Method for manufacturing conductive film, and corona discharge treated conductive film

Corona discharge treatment effectively reduces the volume resistivity of conductive films made from polypropylene polymer and metal fillers, achieving low resistivity and improved surface properties.

JP7561055B2Active Publication Date: 2024-10-03GUNZE LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021025007
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-19
Publication Date
2024-10-03
Estimated Expiration
2041-02-19

AI Technical Summary

Technical Problem

Existing methods for manufacturing conductive films, such as those containing polypropylene polymer and conductive metal fillers, do not effectively reduce volume resistivity.

Method used

Applying corona discharge treatment to conductive films composed of polypropylene polymer and conductive metal fillers, using a roller-shaped electrode and a discharge electrode to generate corona discharge, with a controlled discharge amount to reduce volume resistivity.

Benefits of technology

The corona discharge treatment results in conductive films with reduced volume resistivity and a contact angle of water of 110 degrees or less, achieving a volume resistivity of 1200 Ω·cm or less.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007561055000003
    Figure 0007561055000003
  • Figure 0007561055000004
    Figure 0007561055000004
  • Figure 0007561055000005
    Figure 0007561055000005
Patent Text Reader

Abstract

To provide a method for producing a conductive film and the like that allows reduction in volume resistivity.SOLUTION: The present invention discloses a method for producing a conductive film that is composed of a resin composition containing a polypropylene polymer and a conductive metal filler. The production method includes the steps of: using a resin composition to make a conductive film; and subjecting the conductive film to a corona discharge treatment, causing reduction in the volume resistivity of the conductive film.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a conductive film and a corona discharge-treated conductive film. [Background technology]

[0002] JP 2014-91248 A (Patent Document 1) discloses a method for producing a conductive film. This conductive film is produced by using a resin composition containing a thermoplastic resin and a conductive filler. In this production method, the resin composition extruded from a T-die is conveyed backward by a roller to produce the conductive film. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2014-91248 A Summary of the Invention [Problem to be solved by the invention]

[0004] For example, in a conductive film made of a resin composition containing a polypropylene-based polymer and a conductive metal filler, it is required to reduce the volume resistivity of the conductive film. However, the above-mentioned Patent Document 1 does not disclose a technique for reducing the volume resistivity.

[0005] The present invention has been made to solve such problems, and its object is to provide a method for producing a conductive film that can reduce the volume resistivity. [Means for solving the problem]

[0006] A method for producing a conductive film according to one aspect of the present invention is a method for producing a conductive film made of a resin composition containing a polypropylene-based polymer and a conductive metal filler, the method including the steps of producing a conductive film using the resin composition and subjecting the conductive film to a corona discharge treatment to reduce the volume resistivity of the conductive film.

[0007] The present inventors have found that the volume resistivity of a conductive film made of a resin composition containing a polypropylene-based polymer and a conductive metal filler is reduced by subjecting the conductive film to a corona discharge treatment. According to this method for producing a conductive film, the volume resistivity of the conductive film is reduced by the corona discharge treatment, so that a conductive film with a relatively low volume resistivity can be produced.

[0008] In the above-mentioned method for manufacturing a conductive film, the corona discharge treatment may be performed by rotating a roller-shaped electrode in contact with one side of the conductive film to transport the conductive film, while generating a corona discharge between an opposing discharge electrode and the roller-shaped electrode in a non-contact state on the other side of the conductive film.

[0009] In the corona discharge treatment in the above-mentioned conductive film manufacturing method, the discharge amount D (W min / m) is defined by the following formula (1). 2 ) at 65W·min / m 2 Greater than 200W·min / m 2 It may be smaller than. Discharge amount D=P / (L×V)...(1) P (W) indicates the discharge power by the discharge electrode, L (m) indicates the length of the discharge electrode in the width direction of the conductive film, and V (m / min) indicates the transport speed of the conductive film.

[0010] In the method for producing a conductive film, the discharge amount D is 100 W min / m 2 Greater than 170W·min / m 2 It may be smaller than.

