094] 3. Dyeing and soaping treatment 3.1 First embodiment (two-bath, two-stage process): Examples 1-1 and 1-2, Comparative Examples 1-1, 2-1, 3-1, 1-2, 2-2, and 3-2 Polyester fibers were dyed and soaped using a two-bath, two-step method.
[0095] 3.1.1 Dyeing process A 100% polyester fabric was used as the test cloth, and a mini color dyeing machine (Rapid) was used as the test equipment. The test cloth was placed in a dyeing solution having the following composition so that the bath ratio was 1:15, and dyeing was performed at 130°C for 60 minutes (heating was increased from 60°C at 2°C / min).
[0096] <Composition of staining solution> 80% acetic acid 0.4g / L Dyeing assistant NICCA SUNSOLT RM-3406 0.5g / L disperse dye Foron Rubine (manufactured by ARCHROMA) 4.5%owf or Disperse Black (Kowa Emori) 7.5% owf
[0097] 3.1.2 Soaping process After the above dyeing process, the dyeing solution was cooled to about 80°C and then drained. A new soaping solution having the following composition was prepared and soaping was carried out at a bath ratio of 1:15 at 80°C for 20 minutes.
[0098] <Soaping liquid composition> Soaping agent 0 or 1g / L Caustic soda 48% 0.8 or 1.0g / L Sodium hydrosulfite 0.8 or 1.0g / L
[0099] 3.1.3 Cleaning process, etc. The polyester fiber after the above soaping treatment was washed with water, dehydrated and dried to obtain a polyester dyed fiber product. The washing liquid used for washing did not contain a soaping agent.
[0100] 3.2 Second embodiment (one-bath, two-stage process): Examples 2-3, Comparative Examples 4-7 A dyeing assistant and a soaping agent were used in the dyeing solution to dye polyester fibers, and then the agents were added to the dye bath to prepare a soaping solution, followed by soaping.
[0101] 3.2.1 Dyeing process A 100% polyester fabric was used as the test cloth, and a mini color dyeing machine (Rapid) was used as the test equipment. The test cloth was placed in a dyebath having the following composition so that the bath ratio was 1:15, and dyeing was performed at 130°C for 60 minutes (heating from 60°C at 2°C / min).
[0102] <Dye bath composition> 80% acetic acid 0.4g / L Dyeing assistant NICCA SUNSOLT RM-3406 0.5g / L Soaping agent 0 or 1g / L disperse dye Foron Rubine (manufactured by ARCHROMA) 4.5%owf or Disperse Black (Kowa Emori) 7.5% owf
[0103] 3.2.2 Soaping process After the above dyeing process, the dyeing solution was cooled to about 80° C., the following chemicals were added to prepare a soaping solution, and soaping was carried out for 20 minutes at 80° C. Here, the following chemicals were added at 1 g / L each so that the bath ratio of polyester fiber to soaping solution remained at 1:15.
[0104] <Drugs> Caustic soda 48% 1g / L Sodium hydrosulfite or thiourea dioxide 1g / L
[0105] 3.2.3 Cleaning process, etc. The polyester fiber after the above soaping treatment was washed with water, dehydrated and dried to obtain a polyester dyed fiber product. The washing liquid used for washing did not contain a soaping agent.
[0106] 3.3 Third embodiment (one-bath, two-stage process): Examples 4 to 15, Comparative Examples 8 to 20 A dyeing process for polyester fibers was carried out using a dyeing assistant in a dyeing solution, and then a soaping agent and chemicals were added to the dye bath to prepare a soaping solution, and a soaping process was carried out.
[0107] 3.3.1 Dyeing process A 100% polyester fabric was used as the test cloth, and a mini color dyeing machine (Rapid) was used as the test equipment. The test cloth was placed in a dyeing solution having the following composition so that the bath ratio was 1:15, and dyeing was performed at 130°C for 60 minutes (heating was increased from 60°C at 2°C / min).
