SUBSTRATE PROCESSING METHOD, SEMICONDUCTOR DEVICE MANUFACTURING METHOD, SUBSTRATE PROCESSING APPARATUS, AND PROGRAM
By modifying the surface of a first base layer with a hydrocarbon group-containing gas and applying oxygen and hydrogen-containing gases in a controlled non-plasma atmosphere, the method enhances selectivity in selective growth processes, simplifying semiconductor manufacturing and reducing costs.
Patent Information
- Application Number
- JP2023018354
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-02-09
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2039-12-27
AI Technical Summary
Existing selective growth processes in semiconductor manufacturing lack sufficient selectivity in forming films on specific bases, leading to inefficiencies and challenges in processing complexity and cost.
A method involving the use of a hydrocarbon group-containing gas to modify the surface of a first base layer, followed by the application of oxygen and hydrogen-containing gases to selectively form a film on a second base layer, utilizing a non-plasma atmosphere and controlled temperature conditions to enhance selectivity.
This approach significantly enhances the selectivity of film formation on specific bases, simplifying the manufacturing process, reducing costs, and improving productivity by minimizing plasma damage and hydrocarbon group detachment during film formation.
Smart Images

Figure 0007561896000001 
Figure 0007561896000002 
Figure 0007561896000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a substrate processing method, a semiconductor device manufacturing method, a substrate processing apparatus, and a program. [Background technology]
[0002] As one step in the manufacturing process of a semiconductor device, a process may be performed in which a film is selectively grown and formed on the surface of a specific base among multiple types of bases exposed on the surface of a substrate (hereinafter, this process is also referred to as selective growth or selective film formation) (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-243193 A Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present disclosure is to provide a technique capable of improving the selectivity in the above-mentioned selective growth. [Means for solving the problem]
[0005] According to one aspect of the present disclosure, (a) supplying a hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer exposed on a surface thereof to modify the surface of the first underlayer so as to terminate the surface with a hydrocarbon group; (b) supplying an oxygen- and hydrogen-containing gas to the substrate after modifying the surface of the first underlayer, and selectively forming a film on the surface of the second underlayer; Techniques for doing so are provided. Effect of the Invention
[0006] According to the present disclosure, it is possible to improve the selectivity in the selective growth described above. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus suitably used in one embodiment of the present disclosure, showing a processing furnace 202 portion in vertical cross section. [Diagram 2] FIG. 2 is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus preferably used in one embodiment of the present disclosure, showing a processing furnace 202 portion in a cross-sectional view taken along line AA in FIG. [Diagram 3] FIG. 3 is a schematic configuration diagram of a controller 121 of a substrate processing apparatus suitably used in one embodiment of the present disclosure, and is a block diagram showing a control system of the controller 121. [Figure 4] FIG. 4 is a diagram showing a process sequence in selective growth according to one embodiment of the present disclosure. [Diagram 5] Fig. 5(a) is a diagram showing the chemical structural formula of DMATMS, Fig. 5(b) is a diagram showing the chemical structural formula of a hydrocarbon group-containing gas having a trialkylsilyl group and an amino group, and Fig. 5(c) is a diagram showing the chemical structural formula of a hydrocarbon group-containing gas having a dialkylsilyl group and an amino group. [Figure 6]FIG. 6(a) is a partial enlarged cross-sectional view of the surface of the wafer 200, in which the underlayer 200a containing a silicon oxide film and the underlayer 200b containing a silicon nitride film are exposed. FIG. 6(b) is a partial enlarged cross-sectional view of the surface of the wafer 200 after the surface of the underlayer 200a is modified to terminate with a hydrocarbon group by supplying a hydrocarbon group-containing gas. FIG. 6(c) is a partial enlarged cross-sectional view of the surface of the wafer 200 after the first layer containing silicon and carbon is selectively formed on the surface of the underlayer 200b by supplying a silicon and halogen-containing gas. FIG. 6(d) is a partial enlarged cross-sectional view of the surface of the wafer 200 after the first layer selectively formed on the surface of the underlayer 200b is oxidized and modified to a second layer containing silicon, oxygen and carbon by supplying an oxygen and hydrogen-containing gas. FIG. 6(e) is a partial enlarged cross-sectional view of the surface of the wafer 200 after the silicon oxycarbonate film is selectively formed on the surface of the underlayer 200b. Figure 6(f) is an enlarged partial cross-sectional view of the surface of wafer 200 after wafer 200 shown in Figure 6(e) has been post-processed to remove the hydrocarbon groups terminating the surface of base 200a from the surface of base 200a. [Figure 7] FIG. 13 is a diagram showing the measurement results of the thickness of silicon oxycarbide films formed on the surfaces of various underlayers exposed on the surface of a wafer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] <One aspect of the present disclosure> Hereinafter, one embodiment of the present disclosure will be described mainly with reference to FIGS.
[0009] (1) Configuration of the substrate processing device 1, the process furnace 202 has a heater 207 as a temperature regulator (heating unit). The heater 207 is cylindrical and is installed vertically by being supported by a holding plate. The heater 207 also functions as an activation mechanism (excitation unit) that activates (excites) gas by heat.
[0010] A reaction tube 203 is disposed concentrically with the heater 207 inside the heater 207. The reaction tube 203 is made of a heat-resistant material such as quartz (SiO2) or silicon carbide (SiC) and is formed in a cylindrical shape with a closed upper end and an open lower end. A manifold 209 is disposed concentrically with the reaction tube 203 below the reaction tube 203. The manifold 209 is made of a metal material such as stainless steel (SUS) and is formed in a cylindrical shape with an open upper end and a closed lower end. The upper end of the manifold 209 engages with the lower end of the reaction tube 203 and is configured to support the reaction tube 203. An O-ring 220a is provided between the manifold 209 and the reaction tube 203 as a seal member. The reaction tube 203 is installed vertically like the heater 207. The reaction tube 203 and the manifold 209 mainly constitute a processing vessel (reaction vessel). A processing chamber 201 is formed in a cylindrical hollow portion of the processing vessel. The processing chamber 201 is configured to be capable of accommodating a wafer 200 as a substrate. In the processing chamber 201, processing of the wafer 200 is performed.
[0011] Nozzles 249a to 249c serving as first to third supply units are provided in the processing chamber 201 so as to penetrate the sidewall of the manifold 209, respectively. The nozzles 249a to 249c are also referred to as first to third nozzles, respectively. The nozzles 249a to 249c are made of a heat-resistant material such as quartz or SiC. Gas supply pipes 232a to 232c are connected to the nozzles 249a to 249c, respectively. The nozzles 249a to 249c are different nozzles, and each of the nozzles 249a and 249c is provided adjacent to the nozzle 249b.
[0012] Gas supply pipes 232a-232c are provided with mass flow controllers (MFCs) 241a-241c, which are flow rate controllers (flow rate control parts), and valves 243a-243c, which are on-off valves, in order from the upstream side of the gas flow. Gas supply pipes 232d and 232e are connected to the gas supply pipe 232a downstream of the valve 243a. Gas supply pipes 232f and 232g are connected to the gas supply pipes 232b and 232c downstream of the valves 243b and 243c, respectively. Gas supply pipes 232d-232g are provided with MFCs 241d-241g and valves 243d-243g in order from the upstream side of the gas flow. Gas supply pipes 232a-232g are made of a metal material, such as SUS.
[0013] As shown in FIG. 2, the nozzles 249a to 249c are provided in a circular space between the inner wall of the reaction tube 203 and the wafers 200 in a plan view, from the lower part to the upper part of the inner wall of the reaction tube 203, so as to rise upward in the arrangement direction of the wafers 200. That is, the nozzles 249a to 249c are provided in a region horizontally surrounding the wafer arrangement region on the side of the wafer arrangement region in which the wafers 200 are arranged, so as to extend along the wafer arrangement region. In a plan view, the nozzle 249b is disposed so as to face an exhaust port 231a (described later) on a straight line across the center of the wafer 200 loaded into the processing chamber 201. The nozzles 249a and 249c are disposed so as to sandwich a straight line L passing through the nozzle 249b and the center of the exhaust port 231a from both sides along the inner wall of the reaction tube 203 (the outer periphery of the wafer 200). The straight line L is also a straight line passing through the nozzle 249b and the center of the wafer 200. In other words, the nozzle 249c is provided on the opposite side of the nozzle 249a across the line L. The nozzles 249a and 249c are arranged symmetrically with respect to the line L. Gas supply holes 250a to 250c for supplying gas are provided on the side surfaces of the nozzles 249a to 249c, respectively. The gas supply holes 250a to 250c are each opened to face (face) the exhaust port 231a in a plan view, and are capable of supplying gas toward the wafer 200. A plurality of gas supply holes 250a to 250c are provided from the lower part to the upper part of the reaction tube 203.
[0014] A hydrocarbon group-containing gas is supplied as a surface modification gas from the gas supply pipe 232a into the processing chamber 201 via the MFC 241a, the valve 243a, and the nozzle 249a.
[0015] As the hydrocarbon group-containing gas, for example, a gas containing an alkyl group can be used. As the gas containing an alkyl group, for example, a gas containing an alkylsilyl group in which an alkyl group is coordinated to silicon (Si), that is, an alkylsilane-based gas can be used. The alkyl group is an alkane (general formula C n H 2n+2It is a general term for the remaining atomic group obtained by removing one hydrogen (H) atom from a chain saturated hydrocarbon represented by the general formula C n H 2n+1 The alkyl group is a functional group represented by the formula: Alkyl groups include methyl, ethyl, propyl, and butyl groups. Since the alkyl group is bonded to the central atom of the alkylsilane molecule, Si, the alkyl group in the alkylsilane can also be called a ligand or alkyl ligand.