[0011] In the method for producing a conductive film, an insulating layer may not be formed on either surface of the conductive film.

[0012] A corona-treated conductive film according to another aspect of the present invention is made of a resin composition containing a polypropylene-based polymer and a conductive metal filler, and the conductive film has a water contact angle of 110° or less on its surface and a volume resistivity of 1200 Ω cm or less. Effect of the Invention

[0013] According to the present invention, it is possible to provide a method for producing a conductive film capable of reducing the volume resistivity. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a diagram illustrating a manufacturing apparatus for a conductive film. [Diagram 2] FIG. 2 is a diagram showing a schematic view of a discharge electrode as viewed from above. [Diagram 3] 1 is a flowchart showing a method for manufacturing a conductive film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] An embodiment according to one aspect of the present invention (hereinafter also referred to as "the present embodiment") will be described in detail below with reference to the drawings. Note that the same or corresponding parts in the drawings are given the same reference numerals and their description will not be repeated. Furthermore, the present embodiment described below is merely an example of the present invention in every respect. Various improvements and modifications can be made to the present embodiment within the scope of the present invention. In other words, in implementing the present invention, specific configurations can be appropriately adopted depending on the embodiment.

[0016] [1. Conductive film manufacturing equipment] 1 is a schematic diagram of a conductive film manufacturing apparatus 10 according to the present embodiment. As shown in Fig. 1, the manufacturing apparatus 10 includes a T-die 100, a casting roll 200, a touch roll 300, a roller-shaped electrode 700, a discharge electrode 400, an AC power source 500, and a take-up roll 600.

[0017] The T-die 100 is configured to melt-extrude a resin composition. The resin composition contains a polypropylene-based polymer and a conductive metal filler. In the manufacturing apparatus 10, a conductive film C2 is manufactured based on the resin composition. The conductive film C2 is used, for example, as a charging film or a discharging film for a copier or a printer, or as various functional films for other electric / electronic devices and parts.

[0018] Examples of the conductive metal filler include platinum, gold, silver, copper, nickel, titanium, and mixtures thereof. That is, the conductive metal filler contained in the resin composition includes at least one metal selected from the group including platinum, gold, silver, copper, nickel, and titanium. Among these, nickel particles are more preferable as the conductive metal filler.

[0019] The casting roll 200 is configured to cool the resin composition extruded by the T-die 100 to produce a conductive film C1, and to transport the conductive film C1 downstream. The touch roll 300 is configured to press the resin composition extruded by the T-die 100 against the casting roll 200 to produce a conductive film C1, and to transport the conductive film C1 downstream. That is, the resin composition is sandwiched between the casting roll 200 and the touch roll 300.

[0020] The roller-shaped electrode 700 is located downstream of the cast roll 200 in the manufacturing apparatus 10. The roller-shaped electrode 700 is in contact with one surface of the conductive film C1. The discharge electrode 400 faces the other surface of the conductive film C1 in a non-contact state. The roller-shaped electrode 700 and the discharge electrode 400 face each other via the conductive film C1.

[0021] The AC power supply 500 is configured to apply a high-frequency voltage between the discharge electrode 400 and the roller-shaped electrode 700. When a voltage is applied by the AC power supply 500, a corona discharge occurs between the discharge electrode 400 and the roller-shaped electrode 700. A corona discharge treatment is applied to the conductive film C1, thereby producing a conductive film (corona-discharge-treated conductive film) C2.

[0022] Fig. 2 is a schematic diagram showing discharge electrode 400 as viewed from above. As shown in Fig. 2, length L1 of discharge electrode 400 is approximately the same as the length in the width direction of conductive films C1, C2. This allows corona discharge treatment to be applied evenly over the entire conductive film C1.

[0023] In the corona discharge treatment performed on the conductive film C1 in the manufacturing apparatus 10, the discharge amount D (W min / m) is defined by the following formula (1): 2 ) at 65W·min / m 2 Greater than 200W·min / m 2 It is preferable that the discharge rate D is less than 100 W min / m 2 Greater than 170W·min / m 2 It is more preferable that the discharge amount D is smaller than 1.0 V. Also, the larger the discharge amount D is, the higher the possibility that the conductive film C1 will melt.