[0108] <Composition of staining solution> 80% acetic acid 0.4g / L Dyeing assistant NICCA SUNSOLT RM-3406 0.5g / L disperse dye Foron Rubine (manufactured by ARCHROMA) 4.5%owf or Disperse Black (Kowa Emori) 7.5% owf
[0109] 3.3.2 Soaping process After the above dyeing process, the dyeing solution was cooled to about 80° C., the following chemicals were added to prepare a soaping solution, and soaping was carried out for 20 minutes at 80° C. Here, the following chemicals were added in the amounts shown below so that the bath ratio of polyester fiber to soaping solution remained at 1:15.
[0110] <Drugs> Soaping agent 1g / L Caustic soda 48% or soda ash 1 or 5g / L Sodium hydrosulfite or thiourea dioxide 1g / L
[0111] 3.3.3 Cleaning process The polyester fiber after the above soaping treatment was washed with water, dehydrated and dried to obtain a polyester dyed fiber product. The washing liquid used for washing did not contain a soaping agent.
[0112] 3.4 Others (one-step two-bath method): Examples 16 to 26, Comparative Examples 21 to 22 The above describes the case where only one type of soaping agent is added to the dyeing solution or soaping solution. Below, we will show the case where multiple types of soaping agents are added in combination to the soaping solution, and the case where a soaping agent is added to the washing solution used in the washing process (hot water washing process and / or water washing process) after the soaping process.
[0113] 3.4.1 Examples 16 to 18 3.4.1.1 Dyeing and soaping processes After dyeing in the same manner as in the third embodiment, the dyeing solution was cooled to about 80° C., and the following chemicals were added as desired to prepare a soaping solution, which was then soaped for 20 minutes at 80° C. Here, the following chemicals were added in the amounts shown below so that the liquor ratio of polyester fiber to soaping solution remained at 1:15.
[0114] Soaping agent 0 or 0.5g / L Caustic soda 48% 1g / L Sodium hydrosulfite or thiourea dioxide 1g / L
[0115] 3.4.1.2 Cleaning process After the above soaping treatment, the following chemicals were added to prepare a washing solution, and then washing treatment was carried out for 20 minutes at 80°C in hot water or 30°C in water. The amounts of the following chemicals added were adjusted as follows so that the bath ratio of polyester fiber to washing solution was 1:15. Then, dehydration and drying were carried out to obtain a polyester dyed fiber product.
[0116] <Drugs> Soaping agent A-3 0.5g / L or 1g / L
[0117] 3.4.2 Examples 19 to 22 and Comparative Example 21 The dyeing and soaping treatments were carried out in the same manner as in the third embodiment, except that 80% acetic acid and soaping agent C-5 (a liquid reducing agent, equivalent to that disclosed in Patent Document 1) were added to the dyeing solution after the dyeing treatment to carry out the soaping treatment. Specifically, the procedure is as follows.
[0118] 3.4.2.1 Dyeing process A 100% polyester fabric was used as the test cloth, and a mini color dyeing machine (Rapid) was used as the test equipment. The test cloth was placed in a dyeing solution (dye bath) having the following composition so that the bath ratio was 1:15, and dyeing was performed at 130°C for 60 minutes (heating from 60°C at 2°C / min).
[0119] <Composition of staining solution> 80% acetic acid 0.4g / L Dyeing assistant NICCA SUNSOLT RM-3406 0.5g / L disperse dye Foron Rubine (manufactured by ARCHROMA) 4.5%owf or Disperse Black (Kowa Emori) 7.5% owf
[0120] 3.4.2.2 Soaping process After the above dyeing process, the dyeing solution was cooled to about 80° C., and the following chemicals were added to prepare a soaping solution, which was then soaped for 20 minutes at 80° C. Here, the amounts of the following chemicals added were adjusted as follows so that the bath ratio of polyester fiber to soaping solution remained at 1:15.
