Positive electrode active material for sodium secondary battery, positive electrode for sodium secondary battery, sodium secondary battery

The development of a composite metal oxide-based positive electrode active material with a carbon layer for sodium secondary batteries addresses the low energy density issue, enhancing discharge voltage and capacity to improve battery performance.

JP7560939B2Active Publication Date: 2024-10-03SUMITOMO CHEM CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2019044936
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-03-12
Publication Date
2024-10-03
Estimated Expiration
2039-03-12

AI Technical Summary

Technical Problem

Sodium secondary batteries using composite metal oxides as positive electrode active materials have low energy density, limiting their effectiveness in non-aqueous electrolyte secondary batteries.

Method used

A positive electrode active material for sodium secondary batteries is developed, comprising composite metal oxide particles with an O3 type crystal structure, containing Na, Mn, Ti, and Mg, and a carbon layer on the surface, represented by the formula Na a (M 1 w M 2 v Mn x Ti y-z Mg z )O 2, where M 1 represents Co, Ni, or other elements, and a carbon layer is formed on the surface of the active material particles to enhance conductivity.

Benefits of technology

The proposed active material achieves high discharge voltage and capacity, resulting in a sodium secondary battery with improved energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560939000004
    Figure 0007560939000004
  • Figure 0007560939000005
    Figure 0007560939000005
  • Figure 0007560939000006
    Figure 0007560939000006
Patent Text Reader

Abstract

To provide a positive electrode active material for a sodium secondary cell, with which a sodium secondary cell high in both discharge voltage and discharge capacity can be obtained, also to provide a positive electrode for a sodium secondary cell and a sodium secondary cell, which have high performance and in which such a positive electrode active material for a sodium secondary cell is used, and further to provide a positive electrode active material intermediate, with which such a positive electrode active material for a sodium secondary cell can be suitably produced.SOLUTION: A positive electrode active material for a sodium secondary cell includes: an active material particle comprising a composite metal oxide that has an O3-type crystal structure and contains Na, Mn, Ti and Mg; and a carbon layer covering the surface of the active material particle.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a sodium secondary battery, a positive electrode for a sodium secondary battery, a sodium secondary battery, and a positive electrode active material intermediate. [Background technology]

[0002] In recent years, lithium secondary batteries have been put to practical use as secondary batteries, and their applications are expanding. However, lithium, nickel, and cobalt, which are used in lithium secondary batteries, are not abundant resources, and there are concerns that lithium, nickel, and cobalt resources will be depleted in the future.

[0003] On the other hand, sodium, which is also an alkali metal, is more abundant than lithium and is an order of magnitude cheaper than lithium. In addition, sodium has a relatively high standard potential, so it is thought that sodium secondary batteries can become high-capacity secondary batteries.

[0004] If sodium secondary batteries could be used instead of current lithium secondary batteries, it would be possible to mass-produce large secondary batteries, such as in-vehicle secondary batteries and distributed power storage secondary batteries, without having to worry about resource depletion.

[0005] Patent Document 1 and Non-Patent Document 1 disclose that a sodium-containing composite metal oxide represented by NaMnO2 is used as a positive electrode active material. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2006-216509 A [Non-patent literature]

[0007] [Non-Patent Document 1] MRS Bulletin Vol.39, p.416 Komaba et.al. Summary of the Invention [Problem to be solved by the invention]

[0008] However, the sodium secondary batteries using the sodium-containing composite metal oxides of Patent Document 1 and Non-Patent Document 1 as the positive electrode active material have low energy density, and therefore cannot be said to be sufficiently usable for non-aqueous electrolyte secondary batteries.

[0009] It is known that there is a close relationship between the energy density of the sodium secondary battery and the performance of the positive electrode active material for the sodium secondary battery used in the sodium secondary battery. Specifically, when the mass energy density of the positive electrode active material for the sodium secondary battery is high, the mass energy density of the resulting sodium secondary battery is high.

[0010] The mass energy density (unit: mWh / g) of a positive electrode active material is expressed as the product of the discharge voltage and the discharge capacity per unit mass of the positive electrode active material. In this specification, the mass energy density may be simply referred to as "energy density". In order to obtain a positive electrode active material with a high energy density, it has been required to increase the discharge voltage and the discharge capacity.

[0011] The present invention has been made in view of the above circumstances, and aims to provide a positive electrode active material for a sodium secondary battery capable of providing a sodium secondary battery having both high discharge voltage and high discharge capacity. Another aim of the present invention is to provide a high-performance positive electrode for a sodium secondary battery and a sodium secondary battery using such a positive electrode active material for a sodium secondary battery. Another aim of the present invention is to provide a positive electrode active material intermediate capable of suitably producing such a positive electrode active material for a sodium secondary battery. [Means for solving the problem]

[0012] In order to achieve the above object, one embodiment of the present invention includes the following inventions [1] to [8]. [1] A positive electrode active material for a sodium secondary battery, comprising: active material particles made of a composite metal oxide having an O3 type crystal structure and containing Na, Mn, Ti, and Mg; and a carbon layer covering the surfaces of the active material particles.

[0013] [2] The positive electrode active material for a sodium secondary battery according to [1], wherein the composite metal oxide is represented by the following formula (1): Na a (M 1 w M 2 v Mn x Ti y-z Mg z )O2(1) (where M 1 represents Co and Ni, and M 2 represents one or more elements selected from the group consisting of Fe, Cu, Mo, and Ca, a is 0.6 or more and 1 or less, w is 0 or more and less than 0.25, v is 0 or more and less than 0.25, w+v is 0 or more and less than 0.25, x is more than 0 and less than 0.98, y is more than 0.02 and 0.5 or less, z is 0.03 or more and less than 0.5, and w+v+x+y=1, y>z.

[0014] [3] The positive electrode active material for a sodium secondary battery according to [2], wherein w=0.

[0015] [4] A positive electrode for a sodium secondary battery, comprising the positive electrode active material according to any one of [1] to [3].

[0016] [5] A sodium secondary battery having a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the positive electrode has the positive electrode for sodium secondary batteries according to [4].

[0017] [6] A positive electrode active material intermediate having an O3 type crystal structure and consisting of a complex metal oxide containing Na, Mn, Ti, and Mg.

[0018] [7] The positive electrode active material intermediate according to [6], wherein the composite metal oxide is represented by the following formula (1): Na a (M 1 w M 2 v Mn x Ti y-z Mg z )O2(1) (where M 1 represents Co and Ni, and M 2 represents one or more elements selected from the group consisting of Fe, Cu, Mo, and Ca, a is 0.6 or more and 1 or less, w is 0 or more and less than 0.25, v is 0 or more and less than 0.25, w+v is 0 or more and less than 0.25, x is more than 0 and less than 0.98, y is more than 0.02 and 0.5 or less, z is 0.03 or more and less than 0.5, and w+v+x+y=1, y>z.