[0016] The hydrocarbon group-containing gas may further contain an amino group. As the hydrocarbon group- and amino group-containing gas, for example, an alkylaminosilane gas may be used. The amino group is a functional group in which one or two hydrocarbon groups containing one or more carbon (C) atoms are coordinated to one nitrogen (N) atom (a functional group in which one or both H of an amino group represented by NH2 are replaced with a hydrocarbon group containing one or more C atoms). When two hydrocarbon groups constituting a part of an amino group are coordinated to one N, the two may be the same hydrocarbon group or different hydrocarbon groups. The hydrocarbon group may contain a single bond like an alkyl group, or may contain an unsaturated bond such as a double bond or a triple bond. The amino group may have a cyclic structure. Since the amino group is bonded to Si, which is the central atom of the aminosilane molecule, the amino group in the aminosilane may also be called a ligand or an amino ligand.
[0017] As the hydrocarbon group-containing gas, for example, an alkylaminosilane-based gas such as dimethylaminotrimethylsilane ((CH3)2NSi(CH3)3, abbreviated as DMATMS) gas containing an alkylsilyl group and an amino group can be used. As shown in the chemical structural formula in FIG. 5(a), the central atom of DMATMS, Si, is bonded with three alkyl groups (methyl groups, Me) and one amino group (dimethylamino group). That is, DMATMS contains three alkyl ligands and one amino ligand.
[0018] From the gas supply pipe 232b, a gas containing Si and halogen is supplied as a raw material (raw material gas) into the processing chamber 201 via the MFC 241b, the valve 243b, and the nozzle 249b. The halogen includes chlorine (Cl), fluorine (F), bromine (Br), iodine (I), and the like. The Si and halogen containing gas preferably includes halogen in the form of a chemical bond between Si and halogen. The Si and halogen containing gas may further include C, and in that case, it is preferable to include C in the form of a Si-C bond. As the Si and halogen containing gas, for example, a silane-based gas containing Si, Cl, and an alkylene group and having a Si-C bond, that is, an alkylene chlorosilane-based gas, can be used. The alkylene group includes a methylene group, an ethylene group, a propylene group, a butylene group, and the like. The alkylene chlorosilane-based gas preferably includes Cl in the form of a Si-Cl bond and C in the form of a Si-C bond. As the alkylenechlorosilane gas, for example, bis(trichlorosilyl)methane ((SiCl3)2CH2, abbreviated as BTCSM) gas can be used.
[0019] From the gas supply pipe 232c, oxygen (O) and H-containing gas are supplied as an oxidizing agent (oxidizing gas) into the processing chamber 201 via the MFC 241c, the valve 243c, and the nozzle 249c. The O and H-containing gas preferably contains an OH bond. As the O and H-containing gas, for example, water vapor (HO gas) can be used.
[0020] A catalyst (catalyst gas) is supplied from the gas supply pipe 232d through the MFC 241d, the valve 243d, the gas supply pipe 232a, and the nozzle 249a into the processing chamber 201. As the catalyst, for example, an amine-based gas containing C, N, and H can be used. As the amine-based gas, for example, pyridine (C5H5N) gas can be used.
[0021] From the gas supply pipes 232e to 232g, an inert gas such as nitrogen (N2) gas is supplied into the processing chamber 201 via the MFCs 241e to 241g, the valves 243e to 243g, the gas supply pipes 232a to 232c, and the nozzles 249a to 249c, respectively. The N2 gas acts as a purge gas, a carrier gas, a dilution gas, etc.
[0022] A hydrocarbon group-containing gas supply system is mainly composed of the gas supply pipe 232a, the MFC 241a, and the valve 243a. A Si- and halogen-containing gas supply system is mainly composed of the gas supply pipe 232b, the MFC 241b, and the valve 243b. A O- and H-containing gas supply system is mainly composed of the gas supply pipe 232c, the MFC 241c, and the valve 243c. A catalyst supply system is mainly composed of the gas supply pipe 232d, the MFC 241d, and the valve 243d. An inert gas supply system is mainly composed of the gas supply pipes 232e to 232g, the MFCs 241e to 241g, and the valves 243e to 243g.
[0023] Any or all of the various supply systems described above may be configured as an integrated supply system 248 in which the valves 243a-243g and the MFCs 241a-241g are integrated. The integrated supply system 248 is connected to the gas supply pipes 232a-232g, and the supply operation of various gases into the gas supply pipes 232a-232g, i.e., the opening and closing operation of the valves 243a-243g and the flow rate adjustment operation by the MFCs 241a-241g, are controlled by a controller 121, which will be described later. The integrated supply system 248 is configured as an integrated or separate integrated unit, and can be attached and detached to and from the gas supply pipes 232a-232g, etc., and maintenance, replacement, expansion, etc. of the integrated supply system 248 can be performed on an integrated unit basis.
[0024] An exhaust port 231a for exhausting the atmosphere in the processing chamber 201 is provided at the lower side of the side wall of the reaction tube 203. As shown in FIG. 2, the exhaust port 231a is provided at a position facing the nozzles 249a to 249c (gas supply holes 250a to 250c) across the wafer 200 in a plan view. The exhaust port 231a may be provided along the side wall of the reaction tube 203 from the lower part to the upper part, that is, along the wafer arrangement area. An exhaust pipe 231 is connected to the exhaust port 231a. A vacuum pump 246 as a vacuum exhaust device is connected to the exhaust pipe 231 via a pressure sensor 245 as a pressure detector (pressure detection unit) for detecting the pressure in the processing chamber 201 and an APC (Auto Pressure Controller) valve 244 as a pressure regulator (pressure adjustment unit). The APC valve 244 can evacuate and stop the evacuation of the processing chamber 201 by opening and closing the valve while the vacuum pump 246 is operating, and further, can adjust the pressure inside the processing chamber 201 by adjusting the valve opening based on pressure information detected by the pressure sensor 245 while the vacuum pump 246 is operating. An exhaust system is mainly configured by the exhaust pipe 231, the APC valve 244, and the pressure sensor 245. The vacuum pump 246 may be included in the exhaust system.
[0025] Below the manifold 209, a seal cap 219 is provided as a furnace port cover body capable of airtightly closing the lower end opening of the manifold 209. The seal cap 219 is made of a metal material such as SUS, and is formed in a disk shape. An O-ring 220b is provided on the upper surface of the seal cap 219 as a seal member that abuts against the lower end of the manifold 209. Below the seal cap 219, a rotation mechanism 267 is provided for rotating the boat 217, which will be described later. A rotation shaft 255 of the rotation mechanism 267 is connected to the boat 217 through the seal cap 219. The rotation mechanism 267 is configured to rotate the wafers 200 by rotating the boat 217. The seal cap 219 is configured to be vertically raised and lowered by a boat elevator 115 as a lifting mechanism installed outside the reaction tube 203. The boat elevator 115 is configured as a transfer device (transfer mechanism) that transfers (transports) the wafers 200 into and out of the processing chamber 201 by raising and lowering the seal cap 219. A shutter 219s is provided below the manifold 209 as a furnace port cover that can airtightly close the lower end opening of the manifold 209 when the seal cap 219 is lowered and the boat 217 is transported out of the processing chamber 201. The shutter 219s is made of a metal material such as SUS and is formed in a disk shape. An O-ring 220c is provided on the upper surface of the shutter 219s as a seal member that contacts the lower end of the manifold 209. The opening and closing operation (lifting and lowering operation, rotating operation, etc.) of the shutter 219s is controlled by a shutter opening and closing mechanism 115s.
[0026] The boat 217 as a substrate support is configured to support a plurality of wafers 200, for example 25 to 200, in multiple stages in a horizontal position and aligned vertically with their centers aligned, i.e., arranged at intervals. The boat 217 is made of a heat-resistant material such as quartz or SiC. At the bottom of the boat 217, heat insulating plates 218 made of a heat-resistant material such as quartz or SiC are supported in multiple stages.
[0027] A temperature sensor 263 serving as a temperature detector is installed in the reaction tube 203. By adjusting the power supply to the heater 207 based on temperature information detected by the temperature sensor 263, the temperature distribution in the process chamber 201 becomes a desired one. The temperature sensor 263 is installed along the inner wall of the reaction tube 203.
[0028] 3, the controller 121, which is a control unit (control means), is configured as a computer including a CPU (Central Processing Unit) 121a, a RAM (Random Access Memory) 121b, a storage device 121c, and an I / O port 121d. The RAM 121b, the storage device 121c, and the I / O port 121d are configured to be able to exchange data with the CPU 121a via an internal bus 121e. An input / output device 122 configured as, for example, a touch panel, is connected to the controller 121.
[0029] The storage device 121c is composed of, for example, a flash memory, a HDD (Hard Disk Drive), etc. A control program for controlling the operation of the substrate processing apparatus, a process recipe in which procedures and conditions of the substrate processing described later are described, etc. are readably stored in the storage device 121c. The process recipe is a combination of procedures in the substrate processing described later that are executed by the controller 121 to obtain a predetermined result, and functions as a program. Hereinafter, the process recipe, the control program, etc. are collectively referred to simply as a program. In addition, the process recipe is also simply referred to as a recipe. In this specification, when the word program is used, it may include only a recipe, only a control program, or both. The RAM 121b is configured as a memory area (work area) in which the programs and data read by the CPU 121a are temporarily stored.
[0030] The I / O port 121d is connected to the above-mentioned MFCs 241a to 241g, valves 243a to 243g, pressure sensor 245, APC valve 244, vacuum pump 246, temperature sensor 263, heater 207, rotation mechanism 267, boat elevator 115, shutter opening / closing mechanism 115s, and the like.
[0031] The CPU 121a is configured to read and execute a control program from the storage device 121c, and also to read a recipe from the storage device 121c in response to an input of an operation command from the input / output device 122, etc. The CPU 121a is configured to control the flow rate adjustment operation of various gases by the MFCs 241a to 241g, the opening and closing operations of the valves 243a to 243g, the opening and closing operation of the APC valve 244 and the pressure adjustment operation by the APC valve 244 based on the pressure sensor 245, the start and stop of the vacuum pump 246, the temperature adjustment operation of the heater 207 based on the temperature sensor 263, the rotation and rotation speed adjustment operation of the boat 217 by the rotation mechanism 267, the lifting and lowering operation of the boat 217 by the boat elevator 115, the opening and closing operation of the shutter 219s by the shutter opening and closing mechanism 115s, etc., in accordance with the contents of the read recipe.