[0121] <Drugs> 80% acetic acid 0.5g / L Soaping agent C-5 (liquid reducing agent) 1g / L Soaping agent A-3 0 or 0.5g / L or 1g / L
[0122] 3.4.2.3 Cleaning Treatment A: Example 19, Comparative Example 21 The polyester fiber after the above soaping treatment was washed with water, dehydrated and dried to obtain a polyester dyed fiber product. The washing liquid used for washing did not contain a soaping agent.
[0123] 3.4.2.4 Cleaning Treatment B: Examples 20 to 22 After the above soaping treatment, the following chemicals were added to prepare a washing solution, and then washing treatment was carried out for 20 minutes at 80°C in hot water or 30°C in water. The amounts of the following chemicals added were adjusted as follows so that the bath ratio of polyester fiber to washing solution was 1:15. Then, dehydration and drying were carried out to obtain a polyester dyed fiber product.
[0124] <Drugs> Soaping agent A-3 0.5g / L or 1g / L
[0125] 3.4.3 Examples 23 to 26 and Comparative Example 22 The dyeing process of polyester fibers was carried out using a dyeing assistant in a dyeing solution, and then a soaping agent and chemicals were added to the dye bath to prepare a soaping solution, followed by a soaping process and a hot water washing process or a water washing process.
[0126] 3.4.3.1 Dyeing process A 100% polyester fabric was used as the test cloth, and a mini color dyeing machine (Rapid) was used as the test equipment. The test cloth was placed in a dyeing solution (dye bath) having the following composition so that the bath ratio was 1:15, and dyeing was performed at 130°C for 60 minutes (heating from 60°C at 2°C / min).
[0127] <Composition of staining solution> 80% acetic acid 0.4g / L Dyeing assistant NICCA SUNSOLT RM-3406 0.5g / L disperse dye Foron Rubine (manufactured by ARCHROMA) 4.5%owf or Disperse Black (Kowa Emori) 7.5% owf
[0128] 3.4.3.2 Soaping process After the above dyeing process, the dyeing solution was cooled to about 80° C., and the following chemicals were added to prepare a soaping solution, which was then soaped for 20 minutes at 80° C. Here, the amounts of the following chemicals added were adjusted as follows so that the bath ratio of polyester fiber to soaping solution remained at 1:15.
[0129] <Drugs> Caustic soda 48% 1g / L Soaping agent C-6 (liquid reducing agent) 1g / L Soaping agent A-3 0 or 0.5g / L or 1g / L
[0130] 3.4.3.3 Cleaning Treatment A: Example 23, Comparative Example 22 The polyester fiber after the above soaping treatment was washed with water, dehydrated and dried to obtain a polyester dyed fiber product. The washing liquid used for washing did not contain a soaping agent.
[0131] 3.4.3.4 Cleaning Treatment B: Examples 24 to 26 After the above soaping treatment, the following chemicals were added to prepare a washing solution, and then washing treatment was carried out for 20 minutes at 80°C in hot water or 30°C in water. The amounts of the following chemicals added were adjusted as follows so that the bath ratio of polyester fiber to washing solution was 1:15. Then, dehydration and drying were carried out to obtain a polyester dyed fiber product.
[0132] <Drugs> Soaping agent A-3 0.5g / L or 1g / L
[0133] 4. Evaluation of polyester dyed textile products 4.1 Evaluation of washing fastness Washing fastness was measured using the A-2 method of JIS L0844:2011, and fastness was judged using the staining gray scale (JIS L 0805:2005). The higher the evaluation grade, the better the fastness. Each grade is divided into four to express the subtle differences in fastness. For example, the gap between grades 4 and 5 is expressed as 4.3, 4.5, and 4.8. The same applies to the other grades.
[0134] 4.2 Evaluation of dry and wet rubbing fastness Dry and wet friction fastness was measured using the JIS L0849:2013 friction tester type II (Gakushin type) method, and was evaluated in the same manner as for washing fastness.
[0135] 5. Evaluation Results The evaluation results are shown in Tables 4 to 8 below.