[0024] Discharge amount D=P / (L×V)...(1) Here, P (W) represents the discharge power of the discharge electrode 400, L (m) represents the length of the discharge electrode 400 in the width direction of the conductive films C1, C2, and V (m / min) represents the transport speed of the conductive films C1, C2 in the manufacturing apparatus 10. Note that performing corona discharge treatment twice with a discharge amount D1 can be regarded as equivalent to performing corona discharge treatment once with a discharge amount D1×2. Also, performing corona discharge treatments with a discharge amount D2 and D3 can be regarded as equivalent to performing corona discharge treatment once with a discharge amount D2+D3.

[0025] 1, the take-up roll 600 is located downstream of the roller-shaped electrode 700. The take-up roll 600 is configured to take up the conductive film C2 manufactured by subjecting the film to a corona discharge treatment. The take-up roll 600 is configured to take up the conductive film C2 at a predetermined speed.

[0026] [2. Manufacturing method of conductive film] 3 is a flowchart showing a method for manufacturing the conductive film C2. The process shown in this flowchart is performed by a manufacturing apparatus 10.

[0027] 3, the manufacturing apparatus 10 produces a conductive film C1 (step S100). The conductive film C1 is produced, for example, by sandwiching a resin composition melt-extruded by a T-die 100 between a cast roll 200 and a touch roll 300.

[0028] The manufacturing apparatus 10 performs a corona discharge treatment on the produced conductive film C1 (step S110). The corona discharge treatment is performed by generating a corona discharge between the discharge electrode 400 and the roller-shaped electrode 700. In this way, a conductive film C2 is produced.

[0029] In this manner, the corona discharge treatment is applied to the conductive film C1 in the manufacturing apparatus 10. The reason why the corona discharge treatment is applied to the conductive film C1 will be explained below.

[0030] In a conductive film made of a resin composition containing a polypropylene-based polymer and a conductive metal filler, it is required to reduce the volume resistivity of the conductive film. The present inventor(s) found that the volume resistivity of the conductive film is reduced by subjecting a conductive film C1 made of a resin composition containing a polypropylene-based polymer and a conductive metal filler to a corona discharge treatment. According to the method for producing a conductive film according to the present embodiment, the volume resistivity of the conductive film C1 is reduced through the corona discharge treatment, so that a conductive film C2 having a relatively low volume resistivity can be produced.

[0031] The surface of the conductive film C2 manufactured by the method for manufacturing a conductive film according to this embodiment has a water contact angle of 110 degrees or less and a volume resistivity of 1200 Ω·cm or less.

[0032] [3. Features] As described above, in the method for producing a conductive film according to the present embodiment, the conductive film C1 is subjected to a corona discharge treatment. Therefore, according to this method for producing a conductive film, the volume resistivity of the conductive film C1 is reduced through the corona discharge treatment, and thus a conductive film C2 having a relatively low volume resistivity can be produced. Note that, although the conductive film C1 is subjected to a corona discharge treatment in the present embodiment, the conductive film C1 may be subjected to another discharge treatment (e.g., spark discharge, arc discharge, glow discharge) as long as the volume resistivity of the conductive film C1 is reduced by the treatment.

[0033] [4. Examples, etc.] <4-1. Examples and Comparative Examples> The conductive films of Examples 1-10 and Comparative Examples 1-3 were produced by using a production apparatus 10 shown in Fig. 1. Hereinafter, the conductive films of Examples 1-10 and Comparative Examples 1-3 will be described.

[0034] The conductive films of Examples 1-10 and Comparative Examples 1-3 are summarized in Table 1 below. [Table 1] The conductive film of Example 1 had a thickness of 75 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and nickel (Ni). The mass % concentration of nickel was 66 wt%. The transport speed of the conductive film in the production apparatus 10 was 16 m / min. The discharge power P by the discharge electrode was 1000 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 101 W min / m 2 It was.