[0032] The controller 121 can be configured by installing the above-mentioned program stored in the external storage device 123 in a computer. The external storage device 123 includes, for example, a magnetic disk such as an HDD, an optical disk such as a CD, a magneto-optical disk such as an MO, a semiconductor memory such as a USB memory, and the like. The storage device 121c and the external storage device 123 are configured as computer-readable recording media. Hereinafter, these are collectively referred to simply as recording media. When the term recording media is used in this specification, it may include only the storage device 121c alone, only the external storage device 123 alone, or both of them. The program may be provided to the computer using a communication means such as the Internet or a dedicated line, without using the external storage device 123.
[0033] (2) Substrate processing An example of a process sequence of selective growth (selective film formation) in which a film is selectively grown on a specific surface of a plurality of types of underlayers exposed on the surface of a wafer 200 as a substrate, using the above-mentioned substrate processing apparatus as one step in the manufacturing process of a semiconductor device, will be described mainly with reference to Figures 4 and 6(a) to 6(f). In the following description, the operation of each part constituting the substrate processing apparatus is controlled by a controller 121.
[0034] In the processing sequence shown in Figure 4, A step of supplying DMATMS gas as a hydrocarbon group-containing gas to a wafer 200 having a first underlayer (underlayer 200a) including a silicon oxide film (SiO film) on its surface and a second underlayer (underlayer 200b) including a silicon nitride film (SiN film) exposed thereon, and modifying the surface of the underlayer 200a so as to terminate it with a methyl group (Me), which is a hydrocarbon group (surface modification); A step of supplying HO gas as an O and H-containing gas to the wafer 200 after the surface of the underlayer 200a has been modified, and selectively forming a film on the surface of the underlayer 200b (selective growth); Do the following.
[0035] 4, pyridine gas is further supplied as a catalyst and BTCSM gas is supplied as a Si- and halogen-containing gas to the wafer 200. Specifically, a cycle of non-simultaneously supplying BTCSM gas and pyridine gas to the wafer 200 and supplying H2O gas and pyridine gas to the wafer 200 is performed a predetermined number of times (n times, n is an integer of 1 or more) to form a silicon oxycarbide film (SiOC film) as a film on the surface of the base 200b.
[0036] In addition, in the processing sequence shown in FIG. 4, the temperature of the wafer 200 after the SiOC film is selectively formed on the surface of the base 200b is set to be equal to or higher than the temperature of the wafer 200 during film formation, preferably higher than the temperature of the wafer 200 during film formation, and a step of post-processing the wafer 200 after the selective growth is performed.
[0037] In this specification, the above-mentioned processing sequence may be expressed as follows for convenience: Similar notations will be used in the following explanations of modified examples, etc.
[0038] DMATMS→(BTCSM+Py→H2O+Py)×n→Post-Treatment ⇒ SiOC
[0039] In this specification, the term "wafer" may refer to the wafer itself or a laminate of the wafer and a predetermined layer or film formed on its surface. In this specification, the term "surface of the wafer" may refer to the surface of the wafer itself or the surface of a predetermined layer or the like formed on the wafer. In this specification, the phrase "forming a predetermined layer on a wafer" may refer to forming a predetermined layer directly on the surface of the wafer itself or forming a predetermined layer on a layer or the like formed on the wafer. In this specification, the term "substrate" is synonymous with the term "wafer".
[0040] (Wafer charge and boat load) When a plurality of wafers 200 are loaded into the boat 217 (wafer charge), the shutter 219s is moved by the shutter opening / closing mechanism 115s to open the lower end opening of the manifold 209 (shutter open). Thereafter, as shown in Fig. 1, the boat 217 supporting the plurality of wafers 200 is lifted by the boat elevator 115 and carried into the processing chamber 201 (boat load). In this state, the seal cap 219 seals the lower end of the manifold 209 via the O-ring 220b.
[0041] As shown in Fig. 6(a), a plurality of types of underlayers are exposed on the surface of the wafer 200 in advance, as an example here, underlayer 200a including a SiO film as an oxygen (O)-containing film, i.e., an oxide film, and underlayer 200b including a SiN film as a non-O film, i.e., a nitride film as a non-oxide film. The underlayer 200a has a surface terminated with hydroxyl groups (OH groups) over the entire area (whole surface). The underlayer 200b has a surface that is not terminated with OH groups in many areas, i.e., a surface that is terminated with OH groups in some areas.
[0042] (Pressure and temperature regulation) The processing chamber 201, i.e., the space in which the wafer 200 is present, is evacuated (reduced pressure exhaust) by the vacuum pump 246 so that the pressure inside the processing chamber 201 is a desired pressure (vacuum level). At this time, the pressure inside the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 244 is feedback-controlled based on the measured pressure information. Also, the wafer 200 inside the processing chamber 201 is heated by the heater 207 so that the processing temperature is a desired processing temperature. At this time, the power supply to the heater 207 is feedback-controlled based on the temperature information detected by the temperature sensor 263 so that the processing chamber 201 has a desired temperature distribution. Also, the rotation mechanism 267 starts rotating the wafer 200. The evacuation inside the processing chamber 201 and the heating and rotation of the wafer 200 are all continued at least until the processing of the wafer 200 is completed.
[0043] (Surface modification) Thereafter, DMATMS gas is supplied to the wafer 200, on whose surface the underlayer 200a and the underlayer 200b are exposed.
[0044] Specifically, the valve 243a is opened to allow the DMATMS gas to flow into the gas supply pipe 232a. The DMATMS gas has a flow rate adjusted by the MFC 241a, is supplied into the processing chamber 201 through the nozzle 249a, and is exhausted from the exhaust port 231a. At this time, the DMATMS gas is supplied to the wafer 200 (DMATMS gas supply). At this time, the valves 243e to 243g may be opened to supply N2 gas into the processing chamber 201 through the nozzles 249a to 249c, respectively.
[0045] By supplying DMATMS gas to the wafer 200 under processing conditions to be described later, it is possible to selectively (preferentially) modify the surface of the underlayer 200a out of the underlayers 200a and 200b. Specifically, while suppressing the adsorption of Si contained in DMATMS to the surface of the underlayer 200b, it is possible to react OH groups terminating the surface of the underlayer 200a with DMATMS gas, and selectively (preferentially) adsorb Si contained in DMATMS to the surface of the underlayer 200a. This makes it possible to terminate the surface of the underlayer 200a with methyl groups (Me) contained in DMATMS. Specifically, as shown in FIG. 6(b), it is possible to terminate the surface of the underlayer 200a with trimethylsilyl groups (Si-Me3) contained in DMATMS. The methyl group (trimethylsilyl group) terminating the surface of the underlayer 200a prevents the adsorption of BTCSM gas onto the surface of the underlayer 200a during the selective growth described below, and acts as an adsorption suppressant (inhibitor) that inhibits the progress of the film formation reaction on the surface of the underlayer 200a.
[0046] In this step, Si contained in the DMATMS gas is adsorbed on a part of the surface of the underlayer 200b, and a part of the surface of the underlayer 200b may be terminated with a methyl group, but the amount of the termination is small, and the amount of the termination by the methyl group on the surface of the underlayer 200a is overwhelmingly larger. Such selective (preferential) termination is possible because the process conditions in this step are set to conditions under which the DMATMS gas does not decompose in the gas phase in the process chamber 201. Also, while the surface of the underlayer 200a is terminated with OH over the entire area, most of the surface of the underlayer 200b is not terminated with OH. In this step, since the DMATMS gas does not decompose in the gas phase in the process chamber 201, Si contained in DMATMS does not deposit multiple times on the surfaces of the underlayers 200a and 200b, and the Si contained in DMATMS is selectively adsorbed on the surface of the underlayer 200a, and the surface of the underlayer 200a is selectively terminated with methyl groups.
[0047] After modifying the surface of the base 200a, the valve 243a is closed to stop the supply of DMATMS gas into the processing chamber 201. Then, the processing chamber 201 is evacuated to remove gas remaining in the processing chamber 201 from the processing chamber 201. At this time, the valves 243e to 243g are opened to supply N2 gas into the processing chamber 201 through the nozzles 249a to 249c. The N2 gas supplied from the nozzles 249a to 249c acts as a purge gas, and the processing chamber 201 is purged (purged).
[0048] The processing conditions for DMATMS gas supply are as follows: DMATMS gas supply flow rate: 1 to 3000 sccm, preferably 1 to 500 sccm DMATMS gas supply time: 1 second to 120 minutes, preferably 30 seconds to 60 minutes N2 gas supply flow rate (per gas supply pipe): 0 to 20,000 sccm Treatment temperature: room temperature (25°C) to 500°C, preferably room temperature to 250°C Processing pressure: 5~1000Pa Examples are given below.
[0049] The processing conditions for purging are as follows: N2 gas supply flow rate (per gas supply pipe): 500 to 20,000 sccm N2 gas supply time: 10 to 30 seconds Processing pressure: 1~30Pa Examples are given below.
[0050] In this specification, the expression of a numerical range such as "5 to 1000 Pa" means that the lower limit and the upper limit are included in the range. Therefore, for example, "5 to 1000 Pa" means "5 Pa or more and 1000 Pa or less." The same applies to other numerical ranges.
[0051] As the hydrocarbon group-containing gas, in addition to DMATMS gas, for example, an aminosilane-based gas represented by the following general formula [1] can be used.
[0052] SiA x [(NB2) (4-x) ][1]
[0053] In the formula [1], A represents a hydrogen atom, an alkyl group such as a methyl group, an ethyl group, a propyl group, or a butyl group, or an alkoxy group such as a methoxy group, an ethoxy group, a propoxy group, or a butoxy group. The alkyl group may be not only a linear alkyl group but also a branched alkyl group such as an isopropyl group, an isobutyl group, a secondary butyl group, or a tertiary butyl group. The alkoxy group may be not only a linear alkoxy group but also a branched alkoxy group such as an isopropoxy group, or an isobutoxy group. B represents a hydrogen atom, or an alkyl group such as a methyl group, an ethyl group, a propyl group, or a butyl group. The alkyl group may be not only a linear alkyl group but also a branched alkyl group such as an isopropyl group, an isobutyl group, a secondary butyl group, or a tertiary butyl group. A plurality of A's may be the same or different, and two B's may be the same or different. x is an integer of 1 to 3. FIG. 5(b) shows the chemical structural formula of an aminosilane containing a trialkylsilyl group in which three alkyl groups and one amino group are bonded to the central atom Si when x is 3. FIG. 5(c) shows the chemical structural formula of an aminosilane containing a dialkylsilyl group in which two alkyl groups and two amino groups are bonded to the central atom Si when x is 2. In these figures, R1 to R6 can be various functional groups exemplified as A and B, respectively.