[0019] [8] The positive electrode active material intermediate according to [7], wherein w=0. Effect of the Invention

[0020] According to the present invention, it is possible to provide a positive electrode active material for a sodium secondary battery capable of providing a sodium secondary battery having both high discharge voltage and high discharge capacity. Also, according to the present invention, it is possible to provide a high-performance positive electrode for a sodium secondary battery and a sodium secondary battery using such a positive electrode active material for a sodium secondary battery. Furthermore, according to the present invention, it is possible to provide a positive electrode active material intermediate capable of suitably producing such a positive electrode active material for a sodium secondary battery. [Brief description of the drawings]

[0021] [Figure 1A] FIG. 1A is a schematic diagram showing an electrode group of a sodium secondary battery. [Figure 1B] FIG. 1B is an exploded perspective view of a sodium secondary battery. [Diagram 2] FIG. 2 is an XRD chart showing the results of powder X-ray diffraction measurement of active material particles 1, 4 and 5. [Diagram 3] FIG. 3 shows charge / discharge curves of positive electrode active materials 1, 4, and 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] <Positive electrode active material for sodium secondary batteries> The positive electrode active material for a sodium secondary battery of this embodiment has an O3 type crystal structure and includes active material particles made of a composite metal oxide containing Na, Mn, Ti, and Mg, and a carbon layer covering the surfaces of the active material particles.

[0023] In the following description, the positive electrode active material for a sodium secondary battery may be simply referred to as the "positive electrode active material".

[0024] In this specification, the "discharge capacity of the positive electrode active material (unit: mAh / g)" refers to the value obtained by dividing the discharge capacity measured for a sodium secondary battery by the mass of the positive electrode active material contained in the positive electrode used in the sodium secondary battery. In other words, the "discharge capacity of the positive electrode active material" refers to the discharge capacity per unit mass of the positive electrode active material.

[0025] In this specification, the "discharge voltage of a positive electrode active material (unit: V)" refers to the discharge voltage measured for a sodium secondary battery.

[0026] (active material particles) The composite metal oxide constituting the active material particles has an O3 type crystal structure, which is represented by a layered rock salt structure. Therefore, when the positive electrode active material for a sodium secondary battery of the present embodiment is used in the positive electrode of a sodium secondary battery, sodium ions are likely to be reversibly inserted and removed from the active material particles in response to charging and discharging of the sodium secondary battery. The active material particles correspond to the "positive electrode active material intermediate" in the present invention.

[0027] In the composite metal oxide constituting the active material particles, some of the sites where tetravalent Ti exists in the crystal are replaced with divalent Mg, as described below. This causes distortion in the crystal structure compared to the crystal of the composite metal oxide not replaced with Mg. Therefore, the composite metal oxide constituting the active material particles ideally has an O3 type crystal structure, but other impurity phases may be mixed in. In the positive electrode active material for sodium secondary batteries of this embodiment, the active material particles may have a crystal structure different from the O3 type, for example, a P2 type and / or P3 type crystal structure, within a range that does not impair the effects of the invention.

[0028] The fact that the active material particles have an O3 type crystal structure can be confirmed by performing powder X-ray diffraction measurement on the positive electrode active material. A known database may be used to identify the crystal structure.

[0029] In XRD (X-ray diffraction) spectra using CuKα radiation, complex metal oxides with an O3 type crystal structure have a characteristically large ratio of the intensity of the diffraction peak at a 2θ angle of approximately 18 degrees, which is due to the stacking direction of the layered crystal structure, to the intensity of the diffraction peak at a 2θ angle of approximately 41 degrees, which is due to the intralayer structure.

[0030] The "diffraction peak at a 2θ angle of about 18 degrees resulting from the structure in the stacking direction of the layered crystal structure" is, for example, a peak corresponding to the 001 or 003 plane. The "diffraction peak at a 2θ angle of about 41 degrees resulting from the structure in the intralayer direction" is, for example, a peak corresponding to the 111 or 104 plane.

[0031] In this embodiment, the crystal structure of the composite metal oxide is measured using a powder X-ray diffraction measuring device RINT2500TTR manufactured by Rigaku Corporation under the following conditions unless otherwise specified.

[0032] X-ray:CuKα Voltage-Current: 40kV-140mA Measurement angle range: 2θ=10~90° Step: 0.02° Scan speed: 4° / min

[0033] The active material particles are preferably a composite metal oxide represented by the following formula (1). When the active material particles are the composite metal oxide, the sodium secondary battery formed using the obtained positive electrode active material has a high discharge voltage and discharge capacity. Therefore, the sodium secondary battery using such a positive electrode active material has a high energy density.

[0034] Na a (M 1 w M 2 v Mn x Ti y-z Mg z )O2(1) (where M 1 represents Co and Ni, and M 2 represents one or more elements selected from the group consisting of Fe, Cu, Mo, and Ca, a is 0.6 or more and 1 or less, w is 0 or more and less than 0.25, v is 0 or more and less than 0.25, w+v is 0 or more and less than 0.25, x is more than 0 and less than 0.98, y is more than 0.02 and 0.5 or less, z is 0.03 or more and less than 0.5, and w+v+x+y=1, y>z.

[0035] In the above formula (1), when a is 0.6 or more, the capacity of a sodium secondary battery formed using the obtained positive electrode material is large and the energy density is high. On the other hand, when a is 1 or less, impurities such as sodium carbonate are unlikely to be mixed into the obtained positive electrode material, and the resistance of the obtained sodium battery is low and the energy density is high.

[0036] In the above formula (1), it is preferable that a is 1 and Na is saturated. When a is 1, the composite metal oxide is likely to have an O3 type crystal structure. Therefore, a sodium secondary battery formed using the obtained positive electrode active material has a large discharge voltage and discharge capacity, and a high energy density.

[0037] In the above formula (1), when x is more than 0 and less than 0.98, the discharge capacity of a sodium secondary battery formed using the obtained positive electrode active material is large.

[0038] In the above formula (1), x is preferably 0.5 or more, more preferably 0.6 or more, and even more preferably 0.7 or more. In addition, in order to increase the discharge capacity of a sodium secondary battery formed using the obtained positive electrode active material, x is preferably 0.95 or less.

[0039] The upper limit and lower limit of x can be combined in any way. In the formula (1), x may be 0.5 or more and less than 0.98, 0.6 or more and less than 0.98, or 0.7 or more and less than 0.98. Also, x may be 0.5 or more and less than 0.95, 0.6 or more and less than 0.95, or 0.7 or more and less than 0.95.

[0040] In the above formula (1), on the premise that y>z, y is greater than 0.02 and is equal to or less than 0.5, and z is equal to or greater than 0.03 and less than 0.5.

[0041] In formula (1), yz represents the molar ratio of Ti. When the molar ratio of Ti in formula (1) is within the range represented by y and z, a sodium secondary battery formed using the obtained positive electrode active material has a high discharge voltage.

[0042] Furthermore, in the positive electrode active material of this embodiment, in the composite metal oxide represented by the above formula (1) constituting the active material particles, a part of Ti is replaced with Mg. That is, in the positive electrode active material of this embodiment, trivalent Mn (Mn 3+ ) is tetravalent Ti(Ti 4+ ) and divalent Mg (Mg 2+ ) has been substituted.

[0043] In the case of such a composition, for example, when Mn is replaced with the same amount of Ti and Mg, the average valence of the replaced Ti and Mg is 3, the same as Mn. Therefore, the crystal structure maintains electrical neutrality as before the replacement, and the structure is difficult to lose Na. As a result, the positive electrode active material of this embodiment can increase the discharge capacity compared to the case where a composite metal oxide substituted with Ti and not substituted with Mg is used for the active material particles.

[0044] In the above formula (1), when z is 0.03 or more and less than 0.5, the discharge capacity of a sodium secondary battery formed using the obtained positive electrode active material is large.