[0035] The conductive film of Example 2 had a thickness of 50 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and nickel (Ni). The mass % concentration of nickel was 66 wt%. The transport speed of the conductive film in the production apparatus 10 was 16 m / min. The discharge power P by the discharge electrode was 1000 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 101 W min / m 2 It was.

[0036] The conductive film of Example 3 had a thickness of 50 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and nickel (Ni). The mass % concentration of nickel was 66 wt%. The transport speed of the conductive film in the production apparatus 10 was 12 m / min. The discharge power P by the discharge electrode was 1000 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 134 W min / m 2 It was.

[0037] The conductive film of Example 4 had a thickness of 75 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and nickel (Ni). The mass % concentration of nickel was 63 wt%. The transport speed of the conductive film in the production apparatus 10 was 18 m / min. The discharge power P by the discharge electrode was 1000 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 90 W min / m 2 It was.

[0038] The conductive film of Example 5 had a thickness of 75 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and nickel (Ni). The mass % concentration of nickel was 66 wt%. The transport speed of the conductive film in the production apparatus 10 was 8 m / min. The discharge power P by the discharge electrode was 500 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 101 W min / m 2 It was.

[0039] The conductive film of Example 6 had a thickness of 75 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and nickel (Ni). The mass % concentration of nickel was 66 wt%. The transport speed of the conductive film in the production apparatus 10 was 16 m / min. The discharge power P by the discharge electrode was 1000 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 101 W min / m 2 In this conductive film, a polyethylene terephthalate (PET) layer was formed on the surface that was in contact with the roller-shaped electrode. The thickness of this PET layer was 50 μm.

[0040] The conductive film of Example 7 had a thickness of 75 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and nickel (Ni). The mass % concentration of nickel was 66 wt%. The transport speed of the conductive film in the production apparatus 10 was 16 m / min. The discharge power P by the discharge electrode was 1000 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 101 W min / m 2 In this conductive film, a polyethylene terephthalate (PET) layer was formed on both sides. Each PET layer had a thickness of 50 μm.

[0041] The conductive film of Example 8 had a thickness of 150 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and nickel (Ni). The mass % concentration of nickel was 73 wt%. The transport speed of the conductive film in the production apparatus 10 was 12 m / min. The discharge power P by the discharge electrode was 500 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 67 W·min / m 2 It was.

[0042] The conductive film of Example 9 had a thickness of 150 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and nickel (Ni). The mass % concentration of nickel was 73 wt%. The transport speed of the conductive film in the production apparatus 10 was 12 m / min. The discharge power P by the discharge electrode was 750 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 101 W min / m 2 It was.

[0043] The conductive film of Example 10 had a thickness of 150 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and nickel (Ni). The mass % concentration of nickel was 73 wt%. The transport speed of the conductive film in the production apparatus 10 was 12 m / min. The discharge power P by the discharge electrode was 1250 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 168 W min / m 2 It was.

[0044] The thickness of the conductive film of Comparative Example 1 was 50 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and carbon black (CB). The mass % concentration of the carbon black was 25 wt%. The transport speed of the conductive film in the production apparatus 10 was 16 m / min. The discharge power P by the discharge electrode was 1000 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 101 W min / m 2 It was.

[0045] The thickness of the conductive film of Comparative Example 2 was 75 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and carbon black (CB). The mass % concentration of the carbon black was 25 wt%. The transport speed of the conductive film in the production apparatus 10 was 16 m / min. The discharge power P by the discharge electrode was 1000 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 101 W min / m 2 It was.

[0046] The thickness of the conductive film of Comparative Example 3 was 50 μm. The resin composition used in the production of this conductive film contained polypropylene (PP) and carbon black (CB). The mass % concentration of the carbon black was 28 wt%. The transport speed of the conductive film in the production apparatus 10 was 16 m / min. The discharge power P by the discharge electrode was 1000 W. The electrode length L of the discharge electrode was 0.62 m. The discharge amount D defined by the above formula (1) was 101 W min / m 2 It was.