[0054] As the inert gas, in addition to N2 gas, rare gases such as Ar gas, He gas, Ne gas, Xe gas, etc. This also applies to each step described later.
[0055] (Selective growth) Thereafter, the following steps 1 and 2 are executed in sequence. In these steps, the output of the heater 207 is adjusted to maintain the temperature of the wafer 200 at or below the temperature of the wafer 200 in the surface modification, preferably at a temperature lower than the temperature of the wafer 200 in the surface modification.
[0056] [Step 1] In this step, BTCSM gas and pyridine gas are supplied to the wafer 200 in the processing chamber 201, that is, the wafer 200 after the surface of the base 200a has been selectively terminated with a methyl group.
[0057] Specifically, the valves 243b and 243d are opened to allow BTCSM gas to flow into the gas supply pipe 232b and pyridine gas to flow into the gas supply pipe 232d. The BTCSM gas and pyridine gas are adjusted in flow rate by the MFCs 241b and 241d, respectively, and are supplied into the processing chamber 201 through the nozzles 249b and 249a. After being supplied into the processing chamber 201, the gases are mixed and exhausted from the exhaust port 231a. At this time, the BTCSM gas and pyridine gas are supplied to the wafer 200 (BTCSM gas + pyridine gas supply). At this time, the valves 243e to 243g may be opened to allow N2 gas to be supplied into the processing chamber 201 through the nozzles 249a to 249c.
[0058] By supplying BTCSM gas and pyridine gas to the wafer 200 under processing conditions described later, it is possible to selectively (preferentially) adsorb Si contained in the BTCSM gas onto the surface of the underlayer 200b while suppressing adsorption of Si contained in the BTCSM gas onto the surface of the underlayer 200a, as shown in Fig. 6(c). As a result, a Si-containing layer containing C and Cl and having a thickness of, for example, less than one atomic layer (one molecular layer) to several atomic layers (several molecular layers) is formed as a first layer on the surface of the underlayer 200b. The first layer is a layer containing Si-C bonds. In this specification, the Si-containing layer containing C and Cl is also simply referred to as a Si-containing layer containing C, or a SiC layer.
[0059] In this step, pyridine gas acting as a catalyst is supplied together with BTCSM gas, so that the above-mentioned reaction can proceed in a non-plasma atmosphere and at a low temperature condition as described later. In this manner, by forming the first layer in a non-plasma atmosphere and at a low temperature condition as described later, it becomes possible to maintain the methyl groups terminating the surface of the base 200a without disappearing (detaching) from the surface of the base 200a.
[0060] In this step, when the first layer is formed, Si contained in the BTCSM gas may be adsorbed on a part of the surface of the underlayer 200a, but the amount of adsorption is smaller than the amount of Si adsorbed on the surface of the underlayer 200b. Such selective (preferential) adsorption is possible because the process conditions in this step are set to conditions under which the BTCSM gas is not decomposed in the gas phase in the process chamber 201. Also, the surface of the underlayer 200a is terminated with methyl groups over its entirety, whereas most of the surface of the underlayer 200b is not terminated with methyl groups. In this step, since the BTCSM gas is not decomposed in the gas phase in the process chamber 201, Si contained in BTCSM is not deposited in multiple layers on the surfaces of the underlayers 200a and 200b, and the Si contained in BTCSM is selectively adsorbed on the surface of the underlayer 200b.
[0061] After the first layer is selectively formed on the surface of the base 200b, the valves 243b and 243d are closed to stop the supply of the BTCSM gas and the pyridine gas into the processing chamber 201. Then, gases remaining in the processing chamber 201 are removed (purged) from the processing chamber 201 by the same processing procedure and processing conditions as those for purging in the surface modification.
[0062] The processing conditions in this step are as follows: BTCSM gas supply flow rate: 1 to 2000 sccm Pyridine gas supply flow rate: 1 to 2000 sccm N2 gas supply flow rate (per gas supply pipe): 0 to 20,000 sccm Each gas supply time: 1 to 60 seconds Treatment temperature: room temperature to 120°C, preferably room temperature to 90°C Processing pressure: 133~1333Pa Examples are given below.
[0063] Examples of Si- and halogen-containing gases that can be used include BTCSM gas, alkylene chlorosilane gases such as 1,2-bis(trichlorosilyl)ethane ((SiCl3)2C2H4, abbreviated as BTCSE) gas, alkyl chlorosilane gases such as 1,1,2,2-tetrachloro-1,2-dimethyldisilane ((CH3)2Si2Cl4, abbreviated as TCDMDS) gas and 1,2-dichloro-1,1,2,2-tetramethyldisilane ((CH3)4Si2Cl2, abbreviated as DCTMDS) gas, and gases that contain a cyclic structure composed of Si and C and halogens, such as 1,1,3,3-tetrachloro-1,3-disilacyclobutane (C2H4Cl4Si2, abbreviated as TCDSCB) gas. In addition, the Si- and halogen-containing gas may be an inorganic chlorosilane gas such as tetrachlorosilane (SiCl4, abbreviated as STC) gas, hexachlorodisilane (Si2Cl6, abbreviated as HCDS) gas, or octachlorotrisilane (Si3Cl8, abbreviated as OCTS) gas. When an inorganic chlorosilane gas is used, the same reaction as described above can be caused, except that the first layer does not contain C.
[0064] In addition to pyridine gas, other catalysts include aminopyridine (C5H6N2) gas, picoline (C6H7N) gas, lutidine (C7H9N) gas, piperazine (C4H 10 N2) gas, piperidine (C5H 11 Alternatively, a cyclic amine gas such as triethylamine ((C2H5)3N, abbreviated as TEA) gas or a chain amine gas such as diethylamine ((C2H5)2NH, abbreviated as DEA) gas may be used. This also applies to step 2 described later.
[0065] [Step 2] After the first layer is formed, H2O gas and pyridine gas are supplied to the wafer 200 in the processing chamber 201, that is, to the first layer selectively formed on the surface of the base 200b.
[0066] Specifically, the valves 243c and 243d are opened to allow H2O gas to flow into the gas supply pipe 232c and pyridine gas to flow into the gas supply pipe 232d. The H2O gas and pyridine gas are adjusted in flow rate by the MFCs 241c and 241d, respectively, and are supplied into the processing chamber 201 through the nozzles 249c and 249a, and are mixed after being supplied into the processing chamber 201 and exhausted from the exhaust port 231a. At this time, the H2O gas and pyridine gas are supplied to the wafer 200 (H2O gas + pyridine gas supply). At this time, the valves 243e to 243g may be opened to allow N2 gas to be supplied into the processing chamber 201 through the nozzles 249a to 249c, respectively.
[0067] By supplying H2O gas and pyridine gas to the wafer 200 under processing conditions to be described later, as shown in FIG. 6(d), it becomes possible to oxidize at least a part of the first layer formed on the surface of the underlayer 200b in step 1. As a result, a Si-containing layer containing O and C with a thickness of, for example, less than one atomic layer (one molecular layer) to several atomic layers (several molecular layers) is formed as a second layer on the surface of the underlayer 200b. When forming the second layer, at least a part of the Si-C bonds contained in the first layer are retained without being broken and are incorporated (remained) in the second layer as they are. As a result, the second layer becomes a layer containing Si-C bonds. In this specification, the Si-containing layer containing O and C is also simply referred to as a SiOC layer. When forming the second layer, impurities such as Cl contained in the first layer constitute a gaseous substance containing at least Cl during the oxidation reaction by H2O gas, and are discharged from the processing chamber 201. The second layer becomes a layer containing fewer impurities such as Cl than the first layer.
[0068] In this step, pyridine gas acting as a catalyst is supplied together with H2O gas, so that the above reaction can proceed in a non-plasma atmosphere and at a low temperature as described below. In this way, by forming the second layer in a non-plasma atmosphere and at a low temperature as described below, it becomes possible to maintain the methyl groups terminating the surface of the base 200a without disappearing (detaching) from the surface of the base 200a.
[0069] After the first layer formed on the surface of the base 200b is oxidized and changed (converted) into the second layer, the valves 243c and 243d are closed to stop the supply of H2O gas and pyridine gas into the processing chamber 201. Then, gases remaining in the processing chamber 201 are removed (purged) from the processing chamber 201 by the same processing procedure and processing conditions as those for purging in the surface modification.
[0070] The processing conditions in this step are as follows: H2O gas supply flow rate: 1 to 2000 sccm Pyridine gas supply flow rate: 1 to 2000 sccm N2 gas supply flow rate (per gas supply pipe): 0 to 20,000 sccm Each gas supply time: 1 to 60 seconds Treatment temperature: room temperature to 120°C, preferably room temperature to 100°C Processing pressure: 133~1333Pa Examples are given below.
[0071] As the O and H containing gas, in addition to HO gas, an O containing gas containing OH bonds such as hydrogen peroxide (HO) gas can be used. In addition, as the O and H containing gas, an O containing gas not containing OH bonds such as hydrogen (H) gas + oxygen (O) gas, H gas + ozone (O) gas, etc. can also be used.
[0072] [Perform the specified number of times] By performing the above-mentioned steps 1 and 2 a predetermined number of times (n times, n being an integer equal to or greater than 1) of cycles in which the steps are performed asynchronously, that is, not simultaneously, it becomes possible to selectively form a SiOC film on the surface of the underlayer 200b of the underlayers 200a and 200b exposed on the surface of the wafer 200, as shown in FIG. 6(e). It is preferable to repeat the above-mentioned cycle multiple times. That is, it is preferable to make the thickness of the second layer formed per cycle thinner than the desired film thickness, and to repeat the above-mentioned cycle multiple times until the film formed by stacking the second layers has the desired film thickness.