[0045] In the above formula (1), z is preferably 0.05 or more. In order to increase the discharge capacity of a sodium secondary battery formed using the obtained positive electrode active material, z is preferably 0.2 or less, more preferably 0.15 or less, and even more preferably 0.12 or less.

[0046] The upper limit and lower limit of z can be combined in any way. In the formula (1), z may be 0.03 or more and 0.2 or less, 0.03 or more and 0.15 or less, or 0.03 or more and less than 0.12. Also, z may be 0.05 or more and 0.2 or less, 0.05 or more and 0.15 or less, or 0.05 or more and 0.12 or less.

[0047] In the above formula (1), yz is preferably 0.05 or more. In addition, in order to increase the discharge capacity of a sodium secondary battery formed using the obtained positive electrode active material, yz is preferably 0.2 or less, more preferably 0.15 or less, and even more preferably 0.12 or less.

[0048] The upper and lower limits of yz can be combined in any combination. In the above formula (1), yz may be 0.05 or more and 0.2 or less, 0.05 or more and 0.15 or less, or 0.05 or more and 0.12 or less.

[0049] In the above formula (1), yz is preferably equal to or greater than z, and more preferably equal to z.

[0050] In the above formula (1), the optional metal is M 1 In the above formula (1), if w exceeds 0, the discharge capacity may become large. If w is less than 0.25, a composite metal oxide having an O3 type crystal structure is likely to be produced. From the viewpoint of reducing the amount of expensive elements such as nickel and cobalt used, it is preferable that w is 0.

[0051] In the above formula (1), the optional metal is M 2 In the above formula (1), when v exceeds 0, the discharge capacity may become large. When v is less than 0.25, a composite metal oxide having an O3 type crystal structure is likely to be produced.

[0052] In the above formula (1), when w, v, x, and y satisfy w+v+x+y=1, the cycle characteristics of a sodium secondary battery formed using the obtained positive electrode active material for a sodium secondary battery are improved.

[0053] The term "cycle characteristics" refers to the capacity retention rate when the battery is repeatedly charged and discharged. A secondary battery that has a high capacity retention rate when the battery is repeatedly charged and discharged is evaluated as having "good cycle characteristics."

[0054] In the above formula (1), when the relational expression y>z is satisfied, the discharge capacity of a sodium secondary battery formed using the obtained positive electrode active material for a sodium secondary battery is improved.

[0055] (carbon layer) The carbon layer covers the surface of the active material particles and is made of one or more materials selected from the group consisting of natural graphite, artificial graphite, cokes, carbon black, acetylene black, ketjen black, carbon nanotubes (CNTs), and carbon nanofibers (CNFs).

[0056] When preparing a positive electrode using a general positive electrode active material, a method is known in which the positive electrode active material is kneaded with a binder together with a conductive material such as acetylene black to prepare a positive electrode mixture, which is then applied to a current collector. In this case, the positive electrode active material and the conductive material are separated from each other unless they come into contact with each other in the binder during the kneading or application process.

[0057] In contrast, in the positive electrode active material of this embodiment, a carbon layer is provided in advance on the surface of the active material particles made of a composite metal oxide, and contact between the active material particles and the carbon layer is ensured. In a positive electrode active material having such a structure, the conduction between the active material particles is improved. In addition, when the carbon is dispersed in a binder in the positive electrode, the carbon is dispersed more uniformly in the binder. This reduces the resistance between the positive electrode active material and the current collector, improving the conduction. Therefore, the discharge capacity is improved.

[0058] The carbon layer can be formed by mixing the active material particles with a material for forming the carbon layer. The kneading can be performed using a ball mill.

[0059] For example, the carbon layer can be formed by placing 10 g of active material particles, 1 g of acetylene black (manufactured by Denka Co., Ltd.), and 150 g of zirconia balls with a diameter of 5 mm in a 100 mL zirconia bottle, mixing them at 300 rpm for 6 hours using a planetary ball mill, and then sieving out the zirconia balls. The kneading conditions, such as the kneading time and the mixing ratio of the active material particles to the material for forming the carbon layer, should be optimized while checking the physical properties of the positive electrode active material obtained after kneading.

[0060] When a carbon layer is formed on the surface of the active material particles by this method, the particle size of the active material particles is reduced during the carbon layer formation process. Therefore, when the resulting positive electrode active material is dispersed in a binder in a positive electrode, it is dispersed more uniformly in the binder, reducing resistance, and thereby improving discharge capacity.

[0061] (others) The BET specific surface area of ​​the positive electrode active material for a sodium secondary battery of this embodiment is 0.1 m 2 / g or more 5m 2When the BET specific surface area of ​​the positive electrode active material for a sodium secondary battery is within this range, the energy density in particular tends to be high.

[0062] The BET specific surface area of ​​the positive electrode active material for a sodium secondary battery is preferably 0.3 m 2 / g or more, more preferably 0.5m 2 / g or more. The BET specific surface area is preferably 4.5 m 2 / g or less, more preferably 4m 2 / g or less. These upper and lower limit values ​​of the BET specific surface area can be combined in any desired manner.

[0063] When the active material particles of the positive electrode active material for a sodium secondary battery of this embodiment are a composite metal oxide represented by formula (1), in addition to the metals contained in formula (1), metal elements such as Li, K, Ag, Ca, Sr, Ba, Al, Ga, In, V, Cr, Cu, Zn, Sc, Y, Nb, Mo, La, Ce, Pr, Nd, Sm, Eu, Gd, Tb, Ho, Er, Tm, Yb, and Lu may be contained within a range that does not impair the effects of the invention.

[0064] <Method of manufacturing positive electrode active material for sodium secondary battery> The positive electrode active material for a sodium secondary battery of this embodiment can be produced by producing active material particles made of a composite metal oxide, and then forming a carbon layer on the surface of the active material particles.

[0065] (Preparation of active material particles) The active material particles can be produced by firing raw materials having a composition corresponding to the composite metal oxide.

[0066] The raw material for the positive electrode active material is a mixture of metal-containing compounds, which is fired to produce a composite metal oxide having a layered crystal structure.

[0067] Specifically, first, a metal element contained in the composite metal oxide of the target positive electrode active material is prepared as a metal-containing compound containing the metal element.

[0068] Next, the metal-containing compounds are weighed out so as to have a composition corresponding to the metal element ratio in the composite metal oxide contained in the positive electrode active material for a sodium secondary battery, and mixed to obtain a mixture.

[0069] Next, the resulting mixture is fired to obtain active material particles, which are composite metal oxide particles.

[0070] For example, a composite metal oxide having a metal element ratio of Na:Mn:Mg:Ti=1:0.9:0.05:0.05 is preferred as an active material particle. Such a composite metal oxide can be produced by weighing out the raw materials Na2CO3, Mn2O3, Mg(OH)2, and TiO2 so that the molar ratio of Na:Mn:Mn:Ti is 1:0.9:0.05:0.05, mixing them, and firing the resulting mixture.

[0071] Examples of metal-containing compounds used as raw materials for active material particles include oxides, hydroxides, carbonates, nitrates, halides, and oxalates, which are compounds that can be converted into oxides at high temperatures by combining with the oxygen atoms they contain or with oxygen molecules in the atmosphere.

[0072] Examples of the sodium compound among the metal-containing compounds include one or more compounds selected from the group consisting of sodium hydroxide, sodium chloride, sodium nitrate, sodium peroxide, sodium sulfate, sodium bicarbonate, sodium oxalate, and sodium carbonate, and these compounds may be hydrates.