[0136] [Table 4]
[0137] [Table 5]
[0138] [Table 6]
[0139] [Table 7]
[0140] [Table 8]
[0141] The results shown in Tables 4 to 8 reveal the following: (1) Comparative Examples 1-1, 2-1, 3-1, 1-2, 2-2, and 3-2 and Examples 1-1 and 1-2 are examples showing the effect on fastness when the amount of reducing agent is reduced in the two-bath, two-stage treatment according to the first embodiment. It is clear that the fastness of Examples 1-1 and 1-2 is less decreased than that of the comparative examples, and that an improvement in fastness can be expected in the two-bath, two-stage treatment. (2) In the case of the one-bath, two-stage treatment according to the second embodiment, the results of Examples 2 and 3 and Comparative Examples 4 to 7 show that the fastness of polyester-based dyed textile products can be improved even when a specific polyester copolymer is used during dyeing. (3) In the case of the one-bath, two-stage treatment according to the third embodiment, Examples 4 to 15 had superior fastness to Comparative Examples 8 to 15, which used soaping agents made of synthetic resins, Comparative Examples 16 to 20, which used conventional activator-based soaping agents, Comparative Example 21, which used an acidic reducing agent, and Comparative Example 22, which used a reducing sugar, and were equal to or better than the fastness of the two-bath, two-stage treatment in Comparative Example 1. In addition, the alkali used during soaping was effective whether it was caustic soda or soda ash. (4) In the case of the one-bath two-stage treatment according to the third embodiment, the results of Examples 7, 16-18, 20-22, and 24-26 show that the soaping agent A-3 may be added to either the soaping treatment or the washing treatment (hot water washing treatment and / or water washing treatment), or may be added in portions. Furthermore, excellent fastness was obtained by adding the soaping agent A-3 to the hot water washing liquid or the water washing liquid. In this case, it was found that the soaping agent A-3 may be added to both the soaping liquid and the washing liquid (hot water washing liquid and / or water washing liquid). Furthermore, as in Examples 19 and 23, in Comparative Example 21 using an acidic reducing agent and Comparative Example 22 using a reducing sugar, by further adding the soaping agent A-3, superior fastness was obtained compared to the respective Comparative Examples. However, a comparison of Examples 4 to 26 revealed that the reducing agent to be combined with the soaping agent is preferably a sulfur-containing compound (particularly, at least one selected from hydrosulfite, sodium hydrosulfite, thiourea dioxide, and sodium hydroxymethanesulfinate) rather than a reducing sugar.
[0142] From the above results, if a polyester copolymer satisfying the following (1) to (5) is used, it is expected that fastness in a two-bath, two-stage process will be improved. Furthermore, even in a one-bath, two-stage process, a decrease in fastness can be suppressed, and a product equivalent to or better than a polyester-based dyed fiber product obtained by a two-bath, two-stage process can be obtained, and CO2 can be reduced by streamlining the process, and water can be saved by reducing the amount of wastewater discharged once. A polyester copolymer satisfying the following (1) to (5) can be used, for example, as a fastness improver. Furthermore, the polyester copolymer can be used, for example, as shown in the above examples, as a component (soaping agent) added to a soaping solution or an agent added to a washing solution during hot water washing and / or water washing after soaping. (1) The polyester copolymer contains dicarboxylic acid units and diol units. (2) The dicarboxylic acid units contain 5 mol % or more and 30 mol % or less of at least one of units derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, and units derived from a tricarboxylic acid. (3) The diol unit is derived from a diol having a molecular weight of 48 or more and less than 900. (4) The polyester copolymer has an intramolecular content of the dicarboxylic acid unit of 50% by mass or more and 75% by mass or less.