[0073] In addition, when steps 1 and 2 are performed, the methyl groups terminating the surface of the underlayer 200a are maintained without disappearing from the surface of the underlayer 200a as described above, so that no SiOC film is formed on the surface of the underlayer 200a. However, when the surface of the underlayer 200a is insufficiently modified due to some factor, a very small amount of SiOC film may be formed on the surface of the underlayer 200a. However, even in this case, the thickness of the SiOC film formed on the surface of the underlayer 200a is much thinner than the thickness of the SiOC film formed on the surface of the underlayer 200b. In this specification, the phrase "selectively forming a SiOC film on the surface of the underlayer 200b" among the underlayers 200a and 200b includes not only the case where no SiOC film is formed on the surface of the underlayer 200a at all, but also the case where a very thin SiOC film is formed on the surface of the underlayer 200a as described above.
[0074] (Post-processing) After the selective growth is completed, the output of the heater 207 is adjusted so that the temperature in the processing chamber 201, i.e., the temperature of the wafer 200 after the SiOC film is selectively formed on the surface of the underlayer 200b, is equal to or higher than the temperature of the wafer 200 in the selective growth, preferably higher than the temperature of the wafer 200 in the selective growth, and the wafer 200 after the selective growth is subjected to post-processing. As a result, as shown in FIG. 6(f), it is possible to remove the methyl groups terminating the surface of the underlayer 200a by desorbing them from the surface of the underlayer 200a, or to invalidate the inhibitor function of the methyl groups. This resets the surface state of the underlayer 200a, and in the subsequent process, it is possible to proceed with a film formation process on the surface of the underlayer 200a. This step may be performed in a state where a gas (assist gas) that promotes the removal (desorption) of the methyl groups, such as N2 gas, H2 gas, or O2 gas, is supplied into the processing chamber 201, or may be performed in a state where the supply of the assist gas into the processing chamber 201 is stopped.
[0075] The processing conditions in this step are as follows: Assist gas supply flow rate: 0 to 50,000 sccm Processing gas supply time: 1 to 18,000 seconds Treatment temperature: 120 to 1000°C, preferably 400 to 700°C Processing pressure: 1~120000Pa Examples are given below.
[0076] (After purging and atmospheric pressure recovery) After the selective formation of the SiOC film on the surface of the base 200b is completed and the resetting of the surface state of the base 200a is completed, N2 gas as a purge gas is supplied from each of the nozzles 249a to 249c into the processing chamber 201 and exhausted from the exhaust port 231a. This purges the processing chamber 201, and the gas and reaction by-products remaining in the processing chamber 201 are removed from the processing chamber 201 (after-purge). Thereafter, the atmosphere in the processing chamber 201 is replaced with an inert gas (inert gas replacement), and the pressure in the processing chamber 201 is returned to normal pressure (atmospheric pressure return).
[0077] (Boat unloading and wafer discharging) Thereafter, the seal cap 219 is lowered by the boat elevator 115, and the lower end of the manifold 209 is opened. Then, the processed wafers 200 are carried out from the lower end of the manifold 209 to the outside of the reaction tube 203 while being supported by the boat 217 (boat unloading). After the boat unloading, the shutter 219s is moved, and the lower end opening of the manifold 209 is sealed by the shutter 219s via the O-ring 220c (shutter close). After being carried out to the outside of the reaction tube 203, the processed wafers 200 are taken out of the boat 217 (wafer discharge).
[0078] (3) Effects of this mode According to this aspect, one or more of the following effects can be obtained.
[0079] (a) In the surface modification, the surface of the underlayer 200a is terminated with a hydrocarbon group, and in the selective growth, a film is formed while maintaining the state in which the surface of the underlayer 200a is terminated with a hydrocarbon group, thereby making it possible to selectively form a SiOC film on the surface of the underlayer 200b of the underlayers 200a and 200b exposed on the surface of the wafer 200. This makes it possible to simplify the process for processing the film, for example, by omitting a patterning process including photolithography when fabricating a semiconductor device. As a result, it becomes possible to improve the productivity of semiconductor devices and reduce manufacturing costs.
[0080] In addition, when an oxide film such as a SiOC film is formed on the surface of the base 200b using an oxidizing agent such as O3 gas, O2 plasma, or O2 gas + H2 gas after the surface of the base 200a is modified by terminating it with a hydrocarbon group such as an alkyl group using DMATMS gas or the like, there is a problem that the hydrocarbon group is easily desorbed from the surface of the base 200a by the oxidizing agent. Therefore, when an oxide film is selectively formed on the surface of the base 200b, it was difficult to think of using a hydrocarbon group that is weak against an oxidizing agent as an inhibitor. However, as a result of intensive research, the present inventors have found that by performing a certain special control when forming an oxide film, specifically, for example, by using H2O gas as an oxidizing agent, lowering the temperature condition as described above, and performing selective growth in a non-plasma atmosphere, it is possible to suppress the desorption of the hydrocarbon group acting as an inhibitor from the surface of the base 200a, and to retain the hydrocarbon group on the surface of the base 200a, even when an oxidizing agent is used. The present disclosure is based on these findings found by the present inventors.
[0081] (b) In the surface modification, by terminating the surface of the underlayer 200a with an alkyl group such as a methyl group, which is a type of hydrocarbon group, it becomes possible to more reliably and selectively form a SiOC film on the surface of the underlayer 200b of the underlayers 200a and 200b exposed on the surface of the wafer 200. In other words, it becomes possible to improve the selectivity in selective growth.
[0082] (c) In the surface modification, the surface of the underlayer 200a is terminated with an alkylsilyl group, particularly a trialkylsilyl group, thereby making it possible to improve the selectivity in selective growth. This effect is more pronounced when the surface of the underlayer 200a is terminated with a trialkylsilyl group in which three alkyl groups are bonded to Si, or a dialkylsilyl group in which two alkyl groups are bonded to Si, than when the surface of the underlayer 200a is terminated with a monoalkylsilyl group in which one alkyl group is bonded to Si.
[0083] (d) In the surface modification, by using a gas containing an amino group in addition to a hydrocarbon group such as an alkyl group, such as DMATMS gas, as the hydrocarbon group-containing gas, it is possible to efficiently perform the process of terminating the surface of the base 200a with a hydrocarbon group. This makes it possible to more reliably obtain the above-mentioned effects. In addition, it is possible to increase the productivity of the substrate processing.
[0084] (e) In selective growth, by using a catalyst such as pyridine gas, it is possible to proceed with the film formation process in a non-plasma atmosphere. In addition, it is possible to lower the processing temperature. As a result, it is possible to suppress the detachment of hydrocarbon groups such as methyl groups that terminate the surface of the underlayer 200a from the surface of the underlayer 200a in selective growth. As a result, it is possible to improve the selectivity in selective growth. In addition, since selective growth is performed in a non-plasma atmosphere, plasma damage to the wafer 200 can be avoided, and this method can be applied to processes where plasma damage is a concern.
[0085] (f) In the selective growth, by using a gas containing O and H, such as HO gas, as an oxidizing agent, it becomes possible to suppress the detachment of hydrocarbon groups, such as methyl groups, that terminate the surface of the underlayer 200a from the surface of the underlayer 200a in the selective growth. As a result, it becomes possible to improve the selectivity in the selective growth.
[0086] (g) Since the underlayer 200a includes a SiO film and the underlayer 200b includes a SiN film other than a SiO film, it is possible to reliably perform a process of selectively terminating the surface of the underlayer 200a, of the underlayers 200a and 200b exposed on the surface of the wafer 200, with a hydrocarbon group such as a methyl group in the surface modification, thereby making it possible to improve the selectivity in selective growth.
[0087] (h) By setting the temperature of the wafer 200 during selective growth to be equal to or lower than the temperature of the wafer 200 during surface modification, it is possible to reliably suppress the detachment of hydrocarbon groups such as methyl groups terminating the surface of the underlayer 200a from the surface of the underlayer 200a during selective growth. As a result, it is possible to improve the selectivity during selective growth.
[0088] (i) By setting the temperature of the wafer 200 during selective growth lower than the temperature of the wafer 200 during surface modification, it is possible to more reliably suppress the detachment of hydrocarbon groups such as methyl groups terminating the surface of the underlayer 200a from the surface of the underlayer 200a during selective growth, thereby making it possible to further increase the selectivity during selective growth.
[0089] (j) By adjusting the temperature of the wafer 200 during selective growth to be equal to or lower than the temperature of the wafer 200 during surface modification, and increasing the temperature of the wafer 200 within that range, it is possible to further improve the selectivity in selective growth.
[0090] (k) By adjusting the temperature of the wafer 200 during selective growth to be equal to or lower than the temperature of the wafer 200 during surface modification and increasing the temperature of the wafer 200 within that range, it is possible to appropriately reduce the formation rate of the SiOC film formed during selective growth. This allows fine adjustment of the thickness of the SiOC film to be formed, enabling precise matching to the target film thickness. In other words, it is possible to improve the film thickness controllability during selective growth.
[0091] (l) After the selective growth, a post-treatment is performed to raise the temperature of the wafer 200 to the temperature of the wafer 200 during the selective growth or higher, thereby making it possible to remove hydrocarbon groups such as methyl groups terminating the surface of the underlayer 200a by desorption from the surface of the underlayer 200a. This makes it possible to form a film on the surface of the underlayer 200a in a subsequent process. This post-treatment also makes it possible to remove impurities in the SiOC film formed on the surface of the underlayer 200b, densify the SiOC film, and improve the film quality of the SiOC film.
[0092] (m) After the selective growth, a post-treatment is performed to raise the temperature of the wafer 200 higher than the temperature of the wafer 200 during the selective growth, thereby making it possible to effectively remove and remove hydrocarbon groups such as methyl groups terminating the surface of the underlayer 200a from the surface of the underlayer 200a. This makes it possible to properly form a film on the surface of the underlayer 200a in the subsequent steps. Furthermore, this post-treatment can sufficiently remove impurities in the SiOC film formed on the surface of the underlayer 200b, more sufficiently densify the SiOC film, and further improve the film quality of the SiOC film.