[0073] Among these, sodium carbonate is preferred because it has low hygroscopicity and is easy to handle, while sodium hydroxide is preferred because it has high reactivity at low temperatures and can be calcined at a relatively low calcination temperature, thereby reducing the production cost.

[0074] Among the metal-containing compounds, the manganese compound is preferably either or both of Mn2O3 and MnO2.

[0075] Of the metal-containing compounds, the magnesium compound is preferably either or both of Mg(OH)2 and MgCO3.

[0076] Of the metal-containing compounds, the titanium compound is preferably TiO2.

[0077] These metal-containing compounds may be in the form of hydrates or basic salts.

[0078] Furthermore, among the metal-containing compounds used as raw materials for the active material particles, those obtained by the following coprecipitation method can also be used except for the sodium compound. In the following description, for convenience, the metal-containing compound other than the sodium compound that is obtained by the coprecipitation method is referred to as a "transition metal-containing compound".

[0079] Specifically, first, compounds such as chlorides, nitrates, acetates, formates, oxalates, or sulfates of Mn, Ti, and Mg are dissolved in water to obtain a mixed aqueous solution.

[0080] The aqueous solution can then be contacted with a precipitating agent to obtain a precipitate containing the desired transition metal-containing compound.

[0081] Among the compounds used as the raw material of the transition metal-containing compound, chlorides or sulfates are preferred. In addition, when a compound that is difficult to dissolve in water, such as an oxide, hydroxide, or metal material, is used as the raw material of the transition metal-containing compound, the aqueous solution may be obtained by dissolving the compound in an acid such as hydrochloric acid, sulfuric acid, or nitric acid, or an aqueous solution of the acid.

[0082] Examples of precipitants used in the preparation of the transition metal-containing compound include one or more compounds selected from the group consisting of LiOH (lithium hydroxide), NaOH (sodium hydroxide), KOH (potassium hydroxide), Li2CO3 (lithium carbonate), Na2CO3 (sodium carbonate), K2CO3 (potassium carbonate), (NH4)2CO3 (ammonium carbonate) and (NH2)2CO (urea). Each of these precipitants may be a hydrate, or the compound and a hydrate may be used in combination.

[0083] In addition, these precipitants are preferably dissolved in water and used as an aqueous solution. Hereinafter, the aqueous solution in which the precipitant is dissolved is referred to as an "aqueous precipitant solution."

[0084] The concentration of the precipitant in the aqueous precipitant solution is about 0.5 mol / L to 10 mol / L, preferably 1 mol / L to 8 mol / L. The precipitant is preferably KOH or NaOH, and the aqueous precipitant solution is preferably a KOH aqueous solution or a NaOH aqueous solution. The aqueous precipitant solution may also include ammonia water. Ammonia water may be used in combination with other aqueous precipitant solutions.

[0085] Examples of the method for contacting the mixed aqueous solution with a precipitant include (1) a method of adding either or both of a precipitant or a precipitant aqueous solution to the mixed aqueous solution, (2) a method of adding the mixed aqueous solution to a precipitant aqueous solution, and (3) a method of adding the mixed aqueous solution and either or both of a precipitant or a precipitant aqueous solution to water.

[0086] In the methods (1) to (3), it is preferable to use stirring. Among the above methods, the method (2) of adding the mixed aqueous solution to the precipitant aqueous solution is preferable. According to this method, it is easy to maintain the pH of the precipitant aqueous solution during the operation, and it is easy to control the particle size of the obtained precipitate. In the method (2), the pH tends to decrease as the mixed aqueous solution is added to the precipitant aqueous solution, but it is preferable to add the mixed aqueous solution while adjusting the pH to 9 or more, preferably 10 or more. The pH can be adjusted by adding the precipitant aqueous solution.

[0087] In the coprecipitation methods according to (1) to (3), the atmosphere during operation is preferably nitrogen or argon in order to suppress the formation of impurities.

[0088] A precipitate containing a transition metal-containing compound can be prepared by the above methods (1) to (3).

[0089] When the mixed aqueous solution and the precipitant are mixed, a slurry containing a precipitate is obtained. The obtained slurry is subjected to solid-liquid separation, and the precipitate is collected to obtain a precipitate containing a transition metal-containing compound. The solid-liquid separation may be performed by any method. Since the operation is easy, solid-liquid separation such as filtration is preferable. In addition, a method of volatilizing the liquid content from the slurry, such as heat drying, air drying, vacuum drying, or spray drying, may be used.

[0090] The collected precipitate may be washed with a washing liquid and then dried. The precipitate obtained after solid-liquid separation may have an excessive amount of precipitant attached thereto, but the amount of the attached precipitant can be reduced by washing. The washing liquid used for washing is preferably water, or a water-soluble organic solvent such as alcohol or acetone, more preferably water.

[0091] Examples of the method for drying the precipitate include heat drying, air drying, vacuum drying, etc. Heat drying is preferably performed at a temperature of 50° C. or higher and 300° C. or lower, more preferably 100° C. or higher and 200° C. or lower.

[0092] These washing and drying steps may be carried out two or more times, with the washing with a washing solution and the drying of the precipitate counted as one time.

[0093] In the mixing of sodium compounds, manganese compounds, titanium compounds and magnesium compounds, or the mixing of sodium compounds and transition metal-containing compounds, examples of the mixing method include dry mixing and wet mixing. Among them, dry mixing is preferred because of its simple operation. Examples of the mixing device include a stirring mixer, a V-type mixer, a W-type mixer, a ribbon mixer, a drum mixer and a ball mill.

[0094] The mixture obtained by the above method is fired to obtain active material particles made of a composite metal oxide. The firing temperature of the mixture depends on the type of sodium compound used and can be appropriately determined.

[0095] The firing temperature is preferably from 400°C to 1200°C, and more preferably from 500°C to 1100°C.

[0096] The time for which the firing temperature is maintained is preferably from 0.1 to 24 hours, more preferably from 0.5 to 20 hours.

[0097] The rate of temperature rise to the firing temperature is preferably 50° C. / hour to 400° C. / hour, and the rate of temperature drop from the firing temperature to room temperature is preferably 10° C. / hour to 400° C. / hour.

[0098] Examples of the atmosphere during firing include air, oxygen, nitrogen, argon, or a mixed gas thereof. From the viewpoint of ease of controlling the atmosphere, air is preferred, and from the viewpoint of stability of the sample after firing, oxygen, nitrogen, argon, or a mixed gas thereof is preferred.

[0099] By using an appropriate amount of a halide such as a fluoride or chloride as the metal-containing compound, the crystallinity of the resulting composite metal oxide and the average particle size of the particles constituting the composite metal oxide can be controlled.

[0100] In addition, a suitable amount of a reaction accelerator (flux) may be added to the mixture during firing. Examples of the flux include NaF, MnF3, FeF2, NiF2, CoF2, NaCl, MnCl2, FeCl2, FeCl3, NiCl2, CoCl2, Na2CO3, NaHCO3, NH4Cl, NHI, B2O3, and H3BO3. Metal-containing compounds such as halides may also function as reaction accelerators (fluxes). These fluxes may be hydrates.

[0101] The product (composite metal oxide) obtained by the above-mentioned calcination may be pulverized, washed, or classified using an industrially commonly used device such as a ball mill, a jet mill, or a vibration mill. By these operations, the particle size of the active material particles may be adjusted. Calcination may be performed two or more times.