[0047] <4-2. Measurement method of volume resistivity> The change in volume resistivity of each conductive film with or without corona discharge treatment was measured. For each conductive film, a sample before corona discharge treatment and a sample after corona discharge treatment were prepared, and the volume resistivity of each sample was measured.

[0048] The method for measuring the volume resistivity of each conductive film is as follows. A 7 cm square sample was cut out from each conductive film, and the volume resistivity of the conductive film was measured using an electrical resistance measuring device [IMC-0240, manufactured by Imoto Manufacturing Co., Ltd.] and a resistance meter [RM3548, manufactured by HIOKI]. The resistance value of the conductive film was measured with a load of 2.16 kg applied to the electrical resistance measuring device, and the value 60 seconds after the load was applied was recorded as the resistance value of the conductive film. As shown in the following formula (2), the area of ​​the contact surface of the jig during resistance measurement (3.14 cm 2 The volume resistivity (Ω cm) was calculated by multiplying the resistance value by the film thickness and dividing the result by the film thickness. Volume resistivity (Ω cm) = resistance value (Ω) × 3.14 (cm) 2 ) ÷ thickness (cm) ··· (2)

[0049] <4-3. How to measure the contact angle of water> We measured how the contact angle of water on the surface of each conductive film changes with and without corona discharge treatment. For each conductive film, samples before and after corona discharge treatment were prepared, and the contact angle of water was measured for each sample. The contact angle was measured using a so-called contact angle meter in accordance with the sessile drop method and θ / 2 method specified in JIS R 3257.

[0050] <4-4. Measurement results> The measurement results for each conductive film are summarized in Table 2 below. [Table 2] In each of Examples 1 to 10, the volume resistivity decreased through the corona discharge treatment, while in each of Comparative Examples 1 to 3, the volume resistivity increased through the corona discharge treatment. In addition, in most of the Examples and Comparative Examples, the water contact angle on the surface decreased. [Explanation of symbols]

[0051] 10 manufacturing equipment, 100 T die, 200 casting roll, 300 touch roll, 400 discharge electrode, 500 AC power source, 600 winding roll, 700 roller-shaped electrode, C1, C2 conductive film.

Claims

1. A method for producing a conductive film made of a resin composition containing a polypropylene-based polymer and a conductive metal filler, comprising: forming a conductive film using the resin composition; and reducing the volume resistivity of the conductive film by subjecting the conductive film to a corona discharge treatment; The corona discharge treatment is carried out by rotating a roller-shaped electrode in contact with one side of the conductive film to transport the conductive film, while generating a corona discharge between the roller-shaped electrode and a discharge electrode that faces the other side of the conductive film in a non-contact state; In the corona discharge treatment, the discharge amount D (W·min / m 2 ) defined by the following formula (1) is greater than 65 W·min / m 2 and less than 200 W·min / m 2 : Discharge amount D=P / (L×V)...(1) The P (W) indicates the discharge power by the discharge electrode, L (m) represents the length of the discharge electrode in the width direction of the conductive film, The method for producing a conductive film, wherein V (m / min) indicates a transport speed of the conductive film.

2. The discharge amount D is 100 W min / m 2 Larger than 170W・min / m 2 The method for producing a conductive film according to claim 1 , wherein the thickness of the conductive film is smaller than or equal to 100 μm.

3. The method for producing a conductive film according to claim 1 , wherein the conductive film has no insulating layer formed on any surface thereof.

4. A conductive film made of a resin composition containing a polypropylene-based polymer and a conductive metal filler, the contact angle of water on the surface of the conductive film is 125 degrees or less; A corona discharge-treated conductive film, wherein the conductive film has a volume resistivity of 1200 Ω·cm or less.

Citation Information

Patent Citations

  • Apparatus for adjusting gap of discharge electrode for plastic film

    JP1997255803A

  • Antibacterial synthetic resin oriented film and antibacterial laminate

    JP1998086290A

  • Surface-modified polyolefin film and its production

    JP2000159915A

  • Atmospheric pressure plasma treatment apparatus

    JP2002018276A

  • Conductive resin film and method of manufacturing the same

    JP2010153307A