[0093] (n) By performing the post-treatment in a state where an assist gas such as N2 gas, H2 gas, O2 gas, or H2O gas is supplied into the treatment chamber 201, it is possible to efficiently and effectively remove the hydrocarbon groups such as methyl groups terminating the surface of the base 200a from the surface of the base 200a. This makes it possible to appropriately form a film on the surface of the base 200a in the subsequent process. In addition, this post-treatment makes it possible to efficiently and effectively remove impurities in the SiOC film formed on the surface of the base 200b, thereby further improving the film quality of the SiOC film.
[0094] (o) The above-mentioned effects can be obtained similarly when a hydrocarbon group-containing gas other than DMATMS gas is used, when a Si- and halogen-containing gas other than BTCSM gas is used, when an O- and H-containing gas other than HO gas is used, when a catalyst other than pyridine gas is used, or when an inert gas other than N gas is used.
[0095] (4) Variations The substrate processing sequence in this embodiment can be modified as shown in the following modified examples. These modified examples can be combined as desired. Unless otherwise specified, the process procedure and process conditions in each step of each modified example can be the same as the process procedure and process conditions in each step of the substrate processing sequence described above.
[0096] (Variation 1) Before the surface modification, the surface of the wafer 200 may be cleaned with, for example, a diluted hydrofluoric acid (DHF) solution, i.e., a hydrogen fluoride (HF) solution (DHF cleaning) to remove a natural oxide film formed on at least one of the surfaces of the underlayer 200a and the underlayer 200b. This modification also provides the same effects as the above-mentioned embodiment. In addition, this modification makes it possible to reliably terminate the surface of the underlayer 200a with OH groups, and in the subsequent surface modification, it becomes possible to reliably perform a process of selectively terminating the surface of the underlayer 200a with methyl groups. This makes it possible to improve the selectivity in selective growth.
[0097] (Variation 2) In the post-treatment, an oxidizing agent or radicals may be supplied to the wafer 200 after a SiOC film has been selectively formed on the surface of the underlayer 200b, and the methyl groups terminating the surface of the underlayer 200a may be removed by being desorbed from the surface of the underlayer 200a, thereby resetting the surface state of the underlayer 200a (supply of oxidizing agent or radicals). As the oxidizing agent, H2O gas, H2O2 gas, O3 gas, H2 gas + O2 gas, H2 gas + O3 gas, etc. may be used. As the radicals, O-containing radicals (O * ), N-containing radicals (N * ), Ar-containing radicals (Ar * ), He-containing radicals (He *) or the like can be used. These radicals are contained in oxygen plasma, nitrogen plasma, argon plasma, and helium plasma, which are generated by plasma excitation of O-containing gas, N-containing gas, Ar-containing gas, and He-containing gas, respectively. According to this modification, it is possible to actively remove the methyl groups terminating the surface of the underlayer 200a from the surface of the underlayer 200a. It is also possible to actively remove impurities in the SiOC film formed on the surface of the underlayer 200b, thereby improving the film quality of the SiOC film. This modification can also be performed in combination with the post-treatment in the above-mentioned embodiment. In this case, it is possible to more reliably remove the methyl groups terminating the surface of the underlayer 200a from the surface of the underlayer 200a, and it is also possible to further improve the film quality of the SiOC film formed on the surface of the underlayer 200b.
[0098] The processing conditions when supplying H2O gas as an oxidizing agent are as follows: H2O gas supply flow rate: 100 to 50,000 sccm H2O gas supply time: 1 to 18,000 seconds Treatment temperature: 120 to 1000°C, preferably 400 to 700°C Processing pressure: 1~120000Pa Examples are given below.
[0099] The processing conditions when supplying H2O2 gas as an oxidizing agent are as follows: H2O2 gas supply flow rate: 100~50000sccm H2O2 gas supply time: 1 to 18,000 seconds Treatment temperature: 120 to 1000°C, preferably 400 to 700°C Processing pressure: 1~120000Pa Examples are given below.
[0100] The processing conditions when supplying O3 gas as an oxidizing agent are as follows: O3 gas supply flow rate: 100~50000sccm O3 gas supply time: 1 to 18,000 seconds Treatment temperature: 120 to 1000°C, preferably 400 to 700°C Processing pressure: 1~120000Pa Examples are given below.
[0101] The processing conditions when supplying H2 gas + O2 gas as oxidizing agents are as follows: H2 gas supply flow rate: 100~50000sccm O2 gas supply flow rate: 100~50000sccm Each gas supply time: 1 to 18,000 seconds Treatment temperature: 400 to 1000°C, preferably 400 to 700°C Treatment pressure: 1 to 2000 Pa, preferably 1 to 1000 Pa Examples are given below.
[0102] The processing conditions when supplying H2 gas + O3 gas as oxidizing agents are as follows: H2 gas supply flow rate: 100~50000sccm O3 gas supply flow rate: 100~50000sccm Each gas supply time: 1 to 18,000 seconds Treatment temperature: 400 to 1000°C, preferably 400 to 700°C Treatment pressure: 1 to 2000 Pa, preferably 1 to 1000 Pa Examples are given below.
[0103] O as radical * The treatment conditions for supplying are as follows: O2 gas supply flow rate: 100~50000sccm O2 gas supply time: 1 to 18,000 seconds RF power: 50~1500W Processing temperature: 25~1000℃ Processing pressure: 1~1000Pa Examples are given below.
[0104] N as radical * The treatment conditions for supplying are as follows: N2 gas supply flow rate: 100 to 50,000 sccm N2 gas supply time: 1 to 18,000 seconds RF power: 50~1500W Processing temperature: 25~1000℃ Processing pressure: 1~1000Pa Examples are given below.
[0105] Ar as radical * The treatment conditions for supplying are as follows: Ar gas supply flow rate: 100 to 50,000 sccm Ar gas supply time: 1 to 18,000 seconds RF power: 50~1500W Processing temperature: 25~1000℃ Processing pressure: 1~1000Pa Examples are given below.
[0106] He as radical * The treatment conditions for supplying are as follows: He gas supply flow rate: 100 to 50,000 sccm Gas supply time: 1 to 18,000 seconds RF power: 50~1500W Processing temperature: 25~1000℃ Processing pressure: 1~1000Pa Examples are given below.
[0107] <Other Aspects of the Disclosure> Although the embodiments of the present disclosure have been specifically described above, the present disclosure is not limited to the above embodiments and can be modified in various ways without departing from the spirit and scope of the present disclosure.
[0108] For example, as shown in the process sequence below, in selective growth, a cycle of non-simultaneously supplying HCDS gas and pyridine gas to the wafer 200 and supplying H2O gas and pyridine gas to the wafer 200 may be performed a predetermined number of times (n times, n is an integer of 1 or more) to form a silicon oxide film (SiO film) as a film on the surface of the base 200b. The process conditions in the step of supplying HCDS gas and pyridine gas to the wafer 200 may be the same as the process conditions in step 1 of the above-mentioned embodiment. The process conditions in the step of supplying H2O gas and pyridine gas to the wafer 200 may be the same as the process conditions in step 2 of the above-mentioned embodiment. In this case, the same effect as in the above-mentioned embodiment can be obtained.
[0109] DMATMS→(HCDS+Py→H2O+Py)×n→Post-Treatment ⇒ SiO
[0110] Also, for example, after selective growth, no post-treatment may be performed, as in the processing sequence shown below. In this case, the same effects as those of the above-mentioned embodiment can be obtained except for the effects of the post-treatment. Depending on the process performed after selective growth, it may not be necessary to reset the surface state of the base 200a, in which case post-treatment is not necessary.
[0111] DMATMS→(BTCSM+Py→H2O+Py)×n ⇒ SiOC DMATMS→(HCDS+Py→H2O+Py)×n ⇒ SiO
[0112] Also, for example, in the surface modification, the supply of DMATMS gas to the wafer 200 and purging may be alternately repeated multiple times. That is, the supply of DMATMS gas to the wafer 200 may be intermittently performed with purging in between. In this case, the purging can remove unnecessary physically adsorbed components of the DMATMS gas adsorbed on the surface of the wafer 200, while terminating the surface of the underlayer 200a with methyl groups contained in DMATMS, thereby increasing the density of methyl groups on the surface of the underlayer 200a. As a result, the selectivity in selective growth can be further improved. In addition, the amount of DMATMS gas used can be reduced.
[0113] Also, for example, in the surface modification, DMATMS gas may be supplied to the wafer 200 with the exhaust system closed, i.e., with the APC valve 244 fully closed. That is, in the surface modification, DMATMS gas may be confined within the processing chamber 201. In this case, it is possible to spread the DMATMS gas throughout the entire processing chamber 201 and throughout the entire surface of the wafer 200, and it is possible to uniformly terminate the surface of the underlayer 200a of each wafer 200 with methyl groups. As a result, it is possible to further improve the selectivity in selective growth. It is also possible to significantly reduce the amount of DMATMS gas used.
[0114] In the surface modification, the containment of DMATMS gas in the processing chamber 201 and purging may be repeated alternately multiple times. That is, the containment of DMATMS gas in the processing chamber 201 may be performed intermittently with purging in between. In this case, the purging can remove unnecessary physically adsorbed components of the DMATMS gas adsorbed on the surface of the wafer 200, while terminating the surface of the underlayer 200a with methyl groups contained in DMATMS, thereby increasing the density of methyl groups on the surface of the underlayer 200a. As a result, the selectivity in selective growth can be further improved.
[0115] In addition, for example, in the selective growth, not only silicon oxide films such as SiOC films and SiO films, but also metal oxide films such as aluminum oxide films (AlO films), titanium oxide films (TiO films), hafnium oxide films (HfO films), and zirconium oxide films (ZrO films) may be formed. In these cases, selective growth can be performed using the above-mentioned hydrocarbon group-containing gas, raw materials containing metal elements such as Al, Ti, Hf, and Zr, and the above-mentioned oxidizing agent, etc., by a process procedure similar to the process conditions in the above-mentioned embodiment. In this case, the same effects as those in the above-mentioned embodiment can be obtained. In addition, when forming a metal oxide film, it is possible to omit the supply of a catalyst such as pyridine.