[0102] The surfaces of the obtained active material particles may be subjected to a surface treatment such as coating with an inorganic substance containing Si, Al, Ti, Y or the like.

[0103] Furthermore, after this surface treatment, a heat treatment may be performed. Depending on the temperature of the heat treatment, the BET specific surface area of ​​the particles after the heat treatment may change from the BET specific surface area of ​​the compound before the heat treatment. Therefore, it is also possible to adjust the BET specific surface area of ​​the active material particles by the heat treatment.

[0104] (Formation of carbonized layer) Next, the active material particles obtained as described above are mixed with a material for forming a carbon layer to form a carbon layer on the surface of the active material particles. For example, the carbon layer can be formed by sealing 10 g of active material particles, 1 g of acetylene black (manufactured by Denka Co., Ltd.) and 150 g of zirconia balls with a diameter of 5 mm in a 100 mL zirconia bottle, mixing them at 300 rpm for 6 hours using a planetary ball mill device, and then sieving out the zirconia balls.

[0105] By using the above-mentioned positive electrode active material for a sodium secondary battery as the positive electrode active material of a sodium secondary battery, a sodium secondary battery having both a higher discharge voltage and a higher discharge capacity than conventional batteries can be obtained.

[0106] <Positive electrode for sodium secondary battery and method for producing same> The positive electrode for a sodium secondary battery of this embodiment contains the positive electrode active material of this embodiment described above. The positive electrode for a sodium secondary battery can be manufactured by supporting a positive electrode mixture containing a positive electrode active material and a binder on a positive electrode current collector. A conductive material may be further added to the positive electrode mixture.

[0107] Examples of the conductive material include carbon materials such as natural graphite, artificial graphite, cokes, and carbon black.

[0108] The binder may be a thermoplastic resin. Specific examples of the thermoplastic resin include fluororesins such as polyvinylidene fluoride (hereinafter sometimes referred to as PVDF), polytetrafluoroethylene (hereinafter sometimes referred to as PTFE), tetrafluoroethylene-hexafluoropropylene-vinylidene fluoride copolymers, hexafluoropropylene-vinylidene fluoride copolymers, and tetrafluoroethylene-perfluorovinyl ether copolymers; and polyolefin resins such as polyethylene and polypropylene. Two or more of these may be used.

[0109] Examples of the positive electrode current collector include Al, Ni, stainless steel, etc. Al is preferred because it is easy to process into a thin film and is inexpensive. Examples of the shape of the positive electrode current collector include foil, plate, mesh, net, lath, and punched shapes, as well as combinations of these (e.g., mesh-shaped plate, etc.). The surface of the positive electrode current collector may be unevenly formed by etching or embossing.

[0110] An example of a method for supporting the positive electrode mixture on the positive electrode current collector is a method in which the positive electrode mixture is fixed to the current collector by pressure molding.

[0111] Alternatively, a method may be adopted in which an organic solvent is further added to the positive electrode mixture to form a positive electrode mixture paste, and the positive electrode mixture paste is applied to a positive electrode current collector and dried to fix the positive electrode mixture to the positive electrode current collector. In this method, the positive electrode mixture may be firmly fixed to the positive electrode current collector by pressing a sheet obtained by fixing the positive electrode mixture to the positive electrode current collector.

[0112] Examples of the organic solvent used in the positive electrode mixture paste include amine-based solvents such as N,N-dimethylaminopropylamine and diethylenetriamine; ether-based solvents such as tetrahydrofuran; ketone-based solvents such as methyl ethyl ketone; ester-based solvents such as methyl acetate; and amide-based solvents such as dimethylacetamide and N-methyl-2-pyrrolidone (hereinafter sometimes referred to as NMP).

[0113] The kneading method for preparing the positive electrode mixture paste is not particularly limited, but the mixer used for kneading is preferably one having a high shear force, specifically, a planetary mixer, a kneader, an extrusion type kneader, a thin film rotary type high speed mixer, etc.

[0114] In terms of the mixing order, the positive electrode active material, the conductive material, the binder, and the solvent may be mixed all at once, or the binder, the positive electrode active material, and the conductive material may be mixed in this order into the solvent. This order is not particularly limited, and the mixture of the positive electrode active material and the conductive material may be added gradually. In addition, the solvent and the binder may be mixed and dissolved in advance.

[0115] Examples of methods for applying the positive electrode mixture paste to the positive electrode current collector include slit die coating, screen coating, curtain coating, knife coating, gravure coating, and electrostatic spraying. In this manner, the positive electrode of the present embodiment can be manufactured.

[0116] The positive electrode for a sodium secondary battery having the above-mentioned configuration contains the positive electrode active material for a sodium secondary battery of the present embodiment described above, and therefore, when used in the production of a sodium secondary battery, it is possible to provide a sodium secondary battery having both high discharge voltage and high discharge capacity.

[0117] <Sodium secondary battery> The sodium secondary battery of this embodiment has the positive electrode, negative electrode, and non-aqueous electrolyte of this embodiment described above.

[0118] (Negative electrode) The negative electrode can be doped with sodium ions and dedoped at a lower potential than the positive electrode. The negative electrode can be an electrode in which a negative electrode mixture containing a negative electrode material is supported on a negative electrode current collector, or an electrode made of a negative electrode material alone. The negative electrode material can be a carbon material, a chalcogen compound (oxide, sulfide, etc.), a nitride, a metal, or an alloy, which can be doped with sodium ions and dedoped at a lower potential than the positive electrode. These negative electrode materials may be mixed.

[0119] Specific examples of negative electrode materials are shown below. Specific examples of carbon materials include graphite such as natural graphite and artificial graphite, cokes, carbon black, pyrolytic carbons, carbon fibers, polymer sinters, and the like, which can be doped with sodium ions and dedoped at a potential lower than that of the positive electrode. These carbon materials, oxides, sulfides, and nitrides may be used in combination and may be either crystalline or amorphous. These carbon materials, oxides, sulfides, and nitrides are mainly supported on a negative electrode current collector and used as a negative electrode. Specific examples of metals include sodium metal, silicon metal, and tin metal. Examples of alloys include sodium alloys such as Na-Al, Na-Ni, and Na-Si; silicon alloys such as Si-Zn; tin alloys such as Sn-Mn, Sn-Co, Sn-Ni, Sn-Cu, and Sn-La; and alloys such as Cu2Sb and La3Ni2Sn7. These metals and alloys are mainly used alone as electrodes (for example, in the form of foil). Further examples of oxides include Li4Ti5O12 and the like oxides.

[0120] The negative electrode mixture may contain a binder as necessary. Examples of the binder include thermoplastic resins. Specific examples of the thermoplastic resin include PVDF, thermoplastic polyimide, carboxymethyl cellulose, polyethylene, and polypropylene. When the electrolyte does not contain ethylene carbonate, which will be described later, and the negative electrode mixture contains polyethylene carbonate, the cycle characteristics and large current discharge characteristics of the resulting battery may be improved.

[0121] Examples of the negative electrode current collector include Cu, Ni, stainless steel, and Al. Cu or Al is preferable because it is difficult to form an alloy with sodium and is easy to process into a thin film. The method of supporting the negative electrode current collector with the negative electrode mixture includes a pressure molding method similar to that of the positive electrode; a method of obtaining a negative electrode mixture paste by further using an organic solvent, applying the paste to the negative electrode current collector, drying the paste to obtain a sheet, and pressing the obtained sheet to fix the negative electrode mixture to the current collector.