Claims
1. A fastness improver composition comprising a polyester copolymer, The polyester copolymer contains dicarboxylic acid units and diol units, the dicarboxylic acid unit contains at least one of a unit derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, and a unit derived from a tricarboxylic acid, in an amount of 5 mol % to 30 mol %; The diol units constituting the polyester copolymer are composed only of units derived from a diol having a molecular weight of 48 or more and less than 900, and the polyester copolymer has an intramolecular content of the dicarboxylic acid unit of 50% by mass or more and 75% by mass or less; The fastness improver composition contains at least one reducing agent selected from hydrosulfite, sodium hydrosulfite, thiourea dioxide, and sodium hydroxymethanesulfinate. Fastness improver composition.
2. A method for producing a polyester dyed fiber product, comprising the steps of: Dyeing polyester fibers; The polyester fiber after the dyeing treatment is subjected to a soaping treatment in a bath separate from the dyeing solution; and subjecting the polyester-based fiber after the soaping treatment to one or both of a hot water washing treatment and a water washing treatment; Including, One or both of the soaping liquid used in the soaping treatment and the cleaning liquid used in the cleaning treatment contain a polyester copolymer; The polyester copolymer contains dicarboxylic acid units and diol units, the dicarboxylic acid unit contains at least one of a unit derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, and a unit derived from a tricarboxylic acid, in an amount of 5 mol % to 20 mol %; The diol unit is derived from a diol having a molecular weight of 48 or more and less than 900, and The intramolecular content ratio of the dicarboxylic acid unit in the polyester copolymer is 50% by mass or more and 75% by mass or less. Manufacturing method.
3. A method for producing a polyester dyed fiber product, comprising the steps of: Dyeing polyester fibers; performing a soaping treatment on the polyester-based fiber after the dyeing treatment in the same bath as the dyeing solution; and subjecting the polyester-based fiber after the soaping treatment to one or both of a hot water washing treatment and a water washing treatment; Including, The soaping solution used in the soaping treatment is prepared by adding at least a polyester copolymer to the dyeing solution after the dyeing treatment, The polyester copolymer contains dicarboxylic acid units and diol units, the dicarboxylic acid unit contains at least one of a unit derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, and a unit derived from a tricarboxylic acid, in an amount of 5 mol % to 20 mol %; The diol unit is derived from a diol having a molecular weight of 48 or more and less than 900, and The intramolecular content ratio of the dicarboxylic acid unit in the polyester copolymer is 50% by mass or more and 75% by mass or less. Manufacturing method.
4. The method according to claim 2 or 3, The amount of the polyester copolymer contained in the soaping liquid is 0.005 g / L or more and 5.0 g / L or less. Manufacturing method.
5. A method for producing a polyester dyed fiber product, comprising the steps of: Dyeing polyester fibers; The polyester-based fiber after the dyeing treatment is subjected to a soaping treatment in the same bath as the dyeing solution or in a separate bath; and subjecting the polyester-based fiber after the soaping treatment to one or both of a hot water washing treatment and a water washing treatment; Including, The cleaning solution used in the cleaning treatment contains a polyester copolymer, The polyester copolymer contains dicarboxylic acid units and diol units, the dicarboxylic acid unit contains at least one of a unit derived from a dicarboxylic acid having one or both of a sulfonic acid group and a sulfonate group, and a unit derived from a tricarboxylic acid, in an amount of 5 mol % to 30 mol %; The diol unit is derived from a diol having a molecular weight of 48 or more and less than 900, and the polyester copolymer has an intramolecular content of the dicarboxylic acid unit of 50% by mass or more and 75% by mass or less; The amount of the polyester copolymer contained in the cleaning solution is 0.005 g / L or more and 5.0 g / L or less. Manufacturing method.
Citation Information
Patent Citations
Dyeing method of polyester-cotton blended fiber
CN108301229A
One-bath dyeing-cleaning method for recycle polyester
CN112593423A
Goseiseniruiokinichinisenshokusuruhoho
JP1976109381A
Dyeability improver for polyester fiber material and disperse dye composition
JP2019065403A
Liquid reducing agent composition and reducing washing method
WO2020196902A1