[0116] It is preferable that the recipes used for each process are prepared individually according to the process contents and stored in the storage device 121c via an electric communication line or an external storage device 123. Then, when starting each process, it is preferable that the CPU 121a appropriately selects an appropriate recipe according to the process contents from among the multiple recipes stored in the storage device 121c. This makes it possible to form films of various film types, composition ratios, film qualities, and film thicknesses with good reproducibility using a single substrate processing device. It is also possible to reduce the burden on the operator and quickly start each process while avoiding operational errors.
[0117] The above-mentioned recipes may not only be newly created, but may also be prepared by modifying an existing recipe that has already been installed in the substrate processing apparatus. When modifying a recipe, the modified recipe may be installed in the substrate processing apparatus via an electric communication line or a recording medium on which the recipe has been recorded. In addition, an existing recipe that has already been installed in the substrate processing apparatus may be directly modified by operating the input / output device 122 provided in the existing substrate processing apparatus.
[0118] In the above-mentioned embodiment, an example of forming a film using a batch-type substrate processing apparatus that processes multiple substrates at a time has been described. The present disclosure is not limited to the above-mentioned embodiment, and can be suitably applied to, for example, a case where a film is formed using a single-wafer type substrate processing apparatus that processes one or several substrates at a time. Also, in the above-mentioned embodiment, an example of forming a film using a substrate processing apparatus having a hot-wall type processing furnace has been described. The present disclosure is not limited to the above-mentioned embodiment, and can be suitably applied to, for example, a case where a film is formed using a substrate processing apparatus having a cold-wall type processing furnace.
[0119] When these substrate processing apparatuses are used, the processes can be performed under the same processing procedures and conditions as in the above embodiment, and the same effects as in the above embodiment can be obtained.
[0120] The above-mentioned aspects may be used in appropriate combination. The processing procedures and processing conditions in this case may be the same as those of the above-mentioned aspects. EXAMPLES
[0121] For samples 1 to 6, a SiOC film was formed on the surface of the base exposed on the surface of the wafer by the process sequence of the above-mentioned embodiment. The bases for samples 1 to 6 were, in this order, the surface of a silicon wafer (single crystal Si), an amorphous carbon film (aC film), a SiO film, an aluminum oxide film (AlO film), a SiN film, and a titanium nitride film (TiN film). The process conditions in each step were predetermined conditions within the range of process conditions in each step of the above-mentioned embodiment, and were the same for each sample.
[0122] Then, the thicknesses of the SiOC films formed in Samples 1 to 6 were measured. The measurement results of the thicknesses of the SiOC films are shown in Fig. 7. The vertical axis of Fig. 7 shows the thickness (Å) of the SiOC film formed on the surface of the base, and the horizontal axis shows Samples 1 to 6 in this order.
[0123] As shown in Fig. 7, it was found that the thickness of the SiOC film in sample 3, which has an SiO film as an underlayer, is much thinner than the thicknesses of the SiOC films in the other samples. That is, it was found that, according to the processing sequence of the above-mentioned embodiment, it is possible to selectively form a SiOC film on the surface of various underlayers (single crystal Si, aC film, AlO film, SiN film, TiN film) other than the SiO film among the multiple types of underlayers exposed on the surface of the wafer.
[0124] <Preferred aspects of the present disclosure> Preferred aspects of the present disclosure will be described below.
[0125] (Appendix 1) According to one aspect of the present disclosure, (a) supplying a hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer exposed on a surface thereof to modify the surface of the first underlayer so as to terminate the surface with a hydrocarbon group; (b) supplying an oxygen- and hydrogen-containing gas to the substrate after modifying the surface of the first underlayer, and selectively forming a film on the surface of the second underlayer; A method for manufacturing a semiconductor device having the above structure or a method for processing a substrate is provided.
[0126] (Appendix 2) 2. The method according to claim 1, comprising: In (b), a catalyst is further provided to the substrate.
[0127] (Appendix 3) 3. The method according to claim 1 or 2, In (b), a silicon and halogen-containing gas is further supplied to the substrate.
[0128] (Appendix 4) The method according to any one of appendix 1 to 3, In (b), a cycle of non-simultaneously supplying a silicon- and halogen-containing gas, and a catalyst to the substrate, and supplying the oxygen- and hydrogen-containing gas, and a catalyst to the substrate is performed a predetermined number of times.
[0129] (Appendix 5) The method according to any one of appendix 1 to 4, The temperature of the substrate in (b) is set to be equal to or lower than the temperature of the substrate in (a).
[0130] (Appendix 6) The method according to any one of appendix 1 to 5, The temperature of the substrate in (b) is made lower than the temperature of the substrate in (a).
[0131] (Appendix 7) 7. The method according to claim 5 or 6, By adjusting the temperature of the substrate in (b) to be higher, the selectivity is controlled to be higher.
[0132] (Appendix 8) The method according to any one of appendix 5 to 7, By adjusting the temperature of the substrate in (b) to be higher, the film formation rate is controlled to be lowered.
[0133] (Appendix 9) The method according to any one of appendix 1 to 8, (c) The method further includes a step of supplying an oxidizing agent or radicals to the substrate after a film has been selectively formed on the surface of the second underlayer, and removing the hydrocarbon group terminating the surface of the first underlayer.
[0134] (Appendix 10) The method according to any one of appendix 1 to 9, (c) The method further includes a step of increasing the temperature of the substrate after a film has been selectively formed on the surface of the second underlayer to a temperature equal to or higher than the temperature of the substrate in (b) and removing the hydrocarbon groups terminating the surface of the first underlayer.
[0135] (Appendix 11) The method according to any one of appendix 1 to 9, (c) further comprising a step of increasing the temperature of the substrate after a film has been selectively formed on the surface of the second underlayer to a temperature higher than the temperature of the substrate in (b) to remove the hydrocarbon groups terminating the surface of the first underlayer.
[0136] (Appendix 12) The method according to any one of appendix 1 to 11, The method further includes a step of (d) (removing a native oxide film formed on at least one of the surfaces of the first underlayer and the second underlayer) terminating the surface of the first underlayer with hydroxyl groups before carrying out (a).
[0137] (Appendix 13) The method according to any one of appendix 1 to 12, The hydrocarbon group includes an alkyl group.
[0138] (Appendix 14) The method according to any one of appendix 1 to 12, The hydrocarbon group includes an alkylsilyl group. Among the alkylsilyl groups, a trialkylsilyl group or a dialkylsilyl group is more preferable.
[0139] (Appendix 15) The method according to any one of appendix 1 to 14, The hydrocarbon group-containing gas further contains an amino group.
[0140] (Appendix 16) The method according to any one of appendix 1 to 15, The oxygen and hydrogen containing gas is H2O gas.
[0141] (Appendix 17) The method according to any one of appendix 1 to 16, The first underlayer is an oxide film (for example, a silicon oxide film), and the second underlayer is a film other than an oxide film (for example, a silicon oxide film).
[0142] (Appendix 18) The method according to any one of appendix 1 to 17, (a) and (b) are carried out in a non-plasma atmosphere.
[0143] (Appendix 19) According to another aspect of the present disclosure, a processing chamber in which the substrate is processed; a hydrocarbon group-containing gas supply system for supplying a hydrocarbon group-containing gas to the substrate in the processing chamber; an oxygen and hydrogen containing gas supply system for supplying an oxygen and hydrogen containing gas to the substrate in the processing chamber; a temperature regulator for adjusting the temperature of the substrate in the processing chamber; a control unit configured to be able to control the hydrocarbon group-containing gas supply system, the oxygen and hydrogen-containing gas supply system, and the temperature regulator so as to perform each treatment (each step) of Appendix 1 in the treatment chamber; A substrate processing apparatus having a
[0144] (Appendix 20) According to yet another aspect of the present disclosure, There is provided a program for causing a substrate processing apparatus to execute each procedure (each step) of Supplementary Note 1 by a computer, or a computer-readable recording medium having the program recorded thereon. [Explanation of symbols]
[0145] 200 wafers (substrates) 200a 1st base 200b 2nd Base
Claims
1. (a) (a1) a step of supplying a hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer on a surface thereof, thereby terminating a surface of the first underlayer with a hydrocarbon group; and (a2) a step of evacuating a space in which the substrate is present; (b) (b1) supplying a silicon-containing gas or a metal element-containing gas to the substrate having the surface of the first underlayer terminated with a hydrocarbon group to form a first layer, and (b2) supplying an oxygen- and hydrogen-containing gas to the substrate to oxidize the first layer to form a second layer, thereby forming a film on the surface of the second underlayer by repeating these steps a predetermined number of times; having (b) setting the temperature of the substrate to be equal to or lower than the temperature of the substrate in (a); (b1) supplies the silicon-containing gas and a catalyst to the substrate; (b2) is a substrate processing method in which the oxygen- and hydrogen-containing gas and a catalyst are supplied to the substrate.
2. (a) (a1) a step of supplying a hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer on a surface thereof, thereby terminating a surface of the first underlayer with a hydrocarbon group; and (a2) a step of evacuating a space in which the substrate is present; (b) (b1) supplying a silicon-containing gas or a metal element-containing gas to the substrate having the surface of the first underlayer terminated with a hydrocarbon group to form a first layer, and (b2) supplying an oxygen- and hydrogen-containing gas to the substrate to oxidize the first layer to form a second layer, thereby forming a film on the surface of the second underlayer by repeating these steps a predetermined number of times; having (b) setting the temperature of the substrate lower than the temperature of the substrate in (a); (b1) supplies the silicon-containing gas and a catalyst to the substrate; (b2) is a substrate processing method in which the oxygen- and hydrogen-containing gas and a catalyst are supplied to the substrate.