[0122] (Non-aqueous electrolyte) Examples of non-aqueous electrolytes that can be used in the sodium secondary battery of this embodiment include NaClO4, NaPF6, NaAsF6, NaSbF6, NaBF4, NaCF3SO3, NaN(SO2CF3)2, lower aliphatic carboxylic acid sodium salts, and NaAlCl4. A mixture of two or more of these may be used. The electrolyte preferably contains at least one fluorine-containing sodium salt selected from the group consisting of NaPF6, NaAsF6, NaSbF6, NaBF4, NaCF3SO3, and NaN(SO2CF3)2. The non-aqueous electrolyte can be dissolved in an organic solvent and used as a non-aqueous electrolytic solution.

[0123] Examples of the organic solvent in the nonaqueous electrolyte include: Carbonates such as propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, isopropyl methyl carbonate, vinylene carbonate, 4-trifluoromethyl-1,3-dioxolan-2-one, and 1,2-di(methoxycarbonyloxy)ethane; Ethers such as 1,2-dimethoxyethane, 1,3-dimethoxypropane, pentafluoropropyl methyl ether, 2,2,3,3-tetrafluoropropyl difluoromethyl ether, tetrahydrofuran, and 2-methyltetrahydrofuran; Esters such as methyl formate, methyl acetate, and gamma-butyrolactone; Nitriles such as acetonitrile and butyronitrile; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; Carbamates such as 3-methyl-2-oxazolidone; Sulfur-containing compounds such as sulfolane, dimethyl sulfoxide, and 1,3-propane sultone; It is also possible to use an organic solvent having a fluorine substituent, which is obtained by further introducing a fluorine substituent into the above organic solvent.

[0124] A part of the organic solvent in the non-aqueous electrolyte preferably contains an organic solvent having a fluorine substituent.

[0125] Examples of organic solvents having a fluorine substituent include 4-fluoro-1,3-dioxolan-2-one (hereinafter sometimes referred to as FEC or fluoroethylene carbonate), trans- or cis-4,5-difluoro-1,3-dioxolan-2-one (hereinafter sometimes referred to as DFEC or difluoroethylene carbonate), and the like.

[0126] The organic solvent having a fluorine substituent is preferably 4-fluoro-1,3-dioxolan-2-one.

[0127] These organic solvents having fluorine substituents may be used alone, but are preferably used as a mixed solvent in combination with an organic solvent having no fluorine substituent.When the organic solvent in the non-aqueous electrolyte contains an organic solvent having fluorine substituents, the ratio of the organic solvent having fluorine substituents to the entire non-aqueous electrolyte is in the range of 0.01% by volume or more and 10% by volume or less, preferably 0.1% by volume or more and 8% by volume or less, more preferably 0.5% by volume or more and 5% by volume or less.

[0128] The above-mentioned nonaqueous electrolyte may be used in a state in which the nonaqueous electrolytic solution is held in a polymer compound, that is, in the form of a gel electrolyte.

[0129] In addition, as the non-aqueous electrolyte that can be used in the sodium secondary battery of this embodiment, a solid electrolyte can also be used.

[0130] As the solid electrolyte, for example, a polymer electrolyte such as a polyethylene oxide-based polymer compound, a polymer compound containing at least one of a polyorganosiloxane chain or a polyoxyalkylene chain can be used. In addition, if a sulfide electrolyte such as Na2S-SiS2, Na2S-GeS2, Na2S-P2S5, or Na2S-B2S3, or an inorganic compound electrolyte containing a sulfide such as Na2S-SiS2-Na3PO4 or Na2S-SiS2-Na2SO4, or a NASICON-type electrolyte such as NaZr2(PO4)3 is used as the solid electrolyte, safety may be further improved.

[0131] In the sodium secondary battery of the present embodiment, when a solid electrolyte is used, the solid electrolyte may also function as a separator, which will be described later. In that case, the separator may not be necessary.

[0132] (Separator) The sodium secondary battery of the present embodiment may have a separator disposed between the positive electrode and the negative electrode. Examples of the form of the separator include a porous film, a nonwoven fabric, and a woven fabric.

[0133] Examples of materials for forming the separator include polyolefin resins such as polyethylene and polypropylene, fluororesins, nitrogen-containing aromatic polymers, etc. Furthermore, a single-layer or laminated separator using two or more of these materials may be used.

[0134] Examples of the separator include those described in JP-A-2000-30686 and JP-A-10-324758.

[0135] The thickness of the separator is preferably as thin as possible while maintaining mechanical strength, in order to increase the volumetric energy density of the battery and reduce the internal resistance. The thickness of the separator is generally preferably 5 μm to 200 μm, more preferably 5 μm to 40 μm.

[0136] The separator preferably has a porous film containing a thermoplastic resin. In a sodium secondary battery, when an abnormal current flows in the battery due to a short circuit between the positive electrode and the negative electrode, it is preferable to cut off the current and prevent an excessive current from flowing (shutdown).

[0137] When the separator has a porous film containing a thermoplastic resin, shutdown occurs when the separator at the short-circuited portion is overheated by a short circuit and exceeds a previously assumed (normal) use temperature, causing the porous film in the separator to soften or melt and block the micropores. It is preferable that the separator has high heat resistance so that it can maintain the shutdown state without being broken by the temperature even if the temperature inside the battery rises to a certain high temperature after shutdown.

[0138] By using a separator made of a laminated porous film in which a heat-resistant porous layer containing a heat-resistant resin and a porous film containing a thermoplastic resin are laminated as the separator, it becomes possible to more effectively prevent thermal breakage of the film. Here, the heat-resistant porous layer may be laminated on both sides of the porous film.

[0139] (Manufacturing method of sodium secondary battery) 1A and 1B are schematic diagrams showing an example of a sodium secondary battery of this embodiment. Fig. 1A is a schematic diagram showing an electrode group of the sodium secondary battery. Fig. 1B is an exploded perspective view of the sodium secondary battery. The cylindrical sodium secondary battery 10 of this embodiment is manufactured as follows.

[0140] First, as shown in FIG. 1A, a pair of strip-shaped separators 1, a strip-shaped positive electrode 2 having a lead 21 at one end, and a strip-shaped negative electrode 3 having a lead 31 at one end are laminated in the order of separator 1, positive electrode 2, separator 1, and negative electrode 3, and then wound to form an electrode group 4.

[0141] 1B, an electrode group 4 and an insulator (not shown) are housed in a battery can 5, the bottom of the can is sealed, the electrode group 4 is impregnated with an electrolyte solution 6, and the electrolyte is disposed between the positive electrode 2 and the negative electrode 3. Furthermore, the top of the battery can 5 is sealed with a top insulator 7 and a sealing body 8, whereby a sodium secondary battery 10 can be manufactured.

[0142] Examples of the shape of the electrode group 4 include a columnar shape such that the cross-sectional shape when the electrode group 4 is cut perpendicular to the winding axis is a circle, an ellipse, a rectangle, or a rectangle with rounded corners.

[0143] The shape of a sodium secondary battery having such an electrode group 4 can be any shape defined by IEC60086, which is a standard for batteries defined by the International Electrotechnical Commission (IEC), or JIS C 8500. For example, cylindrical or rectangular shapes can be used.