3. (a) (a1) a step of supplying a hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer on a surface thereof, thereby terminating a surface of the first underlayer with a hydrocarbon group; and (a2) a step of evacuating a space in which the substrate is present; (b) (b1) supplying a silicon-containing gas or a metal element-containing gas to the substrate having the surface of the first underlayer terminated with a hydrocarbon group to form a first layer, and (b2) supplying an oxygen- and hydrogen-containing gas to the substrate to oxidize the first layer to form a second layer, thereby forming a film on the surface of the second underlayer by repeating these steps a predetermined number of times; (c) performing post-treatment on the substrate on which the film is formed on the surface of the second undercoat; having (b) setting the temperature of the substrate to be equal to or lower than the temperature of the substrate in (a); A substrate processing method, comprising: setting the temperature of the substrate in (c) equal to or higher than the temperature of the substrate in (b); or setting the temperature of the substrate higher than the temperature of the substrate in (b).
4. 3. The substrate processing method according to claim 1, further comprising the step of: (c) supplying an oxidizing agent or radicals to the substrate having a film formed on the surface of the second base, and removing hydrocarbon groups terminating the surface of the first base.
5. 4. The substrate processing method according to claim 3, wherein in step (c), an oxidizing agent or radicals are supplied to the substrate to remove hydrocarbon groups terminating the surface of the first underlayer.
6. (a) (a1) a step of supplying a hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer on a surface thereof, thereby terminating a surface of the first underlayer with a hydrocarbon group; and (a2) a step of evacuating a space in which the substrate is present; (b) (b1) supplying a silicon-containing gas or a metal element-containing gas to the substrate having the surface of the first underlayer terminated with a hydrocarbon group to form a first layer, and (b2) supplying an oxygen- and hydrogen-containing gas to the substrate to oxidize the first layer to form a second layer, thereby forming a film on the surface of the second underlayer by repeating these steps a predetermined number of times; (c) raising the temperature of the substrate on which a film has been formed on the surface of the second underlayer to a temperature equal to or higher than the temperature of the substrate in (b) or higher than the temperature of the substrate in (b); having A substrate processing method comprising: (b) setting the temperature of the substrate to a temperature equal to or lower than the temperature of the substrate in (a).
7. 7. The substrate processing method according to claim 6, wherein in (c), at least one of removing hydrocarbon groups terminating the surface of the first underlayer and nullifying their function as inhibitors is carried out.
8. 8. The substrate processing method according to claim 1, further comprising the step of: (d) terminating the surface of the first underlayer with a hydroxyl group, before carrying out (a).
9. The substrate processing method according to any one of claims 1 to 7, further comprising the step of: (d) removing a native oxide film formed on a surface of at least one of the first base and the second base before performing (a).
10. 10. The method of claim 1, wherein the hydrocarbon group includes an alkyl group. Law.
11. 11. The substrate processing method according to claim 1, wherein the hydrocarbon group includes an alkylsilyl group.
12. 12. The substrate processing method according to claim 1, wherein the hydrocarbon group-containing gas further contains an amino group.
13. The oxygen and hydrogen containing gas is H 2 The substrate processing method according to any one of claims 1 to 12, wherein the gas is O gas.
14. 14. The substrate processing method according to claim 1, wherein the first underlayer is an oxide film, and the second underlayer is a film other than an oxide film.
15. The substrate processing method according to any one of claims 1 to 14, wherein in (a1), the hydrocarbon group-containing gas is sealed in a space in which the substrate is present.
16. The substrate processing method according to any one of claims 1 to 15, wherein in (a), (a1) and (a2) are alternately repeated a plurality of times.
17. The substrate processing method according to any one of claims 1 to 16, wherein (a) and (b) are carried out in a non-plasma atmosphere.
18. (a) (a1) a step of supplying a hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer on a surface thereof, thereby terminating a surface of the first underlayer with a hydrocarbon group; and (a2) a step of evacuating a space in which the substrate is present; (b) (b1) supplying a silicon-containing gas or a metal element-containing gas to the substrate having the surface of the first underlayer terminated with a hydrocarbon group to form a first layer, and (b2) supplying an oxygen- and hydrogen-containing gas to the substrate to oxidize the first layer to form a second layer, thereby forming a film on the surface of the second underlayer by repeating these steps a predetermined number of times; having (b) setting the temperature of the substrate to be equal to or lower than the temperature of the substrate in (a); (b1) supplies the silicon-containing gas and a catalyst to the substrate; (b2) A method for manufacturing a semiconductor device, comprising supplying the oxygen- and hydrogen-containing gas and a catalyst to the substrate.
19. (a) (a1) a step of supplying a hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer on a surface thereof, thereby terminating a surface of the first underlayer with a hydrocarbon group; and (a2) a step of evacuating a space in which the substrate is present; (b) (b1) supplying a silicon-containing gas or a metal element-containing gas to the substrate having the surface of the first underlayer terminated with a hydrocarbon group to form a first layer, and (b2) supplying an oxygen- and hydrogen-containing gas to the substrate to oxidize the first layer to form a second layer, thereby forming a film on the surface of the second underlayer by repeating these steps a predetermined number of times; (c) raising the temperature of the substrate on which a film has been formed on the surface of the second underlayer to a temperature equal to or higher than the temperature of the substrate in (b) or higher than the temperature of the substrate in (b); having A method of manufacturing a semiconductor device, comprising the steps of: (b) setting the temperature of the substrate to be equal to or lower than the temperature of the substrate in (a).
20. a first gas supply system for supplying a hydrocarbon group-containing gas to the substrate; a second gas supply system that supplies a silicon-containing gas or a metal element-containing gas to the substrate; a third gas supply system that supplies an oxygen- and hydrogen-containing gas to the substrate; a catalyst supply system for supplying a catalyst to the substrate; A temperature regulator for adjusting the temperature of the substrate; an exhaust system that exhausts a space in which the substrate is present; (a) (a1) a process of supplying the hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer on a surface thereof, and terminating the surface of the first underlayer with a hydrocarbon group, (a2) a process of evacuating a space in which the substrate is present, (b) (b1) a process of supplying the silicon-containing gas or the metal element-containing gas to the substrate having the surface of the first underlayer terminated with a hydrocarbon group, and forming a first layer, and (b2) a process of supplying the oxygen- and hydrogen-containing gas to the substrate, and oxidizing the first layer to form a second layer, the process being repeated a predetermined number of times. a control unit configured to be able to control the first gas supply system, the second gas supply system, the third gas supply system, the catalyst supply system, the temperature regulator, and the exhaust system so as to perform a process of forming a film on the surface of the second base by performing a process of (b) making the temperature of the substrate equal to or lower than the temperature of the substrate in (a), supplying the silicon-containing gas and the catalyst to the substrate in (b1), and supplying the oxygen- and hydrogen-containing gas and the catalyst to the substrate in (b2); A substrate processing apparatus comprising:
21. a first gas supply system for supplying a hydrocarbon group-containing gas to the substrate; a second gas supply system that supplies a silicon-containing gas or a metal element-containing gas to the substrate; a third gas supply system that supplies an oxygen- and hydrogen-containing gas to the substrate; A temperature regulator for adjusting the temperature of the substrate; an exhaust system that exhausts a space in which the substrate is present; (a) (a1) a process of supplying the hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer on a surface thereof, and terminating the surface of the first underlayer with a hydrocarbon group, (a2) a process of evacuating a space in which the substrate is present, (b) (b1) a process of supplying the silicon-containing gas or the metal element-containing gas to the substrate having the surface of the first underlayer terminated with a hydrocarbon group, and forming a first layer, (b2) a process of supplying the oxygen- and hydrogen-containing gas to the substrate, and oxidizing the first layer to form a second layer, a control unit configured to control the first gas supply system, the second gas supply system, the third gas supply system, the temperature regulator, and the exhaust system so as to perform a process of forming a film on the surface of the second base by performing the process above a predetermined number of times, and a process of making the temperature of the substrate on which the film has been formed on the surface of the second base equal to or higher than the temperature of the substrate in the process above (b) or higher than the temperature of the substrate in the process above (b), and to make the temperature of the substrate in the process above (b) equal to or lower than the temperature of the substrate in the process above (a); A substrate processing apparatus comprising:
22. (a) (a1) supplying a hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer on a surface thereof, thereby terminating a surface of the first underlayer with a hydrocarbon group; and (a2) evacuating a space in which the substrate is present; (b) forming a film on the surface of the second underlayer by repeating the steps of (b1) supplying a silicon-containing gas or a metal element-containing gas to the substrate having the surface of the first underlayer terminated with a hydrocarbon group to form a first layer, and (b2) supplying an oxygen- and hydrogen-containing gas to the substrate to oxidize the first layer to form a second layer a predetermined number of times; (b) setting the temperature of the substrate to a temperature equal to or lower than the temperature of the substrate in (a); (b1) supplying the silicon-containing gas and a catalyst to the substrate; (b2) supplying the oxygen and hydrogen containing gas and a catalyst to the substrate; A program for causing a computer to execute the above in a substrate processing apparatus.
23. (a) (a1) supplying a hydrocarbon group-containing gas to a substrate having a first underlayer and a second underlayer on a surface thereof, thereby terminating a surface of the first underlayer with a hydrocarbon group; and (a2) evacuating a space in which the substrate is present; (b) forming a film on the surface of the second underlayer by repeating the steps of (b1) supplying a silicon-containing gas or a metal element-containing gas to the substrate having the surface of the first underlayer terminated with a hydrocarbon group to form a first layer, and (b2) supplying an oxygen- and hydrogen-containing gas to the substrate to oxidize the first layer to form a second layer a predetermined number of times; (c) raising the temperature of the substrate on which a film has been formed on the surface of the second underlayer to a temperature equal to or higher than the temperature of the substrate in (b) or higher than the temperature of the substrate in (b); (b) setting the temperature of the substrate to a temperature equal to or lower than the temperature of the substrate in (a); A program for causing a computer to execute the above in a substrate processing apparatus.
Citation Information
Patent Citations
Semiconductor device manufacturing method
JP2013243193A
Semiconductor device manufacturing method, substrate processing apparatus, and program
JP2015053445A
Method for forming nitride film
JP2017174919A
Selective accumulation by surface treatment
JP2017222928A
Pile of oxide thin film
JP2018100446A