[0144] Furthermore, the sodium secondary battery is not limited to the above-mentioned wound type configuration, and may be a laminated type configuration in which a laminated structure of a positive electrode, a separator, a negative electrode, and a separator is repeatedly stacked. Examples of the laminated type sodium secondary battery include so-called coin type batteries, button type batteries, and paper type (or sheet type) batteries.

[0145] The sodium secondary battery having the above-mentioned configuration has the positive electrode for a sodium secondary battery of the present embodiment described above, and therefore has high discharge voltage and high discharge capacity.

[0146] <Applications of sodium secondary batteries> The sodium secondary battery of the present embodiment has both high discharge voltage and high discharge capacity and high energy density, and is therefore suitable as a small battery that is a power source for small devices such as mobile phones, portable audio devices, and laptop computers; a power source for transportation devices such as automobiles, motorcycles, electric chairs, forklifts, trains, airplanes, ships, spacecraft, and submarines; a power source for machines such as tillers; an outdoor power source for camping purposes; and a medium- to large-sized battery that is a mobile battery such as an outdoor / indoor power source for vending machines.

[0147] In addition, since the sodium secondary battery of this embodiment uses inexpensive raw materials which are in abundant supply, it is suitable as a medium- to large-sized battery that is a stationary battery such as an outdoor / indoor installed power source for factories, homes, etc.; a load-leveling power source for various power generation such as a solar battery charger and a wind power generation charger; an installed power source for low-temperature environments such as inside a refrigerated or frozen warehouse and in extremely cold regions; an installed power source for high-temperature environments such as a desert; and an installed power source for a space environment such as a space station.

[0148] Although the preferred embodiment of the present invention has been described above with reference to the attached drawings, it goes without saying that the present invention is not limited to the above embodiment. The shapes and combinations of the components shown in the above embodiment are merely examples, and various modifications can be made based on design requirements, etc., without departing from the spirit of the present invention. EXAMPLES

[0149] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples unless the gist of the present invention is changed.

[0150] <Evaluation method> In this example, the produced composite metal oxide was measured by the following method. In addition, a sodium secondary battery was produced by using the produced positive electrode active material by the following method and evaluated.

[0151] (1) Powder X-ray diffraction measurement The crystal structure of the composite metal oxide was measured using a powder X-ray diffraction measuring device RINT2500TTR manufactured by Rigaku Corporation under the following conditions unless otherwise specified.

[0152] X-ray:CuKα Voltage-Current: 40kV-140mA Measurement angle range: 2θ=10~90° Step: 0.02° Scan speed: 4° / min

[0153] (2) Preparation of the positive electrode For Examples 1 and 2 and Comparative Examples 2 and 3 produced by the methods described below, the positive electrode active material, acetylene black (manufactured by Denka Co., Ltd.) as a conductive material, and PVDF (manufactured by Kureha Co., Ltd.) as a binder were weighed out so as to achieve a composition of positive electrode active material:conductive material:binder = 85:5:10 (mass ratio). For Comparative Example 1 produced by the method described below, the positive electrode active material, acetylene black (manufactured by Denka Co., Ltd.) as a conductive material, and PVDF (manufactured by Kureha Co., Ltd.) as a binder were weighed out to achieve a composition of positive electrode active material:conductive material:binder = 80:10:10 (mass ratio). Thereafter, the positive electrode active material and acetylene black were first thoroughly mixed in an agate mortar, N-methyl-2-pyrrolidone (NMP: manufactured by Tokyo Chemical Industry Co., Ltd.) was added to this mixture, and then PVDF was added and mixed in the agate mortar until homogenous, thereby obtaining a positive electrode mixture paste.

[0154] The obtained positive electrode mixture paste was applied to a thickness of 100 μm on a 40 μm thick aluminum foil current collector using an applicator. The current collector coated with the positive electrode mixture paste was placed in a dryer and dried while removing NMP to obtain an electrode sheet. This electrode sheet was punched out to a diameter of 1.5 cm using an electrode punching machine, and then pressed with a hand press to obtain a positive electrode containing a positive electrode active material.

[0155] (3) Battery construction The above-mentioned positive electrode was placed with the aluminum foil facing down in the recess of the lower part of a coin cell (manufactured by Hosen Co., Ltd.), and a sodium secondary battery was produced by combining this with 1M NaPF6 / propylene carbonate as an electrolyte, a polypropylene porous film (thickness 20 μm) as a separator, and metallic sodium (manufactured by Aldrich Co.) as a negative electrode. The battery was assembled in a glove box with an argon atmosphere.

[0156] <Example 1> (Na:Mn:Ti:Mg=1:0.9:0.05:0.05) As metal-containing compounds, sodium carbonate (Na2CO3: manufactured by Wako Pure Chemical Industries, Ltd., purity 99.8%), manganese oxide (IV) (MnO2: manufactured by Kojundo Chemical Laboratory Co., Ltd., purity 99.9%), titanium oxide (TiO2: manufactured by Kojundo Chemical Laboratory Co., Ltd., purity 99.9%) and magnesium hydroxide (Mg(OH)2: manufactured by Wako Pure Chemical Industries, Ltd., purity 99.8%) were used and weighed out so that the molar ratio of Na:Mn:Ti:Mg was 1.00:0.90:0.05:0.05. The mixture was mixed in a wet ball mill at 300 rpm for 5 hours to obtain a mixture of metal-containing compounds.

[0157] The obtained mixture of metal-containing compounds was subjected to solid-liquid separation, and the wet cake was dried and then placed in a mold to form pellets. The obtained pellets were then placed on an alumina firing boat and fired in an argon atmosphere at 1000°C for 10 hours using an electric furnace. After firing the mixture, the fired product was cooled to room temperature to obtain active material particles 1, which are composite metal oxide particles. The active material particles 1 correspond to the "positive electrode active material" of the present invention.

[0158] Fig. 2 is an XRD chart showing the results of powder X-ray diffraction measurement of active material particle 1 and the later-described active materials 4 and 5. Fig. 2 shows XRD charts in the range of 10° to 100° from the measurement results in the above-mentioned measurement angle range.

[0159] As a result of powder X-ray diffraction measurement, it was found that the crystal structure of active material particle 1 belongs to the O3 type crystal structure, which is one of the layered types.

[0160] Next, 10 g of active material particles, 1 g of acetylene black (manufactured by Denka Co., Ltd.), and 150 g of zirconia balls having a diameter of 5 mm were placed in a 100 mL zirconia bottle and mixed at 300 rpm for 6 hours using a planetary ball mill. The zirconia balls were then sieved out to obtain positive electrode active material 1 in which a carbon layer was formed on the surface of the active material particles.

[0161] Example 2 (Na:Mn:Ti:Mg=1:0.8:0.1:0.1) Active material particles 2, which are composite metal oxide particles, were obtained in the same manner as in Example 1, except that the metal-containing compound was used in an amount such that the molar ratio of Na:Mn:Ti:Mg was 1.00:0.80:0.10:0.10.

[0162] As a result of powder X-ray diffraction measurement, it was found that the crystal structure of active material particle 2 belongs to an O3 type crystal structure, which is one of the layered types.

[0163] Furthermore, a positive electrode active material 2 was obtained in the same manner as in Example 1, except that active material particles 2 were used.

[0164] Comparative Example 1 (Na:Mn=0.7:1.0) Composite metal oxide particles were obtained in the same manner as in Example 1, except that no TiO2 source or Mg(OH)2 source was used, and a metal-containing compound was used in an amount such that the molar ratio of Na:Mn was 0.70:1.00. In Comparative Example 1, the composite metal oxide particles were used as positive electrode active material 3.

[0165] As a result of powder X-ray diffraction measurement, it was found that the crystal structure of the positive electrode active material 3 belongs to a P2 type crystal structure, which is one of the layered types.

[0166] Comparative Example 2 (Na:Mn=1:1) Active material particles 4, which are composite metal oxide particles, were obtained in the same manner as in Example 1, except that no TiO2 source or Mg(OH)2 source was used, and a metal-containing compound was used in an amount such that the molar ratio of Na:Mn was 1.00:1.00.

[0167] As shown in FIG. 2, the results of powder X-ray diffraction measurement showed that the crystal structure of active material particle 4 belongs to an O3 type crystal structure, which is one of the layered types.

[0168] As a result of powder X-ray diffraction measurement, it was found that the crystal structure of the positive electrode active material 4 belongs to an O3 type crystal structure, which is one of the layered types.

[0169] Furthermore, a positive electrode active material 4 was obtained in the same manner as in Example 1, except that active material particles 4 were used.

[0170] <Comparative example 3> (Na:Mn:Ti=0.8:0.8:0.2) Active material particles 5, which are composite metal oxide particles, were obtained in the same manner as in Example 1, except that no Mg(OH)2 was used as the Mg source, and a metal-containing compound was used in an amount such that the molar ratio of Na:Mn:Ti was 0.80:0.80:0.20.

[0171] As shown in FIG. 2, the results of powder X-ray diffraction measurement showed that the crystal structure of active material particle 5 belongs to an O3 type crystal structure, which is one of the layered types.

[0172] Furthermore, a positive electrode active material 5 was obtained in the same manner as in Example 1, except that active material particles 5 were used.

[0173] <Evaluation of sodium secondary batteries> The sodium secondary batteries using the positive electrode active materials of Examples 1 and 2 and Comparative Examples 1 to 3 were evaluated as follows.

[0174] (10 times discharge capacity) The prepared battery was subjected to a charge / discharge test under the following conditions: When repeated charge / discharge was performed in the cycle test, charging and discharging were repeated under the following conditions. Charging conditions: CC (constant current) charging was performed from the rest potential to 4.5V at a rate of 0.2C (a rate that fully charges the battery in 5 hours). Discharge conditions: CC (constant current) discharge was performed at a rate of 0.2C (a rate at which the battery is completely discharged in 5 hours), and the voltage was cut off at 1.0V.

[0175] Each charge and discharge under the above conditions was counted as one cycle, and the tenth charge and discharge cycle was performed, after which the tenth discharge capacity was measured. The obtained value was taken as the tenth discharge capacity.

[0176] (Average discharge voltage) The charging and discharging were performed under the above conditions, and the voltage during discharging was measured. The charging and discharging were repeated 10 times, and the voltage during discharging was measured 10 times. The arithmetic mean value of the obtained discharge voltages was taken as the average discharge voltage.

[0177] The evaluation results are shown in Tables 1 and 2 and Fig. 3. Fig. 3 shows the charge / discharge curves of positive electrode active materials 2, 4, and 5.

[0178] [Table 1]

[0179] In the table, "Mn ratio," "Ti ratio," and "Mg ratio" respectively indicate the molar ratio of each element per mole of the composition formula of the composite metal oxide that constitutes the active material particles.

[0180] [Table 2]

[0181] As for Comparative Example 1, as described above, the crystal structure is of P2 type, and there is a problem in comparing the 10-cycle discharge capacity, so it is not shown.

[0182] As a result of the evaluation, the sodium secondary batteries using the positive electrode active materials of Examples 1 and 2 exhibited higher 10-cycle discharge capacity and average discharge voltage than the sodium secondary batteries using the positive electrode active materials of Comparative Examples 1 to 3.

[0183] The positive electrode active material of Example 1 had an initial Coulombic efficiency (=discharge capacity / charge capacity×100(%)) of about 94%, and it was confirmed that the positive electrode active material of Example 1 is highly practical as a positive electrode material for secondary batteries.

[0184] <Effect of carbon layer> (Reference example 1) A sodium secondary battery having active material particle 1 as a positive electrode active material was prepared in the same manner as in the above "(2) Preparation of positive electrode" and "(3) Preparation of battery", except that active material particle 1 was used instead of positive electrode active material 1.

[0185] (Reference example 2) A sodium secondary battery having active material particles 2 as a positive electrode active material was prepared in the same manner as in “(2) Preparation of positive electrode” and “(3) Preparation of battery” above, except that active material particles 2 were used instead of positive electrode active material 2.

[0186] <Evaluation of sodium secondary batteries> The sodium secondary batteries using the positive electrode active materials of Examples 1 and 2 and the sodium secondary batteries using the active material particles of Reference Examples 1 and 2 as the positive electrode active material were evaluated as follows.

[0187] (Initial discharge capacity) The produced battery was charged and discharged under the above-mentioned conditions, and the discharge capacity at the first discharge was measured as the first discharge capacity.

[0188] The evaluation results are shown in Table 3.

[0189] [Table 3]

[0190] As shown in Table 3, it was found that the active material particles 1 and 2 used in Reference Examples 1 and 2 functioned as active material particles for a sodium secondary battery, respectively.

[0191] Furthermore, when the results of Reference Examples 1 and 2 are compared with the results of Examples 1 and 2, it is found that the initial discharge capacity increases when a carbon layer is provided.

[0192] These results confirmed the usefulness of the present invention. [Explanation of symbols]

[0193] 1...separator, 2...positive electrode, 3...negative electrode, 4...electrode group, 5...battery can, 6...electrolyte, 7...top insulator, 8...sealing body, 10...sodium secondary battery, 21...lead, 31...lead

Claims

1. active material particles made of a composite metal oxide having an O3 type crystal structure and containing Na, Mn, Ti and Mg; a carbon layer covering the surface of the active material particle; The carbon layer is formed of acetylene black, The composite metal oxide is a positive electrode active material for a sodium secondary battery represented by the following formula (1). Yes a (M) 1 w M 2 v Mn x Three y-z Mẹ z )O 2 (1) (Here, M 1 represents Co or Ni; M 2 represents one or more elements selected from the group consisting of Fe, Cu, Mo, and Ca, a is 0.6 or more and 1 or less, w is 0 or more and less than 0.25, v is 0 or more and less than 0.25, w+v is 0 or more and less than 0.25, x is 0.7 or more and less than 0.98, y is more than 0.02 and 0.5 or less, z is 0.03 or more and less than 0.5, and w+v+x+y=1, y>z.

2. 2. The positive electrode active material for a sodium secondary battery according to claim 1, wherein w=0.

3. A positive electrode active material for a sodium secondary battery as described in claim 2, wherein v = 0.

4. A positive electrode for a sodium secondary battery, comprising the positive electrode active material according to claim 1 .

5. A sodium secondary battery having a positive electrode, a negative electrode and a non-aqueous electrolyte, wherein the positive electrode has the positive electrode for sodium secondary batteries according to claim 4.

Citation Information

Patent Citations

  • Positive electrode and nonaqueous electrolyte secondary battery using the same

    JP2006216509A

  • Layered oxide materials for batteries

    US20170025678A1